Polyester resin, its manufacturing method and coating material

A polyester resin with biomass-derived components and a controlled carbon ratio, using a titanium catalyst, addresses brown coloration and poor solubility, offering improved environmental and safety profiles for light-colored applications.

JP7568063B2Active Publication Date: 2024-10-16MITSUBISHI CHEM CORP
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2023509128
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-09-22
Filing Date
2022-03-18
Publication Date
2024-10-16
Estimated Expiration
2042-03-18

AI Technical Summary

Technical Problem

Existing polyester resins face issues such as brown coloration, poor solvent solubility, and the use of environmentally harmful catalysts like organic tin, particularly when isosorbide is used, and the reliance on recycled PET without addressing broader environmental impacts.

Method used

A polyester resin composed of structural units derived from biomass-derived polyhydric alcohols and polyhydric carboxylic acids, with a carbon atom ratio of 5 to 40% from polyethylene terephthalate, and a methyl ethyl ketone insoluble content of 5% or less, using a titanium compound as a catalyst, and a production method involving esterification and transesterification reactions at elevated temperatures.

Benefits of technology

The resin achieves good solvent solubility, a light color, and reduced environmental impact, suitable for light-colored inks and paints, while minimizing petroleum-derived materials and shortening production time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568063000001
    Figure 0007568063000001
  • Figure 0007568063000002
    Figure 0007568063000002
Patent Text Reader

Abstract

The present invention is a polyester resin, including: a constituent unit derived from at least one of a biomass-derived polyhydric alcohol and a biomass-derived polyvalent carboxylic acid; and a constituent unit derived from polyethylene terephthalate. The ratio of carbon atoms derived from the polyethylene terephthalate with respect to 100% of the total carbon atoms is 5-40%, and a methyl ethyl ketone insoluble portion is 5 wt.% or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester resin, a production method thereof, and a coating material. This application claims priority to Patent Application No. 2021-047375, filed in Japan on March 22, 2021, and Patent Application No. 2021-154388, filed in Japan on September 22, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] Due to its excellent properties, polyester resin is used as a raw material for fibers and films, etc., and is also widely used as a binder resin for paints, inks, toners, etc. Recently, from the perspective of reducing CO2 emissions, technologies that use raw materials derived from biomass and recycled raw materials have been attracting attention.

[0003] For example, Patent Document 1 proposes a toner using a polyester resin copolymerized with biomass-derived isosorbide, and shows that a toner having good fixing properties, hot offset resistance, and storage stability can be obtained while reducing the environmental load. Patent Document 2 also presents a method of producing a polyester resin by introducing recycled PET into an apparatus together with other raw materials.

[0004] On the other hand, when isosorbide is used as a raw material for polyester resin, phenomena occur in which the polyester resin is easily colored brown and has poor solvent solubility. Regarding the color of polyester resin, for example, Patent Document 3 discloses an attempt to reduce the coloring of polyester resin using isosorbide by improving the catalyst. In addition, regarding the phenomenon of low solvent solubility, Patent Document 4 proposes a solvent-soluble polyester copolymerized with isosorbide. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-285555 A [Patent Document 2] JP 2002-155133 A [Patent Document 3] Special Publication No. 2017-533320 [Patent Document 4] JP 2010-095696 A Summary of the Invention [Problem to be solved by the invention]

[0006] Regarding the problem that the resin tends to turn brown during copolymerization with isosorbide, the brown color of the resin was not a problem because the technology in Patent Document 1 was evaluated for magenta, but it is unclear whether it can be used for light-colored applications. In addition, it is widely known that the catalyst used in the technology in Patent Document 3 is expensive, and other technologies are expected.

[0007] As for the low solvent solubility, in the technology of Patent Document 4, in order to dissolve in a general-purpose solvent such as methyl ethyl ketone (hereinafter also referred to as "MEK"), it is necessary to suppress the copolymerization amount of isosorbide to less than 30 mol% relative to 100 mol% of the total acid components used in copolymerization. Furthermore, only examples are shown in which organotin is used as a catalyst, which is of concern for its adverse effects on the human body and the environment, and no resin obtained without using the above catalyst is disclosed.

[0008] Furthermore, regarding the use of PET, the technology of Patent Document 2 uses organic tin or lead-containing catalysts, which are of concern for their adverse effects on the human body and the environment. When no catalyst is used, the production time is prolonged, and it is unclear whether resin can be obtained in a similarly short time when other catalysts that do not pose the above concerns are used. Furthermore, the technology of Patent Document 2 does not mention raw materials other than recycled polyethylene terephthalate, and there is room for consideration from the perspective of reducing the environmental load.

[0009] The present invention aims to provide a polyester resin which has good solvent solubility, excellent storage stability, and a light color and can be used in light-colored inks and paints, while taking into consideration environmental and safety aspects by reducing the amount of petroleum-derived raw materials used, as well as a production method thereof, paint, ink, adhesive, and image-forming material. [Means for solving the problem]

[0010] The present invention has the following aspects. [1] A polyester resin comprising a structural unit derived from at least one of a biomass-derived polyhydric alcohol and a biomass-derived polycarboxylic acid, and a structural unit derived from polyethylene terephthalate, wherein the ratio of carbon atoms derived from the polyethylene terephthalate to total carbon atoms (100%) is 5 to 40%, and the content of methyl ethyl ketone insoluble matter is 5 mass% or less. [2] The polyester resin according to [1], wherein the structural unit derived from the biomass-derived polyhydric alcohol is a structural unit derived from a polyhydric alcohol containing a heterocycle. [3] The polyester resin according to [1] or [2], wherein the biomass-derived polyhydric alcohol is at least one of isosorbide and erythritan. [4] The polyester resin according to any one of [1] to [3], wherein the structural unit derived from the biomass-derived polycarboxylic acid is a structural unit derived from a polycarboxylic acid containing a heterocycle. [5] The polyester resin according to any one of [1] to [4], wherein the biomass-derived polycarboxylic acid is at least one of succinic acid and 2,5-furandicarboxylic acid. [6] The polyester resin according to any one of [1] to [5], wherein a ratio of carbon atoms derived from the biomass-derived polyhydric alcohol and the biomass-derived polycarboxylic acid is 1 to 95% of the total carbon atoms contained in the polyester resin. [7] The polyester resin according to any one of [1] to [6], wherein the ratio of carbon atoms derived from the biomass-derived polyhydric alcohol, the biomass-derived polycarboxylic acid, and the polyethylene terephthalate is 6 to 100% relative to the total carbon atoms contained in the polyester resin. [8] The polyester resin according to any one of the items [1] to [8], wherein the polyester resin having a particle size of 1 to 2 mm is separated by sieving and measured with a spectrophotometer, whereby the L value is 40 or more and the a value is 2.4 or less. [9] A coating material comprising the polyester resin according to any one of [1] to [8] and a solvent.

[10] An ink comprising the polyester resin according to any one of [1] to [8].

[11] An adhesive material comprising the polyester resin according to any one of [1] to [8].

[12] An image-forming material comprising the polyester resin according to any one of [1] to [8].

