Mixed ink, its manufacturing method, and sintering method for mixed ink
A mixed ink with copper fine particles and a nickel formate complex addresses copper oxidation, allowing low-temperature sintering and stable copper wiring formation, simplifying and cost-reducing the manufacturing process.
Patent Information
- Application Number
- JP2020180857
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Conductive copper inks used in printed electronics face issues with copper oxidation, leading to increased electrical resistance and the need for high sintering temperatures, which complicates the manufacturing process and increases costs.
A mixed ink containing copper fine particles and a nickel formate complex with an amino group ligand is developed, which suppresses copper oxidation and allows for low-temperature sintering.
The mixed ink effectively prevents copper oxidation, enabling low-temperature sintering and stable formation of fine copper wiring on heat-sensitive substrates, reducing manufacturing complexity and costs.
Smart Images

Figure 0007568891000009 
Figure 0007568891000010 
Figure 0007568891000011
Abstract
Description
[Technical field]
[0001] The present invention relates to an ink mixture, a method for producing the ink mixture, and a method for sintering the ink mixture. [Background technology]
[0002] Conventionally, the method of manufacturing fine electrical circuit wiring has been to form circuits using lithography and etching techniques, but this requires large-scale sputtering and exposure equipment, and the manufacturing process is complicated, resulting in high costs. For this reason, printed electronic technology, which can manufacture electronic circuits on various materials using printing technology, has attracted attention and is being applied.
[0003] Conductive paste (ink) is used as a material to form electrical circuits in printed electronics technology. Numerous conductive inks using metal particles such as Ag particles and copper particles have been developed as conductive paste (ink).
[0004] Among the above-mentioned metal particles, copper particles are inexpensive, have excellent electrical conductivity, and have a low tendency to migrate, making them useful as conductive paste (ink) materials for printed electronics (PE) and bonding material applications. Considering the formation of wiring on polymer films using PE, there is a demand for conductive pastes that can be sintered at low temperatures of 200°C or less and that can achieve low electrical resistivity close to that of bulk copper after sintering.
[0005] As a conductive ink composition, a conductive ink composition containing copper formate and two or more kinds of ethanolamines has been proposed (see, for example, Patent Document 1).
[0006] However, the conductive ink composition described in Patent Document 1 has not been thoroughly studied for the prevention of copper oxidation. Copper is easily oxidized, and a copper oxide film is formed on the copper surface. The oxidation of copper increases electrical resistance and raises the sintering temperature.
[0007] Therefore, there is a need to develop a mixed ink that can be suitably used as a conductive copper ink material because the oxidation of copper is suppressed and low-temperature sintering is possible, a method for producing the mixed ink, and a method for sintering the mixed ink. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2013-108005 A Summary of the Invention [Problem to be solved by the invention]
[0009] The present invention aims to provide a mixed ink that can be suitably used as a conductive copper ink material because copper oxidation is suppressed and low-temperature sintering is possible, and a method for manufacturing the mixed ink.
[0010] Another object of the present invention is to provide a method for sintering the above mixed ink. [Means for solving the problem]
[0011] As a result of extensive research, the inventors discovered that the above-mentioned objective can be achieved by a mixed ink containing copper microparticles and a nickel formate complex having a ligand containing an amino group, and thus completed the present invention.
[0012] That is, the present invention relates to the following mixed ink, a method for producing the same, and a method for sintering the mixed ink. 1. A mixed ink comprising copper fine particles and a nickel formate complex having a ligand containing an amino group. 2. The mixed ink according to item 1, wherein the ligand containing an amino group has a group represented by the following formula (1) or (2): [ka] (In formulas (1) and (2), * indicates a bond.) 3. The mixed ink according to item 1, wherein the ligand containing an amino group is a ligand represented by the following formula (6): [C2] H2N(C2H4NH) n H (6) (In formula (6), n represents an integer of 1 to 5.) 4. The mixed ink according to item 1, wherein the ligand containing an amino group is at least one selected from the group consisting of 1-amino-2-propanol, ethylenediamine, and 2-amino-1-butanol. 5. The mixed ink according to any one of items 1 to 4, wherein the ratio of the mass of the metallic nickel (MNi) to the total mass (MCu+MNi) of the metallic copper (MCu) and the metallic nickel (MNi) is 3 to 40 mass%. 6. A method for sintering an ink mixture, comprising sintering the ink mixture according to any one of items 1 to 5 at a temperature of 200° C. or lower. 7. A method for producing a mixed ink containing copper fine particles and a nickel formate complex having a ligand containing an amino group, comprising the steps of: (1) Step 1 of mixing nickel formate, a ligand containing an amino group, and a solvent to prepare a composition containing a nickel formate complex having a ligand containing an amino group; and (2) Step 2 of adding copper fine particles to the composition; The manufacturing method according to claim 1, Effect of the Invention
[0013] The mixed ink of the present invention is suitable for use as a conductive copper ink because oxidation of copper is suppressed and low-temperature sintering is possible. Furthermore, the manufacturing method of the present invention makes it possible to easily manufacture the mixed ink.
