Low melting point metal or alloy powder atomization manufacturing process
The novel atomization process for low melting point metals and alloys achieves precise control over particle size and shape, addressing the limitations of conventional methods by producing fine, spherical powders suitable for electronic components and other applications.
Patent Information
- Application Number
- JP2022189250
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2016-08-24
- Filing Date
- 2022-11-28
- Publication Date
- 2024-10-16
- Estimated Expiration
- 2037-05-05
AI Technical Summary
Conventional techniques struggle to produce fine metal powders with low melting points, particularly those with a small standard deviation in particle size and spherical shape, which are essential for smaller electronic components and other applications like metal injection molding and thermal spraying.
A novel atomization process involving a melt diversion and controlled atomizing gas stream, combined with water in the atomization chamber, to achieve a spherical fine powder with a narrow particle size distribution and low geometric standard deviation.
The process effectively produces metal powders with an average particle diameter of less than 20 microns and a geometric standard deviation of less than 2.0, ensuring high product quality and performance.
Smart Images

Figure 0007568700000008 
Figure 0007568700000009 
Figure 0007568700000010
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority to co-pending U.S. Provisional Patent Application No. 62 / 378,734, filed Aug. 24, 2016, which is incorporated herein by reference in its entirety.
[0002] The field of the disclosure relates to the production of fine metal powders for applications in the electronics industry, metal injection molding, thermal spraying, thermal spray welding, and 3D printing. [Background technology]
[0003] During the past few decades, the size of electronic devices and components has been significantly reduced. This has a direct impact on the dimensions of the internal components and metallization of such devices. Solder pastes are widely used for point contacts between different components or layers inside electronic devices. These pastes consist of metal powders and flux to ensure proper melting and adhesion to other components. The metal components in solder pastes are generally in the form of "low melting alloys" or "low melting metals" and the size distribution of such metal powders depends on the size of the point contact. Smaller electronic devices and components require smaller contacts and hence there is an increasing demand for solder pastes with metal powders having smaller size distribution. It is not uncommon for particle size distributions mainly below 20 microns and even below 10 microns to be required or requested.
[0004] There are several other applications for fine metal powders, such as metal injection molding, thermal spraying, thermal spray welding, 3D printing and many others.
[0005] Conventional techniques (atomization, centrifugal disintegration, water atomization...) are able to produce fine powders, but the particle size standard deviation and spherical shape of the particles are difficult to achieve from low melting point alloys, which often results in low recovery of the resulting powders in defined size fractions from these techniques. Summary of the Invention
[0006] This disclosure describes a novel production process for metal powders with low melting points that produces fine spherical powders with small standard deviations in particle diameter.
[0007] In a first aspect, a low melting point metal or alloy powder atomization manufacturing process is provided. In at least one embodiment, the process can include: providing a melt of the low melting point metal or alloy through a supply pipe; diverting the melt at a diverting angle with respect to the central axis of the supply pipe to obtain a diverted melt; directing the diverted melt to an atomization area; and providing at least one atomization gas stream to the atomization area.
[0008] The atomization process may be carried out in the presence of water in the atomization chamber used for said atomization process.
[0009] In a second aspect, a low melting point metal or alloy powder atomization manufacturing process is provided. The process may include: providing a melt of the low melting point metal or alloy through a supply tube; delivering the melt to an atomization area through a diverter; providing at least one atomization gas stream to the atomization area; and delivering water to the atomization chamber used for the atomization process. In such a process, the melt may be diverted in a diverter at a certain diverging angle with respect to the central axis of the supply tube before being delivered to the atomization area.
[0010] In a third aspect, a low melting point metal or alloy powder atomization manufacturing process is provided, comprising providing a melt of said low melting point metal or alloy through a feed tube; directing the melt to an atomization area; and providing at least one atomization gas stream to the atomization area having an average gas velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least 1 / cm 2 of atomized metal. 3 Approximately 5000 to 30000 cm 3 providing at least one atomizing gas stream of at least one atomizing gas having a mean particle diameter of less than 20 microns and a geometric standard deviation of less than about 2.0;
[0011] In a fourth aspect, a low melting point metal or alloy powder atomization manufacturing process is provided, comprising providing a melt of said low melting point metal or alloy through a feed tube; optionally diverting said melt at a diverting angle with respect to a central axis of the feed tube to obtain an optionally diverted melt; optionally directing the diverted melt towards an atomization area; and providing at least one atomization gas stream to the atomization area having a velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least 1 cm 2 of atomized metal. 3 providing at least one atomizing gas stream of about 5,000 to about 30,000 cm3 of gas per cubic centimeter, thereby resulting in a powder particle size distribution having a geometric standard deviation of less than about 2.0.