[13] A method for producing a polyester resin, comprising: a reaction step, which is at least one of an esterification reaction and an ester exchange reaction, in which a raw material containing at least one of a biomass-derived polyhydric alcohol and a biomass-derived polycarboxylic acid, and polyethylene terephthalate is reacted in the presence of a titanium compound; and a polycondensation step of polycondensing a reaction product obtained in the reaction step, A method for producing a polyester resin, wherein a ratio of carbon atoms derived from the polyethylene terephthalate is 5 to 40% based on a total carbon atom amount of the raw materials, and at least a part of the reaction step is carried out at a temperature equal to or higher than a melting point of the polyethylene terephthalate.

[14] The method according to

[13] , wherein the biomass-derived polyhydric alcohol is a polyhydric alcohol containing a heterocycle.

[15] The method according to

[14] , wherein the biomass-derived polyhydric alcohol is at least one of isosorbide and erythritan.

[16] The method according to

[13] , wherein the biomass-derived polycarboxylic acid is a polycarboxylic acid containing a heterocycle.

[17] The method according to

[16] , wherein the biomass-derived polycarboxylic acid is at least one of succinic acid and 2,5-furandicarboxylic acid.

[18] The method according to any one of

[14] to

[17] , wherein the reaction step lasts for 3 hours or less.

[0011] As another aspect, the present invention has the following embodiment. [1-1] A polyester resin comprising a constitutional unit derived from polyethylene terephthalate and a constitutional unit derived from a polyhydric alcohol including isosorbide, wherein the ratio of carbon atoms derived from the polyethylene terephthalate is 5 to 40%, a methyl ethyl ketone insoluble matter is 5 mass% or less, an L value is 40 or more, and an a value is 2.4 or less. [1-2] The polyester resin according to [1-1], which contains a structural unit derived from a polyvalent carboxylic acid. [1-3] The polyester resin according to [1-1] or [1-2], wherein the ratio of carbon atoms derived from the isosorbide is 1 to 30% based on the total carbon atoms contained in the polyester resin. [1-4] The polyester resin according to any one of [1-1] to [1-3], wherein at least a portion of at least one of the constitutional units derived from the polyethylene terephthalate and the constitutional units derived from the polyhydric alcohol containing isosorbide is derived from biomass, and a ratio of the carbon atoms derived from the biomass is 1 to 95% of the total carbon atoms contained in the polyester resin. [1-5] The polyester resin according to [1-2] or [1-3], wherein at least a portion of at least one of the polyethylene terephthalate-derived structural units, the isosorbide-containing polyhydric alcohol-derived structural units, and the polyvalent carboxylic acid-derived structural units is derived from biomass, and the ratio of the carbon atoms derived from the biomass is 1 to 95% of the total carbon atoms contained in the polyester resin. [1-6] A paint comprising the polyester resin according to any one of [1-1] to [1-5] and a solvent. [1-7] A method for producing a polyester resin, comprising: an esterification step of reacting a raw material containing polyethylene terephthalate and a polyhydric alcohol containing isosorbide in the presence of a titanium compound; and a step of polycondensing a reaction product obtained in the esterification step, wherein a ratio of carbon atoms derived from the polyethylene terephthalate is 5 to 40% based on a total carbon atom amount of the raw material; and at least a part of the esterification step is carried out at a temperature equal to or higher than the melting point of the polyethylene terephthalate. [1-8] The method according to [1-7], wherein the raw material contains a polyvalent carboxylic acid. [1-9] The method according to [1-7] or [1-8], wherein the esterification step is carried out for 3 hours or less.

[0012] As another aspect, the present invention has the following embodiment. [2-1] A polyester resin comprising a constitutional unit derived from polyethylene terephthalate and a constitutional unit derived from a biomass-derived monomer, wherein a ratio of carbon atoms derived from the biomass-derived monomer to all carbon atoms constituting the polyester resin is 30.0 to 90.0%, and the biomass-derived monomer contains at least erythritane. [2-2] The polyester resin according to [2-1], wherein the ratio of carbon atoms derived from erythritan is 5.0 to 35.0% of the total carbon atoms constituting the polyester resin. [2-3] The polyester resin according to [2-1] or [2-2], wherein the ratio of carbon atoms derived from petroleum-derived monomers to the total carbon atoms constituting the polyester resin is 30.0% or less. [2-4] The polyester resin according to any one of [2-1] to [2-3], wherein the ratio of carbon atoms derived from the polyethylene terephthalate is 10.0 to 50.0% of the total carbon atoms constituting the polyester resin. [2-5] The polyester resin according to any one of [2-1] to [2-4], which has a glass transition temperature of 30 to 80°C. [2-6] A method for producing a polyester resin, comprising a step of reacting a raw material mixture containing polyethylene terephthalate and a biomass-derived monomer, wherein a ratio of carbon atoms derived from the biomass-derived monomer is 30.0 to 90.0% relative to the total carbon atoms of the raw material mixture, and the biomass-derived monomer contains at least erythritan. [2-7] The method for producing a polyester resin according to [2-6], wherein the ratio of carbon atoms derived from erythritan is 5.0 to 35.0% based on the total carbon atoms in the raw material mixture. [2-8] The method for producing a polyester resin according to [2-6] or [2-7], wherein the ratio of carbon atoms derived from petroleum-derived monomers to the total carbon atoms of the raw material mixture is 30.0% or less. [2-9] The method for producing a polyester resin according to any one of [2-6] to [2-8], wherein the ratio of carbon atoms derived from the polyethylene terephthalate is 10.0 to 50.0% based on the total carbon atoms of the raw material mixture. Effect of the Invention

[0013] According to the present invention, it is possible to provide a polyester resin having good solvent solubility and a light color that can be used in light-colored inks and paints, etc., a production method thereof, paints, inks, adhesives, and image-forming materials. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] [Polyester resin] The polyester resin of the first aspect of the present invention contains a structural unit derived from at least one of a biomass-derived polyhydric alcohol and a biomass-derived polycarboxylic acid, and a structural unit derived from polyethylene terephthalate (hereinafter also referred to as "PET"), in which the ratio of carbon atoms derived from the polyethylene terephthalate is 5 to 40% relative to 100% of all carbon atoms, and the methyl ethyl ketone insoluble matter is 5 mass% or less. The polyester resin according to one embodiment of the present invention is made from a mixture M containing PET, and at least one of a biomass-derived polyhydric alcohol component and a biomass-derived polycarboxylic acid component. In another aspect, the mixture M may contain PET, a biomass-derived polyhydric alcohol component that is at least one of isosorbide and erythritan, and a biomass-derived polycarboxylic acid component. That is, the polyester resin is a reaction product of the mixture M. At least a part of the monomers contained in the mixture M are biomass-derived monomers. The mixture M may contain a petroleum-derived monomer. The term "biomass-derived monomer" refers to a monomer produced using plants as a raw material. The carbon atoms constituting the biomass-derived monomer are derived from plants. "Petroleum-derived monomer" refers to a monomer produced using petroleum as a raw material, excluding PET and biomass-derived monomers. The carbon atoms constituting the petroleum-derived monomer are derived from petroleum.

[0015] <Polyethylene terephthalate> As the PET, for example, PET produced according to a conventional method such as esterification or transesterification of ethylene glycol with terephthalic acid, dimethyl terephthalate, or the like, and polycondensation can be used. As the PET, unused PET may be used, or recycled PET obtained by regenerating (i.e., recycling) used PET or PET products may be used. In addition, PET made from biomass-derived raw materials may be used, or A-PET (amorphous polyethylene terephthalate), C-PET (crystalline polyethylene terephthalate), or G-PET (glycol-modified polyethylene terephthalate) may be used.