[0014] Furthermore, since the sintering method of the present invention uses the above-mentioned mixed ink, the mixed ink can be sintered at a low temperature of 200°C or less, so that copper fine wiring can be easily formed even on substrates such as paper and plastic that are sensitive to heat. [Brief description of the drawings]
[0015] [Figure 1] 1 is a photograph showing the state of the nickel formate complex of Reference Example 2. [Diagram 2] 1 is a photograph showing the state of the nickel formate complex of Reference Example 3. [Diagram 3] 1 is a photograph showing the state of the nickel formate complex of Reference Example 4. [Figure 4] 1 is a photograph showing the state of the nickel formate complex of Reference Example 5. [Diagram 5] FIG. 2 is a graph showing the results of thermal analysis of the nickel formate-containing composition of Reference Example 1 and the nickel formate complexes of Reference Examples 2 to 5. [Figure 6] FIG. 2 is a graph showing the results of XRD measurement of the nickel formate complex of Reference Example 2 after calcination. [Figure 7] FIG. 13 is a diagram showing the results of a thermal analysis of the mixed ink in air. [Figure 8] FIG. 13 is a diagram showing the results of a thermal analysis of the mixed ink in a nitrogen atmosphere. [Figure 9] FIG. 13 is a diagram showing the results of measuring the volume resistivity of a sintered film prepared by sintering a mixed ink in an inert atmosphere (nitrogen atmosphere). [Figure 10] 4 is a photograph showing the results of an adhesion evaluation of a sintered film formed using the ink of Comparative Example 1. [Figure 11] 4 is a photograph showing the results of an adhesion evaluation of a sintered film prepared using the mixed ink of Example 1. [Figure 12] 13 is a photograph showing the results of an adhesion evaluation of a sintered film prepared using the mixed ink of Example 2. [Figure 13] 13 is a photograph showing the results of an adhesion evaluation of a sintered film prepared using the mixed ink of Example 3. [Figure 14] 13 is a photograph showing the results of an adhesion evaluation of a sintered film prepared using the mixed ink of Example 4. [Figure 15] FIG. 2 is a diagram showing the results of EDS measurement, using an energy dispersive X-ray analyzer, of a sintered film prepared using the mixed ink of Example 1. [Figure 16]FIG. 13 is a diagram showing the results of EDS measurement, using an energy dispersive X-ray analyzer, of a sintered film prepared using the mixed ink of Example 2. [Figure 17] FIG. 13 is a diagram showing the results of EDS measurement, using an energy dispersive X-ray analyzer, of a sintered film prepared using the mixed ink of Example 3. [Figure 18] FIG. 13 is a diagram showing the results of EDS measurement, using an energy dispersive X-ray analyzer, of a sintered film prepared using the mixed ink of Example 4. [Figure 19] FIG. 2 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 1. [Figure 20] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 2. [Figure 21] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 3. [Figure 22] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 4. [Figure 23] FIG. 2 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 1. [Figure 24] FIG. 2 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 1. [Diagram 25] FIG. 2 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 1. [Figure 26] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 2. [Figure 27] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 2. [Figure 28] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 2. [Figure 29] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 3. [Diagram 30]FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 3. [Diagram 31] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 3. [Diagram 32] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 4. [Diagram 33] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 4. [Diagram 34] FIG. 13 shows the results of SEM observation of a sintered film prepared using the mixed ink of Example 4. [Diagram 35] FIG. 2 is a graph showing the results of a moist heat resistance test of sintered films prepared using the mixed inks of Examples 1 to 4 and the ink of Comparative Example 1. [Diagram 36] FIG. 2 is a diagram showing the results of XRD measurement of sintered films prepared using the mixed inks of Examples 1 to 4 and the ink of Comparative Example 1. [Figure 37] FIG. 1 shows the results of XRD measurement of sintered films prepared using the mixed inks of Examples 1 to 4 and the ink of Comparative Example 1 after a moist heat resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] The present invention will be described in detail below.
[0017] 1. Mixed ink The mixed ink of the present invention contains copper fine particles and a nickel formate complex having a ligand containing an amino group. Since the mixed ink of the present invention contains copper fine particles, it can be sintered at a relatively low temperature by sintering and is stable in the mixed ink. In addition, the copper fine particles are less likely to be sintered at a low temperature than, for example, when copper nanoparticles are used. However, since the mixed ink of the present invention contains copper fine particles and a nickel formate complex having a ligand containing an amino group, the nickel formate complex is used as the nickel source, not nickel metal having a higher melting point than copper, and the metallic nickel generated by sintering the formate nickel complex promotes the sintering of the copper fine particles. In addition, since the nickel formate complex releases hydrogen during sintering, the hydrogen exhibits a reducing action and can suppress the oxidation of the copper fine particles. Furthermore, the nickel generated from the nickel formate complex during the sintering process covers the surface of the copper fine particles, and the sintered copper film can be given high oxidation resistance. That is, the mixed ink of the present invention contains copper fine particles and a nickel formate complex having a ligand containing an amino group, and thus the oxidation of copper is suppressed, and low-temperature sintering is possible. Therefore, the mixed ink of the present invention can be suitably used as a conductive copper ink.
