Composite spinneret and method for producing composite fiber

The stretch yarn with coiled crimps and an eccentric core-sheath cross-section, combined with a controlled composite die, addresses entanglement and instability issues, offering enhanced motion followability and resistance in textile products.

JP7567986B2Active Publication Date: 2024-10-16TORAY INDUSTRIES INC
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2023087042
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-11-06
Filing Date
2023-05-26
Publication Date
2024-10-16
Estimated Expiration
2039-11-01

AI Technical Summary

Technical Problem

Existing composite fibers with side-by-side crimps face issues such as entanglement, uneven crimp distribution, and instability during stretching, leading to inadequate motion followability and resistance, which affects the comfort and performance of stretchable clothing.

Method used

A stretch yarn with a multifilament structure featuring coiled crimps in two or more groups, an eccentric core-sheath cross-section, and a composite die that controls crimp form and suppresses discharge bending, ensuring stable discharge and crimpability.

Benefits of technology

The solution provides a stretch yarn with controlled crimp distribution, enhancing motion followability and resistance, resulting in comfortable and durable textile products with improved stretchability and abrasion resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007567986000005
    Figure 0007567986000005
  • Figure 0007567986000006
    Figure 0007567986000006
  • Figure 0007567986000007
    Figure 0007567986000007
Patent Text Reader

Abstract

To provide a stretch textured yarn which can be formed into a fiber material having good stretchability and motion following ability due to proper resistance at the time of elongation and has soft surface touch corresponding to a crimped form.SOLUTION: A composite spinneret is composed of a measuring plate having a plurality of measuring holes for measuring each polymeric component, one or more distribution plates having been bored with distribution holes for distribution of each polymeric component, and a discharge plate. In a downstream side undermost layer in a polymer spinning twist path direction of the distribution plate, a polymer distribution hole group having a plurality of first component polymer distribution holes in a semicircular arrangement being surrounded with a plurality of second component polymer distribution holes are bored. At least in a part of the second component polymer distribution holes are arranged in a semi-circumferential shape arrangement on an outside of a circumferential part of the first component polymer distribution hole. A total hole number Ht of the second component polymer distribution holes and a hole number Ho of the second component polymer distribution holes arranged in semi-circumferential shape arrangement on the outside of the circumferential part of the first component polymer distribution holes satisfies a formula (1):1 / 16<Ho / Ht<1 / 4.SELECTED DRAWING: Figure 11
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a stretch textured yarn made of a multifilament having a coil-shaped crimp, and a composite spinneret for producing the stretch textured yarn. [Background technology]

[0002] Fibers made from thermoplastic polymers such as polyester and polyamide have various excellent properties including mechanical properties and dimensional stability, and are therefore used in a wide range of applications, from clothing to interiors, vehicle interiors, industrial materials, etc. As people desire more comfortable lives, the demands for more advanced properties in fiber materials are increasing, and the clothing materials that are most familiar to us are being actively improved in order to provide greater comfort.

[0003] The comfort of clothing materials varies depending on the environment and atmosphere in which the material is used, but it is no exaggeration to say that stretch performance, which refers to the properties related to the elasticity and stretchability of the fabric, is one of the basic properties that is directly linked to wearing comfort.

[0004] Stretch materials have been widely used in high-performance sportswear for athletes who exercise harshly in unique environments, but in recent years, their ease of wear and ease of movement have been recognized by general users, and they are tending to be used in a wide range of apparel materials. Along with this trend, it is no longer enough to simply achieve stretchability such as stretching and shrinking, and active development is being carried out on high-performance stretch materials that add other functions or control the behavior of stretching and shrinking to express more complex and advanced stretchability.

[0005] It is known that when people wear clothing and move, they feel stress due to friction between the clothing and the skin and tension when they move widely, and not feeling this leads to comfortable wear. In other words, improving the ability to follow human movements results in a stress-free, comfortable clothing material. To achieve a stress-free stretch material, it is important that the clothing fits the shape of the body when worn and has a moderate tightness, that is, it stretches well while having a moderate holding feeling. In response to these issues, a technology has been disclosed regarding latent shrinkage-producing fibers in which different polymers are bonded together side-by-side to produce a spiral structure due to the shrinkage difference.

[0006] Patent Document 1 discloses a composite fiber with a side-by-side cross section in which two types of polyethylene terephthalate (PET) with different intrinsic or intrinsic viscosities are bonded to each other, and Patent Document 2 discloses a technology related to a side-by-side composite fiber made of polytrimethylene terephthalate (PTT) and PET. It is known that such side-by-side composite fibers in which two types of polymers are bonded together can exhibit crimping according to the difference in shrinkage rate between the polymers when subjected to heat treatment or the like, and are generally called latent crimp fibers. The crimp of this three-dimensional spiral structure can stretch and shrink, and latent crimp fibers are fibers that appeal to this stretchability.

[0007] Furthermore, the above-mentioned latent crimped fibers can exhibit resistance during elongation, which is essential for fabrics with an appropriate sense of hold, by utilizing the elongation properties due to the polymer structure and controlling the crimp morphology, in addition to the stretchability due to the elongation of the crimped structure.

[0008] Patent Document 3 discloses a technology related to side-by-side type composite fibers made of PTTs with different intrinsic viscosities or copolymerization rates. The composite fibers described in Patent Document 3 are allowed to develop crimp, so that the fibers themselves elongate in the high strain region during elongation deformation, and become fabrics with high resilience and powerful stretch performance according to the elastic polymer properties of the PTT.

[0009] In order to further improve the stretchability of clothing materials in addition to the latent shrinkage that occurs due to the shrinkage difference as described above, it is possible to carry out yarn processing, and this is disclosed in Patent Documents 4 and 5.

[0010] Patent Document 4 proposes a PTT-based false twisted fiber obtained by false twisting a side-by-side composite fiber made of PTT. In the technology of Patent Document 4, in addition to the latent crimp caused by the false twisting, a false twisting process is imparted, so that the crimp stretching force of a single fiber can be effectively utilized, resulting in a fabric with excellent stretchability and instantaneous elongation recovery.

[0011] Patent Document 5 proposes a composite crimped yarn having converging and non-converging parts in the length direction of the textured yarn, which is produced by mixing at least two types of latent crimped fibers through post-processing. In the textured yarn described in Patent Document 5, the non-converging parts are responsible for the stretchability, and the converging parts are responsible for the resilience, resulting in a fabric with resilient stretch properties.

[0012] Furthermore, the greater the shrinkage difference in the spinning process between the high shrinkage side polymer A and the low shrinkage side polymer B, the greater the degree of shrinkage of the latent crimp-producing fiber will be, and the greater the stretchability of the fabric produced. To achieve this, for example, it is possible to increase the difference in melt viscosity between the combined polymers A and B, but it is known that increasing the difference in melt viscosity between the polymers can reduce extrusion stability, making stable production difficult.

[0013] Figure 8(b) shows a typical composite spinneret used for spinning latent crimp-producing fibers with a composite cross section as shown in Figure 8(a). When two types of thermoplastic polymers with different melt viscosities are spun using such a composite spinneret, the polymer on the higher viscosity side (high-viscosity polymer A) is pushed by the polymer on the lower viscosity side (low-viscosity polymer B), resulting in a phenomenon of discharge bending in which the composite polymer is discharged in a curved state, causing yarn swaying and yarn breakage due to contact with the spinneret surface. Therefore, in order to achieve stable discharge, the discharge conditions may be limited.

[0014] It is believed that this discharge bending phenomenon is caused by the flow behavior of the composite polymer stream in the composite spinneret. When two kinds of polymers with different melt viscosities are spun using a composite spinneret as shown in Fig. 8(b), a polymer stream of high-viscosity polymer A introduced through induction hole 1 and a polymer stream of low-viscosity polymer B introduced through induction hole 2 are joined at introduction hole 4 as shown in Fig. 8(c). Due to the difference in melt viscosities of the two kinds of polymers, the resistance that each polymer stream receives from the wall surface of introduction hole 4 differs, and as a result, the radial velocity distribution in introduction hole 4 becomes asymmetrical as shown in Fig. 8(c) as the stream progresses through introduction hole 4, and it is presumed that the discharge bending phenomenon occurs in polymer stream G discharged from spinneret discharge hole 8.

[0015] Discharging a composite polymer having this asymmetric velocity distribution creates a difference in the linear velocity of the polymers immediately after discharging, resulting in a curved state toward the high viscosity polymer side.

[0016] To address such spinnability issues, for example, Patent Document 6 proposes a composite spinneret that suppresses the phenomenon of bent discharge by controlling the flow speed when polymer streams join together.

[0017] The composite spinneret described in Patent Document 6 will be described with reference to Figs. 9(a) and 9(b). In the composite spinneret described in Patent Document 6, a polymer flow of a high-viscosity polymer A (high-viscosity polymer flow) introduced through an induction hole 1 and a polymer flow of a low-viscosity polymer B (low-viscosity polymer flow) introduced through an induction hole 2 are joined at an introduction hole 4. At this time, as shown in Fig. 9(b), in the low-viscosity polymer flow, a flow path 5 in which the groove width W is continuously widened along the flow direction of the low-viscosity polymer B is present between the induction hole 2 and the introduction hole 4. Therefore, when the low-viscosity polymer flow is joined with the high-viscosity polymer flow, the flow velocity of the low-viscosity polymer flow becomes sufficiently low, and as shown in Fig. 9(c), the velocity distribution in the cross-sectional direction of the composite polymer flow can be made close to symmetrical at the bottom of the introduction hole 4 (symbol "V4" in Fig. 9(c)), and the discharge bending phenomenon of the polymer flow G discharged from the spinneret discharge hole 8 can be suppressed.

[0018] Furthermore, Patent Document 7 proposes a composite nozzle that suppresses discharge bending by controlling the composite cross section.

[0019] The composite spinneret described in Patent Document 7 is explained with reference to Fig. 10(b). In the composite spinneret described in Patent Document 7, a polymer flow of high-viscosity polymer A (high-viscosity polymer flow) introduced through induction hole 1 and a polymer flow of low-viscosity polymer B (low-viscosity polymer flow) introduced through induction hole 2 are joined at induction hole 4, and the joined polymer flow is caused to flow down into induction hole 7, while a low-viscosity polymer flow that has entered another induction hole 3 is introduced into the introduction hole 7 via a flow path 6. By causing the joined polymer flow to flow down into the spinneret discharge hole 8 while covering the periphery with the low-viscosity polymer flow introduced from the other induction hole 3, it is possible to obtain an eccentric core-sheath cross section in which the first component polymer A is surrounded by the second component polymer B as shown in Fig. 10(a). As a result, the resistance received from the wall surface of the introduction hole 7 of each polymer stream becomes constant, and the velocity distribution in the cross-sectional direction of the composite polymer stream when the first component polymer A is a high-viscosity polymer and the second component polymer B is a low-viscosity polymer becomes three peaks as shown in FIG. 10(c) (symbol "V5" in FIG. 10(c)). However, since the radial velocity distribution in the introduction hole 7 can be made close to symmetrical, the curvature of the polymer stream G discharged from the nozzle outlet 8 toward the high-viscosity polymer side is reduced, and the discharge bending phenomenon can be suppressed. In addition, it is generally known that if the entire circumference of the side-by-side cross section is coated, the distance between the centers of gravity of each polymer on the composite cross section is shortened, thereby suppressing the curvature toward the high-shrinkage component side during heat treatment and reducing the crimping expression, but it is proposed that the composite spinneret of Patent Document 7 can make the coated portion a thin skin by adjusting and controlling the pressure applied to the induction hole 2 and the induction hole 3 for the low-viscosity polymer stream introduced to the induction hole 3, and can maintain the same crimping property as the side-by-side cross section. [Prior art documents] [Patent documents]

[0020] [Patent Document 1] Japan Special Publication No. 44-2504 [Patent Document 2] Japanese Patent Publication No. 2005-113369 [Patent Document 3] Japanese Patent Publication No. 2000-256918 [Patent Document 4] International Publication No. 2002 / 086211 [Patent Document 5] Japanese Patent Application Publication No. 2017-172080 [Patent Document 6] Japanese Patent Publication No. 2-307905 [Patent Document 7] Japan Special Publication No. 55-27175 Summary of the Invention [Problem to be solved by the invention]

[0021] In the case of the side-by-side type composite fibers proposed in Patent Documents 1 and 2, which simply exhibit crimps of approximately the same size, when a load is applied to the fibers or fabric, the fibers do not become entangled, and each individual fiber ultimately bears the stress, resulting in a material that stretches well with a relatively small force. As a result, the objective of the present invention, an appropriate sense of hold, is not obtained, and it is difficult to achieve a material with excellent movement tracking properties.

[0022] In addition, in Patent Document 3, the behavior of the stretching of the crimped structure is similar to that of Patent Documents 1 and 2, and in addition to making it difficult to obtain an adequate feeling of hold, when the crimped structure is fully stretched, resistance is applied due to the elastic properties of the polymer. Depending on the structure of the fabric and the part used, the resistance may be excessive, and a feeling of tightness may be felt.

[0023] In Patent Document 4, the apparent crimp is imparted by false twisting, and large and small crimps of different sizes are mixed in the multifilament, resulting in a wide distribution of coil pitch and coil diameter between fibers. In such a state, the fibers with a large coil diameter are slackly fixed on the multifilament. Since the slackened fibers do not contribute to the stretching and shrinking of the multifilament and the associated resistance, the resistance during stretching may decrease. Furthermore, since it is a false twisted yarn of a side-by-side type composite fiber, if the false twisting process in which the multifilament is twisted while being heated is performed under unreasonable conditions, peeling between polymers may occur due to friction or impact during processing or use, and there may be problems such as whitening when made into a fabric. For this reason, the use may be limited in sportswear and outdoor clothing applications that require high abrasion resistance because they are used in harsh environments.

[0024] In Patent Document 5, the converging portion that bears the resistance force during yarn elongation forms one large spiral structure regardless of the crimp form of the fiber, so that the spiral structure cannot be formed well under the constraint of the fabric structure, and the fabric lacks a resilience during elongation. Furthermore, when focusing on the non-converging portion, the difference in crimp form between the constituent fibers is large, so that the same type of fiber is unevenly distributed in the cross section of the multifilament, and the crimps of the same size may be bitten into each other, resulting in the crimp phase of multiple fibers being aligned. In this case, the fibers on the low crimp side are present floating on the surface of the multifilament, and the surface of the fabric may have a rough texture that feels unnecessarily uneven.

[0025] Further, a common feature of conventional composite spinnerets used in spinning latent crimp-producing fibers is that they have a flow path between the induction hole and the introduction hole. This flow path is a groove flow path arranged perpendicular to the induction hole and the introduction hole, and at least one of the polymer flows passes through the flow path and is joined to the other polymer just before the introduction hole. At this time, since the polymer flows collide in the perpendicular direction, there are problems such as changes in the composite cross section due to minute changes in the flow rate of the polymer flows and abnormal retention during long-term spinning, which may lead to problems in spinning stability such as sudden deterioration in crimping and yarn breakage due to discharge bending.

[0026] In addition, by not providing a flow path between the induction hole and the introduction hole, it is possible to improve the dimensional stability of the composite cross section and suppress abnormal retention, but then the flow rate cannot be controlled through a flow path, and the asymmetry of the velocity distribution at the introduction hole increases, which can sometimes lead to a worsening of the discharge bending phenomenon.

[0027] In addition, the composite spinneret described in Patent Document 7 can form a composite cross section with a thin coating, so that it is possible to suppress discharge bending even with a sudden change in viscosity, but since there is a flow path between the induction hole and the introduction hole, the dimensional stability of the composite cross section is not guaranteed. In addition, in order to form a coating, it is necessary to form a pool of low-viscosity polymer flow introduced from another induction hole 3 in the flow path 6 and to flow the joining polymer flow from the introduction hole 4 down there, but in order to form a thin coating, the low-viscosity polymer flow introduced from the other induction hole 3 must be extremely small, and by making the polymer flow extremely small, it is inevitable that abnormal retention will occur in the polymer pool in the flow path 6, which may cause problems in spinning stability.