[0016] The recycled PET may be used after processing used PET into pellets, or may be used after crushing products such as films and bottles or scraps. An example of PET using biomass-derived raw materials is PET in which at least one of ethylene glycol and terephthalic acid is derived from biomass. Whether or not PET uses biomass-derived raw materials can be confirmed, for example, by ASTM D6866 "Standard for determining biogenic carbon concentration using radiocarbon (C14) measurement method." From the viewpoint of environmental conservation, recycled PET or PET made from biomass-derived raw materials is preferred. The PET made from biomass-derived raw materials may be either unused or used. The PET may be used alone or in combination of two or more kinds.

[0017] The content of carbon atoms derived from PET, that is, the carbon atom ratio of carbon atoms derived from PET, is 5 to 40% relative to the total carbon atoms in the mixture M. PET is an ester bond between an ethylene skeleton derived from ethylene glycol and a benzene ring having a functional group at the para position derived from terephthalic acid or a lower alkyl ester thereof. Therefore, if PET is used as a part and polymerized together with a polyvalent carboxylic acid component and a polyhydric alcohol component, a random polymer is quickly formed by an ester exchange reaction. By making the ratio of carbon atoms derived from PET 5% or more relative to the total carbon atoms in the mixture M, it is possible to contribute to shortening the polymerization time and to suppress coloring of the resin due to heating during polymerization. In addition, by making the content of carbon atoms derived from PET 40% or less relative to the total carbon atoms in the mixture M, the solvent solubility of the resulting polyester resin is improved. The content of carbon atoms derived from PET is more preferably 30% or less relative to the total carbon atoms in the mixture M, and even more preferably 5 to 30%. The ratio of carbon atoms derived from PET to the total carbon atoms in mixture M can be calculated based on the number of carbon atoms and the molar ratio of each component constituting mixture M. The ratio of carbon atoms derived from isosorbide, the ratio of carbon atoms derived from erythritan, and the carbon atom ratio of biomass-derived monomers described below can also be calculated in the same manner.

[0018] The IV (intrinsic viscosity) value of the PET usable in the present invention is preferably 0.2 to 1.2, more preferably 0.3 to 1.1, further preferably 0.4 to 0.8, and most preferably 0.4 to 0.6, from the viewpoint of controlling the crystallinity of the resulting polyester resin. The IV value of PET was determined by dissolving 0.3 g of PET in 30 mL of a mixed solvent of phenol and 1,1,2,2-tetrachloroethane in a mass ratio of 1:1, and measuring the resulting solution at 30°C using an Ubbelohde viscometer.

[0019] <Biomass-derived polycarboxylic acid components> Examples of polyvalent carboxylic acids derived from biomass include divalent carboxylic acids and trivalent or higher carboxylic acids. Examples of divalent carboxylic acids include aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, and isomers of naphthalenedicarboxylic acid (specifically, 1,4-, 1,5-, 1,6-, 1,7-, 2,5-, 2,6-, 2,7-, and 2,8-), and lower alkyl esters or acid anhydrides thereof; and aliphatic dicarboxylic acids such as succinic acid, isodecyl succinic acid, dodecenyl succinic acid, maleic acid, fumaric acid, adipic acid, sebacic acid, 2,5-furandicarboxylic acid, and lower alkyl esters or acid anhydrides thereof. Examples of the lower alkyl esters of terephthalic acid and isophthalic acid include dimethyl terephthalate, dimethyl isophthalate, diethyl terephthalate, diethyl isophthalate, dibutyl terephthalate, and dibutyl isophthalate. Among these, the divalent carboxylic acid is preferably a polyvalent carboxylic acid containing a heterocycle.Furthermore, from the viewpoints of excellent handling properties and cost, terephthalic acid, isophthalic acid, adipic acid, 2,5-furandicarboxylic acid, and succinic acid are preferred, and 2,5-furandicarboxylic acid and succinic acid are more preferred. The divalent carboxylic acid may be used alone or in combination of two or more kinds thereof, and may also be used in combination with a trivalent or higher carboxylic acid described below.

[0020] Examples of trivalent or higher carboxylic acids include trimellitic acid, pyromellitic acid, 1,2,4-cyclohexanetricarboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,2,7,8-octanetetracarboxylic acid, and acid anhydrides and lower alkyl esters thereof. Among these, as the trivalent or higher carboxylic acid, trimellitic acid, trimellitic anhydride, pyromellitic acid, and pyromellitic anhydride are preferred from the viewpoints of excellent handling properties and cost, and trimellitic acid and its anhydride are particularly preferred. The trivalent or higher carboxylic acids may be used alone or in combination of two or more kinds.

[0021] <Biomass-derived polyhydric alcohol component> Examples of the polyhydric alcohol component derived from biomass include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, glycerin, isosorbide, isomannide, erythritan, sorbitol, erythritol, etc., and are preferably polyhydric alcohol components containing a heterocycle. The polyhydric alcohol component derived from biomass is more preferably at least one of isosorbide and erythritan.

[0022] Isosorbide includes D-isosorbide and L-isosorbide. The content of carbon atoms contained in the isosorbide-derived structural unit in the polyester resin is preferably 1 to 30% of the total carbon atoms contained in the polyester resin. Using 1% or more of carbon atoms contained in the isosorbide-derived structural unit is preferable in terms of reducing the environmental load, and has the effect of increasing the glass transition temperature (also called Tg) of the polyester resin. In addition, by making the carbon atoms contained in the isosorbide-derived structural unit 30% or less, the polyester resin tends to be less likely to be discolored and to have good solvent solubility. The content of carbon atoms contained in the isosorbide-derived structural unit is more preferably 5 to 25%.

[0023] The erythritan is preferably erythritan (1,4-anhydroerythritol), which is a biomass-derived monomer synthesized by an intramolecular dehydration reaction of erythritol, a natural polysaccharide.

[0024] The ratio of carbon atoms derived from erythritan in the polyester resin is preferably 5 to 35% relative to the total carbon atoms constituting the polyester resin. If the ratio of carbon atoms derived from erythritan is 5% or more, this is preferable in terms of reducing the environmental load, and also has the effect of increasing the glass transition temperature (also called Tg) of the polyester resin. If the ratio of carbon atoms derived from erythritan is 35% or less, the solvent solubility of the resulting polyester resin tends to be good. The ratio of carbon atoms derived from erythritan is more preferably 8 to 28% relative to the total carbon atoms constituting the polyester resin.

[0025] The polyhydric alcohol component may contain a dihydric alcohol other than isosorbide and erythritan (hereinafter also referred to as "other dihydric alcohol"), and a trihydric or higher alcohol (hereinafter also referred to as "other trihydric alcohol"). Other dihydric alcohols include, for example, aliphatic alcohols such as ethylene glycol, neopentyl glycol, propylene glycol, hexanediol, polyethylene glycol, 1,3-propanediol, 1,4-butanediol, diethylene glycol, triethylene glycol, 1,4-cyclohexanedimethanol, isomannide, and 1,4-dihydroxy-2-butene, for example, polyoxypropylene-(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.2)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.3)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.4)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.5)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.6)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.7)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.8)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.9)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.10)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.11)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.12)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.13)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.14)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.15)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.16)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene-(2.17)-2,2-bis(4- Aromatic alcohols such as propylene-(2.4)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(3.3)-2,2-bis(4-hydroxyphenyl)propane, polyoxypropylene(6)-2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene-(2.0)-2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene-(2.2)-2,2-bis(4-hydroxyphenyl)propane, polyoxyethylene-(2.3)-2,2-bis(4-hydroxyphenyl)propane, and polyoxypropylene(2.2)-polyoxyethylene-(2.0)-2,2-bis(4-hydroxyphenyl)propane, and the like. The other dihydric alcohols may be used alone or in combination of two or more kinds, and may be derived from petroleum or biomass. The number in parentheses after "ethylene" is the average number of moles of ethylene oxide added, and the number in parentheses after "propylene" is the average number of moles of propylene oxide added.

