Substrates, liquid crystal antennas and high frequency devices

A substrate with controlled dielectric properties addresses frequency and temperature-related issues in conventional substrates, ensuring stable signal transmission in high-frequency devices and liquid crystal antennas.

JP7568503B2Active Publication Date: 2024-10-16AGC INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2020508281
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-03-20
Filing Date
2019-03-13
Publication Date
2024-10-16
Estimated Expiration
2039-03-13

AI Technical Summary

Technical Problem

Conventional resin and glass substrates exhibit significant changes in dielectric properties with frequency and temperature, making them unsuitable for high-frequency communication devices, especially in environments with large temperature fluctuations.

Method used

A substrate with controlled dielectric loss tangent and relative permittivity across a wide temperature range (-40 to 150°C) is developed, maintaining stable dielectric characteristics by adjusting the composition of glass substrates to achieve specific ratios of dielectric loss tangent and relative permittivity.

Benefits of technology

The substrate reduces dielectric loss and maintains signal stability over a wide temperature range, suitable for high-frequency circuits and liquid crystal antennas in varying environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568503000010
    Figure 0007568503000010
  • Figure 0007568503000011
    Figure 0007568503000011
  • Figure 0007568503000001
    Figure 0007568503000001
Patent Text Reader

Abstract

The present invention provides a substrate that can reduce the dielectric loss of high frequency signals and can be used stably over a wide temperature range. The present invention relates to a substrate having a dielectric loss tangent (A) of 0.1 or less at 20°C and 10 GHz, a dielectric loss tangent (B) of 0.1 or less at 20°C and 35 GHz, and a ratio of {dielectric loss tangent (C) at any temperature between -40°C and 150°C and 10 GHz / dielectric loss tangent (A)} of 0.90 to 1.10. The present invention also relates to a substrate having a dielectric constant (a) of 4 or more and 10 or less at 20°C and 10 GHz, a dielectric constant (b) of 4 or more and 10 or less at 20°C and 35 GHz, and a ratio of {dielectric constant (c) at any temperature between -40°C and 150°C and 10 GHz / dielectric constant (a)} of 0.993 to 1.007.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a substrate, and a liquid crystal antenna and a high-frequency device having the substrate. [Background technology]

[0002] In electronic devices such as communication devices such as mobile phones, smartphones, personal digital assistants, and Wi-Fi devices, surface acoustic wave (SAW) devices, radar components, and antenna components, signal frequencies are becoming higher in order to increase communication capacity and speed. Insulating substrates such as resin substrates, ceramic substrates, and glass substrates are generally used for circuit boards used in such high-frequency communication devices and electronic devices. Insulating substrates used in high-frequency communication devices and electronic devices are required to reduce transmission loss due to dielectric loss, conductor loss, and the like in order to ensure characteristics such as the quality and strength of high-frequency signals.

[0003] In addition, with the spread of IoT, various devices are now equipped with communication functions, and there is a need to install communication devices even in things that have not previously performed wireless communication, such as automobiles. For this reason, it is conceivable that a communication device such as a liquid crystal antenna could be attached to the roof of a car to communicate with a satellite (see Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japan Special Publication No. 2017-506467 [Patent Document 2] Japan Special Publication No. 2017-506471 Summary of the Invention [Problem to be solved by the invention]

[0005] For high-frequency, large-capacity communications, it is desirable for the dielectric properties of the substrate to be stable over a wide frequency band. However, with conventional resin and glass substrates, the amount of change in dielectric properties is large when the frequency changes, especially in the GHz band, making them unsuitable for use as substrates for communications devices.

[0006] In addition, up until now, communication devices have mainly been used indoors as antennas. However, when used as liquid crystal antennas in vehicles that are used over a wide temperature range, such as automobiles or ships, it is expected that they will be used in harsh environments with large temperature changes. In contrast, with conventional glass substrates used in electronic devices, the dielectric properties of the substrate change with temperature changes, significantly affecting the circuit and antenna performance.

[0007] In view of the above circumstances, an object of the present invention is to provide a substrate that can reduce the dielectric loss of high-frequency signals and can be stably used over a wide temperature range, as well as a liquid crystal antenna and a high-frequency device that use the same. [Means for solving the problem]

[0008] As a result of intensive research by the present inventors to achieve the above object, it was found that by reducing the frequency dependency of the dielectric loss tangent or relative dielectric constant and keeping the difference in the dielectric loss tangent or relative dielectric constant within a certain range in the temperature range of -40 to 150°C, desired dielectric characteristics can be stably obtained regardless of the environment when performing signal processing. As a result, the substrate can be suitably used for substrates used in various environments such as equatorial regions and cold regions, and for substrates for high-frequency circuits.

[0009] That is, one embodiment of the substrate according to the present invention has a dielectric loss tangent (A) of 0.1 or less at 20°C and 10 GHz, a dielectric loss tangent (B) of 0.1 or less at 20°C and 35 GHz, and a ratio of {dielectric loss tangent (C) at any temperature between -40°C and 150°C and 10 GHz / dielectric loss tangent (A)} of 0.90 to 1.10.

[0010] In another embodiment of the substrate according to the present invention, the dielectric constant (a) at 20°C and 10 GHz is 4 or more and 10 or less, the dielectric constant (b) at 20°C and 35 GHz is 4 or more and 10 or less, and the ratio expressed as {dielectric constant (c) at any temperature in the range of -40 to 150°C and 10 GHz / dielectric constant (a)} is 0.993 to 1.007.

[0011] The substrate is used in a liquid crystal antenna or a high-frequency circuit.

[0012] A liquid crystal antenna or a high-frequency device according to an aspect of the present invention has the above-mentioned substrate. Effect of the Invention

[0013] The substrate according to the present invention can prevent changes in the dielectric properties of the substrate due to temperature changes and can stably reduce the dielectric loss of high-frequency signals over a wide temperature range, thereby providing a high-performance and practical liquid crystal antenna or high-frequency device. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the configuration of a high-frequency circuit. [Diagram 2] FIG. 2 shows the temperature dependence of the dielectric tangent (FIG. 2(a)) and the temperature dependence of the relative dielectric constant (FIG. 2(b)) at 10 GHz for various substrates. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below, but the present invention is not limited to the following embodiments, and can be modified as desired without departing from the gist of the present invention. In addition, the symbol "to" indicating a numerical range is used to mean that the numerical values ​​before and after it are included as the lower and upper limits. When the substrate is a glass substrate made of glass, the content of each component in the glass substrate is expressed as a mole percentage based on the oxide unless otherwise specified. In addition, "high frequency" means a frequency of 10 GHz or more, preferably more than 30 GHz, and more preferably 35 GHz or more.

[0016] <Substrate> One embodiment of the substrate according to the present invention (hereinafter also referred to as the first embodiment) is characterized in that the dielectric loss tangent (A) at 20°C and 10 GHz is 0.1 or less, the dielectric loss tangent (B) at 20°C and 35 GHz is 0.1 or less, and the ratio expressed as {dielectric loss tangent (C) at any temperature between -40°C and 150°C and 10 GHz / the dielectric loss tangent (A)} is 0.90 to 1.10.