[0028] Furthermore, in the technology of Patent Document 7, the polymer flow is merged twice in the spinneret flow path, so the processing area in the spinneret needs to be large, and as a result, the number of fibers (number of filaments) that can be obtained from one composite spinneret is limited. This significantly reduces productivity and sometimes limits the expansion to a wide variety of products.

[0029] As described above, a composite spinneret capable of stably discharging fibers over a wide range of conditions is an extremely important element in producing fibers with potential for crimp development. However, as described above, there are problems associated with such a composite spinneret, and a need has arisen for a composite spinneret for fibers with potential for crimp development that can solve these problems.

[0030] That is, the present invention aims to overcome the problems of the prior art and provide a stretch-processed yarn capable of imparting good stretchability to clothing, a textile product containing the stretch-processed yarn, a composite spinneret for producing the stretch-processed yarn, and a method for producing a composite fiber. Specifically, the present invention aims to form a composite cross section capable of significantly suppressing the extrusion bending phenomenon while maintaining the same crimp expression as a conventional side-by-side cross section (see FIG. 8(a)) in a stretch-processed yarn that can be made into a textile material having good stretchability, movement followability due to appropriate resistance when stretched, and a soft surface feel according to the crimp morphology by precisely controlling and improving the crimp morphology of the fibers constituting the crimped yarn, and a composite spinneret for producing the stretch-processed yarn, and further to provide a composite spinneret that can maintain high dimensional stability of the composite cross section regardless of the extrusion range, thereby enabling stable extrusion over a wide range of conditions. [Means for solving the problem]

[0031] The above object can be achieved by any one of the following means (1) to (8). (1) A stretch-processed yarn comprising a multifilament made of fibers having a coil-shaped crimped form in the fiber axis direction, the coil diameter distribution of the crimp in the fibers having two or more groups, the ratio of the maximum group average value of the coil diameter to the minimum group average value (maximum group average value / minimum group average value) being less than 3.00, and the cross section of the fibers constituting the multifilament being an eccentric core-sheath cross section. (2) The stretch-processed yarn according to (1) above, in which the number of fibers included in the group with the smallest group average value of the coil diameter is 20% or more of the total number of fibers constituting the multifilament. (3) The stretch-processed yarn according to (1) or (2), wherein the average diameter of the fibers constituting the multifilament is 15 μm or less. (4) The stretch - textured yarn according to any one of (1) to (3) above, wherein the elongation energy is 1.5 μJ / dtex or more. (5) A fiber product containing at least a part of the stretch - textured yarn according to any one of (1) to (4) above. (6) A composite spinneret for discharging a composite polymer stream composed of a first - component polymer and a second - component polymer, the composite spinneret comprising a metering plate having a plurality of metering holes for metering each polymer component, one or more distribution plates having distribution holes for distributing each polymer component, and a discharge plate. In the lowermost layer on the downstream side in the polymer spinning path direction of the distribution plate, a polymer distribution hole group is formed in which a plurality of first - component polymer distribution holes arranged in a semicircular array are surrounded by a plurality of second - component polymer distribution holes, and at least a part of the second - component polymer distribution holes in the polymer distribution hole group is arranged in a semi - circumferential array outside the circumferential part of the plurality of first - component polymer distribution holes arranged in a semicircular array. (7) The composite spinneret according to (6) above, wherein the total number of holes Ht of the second - component polymer distribution holes in the polymer distribution hole group and the number of holes Ho of the second - component polymer distribution holes arranged in a semi - circumferential array outside the circumferential part of the plurality of first - component polymer distribution holes arranged in a semicircular array satisfy the following formula (1). 1 / 16 < Ho / Ht < 1 / 4 ··· Formula (1) (8) A method for producing composite fibers using the composite spinneret according to (6) or (7) above. [Advantages of the Invention]

[0032] The stretch - textured yarn of the present invention has a mixture of a plurality of groups of coiled crimps with controlled coil diameters in the multifilament, and exhibits an appropriate elongation resistance from the initial stage of elongation according to the size of the coil diameter. When made into a woven or knitted fabric, it has good elongation deformation while having an appropriate hold property. Therefore, it can be used as a stretch material that exhibits stress - free motion followability, and is expected to be applied to fiber products for a wide range of uses, from sports apparel to industrial materials such as sanitary materials.

[0033] Furthermore, the composite spinneret used in producing the stretched yarn of the present invention can form a composite cross section that can significantly suppress the extrusion bending phenomenon while maintaining the same crimp development as conventional latent crimp developing fibers, and can maintain the dimensional stability of the composite cross section at a high level regardless of the viscosity of the polymer to be combined or the extrusion range, thereby making it possible to produce composite fibers that have excellent stretchability stably over a wide range of conditions. [Brief description of the drawings]

[0034] [Figure 1] FIG. 1 is a diagram showing an example of a fiber constituting a stretch processed yarn of the present invention, and is a diagram showing an observed crimp form for explaining the coil diameter in the crimp form. [Diagram 2] FIG. 2 is a diagram showing an example of the distribution of coil diameters of the fibers constituting the stretch textured yarn of the present invention. [Diagram 3] FIG. 3 is a diagram showing the relationship between the elongation deformation profile of the stretch textured yarn of the present invention and that of a conventional stretch yarn. [Figure 4] FIG. 4 is a diagram for explaining the elongation energy using an example of the elongation deformation profile of the stretch textured yarn of the present invention. [Diagram 5] FIG. 5 is a diagram showing an example of the fiber diameter distribution of the fibers constituting the stretch textured yarn of the present invention. [Figure 6] 6(a) and 6(b) are cross-sectional views of a fiber for explaining the cross-sectional parameters of a composite fiber having a thin-skin eccentric core-sheath structure of the present invention. [Figure 7] FIG. 7 is a schematic diagram of the arrangement of discharge holes in the discharge plate of the die used in Example 10. [Figure 8] 8(a) to 8(c) are diagrams relating to a conventional latent crimp developable fiber, in which FIG. 8(a) is a morphology diagram of a side-by-side cross section, which is a composite cross section, of a conventional latent crimp developable fiber, FIG. 8(b) is a schematic diagram of a general composite spinneret used in spinning the latent crimp developable fiber having the side-by-side cross section of FIG. 8(a), and FIG. 8(c) is a radial velocity distribution diagram within an introduction hole where the respective polymer streams flowing within the composite spinneret of FIG. 8(b) join together. [Figure 9] 9(a) to 9(c) are diagrams relating to the composite spinneret of Patent Document 6, in which FIG. 9(a) is a schematic diagram of the composite spinneret used in an embodiment of Patent Document 6, FIG. 9(b) is a cross-sectional view taken along line I-I' of FIG. 9(a), and FIG. 9(c) is a radial velocity distribution diagram within an introduction hole where the respective polymer streams flowing within the composite spinneret of FIG. 9(a) join together. [Figure 10] Figures 10(a) to 10(c) are diagrams relating to the composite spinneret of Patent Document 7, where Figure 10(a) is a morphology diagram of an eccentric core-sheath cross section, which is the composite cross section of the composite fiber of Patent Document 7, Figure 10(b) is a schematic diagram of a composite spinneret used to prevent the composite fiber of Patent Document 7, and Figure 10(c) is a radial velocity distribution diagram within an introduction hole where the respective polymer streams flowing within the composite spinneret of Figure 10(b) join together. [Figure 11] Figures 11(a) and 11(b) are views relating to a distribution plate used in an embodiment of the present invention, where Figure 11(a) is a schematic plan view of a group of polymer distribution holes formed in the lowermost layer on the downstream side in the polymer spinning path direction of the distribution plate, and Figure 11(b) is a diagram of the composite cross-sectional shape of a composite fiber obtained from a composite spinneret using the distribution plate of Figure 11(a). [Figure 12] Figures 12(a) to 12(c) are diagrams for explaining the manufacturing method of the composite fiber of the present invention, and are one example of the configuration of a composite spinneret, where Figure 12(a) is a cross-sectional front view of the main parts that make up the composite spinneret, Figure 12(b) is a cross-sectional front view of a part of the distribution plate, and Figure 12(c) is a cross-sectional front view of the discharge plate. [Figure 13] FIG. 13 is a schematic partial cross-sectional view of a distribution plate used in an embodiment of the present invention. [Figure 14] Figures 14(a) and 14(b) are views relating to a conventional distribution plate different from that of the present invention, where Figure 14(a) is a schematic plan view of a group of polymer distribution holes formed in the lowermost layer on the downstream side in the polymer spinning path direction of the distribution plate, and Figure 14(b) is a diagram of the composite cross-sectional shape of a composite fiber obtained from a composite spinneret using the distribution plate of Figure 14(a). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] The present invention will be described in detail below together with preferred embodiments. In this invention, the term "stretchable yarn" refers to a processed yarn that has the property of stretching or shrinking when subjected to elongation deformation, and this stretchable yarn is made of a multifilament made of fibers having a coil-shaped crimped form in the fiber axis direction, and the first requirement of the present invention is that the coil diameter distribution of the crimp in the fiber has two or more groups.

[0036] The coil diameter of the coiled crimp referred to here is one of the indices showing the crimp size of the fibers constituting the stretch processed yarn, and when the fibers separated from the multifilament are observed two-dimensionally from the side (perpendicular to the fiber axis direction), peaks and valleys are observed alternately in the fiber width direction as shown in Fig. 1, and the coil diameter of the present invention can be measured from this observation image. The coil diameter of the crimp referred to in the present invention will be described in more detail using an example (Fig. 1) of the fibers constituting the stretch processed yarn of the present invention photographed by the above-mentioned method.

[0037] First, the multifilament sample to be evaluated is cut into a 10 m skein using a measuring machine or the like, and immersed in boiling water at 98 ° C or higher with a load of 0.2 mg / d for 15 minutes. After thoroughly drying the boiled water-treated multifilament sample by air drying, a load of 1 mg / d is applied for 30 seconds or more, and then marking is performed at any point on the multifilament so that the distance between two points is 3 cm. Then, fibers are separated from the multifilament without plastic deformation, and the distance between the pre-applied markings is adjusted to the original 3 cm, and the sample is fixed on a slide glass, and an image is taken with a digital microscope or the like at a magnification where 5 to 10 crimp peaks can be observed. In each captured image (Fig. 1), if the apexes of any adjacent peaks are M1 and M2, and the apex of the valley between the peaks M1 and M2 is V1, the shortest distance between the line connecting the peaks M1 and M2 and the apex of the valley V1 is the crimped coil diameter (Dc) referred to in the present invention. This crimped coil diameter Dc is measured in units of µm to one decimal place.

[0038] The same operation is randomly performed on different fibers constituting the multifilament, and the coil diameter is measured so that the total number of data is 100 by repeating this process. The measured coil diameters are divided into classes with a width of 10 μm, with the boundary value set at 10×n (n: natural number) μm, and the vertical axis is a histogram of frequency. When the measured coil diameters have two or more groups (peaks) as illustrated in Figure 2, this means that the "coil diameter distribution of crimp has two or more groups" as referred to in the present invention. The group referred to here means a case where either (1) or (2) below is satisfied, and Figure 2 illustrates the coil diameter measurement results of a stretch-processed yarn having two groups (black colored parts) shown in 2-(a) and 2-(b). (1) When there are two or more consecutive classes with a frequency of 5% or more, all the relevant classes are considered to be one group (example shown in Figure 2, 2-(a)). (2) When the frequency of a class exceeds 10% and the frequency of both the adjacent classes is less than 5%, the classes with a frequency of 10% or more are grouped together (see 2-(b) in Figure 2).

[0039] A textured yarn having a coil diameter distribution as shown in FIG. 2 means that the multifilament is composed of two or more types of fiber groups with a clear difference in crimp size (average coil diameter). In the case of textured yarn having crimp, the crimped coil expands and contracts to generate resistance (stress) during elongation deformation, and in the case of a multifilament composed of only one type of coil diameter, the fibers constituting the multifilament are uniformly deformed, resulting in a monotonous profile as shown by dotted line 3-(a) in FIG. 3, in which stress (resistance) is not generated until the crimp is fully extended. On the other hand, when two or more types of fibers with different coil diameters are present in the multifilament, the fibers with different sizes deform in a graded manner according to the elongation of the textured yarn. That is, in the low elongation region, the fibers with small coil diameters deform, and then in the high elongation region, the fibers with large coil diameters deform, resulting in a specific deformation profile in which stress is generated from low elongation as shown by solid line 3-(b) in FIG. 3.

[0040] This is an important characteristic that characterizes the stretched textured yarn of the present invention, and since the stress gradually increases from this low elongation and a moderate resistance force is expressed according to the elongation deformation, when worn as clothing, a good hold is created. In addition, in actual textured yarn, the multifilament is formed in a state in which the fibers with a small coil diameter are partially entangled with the fibers with a large coil diameter. Therefore, the multifilament itself is integrated without being separated, and is easy to handle, and the fibers with a large coil diameter partially follow the elongation deformation of the fibers with a small coil diameter, so that the multifilament as a whole has good elongation deformation.

[0041] This effect can be evaluated by the extension energy seen in the tensile properties. First, stretch-processed yarn that has not been subjected to heat treatment is left unloaded for 24 hours at a temperature of 20±2°C and a relative humidity of 65±2%. After 24 hours of leaving, a load of 1 mg / d is applied to the yarn sample, and after 30 seconds or more have elapsed, the sample is fixed to a tensile tester (such as TENSILON UCT-100 manufactured by Orientec Co., Ltd.) with the initial sample length set to 50 mm while still under load. A tensile test is carried out on the yarn sample at a tensile speed of 50 mm / min, and an elongation-stress curve is created with the horizontal axis representing elongation (unit: mm) and the vertical axis representing stress (unit: cN / dtex) as shown in FIG. 4. In the obtained elongation-stress curve, the point where the strength is 0.05 cN / dtex is 4-(a), and the point where a perpendicular line is dropped from point 4-(a) to the horizontal axis (stress 0 cN / tex) and intersects with the horizontal axis is 4-(b), the area Ae surrounded by points 4-(a), 4-(b), and the origin represents the elongation energy, which can be calculated in units of μJ / dtex. The same operation was performed on 10 different yarn samples, and the simple number average was calculated, and the value rounded off to one decimal place is the elongation energy referred to in the present invention.

[0042] The term "extension energy" refers to the amount of energy required for a material to undergo elongation deformation, and when the yarn's elongation-stress curve has a monotonous profile, as shown by the dotted line 3-(a) in Figure 3, the elongation energy is low, meaning that the material deforms without resistance at low elongation deformations caused by normal human movements, resulting in a difference between the deformation of the fabric and human movement. On the other hand, in the case of multifilament yarns, which have high elongation energy as shown by the solid line 3-(b) in Figure 3, resistance appears at low elongation deformations, and the material deforms while fitting the human movement, making it possible to provide a comfortable hold and good movement tracking ability.

[0043] In order to obtain a fabric that has the above-mentioned good movement-following property, the elongation energy measured by the above-mentioned method is preferably 1.5 μJ / dtex or more. This range means that the fabric exhibits an elongation resistance suitable for following human movement even at low elongation deformation, and even when worn for a long time with gentle movements such as hiking or when moving the body widely such as stretching exercise, the garment stretches while holding the body comfortably, making it a comfortable stretch garment that does not cause stress. In addition, in order to apply the fabric to sports clothing applications such as track and field events that require relatively agile movements or large instantaneous movements, a more preferable range of elongation energy is 2.5 μJ / dtex or more. According to this concept, it can be said that the higher the elongation energy, the better the holding feeling and the better the movement tracking ability; however, increasing it too much can hinder body movement and the excessive holding feeling can be stressful as it is too tight, so the upper limit that substantially achieves the object of the present invention is 10.0 μJ / dtex or less, and a range of 2.5 to 10.0 μJ / dtex for the elongation energy can be cited as a particularly preferred range.

