Polarizing plate, its manufacturing method, and optical device
The polarizing plate with a wire grid structure and protective film enhances light transmission and durability, addressing the challenges of maintaining high transmittance and low reflectance under intense light sources.
Patent Information
- Application Number
- JP2020083839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-05-12
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-05-12
AI Technical Summary
Existing wire grid polarizing plates struggle to maintain high transmittance and low reflectance characteristics while ensuring durability, particularly under intense light sources like LEDs and lasers, due to issues with grid structure and protective layers.
A polarizing plate with a wire grid structure on a transparent substrate, featuring convex portions with a reflective layer, dielectric layers, and an antireflection layer, covered by a protective film, optimized to enhance light transmission and durability.
The solution provides improved light transmission characteristics in the transmission axis direction while maintaining durability, suitable for high-intensity light environments, such as liquid crystal projectors.
Smart Images

Figure 0007569164000002 
Figure 0007569164000003 
Figure 0007569164000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing plate, a manufacturing method thereof, and an optical device. [Background technology]
[0002] A polarizing plate is an optical element that absorbs light polarized in one direction and transmits light polarized in the direction perpendicular to the direction. In principle, polarizing plates are necessary for liquid crystal display devices. In particular, in liquid crystal display devices that use a light source with a large amount of light, such as a transmissive liquid crystal projector, the polarizing plate is exposed to strong radiation, so it needs to have excellent heat resistance and light resistance, as well as a size of about several centimeters and high control of the extinction ratio and reflectance characteristics. In order to meet these requirements, a wire grid type inorganic polarizing plate has been proposed.
[0003] A wire grid polarizer has a structure in which a large number of conductive wires extending in one direction are arranged on a substrate with a pitch (tens to hundreds of nm) narrower than the wavelength band of the light being used. When light is incident on this polarizer, polarized light parallel to the extension direction of the wires (TE waves (S waves)) cannot be transmitted, and polarized light perpendicular to the extension direction of the wires (TM waves (P waves)) is transmitted as is.
[0004] Wire grid polarizers have excellent heat and light resistance, can be made into relatively large elements, and have a high extinction ratio. In addition, by making them multi-layered, it is possible to control the reflectance characteristics, and they are suitable for use in liquid crystal projectors, etc., because they reduce image degradation caused by ghosts, which are caused by the return light reflected on the surface of the polarizer being reflected again inside the liquid crystal projector.
[0005] In response to this, various types of wire grid type polarizing plates have been proposed. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 2016-536651 [Patent Document 2] Special Publication No. 2019-536074 Summary of the Invention [Problem to be solved by the invention]
[0007] Patent Document 1 discloses a polarizing plate in which side bars that can support each other are formed on the side walls of a wire grid polarizer (polarizing plate), and a polarizing plate in which the wire grid polarizers are embedded. It is described that the durability of the wire grid polarizer can be improved, and good polarization characteristics are shown in the visible spectrum. However, in order to improve the durability of a high aspect ratio wire grid polarizer using only side bars, the side bar width naturally becomes wider, and good polarization characteristics such as a decrease in transmittance and an increase in reflectance cannot be obtained. The same is true when the side bars are embedded, and although the durability of the wire grid polarizer is improved to the extent that it can be wiped away, good polarization characteristics such as a decrease in transmittance and an increase in reflectance cannot be obtained.
[0008] Patent Document 2 discloses a polarizing plate in which an overcoat layer is formed from the tip to the sidewall of a wire grid polarizer (polarizing plate), and a polarizing plate in which an antireflection layer is formed on the overcoat layer. It is described that the wire grid polarizer can be durable and have high performance. However, even if the wire grid polarizer is supported by the overcoat layer to prevent collapse, high-performance polarization characteristics such as a decrease in transmittance and an increase in reflectance due to the inclusion of an air layer cannot be obtained. In addition, although it is thought that the polarization characteristics can be restored by forming an antireflection layer thereon, the durability of the antireflection layer itself cannot be improved.
[0009] In recent years, lighting and display light sources have evolved from lamps to LEDs and then to lasers, and even liquid crystal projectors are using multiple semiconductor lasers (LDs) to achieve high luminous flux and brightness. As a result, polarizing plates are required to have high transmittance characteristics while being able to withstand environments with high luminosity and strong light. To achieve this, it is necessary to propose polarizing plates with an optimized grid structure, including a protective film.
[0010] The present invention has been made in consideration of the above-mentioned circumstances, and aims to provide a polarizing plate and a manufacturing method thereof, as well as an optical device equipped with the polarizing plate, in which the grid structure, including the protective film, is optimized to improve the light transmission characteristics in the transmission axis direction while maintaining durability. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides the following means.