[0018] (copper fine particles) The copper fine particles are not particularly limited as long as they are copper particles, and may be copper fine particles consisting of copper single crystals or copper fine particles in the form of secondary particles formed by aggregation of primary copper particles.
[0019] In this specification, the term "single crystal" refers to a crystal in which every part has the same crystal orientation and the atoms that make up the crystal are arranged in a regular spatial order. In other words, in this specification, when the copper microparticles are made of single crystals of copper, the whole particle is a single crystal, and crystals that have grown in various directions are not mixed together, and the copper microparticles are not aggregated. This can be confirmed by peak measurements in XRD analysis of the copper microparticles and direct observation of the atomic arrangement using a high-resolution electron microscope.
[0020] The average particle size of the copper fine particles is preferably 0.05 μm or more, more preferably 0.1 μm or more, even more preferably 0.5 μm or more, and particularly preferably 0.7 μm or more. The average particle size of the copper fine particles is preferably 5 μm or less, more preferably 3 μm or less, even more preferably 2.5 μm or less, particularly preferably 2 μm or less, and most preferably 1.5 μm or less. When the lower limit of the average particle size of the copper fine particles is in the above range, the oxidation of the copper fine particles is further suppressed, and the increase in the electrical resistivity of the sintered film is further suppressed. When the upper limit of the average particle size of the copper fine particles is in the above range, the sintered film can be formed more easily at a low temperature.
[0021] In this specification, the average particle size of the copper fine particles is the arithmetic mean value of particle sizes of 100 random particles in a TEM observation image.
[0022] The shape of the copper fine particles is not particularly limited, and may be flake-like (flat) or spherical. The flake-like shape is preferred from the viewpoint of being easily sintered in the air and capable of forming a sintered film having a lower volume resistivity.
[0023] As the flake-shaped copper fine particles, commercially available products can be used, such as those manufactured by Mitsui Kinzoku Co., Ltd. under the product names 1050YF and 1050YP.
[0024] The content of copper microparticles in the mixed ink is preferably 20% by mass or more, more preferably 40% by mass or more, based on 100% by mass of the mixed ink. The content of copper microparticles is preferably 80% by mass or less, more preferably 60% by mass or less, based on 100% by mass of the mixed ink. When the lower limit of the content of copper microparticles is within the above range, the volume resistivity of the sintered film formed using the mixed ink is further reduced. When the upper limit of the content of copper microparticles is within the above range, the content of nickel formate complex is increased, so that sintering of the mixed ink is further facilitated by thermal decomposition of the nickel formate complex, and the volume resistivity of the sintered film formed is further reduced.
[0025] (Nickel formate complexes with amino group-containing ligands) The mixed ink of the present invention contains a nickel formate complex having a ligand containing an amino group. The nickel formate complex having a ligand containing an amino group (hereinafter, also simply referred to as "nickel formate complex") can be prepared by mixing nickel formate, the ligand containing an amino group, and a solvent, for example, as in step 1 of the production method described below.
[0026] As nickel formate, anhydrous nickel formate, nickel formate dihydrate, etc. can be used. From the viewpoint of easier ligand formation, anhydrous nickel formate is preferred.
[0027] The nickel formate may be used alone or in combination of two or more.
[0028] The ligand containing an amino group (hereinafter also referred to as the unit "ligand") is not particularly limited as long as it has an amino group and can be used as a ligand, and a monodentate ligand or a polydentate ligand having an amino group can be used. Examples of such ligands include 1-amino-2-propanol (IPA), 3-amino-1-propanol (3AP), 2-amino-1-butanol (2AB), ethylenediamine (EDA), diethyltriamine (DETA), triethyltetraamine (TETA), tetraethylenepentaminetrimethylamine (TEPA), trimethylamine, triethylamine, diisopropylethylamine, propylamine, octylamine, diethylamine, tetramethylethylenediamine, dimethylethylenediamine, etc. Among these, from the viewpoint of enabling the mixed ink to be sintered at an even lower temperature, 1-amino-2-propanol (IPA), 3-amino-1-propanol (3AP), 2-amino-1-butanol (2AB) and ethylenediamine (EDA) are preferred, and 1-amino-2-propanol (IPA), ethylenediamine (EDA) and 2-amino-1-butanol (2AB) are more preferred.
[0029] The ligand preferably has a group represented by the following formula (1): In the following formulas (1) to (5), * represents a bond.