[0026] Examples of trihydric or higher alcohols include trimethylolpropane, sorbitol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, 2-methyl-1,2,3-propanetriol, 2-methyl-1,2,4-butanetriol, 1,3,5-trihydroxymethylbenzene, and glycerin. The other trihydric or higher alcohols may be used alone or in combination of two or more kinds, and may be derived from petroleum or biomass.

[0027] From the viewpoint of reducing the environmental load, the ratio of carbon atoms derived from biomass-derived monomers in the polyester resin is preferably 1 to 95% relative to the total carbon atoms contained in the mixture M. If the ratio of carbon atoms derived from biomass-derived monomers is 1% or more, the effect of reducing the amount of petroleum-derived monomers used can be enhanced. Furthermore, if the ratio of carbon atoms derived from biomass-derived monomers is 95% or less, the storage stability and solvent solubility of the resulting polyester resin tend to be good. The ratio of carbon atoms derived from biomass is preferably 1 to 95% relative to the total carbon atoms contained in the polyester resin, and may be 2 to 85%, or may be 3 to 70%.

[0028] Furthermore, from the viewpoint of reducing the environmental load, the ratio of carbon atoms derived from the biomass-derived polyhydric alcohol, the biomass-derived polycarboxylic acid, and the polyethylene terephthalate to the total carbon atoms contained in the polyester resin is preferably 6 to 100%, and more preferably 10 to 100%.

[0029] <Other ingredients> The mixture M may contain components (hereinafter also referred to as other components) other than PET, the polyvalent carboxylic acid component, and the polyhydric alcohol component. That is, the polyester resin may contain structural units derived from other components. Examples of other components include monovalent carboxylic acids, monovalent alcohols, and monoesters of monovalent carboxylic acids and monovalent alcohols. Examples of monovalent carboxylic acids include aromatic carboxylic acids having 30 or less carbon atoms, such as benzoic acid and p-methylbenzoic acid; aliphatic carboxylic acids having 30 or less carbon atoms, such as stearic acid and behenic acid; and unsaturated carboxylic acids having one or more double bonds in the molecule, such as cinnamic acid, oleic acid, linoleic acid, and linolenic acid. Examples of monohydric alcohols include aromatic alcohols having 30 or less carbon atoms, such as benzyl alcohol; and aliphatic alcohols having 30 or less carbon atoms, such as oleyl alcohol, lauryl alcohol, cetyl alcohol, stearyl alcohol, and behenyl alcohol. Examples of the monoester of a monohydric alcohol and a monocarboxylic acid include natural ester waxes such as carnauba wax and rice wax. The other components may be derived from petroleum or biomass, but are more preferably derived from biomass.

[0030] <Physical Properties> The polyester resin of the present embodiment has an MEK insoluble content of 5% by mass or less. The lower the MEK insoluble content, the more preferable, and the most preferable is 0% by mass. If the MEK insoluble content is 5% by mass or less, the suitability for solvent-based inks, paints, etc. and for use in solvents is increased. Even if the polyester resin is processed into an emulsion and used as a water-based ink or paint binder, etc., solvent solubility is essential when emulsifying using a phase inversion emulsification method, etc., and a content of 5% by mass or less increases suitability.

[0031] The polyester resin according to the first aspect of the present invention preferably has an L value of 40 or more and an a value of +2.4 or less. Here, the L value and the a value are Hunter Lab values ​​obtained by separating polyester resin particles having a particle size of 1 to 2 mm by sieving and measuring the L value and the a value with a spectrophotometer (e.g., CM-5 manufactured by Konica Minolta) at a field of view of 2°. The L value indicates lightness and ranges from black (0) to white (100). The higher the value, the higher the lightness. The a-value takes a positive value when the color is red and a negative value when the color is green. The polyester resin according to the first aspect of the present application is a resin that has high brightness and suppresses reddish tinge, even when copolymerized with isosorbide, which tends to turn brown.

[0032] It is preferable that the polyester resin of the present invention be dissolved in MEK to give a solid content of 30% by mass, and that it be dissolved in MEK to give a solid content of 40% by mass, both of which become homogeneous solutions. If a homogeneous MEK solution is obtained, it will be more suitable for use in solvent-based inks, paints, etc., and in applications where it is dissolved in a solvent. Even if it is assumed that polyester resins are processed into emulsions for use as water-based inks and paint binders, etc., solvent solubility is essential when emulsifying using the phase inversion emulsification method, etc., and emulsification suitability will be improved. A homogeneous solution means a state in which no separation of liquid phases is observed when the solution is allowed to stand, and no or only a very small amount of precipitate is observed.

[0033] From the viewpoint of storage stability of the polyester resin, the Tg of the polyester resin is preferably 30° C. or higher, more preferably 40° C. or higher, and even more preferably 50° C. or higher. From the viewpoint of ease of melting, the Tg of the polyester resin is preferably 100° C. or lower, and may be 80° C. or lower. The upper and lower limits of the preferred range of the Tg of the polyester resin can be arbitrarily combined. For example, the Tg of the polyester resin is preferably 30 to 100° C. The glass transition temperature of the polyester resin is determined as follows: A differential scanning calorimeter (e.g., "DSC60 Plus" manufactured by Shimadzu Corporation) is used to measure at a temperature rise rate of 5°C / min, and the temperature at the intersection between the baseline on the low temperature side of the chart and the tangent to the endothermic curve near the glass transition temperature is determined, and this is taken as the glass transition temperature.

[0034] The softening temperature (also referred to as T4) of the polyester resin is preferably 80°C or higher, more preferably 90°C or higher, and even more preferably 100°C or higher, from the viewpoint of the storage stability of the resin. Also, from the viewpoint of ease of melting, it is preferably 170°C or lower, and more preferably 150°C or lower. The upper and lower limits of T4 of the polyester resin can be arbitrarily combined. For example, T4 of the polyester resin is preferably 90 to 170°C, more preferably 90 to 170°C, and even more preferably 100 to 150°C.

[0035] The softening temperature of the polyester resin is determined as follows: using a flow tester (e.g., Shimadzu Corporation's "CFT-500D"), a nozzle of 1 mmφ×10 mm is used to measure the temperature at a constant rate of temperature rise of 3° C. / min under a load of 294 N (30 kgf), and the temperature at which half of 1.0 g of polyester resin flows out is measured, and this is taken as the softening temperature.

[0036] The acid value (AV) of the polyester resin is preferably 1 to 40 mgKOH / g, more preferably 3 to 30 mgKOH / g. If the acid value of the polyester resin is equal to or higher than the lower limit, the productivity of the polyester resin is improved. If the acid value of the polyester resin is equal to or lower than the upper limit, the moisture resistance of the polyester resin is improved, and the polyester resin is less susceptible to the effects of the usage environment. If the acid value of the polyester resin is in the range of approximately 6 to 15 mgKOH / g, neutralization phase inversion emulsification becomes possible, and the polyester resin is suitable for use as an emulsion.