[0012] (1) A polarizing plate according to one embodiment of the present invention has a wire grid structure and comprises a transparent substrate, a plurality of convex portions formed on a first surface of the transparent substrate, extending in a first direction, and arranged periodically and spaced apart at a pitch shorter than the wavelength of light in a used band, and an anti-reflection layer formed on a second surface of the transparent substrate opposite the first surface, wherein each of the plurality of convex portions has, in order from the transparent substrate side, a reflective layer, a dielectric layer made of a first dielectric, and an absorbing layer, and the surfaces of the convex portions and the surface of the anti-reflection layer are covered with a protective film made of a dielectric layer made of a second dielectric.
[0013] (2) In the above aspect, the protective film may have a thickness of 2.5 nm or less.
[0014] (3) In the above aspect, the protective film may have a thickness of 2.5 nm or more.
[0015] (4) In the above aspect, the dielectric layer made of the first dielectric may be made of SiO2, and the protective film made of the second dielectric may be made of Al2O3.
[0016] (5) In the above aspect, the protective film made of the second dielectric may be an ALD film.
[0017] (6) In the above embodiment, the antireflection layer may be an alternating laminate of high refractive index films and low refractive index films.
[0018] (7) In the above aspect, the antireflection layer may be an ion beam assisted deposition film or an ion beam sputtering film.
[0019] (8) In the above aspect, the high refractive index film may be made of TiO2, and the low refractive index film may be made of SiO2.
[0020] (9) In the above aspect, the transparent substrate may be transparent to the wavelength of light in the used band and may be made of any material selected from the group consisting of glass, crystal, quartz, and sapphire.
[0021] (10) In the above aspect, the dielectric layer made of the first dielectric may be made of any material selected from the group consisting of Si oxide, Ti oxide, Zr oxide, Al oxide, Nb oxide, and Ta oxide.
[0022] (11) In the above aspect, the reflective layer may be made of aluminum or an aluminum alloy.
[0023] (12) In the above aspect, the absorption layer may be made of any material that has an absorption effect for wavelengths of light in the used band and is selected from the group consisting of metals, alloy materials, and semiconductor materials.
[0024] (13) In the above embodiment, the surface of the polarizing plate may be covered with an organic water-repellent film.
[0025] (14) A method for manufacturing a polarizing plate according to another aspect of the present invention is a method for manufacturing a polarizing plate having a wire grid structure, comprising the steps of: forming a reflective layer, a dielectric layer made of a first dielectric, and an absorbing layer, in that order, on a first surface of a transparent substrate to produce a laminate made of the reflective layer, the dielectric layer, and the absorbing layer; selectively etching the laminate to form a plurality of convex portions extending in a first direction and spaced apart from one another periodically at a pitch shorter than the wavelength of light in a used band; forming an anti-reflection layer on a second surface of the transparent substrate opposite the first surface; and forming a protective film made of a second dielectric on surfaces of the convex portions and on a surface of the anti-reflection layer.
[0026] (15) In the above aspect, the protective film may be formed to a thickness of 2.5 nm or less.
[0027] (16) In the above aspect, the protective film may be formed to a thickness of 2.5 nm or more.
[0028] (17) In the above embodiment, a step of forming an organic water-repellent film on the surface of the polarizing plate may be included.
[0029] (18) An optical device according to yet another aspect of the present invention includes the polarizing plate of the above aspect. Effect of the Invention
[0030] According to the present invention, it is possible to provide a polarizing plate having improved light transmission characteristics in the transmission axis direction while maintaining durability. [Brief description of the drawings]
[0031] [Figure 1] FIG. 1 is a schematic perspective view of a polarizing plate according to one embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. [Diagram 3] FIG. 2 is a schematic cross-sectional view for explaining dimensions of a polarizing plate. [Figure 4]1 is a schematic cross-sectional view of an antireflection layer having a structure in which low refractive index layers and high refractive index layers having different refractive indexes are alternately laminated. [Diagram 5] 1 is a graph showing the transmission axis transmittance in the optical characteristics calculated by simulation in a polarizing plate according to one embodiment of the present invention. [Figure 6] 1 is a graph showing the results of measuring the transmission axis transmittance for Examples 1-1 to 1-3. [Figure 7] 11 is a graph showing an average transmission axis transmittance for each wavelength band calculated by simulation in a polarizing plate according to one embodiment of the present invention. [Figure 8] 1 is a graph showing the results of measuring the average transmission axis transmittance for each wavelength band for Examples 1-1 to 1-3. [Figure 9] 1 is a graph comparing contrast in optical characteristics of polarizing plates according to one embodiment of the present invention that were actually produced, through evaluation of heat resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] The present embodiment will be described in detail below with reference to the drawings as appropriate. The drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may differ from the actual ones. The materials, dimensions, etc. exemplified in the following description are merely examples, and the present invention is not limited thereto. They may be modified as appropriate within the scope of the effects of the present invention.
