Ceramic electronic components and their manufacturing method

The ceramic electronic component addresses stress-induced cracks by optimizing curvature and distances between layers, maintaining reliability and uniform plating, thus enhancing structural integrity and performance.

JP7569131B2Active Publication Date: 2024-10-17TAIYO YUDEN KK
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021016082
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-02-03
Publication Date
2024-10-17
Estimated Expiration
2041-02-03

AI Technical Summary

Technical Problem

The stress due to the difference in thermal expansion coefficient between the external electrode and the ceramic portion in ceramic electronic components tends to concentrate at the corners, leading to potential cracks and reduced reliability.

Method used

A ceramic electronic component with a laminated structure featuring internal electrode layers and dielectric layers, covered by ceramic-based cover layers, where the radius of curvature (R1) and distances (C1, P1) are optimized to suppress cracks while maintaining reliability, with specific ratios (0.20≦R1/√(P1² - C1²)≦0.80, ensuring uniform plating and adequate electrode thickness.

Benefits of technology

The solution effectively suppresses cracks and maintains reliability by optimizing the curvature and distances, ensuring uniform plating and preventing reliability issues due to stress concentration.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569131000002
    Figure 0007569131000002
  • Figure 0007569131000003
    Figure 0007569131000003
  • Figure 0007569131000004
    Figure 0007569131000004
Patent Text Reader

Abstract

To suppress a crack while maintaining reliability.SOLUTION: In a case where a direction in which a first end surface and a second end surface of a lamination chip are opposite is an X-axis, a lamination direction is a Z-axis, a direction orthogonal to the X-axis and the Z-axis is a Y-axis, a curvature radius R1 is a curvature radius of a corner part on a first external part electrode side of a first cover layer in a cross section of a XZ plane passing through a center of the Y-axis of the lamination chip, a straight line obtained by connecting ends on the first external part electrode side of internal electrode layers which are not connected to the first external part electrode is a straight line L, an intersection point of the straight line L and the internal electrode layer nearest to the first cover layer is an intersection point N1, a straight line M is a straight line drawn in an X-axis direction so as to be in contact with an upper surface of the lamination chip, a straight line N is a straight line drawn in a Z-axis direction so as to be in contact with the first end surface, an intersection point of the straight line M and the straight line N is an intersection point O, a distance between the intersection point N1 and the straight line M is C1, and a distance between the intersection point N1 and the intersection point O is P1, a relationship of 0.20≤R1 / √(P12-C12)≤0.80 is established.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceramic electronic component and a method for manufacturing the same. [Background technology]

[0002] Ceramic electronic components such as multilayer ceramic capacitors include a multilayer chip that is constructed by alternately stacking multiple dielectric layers, the main component of which is ceramic, and multiple internal electrode layers. The internal electrode layers are extended to the end faces of the multilayer chip, and external electrodes are formed to cover the surfaces (see, for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-102766 A [Patent Document 2] JP 2001-210545 A [Patent Document 3] JP 2006-310700 A Summary of the Invention [Problem to be solved by the invention]

[0004] At the corners of the laminated chip, stress caused by the difference in thermal expansion coefficient between the external electrodes and the ceramic part tends to concentrate. This may cause cracks to form at the corners of the laminated chip. If an attempt is made to relieve this stress, it may result in a decrease in reliability.

[0005] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a ceramic electronic component that can suppress cracks while maintaining reliability, and a manufacturing method thereof. [Means for solving the problem]

[0006] A ceramic electronic component according to the present invention is a laminated chip having a substantially rectangular parallelepiped shape, the laminated chip including a first cover layer mainly made of ceramic provided on an upper surface of an end of the laminated structure in a lamination direction, and a second cover layer mainly made of ceramic provided on a lower surface of the end of the laminated structure in a lamination direction, the laminated chip being formed so that the laminated multiple internal electrode layers are alternately exposed on a first end face and a second end face that face each other, a first external electrode formed on the first end face and a second external electrode formed on the second end face, the direction in which the first end face and the second end face face each other is defined as an X-axis, the laminated direction is defined as a Z-axis, and a direction perpendicular to the X-axis and the Z-axis is defined as a Y-axis, In a cross section of an XZ plane passing through the center of the Y axis of the chip, a radius of curvature R1 is defined as a radius of curvature of the same size as the shape of a corner of the first cover layer on the side of the first external electrode, a straight line obtained by connecting the ends of each internal electrode layer on the side of the first external electrode that is not connected to the first external electrode is defined as a straight line L, an intersection point of the line L and the internal electrode layer closest to the first cover layer is defined as an intersection point N1, a straight line M is defined as a straight line drawn in the X-axis direction so as to be tangent to the top surface of the laminated chip, a straight line N is defined as a straight line drawn in the Z-axis direction so as to be tangent to the first end surface, an intersection point of the lines M and N is defined as an intersection point O, the shortest distance between the intersection point N1 and the line M is defined as a distance C1, and the shortest distance between the intersection point N1 and the intersection point O is defined as a distance P1. 2 -C1 2 )≦0.80.

[0007] In the ceramic electronic component, a surface of the first external electrode may not have an inflection point, and the surface of the first external electrode may include a plating layer.

[0008] In the ceramic electronic component, the radius of curvature R1 may be 1% or more and 15% or less of the dimension of the laminated chip in the longitudinal direction.

[0009] In the ceramic electronic component, the distance C1 may be 3% or more and 35% or less of the dimension of the laminated chip in the height direction.

[0010] In the ceramic electronic component, the distance P1 may be 10% or more and 45% or less of the dimension of the laminated chip in the height direction.