[0012] For a better understanding of the various embodiments described herein, and to show more clearly how these may be put into effect, reference is made to the accompanying drawings, in which is shown, by way of example, at least one example embodiment. [Brief description of the drawings]
[0013] [Figure 1]FIG. 2 is a block diagram illustrating the steps involved in an atomization process, according to at least one embodiment. [Diagram 2] FIG. 1 shows a schematic side view of an atomization nozzle having a feed tube with diverter channels for providing melt to an atomization area, according to at least one embodiment. [Diagram 3] FIG. 1 illustrates a perspective view of an atomization chamber showing tangential gas incidence on the gas inlet according to at least one embodiment. [Figure 4A] 1 is a scanning electron microscope (SEM) photograph of the powder obtained in Example 1, showing Type 5 powder (15-25 μm). [Figure 4B] 1 is a scanning electron microscope (SEM) photograph of the powder obtained in Example 1, showing Type 7 powder (1-11 μm). [Figure 5A] FIG. 2 is an SEM photograph of the powder obtained in Example 3, showing Type 5 powder (15-25 μm). [Figure 5B] FIG. 2 is an SEM photograph of the powder obtained in Example 3, showing Type 6 powder (5-15 μm). [Figure 6] 1 shows an SEM photograph of the powder (7-25 μm) obtained in Example 4. [Figure 7A] 1 is a SEM photograph of the powder obtained in Example 5, showing +25 μm powder. [Figure 7B] 1 is a SEM photograph of the powder obtained in Example 5, showing −25 μm / +10 μm powder. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The following examples are provided in a non-limiting fashion.
[0015] The expression "low melting point metal" as used herein refers to a metal having a melting point temperature between about 50°C and about 500°C.
[0016] The expression "low melting point alloy" as used herein refers to an alloy having a liquidus temperature between about 50°C and about 500°C.
[0017] In the production of fine metal powders there are several parameters that can affect the product quality. Some of the parameters used to characterize the powder include the average size distribution, the standard deviation of the size distribution, the percentage of coarser and finer particles above / below a predefined size, the sphericity of the powder, the level of metal impurities and the oxygen level.
[0018] In at least one embodiment, the diversion angle (90-β) may be from about 30 to about 70 degrees.
[0019] In at least one embodiment, the diversion angle may be from about 10 to about 90 degrees.
[0020] In at least one embodiment, the angle formed between the atomizing gas and the melt may be from about 10 to about 90 degrees.
[0021] In at least one embodiment, the angle formed between the atomizing gas and the melt may be from about 40 degrees to about 90 degrees.
[0022] In at least one embodiment, the process can include providing a low melting point metal.
[0023] In at least one embodiment, the low melting point metal can have a melting point of about 150°C to about 500°C.
[0024] In at least one embodiment, the ratio of atomizing gas to low melting point metal in the atomizing area is 1 / cm 2 of atomizing metal. 3 Approximately 10,000 to 20,000 cm 3 The gas may be
[0025] In at least one embodiment, the ratio of atomizing gas to low melting point metal in the atomizing area is 1 / cm 2 of atomizing metal. 3 Approximately 5000 to 30000 cm 3 The gas may be
[0026] In at least one embodiment, the low melting point metal may be an element selected from Zn, In, Sn, Pb, Se, Te, and Bi.
[0027] In at least one embodiment, the process can include providing a low melting point alloy.
[0028] In at least one embodiment, the low melting point alloy can have a liquidus between about 75°C and about 500°C.
[0029] In at least one embodiment, the low melting point alloy can have a liquidus between about 100°C and about 300°C.
[0030] In at least one embodiment, the ratio of atomizing gas to low melting alloy is 1 cm of metal. 3 Approximately 10,000 to 20,000 cm 3 The gas may be
[0031] In at least one embodiment, the ratio of atomizing gas to low melting alloy is 1 cm 2 of metal 3 Approximately 5000 to 30000 cm 3 The gas may be
[0032] In at least one embodiment, the low melting alloy may include at least one element selected from Cu, Sb, Zn, In, Mg, Sn, Pb, Ag, Se, Te, Ga, and Bi.
[0033] In at least one embodiment, the atomized gas stream can have a velocity of about 300 m / s to about 700 m / s.
[0034] In at least one embodiment, the atomized gas stream can have a velocity of about 450 m / s to about 600 m / s.
[0035] In at least one embodiment, the atomized gas stream can have a supersonic velocity.
[0036] In at least one embodiment, the atomizing gas may be delivered to the atomizing head through at least one gas inlet oriented non-perpendicular to the atomizing head, the gas inlet providing a swirling motion in the atomizing head before the gas exits.
[0037] In at least one embodiment, the at least two gas injectors may be offset relative to a central axis of the supply tube to create a dynamic rotation effect about the central axis in the atomization area.
[0038] In at least one embodiment, the process may thus provide a powder particle size distribution having a geometric standard deviation of about 1.8 or less.
[0039] In at least one embodiment, the process may thus provide a powder particle size distribution having a geometric standard deviation of from about 1.5 to about 1.8.
[0040] In at least one embodiment, the atomization chamber can contain from about 0 to about 20% oxygen.
[0041] In at least one embodiment, the water may include at least one additive to reduce the redox potential of the water.
[0042] In at least one embodiment, the redox potential of the water is reduced prior to atomization.
[0043] In at least one embodiment, the temperature of the water used in the atomization chamber is reduced to reduce powder oxidation during the atomization process.