[0037] The acid value of a polyester resin is the amount of potassium hydroxide required to neutralize the carboxyl groups per 1 g of sample, expressed in milligrams, and is expressed in mgKOH / g. The acid value of the polyester resin is a value obtained by dissolving the polyester resin in benzyl alcohol and titrating it with a 0.02N KOH solution using cresol red as an indicator.

[0038] The hydroxyl value (OHV) of the polyester resin is preferably 10 to 70 mgKOH / g, more preferably 10 to 50 mgKOH / g. If the hydroxyl value of the polyester resin is equal to or higher than the lower limit, the productivity of the polyester resin is improved. If the hydroxyl value of the polyester resin is equal to or lower than the upper limit, the moisture resistance of the polyester resin is improved and the polyester resin is less susceptible to the effects of the usage environment.

[0039] The hydroxyl value of a polyester resin is the amount of potassium hydroxide in milligrams equivalent to the number of hydroxyl groups per gram of sample, and is expressed in mgKOH / g. The hydroxyl value of the polyester resin is a value calculated from the amount of acetic anhydride consumed by dissolving the polyester resin in tetrahydrofuran, reacting the polyester resin with acetic anhydride in the presence of dimethylaminopyridine to acetylate the hydroxyl groups, hydrolyzing the excess acetic anhydride to acetic acid, and then titrating the resulting solution with a 0.5 N KOH solution using phenolphthalein as an indicator.

[0040] When the polyester resin is used as an emulsion, the particle size of the emulsion after phase inversion emulsification is preferably 50 to 500 nm, more preferably 60 to 300 nm. When the particle size of the emulsion after phase inversion emulsification is 50 to 500 nm, the stability of the emulsion tends to be good, and the emulsion can be suitably used for water-based inks and coatings.

[0041] The particle size of the emulsion is measured using an emulsion obtained by the following phase inversion emulsification method. In a glass beaker, the polyester resin is dissolved in MEK in an amount three times the amount of the polyester resin, and a base is added to the beaker in an amount capable of neutralizing 100% or more of the carboxylic acid of the polyester resin, and the mixture is thoroughly mixed. As the base, ammonia water, dimethylaminoethanol, sodium hydroxide, potassium hydroxide, etc. can be appropriately used. Next, pure water in an amount four times the amount of the polyester resin is charged into a round-bottom flask, and the above MEK solution is charged thereto and treated with a homogenizer at 8000 rpm for 10 minutes. Next, a flask cover, stirring blades, and a cooling tube were attached, and the flask was heated to 70°C in a water bath while reducing the pressure with an aspirator to distill off the MEK, obtaining an emulsion consisting only of water and resin. The particle size of the emulsion was measured using a laser diffraction / scattering type particle size distribution measuring device (LA-960, manufactured by Horiba, Ltd.), and the median diameter (D 50 (also called "particle size") is defined as the particle size of the emulsion.

[0042] <Method of producing polyester resin> The second aspect of the present invention is a method for producing a polyester resin, comprising a reaction step, which is at least one of an esterification reaction and an ester exchange reaction, in which a raw material containing at least one of a biomass-derived polyhydric alcohol and a biomass-derived polycarboxylic acid, and polyethylene terephthalate is reacted in the presence of a titanium compound, and a polycondensation step of polycondensing the reaction product obtained in the reaction step, wherein the ratio of carbon atoms derived from the polyethylene terephthalate is 5 to 40% based on the total carbon atoms of the raw material, and at least a part of the reaction step is carried out at a temperature equal to or higher than the melting point of polyethylene terephthalate. Hereinafter, an example of a method for producing a polyester resin according to the second aspect of the present invention will be described. The method for producing a polyester resin according to this embodiment includes a step of reacting a mixture M, which is a raw material containing at least one of the above-mentioned biomass-derived polyhydric alcohol and biomass-derived polycarboxylic acid, and polyethylene terephthalate. The ratio of carbon atoms derived from PET to the total carbon atom amount of the mixture M, i.e., the raw material, is 5 to 40%.

[0043] The ratio of carbon atoms derived from biomass-derived monomers in mixture M to the total carbon atoms derived from mixture M is preferably 1 to 95%, more preferably 2 to 85%, and even more preferably 3 to 70%. The ratio of carbon atoms derived from PET in the mixture M to the total carbon atoms derived from the mixture M is more preferably 5 to 30%. When raw material mixture M contains erythritan, the ratio of carbon atoms derived from erythritan to the total carbon atoms derived from raw material mixture M is preferably 5 to 35%, and more preferably 8 to 28%.

[0044] When raw material mixture M contains isosorbide, the ratio of carbon atoms derived from isosorbide to the total carbon atoms derived from raw material mixture M is preferably 1 to 30%, and more preferably 5 to 25%.

[0045] In the step of reacting the mixture M, it is preferable to carry out at least one of an esterification reaction and an ester exchange reaction, followed by a polycondensation reaction. Specifically, the mixture M and a catalyst such as a titanium compound are charged into a reaction vessel, heated to raise the temperature, and at least one of an esterification reaction and an ester exchange reaction is carried out, and water or alcohol generated by the reaction is removed. Thereafter, the polycondensation reaction is carried out. At this time, the pressure inside the reaction vessel is gradually reduced, and the polycondensation is carried out while distilling and removing the polyhydric alcohol component under a pressure of 150 mmHg (i.e., 20 kPa) or less, preferably 15 mmHg (i.e., 2 kPa) or less, to produce a polyester resin.

[0046] In the polyester resin production method according to the second embodiment of the present invention, only titanium-based compounds are used as catalysts in the esterification reaction or transesterification reaction and polycondensation reaction from the viewpoint of safety. Examples of titanium-based compounds include titanium alkoxide compounds having an alkoxy group, titanium carboxylates, titanyl carboxylates, titanyl carboxylate salts, and titanium chelate compounds.

[0047] Examples of titanium alkoxide compounds having an alkoxy group include tetramethoxytitanium, tetraethoxytitanium, tetrapropoxytitanium, tetrabutoxytitanium, tetrapentoxytitanium, and tetraoctoxytitanium. Examples of the carboxylate titanium compound include titanium formate, titanium acetate, titanium propionate, titanium octanoate, titanium oxalate, titanium succinate, titanium maleate, titanium adipate, titanium sebacate, titanium hexanetricarboxylate, titanium isooctanetricarboxylate, titanium octanetetracarboxylate, titanium decanetetracarboxylate, titanium benzoate, titanium phthalate, titanium terephthalate, titanium isophthalate, titanium 1,3-naphthalenedicarboxylate, titanium 4,4-biphenyldicarboxylate, titanium 2,5-toluenedicarboxylate, titanium anthracenedicarboxylate, titanium trimellitate, titanium 2,4,6-naphthalenetricarboxylate, titanium pyromellitate, and titanium 2,3,4,6-naphthalenetetracarboxylate. Among these, titanium tetrabutoxide is particularly preferred due to its availability. The above catalysts may be used alone or in combination of two or more kinds.

