Cooling structure, battery unit, and method for manufacturing cooling structure

The cooling structure for water-cooled battery packs uses laser-welded Zn-based plated steel sheets with optimized gap formation to enhance corrosion resistance and liquid tightness, achieving high cooling efficiency and addressing previous structural limitations.

JP7568983B2Active Publication Date: 2024-10-17NIPPON STEEL CORPORATION
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2023522336
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-20
Filing Date
2022-04-15
Publication Date
2024-10-17
Estimated Expiration
2042-04-15

AI Technical Summary

Technical Problem

Existing water-cooled battery packs face challenges in achieving high cooling efficiency, liquid tightness, and corrosion resistance due to the use of aluminum or steel materials, particularly in environments exposed to coolant and external conditions, with limited methods for joining plated steel plates effectively.

Method used

A cooling structure using laser-welded Zn-based plated steel sheets with a chemical conversion coating, featuring a press-formed member and flow top cover, where the laser welding is optimized to minimize blowholes and pits, and the use of spacers or spot welding to ensure gap formation, enhancing corrosion resistance and liquid tightness.

Benefits of technology

The solution provides a cooling structure with high cooling efficiency, excellent liquid tightness, and robust corrosion resistance, suitable for various sizes and shapes, effectively addressing the limitations of previous technologies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007568983000003
    Figure 0007568983000003
  • Figure 0007568983000004
    Figure 0007568983000004
  • Figure 0007568983000005
    Figure 0007568983000005
Patent Text Reader

Abstract

A cooling structure according to one aspect of the present invention comprises: a press-molded member having a groove part and a bank part provided around the groove part; a flow-path upper lid constituting a flat cooling surface; and a laser welding part forming a flow path through which a cooling liquid can flow. The press-molded member and the flow-path upper lid are plated steel sheets each including a Zn-based plating, and a resin coating or an organic coating provided as a chemical conversion coating. The inorganic coating contains at least 50 mass% of a Si-based component or a Zr-based component. The flow path has parallel flow path parts. For a portion or the entirety of the parallel flow path parts, adjacent partial flow paths are disposed at an interval of 20 mm or less, and the proportion in length of a region in which a blow hole and a pit are formed is 0.2 or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cooling structure, a battery unit, and a method for manufacturing a cooling structure. This application claims priority based on Japanese Patent Application No. 2021-085197, filed on May 20, 2021, the contents of which are incorporated herein by reference. [Background technology]

[0002] In order to reduce carbon dioxide emissions, automobiles are increasingly being converted to EVs (Electric Vehicles). In the battery boxes of EVs, a cooling structure must be provided to prevent deterioration of the batteries due to temperature rise. Until now, air-cooled cooling structures have been the mainstream, but in recent years, as batteries have become larger in capacity, there have been an increasing number of cases where water-cooled structures with high cooling capacity are being adopted (e.g., Patent Documents 1 to 4). In water-cooled battery packs, a water coolant flow path through which a coolant flows is formed on the outside of the battery pack. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Japanese Patent Application Publication No. 2020-107443 [Patent Document 2] Japanese Patent No. 6125624 [Patent Document 3] Japanese Patent Application Publication No. 2012-17954 [Patent Document 4] Japanese Patent Application Publication No. 2021-64448 [Patent Document 5] Japanese Patent Publication No. 2001-276990 Summary of the Invention [Problem to be solved by the invention]

[0004] The outer wall and cooling structure of a water-cooled battery pack are often made of aluminum, which has high corrosion resistance against the coolant. However, aluminum has a problem in terms of cost. In addition, since aluminum is soft, it is difficult to reduce the weight of the outer wall by making it thin while maintaining the strength of the outer wall in a cooling structure made of aluminum plate. If these components are made of steel plate, it is possible to provide a water-cooled battery pack at low cost and reduce its weight.

[0005] Here, an aqueous solution of LLC (long life coolant) containing organic components flows as a coolant through the water coolant flow path. Therefore, the members constituting the water coolant flow path are required to have corrosion resistance against the coolant. In addition, the battery pack and the cooling structure are placed on the bottom surface of the automobile, and are exposed to the external environment. Therefore, the members constituting the battery pack and the cooling structure are required to have corrosion resistance equivalent to that of the chassis parts of an automobile. Hereinafter, corrosion resistance against the coolant is referred to as coolant corrosion resistance or inner surface corrosion resistance, and corrosion resistance against the external environment is referred to as outer surface corrosion resistance. In addition, when simply described as "corrosion resistance", it refers to both coolant corrosion resistance and outer surface corrosion resistance.

[0006] One of the means for improving the corrosion resistance of steel sheets is plating. For example, by forming a plating such as a Zn-based plating on the surface of a steel sheet, both the corrosion resistance to coolants and the corrosion resistance of the outer surface can be improved.

[0007] Naturally, the cooling structure must have high cooling efficiency. In addition, the flow paths must be liquid-tight to maintain cooling efficiency and prevent LLC leakage. However, there have been few examples of cooling structures that use galvanized steel sheets to form flow paths, and therefore no studies have been conducted on methods for joining galvanized steel sheets. Spot welding is usually used as a means for firmly joining plated steel sheets. However, since spot welding is a point joining method, it is difficult to ensure liquid-tightness of the flow passages. It is possible to ensure liquid-tightness of the spot welded parts by using a sealer, but there is a risk that the sealer will deteriorate due to LLC. Therefore, when manufacturing a cooling structure, a joining method that can ensure liquid-tightness of the flow passages while maintaining corrosion resistance is also required. In the technology of Patent Document 3, a cooler is manufactured by brazing aluminum-based plated steel sheets. However, the technology of Patent Document 3 is intended to be applied mainly to small devices, and it is difficult to apply it to coolers of various sizes. In addition, the issue of Patent Document 3 is to prevent deformation of the exterior member, and it is difficult to change the joining means of the exterior member. Patent Document 4 discloses a method for manufacturing a battery case using FSW (Friction Stir Welding). According to this document, FSW does not cause blowholes. However, FSW cannot be applied to joining narrow flat areas or curved areas. It is difficult to improve the cooling efficiency by narrowing the flow passage interval of the cooling structure with the technology of Patent Document 3. Patent Document 5 discloses a laser-welded overlap structure of plated steel sheets that uses an adhesive as a spacer to suppress the occurrence of blowholes. However, the technology of Patent Document 5 does not take into account the corrosive environment in which the sheets are exposed to LLC.

[0008] In consideration of the above circumstances, the present invention has an objective of providing a cooling structure, a battery unit, and a method for manufacturing a cooling structure that have high cooling efficiency, excellent liquid-tightness of the flow path, and high coolant corrosion resistance and external corrosion resistance. [Means for solving the problem]

[0009] The gist of the present invention is as follows.

[0010] (1) A cooling structure according to one aspect of the present invention includes a press-formed member having a groove and a bank portion provided around the groove, a flow passage cover which is a flat plate overlapped in a position covering the groove of the press-formed member and constitutes a flat cooling surface, and a laser welded portion which joins opposing surfaces of the flow passage cover and the bank portion to form a flow passage through which a coolant can flow, and the press-formed member and the flow passage cover are each formed by a base steel plate, a Zn-based plating provided on a surface of the base steel plate, and a chemical conversion coating on the surface of the Zn-based plating. and an inorganic coating or a resin coating formed as a film, the inorganic coating containing 50 mass % or more of a Si-based component or a Zr-based component, the flow path having a parallel flow path portion in which a plurality of partial flow paths extending along a first direction are aligned in a second direction perpendicular to the first direction, and in some or all of the parallel flow path portion, a distance between adjacent partial flow paths is 20 mm or less, and a ratio of a length of a region in which blowholes and pits are formed to a total length of the laser weld facing the flow path is 0.2 or less. (2) In the cooling structure described in (1) above, in the parallel flow path portion, the interval between the adjacent partial flow paths may be 0.8 to 15 mm. (3) In the cooling structure described in (1) or (2) above, the partial flow passage may have a width of 6 to 60 mm. (4) In the cooling structure described in (1) or (2) above, the partial flow passage may have a width of 6 to 20 mm. (5) In the cooling structure described in any one of (1) to (4) above, a gap between the press-formed member and the flow path upper cover around the weld metal of the laser weld may be 0.03 mm or more. (6) The cooling structure described in (5) above may further include a spacer having a thickness of 0.03 mm or more arranged between the press-formed member and the flow path upper cover, in the periphery of the weld metal of the laser welded portion. (7) In the cooling structure described in (6) above, the spacer may be a protrusion formed by deforming the flow path upper cover or the press-molded member. (8) The cooling structure described in (5) above may further include a spot weld at or near the laser weld for joining the flow path upper cover and the press-formed member. (9) In the cooling structure described in any one of (1) to (8) above, the cross-sectional shape of the bank portion may be a substantially circular arc, and the radius of curvature of the bank portion at the contact portion between the flow path upper cover and the bank portion may be 15 mm or less. (10) In the cooling structure according to any one of the above (1) to (9), the plated steel sheet constituting the press-formed member and the flow path upper cover may have a thickness of 0.3 to 1.2 mm. (11) In the cooling structure described in any one of (1) to (10) above, the laser weld may have a flow path outer edge weld surrounding all of the flow paths, and a start end and an end end of the laser weld may be excluded from the flow path outer edge weld. (12) In the cooling structure according to any one of (1) to (11) above, a start end and a finish end of the laser weld may be excluded from the cooling structure. (13) In the cooling structure according to any one of (1) to (12) above, a bead height of the laser welded portion on the flow path upper cover may be 0.3 mm or less.

[0011] (14) A battery unit according to another aspect of the present invention comprises a battery cell, a battery pack in which the battery cell is housed, and a cooling structure described in any one of (1) to (13) above, wherein the flow path upper cover of the cooling structure is joined to the battery pack. (15) A battery unit according to another aspect of the present invention comprises a battery cell, a battery pack in which the battery cell is housed, and a cooling structure described in any one of (1) to (13) above, wherein the flow path upper cover of the cooling structure is the battery pack.