[0044] In at least one embodiment, the process may thus provide an average powder particle size of from about 3 microns to about 20 microns in diameter.
[0045] In at least one embodiment, the melt of the low melting point metal can be diverted through at least one melt diverter channel, and a diverter angle can be formed between a central axis of the supply tube and the at least one melt diverter channel.
[0046] In at least one embodiment, the alloy melt may be diverted through at least two melt diverter channels, and a diverter angle may be formed between a central axis of the supply tube and the at least two melt diverter channels.
[0047] In at least one embodiment, at least one jet of water can be sprayed into the atomization chamber.
[0048] In at least one embodiment, at least one jet of water can be sprayed onto at least one wall of the atomization chamber.
[0049] In at least one embodiment, the process may thus provide a powder having an average particle size of less than about 20 microns.
[0050] In at least one embodiment, the process may thus provide a powder having an average particle size of less than about 10 microns.
[0051] In at least one embodiment, the powder produced can be vacuum dried to avoid powder oxidation.
[0052] In at least one embodiment, the powder produced may be washed with an organic solvent to remove most of the water prior to the drying step.
[0053] In a fifth aspect, an atomization apparatus for producing low melting point metal or alloy powder is provided. The apparatus may include: a supply pipe for providing a melt of the low melting point metal or alloy; a diverter in fluid communication with the supply pipe for diverting the melt at a diversion angle with respect to a central axis of the supply pipe to obtain a diverted melt and directing the diverted melt to an atomization area of the atomization apparatus; at least one atomization gas injector for providing at least one atomization gas stream to an atomization area disposed inside the atomization chamber; and at least one water inlet for providing water in the atomization chamber of the atomization apparatus.
[0054] In at least one embodiment, the diverter may include a melt diversion conduit that is oriented at a diversion angle relative to a central axis of the feed pipe.
[0055] In at least one embodiment, the diverter may include at least two melt diversion conduits, each of the at least two melt diversion conduits oriented at a diversion angle relative to a central axis of the feed pipe.
[0056] In at least one embodiment, the apparatus may include at least one gas inlet, the at least one gas inlet being non-perpendicular to the atomizing head to provide a pivoting motion in the atomizing head and a dynamic rotational motion in the atomizing area and atomizing chamber.
[0057] In at least one embodiment, at least one non-vertical gas inlet can generate a circular flow in the atomizing head, resulting in a dynamic rotational motion of the gas in the atomizing area and atomizing chamber.
[0058] In at least one embodiment, the at least two gas inlets may be non-perpendicular to the atomizing head, creating a swirling effect in the atomizing head and a dynamic rotation effect in the atomizing area and atomizing chamber.
[0059] In at least one embodiment, the at least one water inlet can be disposed inside the atomization chamber.
[0060] In at least one embodiment, at least one water inlet may be suitable for providing water for cooling the powder.
[0061] In at least one embodiment, at least one water inlet may be suitable for providing water for transporting the powder to a screening / drying area.
[0062] In at least one embodiment, at least one water inlet may be suitable for providing water to facilitate sorting / sieving of the powder.
[0063] The described process is based on a known concept, atomization, but with some specific improvements. These improvements include changes to the atomization head operating parameters, the atomization chamber configuration and the means of post-processing of the powder before final product packaging (collection, sieving and drying). The process is designed to reach high product quality and high process performance.
[0064] 1 shows a block diagram 100 of the equipment and steps involved in an atomization process, according to at least one embodiment. FIG 1 shows a melting furnace 102, an atomization nozzle 200, an atomization chamber 108, a powder recovery system 112, and a sieving system 114.
[0065] Most low melting alloys and / or metals produced using this process are sensitive to oxidation, so the atomizing gas can conveniently be an inert gas. The system can be maintained at near inert conditions, typically with oxygen levels well below 21% in the atomizing chamber 108. To reduce operating costs, this gas can be purified / recycled in the process.
[0066] In at least one embodiment, the atomization manufacturing process can be performed by an atomization nozzle 200, where an atomization gas meets the metal flow at certain conditions described herein. Also shown in Figure 1 is a schematic side view of the atomization nozzle 200, where the molten metal can contact the atomization gas in the atomization zone.
[0067] Once the metal has been solidified into a fine powder, it is sieved and packaged.
[0068] Referring to FIG. 1, some water may be added to the atomization chamber 108 through side nozzles 120 and 122 to aid in powder recovery and deliver the liquid mixture of powder and water to the sieving area 114. These water-addition side nozzles 120 and 122 may be oriented toward the atomization chamber walls to aid in powder cooling and to avoid particle adhesion / deformation on the atomization chamber walls, or may be located within the atomization area. Water may also be added to facilitate powder recovery and sieving. The powder produced may then be sieved and dried. After recovery of the majority of the powder from the liquid stream, the majority of the powder passes into a filter press 116 to recover any remaining powder in suspension before water recycle / disposal.