[0044] In order to achieve the above-mentioned elongation deformation of the multifilament, it is very important that the correlation between groups in the coil diameter distribution is within an appropriate range as in the present invention, and this results in the specific deformation profile of the present invention. That is, in the stretch textured yarn of the present invention, control of the coil diameter difference between the fibers constituting the multifilament is an important requirement, and specifically, it is necessary that the ratio of the maximum group average value of the coil diameter to the minimum group average value (maximum group average value / minimum group average value) is less than 3.00.

[0045] The group average value of coil diameter in the present invention means a value obtained by classifying groups based on the coil diameter distribution of the multifilament measured by the above-mentioned method, calculating the number average of the coil diameters contained in each group, and rounding off the value to the third decimal place. When comparing the group average values ​​calculated by the above-mentioned method among groups of coil diameter distribution, the largest group average value is the largest group average value, and the smallest group average value is the smallest group average value. The value obtained by dividing the smallest group average value by the largest group average value and rounding off the value to the second decimal place is the ratio of the largest group average value to the smallest group average value. The larger this value is, the greater the deviation in coil diameter between the fibers constituting the stretch textured yarn.

[0046] In the stretch-processed yarn of the present invention, in order to prevent the elongation-stress curve of the multifilament from undergoing stepwise deformation and to obtain good elongation energy, a more preferable range for the ratio of the maximum group average value to the minimum group average value is 1.50 to 2.50.

[0047] Furthermore, in order to make the above-mentioned effects of the present invention more remarkable, it is preferable that the number of fibers included in the group with the smallest group average value of the coil diameter is 20% or more of the total number of fibers constituting the multifilament. In this range, the stress in the low elongation region is improved in the elongation-stress curve of the multifilament, and since the stress is well expressed from the low elongation region, the elongation energy is increased, and the holding feeling when making small movements, which is a characteristic of the stretch textured yarn of the present invention, can be preferably expressed. As the number of fibers included in the group with the smallest group average value of the coil diameter increases, there is an effect of improving the holding feeling at low elongation, and as a suitable range for application as a full-fledged sportswear, the number of yarns included in the group with the smallest group average value can be 40% or more, which can be cited as a more preferable range of the present invention. Although there is no particular upper limit on the number of fibers included in the group with the smallest group average value of coil diameter, it is preferable that a certain proportion of fibers with large coil diameters are also present in order for fibers of different sizes to deform gradually in response to the elongation of the processed yarn, which is the purpose of the present invention. From this perspective, it is preferable that the number of yarns included in the group with the smallest group average value be 90% or less of the total number of fibers, and more preferably 80% or less.

[0048] In order to improve the adhesion of clothing made of the stretch processed yarn of the present invention to human skin, innerwear, etc., it is effective to increase the surface area in contact with the object, and it is preferable to reduce the fiber diameter of the fibers in the multifilament, and in the present invention, it is preferable that the average fiber diameter is 15 μm or less. If it is within this range, in addition to appropriate holding power, the fabric will be able to follow the stretch of the skin, greatly suppressing friction between the clothing and the skin, resulting in a comfortable stretch material that exhibits stress-free movement following ability.

[0049] The average fiber diameter in the present invention can be determined as follows. First, the stretch processed yarn is embedded in an embedding agent such as epoxy resin while remaining as a multifilament, and images of all fibers are taken of the cross section at a magnification such that 10 or more fibers can be observed using a scanning electron microscope (SEM). For each image taken, the cross-sectional area Af of the fiber is measured using image analysis software (for example, "WinROOF2015" manufactured by Mitani Shoji Co., Ltd.), and the diameter of a perfect circle having the same area as this cross-sectional area Af is calculated. This is measured for all fibers constituting the multifilament, and a simple number average is calculated. The unit is μm, and the value rounded off to one decimal place is the average diameter of the fiber referred to in the present invention.

[0050] If we push the above idea forward, when the total fineness of the multifilament is the same, the smaller the average diameter of the fibers, the larger the surface area, so the more preferable range of the average diameter of the fibers is 12 μm or less. Furthermore, as the average diameter of the fibers becomes smaller, the adhesion when made into a fabric decreases, and the rigidity of the fibers decreases, so a soft touch that is essential for comfortable wear is obtained. For this reason, in order to make a fabric applicable to innerwear that directly touches the skin and sports underwear that requires high movement tracking, it is particularly preferable to make the average diameter of the fibers 10 μm or less.

[0051] The stretch-processed yarn of the present invention has excellent movement-following properties when made into a fabric, and can naturally be used in sports and outdoor applications that are used in harsh environments, so it is necessary for the fiber cross-section to be an eccentric core-sheath cross-section that has excellent abrasion resistance.

[0052] The eccentric sheath-core cross section referred to in the present invention means that in a fiber cross section made of two or more different polymers, as shown in Fig. 6(a), the sheath component polymer B completely covers the core component polymer A, and the center of gravity a of the core component is different from the center point c of the fiber cross section. Fig. 6(a) shows an example of a cross section of a composite fiber having such an eccentric sheath-core cross section, in which the horizontal hunting is the sheath component (polymer B), the 30 deg hunting (diagonal line rising to the right) is the core component (polymer A), the center of gravity of the core component in the fiber cross section is the center of gravity a, and the center of the fiber cross section is the center point c.

[0053] In such an eccentric core-sheath cross section, the sheath component completely covers the core component, thereby preventing peeling between the core component and the sheath component (hereinafter also referred to as "core-sheath component"). Therefore, even if the fibers or fabric are subjected to friction or impact, whitening or pilling does not occur, and the quality of the fabric can be maintained.

[0054] However, in the eccentric core-sheath cross section of the conventional technology as exemplified in Figure 14(b), the thickness of the sheath component A is locally thin. Therefore, when friction or impact is applied to the fiber, stress is concentrated in the part where the sheath component A is thin, and peeling may occur between the core and sheath components starting from this part.

[0055] Furthermore, if the thickness of the sheath component is set to be thick in order to avoid this, the distance between the center of gravity a of the core component and the center of the fiber cross section c (center-to-center distance) will become closer, which may weaken the expression of fiber crimp. That is, in composite fibers with an eccentric core-sheath cross section, a difference in shrinkage between the core component and the sheath component occurs due to heat treatment, etc., and the fiber is greatly curved, resulting in the expression of three-dimensional coil-like crimp, but if the center-to-center distance is close, the moment that curves the fiber is small, so the fiber crimp becomes coarse and the stretchability is impaired.

[0056] For this reason, in the stretch textured yarn of the present invention, it is preferable that a part of the sheath component in the cross section of the fiber is a uniform thin skin, that is, a thin-skin eccentric core-sheath cross section, as exemplified in FIG. 6(b). The characteristic sheath component arrangement in the fiber cross section as described above makes it possible to disperse the stress acting between the core and sheath components and ensure a large distance between the centers of gravity, which is important for crimp properties.

[0057] The thin-skin eccentric sheath-core cross section referred to here means an eccentric sheath-core cross section that satisfies the following requirements. (A) The ratio S / D of the minimum thickness S of the component covering the core component to the fiber diameter D of the fiber is 0.01 to 0.10. (B) The portion of the perimeter whose thickness is within 1.05 times the minimum thickness S (S ratio) accounts for 30% or more of the total perimeter of the fiber cross section.

[0058] The minimum thickness S of the sheath component referred to here is found as follows, and will be explained using Fig. 6(b). Fig. 6(b) shows an example of a cross-sectional view of a composite fiber having a thin-skinned eccentric core-sheath cross section, in which the horizontal haunch is the sheath component, the 30 deg haunch is the core component, S is the minimum thickness of the sheath component, and D is the fiber diameter. First, the stretched yarn is embedded in an embedding agent such as epoxy resin as a multifilament, and an image of the cross section is taken with a transmission electron microscope (TEM) at a magnification where 10 or more fibers can be observed. In this case, if metal dyeing is applied, the dyeing difference between the polymers can be utilized to clarify the contrast of the joint between the core component and the sheath component. The fiber diameter of 10 fibers randomly selected from each of the images taken and measured by the above-mentioned method corresponds to the fiber diameter D of the fiber referred to in the present invention. Here, if it is impossible to observe 10 or more fibers, it is sufficient to observe a total of 10 or more fibers including other fibers.

[0059] Furthermore, the minimum thickness of the sheath component covering the core component is measured for 10 or more fibers using the images in which the fiber diameter D of the fibers is measured, and this value corresponds to the minimum thickness S referred to in the present invention. Furthermore, the fiber diameter D and minimum thickness S of these fibers are measured in units of μm, and S / D is calculated. The above operation is carried out on 10 images, and a simple number average value is calculated and rounded off to two decimal places to obtain a value.

[0060] The stretch-processed yarn of the present invention has a fiber cross-section with a thin skin eccentric core-sheath cross-section as described above, which allows the stress applied between the core-sheath components to be distributed while still providing good stretchability, thereby achieving good abrasion resistance.

[0061] Here, the abrasion resistance referred to in the present invention can be evaluated, for example, by the Martindale method shown in JIS L1096 (2010). In this measurement method, an abrasion test is performed on a fabric sample woven and dyed from the target fiber and a standard abraded fabric, and the discoloration of the fabric sample is evaluated every 100 abrasions, and the abrasion resistance is evaluated based on the number of abrasions at which the degree of discoloration is equivalent to the standard scale. In the stretch-processed yarn of the present invention, a preferable range of abrasion resistance is 2000 times or more. In particular, when used in harsh environments such as sports and outdoor applications, abrasion resistance of 2500 times or more is more preferable, and abrasion resistance of 3000 times or more is particularly preferable.

[0062] Considering the processability in advanced processing and the practical use after processing into a fabric, it is preferable that the stretch-processed yarn of the present invention has a certain level of toughness or higher, and it is preferable that the strength and elongation at break of the fiber be as follows. In the present invention, the strength is the value obtained by dividing the load value at break by the initial fineness when the load-elongation curve of the fiber is obtained under the conditions specified in JIS L1013 (2010), and the elongation is the value obtained by dividing the elongation at break by the initial sample length. Here, the initial fineness means the value calculated as the weight per 10,000 m from the simple average value obtained by measuring the weight of a unit length of the fiber multiple times.

[0063] The strength and elongation referred to here are preferably adjusted by controlling the conditions of the manufacturing process described below depending on the intended use, etc., but as a guideline for the stretch-processed yarn of the present invention, preferred ranges can be mentioned as a strength of 0.5 to 10.0 cN / dtex and an elongation of 5 to 700%. When the stretch processed yarn of the present invention is used for general clothing applications such as innerwear and outerwear, the strength is preferably 1.0 to 4.0 cN / dtex and the elongation is preferably 20 to 40%. For sports clothing applications in harsh environments, the strength is preferably 3.0 to 5.0 cN / dtex and the elongation is preferably 10 to 40%.

[0064] In addition, the stretch textured yarn of the present invention preferably has a Uster unevenness U%, which is an index of fiber diameter unevenness in the longitudinal direction of the fiber, i.e., fineness unevenness, of 1.5% or less. This not only prevents dyeing unevenness in the fabric, but also prevents deterioration of the fabric quality due to shrinkage unevenness, and allows good fabric quality to be obtained. The Uster unevenness U% is more preferably 1.0% or less.

[0065] The stretch processed yarn of the present invention can be made into various textile products as intermediates such as fiber winding packages, tows, cut fibers, cotton, fiber balls, cords, piles, woven and knitted fabrics, nonwoven fabrics, etc. The textile products referred to here can be used for everyday clothing such as jackets, skirts, pants, underwear, sports clothing, clothing materials, interior products such as carpets, sofas, curtains, automotive interior products such as car seats, cosmetics, cosmetic masks, wiping cloths, health products, etc., and environmental and industrial material applications such as polishing cloths, filters, harmful substance removal products, and battery separators.

[0066] Next, a preferred method for producing the stretch textured yarn of the present invention will be described. In order to produce the stretch-processed yarn of the present invention, it is necessary that the multifilament made of composite fiber having an eccentric core-sheath cross section has two or more groups in the coil diameter distribution of the crimp, and that the deviation of the group average value of each group is controlled within a specific range.

[0067] As a method for producing a composite fiber having an eccentric core-sheath cross section, composite spinning using a composite spinneret of a distribution system as described in the specifications of Japanese Patent No. 5,505,030 and Japanese Patent No. 5,703,785 is suitably used.

[0068] 12(a) to 12(c) are schematic cross-sectional views of a composite spinneret preferably used in the present invention. It should be noted that, since Figures 12(a) to 12(c) are front cross-sectional views, only two discharge hole groups each consisting of a group of first component polymer discharge holes and second component polymer discharge holes are shown, but the number of discharge hole groups in the practice of the present invention is not limited.

[0069] The composite spinneret used in the present invention is a composite spinneret for discharging a composite polymer stream composed of a first component polymer and a second component polymer, and as shown in FIG. 12(a), is composed of a metering plate 14 having a plurality of metering holes for metering each polymer component, one or more distributor plates 15 having distribution holes 18 for distributing each polymer component, and a discharge plate 16. The composite spinneret shown in FIG. 12(a) further includes a distributor plate 15 having a distribution groove 17 formed therein as the distributor plate 15. Each distributor plate 15 is preferably composed of a thin plate. In FIG. 12(a), two distributor plates 15 are used. The metering plate 14 and the distributor plate 15, and the distributor plate 15 and the discharge plate 16 are positioned by positioning pins so that the centers (cores) of the spin packs are aligned, and after stacking, they may be fixed with screws or bolts, or may be metal-bonded (diffusion-bonded) by thermocompression. In particular, since the distribution plates 15 are made of thin plates, it is preferable that the distribution plates 15 are metallically bonded (diffusion bonded) to each other by thermocompression bonding.

[0070] The component polymers supplied from the metering plate 14 pass through the distribution grooves 17 and distribution holes 18 of at least one laminated distributor plate 15, and then join together to form a composite polymer stream. The composite polymer stream then passes through the discharge introduction hole 19 and reduction hole 20 of the discharge plate 16, and is discharged from the nozzle hole 21.

[0071] Although not shown in the figure to avoid complicating the explanation of the composite spinneret, the members stacked on the upstream side of the metering plate 14 opposite the distribution plate 15 side may be members with flow paths formed in accordance with the spinning machine and spinning pack. Incidentally, by designing the metering plate 14 to match existing flow path members, it is possible to utilize the existing spinning pack and its members as they are. Therefore, there is no need to exclusively use a spinning machine for the composite spinneret.

[0072] It is also preferable to stack a plurality of flow path plates (not shown) between the flow path and the metering plate 14 or between the metering plate 14 and the distribution plate 15. This is intended to provide a flow path through which the polymer is efficiently transported in the cross-sectional direction of the spinneret and the cross-sectional direction of the fiber, and to configure the polymer to be introduced into the distribution plate 15. The composite polymer stream discharged from the discharge plate 16 is cooled and solidified, and then an oil is added thereto, and the composite fiber of the present invention is produced by being taken up by rollers having a specified peripheral speed, according to a conventional melt spinning method.

[0073] Here, the principle of being able to express a high level of crimp in the composite fiber while significantly suppressing the phenomenon of discharge bending, which is a fundamental problem in the production methods of the prior art, which is an important point for achieving the object of the present invention, will be described below.

[0074] In order to suppress the discharge bending phenomenon by using a composite cross section, it is most effective to shorten the distance between the centers of gravity of each polymer on the composite cross section and reduce the asymmetry of the velocity distribution in the cross-sectional direction of the composite polymer flow. However, if the distance between the centers of gravity of the components is short, even if a shrinkage treatment such as heating is performed, the curvature of the fiber toward the high shrinkage component side becomes small, and only gentle crimping occurs. In other words, in the case of the conventional technology, it is not possible to suppress the discharge bending and to generate a high degree of crimp at the same time, and there is a trade-off between the discharge bending and the generation of crimping.