[0012] (16) A method for manufacturing a cooling structure according to another aspect of the present invention includes the steps of: press-forming a steel plate to obtain a press-formed member having a groove and a bank portion provided around the groove; and overlapping a flat flow path cover at a position covering the groove of the press-formed member, and laser-welding the flow path cover to the bank portion of the press-formed member to obtain a laser welded portion that forms a flow path through which a coolant can flow. The press-formed member and the flow path cover are made of a base steel plate, a Zn-based plating provided on a surface of the base steel plate, and a Zn-based plating on the surface of the Zn-based plating. and an inorganic coating or resin coating provided as a chemical conversion coating on a surface of the plated steel sheet, the inorganic coating containing a Si-based component or a Zr-based component in a proportion of 50 mass % or more, the flow path having a parallel flow path portion in which a plurality of partial flow paths extending along a first direction are aligned in a second direction perpendicular to the first direction, a distance between adjacent partial flow paths is 20 mm or less in some or all of the parallel flow path portion, and a ratio of a length of an area in which blowholes and pits are formed to a total length of the laser weld facing the flow path is 0.2 or less. (17) In the manufacturing method of the cooling structure described in (16) above, before the laser welding, a spacer having a thickness of 0.03 mm or more may be placed between the press-formed member and the flow path upper cover at the location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed, thereby making the gap between the press-formed member and the flow path upper cover at the location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed 0.03 mm or more. (18) In the method for producing a cooling structure described in (17) above, the spacer may be a protrusion formed by deforming the flow path upper cover or the press-molded member. (19) In the manufacturing method of the cooling structure described in (16) above, before the laser welding, the press-formed member and the flow path upper cover may be spot welded at the location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed, thereby making the gap between the press-formed member and the flow path upper cover at the location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed 0.03 mm or more. Effect of the Invention

[0013] According to the present invention, it is possible to provide a cooling structure, a battery unit, and a method for manufacturing a cooling structure that have high cooling efficiency, excellent liquid-tightness of the flow passages, and high coolant corrosion resistance and outer surface corrosion resistance. [Brief description of the drawings]

[0014] [Figure 1] 1 is a cross-sectional view perpendicular to the extension direction of partial flow paths of a cooling structure in which the cross-sectional shape of a press-formed member is rectangular. FIG. [Figure 2A] 1 is a plan view of a cooling structure in which a flow passage communication portion and a partial flow passage intersect at right angles, as viewed from the side of a press-formed member. FIG. [Figure 2B] 1 is a plan view of a cooling structure in which a flow passage communication portion has a branch structure, as viewed from the press-formed member side. FIG. [Diagram 3] 1 is a cross-sectional view perpendicular to the extension direction of partial flow paths of a cooling structure in which the cross-sectional shape of a press-formed member is corrugated. FIG. [Figure 4] FIG. 11 is an enlarged cross-sectional view of the cooling structure for explaining a distance D between the partial flow paths. [Figure 5A] FIG. 1 is a schematic diagram of a blowhole. [Figure 5B] FIG. 2 is a schematic diagram of a pit. [Figure 5C] FIG. 1 is a schematic diagram showing how vaporized Zn-based coating is released through a gap between plated steel sheets. [Figure 5D] FIG. 4 is a schematic diagram illustrating a method for forming a gap between plated steel sheets using a protrusion. [Figure 5E] FIG. 2 is a schematic diagram illustrating a method for forming a gap between plated steel sheets by using a spot weld. [Figure 6A] 1 is a perspective view of a cooling structure in which an intermediate portion of a laser weld is disposed between a start end and an end end of the laser weld and a flow path. [Figure 6B] FIG. 1 is a perspective view of a cooling structure with the beginning and end portions of a laser weld removed; [Figure 7A] 1 is a schematic diagram of a cooling structure in which the start and end portions of a laser weld are removed from the flow passage outer edge weld. FIG. [Figure 7B] 1 is a schematic diagram of a cooling structure in which the start and end portions of a laser weld are removed from the flow passage outer edge weld. FIG. [Figure 8A] FIG. 2 is a perspective view of the battery unit. [Figure 8B] FIG. 11 is a cross-sectional view of a battery unit using a battery pack as a flow path upper cover. [Figure 8C] 1 is a cross-sectional view of a battery unit in which a battery pack and a flow path upper cover are joined together. FIG. [Figure 9A] 11 is a perspective view showing a state in which a flow path upper cover and a press-formed member provided with a protrusion are overlapped. FIG. [Figure 9B] FIG. 4 is a perspective view showing a state in which a flow passage upper cover and a press-formed member are spot-welded to each other. [Figure 10] FIG. 1 is a perspective view of a cooling structure according to a first embodiment. [Figure 11A] FIG. 11 is a perspective view of a press-formed member before laser welding in the cooling structure of Example 2. [Figure 11B] FIG. 11 is a perspective view of a flow path upper cover before laser welding in the cooling structure of the second embodiment. [Figure 11C] FIG. 11 is a perspective view of a cooling structure according to a second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.

[0016] (1. Cooling structure) First, a cooling structure according to a first embodiment of the present invention will be described. As shown in Fig. 1 and Fig. 2A, the cooling structure 1 according to this embodiment has a press-formed member 11, a flow path upper cover 12, and a laser welded portion 13 that joins them. The laser welded portion is a joint formed of a linear bead (i.e., weld metal). Fig. 1 is a cross-sectional view of the cooling structure 1, and Fig. 2A is a plan view of the cooling structure 1 from the press-formed member 11 side.

[0017] (1.1 Overview of cooling structure) The press-formed member 11 is a member obtained by press-forming a plated steel sheet, and has a groove portion 111 and a bank portion 112 provided around the groove portion 111. In Fig. 1, the bottom of the press-formed member 11 and its periphery form the groove portion 111, and the top of the press-formed member 11 and its periphery form the bank portion 112. The flow path upper cover 12 is a member that forms a flat cooling surface, has a flat plate shape, and is superimposed in a position that covers the groove portion 111 of the press-formed member 11.

[0018] (1.2 Shape of press-formed parts) The press-formed member 11 and the flow passage lid 12 are joined by a laser welded portion 13. Specifically, the laser welded portion 13 joins the opposing surfaces of the flow passage lid 12 and the bank portion 112 of the press-formed member 11. As a result, the flow passage lid 12 and the groove portion 111 form a flow passage 14 through which the coolant can flow. As shown by the dashed line in FIG. 2A, any coolant such as LLC introduced from a coolant inlet 143 can flow through the flow passage 14 to a coolant outlet 144. As a result, the flow passage lid 12, which is a cooling surface, and any object in contact with the flow passage lid 12 can be cooled. Note that the flow passage shown in FIG. 2A has a parallel flow passage portion 141 in which a plurality of partial flow passages 1411 extending along a first direction are arranged in a second direction perpendicular to the first direction, and a flow passage communication portion 142 that communicates these partial flow passages 1411. The first direction is, for example, the longitudinal direction or the lateral direction of the cooling structure 1. The specific configuration of the flow path 14 will be described later.

[0019] The shapes of the banks 112 and the grooves 111 are not particularly limited. In the press-molded member 11 illustrated in Fig. 1, the banks 112 and the grooves 111 have cross sections that are substantially rectangular (trapezoidal). On the other hand, the cross-sectional shape of one or both of the banks 112 and the grooves 111 of the press-molded member 11 may be partially circular or substantially arc-shaped. As shown in Fig. 3, the press-molded member 11 in which the cross-sectional shapes of both the banks 112 and the grooves 111 are partially circular or substantially arc-shaped is called a corrugated sheet. When the press-molded member 11 is a corrugated sheet, the effect of further suppressing the occurrence of blowholes and pits, which will be described later, can be obtained.

[0020] When the cross-sectional shape of the bank portion 112 is a substantially circular arc, the radius of curvature of the bank portion 112 at the contact portion between the flow path upper cover 12 and the bank portion 112, i.e., the laser welded portion 13, may be 15 mm or less, 13 mm or less, or 10 mm or less. The smaller the radius of curvature of the bank portion 112 at the laser welded portion 13, the wider the width W of the partial flow path 1411, and the more the cooling efficiency of the cooling structure 1 is improved.

[0021] The radius of curvature of the bank portion 112 at the contact portion between the flow path top cover 12 and the bank portion 112 is measured in a cross section of the partial flow path 1411 that is parallel to a second direction perpendicular to the first direction in which the partial flow path 1411 extends and is perpendicular to the surface of the flow path top cover 12. As shown in Fig. 3, in this cross section, the radius of a circle R including a total of three points, namely, the center of the weld metal at the center in the plate thickness direction of the bank portion 112 and two points 1 mm away from the center of the weld metal along the second direction, is the radius of curvature of the bank portion 112 at the contact portion between the flow path top cover 12 and the bank portion 112.

[0022] (1.3 Composition of plated steel sheets) The press-formed member 11 and the flow passage upper cover 12 are plated steel sheets having a base steel sheet and a Zn-based plating provided on the surface of the base steel sheet. The configuration of the Zn-based plated steel sheet is not particularly limited, but a preferred example is as follows.

[0023] The plated steel sheets constituting the press-formed member 11 and the flow passage upper cover 12 may have a thickness of 0.3 mm or more. By making the plate thickness 0.3 mm or more, the press formability and the rigidity of the cooling structure 1 can be further improved. The plated steel sheets constituting the press-formed member 11 and the flow passage upper cover 12 may have a thickness of 0.4 mm or more, 0.6 mm or more, or 0.8 mm or more. On the other hand, the plated steel sheets constituting the press-formed member 11 and the flow passage upper cover 12 may have a thickness of 1.2 mm or less. By making the plated steel sheets constituting the press-formed member 11 have a thickness of 1.2 mm or less, it becomes easier to make the press-formed member 11 adhere to the flow passage upper cover 12, and the liquid-tightness of the flow passage is further improved. In addition, by making the plated steel sheets constituting the flow passage upper cover 12 have a thickness of 1.2 mm or less, the cooling efficiency of the cooling structure 1 can be further improved. The plated steel sheets constituting the press-formed member 11 and the flow passage upper cover 12 may have a thickness of 1.1 mm or less, 1.0 mm or less, or 0.8 mm or less. The press-formed member 11 and the flow passage lid 12 may have different thicknesses. Since the thinner the plate thickness, the higher the cooling efficiency, it is preferable that the flow passage lid 12 is thin.

[0024] (1.4 Composition of base steel sheet of plated steel sheet) The base steel plate of the plated steel plate constituting the press-formed member 11 and the flow passage upper cover 12 is not particularly limited. For example, in order to further increase the rigidity of the cooling structure 1, the base steel plate of the flow passage upper cover 12 may be a high-strength steel plate having a tensile strength of 980 MPa or more. On the other hand, in order to further increase the press formability, the base steel plate of the press-formed member 11 may be a mild steel plate having a tensile strength of about 270 MPa, for example, SPCC. Various forms according to the shape and application of the cooling structure 1 can be applied to the base steel plate constituting the press-formed member 11 and the flow passage upper cover 12. Examples of the base steel plate include IF steel with Ti, Nb, B, etc. added, Al-k steel, Cr-added steel, stainless steel, high tensile steel, low carbon steel, medium carbon steel, high carbon steel, alloy steel, etc.