[0011] A method for producing a ceramic electronic component according to the present invention includes the steps of: laminating a plurality of pattern forming sheets obtained by printing a conductive paste for forming internal electrodes on ceramic-containing dielectric green sheets, laminating a ceramic-containing first cover sheet on an upper surface of an end in the lamination direction, laminating a ceramic-containing second cover sheet on a lower surface of the end in the lamination direction, and exposing the laminated plurality of conductive pastes for forming internal electrodes alternately on a first end face and a second end face that face each other, thereby forming a ceramic laminate having a substantially rectangular parallelepiped shape; polishing corners of the ceramic laminate; applying a conductive paste for forming a first external electrode to the first end face and a conductive paste for forming a second external electrode to the second end face; and firing the ceramic laminate, the conductive paste for forming the first external electrode, and the conductive paste for forming the second external electrode, thereby forming a ceramic electronic component having a substantially rectangular parallelepiped shape, the dielectric green sheets as dielectric layers, the conductive paste for forming internal electrodes as internal electrode layers, the first cover sheet as a first cover layer, the second cover sheet as a second cover layer, and the first external a step of forming the conductive paste for forming an electrode as a first external electrode and forming the conductive paste for forming the second external electrode as a second external electrode, wherein a direction in which the first end face and the second end face face each other is opposed to each other is defined as an X-axis, the lamination direction is defined as a Z-axis, and a direction perpendicular to the X-axis and the Z-axis is defined as a Y-axis, and a radius of curvature R1 is defined as a radius of curvature of a shape of a corner of the first cover layer on the side of the first external electrode in a cross section of an XZ plane passing through a center of the Y-axis of a laminated chip obtained by firing the ceramic laminate, a line L connecting the ends of each internal electrode layer on the first external electrode side that is not connected to the first cover layer, an intersection point N1 between the line L and the internal electrode layer closest to the first cover layer, a line M drawn in the X-axis direction so as to be tangent to the top surface of the laminated chip, a line N drawn in the Z-axis direction so as to be tangent to the first end surface, an intersection point O between the line M and the line N, a distance C1 being the shortest distance between the intersection N1 and the line M, and a distance P1 being the shortest distance between the intersection N1 and the intersection O, 2 -C1 2 The corners of the ceramic laminate are polished so as to satisfy the relationship: Effect of the Invention

[0012] According to the present invention, it is possible to provide a ceramic electronic component that can suppress cracks while maintaining reliability, and a method for manufacturing the same. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a partial cross-sectional perspective view of a multilayer ceramic capacitor. [Diagram 2] 2 is a cross-sectional view taken along line AA in FIG. 1. [Diagram 3] FIG. 4A is a diagram illustrating an example of the radius of curvature, and FIG. 4B is a diagram illustrating an example of the position of the cross section. [Figure 4] 13(a) and (b) are diagrams illustrating the radius of curvature. [Diagram 5] 4 is a diagram for explaining the positions and distances of each part of the multilayer ceramic capacitor. FIG. [Figure 6] 1 is a diagram illustrating a straight line L. [Figure 7] 11 is a diagram illustrating an example of an inflection point (step) of an external electrode. [Figure 8] FIG. 2 is a diagram illustrating a plating layer. [Figure 9] 1A to 1C are diagrams illustrating a flow of a method for manufacturing a multilayer ceramic capacitor. [Figure 10] 1(a) and (b) are diagrams illustrating the lamination process. [Figure 11] FIG. 1 is a diagram illustrating a lamination process. [Figure 12] FIG. 1 is a diagram illustrating a lamination process. [Figure 13] FIG. 1 is a diagram in which the results of Examples and Comparative Examples are plotted. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment will be described with reference to the drawings.

[0015] (First embodiment) Fig. 1 is a partial cross-sectional perspective view of a multilayer ceramic capacitor 100 according to an embodiment. As illustrated in Fig. 1, the multilayer ceramic capacitor 100 includes a laminated chip 10 having a substantially rectangular parallelepiped shape, and external electrodes 20a, 20b provided on two opposing end faces of the laminated chip 10. Of the four faces of the laminated chip 10 other than the two end faces, the two faces other than the top and bottom faces in the stacking direction are referred to as side faces. The external electrodes 20a, 20b extend on the top, bottom and two side faces in the stacking direction of the laminated chip 10. However, the external electrode 20a (first external electrode) and the external electrode 20b (second external electrode) are spaced apart from each other.

[0016] 1, the X-axis direction is the length direction of the laminated chip 10, the direction in which the two end faces of the laminated chip 10 face each other, and the direction in which the external electrodes 20a and 20b face each other. The Y-axis direction (second direction) is the width direction of the internal electrode layers, and the direction in which the two side faces of the laminated chip 10 face each other. The Z-axis direction is the stacking direction, and the direction in which the upper and lower faces of the laminated chip 10 face each other. The X-axis direction, the Y-axis direction, and the Z-axis direction are perpendicular to each other.

[0017] The laminated chip 10 has a configuration in which dielectric layers 11 containing a ceramic material functioning as a dielectric and internal electrode layers containing a base metal material are alternately laminated. The edges of the internal electrode layers are alternately exposed to a first end face on which the external electrode 20a of the laminated chip 10 is provided and a second end face on which the external electrode 20b is provided. As a result, the internal electrode layers are alternately conductive to the external electrodes 20a and 20b. As a result, the laminated ceramic capacitor 100 has a configuration in which a plurality of dielectric layers 11 are laminated via internal electrode layers. In the laminated structure of the dielectric layers 11 and the internal electrode layers, the internal electrode layers are arranged on the outermost layers in the lamination direction, and the upper surface of the end of the laminate in the lamination direction is covered by a cover layer 13 (first cover layer). The lower surface of the end of the laminate in the lamination direction is covered by a cover layer 13 (second cover layer). The cover layer 13 is mainly composed of a ceramic material. For example, the material of the cover layer 13 has the same main component ceramic material as that of the dielectric layers 11.

