Polyester resin molded products, recycled molded products, and their manufacturing method

A laminated polyester resin structure with a water-soluble anchoring agent and barrier layer maintains transparency and recyclability, addressing thermal decomposition issues in PET materials, enhancing gas barrier properties and reducing waste.

JP7568383B2Active Publication Date: 2024-10-16RISU PACK CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2017173259
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2017-09-08
Publication Date
2024-10-16
Estimated Expiration
2037-09-08

AI Technical Summary

Technical Problem

Current high-barrier PET materials, when extruded like regular PET, thermally decompose into gels, preventing recycling and increasing disposal costs and environmental burden, while lacking transparency studies in packaging applications.

Method used

A laminated polyester resin structure comprising a polyester base sheet, a water-soluble polyester anchoring agent layer, and a barrier layer, ensuring a haze value of 90 to 110, which maintains transparency and allows recycling.

Benefits of technology

The laminated structure provides gas barrier properties and transparency comparable to new PET, enabling recycling and reducing waste, thus lowering disposal costs and environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568383000001
    Figure 0007568383000001
  • Figure 0007568383000002
    Figure 0007568383000002
  • Figure 0007568383000003
    Figure 0007568383000003
Patent Text Reader

Abstract

To provide a polyester-based resin molded article excellent in transparency and recyclability, and a manufacturing method therefor.SOLUTION: The molded article is a molded article of a sheet in which a polyester-based substrate sheet layer, and an anchor layer and a barrier layer on at least one surface of a polyester-based substrate sheet layer laminated in this order, in which the anchor agent layer is a layer formed by a water-soluble ester-based anchor agent, a haze value is 90 to 110 as a relative value when the haze value of a molded article of a sheet consisting of only the polyester-based substrate sheet layer is 100. The manufacturing method of the molded article contains a process for manufacturing a recycled molded article by molding the molded body or a recycle polyester-based resin derived from the sheet, and a haze value of the recycled molded article is 90 to 110 as a relative value when the haze value of the molded article of the sheet consisting of only the polyester-based substrate sheet layer is 100.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyester resin molded article having excellent transparency and recyclability, a recycled molded article, and a method for producing the same. [Background technology]

[0002] Polyester resins, such as polyethylene terephthalate (hereinafter referred to as "PET"), have excellent chemical and physical properties. In addition, polyester resins have excellent mechanical strength and transparency, and are therefore widely used in packaging containers such as beverage bottles, films, sheets, and the like.

[0003] Packaging containers, particularly food and beverage packaging containers, may require gas barrier properties to prevent the contents (beverages, foods, etc.) to be stored therein from being adversely affected by gases such as oxygen or water vapor in the air, or to prevent loss of moisture during long-term storage. Conventionally, gas barrier films in which a barrier layer is formed on a resin film substrate have been developed to improve gas barrier properties. Such a barrier layer is usually formed on the surface of the resin film substrate via an anchor agent (AC agent). For example, Patent Document 1 describes a gas barrier film in which a barrier layer containing montmorillonite or the like is formed on the surface of a PET substrate sheet via an AC agent containing a silane coupling agent.

[0004] In recent years, the consumption of polyester resins has increased, and therefore, from the viewpoints of cost reduction and reduction of the burden on the environment, reuse of polyester resins has been promoted. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-1242 A Summary of the Invention [Problem to be solved by the invention]

[0006] Current high-barrier PET, which has improved gas barrier properties, is laminated with ethylene-vinyl alcohol copolymer (EVAL) and non-oriented polypropylene film (CPP). However, this high-barrier PET gels due to thermal decomposition when extruded under the same conditions as PET, so it cannot be crushed and recycled like regular PET and must be disposed of.

[0007] As described above, transparency is required when using a resin film for a packaging container, etc. However, although Patent Document 1 considers the transparency of the sheet, it does not disclose any technical findings regarding the transparency of the container.

