One-step method for producing liquid-tight, completely dense coatings

JP7568611B2Active Publication Date: 2024-10-16PRAXAIR ST TECHNOLOGY INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2021503015
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-08-05
Filing Date
2019-08-06
Publication Date
2024-10-16
Estimated Expiration
2039-08-06

AI Technical Summary

Technical Problem

Conventional thermal spray coating processes fail to produce liquid-tight, fully dense coatings suitable for high-pressure and high-temperature applications due to thermal degradation of polymer sealers and potential distortion or cracking, especially in components like aeronautical seals and valves.

Method used

A one-step high velocity oxy-fuel (HVOF) process with controlled oxygen dilution using inert gas reduces flame temperature, enabling the use of small particle sizes to create coatings without sealers, ensuring liquid-tightness and full density.

Benefits of technology

The process produces coatings that are impermeable to gases and liquids at pressures up to 10,000 psi and temperatures exceeding 350°F, eliminating the need for post-coating treatments and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000012_0000
    Figure 00000012_0000
  • Figure 00000012_0001
    Figure 00000012_0001
  • Figure 00000013_0000
    Figure 00000013_0000
Patent Text Reader

Abstract

Liquid-tight, fully dense coatings are prepared by a high velocity oxygen-fuel ("HVOF") process in which oxygen is diluted with an inert gas. The inert gas is combusted with the oxygen before it enters the combustion chamber. The resulting flame temperature is reduced by a controlled amount to eliminate, minimize, or reduce oxidation of the power feedstock injected into the thermal spray torch. The ability to reduce the flame temperature allows relatively small particle feedstock to be deposited without significant oxidation. The dilution process creates a fully dense, liquid-tight coating in the as-deposited state. [Selected Figure] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] (Related Applications) This application claims the benefit of priority to U.S. Patent Application No. 62 / 717,355, filed Aug. 10, 2018, which is hereby incorporated by reference in its entirety for all purposes.

[0002] (Field of the Invention) The present invention generally relates to a one - stage high - velocity oxygen fuel (“HVOF”) process for creating liquid - sealed, completely tight films for various applications. In particular, the HVOF process controls and dilutes oxygen with an inert gas to lower the flame temperature, thereby allowing the creation of a liquid - sealed, completely tight film without using a sealant and using a relatively small particle - size powder feedstock.

Background Art

[0003] Wear and corrosion are problems for substrate surfaces (e.g., metal substrate surfaces formed from nickel, cobalt, iron, and copper alloys) that are exposed to harsh corrosion conditions that can degrade their structural integrity. For example, aerospace seal components and valves used in oil and gas applications typically encounter high contact pressures and high - temperature conditions over their service life. Corrosion of these surfaces exacerbates wear and friction problems. Therefore, these components need to exhibit resistance to corrosion and be impermeable to gases and liquids.

[0004] Thermal spray coatings such as WCCrCo are routinely used for abrasion and corrosion protection. A second coating process, such as coating impregnation with a polymer sealer, is required to achieve near-perfect density. While abrasion-resistant coatings with polymer sealers have proven successful in lower operating pressure regimes below 15,000 psi and temperatures below 350°F, they typically become insufficient as oil supply and pump lines approach higher pressures and temperatures. At high temperatures, the coating can leak gases from itself due to thermal degradation of the polymer sealer. Without a coating with sufficient fluid impermeability, fluids can leak through the coating and ultimately through valves and seals.

[0005] Another two-step process for creating a perfectly dense coating involves the deposition of a self-fluxing alloy or a blend of a WC-based material and a self-fluxing alloy by thermal spraying, followed by flame melting or oven melting at temperatures exceeding 1800°F. In addition to employing a time-consuming and costly melting process, the main drawbacks of spray-molded coatings are the potential risks of distortion of the coated part and cracking of the coating if it does not conform to the substrate.

[0006] Considering the shortcomings of conventional coatings, there is an unmet need for an improved coating process to create a completely dense coating with liquid sealing capabilities. [Overview of the project]

[0007] The present invention may include any of the following embodiments in various combinations, and may also include any other embodiments of the present invention described below in the written description.

[0008] Other aspects, features, and embodiments of this disclosure will become more fully apparent from the following description and the appended claims.

[0009] In the first embodiment, there is a one-step method for creating a thin, liquid-sealed film immediately after deposition without sealing the film immediately after deposition, and the method includes the steps of: providing a substrate; providing a powder raw material having a particle size in the range of 1 to 15 micrometers; providing a thermal spray torch, wherein the thermal spray torch has a combustion chamber including a nozzle downstream of the combustion chamber; introducing fuel into the combustion chamber; pre-mixing oxygen gas with an inert gas to produce diluted oxygen gas, the pre-mixing being performed before the oxygen gas enters the combustion chamber, and the flow rate ratio of the inert gas to the oxygen gas being in the range of 8:92 to 50:50; introducing the diluted oxygen gas into the combustion chamber; burning the fuel with the diluted oxygen gas to generate a flame; introducing the powder raw material into the nozzle; contacting the powder raw material with the flame to produce substantially molten and semi-molten droplets; and directing the substantially molten and semi-molten droplets onto the substrate.