[0018] The size of the multilayer ceramic capacitor 100 is, for example, 0.25 mm in length, 0.125 mm in width, and 0.125 mm in height, or 0.4 mm in length, 0.2 mm in width, and 0.2 mm in height, or 0.6 mm in length, 0.3 mm in width, and 0.3 mm in height, or 1.0 mm in length, 0.5 mm in width, and 0.5 mm in height, or 1.6 mm in length, 0.8 mm in width, and 0.8 mm in height, or 2.0 mm in length, 1.25 mm in width, and 1.25 mm in height, or 3.2 mm in length, 1.6 mm in width, and 1.6 mm in height, or 4.5 mm in length, 3.2 mm in width, and 2.5 mm in height, but is not limited to these sizes.

[0019] The internal electrode layers 12 are mainly composed of base metals such as Ni (nickel), Cu (copper), and Sn (tin). Noble metals such as Pt (platinum), Pd (palladium), Ag (silver), and Au (gold), or alloys containing these metals, may also be used as the internal electrode layers 12. The average thickness of the internal electrode layers 12 is, for example, 1 μm or less. The dielectric layers 11 are mainly composed of a ceramic material having a perovskite structure represented by the general formula ABO3. The perovskite structure is an ABO that deviates from the stoichiometric composition. 3-α For example, the ceramic material includes BaTiO3 (barium titanate), CaZrO3 (calcium zirconate), CaTiO3 (calcium titanate), SrTiO3 (strontium titanate), BaTiO3 (barium titanate) which forms a perovskite structure, 1-x-y Ca x Sr y Ti 1-z Zr z O3 (0≦x≦1, 0≦y≦1, 0≦z≦1) can be used. The average thickness of the dielectric layer 11 is, for example, 1 μm or less. The number of layers of the internal electrode layer is, for example, 100 to 800.

[0020] Fig. 2 is a cross-sectional view taken along line AA in Fig. 1. Hatching is omitted in Fig. 2. A difference in thermal expansion coefficient occurs between the external electrodes 20a, 20b and the ceramic parts with which the external electrodes 20a, 20b are in contact. As illustrated in Fig. 2, the external electrodes 20a, 20b contract in the direction of the large arrow at the corners (also referred to as edges) B. In this case, stress is concentrated in the direction of the small arrow at the corners B of the cover layer 13. This stress may cause cracks as illustrated by dotted lines in Fig. 2. If cracks occur, there is a concern that the multilayer ceramic capacitor 100 may have a poor appearance or a deteriorated reliability.

[0021] Therefore, it is conceivable to suppress the occurrence of cracks by alleviating the stress on the corner B. For example, it is conceivable to form the external electrode at the corner B to be thin. However, in this case, there is a risk that the reliability of the multilayer ceramic capacitor 100 will decrease, for example, due to a decrease in moisture resistance and a decrease in insulation properties.

[0022] Therefore, the multilayer ceramic capacitor 100 in accordance with this embodiment has a configuration that can suppress cracks while maintaining reliability.

[0023] In this embodiment, the corner portion refers to a region having a curvature at the corner of the laminated chip 10 (corner of the cover layer 13). As illustrated in FIG. 3(a), the radius of curvature R1 is defined as the same size as the shape of the corner portion of the cross section obtained by placing one of the two side surfaces of the laminated chip 10 on top and polishing it to the center by lateral filling. As illustrated in FIG. 3(b), the cross section is a cross section of the XZ plane (a dashed line portion) at the center in the Y-axis direction in the laminated chip 10. In FIG. 3(a), hatching is omitted. In addition, the corner portion B may not necessarily be a perfect circular arc as in FIG. 4(a) or FIG. 4(b). In this case, the average value of the length r1 in the X-axis direction of the corner portion B and the length r2 in the Z-axis direction, ie, (r1+r2) / 2, can be defined as the radius of curvature R1.

[0024] In this embodiment, attention is focused on the distance between the internal electrode layer 12 and the corner B, and the shape of the corner B is defined.

[0025] First, the positions and distances of each part of the multilayer ceramic capacitor 100 will be described with reference to Fig. 5. Fig. 5 is a cross-sectional view of the multilayer chip 10 near the external electrode 20a and near the top surface. The cross section of Fig. 5 is a cross section of the XZ plane at the center in the Y-axis direction, similar to the cross section of Fig. 3(b). Hatching is omitted in Fig. 5.

[0026] In the cross section of FIG. 5, the radius of curvature R1 is the same as the radius of curvature of the corners on the external electrode 20a side of the cover layer 13 on the upper surface side of the laminated chip 10. A straight line obtained by connecting the ends of the internal electrode layers 12 on the external electrode 20a side that are not connected to the external electrode 20a is defined as a straight line L. The intersection of the straight line L and the outermost internal electrode layer 12 on the upper surface side of the laminated chip 10 is defined as an intersection N1. In the cross section of FIG. 5, straight lines M and N are drawn along the outer shape of the laminated chip 10. The straight line M is a straight line drawn in the X-axis direction so as to be tangent to the upper surface of the laminated chip 10. The straight line N is a straight line drawn in the Z-axis direction so as to be tangent to the end face of the laminated chip 10 on the external electrode 20a side. The intersection of the straight lines M and N is defined as an intersection O. The shortest distance between the intersection N1 and the straight line M is defined as a distance C1. The shortest distance between the intersection N1 and the intersection O is defined as a distance P1.

[0027] When the ends of the internal electrode layers 12 not connected to the external electrode 20a on the external electrode 20a side coincide in the X-axis direction, the straight line L is parallel to the Z-axis direction. When the ends of the internal electrode layers 12 not connected to the external electrode 20a on the external electrode 20a side do not coincide in the X-axis direction, as illustrated in Fig. 6, the straight line L can be defined as a straight line that passes through the midpoint between the end position of the internal electrode layer 12 with the maximum distance from the unexposed end face and the end position of the internal electrode layer 12 with the minimum distance.