[0008] An object of the present invention is to provide a polyester resin molded article and a recycled molded article which are excellent in transparency and recyclability, and a method for producing the same. [Means for solving the problem]

[0009] The polyester-based resin molded product of the present invention is a sheet molded product comprising a polyester-based base sheet layer and, on at least one side of the polyester-based base sheet layer, an anchor agent layer and a barrier layer laminated in this order, wherein the anchor agent layer is a layer formed from a water-soluble polyester-based anchor agent, and the molded product has a haze value of 90 to 110 relative to the haze value of a sheet molded product consisting only of the polyester-based base sheet layer, which is taken as 100.

[0010] The recycled molded product of the present invention is a recycled molded product made of recycled polyester resin derived from the molded product of the present invention or the sheet, and is characterized in that the haze value of the recycled molded product is 90 to 110, expressed as a relative value when the haze value of a molded product made of a sheet consisting only of the polyester base sheet layer is taken as 100.

[0011] The method for producing a recycled molded product of the present invention is characterized by comprising a step of producing a recycled molded product by molding a recycled polyester resin derived from the molded product or the sheet of the present invention. Effect of the Invention

[0012] The molded article of the present invention has gas barrier properties and transparency equivalent to that of a PET molded article. Therefore, the molded article of the present invention can be suitably used in applications requiring transparency, such as packaging containers for food and beverages. In addition, the recycled molded article of the present invention has transparency equivalent to that of a molded article obtained using new materials. Therefore, the molded article of the present invention can be crushed and recycled in the same way as ordinary PET. As a result, according to the present invention, the amount and cost of disposal of molded articles can be reduced, and the burden on the environment can be reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The following describes an embodiment of the present invention. The embodiment is merely an example of implementing the present invention, and the present invention is not limited to the embodiment.

[0014] (1) Polyester resin molded products The polyester-based resin molded article according to the present embodiment (hereinafter referred to as "the molded article") is a molded article of a sheet in which a polyester-based base sheet layer, an anchor agent layer and a barrier layer are laminated in this order on at least one side of the polyester-based base sheet layer, the anchor agent layer being a layer formed by a water-soluble polyester-based anchor agent, and the haze value of the molded article is 90 to 110 as a relative value when the haze value of a molded article of a sheet consisting of only the polyester-based base sheet layer is taken as 100. The molded article of the present embodiment has excellent transparency by suppressing whitening after container molding. In addition, as described later, a molded article obtained by reusing the molded article of the present embodiment has the same physical properties and transparency as a molded article obtained using a new material. Therefore, the molded article of the present embodiment can be reused in the same way as ordinary PET.

[0015] The polyester resin constituting the polyester-based base sheet (hereinafter simply referred to as "base sheet") layer is not limited in its specific structure and type as long as it is a polycondensation product of a polycarboxylic acid or its derivative (ester, anhydride, etc.) and a polyalcohol. A dicarboxylic acid is usually used as the polycarboxylic acid, and a diol is usually used as the polyalcohol. For example, an aromatic polycarboxylic acid can be used as the polycarboxylic acid. The polyester resin may be a polycondensation product of the polycarboxylic acid or its derivative and the polyalcohol, or may be a copolymer copolymerized with another monomer, for example, a monomer having a vinyl group such as styrene. The polyester resin may also be a polyester resin modified with another resin (for example, an epoxy resin).

[0016] Specific examples of the polyester resin include polyethylene terephthalate (PET), polypropylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, polyethylene-1,2-bis(phenoxy)ethane-4,4'-dicarboxylate, and polycyclohexylene dimethylene terephthalate. PET is preferred as the polyester resin.

[0017] The polyester resin may be either crystalline or amorphous. The polyester resin is preferably an amorphous polyester resin, more preferably an amorphous PET. The term "amorphous PET" includes PET in an uncrystallized state such as A-PET and PET in a completely uncrystallized state such as PET-G. The term "amorphous PET" is preferably PET in an uncrystallized state such as A-PET.