[0075] As an effective countermeasure, for example, forming an eccentric core-sheath cross section coated with a thin skin on a side-by-side cross section, as proposed in Patent Document 7, is considered. However, with the conventional composite spinneret as shown in Figures 10(b) and 10(c), it is difficult to precisely control the flow of the extremely small amount of polymer required to stably form an ideal thin film portion, and to form a stable flow over time without causing abnormal retention, and there are virtually few cases in which this method has been adopted as a manufacturing method for potentially crimp-developing fibers. For this reason, a side-by-side cross section has mainly been adopted for spinning potentially crimp-developing fibers, and production has been forced to be carried out under restrictions on discharge conditions such as the single-hole discharge amount, which affects the viscosity of the applied polymer and the single fiber fineness.

[0076] As a result of extensive investigations into the above-mentioned problems, the present inventors have found that, as in the present invention, a polymer distribution hole group, in which a plurality of first component polymer distribution holes arranged in a semicircular shape are surrounded by a plurality of second component polymer distribution holes, is provided in the lowermost layer on the downstream side of the distribution plate 15 in the polymer spinning path direction, and at least a part of the second component polymer distribution holes in the polymer distribution hole group are arranged in a semicircular shape outside the circumferential part of the plurality of first component polymer distribution holes arranged in a semicircular shape, thereby making it possible to eliminate the above-mentioned trade-off relationship between discharge bending and crimp occurrence.

[0077] In the present invention, the "direction of the polymer discharge path" refers to the main direction in which each polymer component flows from the metering plate to the nozzle discharge holes of the discharge plate. The "polymer distribution hole group" in the present invention refers to a group of distribution holes formed in the lowermost layer on the downstream side of the distributor plate 15 in the polymer spinning path direction, through which the polymer flows of each component pass when they are discharged from the distributor plate 15 toward the single discharge introduction hole 19.

[0078] In the present invention, "a plurality of first component polymer distribution holes in a semicircular arrangement" refers to an arrangement such as the first component polymer distribution holes 9 in the polymer distribution hole group shown in Figure 11(a) in which it is possible to draw a straight line 12 that bisects the circumscribing circle 11 of the polymer distribution hole group and that allows all of the first component polymer distribution holes 9 to be included in one of the two halves of the circumscribing circle. "All of the first component polymer distribution holes 9 included in one semicircle" here refers to a state in which the first component polymer distribution holes 9 are present inside the semicircle and on the straight line 12. An arrangement in which it is not possible to draw a straight line 12 is called a "circular arrangement".

[0079] In the present invention, "at least some of the second component polymer distribution holes are arranged in a semicircular arrangement outside the circumferential portion of the plurality of first component polymer distribution holes in the semicircular arrangement" refers to an arrangement in which, as in the case of second component polymer distribution holes 10 in the polymer distribution hole group shown in Figure 11(a), of the two semicircles formed by straight line 12 and circumscribing circle 11, all of the second component polymer distribution holes 10 in the semicircle containing first component polymer distribution hole 9 are arranged outside the first component polymer distribution hole 9 and on curve 13 along the circumferential direction of said semicircle. In Figure 11(a), the semicircular arrangement is in a single row, but it may be in any number of rows.

[0080] The principle of the present invention will be described with reference to the polymer flow pattern. Both the first component polymer and the second component polymer streams are discharged simultaneously from the distribution holes 18 formed in the lowest layer on the downstream side in the polymer spinning path direction of the distribution plate 15 toward the discharge introduction holes 19, and each polymer stream flows along the polymer spinning path direction while expanding in the direction perpendicular to the polymer spinning path direction, and the two polymers join to form a composite polymer stream. At this time, first, by arranging the multiple first component polymer distribution holes 9 in a semicircular arrangement to be surrounded by the multiple second component polymer distribution holes 10, a distance is generated between the centers of gravity of the polymers on the composite cross section in the composite fiber discharged from the spinneret discharge holes, and the composite fiber is curved toward the high shrinkage component side during heat treatment, thereby imparting crimp development to the composite fiber. Furthermore, the resistance that the composite polymer stream passing through the discharge introduction hole 19 experiences from the wall surface of the hole becomes constant, and the asymmetry of the velocity distribution in the cross-sectional direction of the composite polymer stream can be mitigated. As a result, the bending of the composite polymer stream toward the high-viscosity polymer side that occurs when the composite polymer stream is discharged from the nozzle hole 21 is reduced, and the discharge bending phenomenon can be suppressed.

[0081] Also, as for the method of distributing each polymer on the distribution plate 15 in the present invention, as shown in FIG. 13, it is preferable to use a tournament-type flow path that forms one distribution groove 17 for one distribution hole 18. By disposing the distribution hole 18 for introducing the polymer flow to the downstream side at the end of the distribution groove 17, abnormal retention of the polymer can be eliminated, the distributability of the polymer is high, and the polymer flows can be merged while precisely controlling the flow rate and flow velocity within a wide discharge range. As a result, it is possible to form a stable flow over time without generating abnormal retention while precisely controlling the flow of the polymer amount, which was a problem in polymer merging in conventional composite dies.

[0082] Furthermore, if at least a part of the second component polymer distribution holes 10 is arranged in a semi-circular array outside the circumferential part of the plurality of first component polymer distribution holes 9 arranged in a semi-circular array, the composite cross-section of the composite fiber obtained by discharging the composite polymer flow discharged from the discharge introduction hole 19 from the die discharge hole can be an eccentric core-sheath cross-section with a thin skin coating on the side-by-side cross-section (see FIG. 11(b)), and good crimp manifestation can be expected. Also, as described above, by adopting the tournament method as shown in FIG. 13 for the method of distributing each polymer on the distribution plate 15, the flow of the extremely small amount of polymer forming the thin skin part can be precisely controlled, and since there is no need for a polymer accumulation part as in the conventional die such as Patent Document 7, a stable flow can be formed over time without generating abnormal retention.

[0083] In the polymer distribution hole group formed in the lowermost layer on the downstream side in the polymer spinning path direction of the distribution plate 15 of the present invention, it is preferable to arrange the total number of holes Ht of the second component polymer distribution holes 10 and the number of holes Ho of the second component polymer distribution holes 10 arranged in a semi-circular array outside the circumferential part of the plurality of first component polymer distribution holes 9 arranged in a semi-circular array so as to satisfy the following formula (1). 1 / 16 < Ho / Ht < 1 / 4 ··· Formula (1)

[0084] By arranging the second component polymer-distribution holes 10 so as to satisfy formula (1), the discharge bending phenomenon at the discharge hole of the spinneret can be suppressed, and a composite fiber exhibiting the same degree of crimp developability as that of a side-by-side cross section (see Figure 8(a)) can be obtained.

[0085] Here, the derivation of formula (1) will be described in detail. The relationship between the total number Ht of second component polymer distribution holes 10 in the polymer distribution hole group formed in the downstream lowest layer in the polymer spinning path direction of the distribution plate 15 of the present invention and the number Ho of second component polymer distribution holes 10 arranged in a semicircular arrangement outside the circumferential portion of the plurality of first component polymer distribution holes 9 arranged in a semicircular arrangement therein determines the thickness of the thin skin portion in the composite cross section of the composite fiber obtained by using the composite spinneret of the present invention.

[0086] In the present invention, the "thickness of the thin skin portion" refers to the minimum thickness of the second component polymer covering the first component polymer, for example as shown by the symbol "S" in FIG. 11(b).

[0087] By making the value of Ho / Ht smaller than 1 / 4, the thickness of the thin skin portion becomes sufficiently thin, and the distance between the center of gravity a of the first component polymer and the center point c of the cross section of the composite fiber becomes sufficiently large, so that the obtained composite fiber can be given good crimp development, which is preferable. In particular, by making the value of Ho / Ht smaller than 1 / 6, the obtained composite fiber can be made to have crimp development performance that is comparable to that of conventional latent crimp development fibers having a side-by-side cross section, so this can be mentioned as a more preferable range.

[0088] On the other hand, as the thickness of the thin skin portion is made thinner, the asymmetry of the velocity distribution in the cross-sectional direction of the composite polymer flow at the discharge introduction hole 19 increases, and the effect of suppressing the discharge deflection phenomenon from the spinneret discharge hole decreases. Therefore, in order to fully obtain the effect of suppressing the discharge deflection phenomenon, it is preferable that the value of Ho / Ht is greater than 1 / 16. In particular, in the present invention in which the composite cross section is formed by point discharge through the distribution hole group, by making the value of Ho / Ht greater than 1 / 10, a sufficient number of the second component polymer distribution holes 10 arranged in a semicircular array forming the thin skin portion can be provided, and a homogeneous composite cross section without unevenness in the thin skin portion can be obtained, so that this range can be cited as being more preferable.

[0089] In the discharge plate 16 of the present invention, from the viewpoint of production efficiency and diversification, the number of nozzle holes for discharging the composite polymer stream is 1.0×10 -2 hole / mm 2 It is preferable that the holes are drilled at a filling density of at least this.

[0090] In the present invention, the "hole packing density" refers to a value obtained by dividing the number of nozzle outlet holes in a composite nozzle by the nozzle area.

[0091] In conventional composite spinnerets, in order to form an eccentric core-sheath cross section, it was necessary to provide a separate flow path for coating in addition to a flow path for joining the polymer flows. This required a large processing area for the introduction hole and flow path to form a single fiber, and the hole packing density was at most 5.0×10 -3 hole / mm 2 This limits the number of fibers (filaments) that can be obtained from one composite spinneret.

[0092] On the other hand, in the composite spinneret of the present invention, the polymers are distributed through the tournament-type flow paths in the distribution plate 15 to form a composite cross section, so that the flow paths for joining the polymer flows and the flow paths for coating can be processed in the same flow path. This makes it possible to maximize the hole packing density, which was a problem in the conventional technology.

[0093] The composite spinneret of the present invention achieves a spin rate of 1.0×10 -2 hole / mm 2 This means that the number of fibers obtained from one composite spinneret is more than doubled, and the effect of improving productivity can be fully exhibited, and this can be cited as a preferred range of the present invention. By pursuing this viewpoint, it becomes possible to maintain productivity equal to or higher than that of the conventional method even when producing a so-called fine fiber variety in which the fiber diameter of the composite fiber obtained is thinned by reducing the amount of polymer per one spinneret discharge hole in order to obtain a soft feel preferred for clothing applications, and a hole packing density of 1.5×10 or more is considered to be within the range in which this can be achieved. -2 hole / mm 2 More preferably, it is equal to or greater than this.

[0094] A higher hole packing density is more favorable for improving productivity and diversifying the product line. However, if the size of the distribution holes, distribution grooves, and discharge introduction holes is made too small in order to increase the hole packing density, clogging due to foreign matter in the polymer during the production of composite fibers may occur, and spinnability may deteriorate. Therefore, the practical upper limit is 5.0 × 10 -2 hole / mm 2 It is.

[0095] Hereinafter, the composite spinneret shown in Figures 12(a) to 12(c) will be described in order from upstream to downstream along the flow of polymers, from the composite spinneret shown in Figures 12(a) to 12(c) through the metering plate 14 and distribution plate 15 to form a composite polymer stream, and from the composite polymer stream to the time when the composite polymer stream is discharged from the spinneret discharge hole of the discharge plate 16.

[0096] The first and second component polymers flow from the upstream of the spin pack into the first and second component polymer metering holes 22a and 22b of the metering plate, are metered by the orifices drilled at the bottom, and then flow into the distribution plate 15. Here, each polymer is metered by the pressure loss caused by the orifices provided in each metering hole. The design guide for these orifices is that the pressure loss is 0.1 MPa or more. On the other hand, in order to prevent the pressure loss from becoming excessive and causing distortion of the components, it is preferable to design the pressure loss to be 30.0 MPa or less. This pressure loss is determined by the inflow amount and viscosity of the polymers per metering hole. For example, at a temperature of 280°C and a strain rate of 1000 s -1 When using a polymer with a viscosity at 100 to 200 Pa·s, melt spinning at a spinning temperature of 280 to 290°C and a discharge rate of 0.1 to 5.0 g / min per metering hole, the metering hole can be regulated to have a hole diameter of 0.01 to 1.00 mm and an L / D (discharge hole length / discharge hole diameter) of 0.1 to 5.0, allowing for good metering. When the melt viscosity of the polymer falls below the above viscosity range or the discharge rate of each hole decreases, the hole diameter can be reduced to approach the lower limit of the above range or the hole length can be extended to approach the upper limit of the above range. Conversely, when the viscosity becomes high or the discharge rate increases, the hole diameter and hole length can be reversed.

[0097] It is also preferable to stack a plurality of measuring plates 14 to measure the amount of polymer in stages, and it is more preferable to provide measuring holes in two to ten stages. -5 This is suitable for controlling minute amounts of polymer, which is on the order of g / min / hole and several orders of magnitude lower than the conditions used in the prior art.

[0098] The polymer discharged from each of the metering holes 22a, 22b flows separately into the distribution grooves 17 of the distribution plate 15. In the distribution plate 15, the distribution grooves 17 for storing the polymer flowing in from each of the metering holes 22a, 22b and the distribution holes 18 for allowing the polymer to flow downstream are formed in the lower surface of the distribution grooves. It is preferable that the distribution grooves 17 are formed with a plurality of distribution holes 18 (two or more).

[0099] In addition, the distribution plate 15 may be a tournament-type flow path in which one distribution groove is formed for one distribution hole 18 as shown in FIG. 13, or a tournament-type flow path in which one distribution groove is formed for multiple distribution holes 18 and each polymer is repeatedly merged and distributed individually in a part. If the flow path is designed to repeat multiple distribution holes 18-distribution groove 17-multiple distribution holes 18, the polymer flow can flow into other distribution holes. Therefore, even if the distribution hole 18 is partially blocked, the missing part is filled in the downstream distribution groove 17. In addition, by drilling multiple distribution holes 18 in the same distribution groove 17 and repeating this, even if the polymer of the blocked distribution hole 18 flows into other holes, the influence is substantially zero. Furthermore, since the polymer that has passed through various flow paths, i.e., has been subjected to thermal history, is merged multiple times in the distribution groove 17 and the viscosity is homogenized, it is also significant in terms of suppressing viscosity variation. In particular, in the case of the conjugated fiber of the present invention, since maintaining a high level of dimensional stability of the conjugated cross section leads to spinning stability, it is effective to take into consideration the thermal history and viscosity variation.

[0100] In addition, when designing the arrangement of such a distribution hole 18-distribution groove 17-distribution hole 18 arrangement, if the downstream distribution groove is arranged at an angle of 1 to 179° in the circumferential direction with respect to the upstream distribution groove, and polymers flowing in from different distribution grooves are joined, the polymers that have been subjected to different thermal histories are joined multiple times, which is effective in controlling the composite cross section. In view of the above-mentioned purpose, it is preferable to adopt this joining and distribution mechanism from a more upstream position, and it is also suitable to apply it to the metering plate 14 and its upstream members. A composite spinneret having such a structure precisely controls the flow of an extremely small amount of polymer as described above, and forms a stable flow over time without causing abnormal retention, and it becomes possible to produce a composite fiber in which the instantaneous stability of the composite cross section required in the present invention can be maintained at a high level regardless of the extrusion range.

[0101] The cross-sectional form of the composite fiber can be controlled by the arrangement of distribution holes formed in the downstream lowest layer in the polymer spinning path direction of the distributor plate 15 immediately above the discharge plate 16. In this case, in order to increase the accuracy of the cross-sectional form, the first component polymer and the second component polymer are distributed in an extremely large number in the downstream lowest layer in the polymer spinning path direction of the distributor plate 15 immediately above the discharge plate 16, so that the discharge amount per distribution hole is extremely small. As a result, the pressure loss across the distribution holes is also reduced to 10 -2 From 10 -5 MPa level, the polymer streams discharged from each distribution hole are easily interfered with by other polymer streams. Therefore, in order to suppress the interference between the polymers, it is preferable to adjust the hole diameters of the first component polymer distribution holes 9 and the second component polymer distribution holes 10 and control the discharge speed of the polymer streams discharged from each distribution hole.