[0025] (1.5 Coating composition of plated steel sheets) Examples of Zn-based plated steel sheets constituting the press-formed member 11 and the flow path upper cover 12 include zinc-plated steel sheets, zinc-nickel-plated steel sheets, zinc-iron-plated steel sheets, zinc-chromium-plated steel sheets, zinc-aluminum-plated steel sheets, zinc-titanium-plated steel sheets, zinc-magnesium-plated steel sheets, zinc-manganese-plated steel sheets, zinc-aluminum (Al)-magnesium (Mg)-plated steel sheets, and zinc-aluminum-magnesium-silicon-plated steel sheets. Furthermore, Zn-based plated steel sheets containing small amounts of different metal elements or impurities such as cobalt, molybdenum, tungsten, nickel, titanium, chromium, aluminum, manganese, iron, magnesium, lead, bismuth, antimony, tin, copper, cadmium, and arsenic in the plating layer, or in which inorganic substances such as silica, alumina, and titania are dispersed, can also be used. Furthermore, the above plating can be combined with other types of plating, and for example, multi-layer plating combined with iron plating, iron-phosphorus plating, nickel plating, cobalt plating, and the like can also be applied. The plating method is not particularly limited, and may be any of known electroplating, hot-dip plating, vapor deposition plating, dispersion plating, vacuum plating, etc. The thickness of the Zn-based plating is not particularly limited, and may be, for example, within the range of 4 to 25 μm. The thickness of the Zn-based plating may be 5 μm or more, 8 μm or more, or 10 μm or more. The thickness of the Zn-based plating may be 22 μm or less, 20 μm or less, or 18 μm or less.

[0026] Furthermore, an inorganic coating or a resin coating is formed on the surface of the Zn-based plated steel sheet as a chemical conversion coating. The inorganic coating contains one or both of a Si-based component and a Zr-based component as main components (for example, 50 mass% or more in terms of mass%). When both a Si-based component and a Zr-based component are contained in the chemical conversion coating, the total content of these components may be 50 mass% or more. The inorganic coating may also contain an organic component. Hereinafter, the "main component" of the chemical conversion coating means a component that accounts for 50 mass% or more of the chemical conversion coating.

[0027] The inorganic film or resin film is preferably conductive. In this case, the weldability or electrodeposition paintability of the Zn-plated steel sheet can be improved. Furthermore, the inorganic film is preferably composed of a compound phase containing one or more of Si-O bonds, Si-C bonds, and Si-OH bonds. In addition, it is preferable that the compound phase contains an acrylic resin, which will be described later. When these requirements are satisfied, the adhesion of the chemical conversion coating can be improved, so that the outer surface corrosion resistance and coolant corrosion resistance of the processed part of the Zn-plated steel sheet can be improved. In addition, it is preferable that the inorganic film contains at least one of V, P, and Co components as a rust-preventive component. The rust-preventive component of the inorganic film is preferably one or more of vanadium oxide, phosphoric acid, and Co nitrate. In addition, the thickness of the inorganic film is preferably more than 0 μm and 1.5 μm or less. In this case, the conductivity or adhesion of the above-mentioned chemical conversion coating can be further improved.

[0028] The resin film preferably contains a resin, an anti-rust pigment, and a conductive pigment. The resin film further contains at least one of metal particles, intermetallic compound particles, conductive oxide particles, and conductive non-oxide ceramic particles as the conductive pigment, and the conductive pigment has a powder resistivity of 185×10 at 25° C. -6 It is preferable that the electrical conductivity of the resin film is Ωcm or less and that the resin film contains at least one constituent element selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, Fe, and W. Furthermore, the resin film preferably contains a conductive pigment in a proportion of 1.0 mass% or more and 30 mass% or less. Furthermore, it is preferable that the average thickness of the resin film is 1.0 μm or more and 15 μm or less. Furthermore, it is preferable that the average particle size of the conductive pigment is 0.5 times or more and 1.5 times or less the average thickness of the resin film. When any one or more of these requirements are satisfied, the outer surface corrosion resistance and coolant corrosion resistance of the Zn-based plated steel sheet can be further improved.

[0029] Examples of chemical conversion coatings are listed in, for example, Japanese Patent No. 4776458, Japanese Patent No. 5336002, Japanese Patent No. 6191806, Japanese Patent No. 6263278, International Publication No. 2020 / 202461, and Japanese Patent No. 4084702. Therefore, the chemical conversion coatings listed in these publications can be suitably used as the chemical conversion coating of this embodiment. Here, an overview of the chemical conversion coating will be described.

[0030] The first example of the chemical conversion coating is an example of an inorganic coating, and is a chemical conversion coating containing an organosilicon compound (silane coupling agent) as the main component. The organosilicon compound is obtained by mixing a silane coupling agent (A) containing one amino group in the molecule and a silane coupling agent (B) containing one glycidyl group in the molecule in a solid content mass ratio [(A) / (B)] of 0.5 to 1.7. The organosilicon compound contains a group represented by the formula -SiR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 each independently represents an alkoxy group or a hydroxyl group, and at least one represents an alkoxy group), and one or more hydrophilic functional groups (b) selected from a hydroxyl group (different from those that may be contained in the functional group (a)) and an amino group, and has an average molecular weight of 1,000 to 10,000.

[0031] In the first example, the Zr-based component is contained in the chemical conversion coating as zirconium hydrofluoric acid. The V component is a vanadium compound, the P component is phosphoric acid, and the Co component is at least one selected from the group consisting of cobalt sulfate, cobalt nitrate, and cobalt carbonate. Examples of vanadium compounds include vanadium pentoxide V2O5, metavanadate HVO3, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide VO2, vanadium oxide, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(OC(=CH2)CH2COCH3))2, vanadium acetylacetonate V(OC(=CH2)CH2COCH3))3, vanadium trichloride VCl3, and phosphorus vanadomolybdic acid. Also usable are pentavalent vanadium compounds reduced to tetravalent or divalent vanadium compounds by an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphoric acid group, and a phosphonic acid group.

[0032] The second example of the chemical conversion coating is an example of an inorganic coating, which is a chemical conversion coating containing an organosilicon compound (silane coupling agent) as a main component. The organosilicon compound has a cyclic siloxane structure in its structure. Here, the "cyclic siloxane bond" refers to a cyclic structure having a structure in which Si-O-Si bonds are continuous, and which is composed only of bonds between Si and O, with the number of Si-O repeats being 3 to 8.

[0033] The organosilicon compound is obtained by blending a silane coupling agent (A) containing at least one amino group in the molecule with a silane coupling agent (B) containing at least one glycidyl group in the molecule in a solid content mass ratio [(A) / (B)] of 0.5 to 1.7. The organosilicon compound (W) thus obtained contains a group represented by the formula -SiR 1 R 2 R 3 (In the formula, R 1 , R 2 and R 3 each independently represents an alkoxy group or a hydroxyl group; R1 , R 2 and R 3 wherein at least one of the functional groups (a) represents an alkoxy group, and at least one hydrophilic functional group (b) selected from the group consisting of a hydroxyl group (when the functional group (a) contains a hydroxyl group, the functional group (b) is separate from the hydroxyl group) and an amino group, and the average molecular weight is preferably 1,000 to 10,000.

[0034] In the second example, the Zr-based component is contained in the chemical conversion coating as a zirconium compound. Examples of the zirconium compound include zirconium hydrofluoric acid, zirconium ammonium fluoride, zirconium sulfate, zirconium oxychloride, zirconium nitrate, and zirconium acetate. Among these, the zirconium compound is more preferably zirconium hydrofluoric acid. When zirconium hydrofluoric acid is used, better corrosion resistance and paintability can be obtained.

[0035] The V component is a vanadium compound, the P component is a phosphate compound, and the Co component is at least one selected from the group consisting of cobalt sulfate, cobalt nitrate, and cobalt carbonate, contained in the chemical conversion coating. Examples of vanadium compounds include vanadium pentoxide V2O5, metavanadate HVO3, ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride VOCl3, vanadium trioxide V2O3, vanadium dioxide VO2, vanadium oxide, vanadium oxysulfate VOSO4, vanadium oxyacetylacetonate VO(OC(=CH2)CH2COCH3)2, vanadium acetylacetonate V(OC(=CH2)CH2COCH3)3, vanadium trichloride VCl3, and phosphorus vanadomolybdic acid. Also usable is a compound obtained by reducing a pentavalent vanadium compound to a tetravalent or divalent vanadium compound using an organic compound having at least one functional group selected from the group consisting of a hydroxyl group, a carbonyl group, a carboxyl group, a primary to tertiary amino group, an amide group, a phosphoric acid group, and a phosphonic acid group.

[0036] Examples of the phosphate compound include phosphoric acid, ammonium phosphate, potassium phosphate, and sodium phosphate. Among these, the phosphate compound is preferably phosphoric acid. When phosphoric acid is used, better corrosion resistance can be obtained.

[0037] The third example of the chemical conversion coating is an example of an inorganic coating, and contains an acrylic resin, zirconium, vanadium, phosphorus, and cobalt. More specifically, the chemical conversion coating contains a particulate acrylic resin (resin particles) and an inhibitor phase. The acrylic resin is preferably a resin containing a polymer of an alkyl (meth)acrylate ester, and may be a polymer obtained by polymerizing only an alkyl (meth)acrylate ester, or may be a copolymer obtained by polymerizing an alkyl (meth)acrylate ester and another monomer. "(Meth)acrylic" means "acrylic" or "methacrylic". The inhibitor phase contains zirconium, vanadium, phosphorus, and cobalt. The zirconium forms a crosslinked structure with the acrylic resin.

[0038] The fourth example of the chemical conversion coating is an example of an inorganic coating, and contains a zirconium carbonate compound, an acrylic resin, a vanadium compound, a phosphorus compound, and a cobalt compound. Examples of the zirconium carbonate compound include zirconium carbonate, ammonium zirconium carbonate, potassium zirconium carbonate, and sodium zirconium carbonate, and one or more of these can be used. Among these, zirconium carbonate and ammonium zirconium carbonate are preferred because of their excellent corrosion resistance.

[0039] The acrylic resin is a resin obtained by copolymerizing a monomer component containing at least styrene (b1), (meth)acrylic acid (b2), (meth)acrylic acid alkyl ester (b3), and acrylonitrile (d4), wherein the amount of acrylonitrile (b4) is 20 to 38% by mass based on the solid content mass of all the monomer components of the resin, and it is a water-soluble resin and an aqueous emulsion resin having a glass transition temperature of -12 to 15°C. That is, the acrylic resin exists in the form of resin particles in the chemical conversion treatment film.

[0040] Examples of the vanadium compound include divalent to tetravalent vanadium compounds. More specifically, for example, pentavalent vanadium compounds such as vanadium pentoxide (V2O5), metavanadic acid (HVO3), ammonium metavanadate, sodium metavanadate, vanadium oxytrichloride (VOCl3) reduced to divalent to tetravalent with a reducing agent, vanadium trioxide (V2O3), vanadium dioxide (VO2), vanadyl sulfate (VOSO4), vanadyl oxalate [VO(COO)2], vanadium oxyacetylacetonate [VO(OC(CH3)=CHCOCH3))2], vanadium acetylacetonate [V(OC(CH3)=CHCOCH3))3], vanadium trichloride (VCl3), phosphovanadomolybdic acid {H 15-X [PV 12-x Mo x O 40 ·nH2O (6 < x < 12, n < 30)}, vanadium sulfate (VSO4·8H2O), vanadium dichloride (VCl2), vanadium compounds with an oxidation number of tetravalent to divalent such as vanadium monoxide (VO), etc. can be mentioned.