[0018] The anchor agent (hereinafter referred to as "AC agent") layer is formed on at least one side of the base sheet layer by the AC agent, and is a layer that bonds the base sheet layer and the barrier layer. The AC agent is a water-soluble polyester-based AC agent. In this molded product, by using the AC agent, whitening (reduction in transparency) after container molding can be suppressed.

[0019] The water-soluble polyester-based AC agent is not particularly limited in its specific structure as long as the polyester resin is dissolved or dispersed in the aqueous medium and can bond the base sheet layer and the barrier layer. As described above, the water-soluble polyester-based AC agent includes not only the case where the polyester resin is dissolved in the aqueous medium, but also the case where the polyester resin is dispersed in the aqueous medium as an emulsion or the like. The aqueous medium is water or a mixed medium of water and an alcohol (e.g., C1-C4 alcohol).

[0020] The polyester resin contained in the water-soluble polyester-based AC agent may be a saturated polyester resin or an unsaturated polyester resin. The polyester resin is preferably a polyester resin having a hydroxyl group or a carboxyl group at the molecular end. Specific examples of the polyester resin include polyacrylic acid ester and ethylene-acrylic acid ester copolymer. Commercially available water-soluble polyester anchor agents include, for example, water-soluble polyesters such as "Pluscoat Z-687" and "Pluscoat Z-880" manufactured by GOO Chemical Industry Co., Ltd.

[0021] When forming the AC agent layer, the water-soluble polyester-based AC agent may be used alone or in combination of two or more. Also, the water-soluble polyester-based AC agent may be used alone or in combination with other anchoring agents within a range that does not impair the effects of the present invention.

[0022] The AC agent layer can be usually formed by applying the AC agent to the surface of the base sheet layer and then drying it. The method and conditions for the application and drying are not particularly limited, and known methods can be used. Specific examples of the application method include ordinary wet coating methods such as gravure coating. Specific examples of the drying method include hot air drying and infrared irradiation.

[0023] The coating amount of the AC agent is not particularly limited as long as it can bond the barrier layer and the base sheet layer. The coating amount can be set to an appropriate range depending on the type of the AC agent and the configurations of the barrier layer and the base sheet layer. Specifically, the coating amount is, for example, 0.05 to 5 g / m2 in terms of solid content. 2 , preferably 0.1 to 2 g / m 2 When the coating amount is within the above range, excellent adhesion can be obtained and the drying time can be shortened, which is preferable.

[0024] The barrier layer is laminated on the outside of the AC agent layer (the surface of the AC agent layer that is not in contact with the base sheet layer) and is not particularly limited in its specific configuration as long as it has gas barrier properties. Specific examples of materials constituting the barrier layer include thin films of resins, metal oxides (aluminum oxide, silicon oxide, magnesium oxide, etc.) or inorganic compounds (nitrides such as aluminum nitride and silicon nitride, carbides such as silicon carbide). The barrier layer is preferably a barrier layer formed of a resin. There is no particular limitation on the type of the resin. Specific examples of the resin include polyvinylidene chloride resins, polyvinyl alcohol resins, and ethylene-vinyl alcohol copolymers.

[0025] The barrier layer may contain other components. When the barrier layer is a barrier layer formed of a resin, the other components may specifically include, for example, layered inorganic compounds. Examples include layered minerals and silicates. By containing layered silicates, gas barrier properties can be improved, which is preferable. Specific examples of the layered silicates include hydrated silicates (phyllosilicate minerals, etc.), kaolinite clay minerals (halloysite, kaolinite, endelite, dickite, nacrite, etc.), antigorite clay minerals (antigorite, chrysotile, etc.), smectite clay minerals (montmorillonite, beidellite, nontronite, saponite, hectorite, sauconite, stevensite, etc.), vermiculite clay minerals (vermiculite, etc.), mica or mica clay minerals (muscovite, phlogopite, etc. mica, margarite, tetrasilylic mica, taeniolite, etc.). These may be natural minerals or synthetic substances. The layered inorganic compound may be used alone or in combination of two or more thereof. The layered inorganic compound is preferably a layered silicate, and more preferably montmorillonite.