[0030] [ka]
[0031] The group represented by the above formula (1) is oxidized to a ketone to generate a group represented by the following formula (3).
[0032] [ka]
[0033] The groups represented by the above formulae (1) and (3) exhibit high coordinating power and form a five-membered ring with the nickel atom to form groups having metallacycle structures represented by the following formulae (4) and (5), which are stable, and therefore the aggregation of the nickel formate complex is further suppressed.
[0034] [ka]
[0035] [ka]
[0036] It is also preferable that the ligand has a group represented by the following formula (2).
[0037] [ka]
[0038] The group represented by the above formula (2) also forms a five-membered ring with the nickel atom to become a group having a metallacycle structure, which is stabilized, and therefore the aggregation of the nickel formate complex is further suppressed.
[0039] The ligand may be a ligand represented by the following formula (6):
[0040] [8] H2N(C2H4NH) n H (6)
[0041] In the formula (6), n represents an integer of 1 to 5. n is preferably an integer of 1 to 3, and more preferably 1.
[0042] The ligand represented by the above formula (6) easily coordinates to the nickel atom, and therefore the aggregation of the nickel formate complex is further suppressed.
[0043] The above ligands may be used alone or in combination of two or more.
[0044] A nickel formate complex can be prepared by mixing the nickel formate, a ligand containing an amino group, and a solvent.
[0045] The content of the nickel formate complex in the mixed ink is preferably 20% by mass or more, more preferably 30% by mass or more, based on 100% by mass of the mixed ink. The content of the nickel formate complex is preferably 60% by mass or less, more preferably 50% by mass or less, based on 100% by mass of the mixed ink. When the lower limit of the content of the nickel formate complex is in the above range, the sintering of the mixed ink is more likely to proceed due to the thermal decomposition of the nickel formate complex, and the volume resistivity of the sintered film formed is further reduced. When the upper limit of the content of the nickel formate complex is in the above range, the ratio of copper fine particles in the mixed ink is increased, and the volume resistivity of the sintered film formed is further reduced.
[0046] In the mixed ink of the present invention, the ratio of the mass of metallic nickel (MNi) to the total (MCu+MNi) of the mass of metallic copper (MCu) and the mass of metallic nickel (MNi) is preferably 3 to 40 mass%, more preferably 5 to 30 mass%, even more preferably 5 to 20 mass%, and particularly preferably 8 to 15 mass%. By setting the lower limit of the ratio of the mass of metallic nickel (MNi) within the above range, the sintering of the mixed ink due to the thermal decomposition of the nickel formate complex is more likely to proceed, and the volume resistivity of the sintered film formed is further reduced. In addition, by setting the upper limit of the ratio of the mass of metallic nickel (MNi) within the above range, the ratio of copper fine particles in the mixed ink is increased, and the volume resistivity of the sintered film formed is further reduced.
[0047] The mixed ink of the present invention may contain a solvent. For example, when the mixed ink is produced by preparing the nickel formate complex in a solvent to form a composition in step 1 of the production method described below, and adding copper fine particles to the composition in step 2, the solvent used in step 1 is the solvent contained in the mixed ink.
[0048] The solvent is not particularly limited, and may be an ether, an alcohol, a polyol, etc. Among these, polyols are preferred because they have reducing properties.
[0049] The alcohol is not particularly limited, and examples of the alcohol that can be used include ethanol, propanol, butanol, ethylene glycol, propylene glycol, glycerin, etc. Among these, ethylene glycol and propylene glycol are preferred, and ethylene glycol is more preferred, in that they have reducing properties and low viscosity.
[0050] The above solvents may be used alone or in combination of two or more.
[0051] 2. Manufacturing method of mixed ink The method for producing a mixed ink of the present invention is a method for producing a mixed ink containing copper fine particles and a nickel formate complex having a ligand containing an amino group, (1) Step 1 of mixing nickel formate, a ligand containing an amino group, and a solvent to prepare a composition containing a nickel formate complex having a ligand containing an amino group; and (2) Step 2 of adding copper fine particles to the composition; The manufacturing method is characterized by having the following features. The above mixed ink of the present invention can be produced by the production method of the present invention having the above steps 1 and 2.
[0052] (Process 1) Step 1 is a step of mixing nickel formate, a ligand containing an amino group, and a solvent to prepare a composition containing a nickel formate complex having a ligand containing an amino group.
[0053] The nickel formate, the ligand containing an amino group, and the solvent used in step 1 above can be the same as the nickel formate, the ligand containing an amino group, and the solvent in the mixed ink described above.
[0054] The content of nickel formate in the composition is preferably 5% by mass or more, more preferably 10% by mass or more, based on 100% by mass of the composition. The content of nickel formate is preferably 50% by mass or less, more preferably 30% by mass or less, based on 100% by mass of the composition. By setting the lower limit of the nickel formate content within the above range, nickel formate complex can be sufficiently formed in the composition.