[0041] Examples of the phosphorus compound include inorganic acid anions having an acid group containing phosphorus and organic acid anions having an acid group containing phosphorus. Examples of the inorganic acid anions having an acid group containing phosphorus include inorganic acid anions in which at least one hydrogen of inorganic acids such as orthophosphoric acid, metaphosphoric acid, condensed phosphoric acid, pyrophosphoric acid, tripolyphosphoric acid, tetraphosphoric acid, hexametaphosphoric acid, etc. is free and salts thereof.

[0042] Examples of organic acid anions having an acid group containing phosphorus include organic acid anions having at least one free hydrogen atom, such as organic phosphonic acids such as 1-hydroxymethane-1,1-diphosphonic acid, 1-hydroxyethane-1,1-diphosphonic acid, 1-hydroxypropane-1,1-diphosphonic acid, 1-hydroxyethylene-1,1-diphosphonic acid, 2-hydroxyphosphonoacetic acid, aminotri(methylenephosphonic acid), ethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), hexamethylenediamine-N,N,N',N'-tetra(methylenephosphonic acid), diethylenetriamine-N,N,N',N'',N''-penta(methylenephosphonic acid), 2-phosphonic acid butane-1,2,4-tricarboxylic acid, inositol hexaphosphonic acid, and phytic acid, and organic phosphoric acid, and salts thereof.

[0043] Examples of the cobalt compound include cobalt sulfate, cobalt nitrate, and cobalt carbonate.

[0044] A fifth example of the chemical conversion coating is an example of a resin coating, and contains at least one of metal particles, intermetallic compound particles, conductive oxide particles, and conductive non-oxide ceramic particles as a conductive pigment. The conductive pigment has a powder resistivity of 185×10 at 25° C. -6 The material has a resistivity of Ωcm or less and contains at least one element selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, Fe, and W.

[0045] Examples of intermetallic compounds include ferrosilicon and ferromanganese. Examples of conductive oxide particles include materials that have conductivity by doping impurities into the crystal lattice of the oxide (doped conductive oxides) or oxides whose surfaces are modified with conductive materials. The former can be generally known metal oxides doped with one or more metal elements selected from Al, Nb, Ga, Sn, etc. (e.g., Al-doped zinc oxide, Nb-doped zinc oxide, Ga-doped zinc oxide, Sn-doped zinc oxide, etc.). The latter can be generally known zinc oxide or silica modified with SnO2, which has conductivity in the oxide. The conductive oxide is preferably a doped conductive oxide, and the doped conductive oxide is preferably Al-doped zinc oxide.

[0046] The conductive non-oxide ceramic particles are composed of ceramics made of elements or compounds that do not contain oxygen. Examples of the conductive non-oxide ceramic particles include boride ceramics, carbide ceramics, nitride ceramics, and silicide ceramics. In addition, boride ceramics, carbide ceramics, nitride ceramics, and silicide ceramics are non-oxide ceramics that have boron (B), carbon (C), nitrogen (N), and silicon (Si) as major non-metallic constituent elements, respectively, and these generally known non-oxide ceramics that contain one or more selected from the group consisting of Zn, Si, Zr, V, Cr, Mo, Mn, and W can be used. Furthermore, the non-oxide ceramic particles are more preferably the non-oxide ceramics exemplified below in terms of the presence or absence of industrial products, stable distribution in domestic and overseas markets, price, electrical resistivity, and the like. For example, particles of Mo2B, MoB, MoB2, Mo2B5, NbB2, VB, VB2, W2B5, ZrB2, Mo2C, V2C, VC, WC, W2C, ZrC, Mo2N, VN, ZrN, Mo3Si, Mo5Si3, MoSi2, NbSi2, Ni2Si, Ta2Si, TaSi2, TiSi, TiSi2, V5Si3, VSi2, W3Si, WSi2, ZrSi, ZrSi2, CrB, CrB2, Cr3C2, Cr2N, CrSi, and particles of a mixture of two or more selected from these are more preferred.

[0047] The sixth example of the chemical conversion coating is an example of a resin coating, which contains a resin having a urethane bond and conductive particles (conductive pigments). The resin having a urethane bond is an organic resin obtained from a film-forming resin raw material that contains (a) a polyester polyol having at least three functional groups, and (b) a blocked product of an organic polyisocyanate or a blocked product of a prepolymer having an NCO group at its end, which is obtained by reacting an organic polyisocyanate with an active hydrogen compound.

[0048] The polyester polyol (a) having a functionality of at least 3 can be obtained by esterifying a dicarboxylic acid, a glycol, and a polyol having at least 3 OH groups.

[0049] Examples of dicarboxylic acids used in the production of polyester polyols include aliphatic dicarboxylic acids such as succinic acid, succinic anhydride, adipic acid, azelaic acid, sebacic acid, dodecanoic diacid, maleic acid, maleic anhydride, fumaric acid, itaconic acid, and dimer acid; and aromatic and alicyclic dicarboxylic acids such as phthalic acid, phthalic anhydride, isophthalic acid, isophthalic acid dimethyl ester, terephthalic acid, terephthalic acid dimethyl ester, 2,6-naphthalenedicarboxylic acid, hexahydrophthalic anhydride, tetrahydrophthalic anhydride, cyclohexanedicarboxylic acid, cyclohexanedicarboxylic acid dimethyl ester, methylhexahydrophthalic anhydride, himic anhydride, and methyl himic anhydride.

[0050] Examples of glycols include ethylene glycol, diethylene glycol, propylene glycol, 1,3-butylene glycol, 1,4-butylene glycol, dipropylene glycol, 1,5-pentanediol, 1,6-hexanediol, neopentyl glycol, neopentyl glycol ester of hydroxydivalanic acid, triethylene glycol, 1,9-nonanediol, 3-methyl-1,5-pentanediol, 2,2,4-trimethyl-1,3-pentanediol, 2-ethyl-1,3-hexanediol, 2,4-diethyl-1,5-pentanediol, polycaprolactone diol, polypropylene glycol, Examples of the polyphenols include aliphatic polyphenols such as glycol, polytetramethylene ether glycol, polycarbonate diol, 2-n-butyl-2-ethyl-1,3-propanediol, and 2,2-diethyl-1,3-propanediol; and aliphatic or aromatic polyphenols such as cyclohexanedimethanol, cyclohexanediol, 2-methyl-1,1-cyclohexanedimethanol, xylylene glycol, bishydroxyethyl terephthalate, 1,4-bis(2-hydroxyethoxy)benzene, hydrogenated bisphenol A, an ethylene oxide adduct of bisphenol A, and a propylene oxide adduct of bisphenol A.

[0051] Examples of polyols having at least three OH groups include glycerin, trimethylolpropane, trimethylolethane, 1,2,6-hexanetriol, pentaerythritol, diglycerin, and ethylene oxide adducts, propionate adducts, and ε-caprolactone adducts using these polyols as initiators.

[0052] Examples of the blocked compounds of (b) include compounds having at least two NCO groups, such as aliphatic diisocyanates such as trimethylene diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, pentamethylene diisocyanate, 1,2-propylene diisocyanate, 2,3-butylene diisocyanate, 1,3-butylene diisocyanate, 2,4,4- or 2,2,4-trimethylhexamethylene diisocyanate, dodecamethylene diisocyanate, and 2,6-diisocyanatomethyl caproate. and other isocyanates such as 1,3-cyclopentane diisocyanate, 1,4-cyclohexane diisocyanate, 1,3-cyclohexane diisocyanate, 3-isocyanatomethyl-3,5,5-trimethylhexyl isocyanate, 4,4'-methylenebis(cyclohexyl isocyanate), methyl-2,4-cyclohexane diisocyanate, methyl-2,6-cyclohexane diisocyanate, 1,2-bis(isocyanatomethyl)cyclohexane, 1,4-bis(isocyanatomethyl)cyclohexane, 1,3-bis(isocyanatomethyl)cyclohexane, Cycloalkylene diisocyanates such as (methyl)cyclohexane and trans-cyclohexane-1,4-diisocyanate, and diisocyanates such as m-xylene diisocyanate, m-phenylene diisocyanate, p-phenylene diisocyanate, 4,4'-diphenyl diisocyanate, 1,5-naphthalene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4- or 2,6-tolylene diisocyanate, 4,4'-toluidine diisocyanate, dianisidine diisocyanate, 4,4'-diphenyl ether diisocyanate, aromatic diisocyanates such as isocyanate, for example, ω,ω'-diisocyanato-1,3-dimethylbenzene, ω,ω'-diisocyanato-1,4-dimethylbenzene, ω,ω'-diisocyanato-1,4-diethylbenzene, α,α,α',α'-tetramethylmetaxylylenediisocyanate, and aromatic aliphatic diisocyanates such as triphenylmethane-4,4',4''-triisocyanate, 1,3,5-triisocyanatobenzene, 2,4,6-triisocyanatotoluene, ω-isocyanatoethyl-2,Examples of such blocked products include triisocyanates such as 6-diisocyanatocaproate, tetraisocyanates such as 4,4'-diphenylmethylmethane-2,2',5,5'-tetraisocyanate, and derivatives of isocyanate compounds such as dimers, trimers, biuret, allophanates, carbodiimides, polymethylene polyphenyl polyisocyanates (crude MDI, c-MDI, polymeric MDI), and crude TDI, as well as blocked products of prepolymers having NCO groups at their ends obtained by reacting these with active hydrogen compounds.

[0053] The conductive particles are corrosion-resistant particles that are alloys or compounds containing 50% by mass or more of Si, or composites thereof. The conductive particles are preferably ferrosilicon. Anti-rust pigments may be added to the chemical conversion coating. Examples of the anti-rust pigments include known anti-rust pigments such as hexavalent chromates, such as strontium chromate and calcium chromate. When it is desired to avoid using hexavalent chromium compounds as anti-rust agents, it is possible to use those that release one or more of silicate ions, phosphate ions, and vanadate ions.

[0054] Examples of the chemical conversion coating of the present embodiment are not limited to those described above.

[0055] The method for forming the above-mentioned chemical conversion coating is not particularly limited, and a chemical conversion solution (coating solution) corresponding to each of the above compositions may be applied to a Zn-based plated steel sheet by a known method, followed by baking and drying. An example of a preferred combination of a Zn-based plated steel sheet and a chemical conversion coating is a combination of a Zn-Al-Mg plated steel sheet and an inorganic coating containing a Si-based component as a main component.