[0017] Another aspect of the substrate according to the present invention (hereinafter also referred to as the second aspect) is characterized in that the dielectric constant (a) at 20°C and 10 GHz is 4 or more and 10 or less, the dielectric constant (b) at 20°C and 35 GHz is 4 or more and 10 or less, and the ratio expressed as {dielectric constant (c) at any temperature in the range of -40 to 150°C and 10 GHz / the dielectric constant (a)} is 0.993 to 1.007.

[0018] By reducing the relative dielectric constant and / or dielectric tangent of the substrate, it is possible to reduce dielectric loss in the high frequency range.

[0019] A first aspect of the substrate according to the present invention has a dielectric loss tangent (tan δ) (A) at 20° C. and 10 GHz of 0.1 or less, preferably 0.05 or less, more preferably 0.01 or less, even more preferably 0.005 or less, and particularly preferably 0.003 or less.

[0020] In the second embodiment of the substrate according to the present invention, the dielectric loss tangent (tan δ) (A) at 20° C. and 10 GHz is preferably 0.1 or less, more preferably 0.05 or less, even more preferably 0.01 or less, even more preferably 0.005 or less, and particularly preferably 0.003 or less.

[0021] The lower limit of the dielectric loss tangent (A) is not particularly limited, but is usually 0.0001 or more.

[0022] A first embodiment of the substrate according to the present invention has a dielectric loss tangent (B) at 20° C. and 35 GHz of 0.1 or less, preferably 0.05 or less, more preferably 0.01 or less, even more preferably 0.005 or less, and particularly preferably 0.003 or less.

[0023] In the second embodiment of the substrate according to the present invention, the dielectric loss tangent (B) at 20° C. and 35 GHz is preferably 0.1 or less, more preferably 0.05 or less, even more preferably 0.01 or less, even more preferably 0.005 or less, and particularly preferably 0.003 or less.

[0024] The lower limit of the dielectric loss tangent (B) is not particularly limited, but is usually 0.0001 or more.

[0025] If the dielectric loss tangent value changes with temperature, the signal characteristics will change when the device is used in a different environment, making it impossible to obtain a desired signal strength.

[0026] Therefore, in the first embodiment of the substrate according to the present invention, the ratio of the dielectric loss tangent at 10 GHz at any temperature in the range of -40 to 150°C divided by the dielectric loss tangent (A) at 20°C and 10 GHz, i.e., {dielectric loss tangent (C) at any temperature in the range of -40 to 150°C and 10 GHz / dielectric loss tangent (A)} is 0.90 to 1.10, and the closer to 1, the more preferable.

[0027] In the second embodiment of the substrate according to the present invention, the ratio {dielectric loss tangent (C) / dielectric loss tangent (A) at any temperature between -40 and 150°C and 10 GHz} is preferably 0.90 to 1.10, and the closer to 1 the better.

[0028] In the case of a glass substrate, the dielectric loss tangent can be adjusted by the glass composition, etc. The dielectric loss tangent can be measured using a cavity resonator and a vector network analyzer according to the method specified in JIS R1641 (2007).

[0029] The ratio represented by {dielectric loss tangent (C) at any temperature between -40 and 150°C and 10 GHz / dielectric loss tangent (A)} is calculated by measuring the dielectric loss tangent at 10 GHz at 10°C intervals from -40 to 150°C, and calculating the ratio of the maximum and minimum values ​​to the dielectric loss tangent (A) at 20°C and 10 GHz.

[0030] In the first embodiment of the substrate according to the present invention, the relative dielectric constant (a) at 20° C. and 10 GHz is preferably 10 or less, more preferably 8 or less, even more preferably 6 or less, even more preferably 5 or less, and particularly preferably 4.5 or less. In the first embodiment of the substrate according to the present invention, the lower limit of the relative dielectric constant (a) is not particularly limited, but is preferably 4 or more from the viewpoint of miniaturizing the shape of the device.

[0031] In addition, in a second embodiment of the substrate according to the present invention, the relative dielectric constant (a) at 20° C. and 10 GHz is 10 or less, more preferably 8 or less, even more preferably 6 or less, even more preferably 5 or less, and particularly preferably 4.5 or less. In the second embodiment of the substrate according to the present invention, the lower limit of the relative dielectric constant (a) is 4 or more from the viewpoint of miniaturizing the shape of the device.

[0032] In the first embodiment of the substrate according to the present invention, the relative dielectric constant (b) at 20° C. and 35 GHz is preferably 10 or less, more preferably 8 or less, even more preferably 6 or less, even more preferably 5 or less, and particularly preferably 4.5 or less. In the first embodiment of the substrate according to the present invention, the lower limit of the relative dielectric constant (b) is not particularly limited, but is preferably 4 or more from the viewpoint of miniaturizing the shape of the device.

[0033] In addition, in a second embodiment of the substrate according to the present invention, the relative dielectric constant (b) at 20° C. and 35 GHz is 10 or less, preferably 8 or less, more preferably 6 or less, even more preferably 5 or less, and particularly preferably 4.5 or less. In the second embodiment of the substrate according to the present invention, the lower limit of the relative dielectric constant (b) is 4 or more from the viewpoint of miniaturizing the shape of the device.

[0034] If the value of the relative dielectric constant changes with temperature, the signal characteristics change when the environment in which the device is used changes, making it impossible to obtain a desired signal strength.

[0035] Therefore, in the first embodiment of the substrate according to the present invention, the ratio obtained by dividing the dielectric constant at 10 GHz at any temperature in the range of -40 to 150°C by the dielectric constant (a) at 20°C and 10 GHz, i.e., {dielectric constant (c) at any temperature in the range of -40 to 150°C and 10 GHz / dielectric constant (a)}, is preferably 0.993 to 1.007, and the closer to 1 the better.

[0036] In addition, in a second embodiment of the substrate according to the present invention, the ratio obtained by dividing the dielectric constant at 10 GHz at any temperature in the range of -40 to 150°C by the dielectric constant (a) at 20°C and 10 GHz, i.e., {dielectric constant (c) at any temperature in the range of -40 to 150°C and 10 GHz / dielectric constant (a)}, is 0.993 to 1.007, and the closer to 1, the more preferable.

[0037] In the case of a glass substrate, the relative dielectric constant can be adjusted by the glass composition, etc. The relative dielectric constant can be measured using a cavity resonator and a vector network analyzer according to the method specified in JIS R1641 (2007).

[0038] The ratio represented by {dielectric constant (c) at any temperature between -40 and 150°C and 10 GHz / dielectric constant (a)} is calculated by measuring the dielectric constant at 10 GHz at 10°C intervals between -40 and 150°C, and finding the ratio of the maximum and minimum values ​​to the value of the dielectric constant (A) at 20°C and 10 GHz, in the same manner as the dielectric loss tangent.

[0039] When the substrate is used in a high-frequency circuit, in order to reduce the amount of bending of the substrate during the manufacturing process (wafer process) of the high-frequency device and thereby prevent the occurrence of manufacturing defects, the Young's modulus is preferably 40 GPa or more, more preferably 50 GPa or more, and even more preferably 55 GPa or more.