[0028] The intersection N1 corresponds to a corner of an internal electrode intersection (capacitive portion) where each internal electrode layer 12 connected to the external electrode 20a and each internal electrode layer 12 connected to the external electrode 20b intersect. The internal electrode intersection is a region where the density of the internal electrode layers mainly composed of metal is higher than other regions. Therefore, the difference in thermal expansion coefficient between the internal electrode intersection and the external electrode becomes relatively small. When the radius of curvature R1 becomes small, the distance between the corner B and the intersection N1 becomes long, and the distance between the external electrode 20a and the internal electrode intersection becomes long. In this case, cracks may occur at the corner due to stress caused by the difference in thermal expansion between the external electrode 20a and the ceramic portion where the external electrode 20a contacts during firing. On the other hand, when the radius of curvature R1 becomes large, the distance between the corner B and the intersection N1 becomes short. In this case, the difference in thermal expansion between the external electrode 20a and the ceramic portion where the external electrode 20a contacts during firing becomes small, and the occurrence of cracks is suppressed. On the other hand, if the distance between the corner B and the intersection N1 is shortened, the ceramic portion protecting the internal electrode intersection will be reduced, and the insulation will be deteriorated due to the decrease in moisture resistance, which may cause a reliability problem.

[0029] As a result of intensive research conducted by the present inventor, the relationship between the radius of curvature R1, the distance C1, and the distance P1 was optimized to satisfy 0.20≦R1 / √(P1 2 -C1 2 It was found that by making the ratio (R) equal to or less than 0.80, it is possible to suppress the occurrence of cracks while maintaining reliability.

[0030] In order to suppress crack generation by shortening the distance between the corner B and the intersection point N1, R1 / √(P1 2 -C1 2 ) is preferably 0.20 or more, and more preferably 0.25 or more. On the other hand, from the viewpoint of increasing the distance between the corner B and the intersection point N1 to improve reliability, R1 / √(P1 2 -C1 2 ) is preferably 0.80 or less, and more preferably 0.75 or less.

[0031] From the viewpoint of suppressing the occurrence of discontinuous portions in the external electrodes at the corners, the radius of curvature R1 is preferably 1% or more, more preferably 3% or more, and even more preferably 5% or more of the dimension in the longitudinal direction (X-axis direction in FIG. 1) of the laminated chip 10. From the viewpoint of preventing the chip from standing up when mounted on the substrate, the radius of curvature R1 is preferably 20% or less, more preferably 15% or less, and even more preferably 10% or less of the dimension in the longitudinal direction of the laminated chip 10.

[0032] If the distance C1 is too long, cracks may occur. Therefore, it is preferable to set an upper limit for the distance C1. For example, the distance C1 is preferably 35% or less of the dimension of the laminated chip 10 in the height direction (the Z-axis direction in FIG. 1), more preferably 30% or less, and even more preferably 25% or less.

[0033] On the other hand, if the distance C1 is too short, there is a risk of insufficient reliability. Therefore, it is preferable to set a lower limit for the distance C1. For example, the distance C1 is preferably 3% or more of the dimension of the laminated chip 10 in the height direction, more preferably 5% or more, and even more preferably 10% or more.

[0034] If the distance P1 is too long, cracks may occur. Therefore, it is preferable to set an upper limit for the distance P1. For example, the distance P1 is preferably 45% or less of the height dimension of the laminated chip 10, more preferably 40% or less, and even more preferably 35% or less.

[0035] On the other hand, if the distance P1 is too short, there is a risk of insufficient reliability. Therefore, it is preferable to set a lower limit for the distance P1. For example, the distance P1 is preferably 10% or more of the dimension of the laminated chip 10 in the height direction, more preferably 15% or more, and even more preferably 20% or more.

[0036] According to the configuration of this embodiment, it is not necessary to thin the external electrode 20a at the corners, so that the plating layer can be formed uniformly on the external electrode 20a. In particular, by not providing a step (inflection point) as illustrated in Fig. 7 on the external electrode, the plating layer can be formed uniformly.

[0037] For example, at the corner B of the laminated chip 10, the minimum thickness of the external electrode 20a is preferably 1 μm or more, more preferably 2 μm or more, and even more preferably 3 μm or more. However, if the external electrode 20a is too thick overall, the laminated chip 10 will become large, so the local maximum thickness of the external electrode 20a is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 5 μm or less.

[0038] In the laminated chip 10, the number of layers of the internal electrode layers 12 relative to the height dimension of the laminated chip 10 is, for example, 500 layers / mm to 1500 layers / mm, or 800 layers / mm to 1000 layers / mm. The thickness of the internal electrode layers 12 is 0.1 μm to 0.5 μm. The thickness of the dielectric layer 11 is 0.1 μm to 0.5 μm.

[0039] 5, the cross section near the external electrode 20a and near the top surface of the laminated chip 10 is focused on, but is not limited thereto. When focusing on a cross section near the external electrode 20a and near the bottom surface of the laminated chip 10, in the same cross section as in FIG. 5, the radius of curvature R1 is the same as the radius of curvature of the shape of the corner of the cover layer 13 on the bottom surface side of the laminated chip 10 on the side of the external electrode 20a. The intersection point N1 is the intersection point between the straight line L and the outermost internal electrode layer 12 on the bottom surface side of the laminated chip 10. The straight line M is a straight line drawn in the X-axis direction so as to be tangent to the bottom surface of the laminated chip 10.

[0040] When focusing on a cross section near the external electrode 20b and near the top surface, in the same cross section as in Fig. 5, the radius of curvature R1 is the same as the radius of curvature of the shape of the corner of the cover layer 13 on the top surface side of the laminated chip 10 on the external electrode 20b side. A straight line L is a straight line obtained by connecting the ends of the internal electrode layers 12 on the external electrode 20b side that are not connected to the external electrode 20b. An intersection point N1 is an intersection point between the straight line L and the outermost internal electrode layer 12 on the top surface side of the laminated chip 10. The straight line N is a straight line drawn in the Z-axis direction so as to be tangent to the end face of the laminated chip 10 on the external electrode 20b side.