[0056] (1.7 Flow Path Configuration) Next, the configuration of the flow passage 14 of the cooling structure 1 according to this embodiment will be described. In order to improve the cooling efficiency of the cooling structure 1, it is preferable to increase the contact area between the cooling liquid and the flow path lid 12, that is, to increase the area of ​​the region of the flow path lid 12 facing the flow path 14. For this reason, the flow path 14 has a parallel flow path portion 141 in which a plurality of partial flow paths 1411 extending along a first direction are arranged in a second direction perpendicular to the first direction. The first direction is, for example, the longitudinal direction or lateral direction of the cooling structure 1. By providing the parallel flow path portion 141 in which a plurality of partial flow paths 1411 are arranged in parallel, the contact area between the cooling liquid and the flow path lid 12 can be increased. However, in order to ensure even better cooling efficiency, the present inventors have conducted further studies.

[0057] Increasing the width W of the partial flow passage 1411 has been considered as a means for further increasing the contact area between the coolant and the flow passage upper cover 12. However, the wider the width W of the partial flow passage 1411, the greater the stress applied to the laser welded portion 13, which may shorten the life of the cooling structure 1. Furthermore, if the width W of the partial flow passage 1411 is too wide, the coolant will not flow stably along the extension direction of the partial flow passage 1411, i.e., the first direction, which may cause uneven cooling.

[0058] Another means for further increasing the contact area between the coolant and the flow path upper cover 12 is to narrow the interval D between the partial flow paths 1411. This means can improve the cooling efficiency while preventing an increase in stress applied to the laser welded portion 13 and the occurrence of cooling unevenness. For the above reasons, in the cooling structure 1 according to this embodiment, the interval D between the adjacent partial flow paths 1411 is set to 20 mm or less in a part or all of the parallel flow path portion 141. The interval D between the partial flow paths 1411 may be set to 18 mm or less, 16 mm or less, or 15 mm or less. The lower limit value of the interval D between the partial flow paths 1411 is not particularly limited, but from the viewpoint of preventing poor joining, the interval D may be set to 0.8 mm or more, 1 mm or more, 3 mm or more, 5 mm or more, or 8 mm or more.

[0059] The interval D of the partial channels 1411 is preferably within the above-mentioned range in the entire parallel channel section 141. However, for example, by arranging another component such as a screw hole between the partial channels 1411, the interval D of the partial channels 1411 may be more than 20 mm in a part of the parallel channel section 141. In other words, the interval D of the partial channels 1411 may be within the above-mentioned range in a part of the parallel channel section 141.

[0060] As long as the interval D of the partial flow paths 1411 is within the above-mentioned range, the width W of the partial flow paths 1411 is not particularly limited. From the viewpoint of further increasing the contact area between the flow path forming portion and the flow path upper cover 12, the width W of the partial flow paths 1411 may be 6 mm or more, 8 mm or more, or 10 mm or more. On the other hand, from the viewpoint of further increasing the bonding strength between the press-formed member 11 and the flow path upper cover 12 and further increasing the uniformity of cooling, the width W of the partial flow paths 1411 may be 60 mm or less, 30 mm or less, 25 mm or less, or 20 mm or less. The height of the partial flow paths 1411 is also not particularly limited, but may be, for example, 1 mm or more in order to further improve the cooling efficiency. On the other hand, in order to reduce the weight of the cooling structure 1, the height of the partial flow paths 1411 may be 10 mm or less. The shape of the partial flow paths 1411 described above may be applied to the partial flow paths constituting the flow path communication portion 142.

[0061] In the cooling structure 1 according to the present embodiment, the flow path 14 and the partial flow path 1411 included therein refer to a space through which the coolant flows easily and exerts a substantial cooling effect. For this reason, the flow path 14 and the partial flow path 1411 are defined as a space between the flow path upper cover 12 and the press-formed member 11, as shown in FIG. 4, and have a thickness of 0.5 mm or more along a direction perpendicular to the flow path upper cover 12. The interval D of the partial flow path 1411 refers to the interval between the spaces defined above. That is, the interval D of the partial flow path 1411 refers to the total length of the width of the region where the laser welded portion 13, the flow path upper cover 12, and the press-formed member 11 are in contact, and the width of the region where the gap between the flow path upper cover 12 and the press-formed member 11 is less than 0.5 mm. Although not shown in FIG. 4, the width W of the partial flow path 1411 refers to the width of the space defined above. That is, the width W of the partial flow channels 1411 refers to the width of a space having a thickness of 0.5 mm or more along a direction perpendicular to the flow channel top cover 12. Moreover, the interval D of the partial flow channels 1411 and the width W of the partial flow channels are values ​​measured along a second direction perpendicular to the first direction in which the partial flow channels 1141 extend.

[0062] (1.8 Structure of laser welds) In order to set the interval D of the partial flow paths 1411 within the above-mentioned range, in the cooling structure 1 according to this embodiment, the joints for forming the flow paths 14 are laser welded parts 13. Laser welding can reduce the bead width. Therefore, it is an effective joining means for narrowing the interval D of the partial flow paths 1411. In addition, since laser welding forms a linear bead, it can improve the liquid-tightness of the flow paths 14 compared to point joining means such as spot welding.

[0063] In the laser welded portion 13, a blowhole B as shown in FIG. 5A and a pit P as shown in FIG. 5B may be formed. The blowhole B is a spherical cavity that occurs in the weld metal. The pit P is an open hole that reaches the surface of the welded portion. The blowhole B and the pit P are caused by the Zn-based plating vaporized during the laser welding. Since the boiling point of the Zn-based plating is lower than the melting point of the base steel sheet, the Zn-based plating is gasified by the laser welding. The blowhole and the pit cause a decrease in the corrosion resistance and the liquid-tightness of the cooling structure 1.

[0064] For the above reasons, in the cooling structure 1 according to the present embodiment, the ratio of the length of the region in which the blowholes B and the pits P are formed to the total length of the laser welds 13 facing the flow path 14 is set to 0.2 or less. Here, the laser welds 13 facing the flow path 14 refer to those of all the laser welds 13 that are not separated from the flow path 14 by other laser welds. For example, in FIG. 6A, four laser welds 13 are formed surrounding the flow path 14. Of these, the region that forms a rectangle surrounding the flow path 14 is the "laser welds 13 facing the flow path 14". The laser welds 13 facing the flow path 14 are exposed to the cooling liquid flowing inside the flow path 14. On the other hand, the laser welds 13 protruding outside the rectangle are separated from the flow path 14 by other laser welds 13, and therefore do not fall under the "laser welds 13 facing the flow path 14". Of the laser welds 13, the region that does not fall under the "laser welds 13 facing the flow path 14" is not exposed to the cooling liquid.

[0065] The laser welded portion 13 facing the flow path 14 strongly affects the liquid tightness of the flow path 14 and the inner surface corrosion resistance of the cooling structure 1. Therefore, it is preferable to make the amount of blowholes B and pits P in the laser welded portion 13 facing the flow path 14 as small as possible. In order to ensure the liquid tightness and coolant corrosion resistance required for the cooling structure 1, it is necessary that the ratio of the length of the region where the blowholes B and pits P are formed to the total length of the laser welded portion 13 facing the flow path 14 is 0.2 or less. The ratio of the length of the region where the blowholes B and pits P are formed to the total length of the laser welded portion 13 facing the flow path 14 is preferably 0.18 or less, 0.15 or less, 0.10 or less, or 0.05 or less. On the other hand, the region of the laser welded portion 13 that does not face the flow path 14 is not exposed to the coolant. Therefore, it is not necessary to limit the amount of blowholes B and pits P in the laser welded portion 13 that does not face the flow path 14.

[0066] The ratio of the length of the region where blowholes B and pits P are formed to the total length of the laser welded portion 13 facing the flow path 14 is measured by the following procedure. By observing the laser welded portion 13 with an X-ray, the presence of blowholes B and the length of blowholes B in the weld line direction can be confirmed. In addition, since pits P are exposed on the surface of the laser welded portion 13, the length of pits P in the weld line direction can be measured visually. The sum of the lengths of blowholes B and pits P in the weld line direction measured in this manner is divided by the total length of the laser welded portion 13 facing the flow path 14 to determine the ratio of the length of the region where blowholes B and pits P are formed to the total length of the laser welded portion 13 facing the flow path 14.

[0067] There is no particular limitation on the means for reducing the blowholes B and pits P. A suitable example will be described below.

[0068] In order to reduce the occurrence of blowholes B and pits P, the gap between the press-formed member 11 and the flow passage upper cover 12 around the weld metal of the laser welded portion 13 may be 0.03 mm or more, 0.05 mm or more, 0.1 mm or more, or 0.2 mm or more. As a result, as shown in FIG. 5C, the Zn-based plating vaporized during laser welding is not introduced into the weld metal and is released to the outside of the welded portion. Therefore, the gap provided on the mating surface between the plated steel sheets can reduce the occurrence of blowholes B and pits P. The upper limit of the gap between the press-formed member 11 and the flow passage upper cover 12 around the weld metal of the laser welded portion 13 is not particularly limited, but in order to reliably perform laser welding, it is preferable to set this gap to 0.5 mm or less. In addition, a gap provided at a location away from the weld metal of the laser welded portion 13, for example, at a location 5 mm or more away from the weld metal, does not affect the occurrence rate of blowholes B and pits P. Therefore, the size of the gap at a location 5 mm or more away from the weld metal is not particularly limited.

[0069] In order to provide the above-mentioned gap, for example, a spacer having a thickness of 0.03 mm or more may be disposed between the press-formed member 11 and the flow passage upper cover 12 around the weld metal of the laser welded portion 13. The thickness of the spacer can be appropriately selected according to the size of the gap to be provided. The thickness of the spacer may be 0.05 mm or more, 0.1 mm or more, or 0.2 mm or more. The thickness of the spacer may be 0.5 mm or less, or 0.3 mm or less. If the gap is too wide, melting may occur, which may cause water leakage, so the size of the gap is preferably equal to or less than the plate thickness t of the thinner of the press-formed member 11 and the flow passage upper cover 12, and more preferably equal to or less than 0.8t. The spacer may be, for example, a metal foil sandwiched between the press-formed member 11 and the flow passage upper cover 12. On the other hand, as shown in FIG. 5D, the flow passage upper cover 12 or the press-formed member 11 may be deformed to form a protrusion 15, which may be used as a spacer. When the projections 15 are used as spacers, the height of the projections 15 is regarded as the thickness of the spacer.

[0070] Instead of or in addition to using a spacer, a gap may be formed by spot welding as shown in FIG. 5E. When plated steel sheets are spot-welded, a gap may be formed at the mating surface of the plated steel sheets. Therefore, by spot-welding the press-formed member 11 and the flow path upper cover 12 before laser welding, a gap is provided between the press-formed member 11 and the flow path upper cover 12, and the occurrence of blowholes B and pits P during laser welding can be suppressed. From the viewpoint of workability, it is more preferable to form the gap by spot welding than by using a spacer.