[0026] There is no particular limitation on the method for forming the barrier layer. The barrier layer can be formed by a known method according to the type of material constituting the barrier layer. When the barrier layer is a barrier layer formed of a resin, it can be formed by applying a resin solution or dispersion (which may contain the layered inorganic compound in the medium as necessary) to the surface of the AC agent layer and then drying it. There is no particular limitation on the method and conditions for the application and drying, and known methods can be used. Specific examples of the application method include ordinary wet coating methods such as gravure coating. Specific examples of the drying method include hot air drying and infrared irradiation.

[0027] The sheet may have other layers as necessary. For example, in order to improve waterproofness, a waterproof protective layer may be provided on the outside of the barrier layer (the surface of the barrier layer that is not in contact with the AC agent layer). There is no particular limitation on the type of the waterproof protective layer. Specific examples of the waterproof protective layer include a protective layer based on an acrylic resin.

[0028] There is no particular limitation on the method for producing the sheet. The sheet can usually be produced by applying and drying an AC agent on the surface of the polyester resin constituting the base sheet layer to form the AC agent layer, and then applying and drying a barrier agent on the outside of the AC agent layer to form the barrier layer.

[0029] There is no particular limitation on the thickness of the sheet and each layer constituting the sheet. The thickness of these layers can be appropriately determined as necessary. The thickness of the sheet is usually 0.5 to 1.5 mm. The thickness of the base sheet layer is usually 0.1 to 1 mm.

[0030] Each layer constituting the sheet may contain other components as necessary within a range that does not significantly impair transparency and recyclability. For example, the base sheet layer may contain other resins other than polyester resin. Specific examples of the other components include additives used in known resin sheets, such as flame retardants, ultraviolet absorbers, fluorescent whitening agents, antistatic agents, antifogging agents, lubricants, antiblocking agents, flow improvers, plasticizers, dispersants, and antibacterial agents.

[0031] The molded product is obtained by molding the sheet. There is no particular limitation on the molding method. The molding method includes known molding methods generally used for polyester resins, specifically, for example, vacuum molding (plug-assist molding, etc.), injection molding, ultra-high-speed injection molding, injection compression molding, two-color molding, gas-assisted hollow molding, molding using a heat-insulating mold, molding using a rapid heating mold, foam molding (including supercritical fluid), insert molding, IMC (in-mold coating molding) molding, extrusion molding, sheet molding, thermoforming, rotational molding, lamination molding, press molding, and blow molding. There is no particular limitation on the molding conditions. The molding conditions can be appropriately determined as needed.

[0032] The haze value of the present molded article is 90 to 110, preferably 92 to 108, and more preferably 95 to 105, relative to the haze value of the molded article consisting of only the base sheet layer, which is set to 100. The "haze value of the molded article consisting of only the base sheet layer is 90 to 110" means a relative value of 90 to 110, relative to the haze value of the molded article obtained by the same method as the present molded article, except that a sheet consisting of only the base sheet layer is used instead of the sheet. The haze value is a value measured in accordance with JIS K 7136. As long as the above conditions are met, there is no particular limitation on the specific range of the haze value of the present molded article. The haze value of the present molded article is usually 10% or less, preferably 8% or less, and more preferably 5% or less.

[0033] There are no particular limitations on the shape, dimensions, and specific uses of the molded article. Uses of the molded article include containers such as packaging containers, for example, food and beverage packaging containers. The term "container" includes not only the entire container, but also a part of the container. For example, the term "container" includes not only the main body of the container, but also the lid of the container.