[0069] The size distribution of the powder produced during the optimized manufacturing process can be influenced by the speed at which the atomizing gas hits the metal. In this regard, a higher speed of the atomizing gas results in a lower size distribution of the powder. If the atomizing nozzle 200 is not properly designed, less metal will interact with the atomizing gas at the required conditions (speed and volume of the atomizing gas) and a greater variation in the size and shape of the powder produced can be observed. Intimate contact between the low melting point metal / alloy and the atomizing gas is also important.
[0070] 2 shows a schematic side view of an atomizing nozzle 200. The atomizing nozzle 200 has a feed tube 210 with a branch channel 216 to provide melt at an atomizing area 230.
[0071] 2, the atomizing nozzle described herein includes a feed pipe 210 disposed between the melting furnace 102 and the atomizing area 230, which includes a diverter 216 (also referred to herein as a diversion channel 216). The role of this diverter 216 is to provide better contact between the metal and the gas in the atomizing zone 230.
[0072] The metal is impinged into the atomizing gas stream at a sheer angle γ, defined as γ=90−β+α. This approach provides additional parameters to improve the atomization process: the β angle, as well as the diameter and number of diverter channels 216.
[0073] In at least one embodiment, the metal may be diverted in the atomization area 230 at a β angle that is between about 20 and about 60°. For example, the atomization gas may be provided to the atomization area 230 at an α angle of between about 20 and about 35°.
[0074] For example, when the shear angle γ is about 90°, or at least about 60 to about 120°, atomization can be improved due to enhanced gas to metal contact and higher sheer energy.
[0075] The melt split angle is also defined herein as 90-β.
[0076] The α angle at which the atomization gas may be provided to the supply tube 210 may also have other limitations. For example, if the angle α exceeds 60°, nearly direct projection of the atomization gas on the atomization chamber wall may require a larger atomization chamber diameter.
[0077] For example, the alpha angle may be as low as about 20 to about 45 degrees.
[0078] For example, the alpha angle may be less than about 20 to about 45 degrees.
[0079] In at least one embodiment, the alpha angle can be from about 0 to about 90 degrees; from about 10 to about 50; from about 15 to about 50; or from about 20 to about 50.
[0080] In at least one embodiment, the α angle can be from about 20 to about 45°, where 2α can be from about 40° to about 90°. In at least one embodiment, the α angle can be from about 20 to about 40;
[0081] As soon as the atomizing gas hits the metal / alloy, small particles are formed. Collisions between those particles can generate satellites (many particles linked together) and can also generate non-spherical metal particles, both of which need to be avoided and / or reduced or prevented. This can be done in part by modifying the α and β angles, as well as the average atomizing gas velocity and dispersion factor.
[0082] In order to avoid collisions before solidification, the density of the particles in the atomizing gas must be controlled within an appropriate range. For example, 1 cubic centimeter (cc) of metal is 1M 3 When spherical particles of 10 microns diameter are atomized in an atomizing gas of 1000 MPa, the density of the particles in the plume is 1.9 million / M 3 5M per cubic centimeter of metal. 3 The use of gas of 10000 m3 per cubic centimeter of metal / alloy would reduce this density by a factor of 5. Therefore, the optimum range of gas volume per volume of metal is important to avoid collisions, to provide the shear energy to break the metal into droplets, and also to provide the proper heat exchange mechanism to rapidly solidify the droplets. 3 The use of an atomizing gas of has been found to be suitable for the production of fine powders (less than 20 microns) of low melting point metals / alloys.
[0083] Velocity and dispersion are described herein as important factors influencing atomization results (finess and avoidance of satellites and non-atomized metal / alloy).
[0084] In at least one embodiment, the atomization apparatus 150 may include at least one atomization gas inlet 214 that is non-perpendicular to the gas supply line axis 212, resulting in rotational motion of the atomization gas stream 240 in the atomization head 222. In an extreme embodiment described below, the gas inlet 214 enters the atomization head tangentially.
[0085] 3 shows a perspective view of an atomization chamber 300 showing tangential gas inlets 311 and 314 according to at least one embodiment. This design allows for an asymmetric atomization plume in dynamic rotation about the central axis 312. This arrangement of the atomization gas inlets can result in improved particle size distribution compared to atomizers with gas inlets perpendicular to the feed tube central axis 312.
[0086] Typically, many low melting point metals / alloys are difficult to solidify. This may be due to poor heat transfer at low temperatures by convection compared to atomization of high temperature alloys / metals where radiation and higher convection cooling may play an important role. If some particles touch the walls of the atomization chamber 108 and are still partially molten or close to their melting point, they may be significantly deformed to reach a flake type morphology, agglomerate, and form non-spherical particles or satellites (several particles are linked together). To reduce these phenomena, the described atomization technique can use water as a cooling medium. Water can be injected in the direction of the atomization chamber walls to provide a water film that carries the generated powder. The water film can ensure that the metal powder or metal droplets are cooled at a sufficient temperature to reduce or avoid attached particles, satellites and / or deformed particles. Water can provide a controlled level of surface oxidation in some cases, which can also contribute to have a free-flowing powder with an acceptable level of oxygen in the final product.