[0102] As a preferred range of the flow rate ratio, when the discharge rate of the first component polymer per single distribution hole is F1 and the discharge rate of the second component polymer per single distribution hole is F2, the ratio (F1 / F2 or F1 / F2) is preferably 0.05 to 20, more preferably 0.1 to 10. Within this range, the polymers discharged from the distribution holes formed in the lowermost layer on the downstream side in the polymer spinning path direction of the distribution plate 15 immediately above the discharge plate 16 do not interfere with each other, and the composite polymer flow is guided as a laminar flow through the discharge introduction hole 19 to the reduction hole 20, so that the cross-sectional shape is stable and the shape can be maintained with high precision.

[0103] In order to achieve the composite fiber of the present invention, in addition to employing such a novel composite spinneret, it is preferable that the melt viscosity ratio (V1 / V2) between the melt viscosity V1 of the first component polymer and the melt viscosity V2 of the second component polymer is 1.1 to 15.0.

[0104] The "melt viscosity" in the present invention refers to the melt viscosity measured by a capillary rheometer after reducing the moisture content of a chip-like polymer to 200 ppm or less using a vacuum dryer, and refers to the melt viscosity at the same shear rate at the spinning temperature.

[0105] In the present invention, the cross-sectional form of the composite fiber is basically controlled by the arrangement of the distribution holes, but after the individual polymers join together to form a composite polymer flow, the flow is significantly reduced in the cross-sectional direction by the reduction hole 20. For this reason, the melt viscosity ratio at that time, i.e., the rigidity ratio of the molten polymers, may affect the formation of the cross section. For this reason, in the present invention, it is more preferable that V1 / V2 is 2.0 to 12.0. In particular, in the relevant range, the rigidity of the polymers is high for the first component polymer, which is a high shrinkage component, and low for the second component polymer, which is a low shrinkage component, and in the elongation deformation in the spinning process and the advanced processing process, stress is preferentially applied to the first component polymer, which is a high shrinkage component. For this reason, the high shrinkage component is highly oriented, and the shrinkage difference is enlarged, allowing a higher degree of crimp to be expressed, which is also preferable from the viewpoint of the crimp expression of the composite fiber.

[0106] From the viewpoint of suppressing the phenomenon of bending of the composite polymer flow at the nozzle outlet, the closer to 1 V1 / V2 is, the better. However, taking into consideration the above-mentioned crimp development, a V1 / V2 ratio of 2.0 to 8.0 is particularly preferred.

[0107] Incidentally, the melt viscosity of the above polymers can be relatively freely controlled by adjusting the molecular weight or copolymerization components, even for the same type of polymer. Therefore, in the present invention, the melt viscosity is used as an index for polymer combinations and spinning condition settings.

[0108] The composite polymer stream discharged from the distribution plate 15 flows into the discharge plate 16. Here, it is preferable to provide the discharge plate 16 with a discharge introduction hole 19. The discharge introduction hole 19 is for allowing the composite polymer stream discharged from the distribution plate 15 to flow perpendicularly to the discharge surface for a certain distance. This is intended to reduce the flow rate difference between the first component polymer and the second component polymer, and to reduce the flow rate distribution in the cross-sectional direction of the composite polymer stream. In the present invention, at least two or more types of polymers are made into a composite polymer stream, so providing the discharge introduction hole 19 is preferable from the viewpoint of discharge stability such as cross-sectional form and suppression of the discharge bending phenomenon.

[0109] In terms of suppressing the flow rate distribution, it is preferable to control the flow rate of the polymers themselves by the discharge amount, hole diameter and number of holes in the distribution holes 18 of each polymer. From the viewpoint of almost completing the relaxation of the flow rate ratio, it is preferable to control the flow rate of the polymers themselves by the discharge amount, hole diameter and number of holes in the distribution holes 18 of each polymer. -1 It is preferable to design the discharge introduction hole 19 with a target value of up to 10 seconds (=discharge introduction hole length / polymer flow rate). Within this range, the distribution of flow rate is sufficiently alleviated, and this is effective in improving the stability of the cross section.

[0110] Next, the composite polymer stream is reduced in the cross-sectional direction along the polymer stream by the reduction hole 20 while being introduced into the discharge hole having a desired diameter. Here, the streamline of the middle layer of the composite polymer stream is almost straight, but as it approaches the outer layer, it is greatly bent. In order to obtain the composite fiber of the present invention, it is preferable to reduce the composite polymer stream without destroying the cross-sectional shape of the composite polymer stream composed of countless polymer streams of the first component polymer and the second component polymer. For this reason, it is preferable to set the angle of the hole wall of this reduction hole 20 to the discharge surface in the range of 30° to 90°.

[0111] As described above, the composite polymer stream passes through the discharge introduction hole 19 and the reduction hole 20, and is discharged from the spinneret discharge hole 21 to the spinning line while maintaining the cross-sectional shape according to the arrangement of the distribution holes 18. The purpose of the spinneret discharge hole 21 is to re-meter the flow rate of the composite polymer stream, i.e., the discharge rate, and to control the draft (=take-up speed / discharge linear speed) on the spinning line. The hole diameter and hole length of the spinneret discharge hole 21 are preferably determined in consideration of the viscosity of the polymer and the discharge rate. When producing the composite fiber of the present invention, it is preferable to select the discharge hole diameter D from 0.1 to 2.0 mm and the L / D (discharge hole length / discharge hole diameter) from the range of 0.1 to 5.0.

[0112] The composite fiber of the present invention can be produced using the composite spinneret described above, and in view of productivity and simplicity of equipment, it is preferable to carry out the process by melt spinning.

[0113] When melt spinning is selected, examples of the first component polymer and the second component polymer include melt-moldable polymers and copolymers thereof, such as polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, polypropylene, polyolefin, polycarbonate, polyacrylate, polyamide, polylactic acid, thermoplastic polyurethane, and polyphenylene sulfide. In particular, the melting point of the polymer is preferably 165°C or higher, since it has good heat resistance. In addition, the polymer may contain various additives, such as inorganic substances such as titanium oxide, silica, and barium oxide, colorants such as carbon black, dyes, and pigments, flame retardants, fluorescent whitening agents, antioxidants, and ultraviolet absorbers.

[0114] The combination of the first component polymer (high shrinkage component) and the second component polymer (low shrinkage component) is preferably a combination of polymers that will cause a shrinkage difference when heat treated. From this perspective, it is preferable to use a combination of polymers with molecular weights or compositions that differ enough to cause a viscosity difference of 10 Pa s or more in melt viscosity.

[0115] As specific combinations of polymers, polyethylene terephthalate, polyethylene naphthalate, polybutylene terephthalate, polytrimethylene terephthalate, polyamide, polylactic acid, thermoplastic polyurethane, and polyphenylene sulfide are preferably used with different molecular weights for the first component polymer and the second component polymer, or one is used as a homopolymer and the other as a copolymer, from the viewpoint of suppressing peeling. From the viewpoint of improving the ability to express crimp, combinations of different polymer compositions are preferred. For example, in the case of a first component polymer / a second component polymer, various combinations such as polyester-based combinations of polybutylene terephthalate / polyethylene terephthalate, polytrimethylene terephthalate / polyethylene terephthalate, thermoplastic polyurethane / polyethylene terephthalate, polyester-based elastomer / polyethylene terephthalate, polyester-based elastomer / polybutylene terephthalate, polyamide-based combinations of nylon 6-nylon 66 copolymer / nylon 6 or 610, PEG copolymerized nylon 6 / nylon 6 or 610, thermoplastic polyurethane / nylon 6 or 610, polyolefin-based combinations of ethylene-propylene rubber finely dispersed polypropylene / polypropylene, propylene-α-olefin copolymer / polypropylene are preferred, and combinations of polyester-based and polyamide-based combinations are particularly preferred because they not only enable the expression of fine shrinkage forms, but also have excellent color development, texture, abrasion resistance, dimensional stability, and the like.

[0116] The spinning temperature in the production method of the present invention is preferably set to a temperature at which the polymers used, determined from the above-mentioned viewpoints, mainly those with high melting points or high viscosity, exhibit fluidity. The temperature at which this fluidity is exhibited varies depending on the polymer properties and its molecular weight, but the melting point of the polymer is a guideline, and it may be set to a temperature not higher than the melting point + 60°C. If the temperature is below this, the polymer does not undergo thermal decomposition or the like in the spinning head or spinning pack, and a decrease in molecular weight is suppressed, allowing for good production of composite fibers.

[0117] The polymer discharge amount in the production method of the present invention can be in the range of 0.1 g / min / hole to 20.0 g / min / hole per nozzle, which allows melt discharge while maintaining stability. In this case, it is preferable to consider the pressure loss in the nozzle that can ensure stable discharge. The pressure loss referred to here is preferably 0.1 MPa to 40 MPa, and the discharge amount is determined based on the relationship with the melt viscosity of the polymer, the nozzle hole diameter, and the nozzle hole length.

[0118] The ratio of the first component polymer to the second component polymer when spinning the composite fiber used in the production method of the present invention is preferably selected within a range of 30 / 70 to 70 / 30 by weight based on the discharge amount. This range ensures long-term stability of the composite cross section and allows for efficient and well-balanced production of composite fibers while maintaining stability. Furthermore, a range of 40 / 60 to 60 / 40 is more preferable as it allows the distance between the center of gravity a and the center point c to be sufficiently far away and allows for good crimp expression.

[0119] The polymer flow melted and discharged from the discharge hole is cooled and solidified, and is focused by adding an oil agent or the like, and is taken up by a roller having a regulated peripheral speed. Here, the take-up speed is determined based on the discharge amount and the target fiber diameter. In the present invention, from the viewpoint of stably producing the composite fiber, the take-up speed of the roller is preferably about 500 to 6000 m / min, and can be changed depending on the physical properties of the polymer and the purpose of use of the fiber. It is preferable to draw the spun composite fiber from the viewpoint that not only the mechanical properties can be improved by promoting the uniaxial orientation of the fiber, but also good crimp expression can be obtained by expanding the thermal contraction difference caused by the stress difference during drawing between the composite polymers and the orientation difference during drawing. Regarding drawing, the spun composite fiber may be drawn after being wound once, or may be drawn immediately after spinning without being wound once. In addition to drawing, false twisting may be applied.

[0120] As for the drawing conditions, for example, in a drawing machine consisting of one or more pairs of rollers, if the fiber is made of a polymer exhibiting thermoplasticity that can be melt-spun, it is naturally drawn in the fiber axis direction by the peripheral speed ratio of the first roller set at a temperature above the glass transition temperature and below the melting point and the second roller set at the crystallization temperature, and then heat-set and wound up. In the case of a polymer that does not exhibit a glass transition, the dynamic viscoelasticity of the composite fiber is measured (tan δ), and a temperature above the peak temperature on the high-temperature side of the obtained tan δ is selected as the preheating temperature. Here, from the viewpoint of increasing the draw ratio and improving the mechanical properties and potential crimpability, it is also preferable to carry out this drawing process in multiple stages. When the composite fiber is produced by the above-mentioned production method, as shown in FIG. 6(b), a part of the fiber cross section becomes a thin-skinned eccentric core-sheath cross section fiber composed of a uniform thin skin made of a sheath component, which can be cited as a more preferable cross-sectional form for use in the present invention. In the thin-skinned eccentric sheath-core cross section fiber, a particularly preferred embodiment is one in which the ratio S / D of the minimum thickness S of the component covering the core component to the fiber diameter D is 0.01 to 0.10, and the perimeter portion (S ratio) having a thickness within 1.05 times the minimum thickness S accounts for 30% or more of the entire perimeter of the fiber cross section. By setting it in this range, the distance between the centers of gravity that affects crimp can be set with a high degree of freedom, and a wide range of control over the coil diameter of the potential crimp of the fiber can be ensured.

[0121] In order to obtain a state in which two or more types of crimp are mixed in the multifilament, which is a feature of the stretch textured yarn of the present invention, various methods can be adopted, such as a method of changing the distance between the centers of gravity of components for each fiber by using eccentric sheath-core cross section fibers, a method of changing the fiber diameter for each fiber of the eccentric sheath-core cross section fibers, a method of applying false twist processing to the eccentric sheath-core cross section fibers to impart obvious crimp in addition to latent crimp, and a method of post-mixing two types of eccentric sheath-core cross section fibers with different coil diameters. From the viewpoint that the multifilament is constructed in a state in which a fiber with a small coil diameter is partially entangled with a fiber with a large coil diameter, which is a feature of the present invention, the fiber with the large coil diameter partially follows the elongation deformation of the fiber with the small coil diameter, and the multifilament as a whole undergoes good elongation deformation, the method of changing the fiber diameter for each fiber of the thin-skin eccentric sheath-core cross section fibers or the method of applying false twist processing to the thin-skin eccentric sheath-core cross section fibers is preferably used.

[0122] When the stretch textured yarn of the present invention is obtained by a method in which the fiber diameter of each of the eccentric sheath-core cross section fibers is changed, it is preferable that "two or more types of eccentric sheath-core composite fibers with different fiber diameters are mixed in the multifilament."

[0123] In the present invention, the state in which "two or more types of eccentric sheath-core composite fibers having different fiber diameters are mixed in a multifilament" refers to a state in which two or more fiber diameter distributions are observed when all single fibers are evaluated with the above-mentioned fiber diameters in the cross section of the yarn bundle. If two types of eccentric sheath-core composite fibers having different fiber diameters are present in a multifilament, two fiber diameter distributions (5-(a) and 5-(c)) as shown in FIG. 5 will be observed.

[0124] That is, a group of single fibers having fiber diameters falling within each distribution range (distribution width) is defined as "one type," and the presence of two or more of these fiber diameter distributions in the measurement results of all the fibers constituting the latent crimped yarn, as shown in Figure 5, means that "two or more types of eccentric core-sheath composite fibers with different fiber diameters are present in the yarn bundle" according to the present invention. The fiber diameter distribution width (5-(e), 5-(f)) referred to here means a range of ±5% of the median fiber diameter (5-(b), 5-(d)), which is the peak value with the greatest number of occurrences in each group of single fibers.

[0125] When the eccentric core-sheath composite fiber used in the present invention is subjected to a heat treatment or the like to induce crimping, the crimped form depends on the fiber diameter, and therefore multiple crimps with different coil diameters are mixed within the multifilament. In other words, it is preferable that the ratio (Dmax / Dmin) of the maximum value (Dmax) and the minimum value (Dmin) of the central fiber diameter of the fibers constituting the multifilament is 1.20 or more.

[0126] The fiber diameter and the median fiber diameter ratio (Dmax / Dmin) referred to here can be determined as follows. First, the latent crimped yarn is embedded in an embedding agent such as epoxy resin, and images of all single fibers are taken of the cross section with a scanning electron microscope (SEM) (e.g., Keyence scanning electron microscope, model number "VE-7800") at a magnification that allows observation of 10 or more single fibers. For each image taken, the cross-sectional area Af of the single fiber is measured using image analysis software (e.g., Mitani Shoji Co., Ltd.'s "WinROOF2015"), and the diameter of a perfect circle having the same area as this cross-sectional area Af is calculated in μm units, and the fiber diameter is calculated by rounding off to the nearest tenth. This measurement is performed on all single fibers that make up the latent crimped yarn, and a fiber diameter distribution as shown in Figure 5 is created from the results. The single fibers are classified by fiber diameter, and then the central center-to-center distance, which is the peak value with the highest number of fibers present in each single fiber group, is obtained. Based on this result, the central center distance ratio (Dmax / Dmin) is calculated using the maximum (Dmax) and minimum (Dmin) central center distances among the potentially crimped yarns.

[0127] If Dmax / Dmin is 1.20 or more, a multifilament can be constructed in which fibers with a smaller coil diameter are partially entangled with fibers with a larger coil diameter, and a stretch-processed yarn in which the fibers with a larger coil diameter partially follow the stretch deformation of the fibers with a smaller coil diameter, which is the object of the present invention, can be obtained. Furthermore, if Dmax / Dmin is 1.30 to 2.00, a crimp phase shift occurs between the fibers, the stretch-stress curve of the multifilament does not deform stepwise, and a stretch-processed yarn with good stretch energy can be obtained, so this can be cited as a more preferable range.