[0071] The spot welds 16 that join the press-formed member 11 and the flow passage upper cover 12 may be formed at a location that overlaps with the laser welds 13 or near the laser welds 13. More preferably, the spot welds 16 are formed near the laser welds 13 and at a location that does not face the flow passage 14. In other words, it is preferable to provide the spot welds 16 so that the laser welds 13 are disposed between the spot welds 16 and the flow passage 14. The size of the gap formed by the spot welds 16 varies depending on the spot welding conditions. The distance between the spot welds 16 and the laser welds 13 is not particularly limited, but if the shortest distance from the spot welds 16 to the laser welds 13 is set to 1 mm, for example, and an appropriate gap is formed, blowholes B and pits P can be prevented. It is preferable to comprehensively determine the distance between the spot welds 16 and the laser welds 13 while taking into consideration the spot welding conditions, the thickness of the plated steel sheet, and the strength of the plated steel sheet.

[0072] The method for measuring the gap between the press-formed member 11 and the flow path lid 12 around the weld metal of the laser weld 13 is as follows: The laser weld 13 is cut in a direction perpendicular to the weld line direction, the cross section is observed, and the distance between the press-formed member 11 and the flow path lid 12 at a position 0.1 mm away from the end of the weld metal between the press-formed member 11 and the flow path lid 12 in the weld width direction is the amount of the gap between the press-formed member 11 and the flow path lid 12 around the weld metal of the laser weld 13.

[0073] Examples of suitable means for suppressing the occurrence of blowholes B and pits P are as described above. However, in the cooling structure 1 according to the present embodiment, various other means can be adopted. For example, the Zn-based plating at the portion to be laser welded may be removed in advance before the base steel sheet of the plated steel sheet is melted and solidified by laser welding. In this case, it is possible to suppress the occurrence of blowholes B and pits P without providing a gap between the press-formed member 11 and the flow path upper cover 12. For example, the welding target portion may be heated using a laser to a temperature range from the melting point of the Zn-based plating to the melting point of the base steel sheet before laser welding. This allows the Zn-based plating to be removed from the welding target portion. In addition, the Zn-based plating may be mechanically removed from the welding target portion of the plated steel sheet by using a means such as grinding before laser welding.

[0074] As long as the occurrence rates of blowholes B and pits P are within the above-mentioned ranges, the configuration of the laser welded portion 13 is not particularly limited, and various configurations can be adopted according to the shape of the flow passage 14. A preferred embodiment of the laser welded portion 13 will be described below.

[0075] For example, the bead width on the laser irradiation side, i.e., the larger of the bead width on the surface of the laser welded portion 13 on the flow path upper cover 12 and the bead width on the surface of the laser welded portion 13 on the press-formed member 11, may be set to 0.8 to 1.5 mm. By setting the bead width to 0.8 mm or more, the liquid-tightness of the flow path 14 can be further improved. On the other hand, by setting the bead width to 1.5 mm or less, evaporation of the plating in the vicinity of the bead can be prevented, and the corrosion resistance of the cooling structure 1 can be further improved.

[0076] 6A, the laser welded portion 13 is composed of a starting portion 131, a terminal portion 132, and an intermediate portion 133 therebetween. The starting portion 131 of the laser welded portion 13 is a portion corresponding to a portion where the laser welding starts, and the terminal portion 132 of the laser welded portion 13 is a portion corresponding to a portion where the laser welding ends. In this embodiment, it is not necessary to distinguish between the starting portion 131 and the terminal portion 132. The starting portion 131 and the terminal portion 132 are clearly different from the intermediate portion 133 in terms of width, etc., so that the starting portion 131 and the terminal portion 132 can be clearly distinguished from the intermediate portion 133.

[0077] The intermediate portion 133 has fewer weld defects than the starting portion 131 and the terminal portion 132, and therefore tends to have better corrosion resistance and liquid tightness. Therefore, it is preferable that the flow path 14 is formed using the intermediate portion 133 of the laser welded portion 13 and is separated from the starting portion 131 and the terminal portion 132. In other words, as illustrated in Fig. 6A, it is preferable that the laser welding is performed so that the intermediate portion 133 of the laser welded portion 13 is disposed between the starting portion 131 and the terminal portion 132 of the laser welded portion 13 and the flow path 14. This makes it possible to prevent the starting portion 131 and the terminal portion 132 from being exposed to the coolant. 6B, it is more preferable that the starting end 131 and the terminal end 132 of the laser welded portion 13 are removed from the cooling structure 1. For example, a tab plate T is provided on the flow path upper cover 12 or the press-formed member 11 before laser welding, and laser welding is performed so that the starting end 131 and the terminal end 132 are formed on the tab plate T, and then the tab plate T is cut and removed, thereby obtaining a cooling structure 1 that does not include the starting end 131 and the terminal end 132 of the laser welded portion 13.

[0078] A configuration in which the start end 131 and the end end 132 are removed only in the portion of the cooling structure 1 where leakage of liquid is a concern may be applied. For example, in the cooling structure 1 shown in Figs. 7A and 7B, when the flow passage upper cover 12 is peeled off from the press-formed member 11 at the portion (dark color portion with reference symbol 13A) of the laser welded portion 13 provided along the outer edge of the press-formed member 11 and the flow passage upper cover 12, the cooling liquid leaks out of the cooling structure 1. On the other hand, in the cooling structure 1 shown in Figs. 7A and 7B, even if the flow passage upper cover 12 is peeled off from the press-formed member 11 at the laser welded portion 13 provided in the area surrounded by the flow passage 14, the cooling water does not leak out of the cooling structure 1. Therefore, when the portion (dark color portion with reference symbol 13A) of the laser welded portion 13 that surrounds all the flow passages 14 is defined as the flow passage outer edge welded portion 13A, it is preferable that the start end 131 and the end end 132 are removed from the flow passage outer edge welded portion 13A. In this case, even if the laser welded portion 13 excluding the flow path outer edge welded portion 13A includes a starting end portion 131 and an ending end portion 132, the leakage of cooling water to the outside of the cooling structure 1 can be sufficiently prevented. The cooling structure 1 illustrated in FIG. 7A is obtained by manufacturing the flow passage outer edge welded portion 13A using only the intermediate portion 133 of the laser welded portion 13, as in FIG. 5A. In this case, the start end and the end end are excluded from the flow passage outer edge welded portion 13A, but remain in the cooling structure 1. On the other hand, the cooling structure 1 illustrated in FIG. 7B is obtained by providing a tab plate T to the flow passage upper cover 12 or the press-formed member 11 before laser welding, performing laser welding so that the start end 131 and the end end 132 are formed on the tab plate T, and then cutting and removing the tab plate T, as in FIG. 5B. In this case, the start end and the end end generated when forming the flow passage outer edge welded portion 13A do not remain in the cooling structure 1. In addition, by starting laser irradiation from a point that does not hit the flow path upper lid 12 and the press-formed member 11, performing laser welding, and irradiating the laser to a point that does not hit the flow path upper lid 12 and the press-formed member 11 in a running manner, and then stopping the laser irradiation, the starting and ending ends of the formation of the flow path outer edge welded portion 13A do not remain in the cooling structure 1.

[0079] The bead height of the laser welded portion 13 on the flow path upper cover 12 may be 0.3 mm or less. By making the bead height of the laser welded portion 13 0.3 mm or less, the gap between the flow path upper cover 12 and the object to be cooled (e.g., a battery pack or a battery cell) can be reduced, and the cooling efficiency can be further improved. The bead height of the laser welded portion 13 may be reduced, for example, by controlling the laser welding conditions. Also, the bead height may be reduced by grinding the bead after the laser welding is completed.

[0080] (1.9 Other Configurations) As shown in FIG. 2A, the flow path 14 may further include a flow path communication part 142 that communicates the plurality of partial flow paths 1411. The flow path 14 may further include a coolant inlet 143 and a coolant outlet 144 for introducing a coolant into the flow path. When the flow path 14 has the flow path communication part 142, the flow path 14 forms one space. In this case, the cooling structure 1 may be provided with one coolant inlet 143 and one coolant outlet 144. On the other hand, the flow path communication part 142 may not be provided in the cooling structure 1. In this case, the plurality of partial flow paths 1411 may each be provided with a coolant inlet 143 and a coolant outlet 144. Only some of the plurality of partial flow paths 1411 may be communicated by the flow path communication part 142, and the flow path 14 may form two or more spaces.

[0081] In FIG. 2A and the like, each of the two flow passage communication parts 142 is a straight flow passage, and the flow passage communication part 142 communicates with all the partial flow passages 1411 so as to be perpendicular to the flow passage communication part 142. However, the shape of the flow passage communication part 142 and the arrangement of the flow passage communication part 142 and the partial flow passages 1411 are not limited to this. For example, the angle between the flow passage communication part 142 and the partial flow passages 1141 is not limited to 90°, and can be appropriately selected according to the application of the cooling structure 1. In addition, the flow passage communication part 142 may have a branch structure. As shown in FIG. 2B, each of the two flow passage communication parts 142 may branch in a fan shape starting from the coolant inlet 143 or the coolant outlet 144, and may communicate with each partial flow passage 1411 at various angles at the branched ends. In FIG. 2B, the laser welded part 13 is omitted.

[0082] The planar shapes of the press-molded member 11 and the flow passage lid 12 constituting the cooling surface of the cooling structure 1 are not particularly limited. For example, when the cooling structure 1 is used to cool the battery of an EV, the planar shape of the flow passage lid 12 is desirably a rectangle. In this case, the size of the flow passage lid 12 in plan view is preferably 1000 to 2300 mm in the longitudinal direction and 200 mm to 1500 mm in the lateral direction. Similarly, the size of the press-molded member 11 in plan view is preferably 1000 to 2300 mm in the longitudinal direction and 200 mm to 1500 mm in the lateral direction. When manufacturing a cooling structure 1 in which the press-molded member 11 and / or the flow passage lid 12 have a large area and the distance D of the flow passage is narrow, poor bonding between the bank portion 112 and the flow passage lid 12 is likely to be a problem, but for example, by using a manufacturing method described later, poor bonding can be easily avoided. The longitudinal size of the flow path lid 12 in plan view may be 1200 mm or more, 1400 mm or more, or 1600 mm or more. The longitudinal size of the flow path lid 12 in plan view may be 2200 mm or less, 2000 mm or less, or 1800 mm or less. The lateral size of the flow path lid 12 in plan view may be 250 mm or more, 500 mm or more, or 700 mm or more. The lateral size of the flow path lid 12 in plan view may be 1400 mm or less, 1300 mm or less, or 1200 mm or less. The size of the press-molded member 11 in the longitudinal direction in a plan view may be 1200 mm or more, 1400 mm or more, or 1600 mm or more. The size of the press-molded member 11 in the longitudinal direction in a plan view may be 2200 mm or less, 2000 mm or less, or 1800 mm or less. The size of the press-molded member 11 in the lateral direction in a plan view may be 250 mm or more, 500 mm or more, or 700 mm or more. The size of the press-molded member 11 in the lateral direction in a plan view may be 1400 mm or less, 1300 mm or less, or 1200 mm or less.