[0087] For example, the addition of water in the atomization chamber (on the wall, at the top of the atomization chamber, or at the bottom of the atomization chamber) may also improve material sorting. It is sometimes difficult to separate particles when dry sieving is used because electrostatic forces are built up between the fine particles. Some low melting point alloy / metal powders tend to clump together for many reasons, such as sintering or adhesion of particles and also due to electrostatic reasons, as mentioned above. The exact reasons for clumping are not fully understood for all low melting point / alloys produced, but for some alloys a wet sieving system is advantageous.
[0088] The use of water in this process may be counterintuitive since some alloying elements / metals may theoretically oxidize in the presence of water. Some elements, such as tin, may even reduce water in the absence of dissolved oxygen in the water. For example, if low oxygen levels are maintained in the atomization chamber, oxidation of the powder produced may be within acceptable levels. In addition to controlling the oxygen in the atmosphere of the atomization chamber, the redox potential and temperature of the water used in the process (for the atomization chamber and sieving) may be controlled, resulting in reduced kinetics of oxidation.
[0089] Some metal powders made of low melting point metals / alloys may require controlled oxidation to remain free-flowing in the final product. For example, if pure tin is produced in fine powder with very low levels of oxygen (100 ppm or less), the products may stick to each other after sieving and drying. The presence of water in the process at a reasonably low temperature and with a controlled redox potential tends to provide this level of oxidation. Optionally, oxygen peroxide or other wet smelting oxidizing agents may be added to allow a controlled level of oxidation. Alternatively, the powder may be left in water (with or without steering) for a predetermined period of time at a controlled temperature to allow controlled oxidation of the powder.
[0090] Controlled oxidation is beneficial for some products, but excessively high levels can generally be harmful. Optionally, the redox potential of the incoming water may be reduced to limit oxidation. This can be done by adding additives to the water used in the atomization process (in the chamber or sieving system) to reduce the level of oxygen in the final product. The additives may be reducing agents, such as organic additives or inorganic reducing agents, such as ethanol, methanol, formic acid, acetic acid, methanesulfonic acid, etc. The redox potential in the water can also be reduced by a variety of other means, including but not limited to electrochemical systems for treating the incoming water, reducing the temperature, and filters with reactive metal powders.
[0091] In at least one embodiment, the dissolved oxygen in the incoming water can be controlled to limit oxidation in the product. In at least one embodiment, the metal film on the powder can be reduced by dissolution with weak acids (HCl, organic acids, etc.). These can be added to the water to reduce the oxide film that forms on the powder surface.
[0092] One of the final product steps of the process is drying the powder. This step can be carried out in air, under vacuum or in an inert gas. The vacuum allows the drying process to operate at a lower temperature, thus reducing the possibility of oxidation by water. Optionally, prior to the drying stage, water may be driven off from the powder using an organic solvent in which it is soluble, such as ethanol and methanol. After the water is removed, the powder, which contains some residual organic liquid, can be dried to produce a final product with low levels of oxygen.
[0093] In at least one embodiment, a low melting point metal or alloy powder atomization manufacturing process may include providing a melt of the low melting point metal or alloy through a supply tube; diverting the melt at a diversion angle with respect to a central axis of the supply tube to obtain a diverted melt; directing the diverted melt to an atomization area; and providing at least one atomization gas stream to the atomization area. The atomization process is carried out in the presence of water in an atomization chamber used for the atomization process.
[0094] In at least one embodiment, a low melting point metal or alloy powder atomization manufacturing process may include providing a melt of the low melting point metal or alloy through a supply tube; delivering the melt to an atomization area through a diverter; providing at least one atomization gas stream to the atomization area; and delivering water to an atomization chamber used for the atomization process, where the melt is diverted in the diverter at a diverting angle relative to a central axis of the supply tube before being delivered to the atomization area.
[0095] In at least one embodiment, a low melting point metal or alloy powder atomization manufacturing process may include providing a melt of said low melting point metal or alloy through a feed tube; directing the melt to an atomization area; and providing at least one atomization gas stream to the atomization area having an average gas velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least 1 / cm 2 of atomized metal. 3 Approximately 5000 to 30000 cm 3of gas, thereby providing a powder distribution having an average particle diameter of less than 20 microns and a geometric standard deviation of less than about 1.8. In at least one embodiment, a low melting point metal or alloy powder atomization manufacturing process may include providing a melt of said low melting point metal or alloy through a feed tube; directing the melt to an atomization area; and providing at least one atomization gas stream to the atomization area having an average gas velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least 1 / cm of metal being atomized. 3 Approximately 5000 to 30000 cm 3 of gas, thus providing a powder distribution having a mean particle diameter of less than 20 microns and a geometric standard deviation of less than about 2.0.
[0096] In at least one embodiment, a low melting point metal or alloy powder atomization manufacturing process may include providing a melt of said low melting point metal or alloy through a feed tube; directing the melt to an atomization area; and providing at least one atomization gas stream to the atomization area having an average gas velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least 1 / cm 2 of atomized metal. 3 Approximately 5000 to 30000 cm 3 of gas, thereby providing a powder distribution having an average particle diameter of less than 20 microns and a geometric standard deviation of less than about 1.8. In at least one embodiment, a low melting point metal or alloy powder atomization manufacturing process may include providing a melt of said low melting point metal or alloy through a feed tube; directing the melt to an atomization area; and providing at least one atomization gas stream to the atomization area having an average gas velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least about 1 / cm of atomized metal. 3 Approximately 5000 to 30000 cm 3of gas, thereby providing a powder distribution having a mean particle diameter of less than 20 microns and a geometric standard deviation of less than about 2.0.