[0040] On the other hand, the Young's modulus is preferably 70 GPa or less, more preferably 67 GPa or less, even more preferably 64 GPa or less, and even more preferably 60 GPa or less, in order to reduce the occurrence of thermal stress due to a sudden temperature change.

[0041] In the case of a glass substrate, the Young's modulus can be adjusted by the composition of the glass substrate. The Young's modulus can be measured by the ultrasonic pulse method according to the method specified in JIS Z 2280 (1993).

[0042] When using the substrate to configure a semiconductor package or the like as a high-frequency device, in order to facilitate more appropriate adjustment of the difference in thermal expansion coefficient with other members, the average thermal expansion coefficient at 50 to 350° C. is preferably 3 to 15 ppm / ° C. This allows more appropriate adjustment of the difference in thermal expansion coefficient with other members, such as semiconductor chips, when configuring, for example, a 2.5D or 3D (three-dimensional) mounting type glass through-hole wiring substrate (TGV substrate) for high-frequency applications.

[0043] In the case of a glass substrate, the thermal expansion coefficient can be adjusted by adjusting the content of alkali metal oxides and alkaline earth metal oxides in the glass composition. The average thermal expansion coefficient at 50 to 350°C can be measured using a differential thermal dilatometer according to the method specified in JIS R3102 (1995).

[0044] The main surface of the substrate is the surface on which a wiring layer is formed when the substrate is used in, for example, a high-frequency circuit, and it is preferable that the surface roughness of at least one of the main surfaces is 1.5 nm or less as the arithmetic mean roughness Ra value, because this can reduce the skin resistance of the wiring layer in which the skin effect occurs even in a high-frequency region exceeding 30 GHz, thereby reducing conductor loss. The arithmetic mean roughness Ra of the main surface of the substrate is more preferably 1.0 nm or less, and even more preferably 0.5 nm or less. The surface roughness of the main surface can be achieved by performing a polishing process or the like on the surface of the main surface as necessary.

[0045] When the substrate is a glass substrate, the polishing treatment may be, for example, mechanical polishing using an abrasive containing cerium oxide, colloidal silica, or the like as a main component, and a polishing pad, chemical mechanical polishing using an abrasive, a polishing slurry containing an abrasive, an acidic liquid, or an alkaline liquid as a dispersion medium, and a polishing pad, chemical polishing using an acidic liquid or an alkaline liquid as an etching liquid, etc. These polishing treatments are applied according to the surface roughness of the glass plate that is the material for the glass substrate, and, for example, preliminary polishing and finish polishing may be applied in combination.

[0046] The size and shape of the substrate are not particularly limited. However, for example, in the case of producing large devices in a device production process or producing multiple devices on the same substrate, it is preferable that the longest part of at least one of the main surfaces is 10 cm or more and the shortest part is 5 cm or more.

[0047] In addition, the area of ​​at least one of the main surfaces must be 50 cm 2 A value of 100 cm or more is preferable in terms of improving detection sensitivity in the manufacture of devices such as liquid crystal antennas, and in terms of simplifying the mounting process in the manufacture of high-frequency devices. 2 More than 225cm is preferable. 2 More preferably, it is 100,000 cm or more. 2 It is preferable that the thickness of the substrate is less than 10,000 cm from the viewpoint of ease of handling. 2 Less than 3600cm is more preferable. 2 The following is even more preferred:

[0048] The thickness of the substrate is preferably 0.05 mm or more in terms of maintaining the strength of the substrate during flow, more preferably 0.1 mm or more, and even more preferably more than 0.2 mm. By making the substrate thicker, it is possible to increase the ultraviolet ray shielding ability and protect the resin that deteriorates due to ultraviolet rays.

[0049] On the other hand, from the viewpoints of thinning and miniaturization of high-frequency devices and liquid crystal antennas using high-frequency circuits, improving production efficiency, etc., the thickness is preferably 2 mm or less, more preferably 1.0 mm or less, even more preferably 0.7 mm or less, and even more preferably 0.5 mm or less. By making the substrate thinner, it is possible to increase the ultraviolet transmittance and to use ultraviolet curing materials in the manufacturing process of devices, antennas, etc. to improve manufacturability.

[0050] The porosity of the substrate is preferably 0.1% or less, more preferably 0.01% or less, and even more preferably 0.001% or less, from the viewpoint of suppressing noise generation during the manufacture of a high-frequency device, and is preferably 0.0001% or less from the viewpoint of a liquid crystal antenna, in order to suppress the occurrence of wiring defects due to exposure of open pores on the surface.

[0051] The porosity can be determined by observing bubbles contained in the substrate under an optical microscope, determining the number and diameter of the bubbles, and calculating the volume of the bubbles contained per unit volume.

[0052] The transmittance of the substrate for light with a wavelength of 350 nm is preferably 50% or more, since this allows the use of ultraviolet-curable materials in the lamination process and the like in the manufacturing process of high-frequency devices, antennas, etc., and improves manufacturability. Furthermore, in order to shorten the irradiation time of ultraviolet rays to the ultraviolet-curable materials in the manufacturing process of devices, antennas, etc., and to reduce uneven curing of the ultraviolet-curable materials in the thickness direction, the transmittance is more preferably 70% or more.

[0053] For the same reasons as above, the transmittance of the substrate for light having a wavelength of 300 nm is preferably 50% or more, more preferably 60% or more, and even more preferably 70% or more. Also, the transmittance of the substrate for light having a wavelength of 250 nm is preferably 5% or more, more preferably 10% or more, and even more preferably 20% or more.

[0054] On the other hand, when a resin that deteriorates due to ultraviolet rays is used as a component in a device, antenna, etc., in order to give the substrate an ultraviolet ray shielding ability and function as a protective material, the transmittance of light with a wavelength of 350 nm is preferably 80% or less, more preferably 60% or less, even more preferably 30% or less, and most preferably 10% or less.

[0055] For the same reasons as above, the transmittance of the substrate for light with a wavelength of 300 nm is preferably 80% or less, more preferably 60% or less, even more preferably 30% or less, and even more preferably 10% or less. Also, the transmittance of light with a wavelength of 250 nm is preferably 60% or less, more preferably 30% or less, even more preferably 10% or less, and even more preferably 5% or less.

[0056] The light transmittance of the substrate at each wavelength can be measured using a visible / ultraviolet spectrophotometer, and the external transmittance including loss due to reflection is used.

[0057] The substrate of the present invention is not particularly limited in type as long as it has the above-mentioned characteristics, and may include any of a resin substrate, a ceramic substrate, and a glass substrate. The glass substrate may be an amorphous substrate made of a nonmetallic inorganic solid that exhibits glass transition, and a substrate made of oxide glass is more preferable. Note that this does not include crystallized glass, which is a mixture of glass and crystals, or a glass sintered body containing a crystalline filler. Note that the crystallinity of glass can be confirmed to be amorphous by, for example, performing X-ray diffraction measurement and finding that no clear diffraction peaks are observed.

[0058] If the substrate is a glass substrate, the β-OH value of the glass substrate is 0.05 to 0.8 mm -1 The β-OH value is a value used as an index of the water content of glass, and is determined by measuring the absorbance of a glass substrate with respect to light having a wavelength of 2.75 to 2.95 μm, and determining the maximum value β max This value is calculated by dividing by the thickness of the board (mm).