[0010] In a second embodiment, a one-step method for creating a thin, liquid-sealed film immediately after deposition without sealing the film immediately after deposition is provided, comprising the steps of: providing a substrate; providing a powder raw material having a particle size in the range of 1 to 15 micrometers; providing a thermal spray torch, the thermal spray torch including a combustion chamber, and the torch further including a nozzle downstream of the combustion chamber enclosed therein; introducing fuel into the combustion chamber; pre-mixing oxygen gas with an inert gas to produce diluted oxygen gas; directing the diluted oxygen gas into the combustion chamber; burning the fuel with the diluted oxygen gas to generate a flame in the combustion chamber; controlling the flame temperature in the combustion chamber; introducing the powder raw material into the nozzle; and heating the powder raw material to produce substantially molten or semi-molten droplets with reduced oxidation compared to a conventional high-speed oxygen fuel process using powder raw material having a particle size in the range of 1 to 15 micrometers.

[0011] In a third embodiment, a one-step thermal spray coating is produced by an oxygen-diluted high-speed oxygen fuel ("HVOF") process, without the use of a sealer, and is thin, liquid-sealed, and immediately after deposition. The coating is derived from a tungsten carbide-based powder composition having a particle size in the range of 1 to 15 micrometers and a coating thickness of 100 micrometers or less, and is characterized by a completely dense structure defined by the absence of visually detectable leaks at pressures of 10,000 psi or more and the absence of interconnected pores. [Brief explanation of the drawing]

[0012] The object and advantages of the present invention will be better understood from the following detailed description of its preferred embodiments, in reference to the accompanying drawings, which all have the same numbering and feature.

[0013] [Figure 1] A schematic diagram of a typical process according to the principle of the present invention is shown below.

[0014] [Figure 2] A schematic diagram of an alternative process according to the principle of the present invention is shown below.

[0015] [Figure 3] This shows the test setup used to reproduce high-pressure leaks.

[0016] [Figure 4] As described in Comparative Example 1, the results of a high-pressure leak test of a tungsten carbide-based thermal spray coating prepared using conventional HVOF are shown.

[0017] [Figure 5] As described in Comparative Example 2, the results of a high-pressure leak test of a tungsten carbide-based thermal spray coating using a powder size of 1 to 15 micrometers without oxygen dilution are shown.

[0018] [Figure 6] As described in Example 1, the results of the high-pressure leak test of the tungsten carbide-based thermal spray coating created by the present invention are shown,

[0019] [Figure 7] Under an optical microscope with a magnification of 500 times, the microstructure of the coating created by the present invention is shown,

[0020] [Figure 8] Under an optical microscope with a magnification of 500 times, the microstructure of the coating created by HVOF using a powder size of 1 to 15 micrometers without oxygen dilution is shown,

[0021] [Figure 9] The results of the substrate corrosion test of the tungsten carbide coating created by conventional HVOF are shown,

[0022] [Figure 10] The results of the substrate corrosion test of the tungsten carbide coating created by HVOF using a powder size of 1 to 15 micrometers without oxygen dilution are shown,

[0023] [Figure 11] As described in Example 2, the results of the substrate corrosion test of the tungsten carbide coating created by the present invention are shown.

Modes for Carrying Out the Invention

[0024] This disclosure is described herein in various embodiments and with reference to various features and aspects of the present invention. This disclosure contemplates various substitutions and combinations of features, aspects, and embodiments within the scope of this disclosure. Accordingly, this disclosure may be specified to comprise, consist of, or consist essentially of any such combination and substitution of these particular features, aspects, and embodiments, or of one or more selected ones thereof.

[0025] As described, the present invention provides a novel one-step method for creating a complete, dense coating with liquid sealing without using a sealer or melting step.

[0026] Unless otherwise stated, all compositions herein are expressed in weight percent and are intended to contain unavoidable trace amounts of contaminants.

[0027] As used herein, the term “fluid” is intended to refer to a liquid, slurry, gas, or vapor, or any combination thereof.

[0028] As used herein, the term “perfectly dense” is characterized by liquid sealing performance such that no visible fluid leakage is observed in high-pressure leak tests and no corrosion of the substrate is observed.

[0029] The term "high-pressure leak test" refers to the leak test performed in the examples and shown in Figures 4, 5, and 6.

[0030] As used in this specification and throughout, "one step" refers to the state immediately after film deposition.

[0031] As used herein and throughout this text, "flow ratio" means the flow ratio of the inert gas to the oxygen gas.

[0032] The terms “conventional HVOF” and “standard HVOF” are used interchangeably and are intended to refer to fast oxygen-fueled processes that do not use relatively fine particle sizes of 1–15 micrometers without oxygen dilution.

[0033] The terms "particle diameter" and "relatively fine particle size" are used interchangeably and are intended to refer to particle sizes between 1 and 15 micrometers.