[0034] (2) Recycled molded products and their manufacturing methods The recycled molded product according to the present embodiment (hereinafter referred to as "the present recycled molded product") is a recycled molded product of the present molded product or the recycled polyester resin derived from the sheet, and the haze value of the recycled molded product is 90 to 110 as a relative value when the haze value of a molded product of a sheet consisting of only the polyester base sheet layer is set to 100. In addition, the manufacturing method of the recycled molded product according to the present embodiment (hereinafter referred to as "the present method") includes a step of manufacturing a recycled molded product by molding the present molded product or the recycled polyester resin derived from the sheet. The present recycled molded product has physical properties (for example, IV value and strength such as bending elastic modulus and tensile elastic modulus) and transparency equivalent to those of a molded product obtained using new material. In addition, in the present method, the recycled polyester resin can be recycled in the same way as ordinary PET. As a result, the load on the environment is reduced by reducing the amount of waste material, and the production cost of polyester resin can be reduced, which is preferable.

[0035] The recycled polyester resin is not particularly limited in its preparation method as long as it is derived from the present molded product or the sheet. The recycled polyester resin can be prepared, for example, by crushing the present molded product or the sheet. In addition, the recycled polyester resin can be, for example, waste material derived from the present molded product or the sheet (for example, waste material from container molding) generated in a factory when manufacturing the present molded product or the sheet.

[0036] There is no particular limitation on the method of producing the present recycled molded product by molding the recycled polyester resin. Usually, the recycled polyester resin or other resins and / or other components as necessary are kneaded using a general kneader, roll, mixer or extruder, and then a resin sheet is produced by a known molding method such as extrusion molding, injection molding, calendar molding, blow molding, vacuum molding, and pressure molding, and the resin sheet is molded, for example, by the molding method exemplified in the section on the present molded product, to produce the present recycled molded product. There is no particular limitation on the specific conditions (for example, temperature, time) in each of these steps. The conditions can be appropriately determined as needed.

[0037] In the present recycled molded product and the present method, in addition to the recycled polyester resin, other resins and / or other components may be used as necessary. For example, polyester resin, particularly new polyester resin (virgin polyester resin), can be used as the other resin. In addition, other components described in the section on the present molded product can be used as the other components. When the other resins are used in combination, there is no particular limitation on the ratio of the recycled polyester resin to the other resins. For example, the ratio of the recycled polyester resin to the total of the recycled polyester resin and the other resins (100% by mass) can be 10 to 70% by mass.

[0038] The haze value of the present recycled molded product is 90 to 110, preferably 92 to 108, and more preferably 95 to 105, relative to the haze value of the molded product consisting of only the base sheet layer, which is set to 100. The "haze value of 90 to 110 of the molded product consisting of only the base sheet layer" means a relative value of 90 to 110, relative to the haze value of a molded product obtained by the same method as the present recycled molded product, except that a sheet consisting of only the base sheet layer is used. The haze value is a value measured in accordance with JIS K 7136. As long as the above conditions are met, there is no particular limitation on the specific range of the haze value of the present recycled molded product. The haze value of the present recycled molded product is usually 10% or less, preferably 8% or less, and more preferably 5% or less.

[0039] The recycled molded product is obtained by molding the recycled polyester resin, and there is no particular limitation on its specific structure as long as the haze value satisfies the above range. The recycled molded product may have a single layer structure or a multi-layer structure including two or more layers. There is also no particular limitation on the shape, dimensions, and specific use of the recycled molded product. The explanation in the section on the molded product applies to these. EXAMPLES

[0040] The present invention will be specifically described below with reference to examples. Note that the present invention is not limited to the embodiments shown in the examples. The embodiments of the present invention can be modified in various ways within the scope of the present invention depending on the purpose, application, etc.