[0059] β-OH value is 0.8mm -1By setting the thickness to 0.6 mm or less, the low dielectric loss of the substrate can be further improved, and this is preferable. -1 Less than 0.5mm is more preferable. -1 Less than 0.4 mm is more preferable. -1 Even more preferred is the following:

[0060] On the other hand, the β-OH value is 0.05 mm -1 By setting the value at or above this level, it is not necessary to melt the glass in an extremely dry atmosphere or to drastically reduce the amount of water in the raw materials, and this is preferable because it is possible to improve the productivity of the glass and the bubble quality. -1 More preferably, 0.2 mm or more -1 The above is more preferable. The β-OH value can be adjusted by the composition of the glass in the substrate and the selection of the raw materials.

[0061] The devitrification temperature of the glass substrate is preferably 1400° C. or less. When the devitrification temperature is 1400° C. or less, the temperature of the components of the forming equipment can be lowered when forming the glass, and the life of the components can be extended. The devitrification temperature is more preferably 1350° C. or less, further preferably 1330° C. or less, and particularly preferably 1300° C. or less.

[0062] The devitrification temperature of glass is the average of the maximum temperature at which crystals precipitate on the surface or inside of the glass and the minimum temperature at which no crystals precipitate when crushed glass particles are placed in a platinum dish and heat-treated for 17 hours in an electric furnace controlled at a constant temperature.The sample after heat treatment is observed under an optical microscope.

[0063] The method for producing the substrate will be described in detail later, but in the case of a glass substrate, the substrate is formed by melting and hardening a glass raw material. The method for producing the substrate is not particularly limited, but for example, a method in which a general molten glass is formed into a predetermined plate thickness by a float method, and then slowly cooled and cut into a desired shape to obtain a plate glass can be applied.

[0064] The glass composition of the glass substrate will be described below. In this specification, "substantially free" means that it is not contained except for inevitable impurities mixed from raw materials, that is, it is not intentionally contained, and is about 0.1 mol % or less, but is not limited thereto.

[0065] The glass preferably contains SiO2 as a main component. In this specification, "containing SiO2 as a main component" means that the content of SiO2 is the largest in terms of the ratio of components in mole percent based on oxide. SiO2 is a network forming substance, and its content is more preferably 40% or more, even more preferably 45% or more, even more preferably 50% or more, and particularly preferably 55% or more, since it can improve glass forming ability and weather resistance and can suppress devitrification. On the other hand, from the viewpoint of improving the melting property of the glass, it is preferably 75% or less, more preferably 74% or less, even more preferably 73% or less, and even more preferably 72% or less.

[0066] The total content of Al2O3 and B2O3 (including the case where the content of Al2O3 is 0) is preferably 1% or more, more preferably 3% or more, even more preferably 5% or more, and even more preferably 7% or more, since it can improve the solubility of glass, etc. Also, since it can improve the low dielectric loss of the substrate while maintaining the solubility of glass, etc., the total content of Al2O3 and B2O3 is preferably 40% or less, more preferably 37% or less, even more preferably 35% or less, and even more preferably 33% or less.

[0067] The molar ratio of the content expressed by {Al2O3 / (Al2O3+B2O3)} is preferably 0.45 or less, more preferably 0.4 or less, and even more preferably 0.3 or less, because it can enhance the low dielectric loss of the glass substrate. The molar ratio of the content expressed by {Al2O3 / (Al2O3+B2O3)} is preferably 0 or more (including 0), more preferably 0.01 or more, and even more preferably 0.05 or more.

[0068] The content of Al2O3 is preferably 15% or less, more preferably 14% or less, and even more preferably 10% or less, because it can improve the melting property of glass, etc. In addition, since Al2O3 is a component that is effective in improving weather resistance, suppressing phase separation of glass, and reducing the thermal expansion coefficient, etc., it does not have to be contained, but if it is contained, the content is more preferably 0.5% or more.

[0069] The content of B2O3 is preferably 30% or less, more preferably 28% or less, even more preferably 26% or less, even more preferably 24% or less, and particularly preferably 23% or less, because it can improve the acid resistance and strain point. In addition, since B2O3 is a component that is effective in improving the melt reactivity and lowering the devitrification temperature, the content of B2O3 is preferably 9% or more, more preferably 13% or more, and even more preferably 16% or more.

[0070] Examples of alkaline earth metal oxides include MgO, CaO, SrO, and BaO, all of which function as components that enhance the melting reactivity of glass. The total content of such alkaline earth metal oxides is preferably 13% or less, more preferably 11% or less, even more preferably 10% or less, even more preferably 8% or less, and particularly preferably 6% or less, because it can enhance the low dielectric loss of the glass substrate. In addition, the total content of alkaline earth metal oxides is preferably 0.1% or more, more preferably 3% or more, and even more preferably 5% or more, because it can maintain good melting properties of glass.

[0071] MgO is not an essential component, but it is a component that can increase the Young's modulus without increasing the specific gravity. In other words, MgO is a component that can increase the specific elastic modulus, and by including MgO, the problem of deflection can be reduced, and the fracture toughness value can be improved to increase the glass strength. MgO is also a component that improves solubility. Although MgO is not an essential component, the effect of including MgO can be sufficiently obtained, and the thermal expansion coefficient can be prevented from becoming too low, so that the content is preferably 0.1% or more, more preferably 1% or more, and even more preferably 3% or more. On the other hand, in terms of suppressing the rise in the devitrification temperature, the content of MgO is preferably 13% or less, more preferably 11% or less, and even more preferably 9% or less.

[0072] CaO is a component that increases the specific elastic modulus next to MgO among alkaline earth metals and does not excessively lower the strain point, and improves solubility like MgO. Furthermore, it is a component that is less likely to increase the devitrification temperature than MgO. Although CaO is not an essential component, the effect of including CaO can be fully obtained, so its content is preferably 0.1% or more, more preferably 1% or more, and even more preferably 3% or more. In addition, the average thermal expansion coefficient does not become too high, and the increase in the devitrification temperature can be suppressed to prevent devitrification during glass production, so that the CaO content is preferably 13% or less, more preferably 10% or less, and even more preferably 8% or less.

[0073] SrO is a component that does not increase the devitrification temperature of glass and improves the melting point. Although SrO is not an essential component, the effect of including SrO can be sufficiently obtained, so that the content is preferably 0.1% or more, more preferably 0.5% or more, even more preferably 1% or more, even more preferably 1.5% or more, and particularly preferably 2% or more. In addition, since the specific gravity is not too high and the average thermal expansion coefficient is prevented from becoming too high, the content of SrO is preferably 13% or less, more preferably 10% or less, even more preferably 7% or less, and particularly preferably 5% or less.

[0074] BaO is not an essential component, but it is a component that does not increase the devitrification temperature of glass and improves the solubility. However, if BaO is contained in a large amount, the specific gravity increases, the Young's modulus decreases, the relative dielectric constant increases, and the average thermal expansion coefficient tends to become too large. Therefore, the content of BaO is preferably 10% or less, more preferably 8% or less, even more preferably 5% or less, even more preferably 3% or less, and it is particularly preferable that BaO is not substantially contained.