[0041] When focusing on a cross section near the external electrode 20b and near the bottom surface of the laminated chip 10, in the same cross section as in FIG. 5, the radius of curvature R1 is the same as the radius of curvature of the shape of the corner of the cover layer 13 on the bottom surface side of the laminated chip 10 on the side of the external electrode 20b. A straight line L is a straight line obtained by connecting the ends of each internal electrode layer 12 on the external electrode 20b side that are not connected to the external electrode 20b. An intersection point N1 is an intersection point between the straight line L and the outermost internal electrode layer 12 on the bottom surface side of the laminated chip 10. A straight line M is a straight line drawn in the X-axis direction so as to be tangent to the bottom surface of the laminated chip 10.

[0042] As illustrated in FIG. 8, a plating layer 21 may be provided on the surface of the external electrode 20a. Hatching is omitted in FIG. 8. The plating layer 21 is mainly composed of a metal such as Cu, Ni, Al, Zn, Sn, or an alloy of two or more of these metals. The plating layer 21 may be a plating layer of a single metal component, or may be a plurality of plating layers of different metal components. For example, the plating layer 21 has a structure in which a first plating layer 22, a second plating layer 23, and a third plating layer 24 are formed in this order from the external electrode 20a side. The first plating layer 22 is, for example, a Cu plating layer. The second plating layer 23 is, for example, a Ni plating layer. The third plating layer 24 is, for example, a Sn plating layer. Although FIG. 8 illustrates the external electrode 20a, the external electrode 20b also has a similar structure.

[0043] Next, a description will be given of a method for manufacturing the multilayer ceramic capacitor 100. FIG 9 is a diagram illustrating a flow of the method for manufacturing the multilayer ceramic capacitor 100.

[0044] (Raw powder production process) First, a dielectric material for forming the dielectric layer 11 is prepared. The dielectric material includes the main component ceramic of the dielectric layer 11. The A-site elements and B-site elements included in the dielectric layer 11 are usually included in the dielectric layer 11 in the form of a sintered body of ABO3 particles. For example, BaTiO3 is a tetragonal compound having a perovskite structure and exhibits a high dielectric constant. This BaTiO3 can generally be obtained by reacting a titanium raw material such as titanium dioxide with a barium raw material such as barium carbonate to synthesize barium titanate. Various methods have been known so far as a method for synthesizing the main component ceramic of the dielectric layer 11, such as a solid-phase method, a sol-gel method, a hydrothermal method, and the like. In this embodiment, any of these methods can be adopted.

[0045] To the obtained ceramic powder, a predetermined additive compound is added according to the purpose. Examples of the additive compound include oxides of Zr (zirconium), Ca (calcium), Sr (strontium), Mg (magnesium), Mn (manganese), V (vanadium), Cr (chromium), and rare earth elements, as well as oxides or glasses of Co (cobalt), Ni, Li (lithium), B (boron), Na (sodium), K (potassium), and Si (silicon).

[0046] (Lamination process) Next, a binder such as polyvinyl butyral (PVB) resin, an organic solvent such as ethanol or toluene, and a plasticizer are added to the dielectric material obtained in the raw powder preparation process and wet mixed. The obtained slurry is used to coat a dielectric green sheet 51 on a substrate by, for example, a die coater method or a doctor blade method, and then dried.

[0047] 10(a), a metal conductive paste for forming an internal electrode containing an organic binder is printed on the surface of the dielectric green sheet 51 by screen printing, gravure printing, or the like to arrange a first pattern 52 for an internal electrode layer. Ceramic particles are added to the metal conductive paste as a co-material. The main component of the ceramic particles is not particularly limited, but is preferably the same as the main component ceramic of the dielectric layer 11.

[0048] 10(a), a reverse pattern paste is printed on the dielectric green sheet 51 in the peripheral area where the first pattern 52 is not printed, thereby disposing the second pattern 53 and filling in the step with the first pattern 52. The reverse pattern paste may have the same components as the dielectric green sheet 51, or may have a different additive compound.

[0049] Thereafter, as illustrated in Figure 10(b), the dielectric green sheet 51, the first pattern 52 and the second pattern 53 are laminated so that the internal electrode layers 12 and the dielectric layers 11 are alternated and so that the edges of the internal electrode layers 12 are alternately exposed at both end faces in the longitudinal direction of the dielectric layer 11 and are alternately drawn out to a pair of external electrodes 20a, 20b having opposite polarities.

[0050] Next, as illustrated in FIG. 11, a predetermined number (e.g., 2 to 10 layers) of cover sheets 54 (first cover sheets) are laminated on the laminated dielectric green sheets 51, and a predetermined number (e.g., 2 to 10 layers) of cover sheets 54 (second cover sheets) are laminated under the laminated dielectric green sheets 51, thermocompression-bonded, and cut to a predetermined chip size (e.g., 1.0 mm×0.5 mm). The cover sheets 54 may have the same components as the dielectric green sheets 51, or may have different additive compounds. Thereafter, a metal conductive paste that will become the external electrodes 20a, 20b is applied to both sides of the cut laminate by a dipping method or the like and dried. This results in a ceramic laminate. Note that a predetermined number of cover sheets 54 may be laminated and compressed, and then attached to the top and bottom of the laminated dielectric green sheets 51.

[0051] On the dielectric green sheet 51, the second pattern 53 does not necessarily have to be formed as a reverse pattern.

[0052] The laminated portion of the second pattern 53 may be attached after lamination. Specifically, as illustrated in Fig. 12, the laminated portion is obtained by alternately laminating dielectric green sheets 51 and first patterns 52 having the same width as the dielectric green sheets 51. Next, a side margin sheet 55 is attached to the side surface of the laminated portion. The side margin sheet 55 may have the same components as the dielectric green sheets 51, or may have a different additive compound.

[0053] (Corner adjustment process) The ceramic laminate thus obtained is subjected to barrel polishing to round the corners of the ceramic laminate and form a radius of curvature. By adjusting the length of time for which the barrel polishing is performed, the desired radius of curvature R1 can be obtained.