[0033] [Polarizing plate] FIG. 1 is a schematic perspective view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 shown in Figure 1 is a polarizing plate having a wire grid structure, and includes a transparent substrate 10, a plurality of protrusions 20 formed on a first surface 10a of the transparent substrate 10, the protrusions 20 being arranged at a pitch shorter than the wavelength of light in the band of light used and extending in a first direction (Y direction), and an anti-reflection layer 30 formed on a second surface 10b opposite the first surface 10a of the transparent substrate 10, and the surfaces of the plurality of protrusions 20 and the surface of the anti-reflection layer 30 are each covered with a protective film (not shown) made of a dielectric.
[0034] Here, as shown in FIG. 1, the direction in which the multiple protrusions extend (first direction) is referred to as the Y-axis direction. The direction perpendicular to the Y-axis direction and in which the multiple protrusions are arranged along the main surface of the transparent substrate is referred to as the X-axis direction. The direction perpendicular to the Y-axis and X-axis directions and perpendicular to the main surface of the transparent substrate is referred to as the Z-axis direction. Note that the light incident on the polarizing plate may be from either the first surface side or the second surface side of the transparent substrate, but is preferably incident from the Z-axis direction perpendicular to the X-axis and Y-axis directions on the first surface side (grid surface side) of the transparent substrate on which the multiple protrusions are formed, as exemplified in FIG. 1.
[0035] A polarizing plate with a wire grid structure utilizes four actions: transmission, reflection, interference, and selective light absorption of polarized waves due to optical anisotropy, to attenuate polarized waves with electric field components parallel to the Y-axis direction (TE waves (S waves)) and transmit polarized waves with electric field components parallel to the X-axis direction (TM waves (P waves)). Therefore, in Figure 1, the Y-axis direction is the absorption axis direction of the polarizing plate, and the X-axis direction is the transmission axis direction of the polarizing plate.
[0036] FIG. 2 is a schematic cross-sectional view of a polarizing plate according to one embodiment of the present invention. The polarizing plate 100 shown in Figure 2 comprises a transparent substrate 10, a plurality of protrusions 20 formed on a first surface 10a of the transparent substrate 10, extending in a first direction, and arranged periodically at a distance from one another at a pitch shorter than the wavelength of light in the band of light used, and an antireflection layer 30 formed on a second surface 10b of the transparent substrate 10 opposite the first surface 10a, and the plurality of protrusions 20 have, in order from the transparent substrate 10 side, a reflective layer 21, a dielectric layer 22 made of a first dielectric, and an absorbing layer 23, and the surfaces 20a of the plurality of protrusions 20 and the surface 30a of the antireflection layer 30 are covered with protective films 40A, 40B made of a second dielectric, respectively. In addition, the polarizing plate of the present invention may contain a transparent substrate, a reflective layer, a dielectric layer, an absorbing layer, a protective film, an anti-reflection layer, and other layers, as long as the effects of the present invention are achieved.
[0037] A part of the light incident from the side (grid surface side) of the polarizing plate shown in FIG. 2 on which a plurality of convex portions are formed is absorbed and attenuated when passing through the absorbing layer and the dielectric layer. Of the light transmitted through the absorbing layer and the dielectric layer, the polarized wave (TM wave (P wave)) is transmitted through the reflective layer with high transmittance. On the other hand, of the light transmitted through the absorbing layer and the dielectric layer, the polarized wave (TE wave (S wave)) is reflected by the reflective layer. The TE wave reflected by the reflective layer is partially absorbed when passing through the absorbing layer and the dielectric layer, and partially reflected and returned to the reflective layer. In addition, the TE wave reflected by the reflective layer is attenuated by interference when passing through the absorbing layer and the dielectric layer. By selectively attenuating the TE wave as described above, the polarizing plate can obtain the desired polarization characteristics.
[0038] Here, the dimensions of the polarizing plate in this specification will be explained with reference to Fig. 3. The height h of the grid is the dimension in the Z-axis direction perpendicular to the main surface of the transparent substrate in Fig. 3, and refers to the height of the multiple convex portions having a protective film (height (thickness) h1). The width w refers to the dimension in the X-axis direction perpendicular to the height h direction when viewed from the Y-axis direction along the extension direction of the multiple convex portions having a protective film. In addition, when the polarizing plate is viewed from the Y-axis direction along the extension direction of the multiple convex portions, the repeat interval in the X-axis direction of the multiple convex portions is referred to as the pitch p.
[0039] In the polarizing plate of the present invention, the pitch p of the multiple convex portions is not particularly limited as long as it is shorter than the wavelength of light in the band used. From the viewpoint of ease of production and stability, the pitch p of the multiple convex portions is preferably, for example, 100 nm to 200 nm. This pitch p of the multiple convex portions can be measured by observation with a scanning electron microscope or a transmission electron microscope. For example, the pitch p can be measured at any four points using a scanning electron microscope or a transmission electron microscope, and the arithmetic average value can be taken as the pitch p of the multiple convex portions. Hereinafter, this measurement method is referred to as the electron microscopy method.