[0041] 1. Evaluation of transparency and gas barrier properties of molded products (1) Container manufacturing <Example> The following components were used as raw materials. The IV value (dl / g) of the following "(A)A-PET" was measured in accordance with JIS K 7367-5. A mixed solvent of phenol / 1,1,2,2-tetrachloroethane (weight ratio 3 / 1) was used as the solvent. (A) A-PET: PET resin "YS-H01" manufactured by Hainan Yisheng Petrochemical Co., Ltd., China (IV value = 0.78 dl / g, thickness 0.85 mm) (B) Water-soluble polyester-based AC agent: "Pluscoat Z-687" and "Pluscoat Z-880" manufactured by GOO Chemical Co., Ltd. When used, the AC agent was diluted with a diluent (isopropyl alcohol:water = 2:1 by mass) (AC agent:diluent = 16:84 by mass). (C) Barrier agent: "EXCEIER" (containing montmorillonite) manufactured by Sumitomo Chemical Co., Ltd. (D) Protective agent: "Stypri" manufactured by Osaka Printing Ink Co., Ltd. When used, the protective agent was diluted with a diluent (styrene) (protective agent:diluent=1:1 by mass).

[0042] The A-PET was subjected to a corona discharge treatment, and then the AC agent, barrier agent, and protective agent were applied in this order to the corona discharge treated surface of the A-PET using a gravure plate (6-zone printing machine), and dried to produce a sheet having an AC agent layer, a barrier layer, and a protective layer. Specific application and drying conditions are shown in Table 1.

[0043] [Table 1]

[0044] The sheet obtained by the above method was thermoformed by vacuum pressure forming to produce a container (container size: 200mm x 100mm x 30mm). Specifically, a convex resin mold called a plug was used in combination, and a part of the resin sheet softened by heating was pressed with the plug, giving the resin sheet the internal shape of the container corresponding to the external shape of the plug, and then the bottom and side parts of the container were formed by adhering it to the cavity mold by vacuum drawing. The upper heater temperature in the vacuum pressure forming was 375°C, and the lower heater temperature was 395°C.

[0045] <Comparative Example 1> Containers were manufactured in the same manner as in the Examples, except that a polyethyleneimine-based AC agent ("AD-372MW" manufactured by Toyo-Morton and "Seikadyne 4100" manufactured by Dainichi Seikagaku Kagaku Co., Ltd.) was used instead of the AC agent used in the Examples, and the dilution ratio of the AC agent to the diluent was changed from 1:6 ("AD-372MW":diluent) and 1:9 ("Seikadyne 4100":diluent) to 1:9.

[0046] <Comparative Example 2> A container was produced in the same manner as in the example, except that a sheet made of A-PET in the example was used in place of the sheet in the example.

[0047] (2) Performance evaluation The haze value and oxygen permeability of the containers of the Example and Comparative Examples 1 and 2 were measured by the following methods. The haze value of the sheets produced in Example 1 and Comparative Example 1 and the A-PET was also measured. The results are shown in Table 2 below.

[0048] (I) Haze value Measurements were performed in accordance with JIS K 7136.

[0049] (II) Oxygen permeability The measurement was performed using an oxygen transmission rate measuring device (manufactured by Illinois Corporation, "8001") in accordance with JIS K7126 Method A. The measurement was performed in an atmosphere at 23°C.

[0050] [Table 2]

[0051] From Table 2, in Comparative Example 1, in which a polyethyleneimine-based AC agent was used as the AC agent, clouding of the sheet and container was observed, and transparency was reduced. On the other hand, the haze value of the container of the Example was 4.03%, which was 90 to 110 in relative terms when the haze value of the A-PET molded product (Comparative Example 2) was taken as 100, and the container maintained a similar level of transparency. In addition, the oxygen transmission rate of the container of the Example was 0.06 cc / pack / day, and the container had better gas barrier properties than the A-PET molded product (Comparative Example 2). From these results, it can be seen that the container of the Example is superior in transparency and gas barrier properties compared to Comparative Examples 1 and 2.

[0052] 2.Recyclability evaluation (1) Manufacturing of recycled sheets The waste material generated during the molding of the container of the above-mentioned embodiment was crushed to prepare crushed PET as a recycled polyester resin. In addition to the crushed PET, the following components were used as raw materials for the recycled sheet. (A) A-PET (new material): PET resin "YS-H01" manufactured by Hainan Yisheng Petrochemical Co., Ltd., China, used in the above examples (B) Lubricant MB: "RE555" manufactured by Toyobo Co., Ltd. (a fine particle-containing polyester resin obtained by mixing 7000 ppm of spherical silica having an average particle size of 2.4 μm with a polyester resin having an intrinsic viscosity of 0.62 dl / g during polymerization; see JP 2008-30282 A) (C) Black pigment; "APET-BK-3216" manufactured by Nikko Bicks Co., Ltd.