[0034] Figure 1 shows a schematic diagram of a typical process of one embodiment of the present invention, called the oxygen-diluted HVOF process 100. The powder material 6 is introduced into the spray nozzle 2 of a thermal spray torch. The powder material 6 has a particle size in the range of about 1 to 15 micrometers. The powder material 6 may be any suitable chemical composition of thermal spray powder. In a preferred embodiment, the powder material 6 is a tungsten carbide-based material. The tungsten carbide-based material may have an 86%WC-10%Co-4%Cr formulation. Other compositions may also be used, for example, but are not intended to be limiting, such as 88%WC-12%Co, 83%WC-17%Co, 90%WC-10%Ni, and chromium carbide-based powder materials. The powder material 6 is injected radially into the spray nozzle 2 located downstream of the combustion chamber 1. The powder material 6 can be transported to the spray nozzle 2 using a suitable carrier gas such as nitrogen or argon. The carrier gas flow rate can be 20 to 50 scfh, but is generally 35 scfh or less. Higher carrier gas flow rates can cause the powder material 6 to erode the spray nozzle 2 prematurely, thereby shortening the operating life of the spray nozzle 2. Alternatively, or in addition, excessive carrier gas flow rates can adversely affect the coating properties. The exact amount of powder material 6 introduced into the spray nozzle 2 depends on several factors, including but not limited to the ratio of oxygen 4 flow rate to fuel 3 flow rate, the total flow rates of oxygen 4 and fuel 3, and powder chemistry.

[0035] Referring further to Figure 1, oxygen gas 4 is premixed with inert gas 5 before it comes into contact with fuel 3 in combustion chamber 1. Inert gas 5 is nitrogen, as shown in Figures 1 and 2. The inventors have found that the controlled addition of nitrogen gas 5 for premixing with oxygen gas 4 before combustion of fuel 3 can favorably lower the flame temperature compared to the flame temperature produced in a standard HVOF process, such that oxidation of relatively fine powder particles is reduced, eliminated, or minimized. As used herein and throughout, “flame temperature” is intended to refer to the temperature of the various by-products produced from the combustion of fuel 3 using oxygen gas 4 premixed with inert gas 5 or without inert gas 5, and as used herein and throughout, “flame” is intended to refer to the various by-products produced from the combustion of fuel 3 using oxygen gas 4 premixed with inert gas 5 or without inert gas 5.

[0036] Fuel 3 is introduced into the inlet of the combustion chamber 1. Any suitable fuel 3 can be used, including hydrocarbon-based fuels such as kerosene. Alternatively, fuel 3 may be hydrogen. It is preferable that oxygen gas 4 is introduced at a flow rate sufficient to burn substantially all of the fuel 3. Specifically, it is preferable that oxygen be introduced in an amount based on the stoichiometric ratio of fuel 3 to oxygen 4. Optimization of the HVOF dilution process 100 can occur when the flow rate ratio of nitrogen gas 5 to oxygen 4 is maintained above a lower limit and below an upper limit. In this way, the reduction in flame temperature as a result of premixing eliminates, minimizes or reduces the amount of oxidation that the relatively fine powder material 6 undergoes, thereby making it possible to utilize relatively fine particle sizes of about 1 to 15 micrometers. Relatively fine particle sizes preferably have a median particle size in the range of about 6 to 10 micrometers. In another embodiment, the powder material 6 may have a particle size in the range of 4 to 12 micrometers. The ability of the present invention to control the flame temperature and utilize such relatively fine particle sizes makes it possible to create a completely dense, liquid-sealed film.

[0037] The flow rate ratio of nitrogen gas 5 to oxygen gas 4 is maintained between a lower limit of 8:92 and an upper limit of 50:50. The inventors observed that when the flow rate ratio of nitrogen gas 5 to oxygen gas 4 falls below the lower limit of 8:92, the benefits of nitrogen dilution are not achieved. In particular, sufficient cooling of the flame does not occur, and the powder raw material 6 tends to undergo considerable oxidation due to the higher flame temperature, which imparts a considerable amount of heat to the relatively fine powder particles. Compared to conventional HVOF processes that utilize larger particle sizes, the relatively fine particles of the powder raw material 6 used in process 100 have a higher surface area ratio per unit volume, which means that the powder raw material 6 may deteriorate due to severe oxidation and decarburization before the powder raw material 6 particles collide with the surface of the substrate 10 and form a film. Films obtained with severe oxidation do not have the liquid sealing properties and completely dense structure of films prepared by the present invention. Instead, films obtained with severe oxidation have oxide content that essentially function as undesirable channels for gas leakage. Gas leaks through the coating can potentially lead to damage to the coating.

[0038] On the other hand, if nitrogen gas 5 is introduced in an amount exceeding the upper limit of a 50:50 flow ratio of nitrogen gas 5 to oxygen gas 4, the combustion reaction does not continue, and the flame tends to go out. As a result of excessive dilution of oxygen gas 4 beyond a 50:50 flow ratio, the flame temperature becomes too low, making it impossible to process powder particles.