[0040] The polarizing plate of the present invention is characterized by optimizing the thickness of the protective film covering the area between the grid edges and the anti-reflection layer, thereby improving the light transmission characteristics in the transmission axis direction while maintaining durability.
[0041] [Transparent substrate] The transparent substrate 10 is not particularly limited as long as it is a substrate that exhibits translucency for light in the used band, and can be appropriately selected depending on the purpose. "Exhibiting translucency for light in the used band" does not mean that the transmittance of light in the used band is 100%, but it is sufficient that the substrate exhibits translucency that can maintain the function as a polarizing plate. Examples of light in the used band include visible light with a wavelength of about 380 nm to 810 nm. The shape of the main surface of the transparent substrate is not particularly limited, and a shape (for example, a rectangular shape) is appropriately selected depending on the purpose. The average thickness of the transparent substrate is preferably, for example, 0.3 mm to 1 mm.
[0042] The transparent substrate 10 is preferably made of a material having a refractive index of 1.1 to 2.2, such as glass, crystal, quartz, and sapphire. From the viewpoints of cost and light transmittance, it is preferable to use glass, particularly quartz glass (refractive index 1.46) or soda-lime glass (refractive index 1.51). The composition of the glass material is not particularly limited, and inexpensive glass materials such as silicate glass that is widely distributed as optical glass can be used.
[0043] From the viewpoint of thermal conductivity, it is preferable to use quartz crystal or sapphire, which have high thermal conductivity, as this provides high light resistance against strong light and is preferably used as a polarizing plate for the optical engine of a projector that generates a large amount of heat.
[0044] When using a transparent substrate made of optically active crystal such as quartz or sapphire, it is preferable to arrange multiple convex portions in a direction parallel or perpendicular to the optical axis of the crystal. This allows for excellent optical properties to be obtained. Here, the optical axis is the directional axis in which the difference in refractive index between the ordinary ray (O) and extraordinary ray (E) of light traveling in that direction is the smallest.
[0045] [Reflective layer] The reflective layer 21 is formed on a transparent substrate, and is made of metal films extending in strips in the Y-axis direction, which is the absorption axis.
[0046] The reflective layer 21 functions as a wire grid polarizer, attenuating polarized waves (TE waves (S waves)) having an electric field component in a direction parallel to the longitudinal direction of the reflective layer, and transmitting polarized waves (TM waves (P waves)) having an electric field component in a direction perpendicular to the longitudinal direction of the reflective layer. The thickness of the reflective layer is not particularly limited, and is preferably, for example, 100 nm to 300 nm. The thickness of the reflective layer can be measured, for example, by the above-mentioned electron microscopy method.
[0047] The material of the reflective layer is not particularly limited as long as it is a material that is reflective to light in the used band, and examples thereof include single elements such as Al, Ag, Cu, Mo, Cr, Ti, Ni, W, Fe, Si, Ge, and Te, or alloys containing one or more of these elements. Among them, the reflective layer is preferably made of aluminum or an aluminum alloy from the viewpoint of minimizing absorption loss in the wire grid in the visible light region and from the viewpoint of cost. In addition to these metal materials, the reflective layer may be made of a non-metallic inorganic film or a resin film that has a high surface reflectance formed by, for example, coloring.
[0048] The reflective layer 21 can be formed as a high-density film by using, for example, a vapor deposition method or a sputtering method. The reflective layer may be composed of two or more layers made of different materials.
[0049] [Dielectric layer] The dielectric layer 22 is formed on the reflective layer, and is an arrangement of dielectric films extending in a strip shape in the Y-axis direction, which is the absorption axis. The thickness of the dielectric layer is formed in a range in which the phase of the polarized light that passes through the absorbing layer and is reflected by the reflective layer is shifted by half a wavelength from the polarized light reflected by the absorbing layer. Specifically, the thickness of the dielectric layer is appropriately set in a range of 1 nm to 500 nm, which is capable of adjusting the phase of the polarized light to enhance the interference effect. The thickness of this dielectric layer can be measured, for example, by the above-mentioned electron microscope method. The dielectric layer 22b is also formed as a barrier layer that suppresses mutual diffusion of the constituent elements of the reflective layer and the absorbing layer, which will be described later.
[0050] The first dielectric material constituting the dielectric layer 22 may be a common material such as a silicon oxide such as SiO2, a metal oxide such as Al2O3, beryllium oxide, or bismuth oxide, MgF2, cryolite, germanium, titanium dioxide, silicon, magnesium fluoride, boron nitride, boron oxide, tantalum oxide, carbon, or a combination thereof. In particular, from the viewpoint of transmittance and barrier layer function, it is preferable that the dielectric layer 22 is composed of one or more oxides selected from the group consisting of Si oxide, Ti oxide, Zr oxide, Al oxide, Nb oxide, and Ta oxide.