[0075] Examples of alkali metal oxides include Li2O, Na2O, K2O, Rb2O, and Cs2O. The total content of such alkali metal oxides is preferably 5% or less, more preferably 3% or less, even more preferably 1% or less, even more preferably 0.2% or less, particularly preferably 0.1% or less, and most preferably 0.05% or less, from the viewpoint of enhancing the low dielectric loss of the glass substrate. In addition, since excessive raw material purification is not required, practical glass meltability and glass substrate productivity are obtained, and the thermal expansion coefficient of the glass substrate can be adjusted, the total content is preferably 0.001% or more, more preferably 0.002% or more, even more preferably 0.003% or more, and even more preferably 0.005% or more.

[0076] Among the above alkali metal oxides, Na2O and K2O are particularly important, and the total content of Na2O and K2O is preferably in the range of 0.001 to 5%. In addition, the coexistence of Na2O and K2O is preferable because it suppresses the movement of alkali components and can improve the low dielectric loss of the glass substrate. That is, the molar ratio of the content expressed by {Na2O / (Na2O+K2O)} is preferably 0.01 to 0.99, more preferably 0.98 or less, even more preferably 0.95 or less, and even more preferably 0.9 or less. On the other hand, the molar ratio of the content expressed by {Na2O / (Na2O+K2O)} is more preferably 0.02 or more, even more preferably 0.05 or more, and even more preferably 0.1 or more.

[0077] In addition to the above components, optional components such as Fe2O3, TiO2, ZrO2, ZnO, Ta2O5, WO3, Y2O3, La2O3, etc. may be included. Among them, Fe2O3 is a component that controls the light absorption performance of the glass substrate, such as infrared absorption performance and ultraviolet absorption performance, and can be included up to 0.012% or less of Fe content calculated as Fe2O3 as necessary. If the above-mentioned Fe content is 0.012% or less, the low dielectric loss and ultraviolet transmittance of the glass substrate can be maintained. When Fe is contained, the content is more preferably 0.01% or less, and even more preferably 0.005% or less, in order to improve the ultraviolet transmittance. By increasing the ultraviolet transmittance of the glass substrate, ultraviolet curing materials can be used in the lamination process and the like in the manufacturing process of high-frequency devices, antennas, etc., and the manufacturability of high-frequency devices, antennas, etc. can be improved.

[0078] On the other hand, it is also preferable that the glass substrate contains 0.05% or more Fe content calculated as Fe2O3 as necessary, in order to enhance the ultraviolet shielding ability. The Fe content is more preferably 0.07% or more, and even more preferably 0.1% or more. In this way, by enhancing the ultraviolet shielding ability of the glass substrate, the glass substrate can be endowed with a function as a protective material when a resin that deteriorates due to ultraviolet rays is used as a member.

[0079] <Substrate manufacturing method> (Glass substrate) The glass substrate can be obtained by a manufacturing method including a melting step of heating glass raw materials to obtain molten glass, a fining step of removing bubbles from the molten glass, a forming step of forming the molten glass into a plate shape to obtain a glass ribbon, and a slow cooling step of slowly cooling the glass ribbon to room temperature. Alternatively, the glass substrate may be manufactured by forming the molten glass into a block shape, slowly cooling it, and then cutting and polishing it.

[0080] In the melting step, raw materials are prepared so as to have a target composition for the glass substrate, and the raw materials are continuously charged into a melting furnace and heated preferably to about 1450° C. to 1750° C. to obtain molten glass.

[0081] The raw materials may also include oxides, carbonates, nitrates, hydroxides, chlorides, and other halides. When the molten glass comes into contact with platinum during the melting or fining process, minute platinum particles may dissolve into the molten glass and become mixed into the resulting glass substrate as foreign matter. However, the use of a nitrate raw material has the effect of preventing the generation of platinum foreign matter.

[0082] As the nitrate, strontium nitrate, barium nitrate, magnesium nitrate, calcium nitrate, etc. can be used. It is more preferable to use strontium nitrate. The raw material particle size can be appropriately selected from raw materials with a large particle size of several hundred μm that does not leave any residue in the solution, to raw materials with a small particle size of about several μm that does not scatter during raw material transportation and does not aggregate as secondary particles. Granules can also be used.

[0083] The moisture content of the raw material can be adjusted appropriately to prevent the raw material from scattering. 2+ / (Fe 2+ +Fe 3+ )) and other dissolution conditions can also be adjusted appropriately.

[0084] The fining step is a step of removing bubbles from the molten glass obtained in the melting step. The fining step may be a defoaming method using reduced pressure, or may be performed at a temperature higher than the melting temperature of the raw material. In the manufacturing process of the glass substrate in the embodiment, SO3 or SnO2 may be used as a fining agent.

[0085] As the SO3 source, a sulfate of at least one element selected from the group consisting of Al, Na, K, Mg, Ca, Sr, and Ba is preferred, and an alkaline earth metal sulfate is more preferred. Among these, CaSO4·2H2O, SrSO4, and BaSO4 are particularly preferred because they have a significant effect of enlarging bubbles.

[0086] As a clarifying agent in the degassing method under reduced pressure, it is preferable to use a halogen such as Cl or F.

[0087] The Cl source is preferably a chloride of at least one element selected from the group consisting of Al, Mg, Ca, Sr and Ba, more preferably an alkaline earth metal chloride, and among these, SrCl2·6H2O and BaCl2·2H2O are particularly preferred because they have a significant effect of enlarging bubbles and are less deliquescent.

[0088] The F source is preferably a fluoride of at least one element selected from the group consisting of Al, Na, K, Mg, Ca, Sr and Ba, more preferably an alkaline earth metal fluoride, and among these, CaF2 is more preferable because it has a remarkable effect of increasing the solubility of the glass raw materials.

[0089] Tin compounds such as SnO2 generate O2 gas in molten glass. In the molten glass, SnO2 is reduced to SnO at a temperature of 1450°C or higher, generating O2 gas and acting to make bubbles grow larger. In the manufacture of the glass substrate of the embodiment, the glass raw material is heated to about 1450 to 1750°C to melt, so that bubbles in the molten glass grow larger more effectively.

[0090] When SnO2 is used as a fining agent, the tin compound in the raw material is adjusted to be contained in an amount of 0.01% or more in terms of SnO2 relative to the total amount of the matrix composition (100%). By making the SnO2 content 0.01% or more, a fining effect is obtained when the glass raw material is melted, so that it is preferable, more preferably 0.05% or more, and even more preferably 0.10% or more. On the other hand, by making the SnO2 content 0.3% or less, it is preferable because the occurrence of coloring and devitrification of the glass can be suppressed. The content of the tin compound in the alkali-free glass is more preferably 0.25% or less in terms of SnO2 relative to the total amount of the matrix composition (100%), even more preferably 0.2% or less, and particularly preferably 0.15% or less.

[0091] The forming step is a step of forming the molten glass from which bubbles have been removed in the fining step into a sheet shape to obtain a glass ribbon. As the forming step, a known method for forming glass into a sheet shape can be applied, such as a float method in which molten glass is made to flow onto a molten metal such as tin to form a sheet shape and obtain a glass ribbon, an overflow downdraw method (fusion method) in which molten glass is made to flow downward from a trough-shaped member, or a slit downdraw method in which molten glass is made to flow down from a slit.