[0039] In another aspect of the present invention, in addition to maintaining the flow rate ratio above the lower limit and below the upper limit, the total flow rates of nitrogen gas 5 and oxygen gas 4 introduced into the combustion chamber 1 are maintained within the range of 500 scfh to 3000 scfh, thereby creating and maintaining optimal conditions for burning diluted oxygen and fuel 3.

[0040] In another embodiment, the flow rate ratio of nitrogen gas 5 to oxygen gas 4 is maintained at 8:92 to 50:50, preferably 10:90 to 30:70, and more preferably 12:88 to 18:82.

[0041] Exemplary parameters for implementing the HVOF oxygen dilution process shown in Figure 1 include supplying nitrogen gas 5, pre-mixed with oxygen gas 4 at a flow rate of 50–600 scfh to oxygen gas 4 at a flow rate of 400–2500 standard cubic feet per hour (scfh), such that the weight ratio of nitrogen gas 5 to oxygen gas 4 is maintained at 8:92–50:50 and the total flow rate of oxygen gas 4 to nitrogen gas 5 is maintained at approximately 500–3000 scfh. Kerosene can be used as fuel 3 and is generally introduced into the combustion chamber 1 at a flow rate of 2.5–6.5 gallons per hour (gph).

[0042] Alternatively, in another aspect of the present invention, process 100 can be carried out using hydrogen as fuel 3. Hydrogen can be injected into the combustion chamber 1 of the torch at a flow rate of 1000 to 1800 scfh. A tungsten carbide-based powder raw material 6 having a size in the range of approximately 1 to 15 micrometers is supplied axially to the spray nozzle 2 at a supply rate of 20 to 100 grams per minute. Oxygen 4 is pre-mixed with nitrogen 5 to produce an oxygen dilution gas, as described above. The weight ratio of nitrogen gas 5 to oxygen gas 4 is maintained at a lower limit of 8:92 and an upper limit of 50:50, and the total flow rates of oxygen 4 and nitrogen 5 are maintained in the range of 500 scfh to 3000 scfh.

[0043] Referring further to Figure 1, when the powder material 6 is injected radially into the spray nozzle 2, the powder material 6 comes into contact with the flame and melts or partially melts. The particles flow out of the spray nozzle as an effluent 15 and are directed toward the substrate surface 20, where they solidify upon impact to form a film. Actual spraying by the HVOF process 100 in Figure 1 can be produced by a stationary or moving HVOF torch. When the substrate surface 20 is stationary, the HVOF torch device moves across the surface of the substrate 20 at a speed of 600 to 3200 inches per minute and an index of 0.2. The HVOF torch is maintained at a predetermined standoff distance (e.g., 2 to 10 inches) from the surface of the substrate 20.

[0044] Pre-mixing of oxygen gas 4 and nitrogen gas 5 is crucial to the present invention and must be performed before oxygen gas 4 enters the combustion chamber 1, as shown in Figures 1 and 2. If oxygen gas 4 and nitrogen gas 5 are not pre-mixed and instead introduced separately into the combustion chamber 1, a heterogeneous mixture is typically produced, which tends to create a turbulent regime within the combustion chamber 1, resulting in uneven flame temperature. Uneven flame temperature consists of hot and cold spots within the chamber 1. Ultimately, there is no uniform velocity distribution throughout the effluent 15 exiting the spray nozzle 2. As a result, some fine particles in the effluent 15 may be over-processed or under-processed, which can lead to excessive oxidation, decarburization, higher porosity, and unmelted particles in the resulting film deposited on the substrate 20.

[0045] The present invention's ability to create a completely dense, liquid-sealed coating using relatively fine particles by diluting oxygen gas eliminates the need to impregnate the coating with a sealer. Therefore, the so-called "one-step" process 100 does not require a subsequent step of applying a sealer. In contrast, conventional HVOF thermal spray coating processes inherently exhibit interconnected porosity, creating channels for gas to move along them, thereby requiring the application of a subsequent sealer.

[0046] The use of small particle sizes was difficult until the advent of this invention. In particular, the use of small particles was not considered a viable process embodiment for conventional HVOF processes, as it was observed that (i) the relatively fine particles tend to clog the spray nozzle 2, thus shortening the lifespan of the spray nozzle 2, and (ii) the oxidation and decarburization of such small particle sizes from the flame of conventional HVOF processes is excessive, potentially damaging the resulting film.

[0047] The present invention provides an oxygen-diluted HVOF thermal spraying process 100 for creating a liquid-sealing, perfectly dense coating immediately after deposition without the use of a sealer. Process 100 is designed to reduce or remove oxide inclusions by lowering the flame temperature. The liquid-sealing properties of the present invention can withstand relatively high pressure conditions, as shown in Example 1. Thus, the present invention not only provides acceptable liquid-sealing properties, but remarkably, it is provided without post-coating treatments such as the application of a sealer or melting of the coating. The liquid-sealing properties are exhibited at pressures of at least 10,000 psi that may be encountered by components (e.g., gate and seat components and ball valves used in oil and gas applications).