[0051] The refractive index of the dielectric layer 22 is preferably greater than 1.0 and equal to or less than 2.5. Since the optical characteristics of the reflective layer 21 are also affected by the refractive index of the surroundings, the optical characteristics of the polarizing plate can be controlled by selecting the material of the dielectric layer 22. In addition, by appropriately adjusting the film thickness and refractive index of the dielectric layer 22, a part of the TE wave reflected by the reflective layer 21 can be reflected back to the reflective layer 21 when passing through the absorbing layer 23, and the light passing through the absorbing layer 23 can be attenuated by interference. In this way, the TE wave can be selectively attenuated to obtain the desired polarization characteristics.
[0052] The dielectric layer 22 can be formed as a high-density film by using a deposition method, a sputtering method, a chemical vapor deposition (CVD) method, an atomic layer deposition (ALD) method, etc. The dielectric layer may be composed of two or more layers made of different materials.
[0053] [Absorption layer] The absorbing layer 23 has an absorbing effect for the wavelength of light in the used band, is formed on the dielectric layer 22, and is arranged extending in a strip shape in the Y-axis direction, which is the absorption axis. The thickness of the absorbing layer is not particularly limited, and is preferably, for example, 5 nm to 50 nm. The thickness of this absorbing layer can be measured, for example, by the above-mentioned electron microscope method.
[0054] The absorbing layer 23 is preferably made of one or more materials selected from the group consisting of metals, alloy materials, and semiconductor materials.
[0055] The material of the absorbing layer 23 is appropriately selected depending on the wavelength range of the light to be applied. Examples of metal materials include single elements such as Ta, Al, Ag, Cu, Au, Mo, Cr, Ti, W, Ni, Fe, and Sn, or alloys containing one or more of these elements. Examples of semiconductor materials include Si, Ge, Te, ZnO, and silicide materials (β-FeSi2, MgSi2, NiSi2, BaSi2, CrSi2, CoSi2, TaSi, etc.). By using these materials, the polarizing plate can obtain a high extinction ratio in the visible light range to which it is applied. Among these, it is preferable that the absorption layer contains Fe or Ta as well as Si.
[0056] When a semiconductor material is used as the absorption layer 23, the band gap energy of the semiconductor is involved in the absorption action, so that the band gap energy must be equal to or lower than the band to be used. For example, when used with visible light, it is necessary to use a material that absorbs at wavelengths of 400 nm or more, that is, has a band gap of 3.1 eV or less. The absorbing layer 23 can be formed as a high-density film by using, for example, a vapor deposition method or a sputtering method. The absorbing layer 23 may be composed of two or more layers made of different materials.
[0057] [Anti-reflection layer] The antireflection layer 30 is formed on the second surface 10b of the transparent substrate 10. The antireflection layer 30 may be made of a known antireflection material, and may be, for example, made of a multilayer film of at least two layers of a material capable of forming the dielectric layer 22. As an example of a multilayer film, as shown in Fig. 4, low refractive index layers 31 and high refractive index layers 32 having different refractive indices are alternately laminated, so that light reflected at the interface can be attenuated by interference. There are no particular limitations on the film thickness of the antireflection layer 30, and it is appropriately set within the range of 1 nm to 500 nm per dielectric layer constituting the dielectric layer 22. The film thickness of this antireflection layer 30 can be measured, for example, by the above-mentioned electron microscopy method.
[0058] The low refractive index layer 31 is a layer containing as a main component SiO2 (oxide of Si), etc. The refractive index of the low refractive index layer is preferably 1.20 to 1.60, and more preferably 1.30 to 1.50. The refractive index of the high refractive index layer 32 is preferably 2.00 to 2.60, and more preferably 2.10 to 2.45. Examples of such a high refractive index dielectric material include niobium pentoxide (Nb2O5, refractive index 2.33), titanium oxide (TiO2, refractive index 2.33 to 2.55), tungsten oxide (WO3, refractive index 2.2), cerium oxide (CeO2, refractive index 2.2), tantalum pentoxide (Ta2O5, refractive index 2.16), zinc oxide (ZnO, refractive index 2.1), and indium tin oxide (ITO, refractive index 2.06).
[0059] The antireflection layer can be formed as a high-density film by using the same film-forming method as the dielectric layer described above, preferably by ion-beam assisted deposition (IAD) or ion beam sputtering (IBS), which can form a high-density film.
[0060] Furthermore, taking into consideration that a protective film will be formed later, it is desirable to design the antireflection layer so that its optical properties are not deteriorated, such as its material and film thickness.
[0061] [Protective film] The surfaces 20a of the plurality of protrusions 20 and the surface 30a of the antireflection layer 30 are covered with protective films 40A and 40B made of a second dielectric material. Covering with the protective films 40A and 40B can improve the durability of the polarizing plate. The surface 20a of the convex portion 20 consists of the top surface 20aa of the convex portion 20 (which is also the top surface of the absorption layer 23) and the side surface 20ab of the convex portion 20 which is made up of the side surface 21b of the reflective layer 21, the side surface 22b of the dielectric layer 22, and the side surface 23b of the absorption layer 23, and the protective film 40A consists of a protective film 40Aa covering the top surface 20aa of the convex portion 20, and a protective film 40Ab covering the side surface 20ab of the convex portion 20.