[0092] The annealing process is a process of cooling the glass ribbon obtained in the forming process to room temperature under controlled cooling conditions. In the annealing process, the glass ribbon is cooled to a temperature range between the annealing point and the strain point of the formed glass at a predetermined average cooling rate, R (°C / min), and further annealed to room temperature under predetermined conditions. After cutting the annealed glass ribbon, a glass substrate is obtained.

[0093] If the cooling rate R in the slow cooling process is too large, distortion is likely to remain in the glass after cooling. In addition, the equivalent cooling rate, which is a parameter that reflects the fictive temperature, becomes too high, and as a result, low dielectric loss characteristics cannot be obtained. Therefore, it is preferable to set R so that the equivalent cooling rate is 800 ° C. / min or less. The equivalent cooling rate is more preferably 400 ° C. / min or less, even more preferably 100 ° C. / min or less, and particularly preferably 50 ° C. / min or less. On the other hand, if the cooling rate is too small, the time required for the process becomes too long, and productivity decreases. Therefore, it is preferable to set it to 0.1 ° C. / min or more, more preferably 0.5 ° C. / min or more, and even more preferably 1 ° C. / min or more.

[0094] Here, the definition and evaluation method of the equivalent cooling rate are as follows.

[0095] Glass of the target composition to be processed into a rectangular parallelepiped of 10 mm x 10 mm x 0.3 to 2.0 mm is held at strain point +170°C for 5 minutes in an infrared heating electric furnace, and then the glass is cooled to room temperature (25°C). At this time, multiple glass samples are produced by varying the cooling rate in the range of 1°C / min to 1000°C / min.

[0096] Using a precision refractive index measuring device (e.g., Shimadzu Devices KPR2000), the refractive index n of multiple glass samples at the d line (wavelength 587.6 nm) was measured. d The measurement can be done using the V-block method or the minimum deviation method. d is plotted against the logarithm of the cooling rate to obtain n d Obtain a calibration curve.

[0097] Next, we compared n samples of glass with the same composition that were actually produced through processes such as melting, molding, and cooling. d is measured by the above-mentioned measurement method. d The corresponding cooling rate (referred to as an equivalent cooling rate in this embodiment) is obtained from the calibration curve.

[0098] In addition, in a method for producing a glass substrate, it is preferable to thoroughly stir the molten glass at any part in a conveying pipe during production and to reduce the temperature distribution during slow cooling after sheet formation, since this can further reduce the in-plane fluctuation range of the dielectric tangent and the relative dielectric constant at 20° C. and 10 GHz.

[0099] Although the manufacturing method of the glass substrate has been described above, the manufacturing method is not limited to the above embodiment, and the present invention includes modifications and improvements within the scope of achieving the object of the present invention. For example, when manufacturing the glass substrate of the present invention, glass may be formed into a plate shape by a press molding method in which molten glass is directly formed into a plate shape.

[0100] In addition, when manufacturing the glass substrate of the present invention, in addition to the manufacturing method using a melting tank made of refractory material, a crucible made of platinum or an alloy mainly composed of platinum (hereinafter referred to as platinum crucible) may be used as the melting tank or fining tank. When a platinum crucible is used, the melting step involves preparing raw materials so as to obtain the composition of the glass substrate to be obtained, and heating the platinum crucible containing the raw materials in an electric furnace, preferably to about 1450°C to 1700°C. A platinum stirrer is inserted and the mixture is stirred for 1 hour to 3 hours to obtain molten glass.

[0101] In the forming step in the manufacturing process of a glass plate using a platinum crucible, the molten glass is poured onto, for example, a carbon plate or into a mold to form a plate or block. In the slow cooling step, the glass is typically held at a temperature of about Tg+50°C with respect to the glass transition point Tg, and then cooled at about 1 to 10°C / min to the vicinity of the strain point, and then cooled to room temperature at a cooling rate at which no distortion remains. After cutting into a predetermined shape and polishing, a glass substrate is obtained. In addition, the glass substrate obtained by cutting may be heated to, for example, about Tg+50°C, and then slowly cooled to room temperature at a predetermined cooling rate. In this way, the equivalent cooling temperature of the glass can be adjusted.

[0102] <High frequency circuits, liquid crystal antennas> The substrate of the present invention is suitable for circuit boards of high-frequency devices (electronic devices) such as semiconductor devices used in communication devices such as mobile phones, smartphones, personal digital assistants, and Wi-Fi devices, surface acoustic wave (SAW) devices, radar components such as radar transceivers, and antenna components such as liquid crystal antennas. In particular, since the dielectric loss of high-frequency signals can be reduced and stable characteristics can be obtained over a wide temperature range, the substrate of the present invention is more suitable for high-frequency circuits used in high-frequency devices and liquid crystal antenna substrates.

[0103] The substrate for high frequency circuits is particularly suitable for high frequency devices that handle high frequency signals, particularly high frequency signals exceeding 30 GHz, and further high frequency signals of 35 GHz or higher. By using the substrate for high frequency devices, the transmission loss of high frequency signals can be reduced, and characteristics such as the quality and strength of the high frequency signals can be improved.

[0104] It is also suitable as a substrate for drilling holes using a laser or the like, and not only does it improve the characteristics such as the quality and strength of the high frequency signal mentioned above, but it also has high resistance to the thermal shock that occurs when drilling holes.

[0105] FIG. 1 shows an example (cross-sectional view) of the configuration of a high-frequency circuit used in a high-frequency device. The circuit board 1 includes an insulating substrate 2, a first wiring layer 3 formed on a first main surface 2a of the substrate 2, and a second wiring layer 4 formed on a second main surface 2b of the substrate 2. The first and second wiring layers 3 and 4 form a microstrip line as an example of a transmission line. The first wiring layer 3 forms a signal line, and the second wiring layer 4 forms a ground line. However, the structure of the first and second wiring layers 3 and 4 is not limited to this, and the wiring layers may be formed on only one of the main surfaces of the substrate 2.

[0106] The first and second wiring layers 3, 4 are layers formed of a conductor, and their thickness is usually about 0.1 to 50 μm. The conductor forming the first and second wiring layers 3, 4 is not particularly limited, and examples thereof include metals such as copper, gold, silver, aluminum, titanium, chromium, molybdenum, tungsten, platinum, and nickel, as well as alloys and metal compounds containing at least one of these metals.

[0107] The structure of the first and second wiring layers 3, 4 is not limited to a single-layer structure, and may be a multi-layer structure such as a laminated structure of a titanium layer and a copper layer. The method of forming the first and second wiring layers 3, 4 is not particularly limited, and various known forming methods such as a printing method using a conductive paste, a dipping method, a plating method, a vapor deposition method, and a sputtering method can be applied.

[0108] By using the substrate of the present invention in a high-frequency circuit, the transmission loss of the circuit substrate at high frequencies can be reduced. Specifically, the transmission loss at a frequency of, for example, 35 GHz can be reduced to preferably 1 dB / cm or less, more preferably 0.5 dB / cm or less. Therefore, the characteristics such as the quality and strength of high-frequency signals, particularly high-frequency signals exceeding 30 GHz, and further high-frequency signals of 35 GHz or more, are maintained, and a substrate and a circuit substrate suitable for high-frequency devices that handle such high-frequency signals can be provided. This can improve the characteristics and quality of high-frequency devices that handle high-frequency signals.