[0048] The polymerization temperature in the esterification reaction or the ester exchange reaction is higher than the melting point of PET from the viewpoint of shortening the reaction time. The melting point of PET is around 255°C. The polymerization temperature in the esterification reaction or the ester exchange reaction is preferably 260°C or higher, more preferably 265°C or higher. The upper limit of the polymerization temperature in the esterification reaction or the ester exchange reaction is preferably 290°C or lower, more preferably 280°C or lower. The polymerization temperature in the polycondensation reaction is preferably 180 to 280°C, more preferably 200 to 270°C, and particularly preferably 210°C to 255°C. If the polymerization temperature in the polycondensation reaction is equal to or higher than the lower limit, the productivity of the polyester resin is improved. If the polymerization temperature is equal to or lower than the upper limit, the decomposition of the polyester resin and the by-production of volatile matter that causes odor can be suppressed, and TVOC (Total Volatile Organic Compounds) can be reduced.

[0049] In the second embodiment of the present invention, the esterification reaction and / or transesterification reaction time is preferably 3 hours or less. During the esterification reaction and / or transesterification reaction, water, lower alcohol, etc. are distilled from the reaction system as the reaction proceeds, and the "esterification reaction and / or transesterification reaction time" refers to the time from when the distillate starts to come out to when the distillate is completed. The end point of polymerization is determined, for example, by the softening temperature of the polyester resin. For example, the polymerization may be terminated after the polycondensation reaction is carried out until the torque of the stirring blade reaches a value indicating the desired softening temperature. Here, "terminating the polymerization" refers to stopping the stirring in the reaction vessel and introducing nitrogen into the reaction vessel to make the pressure in the vessel normal. The polycondensation reaction time refers to the time from the time when the reaction system is heated to the polycondensation reaction temperature and pressure reduction is started to the time when the polymerization is completed. After cooling, the resulting polyester resin may be pulverized to a desired size.

[0050] <Action and effect> The polyester resin according to the first aspect of the present invention described above is a polyester resin that is environmentally and safely friendly by reducing the amount of petroleum-derived raw materials used, has good solvent solubility, and is light in color, and can therefore be used in applications such as light-colored inks and paints.

[0051] Moreover, the polyester resin of the first aspect of the present invention uses PET as a part of the raw material. Since PET already contains a structural unit derived from ethylene glycol, the polyester resin of the first aspect of the present invention can reduce the amount of ethylene glycol used as a raw material monomer. Ethylene glycol is a VOC (Volatile Organic Compounds), and if unreacted ethylene glycol remains in the polyester resin, the ethylene glycol volatilizes when heat is applied, causing odor. However, the polyester resin of the first aspect of the present invention can reduce the amount of ethylene glycol used, thereby reducing TVOC and suppressing odor. In addition, since ethylene glycol as a monomer does not generally remain in PET, VOC derived from PET is unlikely to be generated.

[0052] The polyester resin according to the first aspect of the present invention can be widely used in solvent-based inks and paints, water-based inks and paints, powder paints, toners, solvent-based liquid developers, water-based developers, adhesives, and image-forming materials.

[0053] According to the method for producing a polyester resin of the second aspect of the present invention, it is possible to easily produce a polyester resin that has good solvent solubility and a light color, while taking into consideration environmental and safety aspects by reducing the amount of petroleum-derived raw materials used. Furthermore, since PET is used as one of the raw materials for the polyester resin, the PET serves as the starting point for esterification and transesterification reactions, which makes it easier to proceed, thereby shortening the reaction time. EXAMPLES

[0054] The present invention will be specifically described below with reference to examples, although the present invention is not limited to the following examples.

[0055] [Measurement and evaluation method] The methods for measuring and evaluating the polyester resins shown in the examples are as follows.

[0056] <Measurement of glass transition temperature and evaluation of storage stability> The glass transition temperature of the polyester resin was measured using a differential scanning calorimeter (Shimadzu Corporation, "DSC-60") from the intersection of the baseline of the chart and the tangent of the endothermic curve at a heating rate of 5°C / min. The measurement sample was weighed out to 10 mg ± 0.5 mg in an aluminum pan, melted at 100°C for 10 minutes, and then rapidly cooled using dry ice. Furthermore, based on the measurement results, the storage stability was evaluated according to the following criteria. (Evaluation Criteria) ◎: Tg is 50°C or higher. ◯: Tg is 30°C or higher and less than 50°C. ×: Tg is less than 30°C.

[0057] <Measurement of softening temperature> The softening temperature of the polyester resin was measured using a flow tester (Shimadzu Corporation, "CFT-500D") with a nozzle of 1 mmφ×10 mm, a load of 294 N, and a constant heating rate of 3°C / min, at the time when half of a 1.0 g resin sample flowed out. This was taken as the softening temperature.

[0058] <Acid value measurement> The acid value of the polyester resin was measured as follows. Approximately 0.2 g of the measurement sample was precisely weighed into an Erlenmeyer flask with a sidearm (a(g)), 20 mL of benzyl alcohol was added, and the sample was dissolved by heating for 15 minutes at 230°C under a nitrogen atmosphere. After cooling to room temperature, 20 mL of chloroform and a few drops of cresol red solution were added, and titration was performed with 0.02N KOH solution (titer amount = b (mL), titer of KOH solution = p). A blank measurement was performed in the same manner (titer amount = c (mL)), and the acid value was calculated according to the following formula. Acid value (mgKOH / g)={(bc)×0.02×56.11×p} / a

[0059] <Measurement of hydroxyl value> The hydroxyl value of the polyester resin was measured as follows. Approximately 5 g of the measurement sample was precisely weighed into an Erlenmeyer flask (a(g)), 50 mL of tetrahydrofuran was added, and the mixture was stirred and dissolved with a stirrer. Next, 30 mL of a solution prepared by dissolving 5.000 g of dimethylaminopyridine in tetrahydrofuran to adjust the volume to 500 mL was added to the Erlenmeyer flask. Next, 10 mL of a mixture of 22 mL of acetic anhydride and 200 mL of tetrahydrofuran was added, and the mixture was stirred for 15 minutes to acetylate. Next, 5 mL of distilled water was added, and the mixture was stirred for 15 minutes to hydrolyze the excess acetic anhydride to acetic acid. After adding 50 mL of tetrahydrofuran, several amounts of phenolphthalein were added, and the mixture was titrated with a 0.5N KOH solution (titer amount = b (mL), KOH titer = p). A blank measurement was performed in the same manner (titer amount = c (mL)), and the hydroxyl value was calculated according to the following formula. Hydroxyl value (mgKOH / g) = {(cb) x 0.5 x 56.11 x p} / a + acid value

[0060] <Evaluation of color difference> Using a spectrophotometer CM-5 (Konica Minolta), the L value and a value of the polyester resin were determined under the following conditions. Resin used: Sieved to particles with a particle size of 1 to 2 mm Measurement conditions: Measurement using a small petri dish Measurement type: Petri dish measurement Measurement diameter: Φ3mm for small petri dishes SCI / SCE:SCE Observation conditions Color system: Hunter Lab ΔE Field of view: 2° Main light source:C Secondary Light Source: None ·Measurement method The resin was filled into a small petri dish, and measurements were taken four times by rotating the dish by 90° each time. The measurement results were averaged to determine the L value and a value.