[0062] In the polarizing plate 100 shown in FIG. 2, a protective film 40AA is also provided on a surface 10aa of the surface 10a of the transparent substrate 10 on which neither the protrusions 20 nor the protective film 40A is formed.
[0063] When forming the protective film 40A and the protective film 40B, it is preferable to use an atomic layer deposition (ALD) method, which is dense, uniform, and has excellent thickness controllability. Also, similar to the above-mentioned dielectric layer 22, the protective film 40A and the protective film 40B may be composed of two or more layers made of different materials.
[0064] In addition, when filling the gaps between the protrusions 20 completely (as in FIG. 2), a SOG (Spin on Glass) method can be used in addition to the above-mentioned method of forming the dielectric layer 22. SOG makes it possible to achieve flatness without including an air layer.
[0065] Furthermore, taking into consideration that the protective film 40B is formed on the surface 30a of the antireflection layer 30, it is desirable to design the protective film so that the optical characteristics are not deteriorated, for example, in terms of the material and film thickness.
[0066] The second dielectric constituting the protective film can be the same as the first dielectric constituting the dielectric film 22. From the viewpoint of heat resistance, Al2O3 is particularly preferable.
[0067] At least one of the protective films 40A and 40B may have a thickness of 2.5 nm or less. In this case, the durability of the polarizing plate is maintained while improving the light transmission characteristics, and a significant decrease in optical characteristics in particular can be avoided. In this case, from the viewpoint of maintaining durability, the thickness is preferably 1 nm or more, more preferably 1.5 nm or more, and even more preferably 2.0 nm or more.
[0068] At least one of the protective films 40A and 40B may have a thickness of 2.5 nm or more. In this case, the durability of the polarizing plate is maintained while improving the light transmission characteristics, and in particular, high heat resistance can be maintained. In this case, from the viewpoint of improving the light transmission characteristics, the thickness is preferably 10 nm or less, more preferably 7.5 nm or less, and even more preferably 5.0 nm or less.
[0069] [Water-repellent film] Furthermore, in the polarizing plate of the present invention, at least one of the surfaces 100a, 100b of the polarizing plate 100 may be covered with an organic water-repellent film. The organic water-repellent film is made of a fluorine-based silane compound such as perfluorodecyltriethoxysilane (FDTS), and can be formed by using the above-mentioned CVD method or ALD method. This can improve the reliability of the polarizing plate, such as its moisture resistance.
[0070] [Method of manufacturing polarizing plate] The method for manufacturing a polarizing plate of the present invention is a method for manufacturing a polarizing plate having a wire grid structure, and includes the steps of forming a reflective layer, a dielectric layer, and an absorbing layer, in that order, on a first surface of a transparent substrate to produce a laminate consisting of the reflective layer, the dielectric layer, and the absorbing layer, selectively etching the laminate to form a plurality of convex portions that extend in a first direction and are periodically arranged at a pitch shorter than the wavelength of light in the band of light used, forming an anti-reflection layer on a second surface of the transparent substrate opposite the first surface, and forming a protective film consisting of a dielectric on the surfaces of the convex portions and the surface of the anti-reflection layer.
[0071] To form the multiple convex portions, a one-dimensional lattice-shaped mask pattern is formed with resist on a laminated film formed on one side of a transparent substrate, for example, by photolithography, nanoimprinting, etc. A portion on which the mask pattern is not formed is selectively etched to form multiple convex portions arranged on the transparent substrate at a pitch shorter than the wavelength of light in the band used. As an etching method, for example, a dry etching method using an etching gas corresponding to the etching target can be mentioned.
[0072] In this manner, the polarizing plate shown in Figures 1 and 2 is produced. The method for producing a polarizing plate of the present invention may further include a step of coating the surface of the polarizing plate with an organic water-repellent film.
[0073] [Optical equipment] The optical device of the present invention includes the polarizing plate according to the present invention described above. The polarizing plate according to the present invention can be used for various purposes. Examples of optical devices to which the polarizing plate according to the present invention can be applied include liquid crystal displays, liquid crystal projectors, head-up displays, and car headlights. In particular, since the polarizing plate according to the present invention has high transmittance, it is possible to achieve high brightness with high transmittance while having excellent heat resistance, even in an environment of high-intensity light using multiple semiconductor lasers (LD). This makes it suitable for use in applications such as liquid crystal projectors.