[0083] As described above, in the cooling structure according to the first embodiment, the press-formed member 11 and the flow path upper cover 12 are made of Zn-based plated steel sheet, thereby ensuring the corrosion resistance of the outer surface and the coolant. This makes it possible to suppress water path corrosion and the occurrence of contamination that causes a decrease in thermal conductivity and clogging. Furthermore, in the cooling structure of the first embodiment, by laser welding the press-formed member 11 and the flow path lid 12, the distance D between the partial flow paths 1411 in the parallel flow path section 141 can be set to 20 mm or less, thereby increasing the area of ​​contact between the coolant and the flow path lid 12 and improving the cooling efficiency. Additionally, in the cooling structure according to the first embodiment, the press-formed member 11 and the flow path upper cover 12 are laser-welded, and further, the occurrence of blowholes and pits is suppressed, thereby making it possible to improve the liquid-tightness of the flow path .

[0084] (2. Battery unit) Next, a battery unit according to a second embodiment of the present invention will be described. As shown in Fig. 8A to Fig. 8C, the battery unit 2 according to this embodiment has a battery cell 21, a battery pack 22 in which the battery cell 21 is housed, and the cooling structure 1 according to the first embodiment.

[0085] When incorporating the cooling structure 1 into the battery unit 2, as shown in Fig. 8B, the battery pack 22 can be used as the flow path upper cover 12 of the cooling structure 1. In other words, the bank portion 112 of the press-formed member 11 and the battery pack 22 can be laser welded. By integrating the battery pack 22 with the cooling structure 1, the battery unit 2 can cool the battery cells 21 extremely efficiently.

[0086] On the other hand, a structure in which the battery pack 22 and the cooling structure 1 are separated may be adopted. For example, the battery unit 2 may be manufactured by joining the flow path upper cover 12 and the battery pack 22. In this case, as shown in FIG. 8C, a gap filler 23 may be disposed between the flow path upper cover 12 and the battery pack 22. Due to some cause (such as an error in dimensional accuracy or a complex uneven shape formed on the battery pack 22), it may be difficult to join the battery pack 22 and the flow path upper cover 12 of the cooling structure 1 without any gaps. In such a case, the gap filler 23 can be used. The gap filler 23 is generally a resin containing a pigment with high thermal conductivity. By inserting the gap filler 23 between different substances, the heat exchange efficiency can be improved. In this embodiment, it is preferable that the thermal conductivity of the gap filler 23 is 3.5 W / m or more. An example of the gap filler 23 is "SDP-3540-A" manufactured by Shin-Etsu Silicone Co., Ltd. The thickness of the gap filler is preferably 0.1 mm to 8.0 mm, and more preferably 0.5 mm to 3.0 mm.

[0087] The configuration of the battery pack 22 is not particularly limited. For example, the battery pack 22 may be substantially rectangular, and the cooling structure 1 may be disposed on its bottom surface, or the bottom surface may serve as the flow path upper cover 12 of the cooling structure 1. From the viewpoint of improving corrosion resistance, the steel plate constituting the battery pack 22 is preferably a Zn-based plated steel plate or an Al-based plated steel plate. However, when a structure in which the battery pack 22 and the cooling structure 1 are separated as shown in FIG. 8C is adopted, it is not essential that the portion of the battery pack 22 where the cooling structure 1 is attached, for example, the bottom surface, is resistant to corrosion by the coolant.

[0088] The thickness of the Zn-plated steel sheet constituting the bottom portion of the battery pack 22 is not particularly limited, but is preferably 0.2 to 1.2 mm or 0.3 to 1.2 mm, and more preferably 0.4 to 0.6 mm, for example. In this case, the bottom portion of the battery pack 22 can be formed thin while maintaining its strength. Therefore, the distance between the coolant and the internal structure of the battery pack 22 can be narrowed, and the cooling efficiency of the battery pack 22 can be improved, and the cooling responsiveness of the battery pack 22 can be improved.

[0089] (3. Manufacturing method of cooling structure) Next, a manufacturing method of the cooling structure according to the third embodiment of the present invention will be described. The manufacturing method of the cooling structure according to the third embodiment includes a step S1 of press-forming a plated steel sheet to obtain a press-formed member 11, and a step S2 of laser-welding the press-formed member and the flow path upper cover. Details of these steps will be described below. This manufacturing method can suitably manufacture the cooling structure according to the first embodiment. However, the following description does not limit the manufacturing method of the cooling structure according to the first embodiment.

[0090] (S1 Press molding) In the manufacturing method of the cooling structure according to the present embodiment, first, a plated steel sheet is press-formed. As a result, a press-formed member 11 having a groove portion 111 and a bank portion 112 provided around the groove portion 111 is obtained. The plated steel sheet to be press-formed has a Zn-based plating and an inorganic film or a resin film provided as a chemical conversion coating on the surface of the Zn-based plating. The inorganic film contains a Si-based component or a Zr-based component as a main component. The preferred form of the plated steel sheet is as described above. In addition, in the cooling structure 1 finally obtained, the flow path 14 has a parallel flow path portion 141 in which a plurality of partial flow paths 1411 extending along a first direction are arranged in a second direction perpendicular to the first direction, and in the parallel flow path portion 141, the interval D between adjacent partial flow paths 1411 is 20 mm or less. It is necessary to form the groove portion 111 in the press forming so that such a shape of the flow path 14 is achieved.

[0091] (S2 Laser Welding) Next, the flow path lid 12, which is a flat plate, is placed at a position covering the groove portion 111 of the press-formed member 11, and the flow path lid 12 and the bank portion 112 of the press-formed member 11 are laser-welded to each other. This results in a laser welded portion 13 that forms a flow path 14 through which a coolant can flow.

[0092] The laser welding conditions are not particularly limited, and suitable conditions can be appropriately adopted according to the thickness of the plated steel sheet, etc. However, in the laser welded portion 13 obtained by laser welding, the ratio of the length of the region where blowholes and pits are formed to the total length of the laser welded portion 13 facing the flow path 14 must be 0.2 or less. The occurrence of blowholes and pits may be suppressed by optimizing the laser welding conditions, or by providing an additional process before the laser welding. Examples of means for suppressing the occurrence of blowholes and pits are described below.

[0093] When Zn-based plated steel sheets are laser-welded, the vaporized Zn-based plating forms blowholes and pits. One of the means for generating blowholes and pits is to provide a gap between the plated steel sheets and release the vaporized Zn from the gap to the outside of the weld.

[0094] One example of a means for forming the gap is a spacer. For example, before laser welding, a spacer having a thickness of 0.03 mm or more may be disposed between the press-molded member 11 and the flow path upper cover 12 at the location where laser welding is performed or in the vicinity of the location where laser welding is performed. This allows the gap between the press-molded member 11 and the flow path upper cover 12 at the location where laser welding is performed or in the vicinity of the location where laser welding is performed to be 0.03 mm or more. The spacer is, for example, a metal foil. Also, as shown in FIG. 9A, the protrusions 15 formed by deforming the flow passage lid 12 or the press-formed member 11 may be used as spacers. In other words, the manufacturing method of the cooling structure 1 may further include a step of forming the protrusions 15 by deforming the flow passage lid 12 or the press-formed member 11. When the protrusions 15 are formed on the press-formed member, the protrusions 15 can be provided in a step of press-forming a plated steel sheet. As shown in FIG. 9A, when the flow passage lid 12 and the press-formed member 11 provided with the protrusions 15 are overlapped with each other, a gap is formed between the flow passage lid 12 and the press-formed member 11. In this state, the flow passage lid 12 and the press-formed member 11 are laser-welded to suppress the occurrence of blowholes and pits.

[0095] Another example of a means for forming a gap is spot welding shown in FIG. 9B. When a plated steel sheet is spot-welded, a gap may be generated at the welded portion. This gap can be used as a means for releasing the Zn-based plating vaporized during laser welding. Therefore, for example, the press-molded member 11 and the flow path upper cover 12 may be spot-welded at the location where the laser welding is performed or in the vicinity of the location where the laser welding is performed before the laser welding. By using the spot welded portion 16, the gap between the press-molded member 11 and the flow path upper cover 12 at the location where the laser welding is performed or in the vicinity of the location where the laser welding is performed can be set to 0.03 mm or more. In addition, by inserting a metal foil into the location to be spot-welded before the spot welding, the size of the gap can be adjusted more easily.

[0096] In addition, the occurrence of blowholes and pits can also be suppressed by removing the Zn-based plating from the welding target portion before laser welding. For example, the Zn-based plating at the portion to be laser welded may be removed in advance before the base steel sheet of the plated steel sheet is melted and solidified by laser welding. For example, the welding target portion may be heated using a laser to a temperature range from the melting point of the Zn-based plating to the melting point of the base steel sheet. In addition, the Zn-based plating may be mechanically removed from the welding target portion of the plated steel sheet by means of grinding or the like before laser welding. EXAMPLES

[0097] The effects of one embodiment of the present invention will be explained more specifically with reference to an example. However, the conditions in the example are merely an example of conditions adopted to confirm the feasibility and effects of the present invention. The present invention is not limited to this example of conditions. Various conditions may be adopted in the present invention as long as they do not deviate from the gist of the present invention and the object of the present invention is achieved.

[0098] (Example 1: Relationship between the distance between flow passages, the feasibility of assembly, and the performance of the cooling structure) A press-formed member was created by press-forming a Zn-based plated steel sheet. This press-formed member was laser-welded to a flow path top cover made of a flat sheet of Zn-based plated steel sheet to manufacture the cooling structure. The flow path widths and flow path intervals of the multiple partial flow paths extending in parallel are shown in Table 1. Note that the manufacturing conditions not included in Table 1 were as follows. No flow path communication parts connecting the partial flow paths were created. The gaps between the plated steel sheets were formed by sandwiching a jig between the plated steel sheets. Type of plated steel sheet: Zn-based plated mild steel sheet with a thickness of 0.5 mm Laser welding machine: Fiber laser welding machine -Heat input condition for laser welding: 45000J / m Shape of the cooling structure of the embodiment: See Figure 10 Partial flow path length: 200mm Partial channel height: 10mm Gap between plated steel sheets: 0.1mm

[0099] Fig. 10 is a schematic diagram of a portion of the manufactured cooling structure. For convenience, only two partial flow paths are shown in Fig. 10, but in reality, the cooling structure was provided with a number of partial flow paths sufficient to cover a battery with a width of 120 mm. In all of the examples shown in Table 1, the cooling structure was able to be assembled by laser welding.