[0048] Figure 7 shows a micrograph of the film produced by process 100 under an optical microscope at 500x magnification. Compared to Figure 8, which shows a film produced using a conventional HVOF process with a powder having a particle size of 1 to 15 micrometers without pre-mixing of oxygen gas and inert gas, Figure 7 shows that the HVOF film produced by the present invention has lower porosity (porosity is indicated by voids) and lower oxide levels (oxide levels are indicated by gray stringers).

[0049] Furthermore, other process modifications can be conceived by the present invention. For example, Figure 2 shows an alternative embodiment of process 100 in which the powdered raw material 6 is injected axially into the combustion chamber 1. Furthermore, oxygen can be diluted to an appropriate level using other suitable inert gases besides nitrogen. For example, though not intended to be limiting, argon can be used as an inert gas to premix with oxygen to produce a diluted oxygen gas, the premixing of which takes place before the oxygen gas enters the combustion chamber.

[0050] In addition to the advantages described, the present invention overcomes many of the drawbacks of high-velocity air-fuel processes (HVAF) that utilize a mixture of air and fuel. Specifically, to maintain combustion in an HVAF, the oxygen content in the air is relatively low, so to maintain fuel combustion, a significantly larger amount of air must be introduced into the combustion chamber of the thermal spray torch of the present invention compared to the present invention. For example, in certain cases, the air flow rate in an HVAF process can be up to 10 times the total flow rate of oxygen and nitrogen gas required in the present invention. The higher the air flow rate for the HVAF, the more compressed air is required, thereby increasing the cost of running the HVAF process. In contrast, the present invention is far less expensive than HVAF because it can utilize lower flow rates of oxygen and inert gas to achieve sufficient combustion. The addition of nitrogen gas 5 is preferably less than 20 vol% of the total oxygen and nitrogen flow rate, which is dramatically different compared to an HVAF process with air consisting of 78 vol% nitrogen.

[0051] Furthermore, and in other embodiments, the present invention can create a fully dense, liquid-sealing film with the required properties at a substantially thinner thickness than conventional HVOF films. For example, in one embodiment of the present invention, the film thickness is 100 micrometers or less, more preferably 50 micrometers or less, and most preferably 25 micrometers or less, while still exhibiting the same properties as a conventional sealed HVOF film with a thickness of 100 micrometers or more. The liquid-sealing properties of the HVOF film produced by the present invention are characterized by the absence of visually detectable fluid leakage at pressures of 10,000 psi or more. The fully dense structure is defined by the absence of interconnected pores, which, by their absence, are sufficient to prevent fluid leakage through the film at the same thickness as or a fraction of that of a conventional sealed HVOF film.

[0052] The coatings prepared according to the present invention can withstand higher temperatures than previously possible with conventional coatings incorporating sealers that tend to degrade at high temperatures (e.g., above 350 degrees Fahrenheit). In this regard, the fully dense, liquid-sealed coatings prepared according to the present invention do not require impregnation and are therefore not formulated with certain types of polymer sealers. The examples described below quantify the improved performance of the fully dense coating system prepared according to the present invention compared to coatings prepared by conventional HVOF.

[0053] The liquid-sealing, fully dense coatings prepared according to the present invention are suitable for any substrate surface having one or more sealing surfaces. For example, but not limited to, coatings can be created on aerospace and industrial hydraulic components where cylinders or their mating surfaces (bushings or bearings) are at least partially coated using an oxygen-diluted HVOF process. Furthermore, the coatings prepared according to the present invention are particularly suitable for metal load-bearing surfaces, including but not limited to gate valve and ball valve components in fluid flow control systems.

[0054] As shown in the examples and discussed below, several experiments were conducted to compare the perfectly dense coatings prepared by the present invention with other HVOF coatings prepared by conventional processes. The criterion for success of the tests depended on the coating's ability to achieve and create a fluid-impermeable seal.

[0055] The experiment simulated the high-pressure conditions commonly encountered by gate valves used in oil and gas applications. High-pressure leaks were reproduced using the test specimens shown in Figure 3. Gas leaks were investigated through the coating using a high-pressure leak test. The test consisted of exposing a portion of the coated specimen to nitrogen at a pressure of 10,000 psi for at least 10 minutes, exposing another portion of the coated specimen to atmospheric pressure, and then coating it with a thin layer of leak detection fluid, as indicated by the arrows in Figure 3. If the coating was permeable to nitrogen gas, bubbles were observed on the coating surface during the test. Comparative Example 1

[0056] A tungsten carbide-based powder with a composition of 86%WC-10%Co-4%Cr powder was used to create a coating using a conventional high-speed oxygen fuel ("HVOF") coating process. Oxygen and kerosene fuel were introduced separately axially into the combustion chamber inlet of a commercially available thermal spray torch (Praxair TAFA JP-5000), and the tungsten carbide-based powder was injected radially into the spray nozzle. The tungsten carbide powder had a particle size in the range of 15 to 45 micrometers, with a median particle size of 30 micrometers. Oxygen gas was introduced at 2000 scfh. The oxygen gas was not diluted. Kerosene was introduced at a flow rate of 6.5 gallons per hour. The tungsten carbide-based powder was injected radially into the spray nozzle at a supply rate of 80 grams per minute. Nitrogen carrier gas at a flow rate of 22 scfh was used to transport the tungsten carbide-based powder to the spray nozzle.