[0061] <Molecular weight measurement> The molecular weight of the polyester resin was determined by the GPC method in terms of polystyrene under the following conditions. Equipment: Tosoh Corporation, HLC8020 Column: Tosoh Corporation, TSKgel GMHXL (column size: 7.8 mm (ID) × 30.0 cm (L)), three columns connected in series Oven temperature: 40℃ Eluent: tetrahydrofuran (THF) Sample concentration: 20mg / 10mL Filtration conditions: Filter the sample solution through a 0.45 μm Teflon membrane filter. Flow rate: 1mL / min Injection volume: 0.1mL Detector: RI Standard polystyrene sample for creating calibration curve: TSK standard, A-500 (molecular weight 5.0 × 10) manufactured by Tosoh Corporation 2 ), A-2500 (molecular weight 2.74×10 3 ), F-2 (molecular weight 1.96×10 4 ), F-20 (molecular weight 1.9×10 5), F-40 (molecular weight 3.55×10 5 ), F-80 (molecular weight 7.06×10 5 ), F-128 (molecular weight 1.09×10 6 ), F-288 (molecular weight 2.89×10 6 ), F-700 (molecular weight 6.77×10 6 ), F-2000 (molecular weight 2.0×10 7 ).

[0062] [Example 1] <Production of polyester resin> For 100 mole parts of the acid component, 34 mole parts (159.2 g) of PET-1, 60 mole parts (242.9 g) of terephthalic acid, 6 mole parts (28.1 g) of trimellitic anhydride, 65 mole parts (570.1 g) of polyoxypropylene-(2.3)-2,2-bis(4-hydroxyphenyl)propane, 20 mole parts (71.2 g) of isosorbide, and 500 ppm (0.215 g) of tetrabutoxytitanium as a catalyst relative to the acid component were charged into a reaction vessel equipped with a distillation column. In addition, PET-1 is defined as a unit consisting of 1 mole of terephthalic acid and 1 mole of ethylene glycol, and for each mole of PET-1, terephthalic acid derived from PET was counted as 1 mole of acid component, and ethylene glycol derived from PET was counted as 1 mole of alcohol component. The isosorbide used was made from biomass-derived raw materials.

[0063] Next, the rotation speed of the stirring blade in the reaction vessel was kept at 200 rpm, and heating was started so that the temperature in the reaction system reached 265°C, and this temperature was maintained to carry out the esterification reaction. The esterification reaction was terminated when water no longer distilled from the reaction system. The time from when water began to be discharged from the reaction system to when the esterification reaction was completed is shown in Table 1 as "esterification reaction time and / or transesterification reaction time."

[0064] Next, the temperature in the reaction system was lowered to 235°C, the pressure in the reaction vessel was reduced for about 20 minutes, and the degree of vacuum was set to 133 Pa to carry out the polycondensation reaction. The viscosity of the reaction system increased with the reaction, and the degree of vacuum was increased with the increase in viscosity, and the condensation reaction was carried out until the torque of the stirring blade reached a value indicating the desired softening temperature. Then, when a predetermined torque was indicated, the stirring was stopped, the reaction system was returned to normal pressure, and the reaction product was removed from the reaction vessel by pressurizing with nitrogen, to obtain a polyester resin. The time required for the polycondensation reaction (i.e., the polycondensation reaction time) is shown in Table 1 as "polycondensation reaction".

[0065] The glass transition temperature, softening temperature, acid value, L value, a value and MEK insoluble content of the obtained polyester resin were measured, and the results are shown in Table 1 as Tg, T4, AV, L, a and MEK insoluble content, respectively. The polyester resin obtained in Example 1 contains constituent units derived from terephthalic acid, constituent units derived from trimellitic anhydride, constituent units derived from polyoxypropylene-(2.3)-2,2-bis(4-hydroxyphenyl)propane, constituent units derived from isosorbide, and constituent units derived from ethylene glycol, and the ratio of each constituent unit is roughly consistent with the charged composition. That is, the polyester resin obtained in Example 1 contained 14.1% of carbon atoms derived from PET and 5.0% of carbon atoms derived from isosorbide.

[0066] [Examples 2 to 6, Comparative Examples 1 to 2] <Production of polyester resin> A polyester resin was produced in the same manner as in Example 1, except that the charge composition, esterification reaction time and / or transesterification reaction time, and polycondensation reaction time were changed to those shown in Table 1, and various measurements and evaluations were performed. In Example 5, in addition to isosorbide, succinic acid, propylene glycol, and glycerin derived from biomass were used. The results are shown in Table 1. In Example 6, PET-2, a recycled polyethylene terephthalate with an IV value of 0.73, which was made by regenerating used PET containing a small amount of structural units derived from isophthalic acid, was used instead of PET-1.

[0067] [Example 7] <Production of polyester resin> 20 molar parts (100.0 g) of PET-1, 30 molar parts (129.7 g) of isophthalic acid, 50 molar parts (153.6 g) of succinic acid, 40 molar parts (79.2 g) of propylene glycol, 45 molar parts (121.9 g) of erythritan, and 500 ppm (0.192 g) of tetrabutoxytitanium as a catalyst relative to the acid component were charged into a reaction vessel equipped with a distillation column. The raw material mixture M charged into the reaction vessel in Example 7 contained 100 parts by mole of the acid component and 105 parts by mole of the alcohol component. Among the monomers, succinic acid, propylene glycol, and erythritan were derived from biomass.

[0068] Next, the rotation speed of the stirring blade in the reaction vessel was kept at 200 rpm, and heating was started so that the temperature in the reaction system reached 265° C., and the esterification reaction was carried out while maintaining this temperature. When water no longer distilled from the reaction system, the esterification reaction was terminated.

[0069] Next, the temperature in the reaction system was lowered to 235°C, the pressure in the reaction vessel was reduced for about 20 minutes, and the degree of vacuum was set to 133 Pa to carry out the polycondensation reaction. The viscosity of the reaction system increased with the reaction, and the degree of vacuum was increased with the increase in viscosity, and the condensation reaction was carried out until the torque of the stirring blade reached a value indicating the desired softening temperature. Then, the stirring was stopped at the point where a predetermined torque was indicated, the reaction system was returned to normal pressure, and the reaction product was removed from the reaction vessel by pressurizing with nitrogen to obtain a polyester resin.

[0070] The glass transition temperature, softening temperature, acid value, L value, a value, MEK insoluble content, hydroxyl value, weight average molecular weight, number average molecular weight, and weight average molecular weight / number average molecular weight of the obtained polyester resin were measured. These results are shown in Table 2 as Tg, T4, AV, L, a, MEK insoluble content, OHV, Mw, Mn, and Mw / Mn, respectively. The polyester resin obtained in Example 7 contains constituent units derived from terephthalic acid, constituent units derived from isophthalic acid, constituent units derived from succinic acid, constituent units derived from propylene glycol, constituent units derived from erythritan, and constituent units derived from ethylene glycol, and the ratio of each constituent unit is roughly consistent with the charged composition. That is, the polyester resin obtained in Example 7 contained 21.3% of carbon atoms derived from PET, 19.1% of carbon atoms derived from erythritan, 53.2% of carbon atoms derived from biomass-derived monomers containing erythritan, and 25.5% of carbon atoms derived from petroleum-derived raw materials, relative to the total carbon atoms constituting the polyester resin.

[0071] [Examples 8 to 11, Comparative Examples 1 and 2] <Production of polyester resin> A polyester resin was produced in the same manner as in Example 7, except that the charging composition, the esterification reaction time and / or the ester exchange reaction time, and the polycondensation reaction time were changed to those shown in Table 2, and various measurements and evaluations were carried out. The results are shown in Table 2.