[0055] The content of the ligand containing an amino group in the composition is preferably 8 molar equivalents or less, more preferably 6 molar equivalents or less, based on the content of the nickel formate in the composition as 1 molar equivalent. The content of the ligand containing an amino group in the composition is preferably 4 molar equivalents or more, based on the content of the nickel formate in the composition as 1 molar equivalent. By setting the lower limit of the content of the ligand within the above range, the nickel formate complex can be sufficiently formed in the composition. By setting the upper limit of the content of the ligand within the above range, the complex can be formed more easily.
[0056] The content of the solvent in the composition is preferably 10% by mass or more, more preferably 30% by mass or more, based on 100% by mass of the composition. The content of the solvent is preferably 80% by mass or less, more preferably 60% by mass or less, based on 100% by mass of the composition. By setting the lower limit of the solvent content within the above range, nickel formate and the ligand can be sufficiently dispersed in the composition, and nickel formate complex can be sufficiently formed. By setting the upper limit of the solvent content within the above range, the content of nickel formate complex in the mixed ink becomes even more sufficient, and nickel formate complex can be sufficiently formed.
[0057] In step 1, the temperature of the composition during mixing is not particularly limited, and may be about 0 to 40°C.
[0058] The composition may be stirred when mixed in step 1. The stirring time is not particularly limited and may be about 30 to 60 minutes.
[0059] Step 1 may include a step of preparing anhydrous nickel formate by heating nickel formate hydrate. By including the step of preparing anhydrous nickel formate in step 1, the nickel formate complex can be prepared more efficiently.
[0060] An example of a method for preparing anhydrous nickel formate is a method in which a hydrated nickel formate, such as the nickel formate dihydrate described above, is heated.
[0061] The heating temperature in the nickel formate anhydrate preparation step is not particularly limited, and may be about 170 to 230° C. The heating time may be about 30 to 120 minutes.
[0062] By the above-described step 1, a composition containing a nickel formate complex having a ligand containing an amino group is prepared.
[0063] (Process 2) Step 2 is a step of adding copper fine particles to the composition. The copper fine particles used in step 2 may be the same as the copper fine particles in the mixed ink described above.
[0064] The amount of copper fine particles added in step 2 is preferably 20% by mass or more, more preferably 40% by mass or more, based on 100% by mass of the composition. The amount of copper fine particles added is preferably 80% by mass or less, more preferably 60% by mass or less, based on 100% by mass of the composition. When the lower limit of the amount of copper fine particles added is within the above range, the volume resistivity of the sintered film formed using the mixed ink produced is further reduced. When the upper limit of the amount of copper fine particles added is within the above range, the content of nickel formate complex in the mixed ink is increased, so that sintering of the mixed ink is more likely to proceed due to thermal decomposition of the nickel formate complex, and the volume resistivity of the sintered film formed is further reduced.
[0065] In step 2, the temperature of the composition when the copper fine particles are added is not particularly limited, and may be about 0 to 40°C.
[0066] The composition to which the copper fine particles have been added may be stirred in step 2. The stirring time is not particularly limited and may be about 0.5 to 10 minutes.
[0067] Step 2 may include an oxide film removing step of removing the oxide film on the surface of the copper fine particles before adding the copper fine particles to the composition.
[0068] The method for removing the oxide film is not particularly limited, and may be, for example, a method in which the copper fine particles are immersed in a reducing agent.
[0069] The reducing agent is not particularly limited, and examples thereof include formic acid, hydrazine compounds, etc. Among these, formic acid is preferred from the viewpoint of excellent reducing properties.
[0070] The time for immersion in the reducing agent is not particularly limited, and may be about 30 to 120 minutes.
[0071] In the mixed ink produced through step 2, the ratio of the mass of metallic nickel (MNi) to the total (MCu+MNi) of the mass of metallic copper (MCu) and the mass of metallic nickel (MNi) is preferably 3 to 40 mass%, more preferably 5 to 30 mass%, even more preferably 10 to 20 mass%, and particularly preferably 10 to 15 mass%. By setting the lower limit of the ratio of the mass of metallic nickel (MNi) within the above range, the sintering of the mixed ink produced by the thermal decomposition of the nickel formate complex is more likely to proceed, and the volume resistivity of the sintered film formed is further reduced. In addition, by setting the upper limit of the ratio of the mass of metallic nickel (MNi) within the above range, the ratio of copper fine particles in the mixed ink produced is increased, and the volume resistivity of the sintered film formed is further reduced.
[0072] By the above-described step 2, copper fine particles are added to the composition prepared in step 1, and the mixed ink of the present invention described above can be produced.
[0073] 3. Sintering method of mixed ink Since the mixed ink of the present invention has the above-mentioned configuration, even when heated in a low temperature range of 200°C or less, copper fine wiring can be formed in a short time. The mixed ink sintering method in which the mixed ink is sintered at a temperature of 200°C or less is also one aspect of the present invention. The temperature is preferably 180°C or less, more preferably 150°C or less, and even more preferably 120°C or less. The temperature is preferably 70°C or more, more preferably 80°C or more, and even more preferably 90°C or more.