[0109] Furthermore, since the substrate of the present invention has stable characteristics over a wide temperature range, it can be suitably used for high-frequency devices used in hot or cold regions, or even in regions with drastic temperature changes such as deserts.

[0110] Furthermore, high-frequency circuit boards include boards called universal boards and perforated boards, in which, for example, through holes and copper foil lands are formed in a regular pattern (such as a grid pattern) in an insulating base plate, and copper foil wiring connecting several of the lands is formed by etching. A laser is used to form the through holes and perform the etching, and examples of the laser include an excimer laser, an infrared laser, a CO2 laser, and a UV laser.

[0111] A liquid crystal antenna is a satellite communication antenna that uses liquid crystal technology and can control the direction of radio waves it transmits and receives, and is mainly used on vehicles such as ships, airplanes, and automobiles. Since liquid crystal antennas are mainly expected to be used outdoors, they are required to have stable characteristics over a wide temperature range. Examples of wide temperature ranges include the temperature difference between the ground and the sky, the temperature difference between day and night in the desert, a rainstorm in a scorching desert, use in hot areas, use in cold areas, etc. The substrate of the present invention can provide stable characteristics over a wide temperature range as described above, and is therefore also preferably used for a liquid crystal antenna. EXAMPLES

[0112] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these.

[0113] [Examples 1-26] Glass substrates having the compositions shown in Tables 1 to 4, thicknesses of 0.5 to 10 mm, and dimensions of 50 x 50 mm were prepared. The glass substrates were produced by a melting method using a platinum crucible. Raw materials such as silica sand were mixed so that the glass weight was 1 kg, and a batch was prepared. With respect to 100% of the raw materials of the target composition, 0.1% to 1% sulfate (calculated as SO3), 0.16% F, and 1% Cl were added, expressed as mass percentages based on oxides.

[0114] The raw materials were placed in a platinum crucible and heated in an electric furnace at 1650°C for 3 hours to melt them, producing molten glass. For melting, a platinum stirrer was inserted into the platinum crucible and stirred for 1 hour to homogenize the glass. The molten glass was poured onto a carbon plate and formed into a plate, after which the plate-shaped glass was placed in an electric furnace at a temperature of about Tg+50°C and held for 1 hour, after which the electric furnace was cooled to Tg-100°C at a cooling rate of 1°C / min, and then the glass was allowed to cool until it reached room temperature. The glass was then cut and polished to form a plate.

[0115] The end faces were chamfered (C / R) using a chamfering device. An example of a chamfering device for glass sheets is the device described in JP 2008-49449 A, which uses a rotating grindstone to chamfer the ends of the glass sheets. The rotating grindstone may be either resin-bonded or metal-bonded. Examples of abrasive grains used in the grindstone include diamond, cubic boron nitride (CBN), alumina (Al2O3), silicon carbide (SiC), pumice, garnet, or any combination thereof.

[0116] In addition, in Tables 1 to 4, the total amount of RO *1 indicates the total content of alkaline earth metal oxides (MgO+CaO+SrO+BaO), and is the total amount of RO *2 indicates the total content of alkali metal oxides (Na2O + K2O).

[0117] [Examples 27 and 28] A resin substrate made of polyimide resin (Kapton H (manufactured by Toray DuPont Co., Ltd.), Upilex S50 (manufactured by Ube Industries, Ltd.)) was prepared.

[0118] The dielectric loss tangent at 35 GHz (20°C), the dielectric loss tangent at 10 GHz (-40 to 150°C), the relative dielectric constant at 35 GHz (20°C), the relative dielectric constant at 10 GHz (-40 to 150°C), the average thermal expansion coefficient at 50 to 350°C, Young's modulus, porosity, the transmittance of light with a wavelength of 350 nm, the β-OH value, density, specific elastic modulus, and devitrification temperature were each measured for the obtained substrate.

[0119] The results are shown in Tables 5 to 9. In the tables, the values ​​in parentheses were calculated, and "-" means that the value was not measured.

[0120] The methods for measuring each physical property are shown below.

[0121] (Dielectric constant, dielectric tangent) Measurements were performed using a cavity resonator and a vector network analyzer according to the method specified in JIS R1641 (2007). The measurement frequencies were 35 GHz and 10 GHz, which are the resonance frequencies of the air in the cavity resonator. The sample shape was a flat plate with a size of 40 mm square and a thickness of 0.3 to 0.4 mm for 35 GHz, and a rectangular shape with a size of 3 mm x 60 mm x a thickness of 0.4 to 0.6 mm for 10 GHz. The cavity resonator was placed in a thermostatic chamber to adjust the measurement temperature. The measurement temperature was 20°C for 35 GHz, and was measured in 10°C increments in the range of -40 to 150°C for 10 GHz. In addition, for Examples 27 and 28, which are resin substrates, in order to eliminate the effects of moisture absorption, the samples were dehumidified by holding them at 120°C for 2 hours, and then stored in a dry container before temperature measurement.

[0122] In Tables 5 to 8, "dielectric loss tangent @ 10 GHz" and "relative dielectric loss tangent @ 10 GHz" indicate values ​​measured at 20°C. In addition, FIG. 2(a) shows the results of evaluating the temperature dependence of the dielectric loss tangent by plotting the values ​​of the dielectric loss tangent at 10 GHz measured at 10°C intervals in the range of -40 to 150°C divided by the values ​​of the dielectric loss tangent at 20°C and 10 GHz. In FIG. 2(b) shows the results of evaluating the temperature dependence of the dielectric constant by plotting the values ​​of the dielectric constant at 10 GHz measured at 10°C intervals in the range of -40 to 150°C divided by the values ​​of the dielectric constant at 20°C and 10 GHz.

[0123] (Average thermal expansion coefficient) Measurements were made using a differential thermal dilatometer in accordance with the method specified in JIS R3102 (1995). The measurement temperature range was 50 to 350°C, and the unit was expressed as ppm / °C.

[0124] (Young's Modulus) Glass having a thickness of 0.5 to 10 mm was measured by the ultrasonic pulse method according to the method specified in JIS Z 2280. The unit is GPa.

[0125] (Porosity) The bubbles contained in the glass substrate were observed under an optical microscope, the number and diameter of the bubbles were determined, and the volume of the bubbles contained per unit volume was calculated.

[0126] (transmittance) The transmittance of mirror-polished glass of a given thickness was measured using a visible-ultraviolet spectrophotometer. The transmittance was defined as the external transmittance including loss due to reflection, and was expressed as a value converted into a glass thickness of 0.3 to 0.4 mm.

[0127] (β-OH value) The measurement was performed using the method described in the above embodiment. The unit is mm -1 It is expressed as:

[0128] (density) The density of a glass lump weighing approximately 20 g and containing no bubbles was measured by the Archimedes method and expressed in g / cm 3 It is expressed as:

[0129] (devitrification temperature) Crushed glass particles were placed in a platinum dish and heat-treated for 17 hours in an electric furnace controlled at a constant temperature. After heat treatment, the sample was observed under an optical microscope to determine the average value of the maximum temperature at which crystals precipitated inside the glass and the minimum temperature at which no crystals precipitated.