[0128] Furthermore, when the stretch-processed yarn of the present invention is obtained by applying false twist processing to thin-skinned eccentric core-sheath cross-section fibers, the size of the actual crimp imparted can be easily changed by changing the processing conditions, and by determining the processing conditions according to the size of the latent crimp, it is possible to control the specific coil diameter distribution, which is a requirement of the stretch-processed yarn of the present invention.

[0129] Furthermore, in the stretch-processed yarn obtained by false twisting, the crimp size in the fiber longitudinal direction is not uniform, and latent / actual crimps exist randomly, so that the fibers do not converge to each other for each crimp size. Therefore, separation of multifilaments, which is seen in stretch-processed yarns produced by post-blending, can be suppressed, and the handleability and processability during higher-order processes are excellent, so that the stretch-processed yarn of the present invention can be obtained with good quality.

[0130] In order to stably produce the stretch textured yarn of the present invention using false twist processing, it is preferable to control the coil diameter size of the apparent crimp of the textured yarn by the actual twist number of the multifilament in the twisting region.

[0131] In other words, the number of twists T (unit: turns / m), which is the number of twists of the multifilament in the twisting region, is determined according to the total fineness Df (unit: dtex) of the multifilament after the false twisting process. It is preferable to set the false twisting conditions, such as the rotation speed and processing speed of the twisting mechanism, so as to satisfy the following condition. 20000 / Df 0.5 ≦T≦40000 / Df 0.5

[0132] Here, the false twist number T is determined by sampling a multifilament running in the twisting region of the false twisting process just before the twister, with a length of 50 cm or more, without untwisting the multifilament. The sampled yarn sample is attached to a twist detector without untwisting the multifilament, and the false twist number is measured by the method described in JIS 1013 (2010) 8.13. By satisfying the above-mentioned condition for the false twist number, the coil diameter of the apparent crimp in the obtained multifilament can be finely controlled, and the characteristic coil diameter distribution of the stretch textured yarn of the present invention can be achieved.

[0133] In addition, under the above false twist conditions, in order to impart uniform crimp to the entire fibers in the multifilament and obtain a high-quality textured yarn of the present invention, it is advisable to adjust the draw ratio in the twisting region. The draw ratio referred to here is calculated as Vd / V0, where V0 is the peripheral speed of the roller that supplies the yarn to the twisting region and Vd is the peripheral speed of the roller installed immediately after the twisting mechanism, and is preferably determined according to the properties of the yarn to be supplied.

[0134] When a drawn eccentric sheath-core fiber is used as the supply yarn, Vd / V0 may be set to 0.9 to 1.4 times, and when an undrawn eccentric sheath-core fiber is used as the supply yarn, Vd / V0 may be set to 1.2 to 2.0 times, and drawing may be performed simultaneously with false twisting. By setting the draw ratio within this range, excessive tension does not occur in the twisted region, and slackness of the multifilament does not occur, and uniform crimp can be imparted to all the fibers in the multifilament.

[0135] Furthermore, from the viewpoint of firmly fixing the apparent crimp, the false twist temperature is preferably determined from the range of Tg+50 to Tg+150°C based on the glass transition temperature (Tg) of the sheath component polymer. The false twist temperature here means the temperature of the heater installed in the twisting region. By setting the false twist temperature in this range, the sheath component that has been significantly twisted and deformed in the fiber cross section can be sufficiently structurally fixed, so that the dimensional stability of the apparent crimp becomes good, and a high-quality fabric can be obtained without wrinkles or streaks. The Tg of the sheath component here is measured by differential scanning calorimetry (DSC) of the chip of the polymer used for the sheath component. In addition, in the stretch-processed yarn of the present invention, in order to fix the apparent crimp and achieve the characteristic coil diameter distribution of the stretch-processed yarn of the present invention, it is preferable to use a one-heater method in which a heater is placed only in the twisting region.

[0136] In the present invention, by carrying out false twist processing under the above conditions, the coil diameter of the manifest crimp of the multifilament can be controlled relative to the coil diameter of the latent crimp within a suitable range in which the effects of the present invention can be exerted, and the stretch-processed yarn of the present invention can be produced with high quality.

[0137] As described above, the manufacturing method of the stretch processed yarn of the present invention has been explained based on the general melt spinning method, but it goes without saying that it can also be manufactured by the melt blowing method and the spunbonding method, and it can also be manufactured by solution spinning methods such as wet and dry-wet methods. EXAMPLES

[0138] The stretch textured yarn of the present invention will be specifically described below with reference to examples.

[0139] The following evaluations were carried out for the examples and comparative examples.

[0140] A. Fineness The weight of 100m of fiber was measured and multiplied by 100. This process was repeated 10 times, and the average value was rounded off to the first decimal place to obtain the total fineness (dtex). The value obtained by dividing the total fineness by the number of filaments was the single fiber fineness (dtex).

[0141] B. Fiber strength and elongation at break The specimens were measured using a tensile tester (Orientec Co., Ltd. "TENSILON" UCT-100) under the constant-speed elongation conditions specified in JIS L1013 (2010) 8.5.1 standard time test. The gripping distance was 20 cm, the tensile speed was 20 cm / min, and the number of tests was 10. The breaking elongation was calculated from the elongation at the point showing the maximum strength on the elongation-stress curve.

[0142] C. Coil diameter distribution of multifilament and ratio of maximum group average value to minimum group average value The stretch-processed yarn was cut into a 10 m skein using a measuring machine or the like, and immersed in boiling water at 98 ° C. or higher with a load of 0.2 mg / d, and boiled for 15 minutes. After the treated yarn was thoroughly dried by air drying, a load of 1 mg / d was applied for 30 seconds or more, and then markings were made at any point on the multifilament so that the distance between the two points was 3 cm. Thereafter, the fibers were separated from the multifilament so as not to cause plastic deformation, and the distance between the pre-applied markings was adjusted to the original 3 cm and fixed on a slide glass, and an image of this sample was taken with a VHX-2000 digital microscope manufactured by Keyence Corporation at a magnification at which 5 to 10 crimp peaks could be observed. In each image taken, the coil diameter was measured to the first decimal place in μm units. The same operation was performed randomly for the different fibers constituting the multifilament, and this was repeated to measure the coil diameter so that the total number of data points was 100. These measured values ​​were divided into classes with a width of 10 μm, with the boundary value set at 10×n (n: natural number) μm, and a histogram was created with the vertical axis representing frequency. In the created histogram, when groups as defined in the present invention existed, the group average value was calculated by simply averaging the coil diameters included in each group. Based on these results, the maximum of all group average values ​​included in the coil diameter distribution was divided by the minimum to calculate the ratio. Note that the ratio of the maximum group average value to the minimum group average value was rounded off to two decimal places.

[0143] D. Average diameter of the fibers The stretch-processed yarn was embedded in an embedding agent such as epoxy resin, and images of all fibers were taken of the cross-section of the yarn using a Keyence VE-7800 scanning electron microscope (SEM) at a magnification that allowed observation of 10 or more fibers. For each image, the cross-sectional area Af of the fiber was measured using image analysis software (Mitani Shoji Co., Ltd.'s "WinROOF2015"), and the diameter of a perfect circle with the same area as this cross-sectional area Af was calculated. This was measured for all fibers constituting the multifilament, and the average diameter of the fibers was calculated by taking a simple number average. The average diameter of the fibers is in μm and rounded off to the nearest tenth.

[0144] E. Extension energy in tensile properties The stretch-processed yarn was left unloaded for 24 hours at a temperature of 20±2°C and a relative humidity of 65±2%. After 24 hours of standing, a load of 1 mg / d was applied to the yarn sample, and after 30 seconds or more had elapsed, the sample was fixed to a tensile tester "TENSILON" UCT-100 manufactured by Orientec Co., Ltd. with the initial sample length of 50 mm while still under load. A tensile test was carried out on the yarn sample at a tensile speed of 50 mm / min, and an elongation-stress curve was created as shown in FIG. 4, with the horizontal axis representing elongation (unit: mm) and the vertical axis representing stress (unit: cN / dtex). In the obtained elongation-stress curve, the area Ae enclosed by the point where the strength was 0.05 cN / dtex (4-(a) in FIG. 4), the intersection point of the horizontal axis when a perpendicular line was dropped from the point to the horizontal axis (stress 0 cN / tex) (4-(b) in FIG. 4), and the origin was calculated. This was performed for 10 different yarn samples, and the extension energy was calculated by simply averaging the results. The extension energy is expressed in μJ / dtex and is rounded to one decimal place.

[0145] F. Fabric evaluation (motion tracking, adhesion) A plain weave fabric was produced using stretch-processed yarn for the weft and warp threads with a weft density of 90 threads / inch. The fabric was then scoured at 80°C for 20 minutes, with an intermediate set at 180°C for 1 minute, and then relaxed at 120°C for 20 minutes. The woven fabric samples prepared as described above were evaluated by 10 experienced experts on the basis of the elongation when stretched in the weft direction and the resistance felt when stretched, and on the basis of the ability of the fabric to follow movements when deformation is applied, using the following three-point scale. In addition, the adhesion to the skin was evaluated using the following three-level scale in terms of friction between the skin and the fabric when the fabric was stretched. For motion tracking and adhesion, A was given 5 points, B was given 2 points, and C was given 0 points. A total score of 30 points or more by the 10 panelists was given an "A" rating, 10 to 29 points was given a "B" rating, and 9 points or less was given a "C." Ratings of "A" and "B" are acceptable. A: It has moderate resistance and great stretch. B: There is a little or a little resistance, but it stretches a lot. C: Insufficient resistance when stretching or excessive resistance when stretching.

[0146] G. Abrasion resistance The abrasion resistance of the fabric produced in F above was evaluated according to JIS L1096 (2010) Section 8.19, Method E (Martindale method).

[0147] H. Composite cap (distributor cap) In Examples 12 to 20 and Comparative Examples 4 to 9, when the composite spinneret was a distributor type spinneret, the arrangement of the first component polymer distribution holes in the polymer distribution hole group formed in the lowermost layer on the downstream side in the polymer spinning path direction of the distributor plate was evaluated. In this case, an arrangement in which it was possible to draw an arbitrary straight line in the circumscribing circle of the polymer distribution hole group, which divided the circumscribing circle into two equal parts and included all of the first component polymer distribution holes on one side of the bisecting semicircle, was defined as a semicircular arrangement. Including all on one side of the semicircle here means that the first component polymer distribution holes are present inside the semicircle or on a straight line. An arrangement in which it was not possible to draw an arbitrary straight line was defined as a circular arrangement. Regarding the number of holes of the second component polymer distribution holes in the polymer distribution hole group, the number of holes Ho of the second component polymer distribution holes arranged in a semicircular arrangement outside the circumferential part of the multiple first component polymer distribution holes arranged in a semicircular arrangement was evaluated. In this case, the circumscribed circle of the polymer distribution hole group was divided into two semicircles by any straight line that could bisect the circumscribed circle of the polymer distribution hole group and include all of the first component polymer distribution holes on one side of the bisected semicircle, and the number of holes of the second component polymer distribution holes on any curve parallel to the circumferential direction of the semicircle within the semicircle containing the first component polymer distribution holes was defined as the number Ho of the second component polymer distribution holes arranged in a semicircular arrangement outside the circumferential part of the multiple first component polymer distribution holes arranged in a semicircular arrangement. Ho was also calculated by dividing Ho by the total number of holes Ht of the second component polymer distribution holes in the polymer distribution hole group.

[0148] I. Composite die (hole packing density) The hole packing density (holes / mm ) was calculated by dividing the number of nozzle discharge holes of the composite nozzle in Examples 12 to 20 and Comparative Examples 4 to 9 by the nozzle area. 2 ) was decided.

[0149] J. Polymer Melt Viscosity and Viscosity Ratio The chip-shaped polymer was dried in a vacuum dryer to a moisture content of 200 ppm or less, and the melt viscosity was measured by changing the strain rate stepwise using a Capillograph manufactured by Toyo Seiki Seisakusho Co., Ltd. The measurement temperature was the same as the spinning temperature, and the measurement was started 5 minutes after the sample was put into the heating furnace under a nitrogen atmosphere, and the shear rate was 1216 s -1 The value was evaluated as the melt viscosity of the polymer. Furthermore, the melt viscosity of the first component polymer was divided by the melt viscosity of the second component polymer, and the value was rounded to two decimal places to obtain the viscosity ratio (V1 / V2).

[0150] K. Discharge stability Spinning was performed for Examples 12 to 20 and Comparative Examples 4 to 9, and the polymer flow discharged from the nozzle outlet hole was photographed with a camera at a distance of 300 mm below the nozzle face and at an angle of 45° from the perpendicular to the nozzle face. The discharge stability was evaluated on a three-point scale based on the angle of curvature of the polymer flow relative to the normal to the nozzle face in the photographed image. Very good A: Less than 45° Good B: 45° or more, less than 60° Defective C: 60° or more

[0151] L. Spinning stability Spinning was carried out for Examples 12 to 20 and Comparative Examples 4 to 9, and the spinning stability was evaluated on the basis of the number of yarn breaks per 10 million meters into the following three stages. Very good A: Less than 0.8 times / 10 million m Good B: 0.8 times / 10 million m or more, less than 2.0 times / 10 million m Defective C: 2.0 times / 10 million m or more

[0152] M. Cross section (composite cross section, thickness ratio of thin skin part, variation in thickness of thin skin part) After embedding the fibers in an embedding agent such as epoxy resin, the cross section was photographed with a transmission electron microscope (TEM) at a magnification where more than 10 fibers could be observed, and the composite cross section was observed. In this case, by applying metal staining, the dyeing difference between the polymers was utilized to clarify the contrast of the joints of the composite cross section. Furthermore, when the composite cross section of the photographed image was an eccentric core-sheath cross section as shown in Figure 11(b), the thickness of the thin skin part, which represents the minimum thickness of the sheath component covering the core component (symbol "S" in Figure 11(b)), and the fiber diameter, which represents the width of the fiber in the direction perpendicular to the fiber axis, were calculated in units of μm for 10 or more fibers randomly sampled from each image, and the value was calculated by dividing the thickness of the thin skin part by the fiber diameter. Note that the simple number average of the results obtained by performing this for 10 different fibers was calculated and rounded to two decimal places to obtain the thickness ratio of the thin skin part, and the standard deviation CV% (Coefficient of Variation) of the thickness of the thin skin part for the 10 fibers was used as the thickness variation of the thin skin part.

[0153] N. Shrinkage Spinning was carried out for Examples 12 to 20 and Comparative Examples 4 to 9, and the crimp development of the obtained composite fibers was evaluated based on the stretch extension rate (JISL1013 (2010) Section 8.11, Method C (simplified method)) into the following three levels. Very good A: 60% or more Good B: 40% or more, less than 60% Defective C: Less than 40%

[0154] [Example 1] The core component of the fiber that constitutes the stretchable yarn was polybutylene terephthalate (PBT) with a melt viscosity of 160 Pa s, and the sheath component was polyethylene terephthalate (PET1) with a melt viscosity of 30 Pa s. After melting these polymers separately, they were metered by a pump so that the core / sheath discharge ratio was 50 / 50, and separately flowed into the same spinning pack incorporating a distribution plate with distribution holes as shown in Figure 11(a), and discharged from a spinneret with 72 discharge holes at a spinning temperature of 280°C. When the distribution plate used in Example 1 is made into fibers, part of the polymer of the sheath component B covering the core component A becomes a uniform thin skin, forming a composite cross section (Figure 6(b)) that satisfies the requirements for the thin-skin eccentric core-sheath cross section of the present invention.