[0054] (Firing process) The ceramic laminate after barrel polishing is subjected to binder removal treatment in an N2 atmosphere, and then a conductive paste for forming a first external electrode that will become the external electrode 20a is applied by a dipping method, and a conductive paste for forming a second external electrode that will become the external electrode 20b is applied by a dipping method. -5 ~10 -8 The laminated ceramic capacitor 100 is thus obtained, and is then fired in a reducing atmosphere of 1 atm at 1100 to 1300° C. for 10 minutes to 2 hours.

[0055] (Reoxidation treatment process) After that, a re-oxidation treatment may be performed at 600°C to 1000°C in an N2 gas atmosphere.

[0056] (Plating process) Thereafter, the external electrodes 20a, 20b may be coated with a metal such as Cu, Ni, Sn, etc. by plating.

[0057] In the above embodiments, a multilayer ceramic capacitor has been described as an example of a ceramic electronic component, but the present invention is not limited to this. For example, other electronic components such as a varistor or a thermistor may be used. EXAMPLES

[0058] Next, a multilayer ceramic capacitor according to the embodiment was fabricated, and its characteristics were examined.

[0059] (Examples 1 to 16 and Comparative Examples 1 to 16) A ceramic powder having reduction resistance and mainly composed of barium titanate was kneaded with an organic binder to form a slurry, which was then formed into a sheet shape using a doctor blade or the like to prepare a dielectric green sheet. A metal conductive paste mainly composed of Ni was applied to this dielectric green sheet in a predetermined pattern by screen printing to form an internal electrode pattern. The dielectric green sheets were laminated so that the internal electrode layers 12 and the dielectric layers 11 were alternately arranged, and the internal electrode layers 12 were alternately exposed at both end faces in the length direction of the dielectric layers 11 and alternately drawn out to a pair of external electrodes 20a, 20b having different polarities. Then, a predetermined number of cover sheets were laminated above and below the laminated dielectric green sheets, thermocompressed, and cut to a predetermined chip size. In this case, the number of laminated dielectric green sheets and the number of laminated cover sheets were adjusted so that the distance P1 and distance C1 after firing were the target values. Then, the barrel polishing time was adjusted so that the radius of curvature R1 after firing was the target value. After barrel polishing and binder removal, a conductive paste containing a co-material was applied to the exposed surface of the internal electrode to achieve the specified dimensions. The peripheral thickness was adjusted by diluting the conductive paste. After that, the product was fired in a nitrogen-hydrogen atmosphere at 1250°C and subjected to the specified heat treatment. After that, the external electrode was used as a base layer and a plating process was performed.

[0060] The shapes of Examples 1 to 4 and Comparative Examples 1 to 4 were 1005 shape (length 1.0 mm, width 0.5 mm, height 0.5 mm). The shapes of Examples 5 to 8 and Comparative Examples 5 to 8 were 1608 shape (length 1.6 mm, width 0.8 mm, height 0.8 mm). The shapes of Examples 9 to 12 and Comparative Examples 9 to 12 were 2012 shape (length 2.0 mm, width 1.25 mm, height 1.25 mm). Examples 13 to 16 and Comparative Examples 13 to 16 were 3216 shape (length 3.2 mm, width 1.6 mm, height 1.6 mm).

[0061] The distance C1, distance P1, and curvature radius R1 were measured for each of Examples 1 to 16 and Comparative Examples 1 to 16. Each sample was placed with one of the two sides facing up and polished to the center by lateral embedding to obtain a cross section. The distance C1, distance P1, and curvature radius R1 were averaged for 10 samples.

[0062] In Example 1, the distance C1 is 24.2 μm, the distance P1 is 55.1 μm, the radius of curvature R1 is 11.8 μm, and R1 / √(P1 2 -C1 2 In Example 2, the distance C1 was 25.0 μm, the distance P1 was 56.1 μm, the radius of curvature R1 was 37.8 μm, and R1 / √(P1 2 -C1 2 In Example 3, the distance C1 was 148.0 μm, the distance P1 was 211.0 μm, the radius of curvature R1 was 34.2 μm, and R1 / √(P1 2 -C1 2 In Example 4, the distance C1 was 149.2 μm, the distance P1 was 212.5 μm, the radius of curvature R1 was 114.2 μm, and R1 / √(P1 2 -C1 2 In Example 5, the distance C1 was 40.5 μm, the distance P1 was 108.0 μm, the radius of curvature R1 was 24.0 μm, and R1 / √(P1 2 -C1 2In Example 6, the distance C1 was 38.0 μm, the distance P1 was 105.9 μm, the radius of curvature R1 was 74.8 μm, and R1 / √(P1 2 -C1 2 In Example 7, the distance C1 was 247.2 μm, the distance P1 was 349.0 μm, the radius of curvature R1 was 57.2 μm, and R1 / √(P1 2 -C1 2 In Example 8, the distance C1 was 247.9 μm, the distance P1 was 349.7 μm, the radius of curvature R1 was 185.0 μm, and R1 / √(P1 2 -C1 2 ) was 0.75.

[0063] In Example 9, the distance C1 is 79.3 μm, the distance P1 is 260.2 μm, the radius of curvature R1 is 61.8 μm, and R1 / √(P1 2 -C1 2 In Example 10, the distance C1 was 79.9 μm, the distance P1 was 262.0 μm, the radius of curvature R1 was 190.0 μm, and R1 / √(P1 2 -C1 2 In Example 11, the distance C1 was 394.2 μm, the distance P1 was 553.7 μm, the radius of curvature R1 was 96.8 μm, and R1 / √(P1 2 -C1 2 In Example 12, the distance C1 was 398.5 μm, the distance P1 was 557.0 μm, the radius of curvature R1 was 305.1 μm, and R1 / √(P1 2 -C1 2 In Example 13, the distance C1 was 97.6 μm, the distance P1 was 313.0 μm, the radius of curvature R1 was 74.0 μm, and R1 / √(P1 2 -C1 2 In Example 14, the distance C1 was 98.0 μm, the distance P1 was 313.8 μm, the radius of curvature R1 was 234.3 μm, and R1 / √(P1 2 -C1 2In Example 15, the distance C1 was 488.5 μm, the distance P1 was 700.0 μm, the radius of curvature R1 was 124.8 μm, and R1 / √(P1 2 -C1 2 In Example 16, the distance C1 was 491.1 μm, the distance P1 was 705.4 μm, the radius of curvature R1 was 395.8 μm, and R1 / √(P1 2 -C1 2 ) was 0.78.