[0097] The low melting point metal or alloy powder atomization manufacturing process may include providing a melt of said low melting point metal or alloy through a feed tube; optionally diverting said melt at a diverting angle with respect to a central axis of the feed tube to obtain an optionally diverted melt; optionally directing the diverted melt towards an atomization area; and providing at least one atomization gas stream to the atomization area having a velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least 1 / cm 2 of atomized metal. 3 Approximately 5000 to 30000 cm 3 of gas, thus providing a powder particle size distribution having a geometric standard deviation of less than about 1.8. A low melting point metal or alloy powder atomization manufacturing process may include providing a melt of said low melting point metal or alloy through a feed tube; optionally diverting said melt at a diverting angle with respect to a central axis of the feed tube to obtain an optionally diverted melt; optionally directing the diverted melt towards an atomization area; and providing at least one atomization gas stream to the atomization area having a velocity of at least 300 m / s, wherein the ratio of atomization gas to low melting point metal in the atomization area is at least 1 / cm of atomized metal. 3 Approximately 5000 to 30000 cm 3 of gas, thus providing a powder particle size distribution having a geometric standard deviation of less than about 2.0.
[0098] For example, the flow diversion angle (90-β) may be from about 30 to about 70°.
[0099] For example, the diversion angle may be from about 10 to about 90 degrees.
[0100] For example, the angle formed between the atomizing gas and the molten material may be about 10 to about 90°. For example, the angle formed between the atomizing gas and the molten material may be about 40 to about 90°.
[0101] In at least one embodiment, the process may also include providing a low melting point metal.
[0102] In at least one embodiment, the low melting point metal can have a melting point of about 150°C to about 500°C.
[0103] In at least one embodiment, the ratio of atomizing gas to low melting point metal in the atomizing area is 1 / cm 2 of atomizing metal. 3 Approximately 10,000 to 20,000 cm 3 In at least one embodiment, the ratio of atomizing gas to low melting point metal in the atomizing area is 1 cm of atomizing metal. 3 Approximately 5000 to 30000 cm 3 The gas may be
[0104] In at least one embodiment, the low melting point metal may be an element selected from Zn, In, Sn, Pb, Se, Te, and Bi.
[0105] In at least one embodiment, the process can include providing a low melting point alloy.
[0106] In at least one embodiment, the low melting point alloy can have a liquidus between about 75°C and about 500°C.
[0107] In at least one embodiment, the low melting point alloy can have a liquidus between about 100°C and about 300°C.
[0108] In at least one embodiment, the ratio of atomizing gas to low melting alloy is 1 cm 2 of metal 3 Approximately 10,000 to 20,000 cm 3 The gas may be
[0109] In at least one embodiment, the ratio of atomizing gas to low melting alloy is 1 cm 2 of metal 3 Approximately 5000 to 30000 cm 3 The gas may be
[0110] In at least one embodiment, the low melting point alloy can include at least one element selected from Cu, Sb, Zn, In, Mg, Sn, Pb, Ag, Se, Te, Ga, and Bi.
[0111] In at least one embodiment, the atomized gas stream can have a velocity of about 300 m / s to about 700 m / s. In at least one embodiment, the atomized gas stream can have a velocity of about 450 m / s to about 600 m / s. In at least one embodiment, the atomized gas stream can have a supersonic velocity.
[0112] In at least one embodiment, atomization gas may be delivered to the atomization head through at least one gas inlet 314, 311 oriented non-perpendicular to the metal supply tube axis 312, providing a swirling motion of the atomization gas stream 240 in the atomization head 222 prior to the gas exit.
[0113] In at least one embodiment, the at least two gas inlets 311, 314 may be tangential to the central axis 312 of the supply tube 310. This arrangement can create a dynamic rotation effect about the central axis 312 of the atomization plume within the atomization chamber 108.
[0114] In at least one embodiment, the powder particle size distribution can have a geometric standard deviation of less than or equal to about 2.0. In at least one embodiment, the powder particle size distribution can have a geometric standard deviation of from about 1.5 to about 2.0.
[0115] In at least one embodiment, the powder particle size distribution can have a geometric standard deviation of less than or equal to about 1.8. In at least one embodiment, the powder particle size distribution can have a geometric standard deviation of from about 1.5 to about 1.8.
[0116] In at least one embodiment, the atomization chamber 108 may contain between about 0 and about 20% oxygen.
[0117] In at least one embodiment, the water may include at least one additive to control the redox potential of the water, examples of which include, but are not limited to, ethanol, methanol, acetic acid, HCl, and H2O2.
[0118] In at least one embodiment, the powder average particle size may be from about 3 microns to about 20 microns in diameter.