[0072] <Production of emulsions (phase inversion emulsification process)> The polyester resins obtained in Examples 4, 9 and 10 were subjected to the production of emulsions. In a 200 ml beaker, 25 g of polyester resin was dissolved in 75 g of MEK, and dimethylaminoethanol was added to the beaker in an amount sufficient to neutralize 120% of the carboxylic acid in the polyester resin, and the mixture was thoroughly mixed. Next, 100 ml of pure water was placed in a 300 ml round-bottom flask, and the above MEK solution was added thereto, and the mixture was treated with a homogenizer at 8000 rpm for 10 minutes. Next, a flask cover, stirring blades and a cooling tube were attached, and MEK was distilled off by reducing the pressure with an aspirator while heating to 70°C in a water bath, to obtain an emulsion consisting of only water and resin. The particle size of the obtained emulsion was measured using a laser diffraction / scattering type particle size distribution measuring device (LA-960, manufactured by Horiba, Ltd.), and the median diameter was taken as the particle size of the emulsion. Table 1 shows the particle size of the emulsion using the polyester resin of Example 4, and Table 2 shows the particle size of the emulsion using the polyester resin of Examples 9 and 10.

[0073] [Table 1]

[0074] [Table 2]

[0075] The abbreviations in Tables 1 and 2 are as follows: Furthermore, a blank in the monomer composition column in the tables means that the component is not blended (amount blended: 0 mass % or 0 parts by mole). ·TPA: Terephthalic acid ·IPA: Isophthalic acid TMA: Trimellitic anhydride ·Bio-ScA: Biomass-derived succinic acid Bio-FDCA: Biomass-derived 2,5-furandicarboxylic acid BPP: Polyoxypropylene-(2.3)-2,2-bis(4-hydroxyphenyl)propane Bio-EG: Biomass-derived ethylene glycol Bio-PG: Biomass-derived Propylene Glycol (1,2-Propanediol): Biomass-derived Bio-GLY: Biomass-derived glycerin Bio-isosorbide: Biomass-derived isosorbide, PSA grade manufactured by Rocket Bio-erythritan: Erythritan derived from biomass PET-1: Recycled polyethylene terephthalate with an IV value of 0.57, made from recycled PET. ·PET-2: Recycled polyethylene terephthalate with an IV value of 0.73, made from recycled PET containing a small amount of isophthalic acid-derived structural units. The IV value of PET was measured by dissolving 0.3 g of PET in 30 mL of a mixed solvent of phenol and 1,1,2,2-tetrachloroethane in a mass ratio of 1:1, and measuring the resulting solution at 30° C. using an Ubbelohde viscometer.

[0076] As is clear from Tables 1 and 2, the polyester resins obtained in each Example were polyester resins that were derived from petroleum-derived monomers and had a low carbon atom ratio, reducing the environmental impact, and had good solvent solubility, high brightness, and low redness. It was also confirmed that emulsions could be obtained by phase inversion emulsification. Such polyester resins are also suitable for use in water-based inks and coatings.

[0077] On the other hand, the polyester resin of Comparative Example 1, which did not use PET, underwent a long esterification reaction and / or transesterification reaction time, and was a resin with a strong reddish color. The polyester resin of Comparative Example 2, which used a large amount of PET, had poor solvent solubility. [Industrial Applicability]

[0078] The polyester resin of the present invention is a polyester resin having good solvent solubility and a light color while taking into consideration environmental and safety aspects, and is therefore useful for light-colored inks and paints.

Claims

1. The polyester resin comprises a structural unit derived from at least one of a biomass-derived polyhydric alcohol and a biomass-derived polycarboxylic acid, and a structural unit derived from polyethylene terephthalate, the ratio of carbon atoms derived from the polyethylene terephthalate being 5 to 40% relative to 100% of all carbon atoms, a methyl ethyl ketone insoluble matter being 5 mass% or less, and the polyester resin is thermoplastic.

2. The polyester resin according to claim 1 , wherein the structural unit derived from the biomass-derived polyhydric alcohol is a structural unit derived from a polyhydric alcohol containing a heterocycle.

3. The polyester resin according to claim 1 or 2, wherein the biomass-derived polyhydric alcohol is at least one of isosorbide and erythritan.

4. The polyester resin according to any one of claims 1 to 3, wherein the structural unit derived from the biomass-derived polycarboxylic acid is a structural unit derived from a polycarboxylic acid containing a heterocycle.

5. The polyester resin according to any one of claims 1 to 4, wherein the biomass-derived polycarboxylic acid is at least one of succinic acid and 2,5-furandicarboxylic acid.

6. The polyester resin according to any one of claims 1 to 5, wherein a ratio of carbon atoms derived from the biomass-derived polyhydric alcohol and the biomass-derived polycarboxylic acid is 1 to 95% with respect to a total carbon atoms contained in the polyester resin.

7. The polyester resin according to any one of claims 1 to 6, wherein a ratio of carbon atoms derived from the biomass-derived polyhydric alcohol, the biomass-derived polycarboxylic acid, and the polyethylene terephthalate is 6 to 100% relative to the total carbon atoms contained in the polyester resin.

8. The polyester resin according to any one of claims 1 to 7, wherein the polyester resin having a particle size of 1 to 2 mm is separated by sieving and measured with a spectrophotometer to have an L value of 40 or more and an a value of 2.4 or less.

9. A coating material comprising the polyester resin according to any one of claims 1 to 8 and a solvent.

10. An ink comprising the polyester resin according to any one of claims 1 to 8.

11. An adhesive material comprising the polyester resin according to any one of claims 1 to 8.

12. An image-forming material comprising the polyester resin according to any one of claims 1 to 8.

13. A method for producing a polyester resin, comprising: a reaction step, which is at least one of an esterification reaction and an ester exchange reaction, in which a raw material containing at least one of a biomass-derived polyhydric alcohol and a biomass-derived polycarboxylic acid, and polyethylene terephthalate is reacted in the presence of a titanium compound; and a polycondensation step of polycondensing a reaction product obtained in the reaction step, a ratio of carbon atoms derived from the polyethylene terephthalate to a total carbon atom amount of the raw material is 5 to 40%, and at least a part of the reaction step is carried out at a temperature equal to or higher than a melting point of the polyethylene terephthalate; The method for producing a polyester resin, wherein the polyester resin is thermoplastic.

14. The method according to claim 13, wherein the biomass-derived polyhydric alcohol is a polyhydric alcohol containing a heterocycle.

15. The method according to claim 14, wherein the biomass-derived polyhydric alcohol is at least one of isosorbide and erythritan.

16. The method according to claim 13, wherein the biomass-derived polycarboxylic acid is a polycarboxylic acid containing a heterocycle.

17. The method according to claim 16, wherein the biomass-derived polycarboxylic acid is at least one of succinic acid and 2,5-furandicarboxylic acid.

18. The method according to any one of claims 14 to 17, wherein the reaction step is performed for 3 hours or less.

Citation Information

Patent Citations

  • Process for producing polyester resin

    JP2002155133A

  • Soluble copolyester resin

    JP2010095696A

  • Method for producing industrial polyester fiber

    JP2010280995A

  • Method for producing polyester resin, polyester resin for toner, and toner

    JP2010285555A

  • Polyester for covering

    JP2013510917A