[0064] In Comparative Example 1, the distance C1 is 26.3 μm, the distance P1 is 56.8 μm, the radius of curvature R1 is 8.1 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 2, the distance C1 was 25.6 μm, the distance P1 was 56.4 μm, the radius of curvature R1 was 44.3 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 3, the distance C1 was 150.3 μm, the distance P1 was 213.4 μm, the radius of curvature R1 was 20.4 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 4, the distance C1 was 148.7 μm, the distance P1 was 211.3 μm, the radius of curvature R1 was 129.5 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 5, the distance C1 was 39.4 μm, the distance P1 was 106.5 μm, the radius of curvature R1 was 15.3 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 6, the distance C1 was 39.7 μm, the distance P1 was 107.5 μm, the radius of curvature R1 was 87.4 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 7, the distance C1 was 250.2 μm, the distance P1 was 350.1 μm, the radius of curvature R1 was 35.3 μm, and R1 / √(P1 2 -C1 2In Comparative Example 8, the distance C1 was 248.9 μm, the distance P1 was 349.8 μm, the radius of curvature R1 was 211.4 μm, and R1 / √(P1 2 -C1 2 ) was 0.86.

[0065] In Comparative Example 9, the distance C1 is 78.5 μm, the distance P1 is 259.0 μm, the radius of curvature R1 is 39.5 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 10, the distance C1 was 78.3 μm, the distance P1 was 258.1 μm, the radius of curvature R1 was 213.4 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 11, the distance C1 was 396.5 μm, the distance P1 was 555.5 μm, the radius of curvature R1 was 60.6 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 12, the distance C1 was 396.9 μm, the distance P1 was 556.6 μm, the radius of curvature R1 was 339.7 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 13, the distance C1 was 98.5 μm, the distance P1 was 313.4 μm, the radius of curvature R1 was 50.7 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 14, the distance C1 was 98.8 μm, the distance P1 was 314.4 μm, the radius of curvature R1 was 270.3 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 15, the distance C1 was 489.6 μm, the distance P1 was 702.4 μm, the radius of curvature R1 was 78.7 μm, and R1 / √(P1 2 -C1 2 In Comparative Example 16, the distance C1 was 489.2 μm, the distance P1 was 703.4 μm, the radius of curvature R1 was 464.4 μm, and R1 / √(P1 2 -C1 2 ) was 0.92.

[0066] (Crack determination) For each of Examples 1 to 16 and Comparative Examples 1 to 16, an investigation was conducted to determine whether or not cracks had occurred in 100 samples. The crack occurrence rate was measured by counting the number of samples in which cracks had occurred. The results are shown in Table 1. As shown in Table 1, the crack occurrence rate was 0 / 100 in all of Examples 1 to 16. On the other hand, in Comparative Examples 1, 3, 5, 7, 9, 11, 13, and 15, samples in which cracks had occurred were found. In other words, the crack occurrence rate was 1 / 100 or more. These results were plotted as shown in FIG. 13. From the plot results in FIG. 13, it was found that R1 / √(P1 2 -C1 2 It is believed that the crack occurrence rate was 0 / 100 because R1 / √(P1) was 0.20 or more. This is believed to be because the distance between corner B and intersection point N1 was shortened. On the other hand, R1 / √(P1 2 -C1 2 ) became less than 0.20, the crack occurrence rate became 1 / 100 or more. This is considered to be because the distance between the corner B and the intersection point N1 became longer.

[0067] (Reliability assessment) The reliability of 200 samples was examined for each of Examples 1 to 16 and Comparative Examples 1 to 16. Specifically, in a moisture-resistant chamber, a rated voltage was applied between the external electrodes and maintained for 1000 hours. If the IR value was less than a specified value, it was determined that the reliability was poor, and if the IR was equal to or greater than the specified value, it was determined that the reliability was not poor. The reliability failure rate was measured by counting the number of samples in which reliability failure occurred. The results are shown in Table 1. As shown in Table 1, the reliability failure rate was 0 / 200 in all of Examples 1 to 16. On the other hand, in Comparative Examples 2, 4, 6, 8, 10, 12, 14, and 16, samples in which reliability failure occurred were found. In other words, the reliability failure rate was 1 / 200 or more. These results were plotted as shown in FIG. 13. From the plot results in FIG. 13, it was found that R1 / √(P1 2 -C1 2It is believed that the reliability failure rate was 0 / 200 because R1 / √(P1) was 0.80 or less. This is believed to be because the distance between corner B and intersection point N1 was secured, improving moisture resistance. 2 -C1 2 ) exceeded 0.80, the reliability failure rate was thought to be 1 / 200 or more. This is thought to be because the distance between the corner B and the intersection point N1 was not sufficiently secured.

[0068] (Overall Judgment) If the crack defect rate was 0 / 100 and the reliability defect rate was 0 / 200, the overall judgment was good. If at least either the crack defect rate was 1 / 100 or more or the reliability defect rate was 1 / 200 or more, the overall judgment was bad. The results are shown in Table 1. As shown in Table 1, in Examples 1 to 16, the overall judgment was good. This is because 0.20≦R1 / √(P1 2 -C1 2 It is considered that this is because the relationship of 0.20≦R1 / √(P1)≦0.80 was satisfied. In Comparative Examples 1 to 16, the overall evaluation was judged to be poor. This is because the relationship of 0.20≦R1 / √(P1 2 -C1 2 )≦0.80 was not satisfied.