[0057] The substrate to be coated remained stationary, while the torch was traversed and split across the part. The standoff distance between the torch and the part was 15 inches, and the surface velocity (i.e., torch speed) advanced along the flat surface of the part at 1800 inches per minute.

[0058] The completed film (200 micrometers) was applied to a sample with a diameter of approximately 2.8 inches and a thickness of approximately 1.5 inches for testing.

[0059] A high-pressure leak test was conducted on the coated substrate. At an applied pressure of 10,000 psi, a considerable amount of bubbles were observed around the test specimen, as shown in Figure 4. The large number of bubbles indicated that the coating lacked the ability to prevent leakage. Comparative Example 2

[0060] A tungsten carbide-based powder with a particle size in the range of 1 to 15 micrometers and a composition of 86% WC-10% Co-4% Cr powder was used to create a coating using a conventional HVOF coating process. The median particle size was 8 micrometers. Oxygen and kerosene fuel were introduced separately axially into the combustion chamber inlet of a commercially available thermal spray torch (Praxair TAFA JP-5000), and the tungsten carbide-based powder was injected radially into the spray nozzle. Oxygen gas was introduced at 1200 scfh. The oxygen gas was not diluted. Kerosene was introduced at a flow rate of 4 gallons per hour. The tungsten carbide-based powder was injected radially into the spray nozzle at a supply rate of 30 grams per minute. Nitrogen carrier gas was used at a flow rate of 35 scfh to supply the tungsten carbide-based powder to the spray nozzle.

[0061] The substrate to be coated remained stationary, while the torch was traversed and split across the part. The standoff distance between the torch and the part was 8 inches, and the surface velocity (i.e., torch speed) advanced along the flat surface of the part at 1800 inches per minute.

[0062] A thin, completed film (40 micrometers) was applied to a sample with a diameter of approximately 2.8 inches and a thickness of approximately 1.5 inches for testing.

[0063] A high-pressure leak test was conducted. At an applied pressure of 10,000 psi, a considerable amount of bubbles were observed around the test specimen, as shown in Figure 5. The large number of bubbles indicated that the coating lacked the ability to prevent leakage. Comparative Example 3

[0064] A tungsten carbide-based powder with a composition of 86%WC-10%Co-4%Cr powder was used to create a coating using a conventional high-speed oxygen fuel ("HVOF") coating process. Oxygen and kerosene fuel were introduced separately axially into the combustion chamber inlet of a commercially available thermal spray torch (Praxair TAFA JP-5000), and the tungsten carbide-based powder was injected radially into the spray nozzle. The tungsten carbide powder had particle sizes ranging from 10 to 38 micrometers. The median particle size was 18 micrometers. Oxygen gas was introduced at 1925 scfh. The oxygen gas was not diluted. Kerosene was introduced at a flow rate of 6.0 gallons per hour. The tungsten carbide-based powder was injected radially into the spray nozzle at a supply rate of 80 grams per minute. Nitrogen carrier gas at a flow rate of 32 scfh was used to transport the tungsten carbide-based powder to the spray nozzle.

[0065] The flat substrate to be coated remained stationary, while the torch was traversed and split across the part. The standoff distance between the torch and the part was 15 inches, and the surface velocity (i.e., torch speed) advanced along the flat surface of the part at 1800 inches per minute.

[0066] The completed, unsealed film (50 micrometers) was applied and tested on a flat sample measuring (4 inches x 3 inches x 3 / 4 inches).

[0067] Salt spray corrosion tests were conducted in accordance with ASTM B117 requirements. Within 72 hours of exposure to salt spray, signs of corrosion such as rust on the substrate, blistering of the coating, and fracture were observed (Figure 9). Comparative Example 4

[0068] A tungsten carbide-based powder with a particle size in the range of 1 to 15 micrometers and a composition of 86% WC-10% Co-4% Cr powder was used to create a coating using the HVOF coating process. The median particle size was 8 micrometers. Oxygen and kerosene fuel were introduced separately axially into the combustion chamber inlet of a commercially available thermal spray torch (Praxair TAFA JP-5000), and the tungsten carbide-based powder was injected radially into the spray nozzle. Oxygen gas was introduced at 1200 scfh. The oxygen gas was not diluted. Kerosene was introduced at a flow rate of 4 gallons per hour. The tungsten carbide-based powder was injected radially into the spray nozzle at a supply rate of 30 grams per minute. Nitrogen carrier gas was used at a flow rate of 35 scfh to supply the tungsten carbide-based powder to the spray nozzle.