[0130] (Specific elastic modulus) The specific elastic modulus is calculated using the measured density and Young's modulus, and is expressed in GPa cm. 3 / g.

[0131] [Table 1]

[0132] [Table 2]

[0133] [Table 3]

[0134] [Table 4]

[0135] [Table 5]

[0136] [Table 6]

[0137] [Table 7]

[0138] [Table 8]

[0139] [Table 9]

[0140] 2(a), the value obtained by dividing [dielectric loss tangent at 10 GHz at each temperature from -40 to 150°C] by [dielectric loss tangent at 20°C and 10 GHz] was 0.93 to 1.06 in Example 4, 0.99 to 1.00 in Example 6, 0.98 to 1.13 in Example 27, and 0.85 to 1.20 in Example 28. Examples 4 and 6, which are examples of the first aspect of the present invention, had smaller temperature dependence of the dielectric loss tangent at 10 GHz than Examples 27 and 28, which are comparative examples.

[0141] 2(b), the value obtained by dividing [dielectric constant at each temperature from -40 to 150°C and 10 GHz] by [dielectric constant at 20°C and 10 GHz] was 0.998 to 1.006 for Example 4, 0.994 to 1.013 for Example 6, 0.992 to 1.005 for Example 27, and 0.988 to 1.001 for Example 28. Example 4, which is an embodiment of the second aspect of the present invention, had a smaller temperature dependency of the dielectric constant at 10 GHz than Examples 6, 27, and 28, which are comparative examples.

[0142] The substrate of the present invention has a small temperature dependence of the dielectric constant and / or dielectric tangent at 10 GHz, and also has a small dielectric tangent value at 35 GHz. Therefore, even when used as a substrate for a high-frequency device or a liquid crystal antenna substrate that requires a low dielectric tangent, even when used in an environment with large temperature changes, the change in dielectric properties is small and stable performance can be exhibited.

[0143] Although the present invention has been described in detail with reference to specific embodiments, it is apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the present invention. This application is based on a Japanese patent application (Patent Application No. 2018-53081) filed on March 20, 2018, and is incorporated by reference in its entirety. In addition, all references cited herein are incorporated in their entirety. [Industrial Applicability]

[0144] The substrate of the present invention has excellent dielectric loss properties for high-frequency signals and exhibits stable characteristics over a wide temperature range. Therefore, a circuit board using the substrate has excellent transmission loss properties for high-frequency signals and can be used in any environment.

[0145] Such substrates and circuit boards are extremely useful as components for high-frequency electronic devices in general that handle high-frequency signals exceeding 10 GHz, particularly high-frequency signals exceeding 30 GHz, and even high-frequency signals of 35 GHz or higher, as well as for liquid crystal antennas and the like that are used in environments with large temperature changes. [Explanation of symbols]

[0146] 1 Circuit Board 2. Board 2a First main surface 2b Second main surface 3 First wiring layer 4 Second wiring layer

Claims

1. The dielectric loss tangent (A) at 20° C. and 10 GHz is 0.1 or less, The dielectric loss tangent (B) at 20° C. and 35 GHz is 0.1 or less, and a ratio represented by {dielectric loss tangent (C) at any temperature in the range of −40 to 150° C. and 10 GHz / dielectric loss tangent (A)} is 0.90 to 1.10, It is made of oxide glass, The oxide glass is, in terms of mole percentage based on oxide, Contains 50 to 75% SiO 2 , Contains 0.5 to 15% Al 2 O 3 , Contains 7.8 to 24% B 2 O 3 ; A 2 O 3 and B 2 O 3 Contains a total of 19.1 to 31.0% {Al 2 O 3 / (Al 2 O 3 +B 2 O 3 )) is 0.26 to 0.59, Contains 0 to 7% SrO; Contains 7.0 to 14.8% alkaline earth metal oxides in total; Contains 0.005 to 0.08% in total of alkali metal oxides; Among the alkali metal oxides, {Na 2 O / (Na 2 O+K 2 O)) is 0.67 to 0.88 molar ratio.

2. The dielectric constant (a) at 20° C. and 10 GHz is 4 or more and 10 or less, The dielectric constant (b) at 20° C. and 35 GHz is 4 or more and 10 or less, and a ratio represented by {dielectric constant (c) at any temperature in the range of −40 to 150° C. and 10 GHz / dielectric constant (a)} is 0.993 to 1.007, It is made of oxide glass, The oxide glass is, in terms of mole percentage based on oxide, Contains 50 to 75% SiO 2 , Contains 0.5 to 10% Al 2 O 3 , Contains 13 to 24% B 2 O 3 ; A 2 O 3 and B 2 O 3 Contains more than 19.1% and not more than 31.0% in total, {Al 2 O 3 / (Al 2 O 3 +B 2 O 3 )) is 0.01 to 0.3, Contains 0 to 5% SrO; Contains 0.1 to 7.0% in total of alkaline earth metal oxides, Contains 0.005 to 0.05% in total of alkali metal oxides, Among the alkali metal oxides, {Na 2 O / (Na 2 O+K 2 O)) is 0.67 or more and less than 0.

88.

3. 3. The substrate according to claim 1, wherein the longest portion of at least one of the main surfaces is 10 cm or more and the shortest portion is 5 cm or more.

4. The substrate according to any one of claims 1 to 3, having a thickness of 0.05 to 2 mm.

5. 5. The substrate according to claim 1, having an average thermal expansion coefficient of 3 to 15 ppm / °C at 50 to 350°C.

6. The substrate according to any one of claims 1 to 5, having a Young's modulus of 40 GPa or more.

7. The substrate according to any one of claims 1 to 6, having a Young's modulus of 70 GPa or less.

8. The substrate according to any one of claims 1 to 7, having a porosity of 0.1% or less.

9. 9. The substrate according to claim 1, which has a transmittance of 50% or more for light having a wavelength of 350 nm.

10. β-OH value: 0.05 to 0.8 mm -1 The substrate according to any one of claims 1 to 9,

11. In terms of mole percentage based on oxide, Al 2 O 3 0.5 to 10% and B 2 O 3 The substrate according to any one of claims 1 to 10, containing 13 to 23%.

12. In terms of mole percentage based on oxide, Fe is Fe 2 O 3 The substrate according to any one of claims 1 to 11, containing 0 to 0.012% in terms of Mo converted.

13. The substrate according to any one of claims 1 to 12, which is used for a liquid crystal antenna or a high-frequency circuit.

14. A liquid crystal antenna comprising the substrate according to any one of claims 1 to 13.

15. A high frequency device comprising the substrate according to any one of claims 1 to 13.

Citation Information

Patent Citations

  • Alkali-doped and alkali-free boro-aluminosilicate glass

    JP2016528152A

  • Dynamic Polarization and Coupling Control for Movable Multilayer Cylindrical Feed Holographic Antennas

    JP2017506467A

  • Dynamic Polarization and Coupling Control for Movable Cylindrical Feed Holographic Antennas

    JP2017506471A