[0155] The discharged composite polymer stream was cooled, and then an oil agent was added thereto. The stream was wound around a roller heated to 65°C at a speed of 1000 m / min, and then drawn 3.2 times between the roller and a roller heated to 150°C at a speed of 3200 m / min to obtain a drawn yarn of 56 dtex-72 filaments. The wound drawn yarn was heated with a heater set at 170°C between rollers at a processing speed of 250 m / min and a draw ratio of 1.0, and false twisted using a friction disc at a rotation speed such that the false twist number was 3000 T / m, to obtain a 56 dtex-72 filament stretch-processed yarn of the present invention. Furthermore, since the fiber cross-section of the drawn yarn was precisely controlled in the obtained stretch-processed yarn, there were no defects such as fuzz or whitening due to peeling between the core / sheath components during the false twisting process, and the yarn had excellent quality and processability.

[0156] The obtained stretch-processed yarn had sufficient mechanical properties for practical use, with a strength of 3.5 cN / dtex and an elongation of 28%, and the average fiber diameter was 7.5 μm. When the fiber crimp morphology was observed, two groups were observed in the coil diameter distribution, with the respective group average values ​​being 85.3 μm and 159.7 μm, and the ratio of the maximum group average value to the minimum group average value was 1.87. The proportion of fibers contained in the group with the minimum group average value of coil diameter was 51%.

[0157] As such, the stretch-processed yarn of Example 1 has a mixture of shrinkages with a suitable size difference, and the elongation-stress curve of the stretch-processed yarn of Example 1 shows a high elongation energy of 3.9 μJ / dtex, as shown by the solid line 3-(b) in Figure 3, by favorably expressing stress from the low elongation region, and thus has suitable elongation resistance.

[0158] When the stretch-processed yarn of Example 1 was used as a fabric and subjected to a relaxation treatment, it exhibited good stretchability while having moderate resistance to stretching from the low stretch range, resulting in excellent holding power and excellent movement followability (movement followability: A). Furthermore, because the average fiber diameter of the stretch-processed yarn was small, friction between the skin and the fabric was small when stretched, resulting in excellent adhesion to the skin (adhesion: A). The fabric made of the stretch-processed yarn of Example 1 had a soft feel and comfortable movement-following ability, while also having good abrasion resistance, with a Martindale test result of 3,000 strokes, that could withstand use in harsh environments. The results are shown in Table 1.

[0159] [Examples 2 and 3] In Examples 2 and 3, drawn yarns were produced in the same manner as in Example 1, and false twist processing was performed under the same conditions as in Example 1, except that the false twist numbers were set to 3500 T / m and 2500 T / m, respectively, by changing the rotation speed of the friction disc in the false twist process, to obtain stretch-processed yarns of the present invention. In Examples 2 and 3, although the frictional force received from the friction disc changed, the fiber cross-section of the drawn yarn was controlled to a thin-skinned eccentric core-sheath cross-section that satisfied the requirements of the present invention, and therefore there were no defects such as fuzz or whitening due to peeling between the core and sheath, and the yarn quality and processing passability were excellent.

[0160] In the stretch-processed yarns of Examples 2 and 3, two groups were observed in the coil diameter distribution, and the apparent crimp size changed depending on the number of false twists, so the ratio of the maximum to minimum group average values ​​changed; however, in both cases, this was controlled within a range in which the effects of the present invention could be achieved. In the stretch textured yarn of Example 2, the false twist number in the false twisting process was increased, resulting in extremely fine apparent crimp, and the ratio of the maximum to minimum group average values ​​in the coil diameter distribution was increased. Therefore, in the elongation-stress curve of the stretch textured yarn of Example 2, although the stress expression in the low elongation range was slightly decreased, the yarn was elongated more at low stress, and the elongation energy was high at 4.3 μJ / dtex. Therefore, when stretched as a fabric, it stretched softly from a low elongation region to a high elongation region and had excellent movement followability. The stretch-textured yarn of Example 3 had a low false twist number in the false twisting process, so the ratio of the maximum to minimum group average values ​​in the coil diameter distribution was close. Therefore, in the elongation-stress curve of the stretch-textured yarn of Example 3, the stress generated in the low elongation range increased, while the stress rose at a lower elongation, resulting in an elongation energy of 2.6 μJ / dtex. When stretched as a fabric, the resistance in the low elongation range was soft, and the yarn had a soft movement tracking property suitable for casual clothing. The results are shown in Table 1.

[0161] [Examples 4 and 5] In Examples 4 and 5, stretch textured yarns of the present invention were obtained in the same manner as in Example 1, except that the draw ratios in the false twisting step were 1.1 and 0.9, respectively. In Examples 4 and 5, the tension in the twisting region changed, and the frictional force received from the friction disc also changed. However, because the fiber cross-section of the drawn yarn was precisely controlled, there were no defects such as fuzz or whitening due to peeling between the core and sheath, and the yarn quality and processing passability were excellent.

[0162] In the stretch-processed yarns of Examples 4 and 5, the number of false twists was approximately the same as in Example 1, so both had coil diameter distributions with maximum-to-minimum group average value ratios approximately the same as in Example 1; however, the proportion of crimps contained in the group centered on the minimum group average value changed depending on the tension in the twisted region. The stretch-processed yarn of Example 4 had a high draw ratio and high tension in the twisted region, so it was less susceptible to apparent crimping, and the proportion of crimps in the group centered on the minimum group average value was reduced. As a result, in the stretch-stress curve of the stretch-processed yarn of Example 4, the low-stress region corresponding to the stretching of the small coil diameter was reduced, so the stretching energy was 1.8 μJ / dtex, and when the fabric was stretched, a slight sense of tension was felt, but the movement tracking was superior to that of the conventional yarn, and the level was not problematic. In the stretch-processed yarn of Example 5, the tension in the twisted region is low due to the low draw ratio, and the apparent crimp is easily generated, so the apparent crimp is uniform throughout the multifilament, and the proportion of crimps contained in the group centered on the smallest group average value increased. Therefore, in the stretch-stress curve of the stretch-processed yarn of Example 5, the low stress region corresponding to the stretch of the small coil diameter was expanded, and the stretch energy was good at 3.8 μJ / dtex. The results are shown in Table 1.

[0163] [Example 6] In Example 6, a distribution plate having distribution holes formed therein similar to those in Example 1 was used, and a die having 24 discharge holes was used. The polymers constituting the stretch processed yarn, the core / sheath extrusion ratio, and the spinning temperature were extruded in the same manner as in Example 1, and the yarn was drawn under the same drawing and winding conditions as in Example 1 to obtain a 56 dtex-24 filament drawn yarn. The obtained drawn yarn was subjected to false twist processing under the same processing speed, draw ratio, and heater temperature conditions as in Example 1, and the friction disc rotation speed was adjusted so that the false twist number was 3000 T / m, thereby obtaining a stretch-processed yarn of the present invention.

[0164] In the drawn yarn obtained in Example 6, the absolute value of the skin thickness in the fiber cross section increased with an increase in fiber diameter, and the abrasion resistance improved. Therefore, in the false twisting process, there were no defects such as fuzz or whitening due to peeling between the core / sheath components, and the yarn quality and processability were particularly excellent. The stretch-processed yarn of Example 6 had an average fiber diameter of 15.0 μm, and when the crimped form of the fiber was observed, two groups were observed in the coil diameter distribution, with group average values ​​of 137.0 μm and 344.0 μm, respectively. As the average fiber diameter increased, the coil diameters of the latent and actual crimps also increased, and the moment at which the fiber exhibited a crimped structure also increased, so that the stretch-stress curve of the stretch-processed yarn of Example 6 exhibited high stress, especially at low elongations (elongation energy: 2.5 μJ / dtex). The results are shown in Table 1.

[0165] [Example 7] In Example 7, a distribution plate having distribution holes formed therein similar to those in Example 1 was used, and a die having 18 discharge holes was used. The polymers constituting the stretch processed yarn, the core / sheath extrusion ratio, and the spinning temperature were extruded in the same manner as in Example 1, and the yarn was drawn under the same drawing and winding conditions as in Example 1 to obtain a 56 dtex-18 filament drawn yarn. The obtained drawn yarn was false-twisted under the same processing speed, draw ratio, and heater temperature conditions as in Example 1, and the friction disk rotation speed was adjusted so that the false-twist number was 3000 T / m, to obtain a stretch-textured yarn (56dex-18 filaments, maximum-minimum group average ratio 2.62).

[0166] The stretch-processed yarn of Example 7 had an average fiber diameter of 18.5 μm, and when the crimped form of the fiber was observed, two groups were observed in the coil diameter distribution, with group average values ​​of 163.7 μm and 429.4 μm, respectively. Due to an increase in the average fiber diameter, the coil diameters of the latent / actual crimps and the moment at which the fiber develops a crimped structure increase, and the stretch-stress curve of the stretch-processed yarn of Example 7 did not impair the effects of the present invention at low stretches, but developed very high stress (stretching energy: 1.9 μJ / dtex). When the stretch-processed yarn of Example 7 was used as a fabric, it had inferior adhesion compared to Example 1, but when stretched, it had a high stretch resistance, which provided a strong sense of hold and a suitable wearing pressure that did not impair the effects of the present invention. The results are shown in Table 1.

[0167] [Examples 8 and 9] In Examples 8 and 9, the polymer was changed as shown in Table 1, and the same nozzle as in Example 1 was used for extrusion.

[0168] In Example 8, the multifilament was wound around a roller heated to 60°C at a speed of 1000 m / min, and then drawn between a roller heated to 150°C at a speed of 3400 m / min to obtain a drawn yarn of 56 dtex-72 filaments. The obtained drawn yarn was subjected to false twist processing under the same processing speed, draw ratio, and heater temperature conditions as in Example 1, and the friction disc rotation speed was adjusted so that the false twist number was 3000 T / m, thereby obtaining a stretch-processed yarn of the present invention.

[0169] In Example 9, the discharged composite polymer stream was wound around a roller heated to 80° C. at a speed of 1000 m / min, and then drawn between a roller heated to 150° C. at a speed of 3000 m / min to obtain a drawn yarn of 56 dtex-72 filaments. The obtained drawn yarn was subjected to false twist processing under the same processing speed and draw ratio as in Example 1, with the heater temperature set to 200°C and the friction disc rotation speed adjusted so that the false twist number was 3000 T / m, thereby obtaining a stretch-processed yarn of the present invention.

[0170] In Examples 8 and 9, the shape of the fiber cross section changed slightly due to the change in polymer. However, in all cases, the fiber cross section was controlled to be what is called a thin-skin eccentric core-sheath cross section in the present invention. Therefore, there were no defects such as fuzz or whitening due to peeling between the core / sheath components in the false twisting process, and the yarn had excellent quality and processability. In Example 8, PPT, which shrinks highly when heat-treated, was used as the core component, resulting in fine latent shrinkage, and although the ratio of the maximum to minimum group average values ​​in the coil diameter distribution was reduced, the overall shrinkage was fine. In addition, since PPT has a low Young's modulus, the stretch-stress curve of the stretch-processed yarn of Example 8 was characteristically very stretchable at low stress, and the stretch energy was excellent at 4.0 μm / dtex. When made into a fabric and stretched, it had a soft stretch resistance that did not impair the effects of the present invention, and was particularly excellent in stretchability. In Example 9, the use of PET2 (melt viscosity 290 Pa s) as the core component increased the Young's modulus of the yarn and the elongation resistance of the crimp. As a result, the elongation-stress curve of the stretch-processed yarn of Example 9 showed high stress overall and a low elongation energy of 1.8 μJ / dtex, but when stretched into a fabric, the high elongation resistance provided a strong sense of hold and provided a suitable wearing pressure that did not impair the effects of the present invention. The results are shown in Table 2.

[0171] [Example 10] In Example 10, a distribution plate was used in which two types of distribution hole groups were formed, in which the number of distribution holes (distribution holes present on curve 13 in FIG. 11(a)) forming the thin skin in each distribution hole was changed so that the fiber cross section would have a thin skin eccentric core-sheath cross section and the skin thickness would be 0.04 and 0.09 when the fiber was made. The number of discharge holes consisting of each distribution hole group was 36 holes. FIG. 7 shows the discharge hole arrangement in the discharge plate 16 of the spinneret used in Example 10, and a spinneret with a staggered hole arrangement was used in which the discharge hole group (7-(a)) corresponding to the distribution hole group with a skin thickness of 0.04 and the discharge hole group (7-(b)) corresponding to the distribution hole group with a skin thickness of 0.09 were alternately arranged.

[0172] In Example 10, except that the above-mentioned distribution plate was used, spinning, drawing, and false twisting were carried out in the same manner as in Example 1 to obtain a stretch textured yarn of the present invention.

[0173] In Example 10, although the thickness of the thin skin of the constituent fibers was changed, all of them were controlled to have the thin-skin eccentric core-sheath cross section as defined in the present invention, and therefore there were no defects such as fuzz or whitening due to peeling between the core / sheath components in the false twisting process, and the yarn had excellent quality and processability.

[0174] Observation of the crimp morphology of the stretched yarn of Example 10 showed that two types of latent crimp and apparent crimp were mixed according to the cross-sectional form of the fiber, and the coil diameter distribution had three groups. Therefore, in the elongation-stress curve, these three types of crimp were deformed sequentially according to the elongation of the multifilament, so the rise in stress was gradual from the low elongation region to the high elongation region, and the elongation energy was very high at 5.0 μJ / dtex. Therefore, when the fabric was stretched, stress was generated gradually according to the degree of stretch, so the fabric had excellent holding power and excellent movement tracking ability. The results are shown in Table 2.

[0175] [Example 11] In Example 11, a spinneret was used in which 36 holes each of 0.18 mm and 0.23 mm diameters were drilled so that the fiber diameters would be 7.0 μm and 11.0 μm when the fibers were made, and the spinneret had small diameters corresponding to the thin fiber diameter and large diameters corresponding to the thick fiber diameter arranged on the spinneret surface. Figure 7 shows the arrangement of the spinneret's nozzle plate 16 used in Example 11, and a spinneret with a staggered hole arrangement was used in which a group of 0.18 mm diameter nozzles (7-(a)) and a group of 0.23 mm diameter nozzles (7-(b)) were alternately arranged. In Example 11, spinning and drawing were carried out in the same manner as in Example 1, except that the above-mentioned composite spinneret was used, and a stretch textured yarn of the present invention was obtained without carrying out false twisting.

[0176] Observation of the crimp morphology of the stretch processed yarn of Example 11 revealed that two types of latent crimps corresponding to the fiber diameter of the fiber were mixed, and the coil diameter distribution had two groups. Therefore, in the elongation-stress curve, these two types of crimps were deformed sequentially according to the elongation of the multifilament, so the rise in stress was gradual from the low elongation region to the high elongation region, and the elongation energy showed a high value of 3.2 μJ / dtex, providing suitable elongation resistance. When the stretch-processed yarn of Example 11 was used as a fabric and subjected to a relaxation process, the fabric exhibited good stretchability while having moderate stretch resistance from the low elongation region, resulting in excellent holdability and excellent movement followability. The results are shown in Table 2.

[0177] [Comparative Example 1] In Comparative Example 1, a drawn yarn (56 dtex-72 filament) was produced in the same manner as in Example 1, and then the actual twist in the twisting region was 5500 T / m (the false twist number was 40000 / Df 0.5 The false twisting process was carried out under the conditions of 56dex-72 filaments, maximum-minimum group average ratio 3.00, to obtain stretchable yarn. In the stretch-processed yarn of Comparative Example 1, the maximum-to-minimum coil diameter ratio was larger than that of the stretch-processed yarn of the present invention, so the elongation-stress curve of the stretch-processed yarn of Comparative Example 1 showed gradual deformation and a sudden rise in stress. Therefore, in the fabric made of the processed yarn of Comparative Example 1, resistance suddenly increased with elongation, so that when a large movement was made suddenly, there were parts that could not follow the movement, and a partial tightness was felt. The results are shown in Table 2.