[0119] In at least one embodiment, the melt of the low melting point metal may be diverted through at least one melt diverter channel, and a diverter angle is formed between a central axis of the supply tube and the at least one melt diverter channel.
[0120] In at least one embodiment, the alloy melt may be diverted through at least two melt diversion channels (diverters) 216, and a diversion angle (90°-β) may be formed between the central axis 212 of the supply tube 210 and the at least two melt diversion channels 216.
[0121] In at least one embodiment, at least one jet of water is sprayed into the atomization chamber 108 .
[0122] In at least one embodiment, at least one jet of water is sprayed onto at least one wall of the atomization chamber 108 .
[0123] In at least one embodiment, the powder can have an average particle size of less than about 20 microns.In at least one embodiment, the powder can have an average particle size of less than about 10 microns.
[0124] In at least one embodiment, the powder produced can be dried in a vacuum to avoid powder oxidation.
[0125] In at least one embodiment, the powder produced may be washed with an organic solvent to remove most of the water prior to the drying step. For example, the organic solvent may be ethanol or methanol.
[0126] In at least one embodiment, an atomization apparatus 150 for producing a low melting point metal or alloy powder includes a supply tube 210 for providing a melt of the low melting point metal or alloy; a diverter 216 in fluid communication with the supply tube 210 for diverting the melt at a diverting angle with respect to a central axis of the supply tube 210 to obtain a diverted melt and for directing the diverted melt toward an atomization area 230 of the atomization apparatus 150; at least one atomization gas injector 214 for providing at least one atomization gas stream 240 to an atomization area disposed within the atomization chamber 108; and at least one water inlet 122 for providing water into the atomization chamber 108 of the atomization apparatus 150.
[0127] In at least one embodiment, the diverter 216 may include a melt diversion conduit 218 that is oriented at a diversion angle relative to the central axis 212 of the feed tube 210 .
[0128] In at least one embodiment, the diverter 216 may have at least two melt diversion conduits 218 , each of the at least two melt diversion conduits 218 oriented at a diversion angle relative to the central axis 212 of the feed tube 210 .
[0129] In at least one embodiment, the atomization apparatus 150 may have at least one gas inlet 214 (or 311, 314). At least one gas inlet 311, 314 of the exemplary embodiment of the atomization apparatus 300 may be tangential, or at least non-perpendicular, to the atomization head 310, providing a swirling motion of the atomized gas stream 240 in the atomization head 222 and a dynamic rotational motion of the atomized plume in the atomization chamber 108.
[0130] In at least one embodiment, at least one gas inlet (eg, 311, 314) that is non-perpendicular to the atomization manifold 310 can create a swirling motion of the atomization gas stream 240 in the atomization head 222, resulting in a dynamic rotational motion of the atomization plume in the atomization chamber 108.
[0131] In at least one embodiment, the at least two gas inlets 214 may be non-perpendicular to the atomizing head 222 creating a swirling effect in the atomizing head 222 and a dynamic rotational effect in the atomizing area 230 and the atomizing chamber 108 .
[0132] In at least one embodiment, at least one water inlet (eg, 122 or 120 in FIG. 1) may be located inside the atomization chamber 108.
[0133] In at least one embodiment, at least one water inlet (eg, 122 or 120 in FIG. 1) may be suitable for providing water for cooling the powder.
[0134] For example, at least one water inlet (eg, 122 or 120 in FIG. 1) may be suitable for providing water for transporting the powder to a screening / drying area.
[0135] In at least one embodiment, the at least one water inlet may be suitable for providing water to facilitate sorting / sieving of the powder.
[0136] Working Example Example 1: Sn-3% Ag-0.5% Cu (SAC305) In this exemplary test, atomization of Sn-3%Ag-0.5%Cu (SAC305) was carried out in a large atomizer with a batch size of 20 kg using the atomization manufacturing process and atomization apparatus described herein.
[0137] Table 1A shows the atomization conditions for the test of Example 1. [Table 1]
[0138] The resulting particle size distribution is shown in Table 1B. It is noted that the level of particles between 1 and 25 μm is extremely high (80%). [Table 2]
[0139] 4A and 4B show SEM photographs of the powder obtained in Example 1.
[0140] The morphology was measured as determined by a Malvern Morphology instrument, and the circularity of the powder particles was approximately 0.983 (circularity is 1 for a perfect sphere).
[0141] Example 2: Sn-58% Bi (SnBi) In the test of Example 2, atomization of Sn-58%Bi (SnBi) was carried out in a larger atomizer having a batch size of about 20 Kg using the atomization manufacturing process and atomization apparatus described herein. [Table 3] [Table 4]
[0142] Table 2B shows the particle size distribution observed. It should be noted that the level of particles between 1 and 25 μm is extremely high (90%).
[0143] 5A and 5B show SEM photographs of the powder obtained in Example 2.
[0144] Morphology was also measured as determined by a Malvern Morphology instrument. The circularity of the powder particles was approximately 0.98.