[0053] A mixture for forming a surface layer was prepared by mixing 94% by mass of A-PET (new material) and 6% by mass of lubricant MB. The crushed PET, A-PET (new material), and black pigment were mixed in the ratios shown in Table 3 to prepare a mixture for forming a core layer. The mixture for forming a core layer and the mixture for forming a surface layer were fed into a twin-screw extruder, and melt-kneaded and extruded at a processing temperature of 280°C to prepare recycled sheets (sheets 1 and 2) for evaluating physical properties. The recycled sheets were 0.35 mm thick and had a layer structure of two types and three layers (layer ratio; skin layer / core layer / skin layer=4% / 92% / 4%).

[0054] A surface layer forming mixture was prepared by mixing 94% by mass of A-PET (new material) and 6% by mass of lubricant MB. The crushed product of the above sheet was mixed with A-PET (new material) in the ratio shown in Table 4 to prepare a core layer forming mixture. Using the core layer forming mixture and the surface layer forming mixture, recycled sheets (sheets 3 to 5) for transparency evaluation were prepared by the same method as above. The recycled sheets had a thickness of 0.30 mm and a layer structure of two types and three layers (layer ratio; skin layer / core layer / skin layer = 4% / 92% / 4%).

[0055] (2) Performance evaluation of recycled sheets The IV value, flexural modulus, tensile modulus, and DuPont impact strength were measured by the following methods using the sheets 1 and 2. As a control, a sheet not containing the crushed PET in the core layer was also evaluated for performance. The results are shown in Table 3. (A) IV value: Measured in the same manner as for A-PET (new material). (B) Flexural modulus: measured in accordance with JIS (Japanese Industrial Standards) K7171 using an autograph manufactured by Shimadzu Corporation under the measurement conditions of a support distance of 30 mm and a bending speed of 20 mm / min. (C) Tensile modulus: measured in accordance with JIS K7127. (D) DuPont impact strength: measured in accordance with JIS K7124.

[0056] [Table 3]

[0057] The haze values ​​of the sheets 3 to 5 were measured in accordance with JIS K 7136. As a control, the transparency haze value of A-PET (new material) having the same thickness as the sheets was measured. The results are shown in Table 4.

[0058] [Table 4]

[0059] From Tables 3 and 4, the recycled sheet exhibited strength and transparency comparable to that of a sheet made of A-PET (new material). These results show that the containers of the above examples or the sheets constituting the containers can be suitably used as recycled materials, similar to ordinary PET.

Claims

1. A molded article comprising a polyester-based substrate sheet layer and a sheet having an anchor agent layer and a barrier layer laminated in this order on at least one surface of the polyester-based substrate sheet layer, the anchoring agent layer is a layer formed of a water-soluble polyester-based anchoring agent, the barrier layer is a barrier layer formed of a resin containing a layered silicate, A polyester-based resin molded product, characterized in that the molded product has a haze value of 90 to 110 in relative value when the haze value of a molded product of a sheet consisting of only the polyester-based base sheet layer is taken as 100.

2. 2. The polyester resin molded product according to claim 1, further comprising a waterproof protective layer made of an acrylic resin and laminated on the outside of the barrier layer.

Citation Information

Patent Citations

  • Polyester film

    JP2005097560A

  • Laminated film for packaging and laminate for packaging

    JP1999245346A

  • Gas barrier-coating agent and gas barrier type film

    JP2004315781A

  • Gas-barrier film and packaging material using the film

    JP2005001242A

  • Converted paper, paper material for packaging food, food-packaging container and packaged food