[0074] When the optical device according to the present invention includes a plurality of polarizing plates, at least one of the plurality of polarizing plates may be the polarizing plate according to the present invention. For example, when the optical device according to the present invention is a liquid crystal projector, at least one of the polarizing plates arranged on the entrance side and the exit side of the liquid crystal panel may be the polarizing plate according to the present invention. EXAMPLES
[0075] Next, examples of the present invention will be described. However, the present invention is not limited to these examples, and modifications and improvements within the scope of the present invention are included in the present invention.
[0076] [simulation] Simulations were performed using the polarizing plate shown in Fig. 2 as a model of the polarizing plate according to the present invention. More specifically, the optical properties of these polarizing plates were verified by electromagnetic field simulation using the RCWA (Rigorous Coupled Wave Analysis) method.
[0077] Fig. 5 is a graph showing the spectral waveform of the transmission axis transmittance in the visible light region (red band: wavelength λ = 600 to 680 nm, green band: wavelength λ = 520 nm to 590 nm, blue band: λ = 430 nm to 510 nm) obtained by performing a simulation using the polarizing plate shown in Fig. 2 as a model. The horizontal axis indicates the wavelength λ (nm), and the vertical axis indicates the transmission axis transmittance (%). Here, the transmission axis transmittance means the transmittance of polarized light (TM wave) in the transmission axis direction (X-axis direction) that is incident on the polarizing plate.
[0078] In the polarizing plate model, the following parameters and materials were used. Transparent substrate: material (alkali-free glass), thickness (0.7 mm), Reflective layer: material (Al), thickness (250 nm), width (35 nm), Dielectric layer: material (SiO2), thickness (5 nm), width (35 nm), Absorption layer: material (FeSi), thickness (25 nm), width (35 nm), Anti-reflection layer: Material (alternate laminate of TiO2 layer / SiO2 layer), thickness (641.15 nm), width (35 nm), specific layer structure is shown in Table 1. Layers 1 to 9 were arranged in order from the side closest to the transparent substrate to the side furthest from it. Grid: height h (280 + protective film thickness) nm, width w (35 + protective film thickness × 2) nm, pitch p (141 nm).
[0079] [Table 1]
[0080] In the polarizing plate model, the protective film (reference numerals 40A and 40B in FIG. 2) was made of Al2O3 and had film thicknesses of 1 nm, 2.5 nm, 5 nm, 7.5 nm, and 10 nm. As a comparative example, a simulation was also performed for a case where no protective film was provided, and the result is shown in FIG.
[0081] The protective film can improve the durability of the polarizing plate. However, as shown in Figure 5, as the film thickness increases, the transmission axis transmittance decreases across the entire visible light range, with the drop being particularly large on the short wavelength side.
[0082] [Examples 1-1 to 1-3, Comparative Example 1] Polarizing plates were actually fabricated with protective film thicknesses of 2.5 nm (Example 1-1), 5 nm (Example 1-2), and 7.5 nm (Example 1-3) and other parameters used in the above simulation, and the transmission axis transmittance was measured. The results are shown in Figure 6. In addition, the transmission axis transmittance of a polarizing plate not provided with a protective film (Comparative Example 1) was also measured, and the results are shown in Figure 6.
[0083] It can be seen that the simulation results shown in FIG. 5 closely reflect the optical characteristics of the actual polarizing plate.
[0084] Based on the results of FIG. 5 and FIG. 6, when it is required that the transmission axis transmittance is 80% or more over the entire wavelength range from 400 nm to 700 nm, the thickness of the protective film is set to 5 nm or less. When a transmission axis transmittance of 80% or more is required for all wavelengths from 430 nm to 700 nm, the thickness of the protective film is set to 10 nm or less.
[0085] FIG. 7 is a graph showing the average value of the transmission axis transmittance for each wavelength band obtained by performing a simulation.
[0086] Fig. 8 is a graph showing the average value of the transmission axis transmittance for each wavelength band measured for the polarizing plates of Examples 1-1 to 1-3 and Comparative Example 1. It can be seen that the simulation results shown in Fig. 7 well reflect the optical characteristics of the actual polarizing plates.
[0087] Based on FIG. 7 and FIG. 8, when an average transmission axis transmittance of 86% or more is required across the entire red, green and blue bands, the thickness of the protective film is set to 5 nm or less. When the average transmission axis transmittance is required to be 90% or more across the entire red, green and blue bands, the thickness of the protective film is set to 2.5 nm or less.
[0088] [Heat resistance evaluation] The heat resistance of a polarizing plate actually produced as a polarizing plate according to the present invention was evaluated. The heat resistance evaluation was performed at 300°C in a clean oven, and the contrast, which is an optical characteristic of the polarizing plate, was evaluated based on the initial characteristic, i.e., the rate of change from before it was placed in the clean oven. The contrast can be calculated by the transmission axis transmittance / absorption axis transmittance, and the absorption axis transmittance means the transmittance of polarized light (TE wave) in the absorption axis direction (Y axis) that is incident on the polarizing plate. The contrast change rate is suitable for grasping the influence on the heat resistance of the polarizing plate.