[0074] When the mixed ink is sintered in a non-reducing atmosphere, the sintering temperature is preferably 120° C. or lower, and more preferably 100° C. or lower. The sintering temperature is preferably 70° C. or higher, and more preferably 80° C. or higher.
[0075] When the copper particle mixture is sintered in a non-reducing atmosphere, the mixture may be sintered at normal pressure or under reduced pressure. The pressure for sintering under reduced pressure is not particularly limited, and may be any pressure lower than normal pressure.
[0076] The non-reducing atmosphere is not particularly limited, but examples thereof include nitrogen and argon.
[0077] When the copper particle mixture is sintered in air, the sintering temperature is preferably 150° C. or lower, more preferably 140° C. or lower, and more preferably 80° C. or higher, more preferably 90° C. or higher.
[0078] When the copper particle mixture is sintered in air, it may be sintered at normal pressure.
[0079] The mixed ink of the present invention can be suitably used as an ink material for forming metal fine wiring and a bonding material for power semiconductors, but is not limited to these applications and can also be used as a catalyst material (catalyst or catalyst carrier). It can also be used as a transparent conductive film to replace ITO and an anti-reflective coating material. EXAMPLES
[0080] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the examples.
[0081] (Preparation of nickel formate complex) Reference example 1 Nickel formate dihydrate was heated at 200°C for 1 hour to obtain anhydrous nickel formate. 8 mL of methanol was added to 2 g of the obtained anhydrous nickel formate, mixed, and stirred at room temperature for 1 hour to prepare a nickel formate-containing composition. Next, methanol was removed using an evaporator.
[0082] Reference example 2 (Preparation of nickel formate complexes with amino group-containing ligands) An amine-nickel formate complex was prepared as a nickel formate complex having a ligand containing an amino group. Specifically, nickel formate dihydrate was heated at 200°C for 1 hour to obtain anhydrous nickel formate. 4 molar equivalents of 1-amino-2-propanol (IPA) (4.15mL) and 8mL of methanol were added to 2g of the obtained anhydrous nickel formate, mixed, and stirred at room temperature for 1 hour to prepare an amine-nickel formate complex. A photograph of the state of the nickel formate complex of Reference Example 2 is shown in Figure 1.
[0083] Reference examples 3~5 Amine-nickel formate complexes were prepared in the same manner as in Reference Example 2, except that 4 molar equivalents of 3-amino-1-propanol (3AP) (Reference Example 3), 4 molar equivalents of 2-amino-1-butanol (2AB) (Reference Example 4), or 4 molar equivalents of ethylenediamine (EDA) (Reference Example 5) were used instead of 4 molar equivalents of 1-amino-2-propanol (IPA) in Reference Example 2. Photographs of the states of the nickel formate complexes in Reference Examples 3 to 5 are shown in Figures 2 to 4, respectively.
[0084] (evaluation) Thermal analysis (TG-DTA) Thermal analysis of the nickel formate-containing composition of Reference Example 1 and the nickel formate complexes of Reference Examples 2 to 5 was carried out using a Rigaku Thermo plus EVO under a nitrogen atmosphere at 5° C. / min. The results are shown in FIG.
[0085] From the results in Figure 5, it was found that nickel formate complexes can be decomposed at low temperatures by coordinating a ligand having an amino group. In addition, it was found that among nickel formate complexes having a ligand containing an amino group, the IPA-nickel formate complex decomposes at a lower temperature.
[0086] XRD measurement after air baking The nickel formate complex of Reference Example 2 was calcined in air for 10 minutes at a temperature of 200° C., and subjected to XRD measurement using an X-ray diffractometer (Bruker D2 PHASER). The results are shown in FIG.
[0087] From the results in Figure 6, no peaks of copper oxide or cuprous oxide were observed in the XRD measurement results, and it was found that by coordinating a ligand having an amino group to the nickel formate complex, a reducing action occurs during firing, suppressing the oxidation of copper.
[0088] (Preparation of mixed ink) Examples 1 to 4, Comparative Example 1 0.500 g (Comparative Example 1), 1.425 g (Example 1), 1.350 g (Example 2), 0.600 g (Example 3), and 0.350 g (Example 4) of copper fine particles (manufactured by Mitsui Mining & Smelting Co., Ltd., product name: 1050YF) were added to 20 mL of formic acid and immersed for 1 hour to melt the oxide film on the surface of the copper fine particles. Next, the copper fine particles were washed four times with 30 mL of ethanol. The washed copper fine particles were dried in a N2 atmosphere.