[0100] The evaluation results of the cooling structures created as described above are also shown in Table 1. The evaluation criteria were as follows: Regarding the flow path width W of the partial flow path, those of 20 mm or less were ranked "S", those between 20 mm and 30 mm were ranked "A", and those over 30 mm were ranked "B". This is because the smaller the flow path width W, the more stable the flow of the coolant can be, and the more the cooling efficiency can be improved. "D / 2" is the value obtained by dividing the distance D between multiple partial flow paths by 2. This value is the maximum distance along the flow path width direction at the points where partial flow paths are not in direct contact with each other, and the smaller the value, the better. If D / 2 is too large, the points not in contact with the flow paths will not be cooled sufficiently, and there is a risk that the cooling structure will not function sufficiently. D / 2 of 7.5 mm or less was ranked "A," that of more than 7.5 mm and less than 10 mm was ranked "B," and that of more than 10 mm was ranked "C." Samples rated as rank A or rank B were judged to have sufficiently narrow flow path intervals.

[0101] [Table 1]

[0102] All the examples shown in Table 1 could be manufactured by laser welding. Therefore, it is clear that with laser welding, it is possible to manufacture partial flow channels that can exhibit high cooling capacity, even in the case of the narrowest partial flow channel width of 10 mm among the fabricated partial flow channels.

[0103] (Example 2: Liquid-tightness evaluation) The flow passages were prepared using Zn-based plated mild steel sheets with a thickness of 0.5 mm. The shapes of the press-formed members and the upper cover of the flow passage before welding were basically as shown in Fig. 11A and Fig. 11B, and the shape of the flow passage was as shown in Fig. 11C. For the examples in which "corrugated sheet shape" is written in the remarks column, the cross-sectional shape of the partial flow passage was made to be the corrugated shape shown in Fig. 3, but other shapes were adopted similar to those of the other examples. In all examples, the flow passage shape in plan view was U-shaped, and two flow passages extending in the vertical direction corresponded to the partial flow passages. The flow passage interval and the size of the gap between the plated steel sheets were as described in Table 2. The means for providing the gap are described in the "Remarks" column of Table 2. The flow passage width was 20 mm in all examples.

[0104] Then, the blowhole / pit rate was measured in the cooling structure manufactured by the above-mentioned procedure. The length of each blowhole in the weld line direction was measured by observing the laser welded part with an X-ray. The length of each pit in the weld line direction was also measured visually. The sum of the measured lengths of the blowholes and pits in the weld line direction was divided by the total length of the laser welded part facing the flow path to determine the ratio of the length of the area where the blowholes and pits were formed to the total length of the laser welded part facing the flow path (blowhole / pit rate).

[0105] Furthermore, the liquid-tightness of the cooling structure manufactured by the above-mentioned procedure was evaluated. LLC (long-life coolant liquid), a cooling liquid, was circulated inside the flow passage of the cooling structure. The output during LLC circulation was adjusted so that the pressure inside the flow passage was 1.5 atmospheres. This circulation test confirmed the presence or absence of water leakage from the welded joints. The results are shown in Table 2.

[0106] [Table 2]

[0107] When welding was performed without taking any measures to prevent welding defects, such as leaving gaps between the steel plates, a large number of pits and blowholes occurred, resulting in water leakage. When the jig was adjusted so that the gap between the steel sheets was 0.05 mm and 0.1 mm, the occurrence of blowholes and pits was greatly suppressed, and no water leakage occurred. When the gap between the steel sheets was adjusted to 0.1 mm when overlapping, due to sheet separation when resistance spot welding was performed near the corners of the flow path, or due to formed protrusions, the occurrence of blowholes and pits could be prevented, and no water leakage occurred. Although not shown in Table 2, a cooling structure with protrusions that resulted in a gap between the steel sheets of 0.5 mm was also produced. In this cooling structure, blowholes and pits were prevented in the same way as in the flow paths with other gaps, and no burn-through occurred, so no water leakage occurred. As shown in Figure 3, when the press-formed part is made corrugated, the occurrence of blowholes and pits is suppressed even if the gap between the plated steel sheets is 0 mm. When the radius of curvature R of the bank part at the contact part between the flow path top cover and the bank part is 12 mm, the occurrence of blowholes and pits is prevented and no water leakage occurs. When the radius R is 30 mm, a small number of blowholes and pits occur, but no water leakage occurs. When a corrugated press-formed part is used, the flow path spacing is the same as the bead width, making it possible to narrow the flow path spacing and manufacture flow paths with high cooling capacity.

[0108] As explained above, the cooling structures in which the ratio of the length of the region in which blowholes and pits were formed to the total length of the laser welds facing the flow path was 0.2 or less had excellent liquid-tightness of the flow path. In addition, since the flow path spacing was narrow in all examples, when these are used to cool battery cells, etc., they can exhibit high cooling efficiency. Furthermore, since all examples were manufactured from Zn-based plated steel sheets, they have high coolant corrosion resistance and outer surface corrosion resistance. [Explanation of symbols]

[0109] 1 Cooling structure 11 Press-molded parts 111 Groove 112 Embankment 12 Flow channel cover 13 Laser welding 13A Flow passage outer edge weld 131 Starting end 132 Termination 133 Middle Section 14 Flow Path 141 Parallel flow path section 1411 Partial channel 142 Flow passage connection part 143 Coolant inlet 144 Coolant outlet 15 Protrusions 16 Spot welds 2 Battery Unit 21 Battery Cell 22 Battery Pack 23 Gap Filler R: Circle showing the radius of curvature of the bank P Pit B Blowhole T-tab plate L Laser D Channel Spacing W Width of the flow path

Claims

1. A press-formed member having a groove portion and a bank portion provided around the groove portion; A flow path upper cover which is a flat plate overlapped in a position covering the groove portion of the press-molded member and constitutes a flat cooling surface; a laser welded portion that joins opposing surfaces of the flow path cover and the bank portion to form a flow path through which a coolant can flow; Equipped with The press-formed member and the flow path upper cover are plated steel sheets having a base steel sheet, a Zn-based plating provided on a surface of the base steel sheet, and an inorganic coating or a resin coating provided as a chemical conversion coating on the surface of the Zn-based plating, The inorganic coating contains a Si-based component or a Zr-based component in a ratio of 50% by mass or more, the flow path has a parallel flow path portion in which a plurality of partial flow paths extending along a first direction are arranged in a second direction perpendicular to the first direction, In a part or all of the parallel flow path portion, the interval between adjacent partial flow paths is 20 mm or less, The ratio of the length of the region where blowholes and pits are formed to the total length of the laser weld facing the flow path is 0.2 or less. Cooling structure.

2. 2. The cooling structure according to claim 1, wherein in the parallel flow path portion, a distance between adjacent partial flow paths is 0.8 to 15 mm.

3. 3. The cooling structure according to claim 1, wherein the partial flow passage has a width of 6 to 60 mm.

4. 3. The cooling structure according to claim 1, wherein the partial flow passage has a width of 6 to 20 mm.

5. The cooling structure according to any one of claims 1 to 4, characterized in that a gap between the press-formed member and the flow path upper cover around the weld metal of the laser weld is 0.03 mm or more.

6. The cooling structure according to claim 5, further comprising a spacer having a thickness of 0.03 mm or more arranged between the press-formed member and the flow path upper cover in the periphery of the weld metal of the laser welded portion.

7. 7. The cooling structure according to claim 6, wherein the spacer is a protrusion formed by deforming the flow passage upper cover or the press-formed member.

8. 6. The cooling structure according to claim 5, further comprising a spot weld at or near the laser weld for joining the flow passage upper cover and the press-formed member.

9. The cross-sectional shape of the bank portion is a substantially circular arc, 9. The cooling structure according to claim 1, wherein a radius of curvature of the bank portion at a contact portion between the flow path upper cover and the bank portion is 15 mm or less.

10. The cooling structure according to any one of claims 1 to 9, characterized in that the plated steel sheet constituting the press-formed member and the flow path upper cover has a thickness of 0.3 to 1.2 mm.

11. The laser welds include flow passage outer edge welds surrounding all of the flow passages, The start and end of the laser weld are excluded from the flow passage outer edge weld. The cooling structure according to any one of claims 1 to 10.

12. The cooling structure according to any one of claims 1 to 11, characterized in that a start end and a end end of the laser weld are excluded from the cooling structure.

13. 13. The cooling structure according to claim 1, wherein a bead height of the laser welded portion in the flow passage upper cover is 0.3 mm or less.

14. A battery cell; a battery pack containing the battery cells; The cooling structure according to any one of claims 1 to 13. Equipped with A battery unit in which the flow path upper cover of the cooling structure is joined to the battery pack.

15. A battery cell; a battery pack containing the battery cells; The cooling structure according to any one of claims 1 to 13. Equipped with The battery unit, wherein the flow path upper cover of the cooling structure is the battery pack.

16. A step of press-forming a steel plate to obtain a press-formed member having a groove portion and a bank portion provided around the groove portion; a step of overlapping a flat flow path lid at a position covering the groove portion of the press-formed member, and laser welding the flow path lid and the bank portion of the press-formed member to obtain a laser welded portion that forms a flow path through which a coolant can flow; Equipped with The press-formed member and the flow path upper cover are plated steel sheets having a base steel sheet, a Zn-based plating provided on a surface of the base steel sheet, and an inorganic coating or a resin coating provided as a chemical conversion coating on the surface of the Zn-based plating, The inorganic coating contains a Si-based component or a Zr-based component in a ratio of 50% by mass or more, the flow path has a parallel flow path portion in which a plurality of partial flow paths extending along a first direction are arranged in a second direction perpendicular to the first direction, In a part or all of the parallel flow path portion, the interval between adjacent partial flow paths is 20 mm or less, The ratio of the length of the region where blowholes and pits are formed to the total length of the laser weld facing the flow path is 0.2 or less. A method for manufacturing a cooling structure.

17. Prior to the laser welding, a spacer having a thickness of 0.03 mm or more is disposed between the press-formed member and the upper lid of the flow passage at a location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed, thereby making the gap between the press-formed member and the upper lid of the flow passage at the location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed 0.03 mm or more. The method for manufacturing a cooling structure according to claim 16 .

18. The method for manufacturing a cooling structure according to claim 17, wherein the spacer is a protrusion formed by deforming the flow passage upper cover or the press-formed member.

19. Prior to the laser welding, the press-formed member and the flow passage upper lid are spot-welded at the location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed, thereby making the gap between the press-formed member and the flow passage upper lid at the location where the laser welding is to be performed or in the vicinity of the location where the laser welding is to be performed 0.03 mm or more. The method for manufacturing a cooling structure according to claim 16 .

Citation Information

Patent Citations

  • Separator

    JP1986025624A

  • Laser lap welding structure of plating steel plate

    JP2001276990A

  • Heat exchanger with deep-drawn heat exchanger plates

    JP2009522535A

  • Cooler

    JP2012017954A

  • Battery cooling plate and cooling device

    JP2013101926A