[0145] Example 3: InSn (Sn-50% In) In the test of Example 3, atomization of InSn (Sn-50% In) was carried out using the atomization manufacturing process and atomization apparatus described herein in a larger atomizer having a batch size of about 24 Kg. [Table 5]
[0146] FIG. 6 shows an SEM photograph of the powder obtained in Example 3.
[0147] Morphology was also measured as determined by a Malvern Morphology instrument. The circularity of the powder particles was approximately 0.936.
[0148] Example 4: Pure Bi In the tests of Example 4, atomization of Bi was carried out in a larger atomizer with a batch size of about 16 Kg using the atomization manufacturing process and atomization apparatus described herein. [Table 6] [Table 7]
[0149] Table 5B shows the particle size distribution observed. It should be noted that 86% of the powder was less than 25 microns.
[0150] 7A and 7B show SEM photographs of the powder obtained in Example 4.
Claims
1. An atomization process for producing a metal powder, Se powder, Te powder, or an alloy powder having a liquidus temperature of 50°C to 500°C, the metal powder not including Se powder and Te powder; providing a melt of said metal, Se, Te, or alloy having a liquidus temperature of said 50°C to 500°C via a supply pipe; diverting the melt through a diverter at a diversion angle with respect to a central axis of the supply pipe to obtain a diverted melt, the melt being diverted through at least two melt diverting channels, the diversion angle being formed between the central axis of the supply pipe and the at least two melt diverting channels, the diversion angle being between 10° and 90°; directing the diverted melt toward an atomization area; providing at least one atomizing gas stream having a velocity of at least 300 m / s to the atomizing area; Including, the ratio of the atomizing gas to the metal in the atomizing area is between 5,000 and 30,000 cm3 of gas per cm3 of metal to be atomized, thus providing a powder particle size distribution with a geometric standard deviation of less than 2.0; process.
2. The flow branch angle (90-β) is 30° to 70°.
2. The process of claim 1.
3. The angle formed between the atomizing gas and the melt is 40° to 90°.
2. The process of claim 1.
4. the process includes providing a metal having a melting point of between 50°C and 500°C; 2. The process of claim 1.
5. The metal has a melting point of 150°C to 500°C.
5. The process of claim 4.
6. The ratio of the atomizing gas to the metal in the atomizing area is 10,000 to 20,000 cm3 of gas per cm3 of metal to be atomized; 5. The process of claim 4.
7. The ratio of the atomizing gas to the metal in the atomizing area is 5000 to 30000 cm3 of gas per cm3 of metal to be atomized; 5. The process of claim 4.
8. The metal is an element selected from the group consisting of Zn, In, Sn, Pb, and Bi; 2. The process of claim 1.
9. the process includes providing an alloy having a liquidus temperature of between 50°C and 500°C; 2. The process of claim 1.
10. The alloy has a liquidus temperature of 100°C to 300°C.
10. The process of claim 9.
11. The alloy contains at least one element selected from the group consisting of Cu, Sb, Zn, In, Mg, Sn, Pb, Ag, Se, Te, Ga, and Bi; 10. The process of claim 9.
12. The atomizing gas stream has a velocity of 300 m / s to 700 m / s.
2. The process of claim 1.
13. The atomized gas stream has a supersonic velocity.
2. The process of claim 1.
14. The atomizing gas is delivered to the atomizing head through at least one gas inlet oriented non-perpendicularly to the atomizing head, the gas inlet providing a swirling motion in the atomizing head prior to a gas outlet.
2. The process of claim 1.
15. The process provides a powder particle size distribution having a geometric standard deviation of 1.5 to 1.
8.
2. The process of claim 1.
16. The atomized area contains 0 to 20% oxygen.
2. The process of claim 1.
17. At least one jet of water is sprayed into the atomization area.
2. The process of claim 1.
18. The process provides a powder, At least 80% of the powder has an average particle size of less than 25 μm.
2. The process of claim 1.
19. An atomizing apparatus for producing a metal powder, a Se powder, a Te powder, or an alloy powder having a liquidus temperature of 50°C to 500°C, the metal powder not including a Se powder or a Te powder; a supply tube for providing a melt of said metal, Se, Te, or alloy having a liquidus temperature of said 50°C to 500°C; a diverter in fluid communication with the supply pipe for diverting the melt at a diverting angle with respect to a central axis of the supply pipe to obtain a diverted melt and for directing the diverted melt toward an atomization area of the atomization device, the diverter having at least two melt diverting channels, the diverting angle being formed between the central axis of the supply pipe and the at least two melt diverting channels, the diverting angle being between 10° and 90°; at least one atomizing gas injector for providing at least one atomizing gas stream to the atomizing area disposed inside the atomizing chamber; at least one water inlet for providing water in the atomization chamber of the atomization device; Including, Device.
20. at least one non-vertical gas inlet creates a circular flow in the atomizing gas injector; The circular flow creates a dynamic rotational motion of the gas in the atomization area and in the atomization chamber.
20. The atomizing device according to claim 19.
Citation Information
Patent Citations
JP1973034760A
biryuka
JP1976071865A
Production of metal powder
JP1988137108A
Apparatus for manufacturing metal fine granule
JP1989255609A
Manufacture of metal powder
JP1991153802A