[0089] As a solvent, ethylene glycol was prepared in amounts of 360 μL (Comparative Example 1), 340 μL (Example 1), 340 μL (Example 2), 200 μL (Example 3), and 280 μL (Example 4). In ethylene glycol, the washed copper fine particles and the amine-nickel formate complex prepared in Reference Example 2 were mixed so that the weight ratio of metallic copper to metallic nickel was 100:0 (Comparative Example 1), 95:5 (Example 1), 90:10 (Example 2), 80:20 (Example 3), and 70:30 (Example 4), respectively, and the mixture was stirred using a stirrer (Thinky Corporation, product name: Awatori Rentaro) under conditions of kneading at 2000 rpm for 5 minutes and degassing at 2200 rpm for 5 minutes to prepare mixed inks.
[0090] (evaluation) Thermal analysis (TG-DTA) Thermal analysis of the mixed inks of Examples 1 to 4 and Comparative Example 1 was performed using Rigaku's Thermo plus EVO in air and nitrogen atmosphere at 5° C. / min. The results are shown in FIG. 7 (in air) and FIG. 8 (in nitrogen atmosphere).
[0091] 7 and 8, it was found that in the ink of Comparative Example 1 (copper fine particles only), oxidation began to occur at around 250° C. In contrast, it was found that in the mixed inks of Examples 1 to 4, oxidation did not occur significantly up to 400° C. or higher. This shows that excellent oxidation resistance is exhibited by mixing copper fine particles with a nickel formate complex having a ligand containing an amino group.
[0092] (Preparation of sintered membrane) The mixed inks of Examples 1 to 4 and Comparative Example 1 were applied to a polyimide substrate using a doctor blade (12 μm) to form a film. Sintering was performed in an electric furnace under conditions of a nitrogen atmosphere (flow rate 3.0 L / min), a temperature rise rate of 5° C. / min, a sintering temperature of 180° C., and a sintering time of 30 min to prepare a sintered film.
[0093] (evaluation) Volume resistivity measurement using the four-probe method The sheet resistance (Ω / □) of the sintered film was measured by the four-point probe method. The measurement was performed using a Loresta-EP resistivity meter (Loresta-EP MCP-T360) and a four-point probe (MCP-TPQPP). The film thickness was measured with a micrometer, and the volume resistivity (Ωcm) was calculated by multiplying it by the sheet resistance. The results are shown in Figure 9. In Figure 9, the horizontal axis indicates the value of x (mass%) in Cu-xNi.
[0094] In FIG. 9, Comparative Example 1 (x=0 mass%, 8.3×10 -4 Ωcm) than Example 1 (x=5 mass%, 2.4×10 -5 The electrical resistivity is lower for nickel metal than for copper metal, but the volume resistivity is thought to have decreased due to the progress of sintering caused by the thermal decomposition of the nickel formate complex.
[0095] In addition, in FIG. 9, Example 1 (x=5 mass%, 2.4×10 -5 Ωcm) than Example 2 (x=10 mass%, 6.7×10 -5 Ωcm), Example 3 (x=20 mass%, 2.1×10 -4Ωcm), Example 4 (x=30 mass%, 6.5×10 -4 This is thought to be because when the proportion of nickel increases, the proportion of metallic copper in the sintered film decreases, resulting in an increase in volume resistivity.
[0096] Adhesion evaluation of sintered film The adhesion of the sintered films prepared in Examples 1 to 4 and Comparative Example 1 was evaluated. The specific evaluation method is as follows. That is, according to the cross-cut test method, 6 cuts were made at 1 mm intervals to prepare 25 squares of 1 mm each, and tape was attached to the squares and forcefully peeled off to visually check the degree of peeling from the substrate to evaluate the adhesion. The results are shown in Fig. 10 (Comparative Example 1), Fig. 11 (Example 1), Fig. 12 (Example 2), Fig. 13 (Example 3), and Fig. 14 (Example 4).
[0097] From the results of Figs. 10 to 14, it was found that the sintered film of Example 2 (Fig. 12) had the highest adhesion. From the results of Fig. 10, it was found that in Comparative Example 1, the sintered film was formed of copper metal, and therefore the sintered film was soft and easily peeled off. In Example 2 (Fig. 12), it was found that the sintered film was hard and difficult to peel off due to the presence of nickel in the sintered film. In Examples 3 and 4, since there was more nickel formate complex than in Example 2, the sintered film contained more organic components in the nickel formate complex than in Example 2, and therefore the sintered film was formed slightly less uniformly than in Example 2, and it was found that the copper and nickel were slightly more easily peeled off.
[0098] SEM-EDS measurement of sintered film As an elemental composition analysis of the sintered films prepared in Examples 1 to 4, EDS measurement was performed under the condition of 15 keV using an energy dispersive X-ray analyzer (manufactured by JEOL, model number JCM-6000 SEM). The results are shown in Figure 15 (Example 1), Figure 16 (Example 2), Figure 17 (Example 3), and Figure 18 (Example 4). The measured values obtained are as shown in Table 1 below.