[0069] The flat substrate to be coated remained stationary, while the torch was traversed and split across the part. The standoff distance between the torch and the part was 8 inches, and the surface velocity (i.e., torch speed) advanced along the flat surface of the part at 1800 inches per minute.

[0070] The completed, unsealed film (25 micrometers) was applied and tested on a flat sample measuring (4 inches x 3 inches x 3 / 4 inches).

[0071] Salt spray corrosion tests were conducted in accordance with ASTM B117 requirements. Within 96 hours of exposure to the salt spray, signs of corrosion, such as rust and blistering of the coating, were observed on the substrate (Figure 10). [Examples]

[0072] A tungsten carbide-based powder with a particle size in the range of 1 to 15 micrometers and a composition of 86% WC-10% Co-4% Cr powder was used to create a coating using an HVOF dilution process. The median particle size was 8 micrometers. The HVOF dilution process was carried out as described above in Figure 1, where the tungsten carbide-based powder was injected radially into the spray nozzle of a commercially available thermal spray torch (Praxair TAFA JP-5000). Diluted oxygen gas was produced by pre-mixing oxygen gas at a flow rate of 1200 scfh with nitrogen gas at a flow rate of 200 scfh. Subsequently, the diluted oxygen gas was injected into the combustion chamber at a total flow rate of 1400 scfh. Kerosene fuel was injected separately into the combustion chamber axially at a flow rate of 4 gallons per hour. The tungsten carbide-based powder was injected radially into the spray nozzle at a supply rate of 30 grams per minute. A tungsten carbide-based powder was supplied to the spray nozzle using a nitrogen carrier gas at a flow rate of 35 scfh.

[0073] The substrate to be coated remained stationary, while the torch was traversed and split across the part. The standoff distance between the torch and the part was 8 inches, and the surface velocity (i.e., torch speed) advanced along the flat surface of the part at 1800 inches per minute.

[0074] The completed coating was applied to a sample with a diameter of approximately 2.8 inches and a thickness of approximately 1.5 inches for testing. The resulting coating had a thickness of 40 micrometers.

[0075] A high-pressure leak test was conducted. Fifteen minutes after the test, no bubbles were observed in the test sample at an applied pressure of 10,000 psi, as shown in Figure 6. The absence of bubbles at high pressure indicated that the thin coating had the ability to prevent leakage.

[0076] This test demonstrates that, by pre-mixing oxygen and nitrogen gas in Example 1 according to the principle of the present invention, a liquid-sealed, completely dense coating can be created with a relatively thin thickness compared to Comparative Example 1.

[0077] This test demonstrates that the pre-mixing of oxygen and nitrogen gas in Example 1, based on the principle of the present invention, can create a completely dense film with the same thickness as the film in Comparative Example 2, using liquid sealing. [Examples]

[0078] A tungsten carbide-based powder with a particle size in the range of 1 to 15 micrometers and a composition of 86% WC-10% Co-4% Cr powder was used to create a coating using an HVOF dilution process. The median particle size was 8 micrometers. The HVOF dilution process was carried out as described above in Figure 1, where the tungsten carbide-based powder was injected radially into the spray nozzle of a commercially available thermal spray torch (Praxair TAFA JP-5000). Diluted oxygen gas was produced by pre-mixing oxygen gas at a flow rate of 1200 scfh with nitrogen gas at a flow rate of 200 scfh. Subsequently, the mixture was injected into the combustion chamber at a total flow rate of 1400 scfh. Kerosene fuel was injected separately into the combustion chamber axially at a flow rate of 4 gallons per hour. The tungsten carbide-based powder was injected radially into the spray nozzle at a supply rate of 30 grams per minute. A tungsten carbide-based powder was supplied to the spray nozzle using a nitrogen carrier gas at a flow rate of 35 scfh.

[0079] The flat substrate to be coated remained stationary, while the torch was traversed and split across the part. The standoff distance between the torch and the part was 8 inches, and the surface velocity (i.e., torch speed) advanced along the flat surface of the part at 1800 inches per minute.

[0080] The completed, unsealed film (25 micrometers) was applied and tested on a flat sample measuring (4 inches x 3 inches x 3 / 4 inches).

[0081] Salt spray corrosion tests were conducted according to ASTM B117 requirements. After 1000 hours of exposure to salt spray, no signs of corrosion were observed (Figure 11).

[0082] This test demonstrates that, by pre-mixing oxygen and nitrogen gas in Example 2 according to the principle of the present invention, a relatively thin, liquid-sealed, and dense corrosion-resistant coating can be created compared to Comparative Examples 3 and 4.

[0083] In addition to the advantages already mentioned, the ability of the oxygen-diluted HVOF process 100 to produce liquid-sealed, dense films exhibiting desired properties (including corrosion resistance to the substrate) at a fraction of the thickness of other films prepared by conventional processes substantially reduces the cost of HVOF films, thereby making HVOF films prepared by the present invention a viable alternative for many applications, including those that previously required chromium-based films. In this regard, prior to the present invention, HVOF films prepared by conventional HVOF processes cost an average of three times more than the film processes used to form hard chromium films. However, with the advent of the present invention, HVOF films become significantly more cost-effective as less film is required to produce the desired properties.