[0089] Figure 9 is a graph comparing the contrast of optical characteristics of actually manufactured panels through a heat resistance evaluation. The horizontal axis shows the test time (time spent in a clean oven) and the vertical axis shows the rate of change in contrast, with the example showing a case where the incident light was in the green band of the visible light region (wavelength = 520 nm to 590 nm). Figure 9 also shows the results for a case where no protective film was provided.
[0090] As shown in Figure 9, as the protective film becomes thicker, the rate of change in contrast decreases, and the durability of the polarizing plate improves. Note that, although the example shown is one in which the incident light is in the green band, the same effect was obtained even if the incident light was in the red band (wavelength = 600-680 nm) or blue band (wavelength = 430 nm-510 nm), with only a slight variation in the value of the rate of change in contrast.
[0091] The results in FIG. 9 show that high heat resistance can be maintained if the protective film has a thickness of 2.5 nm or more.
[0092] From the above results, it was found that the polarizing plate of the present invention, which has a protective film on the surface of the convex portions and on the surface of the antireflection layer, can achieve improved light transmission characteristics while maintaining durability. In particular, it was found that a film thickness of 2.5 nm or less is desirable so as not to significantly degrade the optical properties, and that a film thickness of 2.5 nm or more is desirable so as to maintain high heat resistance.
[0093] In addition, when forming the protective film, it is preferable to design the protective film and the antireflection layer taking into consideration not only the plurality of convex portions but also the effect on the antireflection layer. [Explanation of symbols]
[0094] 10 Transparent substrate 10a First Side 10b The second aspect 20 Convex 21 Reflective layer 22 Dielectric layer 23 Absorption layer 30 Anti-reflection layer 40A, 40B Protective film 100, 100A polarizing plate 100a Polarizing plate surface
Claims
1. A polarizing plate having a wire grid structure, A transparent substrate; a plurality of protrusions formed on a first surface of the transparent substrate, extending in a first direction, and periodically arranged at intervals shorter than the wavelength of light in a used band; an anti-reflection layer formed on a second surface of the transparent substrate opposite the first surface; each of the plurality of convex portions includes, in order from the transparent substrate side, a reflective layer, a dielectric layer made of a first dielectric material, and an absorbing layer; a surface of the protrusion and a surface of the antireflection layer are covered with a protective film made of a second dielectric material; The protective film has a thickness of 2.5 nm or less, A polarizing plate, wherein the dielectric layer made of the first dielectric material is made of SiO 2 , and the protective film made of the second dielectric material is made of Al 2 O 3 .
2. 2. The polarizing plate according to claim 1, wherein the antireflection layer is a laminate of high refractive index films and low refractive index films alternately laminated together.
3. The high refractive index film is TiO 2 The low refractive index film is made of SiO 2 The polarizing plate according to claim 2 ,
4. The polarizing plate according to any one of claims 1 to 3, wherein the transparent substrate is transparent to the wavelength of light in the used band and is made of any material selected from the group consisting of glass, crystal, quartz, and sapphire.
5. 5. The polarizing plate according to claim 1, wherein the reflective layer is made of aluminum or an aluminum alloy.
6. The polarizing plate according to any one of claims 1 to 5, wherein the absorption layer has an absorption effect for the wavelength of light in the used band and is made of any material selected from the group consisting of metals, alloy materials, and semiconductor materials.
7. 7. The polarizing plate according to claim 1, wherein a surface of the polarizing plate is covered with an organic water-repellent film.
8. A method for manufacturing a polarizing plate having a wire grid structure, comprising the steps of: A step of forming a reflective layer, a dielectric layer made of a first dielectric material, and an absorbing layer in this order on a first surface of a transparent substrate to prepare a laminate made of the reflective layer, the dielectric layer, and the absorbing layer; a step of selectively etching the laminate to form a plurality of convex portions extending in a first direction and periodically arranged at intervals shorter than the wavelength of light in a used band; forming an anti-reflection layer on a second surface of the transparent substrate opposite the first surface; forming a protective film made of a second dielectric material and having a thickness of 2.5 nm or less on the surfaces of the convex portions and the surface of the antireflection layer; The method for producing a polarizing plate, wherein the dielectric layer made of the first dielectric material is made of SiO 2 , and the protective film made of the second dielectric material is made of Al 2 O 3 .
9. The method for producing a polarizing plate according to claim 8 , further comprising a step of forming an organic water-repellent film on a surface of the polarizing plate.
10. An optical device comprising the polarizing plate according to any one of claims 1 to 7.
Citation Information
Patent Citations
Polarizing element and liquid crystal projector
JP2008216957A
Wire grid splitter with side regions
JP2016536651A
Inorganic polarizer and manufacturing method thereof
JP2018040888A
Imaging device and solid-state imaging device
JP2019047392A
Polarizer, manufacturing method for the same and optical equipment
JP2019061226A