[0099] [Table 1]
[0100] Scanning electron microscope (SEM) observation of sintered film SEM observation of the sintered films prepared in Examples 1 to 4 was performed using an energy dispersive X-ray analyzer (JEOL, model number JCM-6000 SEM) under the condition of 15 keV. The results are shown in Fig. 19 (Example 1), Fig. 20 (Example 2), Fig. 21 (Example 3), Fig. 22 (Example 4), Fig. 23 to Fig. 25 (Example 1), Fig. 26 to Fig. 28 (Example 2), Fig. 29 to Fig. 31 (Example 3), and Fig. 32 to Fig. 34 (Example 4). In Fig. 19 to Fig. 22, the left side shows the dispersibility of metallic nickel, and the right side shows the dispersibility of metallic copper.
[0101] Moisture and heat resistance test (measurement of resistance increase rate of sintered film) The sintered films prepared using the mixed inks of Examples 1 to 4 and the ink of Comparative Example 1 were left to stand for 7 days in a high-temperature, high-humidity environment at a temperature of 80°C and a humidity of 80%. The sheet resistance value (Ω / □) of the sintered film was measured by a four-point probe method. The measurement was performed using a Loresta-EP resistivity meter (Loresta-EP MCP-T360) and a four-point probe (MCP-TPQPP). The film thickness was measured with a micrometer, and the volume resistivity (Ωcm) was calculated by multiplying it by the sheet resistance value. The initial resistance value was taken as R0, and the resistance values after 1, 3, 5, and 7 days were taken as R, and R / R0 was calculated as the resistance increase rate. The results are shown in FIG. 35.
[0102] Fig. 35 shows that the sintered film prepared with the ink of Comparative Example 1 was overloaded on the fifth day. From the results of Fig. 35, it was found that in Examples 1 to 4, the sintered film was formed uniformly and oxidation of the sintered film was suppressed. In addition, it was found that in Comparative Example 1, since it did not contain nickel, the sintered film was easily oxidized, and Cu2O was formed, resulting in an increase in resistance value.
[0103] XRD measurement of sintered film XRD measurements were performed on the sintered films prepared using the mixed inks of Examples 1 to 4 and the ink of Comparative Example 1. The results are shown in FIG. 36. In addition, the sintered films were subjected to the above-mentioned moist heat resistance test, and XRD measurements were performed on the sintered films after 7 days in a high-temperature and high-humidity environment at a temperature of 80°C and a humidity of 80%. The results are shown in FIG. 37. The XRD measurements were performed using an X-ray diffractometer (Bruker D2 PHASER).
[0104] In Fig. 37, a CuO peak was detected by XRD measurement of the sintered film prepared with the ink of Comparative Example 1, and it was found that oxidation had occurred. From the results of Fig. 37, it was found that in Examples 1 to 4, the sintered film was generated uniformly, and the oxidation of the sintered film was suppressed. In addition, it was found that in Comparative Example 1, since it did not contain nickel, the sintered film was easily oxidized, and Cu2O was generated.
Claims
1. A mixed ink comprising copper fine particles and a nickel formate complex having a ligand containing an amino group.
2. The mixed ink according to claim 1 , wherein the ligand containing an amino group has a group represented by the following formula (1) or (2): 【Chemistry 1】 (In formulas (1) and (2), * indicates a bond.)
3. The mixed ink according to claim 1 , wherein the ligand containing an amino group is a ligand represented by the following formula (6): [Chemical 2] H 2 N(C 2 H 4 NH) n H (6) (In formula (6), n represents an integer of 1 to 5.)
4. 2. The mixed ink according to claim 1, wherein the ligand containing an amino group is at least one selected from the group consisting of 1-amino-2-propanol, ethylenediamine, and 2-amino-1-butanol.
5. The mixed ink according to any one of claims 1 to 4, wherein the ratio of the mass of the metallic nickel (MNi) to the total (MCu+MNi) of the mass of the metallic copper (MCu) and the mass of the metallic nickel (MNi) is 3 to 40 mass%.
6. A method for sintering a mixed ink, comprising sintering the mixed ink according to any one of claims 1 to 5 at a temperature of 200°C or less.
7. A method for producing a mixed ink containing copper fine particles and a nickel formate complex having a ligand containing an amino group, comprising the steps of: (1) Step 1 of mixing nickel formate, a ligand containing an amino group, and a solvent to prepare a composition containing a nickel formate complex having a ligand containing an amino group; and (2) Step 2 of adding copper fine particles to the composition; The manufacturing method according to claim 1,
Citation Information
Patent Citations
Metal nanoparticle with core-shell structure and method for producing the same
JP2007224420A
Electrically conductive ink composition and electric conduction part produced using the same
JP2012131894A
Electrically conductive ink composition and electric conduction part produced using the same
JP2012131895A
Conductive ink composition
JP2013108005A
Metal particulate composition and method for producing the same
JP2013108140A