[0069] (Plating Determination) The plating properties were evaluated for Examples 1 to 16 and Comparative Examples 1 to 16. Observation was performed with an optical microscope at 100x magnification. If corner B was covered with the plating layer without any missing parts, the plating properties were evaluated as good, and if there was a missing, discontinuous part in the plating layer at corner B, the plating properties were evaluated as poor. The results are shown in Table 1. As shown in Table 1, the plating properties were evaluated as good in all of Examples 1 to 16 and Comparative Examples 1 to 16. This is thought to be because no inflection points (steps) or the like were provided in the external electrodes, and sufficient thickness was obtained for the external electrodes at the corners. [Table 1]

[0070] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]

[0071] 10 Stacked Chip 11 Dielectric layer 12 Internal electrode layer 13 Cover Layer 20a,20b external electrode 51 Dielectric green sheet 52 First Pattern 53 Second Pattern 54 Cover Sheet 55 Side margin sheet 100 Multilayer ceramic capacitors

Claims

1. a laminated chip comprising a laminated structure in which internal electrode layers and dielectric layers are alternately laminated, a first cover layer mainly composed of ceramic provided on an upper surface of an end of the laminated structure in a lamination direction, and a second cover layer mainly composed of ceramic provided on a lower surface of the end of the laminated structure in a lamination direction, the laminated chip having a substantially rectangular parallelepiped shape, the laminated internal electrode layers being alternately exposed on a first end face and a second end face facing each other; a first external electrode formed on the first end surface and a second external electrode formed on the second end surface, a direction in which the first end face and the second end face face each other is defined as an X-axis, a stacking direction is defined as a Z-axis, a direction perpendicular to the X-axis and the Z-axis is defined as a Y-axis, and in a cross section of the laminated chip in an XZ plane passing through the center of the Y-axis, a radius of curvature R1 is defined as a radius of curvature equal to the shape of a corner of the first cover layer on the side of the first external electrode, a straight line obtained by connecting the ends of each internal electrode layer not connected to the first external electrode on the side of the first external electrode is defined as a straight line L, an intersection point between the line L and the internal electrode layer closest to the first cover layer is defined as an intersection point N1, a straight line M is defined as a straight line drawn in the X-axis direction so as to be tangent to the top surface of the laminated chip, a straight line N is defined as a straight line drawn in the Z-axis direction so as to be tangent to the first end face, an intersection point between the line M and the line N is defined as an intersection point O, the shortest distance between the intersection point N1 and the line M is defined as a distance C1, and the shortest distance between the intersection point N1 and the intersection point O is defined as a distance P1. 2 -C1 2 )≦0.

80.

2. The surface of the first external electrode does not have an inflection point, The ceramic electronic component according to claim 1 , further comprising a plating layer provided on the surface of the first external electrode.

3. 3. The ceramic electronic component according to claim 1, wherein the radius of curvature R1 is 1% or more and 15% or less of a longitudinal dimension of the laminated chip.

4. 4. The ceramic electronic component according to claim 1, wherein the distance C1 is 3% or more and 35% or less of a dimension of the laminated chip in a height direction.

5. 5. The ceramic electronic component according to claim 1, wherein the distance P1 is 10% to 45% of the height dimension of the laminated chip.

6. a step of laminating a plurality of pattern forming sheets obtained by printing a conductive paste for forming internal electrodes on a ceramic-containing dielectric green sheet, laminating a first ceramic-containing cover sheet on an upper surface of an end in the lamination direction, laminating a second ceramic-containing cover sheet on a lower surface of the end in the lamination direction, and exposing the plurality of laminated conductive pastes for forming internal electrodes alternately on a first end surface and a second end surface facing each other, thereby forming a ceramic laminate having a substantially rectangular parallelepiped shape; polishing corners of the ceramic laminate; applying a conductive paste for forming a first external electrode to the first end surface and applying a conductive paste for forming a second external electrode to the second end surface; and firing the ceramic laminate, the conductive paste for forming the first external electrode, and the conductive paste for forming the second external electrode to form the dielectric green sheet as a dielectric layer, the conductive paste for forming the internal electrode as an internal electrode layer, the first cover sheet as a first cover layer, the second cover sheet as a second cover layer, the conductive paste for forming the first external electrode as a first external electrode, and the conductive paste for forming the second external electrode as a second external electrode, A direction in which the first end face and the second end face face each other is defined as an X-axis, a stacking direction is defined as a Z-axis, a direction perpendicular to the X-axis and the Z-axis is defined as a Y-axis, and in a cross section of an XZ plane passing through the center of the Y-axis of a laminated chip obtained by firing the ceramic laminate, a radius of curvature R1 is defined as a radius of curvature equal to the shape of a corner of the first cover layer on the first external electrode side, a straight line obtained by connecting the ends of each internal electrode layer not connected to the first external electrode on the first external electrode side is defined as a straight line L, an intersection point between the line L and the internal electrode layer closest to the first cover layer is defined as an intersection point N1, a straight line M is defined as a straight line drawn in the X-axis direction so as to be tangent to an upper surface of the laminated chip, a straight line N is defined as a straight line drawn in the Z-axis direction so as to be tangent to the first end face, an intersection point between the line M and the line N is defined as an intersection point O, the shortest distance between the intersection point N1 and the line M is defined as a distance C1, and the shortest distance between the intersection point N1 and the intersection point O is defined as a distance P1. 2 -C1 2 and polishing corners of the ceramic laminate so as to satisfy the relationship: (a) 0.80 or less.

Citation Information

Patent Citations

  • Multilayer ceramic capacitor

    JP2000114097A

  • Chip electrical component and chip capacitor

    JP2001210545A

  • Electronic part

    JP2006310700A

  • Ceramic electronic component and manufacturing method thereof