[0084] While we have shown and described what may be considered specific embodiments of the present invention, it will naturally be understood that various modifications and changes to the form or details can be readily made without departing from the spirit and scope of the invention. Accordingly, the present invention is not intended to be limited to the exact forms and details shown and described herein, nor to anything that falls short of the entire scope of the invention disclosed herein and claimed below.

Claims

1. A one-step method for producing thin, liquid-tight as-deposited coatings without sealing the as-deposited coating, providing a substrate; providing a powdered feedstock having a particle size in the range of 1 to 15 micrometers; providing a thermal spray torch, the thermal spray torch comprising a combustion chamber including a nozzle downstream of the combustion chamber; introducing fuel into the combustion chamber; Premixing oxygen gas with an inert gas to generate diluted oxygen gas, the premixing being performed before the oxygen gas enters the combustion chamber, and the flow ratio of the inert gas to the oxygen gas is in the range of 8:92 to 50:50; introducing the diluted oxygen gas into the combustion chamber; combusting the fuel with the diluted oxygen gas to generate a flame; introducing the powdered raw material into the nozzle; contacting the powdered feedstock with the flame to produce substantially molten or semi-molten droplets; directing said substantially molten or semi-molten droplets towards said substrate.

2. 10. The single-step process of claim 1, wherein the fuel is selected from the group consisting of hydrocarbons and hydrogen.

3. 10. The one-step process of claim 1, wherein the oxygen is introduced at a flow rate sufficient to combust the fuel.

4. 10. The one-step process of claim 1, wherein the inert gas is introduced at a flow rate sufficient to produce a flame temperature in the combustion chamber that is lower compared to a flame temperature generated without the inert gas.

5. 10. The one-step process of claim 1, wherein the total flow rate of the oxygen gas and the inert gas is 500 to 3000 scfh.

6. 10. The one-step process of claim 1, wherein the powdered feedstock is a tungsten carbide-based material.

7. 10. The one-step process of claim 1, wherein the powdered raw material has a particle size of about 4 to 12 micrometers.

8. 10. The one-step process of claim 1, wherein the powdered raw material has a median particle size of 6 to 10 micrometers.

9. A one-step method for producing thin, liquid-tight as-deposited coatings without sealing the as-deposited coating, providing a substrate; providing a powdered feedstock having a particle size in the range of 1 to 15 micrometers; providing a thermal spray torch, said thermal spray torch including a combustion chamber, said torch further including a nozzle enclosed therein and downstream of said combustion chamber; introducing fuel into the combustion chamber; premixing oxygen gas with an inert gas to produce diluted oxygen gas; directing the diluted oxygen gas into the combustion chamber; burning the fuel with the diluted oxygen gas to generate a flame in the combustion chamber; controlling a flame temperature in the combustion chamber; introducing the powdered raw material into the nozzle; and heating the powdered feedstock to produce substantially molten or semi-molten droplets with reduced oxidation compared to conventional high velocity oxygen-fuel processes using the powdered feedstock having particle sizes in the range of 1 to 15 micrometers.

10. 10. The one-step process of claim 9, wherein premixing the oxygen gas with the inert gas results in a flow ratio of the inert gas to the oxygen gas ranging from 8:92 to 50:

50.

11. 10. The single-stage process of claim 9, wherein the total flow rate of the oxygen and the nitrogen is from 500 to 3000 scfh.

12. 10. The one-step method of claim 9, wherein the powder feedstock comprises a tungsten carbide-based material or a chromium carbide-based material.

13. 10. The one-step method of claim 9, wherein the powdered raw material is injected into the nozzle in a radial direction.

14. 10. The one-step process of claim 9, wherein the powdered raw material has a median particle size of 6 to 10 micrometers.

15. 10. The one-step process of claim 9, wherein premixing the oxygen gas with the inert gas results in a flow ratio of the inert gas to the oxygen gas ranging from 10:90 to 30:

70.

16. 10. The one-step process of claim 9, wherein premixing the oxygen gas with the inert gas results in a flow ratio of the inert gas to the oxygen gas in the range of 12:88 to 18:

82.

17. 1. A sealer-free, thin, liquid-tight, as-deposited, single-step thermal spray coating produced by an oxygen-diluted high velocity oxygen-fuel ("HVOF") process, said coating being derived from a tungsten carbide-based powder composition having a particle size ranging from 1 to 15 micrometers and a coating thickness of 100 micrometers or less, said liquid-tightness being characterized by the absence of visually detectable leaks at pressures of 10,000 psi or greater and a fully dense structure defined by the absence of interconnected porosity.

18. 18. The coating of claim 17, wherein the corrosion resistance is characterized by the absence of corrosion of the substrate.