[0178] [Comparative Example 2] In Comparative Example 2, spinning and drawing were carried out under the same conditions as in Example 1, and a stretch textured yarn of 56 dtex-72 filaments was obtained without false twisting. In the stretch textured yarn of Comparative Example 2, only one group due to latent crimp was observed in the coil diameter distribution, and the elongation-stress curve showed a monotonous profile as shown by the dotted line 3-(a) in Figure 3. Therefore, when made into a fabric, although it had good stretchability, it lacked resistance at low elongation, and from the viewpoint of good holding feeling and movement following ability over a wide range from low elongation to high elongation when the fabric was stretched, it was inferior to Example 1. The results are shown in Table 2.

[0179] [Comparative Example 3] In Comparative Example 3, polyethylene terephthalate (PET3) with a melt viscosity of 120 Pa s was melted, extruded from a spinneret with 72 extrusion holes, spun, and drawn to obtain a 56 dtex-72 filament PET monofilament. This was false twisted under the same conditions as in Example 1, except that the heater temperature was set to 200°C, to obtain a stretch-textured yarn. (56 dtex-72 filament) Observation of the crimp morphology of the stretch-processed yarn of Comparative Example 3 showed that the coil diameter distribution was broad and did not have the group defined in the present invention, and fibers with large coil diameters were slackly fixed to the surface of the stretch-processed yarn. As a result, the slack fibers did not bear the stress during elongation, and the elongation-stress curve of the stretch-processed yarn of Comparative Example 3 showed an extremely low stress during low elongation, and furthermore, the rise in stress after the crimp was fully elongated was abrupt. The results are shown in Table 2.

[0180] [Example 12] Polybutylene terephthalate (PBT, melt viscosity: 112 Pa s) was prepared as the first component polymer, and polyethylene terephthalate (PET, melt viscosity: 39 Pa s) was prepared as the second component polymer. The first component polymer and the second component polymer were both melted using an extruder at 260°C and 280°C, respectively, and then the spinning temperature was set to 280°C and metered using a pump so that the area ratio of the first component polymer to the second component polymer in the fiber cross section was 50 / 50. The mixture was then allowed to flow into the composite spinneret of this embodiment shown in Figures 12(a) to 12(c) and the hole packing density was adjusted to 1.2 x 10 -2 hole / mm 2The inlet polymer was discharged at 0.35 g / min / hole from the discharge holes arranged in the direction of the polymer spinning path as shown in Fig. 11(a), in which a group of polymer distribution holes was formed in the lowest layer on the downstream side in the direction of the polymer spinning path as shown in Fig. 11(a), in which a group of polymer distribution holes was formed, in which a group of polymer distribution holes was formed in a semicircular arrangement, with a group of second component polymer distribution holes surrounding a group of first component polymer distribution holes, and 8 of the 64 second component polymer distribution holes in the group of polymer distribution holes were arranged in a semicircular arrangement outside the circumference of the group of first component polymer distribution holes arranged in a semicircular arrangement.

[0181] The composite polymer stream discharged from the nozzle had a 36° discharge bending angle, indicating extremely good discharge stability, and the composite polymer stream was cooled and solidified, after which an oil agent was added, taken up at a spinning speed of 1000 m / min, and stretched 3.0 times between rollers heated to 80°C and 130°C to obtain a composite fiber of 56 dtex-48 filaments (single fiber fineness 1.2 dtex) through the spinning and stretching process. The number of yarn breakages during this spinning and stretching process was 0.3 times / 10 million m, indicating extremely good spinning stability.

[0182] The cross section of the composite fiber obtained was an eccentric core-sheath cross section as shown in Figure 11(b), in which the first component polymer was the core and the second component polymer was the sheath. The thickness ratio of the thin skin part was 4%, which was sufficiently thin, while the thickness variation of the thin skin part was 10%, so the composite cross section had high dimensional stability. In addition, the stretch extension ratio of the composite fiber was 65%, and it had extremely good crimp expression. The results are shown in Table 3.

[0183] [Comparative Example 4] The polymer stream was introduced into a conventional composite spinneret used for spinning composite fibers with a side-by-side cross section as shown in Figure 8(b), and the hole packing density was adjusted to the processing limit of 1.2 × 10 -2 hole / mm 2 The same procedure as in Example 12 was followed except that the inlet polymer was discharged from the discharge holes arranged at 0.35 g / min / hole, to obtain a 56 dtex-48 filament composite fiber. In the spinning and drawing process of the obtained composite fiber, the composite polymer stream discharged from the nozzle had a larger discharge bending than in Example 12. In addition, the polymer stream frequently swayed during spinning and broke due to contact with the spinneret surface. The results are shown in Table 3.

[0184] [Comparative Example 5] The polymer stream was introduced into a conventional composite spinneret used for spinning composite fibers with an eccentric core-sheath cross section, as shown in Figure 10(b), and the hole packing density was adjusted to the processing limit of 6.1 × 10 -3 hole / mm 2 The same procedure as in Example 12 was followed except that the inlet polymer was discharged from the discharge holes arranged at 0.35 g / min / hole, to obtain a 56 dtex-48 filament composite fiber. In the spinning and drawing process of the obtained composite fiber, the flow rate of the polymer forming the thin skin portion was extremely small, so that the polymer abnormally stayed in the flow path in the composite spinneret, and the degraded polymer was mixed in, resulting in frequent fiber breakage during drawing. In addition, the composite cross section of the obtained composite fiber had a large variation in the thickness of the thin skin portion compared to Example 12, and the dimensional stability of the composite cross section was poor. The results are shown in Table 3.

[0185] [Comparative Example 6] A composite fiber of 56 dtex-48 filaments was obtained in the same manner as in Example 12, except that a distribution plate for the composite spinning die was used in which the arrangement of the first component polymer distribution holes in the polymer distribution hole group formed in the lowermost layer on the downstream side in the polymer spinning path direction was a circular arrangement as shown in Figure 14(a). The obtained composite fiber had large crimp due to the center of gravity of the core component being close to the center of the cross section of the composite fiber, and the crimp expression was significantly reduced compared to Example 12. The results are shown in Table 3.

[0186] [Examples 13 and 14] A composite fiber of 56 dtex-48 filaments was obtained in the same manner as in Example 12, except that a distribution plate was used in which 6 holes (Example 13) or 4 holes (Example 14) of the 64 second component polymer distribution holes in a polymer distribution hole group drilled in the lowest layer on the downstream side in the polymer spinning path direction were arranged in a semicircular arrangement outside the circumference of the multiple first component polymer distribution holes arranged in a semicircular arrangement. In the obtained composite fiber, the fewer the number of second component polymer distribution holes arranged in a semicircular array, the farther the center of gravity of the core component was from the center of the composite fiber cross section, resulting in finer crimps, and the fiber had better crimp development than Example 12. The results are shown in Table 3.

[0187] [Examples 15 and 16] A composite fiber of 56 dtex-48 filaments was obtained in the same manner as in Example 12, except that a distribution plate for the composite spinning nozzle was used in which 12 holes (Example 15) or 16 holes (Example 16) of the 64 second component polymer distribution holes in the polymer distribution hole group drilled in the lowest layer on the downstream side in the polymer spinning path direction were arranged in a semicircular arrangement outside the circumference of the multiple first component polymer distribution holes arranged in a semicircular arrangement. The composite fiber obtained had an increased number of second component polymer distribution holes arranged in a semicircular array, and therefore the thickness of the thin skin portion increased compared to Example 12, and the discharge bending of the composite polymer stream discharged from the discharge hole was reduced. In addition, there was almost no yarn swaying of the polymer stream during spinning or yarn breakage due to contact with the spinneret surface. The results are shown in Table 3.

[0188] [Example 17] Hole filling density is 1.8×10 -2 hole / mm 2 The same procedure as in Example 12 was followed except that the inlet polymer was discharged from the discharge holes arranged at 0.23 g / min / hole, to obtain a composite fiber of 56 dtex-72 filaments. The obtained composite fiber had a finer single fiber, which resulted in a decrease in the stiffness of the yarn, and therefore the fabric using the composite fiber had good stretchability and excellent feel. The results are shown in Table 4.

[0189] [Comparative Example 7] The polymer stream was introduced into a conventional composite spinneret used for spinning composite fibers with a side-by-side cross section as shown in Figure 8(b), and the hole packing density was adjusted to the processing limit of 1.2 × 10 -2 hole / mm 2 Spinning was performed in the same manner as in Example 12, except that the inflow polymer was discharged from the nozzles arranged at 0.23 g / min / hole, and the discharge rate and gravity were reduced compared to Comparative Example 4, so that the discharge bending of the composite polymer stream discharged from the nozzles became worse, and the polymer stream constantly came into contact with the spinneret surface during spinning, making spinning impossible. The results are shown in Table 4.

[0190] [Comparative Example 8] The polymer stream was introduced into a conventional composite spinneret used for spinning composite fibers with an eccentric core-sheath cross section, as shown in Figure 10(b), and the hole packing density was adjusted to the processing limit of 6.1 × 10 -3 hole / mm 2 The same procedure as in Example 12 was followed except that the inlet polymer was discharged from the discharge holes arranged at 0.23 g / min / hole, to obtain a composite fiber of 56 dtex-72 filaments. In the spinning and drawing process of the obtained composite fiber, the flow rate of the polymer forming the thin skin portion was extremely low compared to Comparative Example 5, which resulted in abnormal retention of the polymer in the flow path inside the composite spinneret, and frequent yarn breakage during drawing due to the inclusion of degraded polymer. In addition, in the composite cross section of the obtained composite fiber, the thickness variation of the thin skin portion became larger, and the dimensional stability of the composite cross section was also significantly deteriorated. The results are shown in Table 4.

[0191] [Example 18] A 56 dtex-48 filament composite fiber was obtained in accordance with Example 12, except that the first component polymer was polybutylene terephthalate (PBT, melt viscosity: 218 Pa·s). In the obtained composite fiber, the first component polymer, which is a high shrinkage component, was highly oriented due to the increased viscosity ratio between the first component polymer and the second component polymer, and the shrinkage difference was enlarged, resulting in finer crimps, and the fiber had better crimp expression than Example 12. The results are shown in Table 4.

[0192] [Comparative Example 9] The first component polymer was polybutylene terephthalate (PBT, melt viscosity: 218 Pa s). The polymer flow was introduced into a conventional composite spinneret used for spinning composite fibers with a side-by-side cross section as shown in Figure 8(b). The hole packing density was adjusted to the processing limit of 1.2 × 10 -2 hole / mm 2 Spinning was performed in the same manner as in Example 12, except that the inflow polymer was discharged from the discharge holes arranged at 0.35 g / min / hole, and as a result, the viscosity ratio of the first component polymer to the second component polymer increased compared to Comparative Example 4, and the discharge bending of the composite polymer stream discharged from the discharge hole further deteriorated, and the polymer stream constantly came into contact with the spinneret surface during spinning, making spinning impossible. The results are shown in Table 4.

[0193] [Example 19] A 56 dtex-48 filament bicomponent fiber was obtained in accordance with Example 12, except that the first component polymer was polytrimethylene terephthalate (PTT melt viscosity: 109 Pa·s). The obtained composite fiber had good crimping properties under load because the first component polymer was changed from PBT to PTT, and when made into a fabric, it had high stretchability. The results are shown in Table 4.

[0194] [Example 20] A composite fiber of 56 dtex-48 filaments was obtained according to the procedure of Example 12, except that the first component polymer was polybutylene terephthalate copolymerized with 20% polyoxytetramethylene glycol (PBT copolymerized with 20% PTMG, melt viscosity: 410 Pa·s). The obtained composite fiber had a stronger elastic behavior because the first component polymer was changed from PBT to PTMG copolymer PBT, and when made into a fabric, it had a spandex-like stretchability. The results are shown in Table 4.

[0195] [Table 1]

[0196] [Table 2]

[0197] [Table 3]

[0198] [Table 4]

[0199] Although the present invention has been described in detail using specific embodiments, it is clear to those skilled in the art that various modifications and variations are possible without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2018-209024) filed on November 6, 2018, and a Japanese patent application (Patent Application No. 2018-209025) filed on November 6, 2018, and is incorporated by reference in its entirety. [Explanation of symbols]

[0200] M1, M2: Any adjacent peaks in the crimped form of the fibers constituting the stretch-processed yarn V1: The apex of the valley in the crimp morphology of the fibers that make up the stretch-textured yarn Dc: crimped coil diameter of the fibers that make up the stretch-processed yarn D: Fiber diameter 2-(a) and 2-(b): Examples of groups in the coil diameter distribution of fibers in stretch-processed yarn 3-(a): An example of the elongation deformation profile of a multifilament consisting of only one type of coil diameter 3-(b): An example of the elongation deformation profile of stretch-textured yarn 4-(a): The point at which the strength becomes 0.05 cN / dtex in the elongation deformation profile of the stretch-textured yarn 4-(b): The intersection point of a perpendicular line drawn from 4-(a) to the horizontal axis 5-(a), 5-(c): Fiber diameter distribution 5-(b), 5-(d): median fiber diameter 5-(e), 5-(f): Fiber diameter distribution width 6-(a): Among the arrangement of the discharge holes in the discharge plate of the die used in Example 10, the discharge hole group corresponding to the distribution hole group with a skin thickness of 0.04 6-(b): Among the arrangements of the discharge holes in the discharge plate of the die used in Example 10, the discharge hole group corresponding to the distribution hole group with a skin thickness of 0.09 A: Core component (first component polymer, high viscosity polymer) B: Sheath component (second component polymer, low viscosity polymer) G: Discharged polymer flow V1-V5: Velocity distribution of polymer inside the inlet W: Groove width a: Center of gravity of polymer A in the composite cross section of the fiber cross section c: Center point of the composite cross section of the fiber cross section S: Minimum thickness of polymer B in the composite cross section of the fiber cross section 1, 2, 3: Guide hole 4, 7: Inlet holes 5, 6: Flow path 8: nozzle outlet 9: First component polymer distribution hole 10: Second component polymer distribution hole 11: Circumscribing circle of polymer distribution hole group 12 : Straight line 13: Curve 14: Measuring plate 15 : Distribution plate 16: Discharge plate 17: Distribution groove 18 : Distribution hole 19: Discharge introduction hole 20 : Reduction hole 21: nozzle outlet 22a: Metering hole for first component polymer 22b: Metering hole for second component polymer

Claims

1. 1. A composite spinneret for discharging a composite polymer stream composed of a first component polymer and a second component polymer, comprising: the composite spinneret comprises a metering plate having a plurality of metering holes for metering each polymer component, one or more distribution plates each having a distribution hole for distributing each polymer component, and a discharge plate, a group of polymer distribution holes is formed in a downstream lowermost layer of the distribution plate in a polymer spinning path direction, the group of polymer distribution holes being arranged in a semicircular shape and including a plurality of first component polymer distribution holes surrounded by a plurality of second component polymer distribution holes; all of the first component polymer distribution holes in the polymer distribution hole group are arranged inside a semicircle obtained by dividing the circumscribing circle of the polymer distribution hole group into two equal parts and on a straight line constituting the semicircle, in the second component polymer distribution holes in the polymer distribution hole group, all of the second component polymer distribution holes in a semicircle including the first component polymer distribution holes are arranged in a semicircular array outside the circumference of the first component polymer distribution holes, A composite spinneret in which the total number of second component polymer distribution holes Ht and the number of second component polymer distribution holes arranged in a semicircular arrangement outside the circumferential portion of a plurality of first component polymer distribution holes arranged in a semicircular arrangement therein satisfy the following formula (1): 1 / 16<Ho / Ht<1 / 4...Formula (1)

2. A method for producing composite fibers using the composite spinneret of claim 1.

Citation Information

Patent Citations

  • JP1969002504B

  • Phenylpropylamine benzoic acid derivative

    JP1980027175A

  • Spinneret of conjugate spinning

    JP1990307905A

  • Latent crimping polyester conjugate fiber

    JP2000256918A

  • Method for producing soft stretch yarn

    JP2005113369A