Anti-reflection film, its manufacturing method, and image display device
The antireflection film with a hard coat layer and laminate structure addresses cracking issues in foldable displays by enhancing bending resistance through a combination of fine particles and refractive index layers, ensuring durability and visibility.
Patent Information
- Application Number
- JP2022074697
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-04-28
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2042-04-28
AI Technical Summary
Foldable image display devices with antireflection films face issues of cracking in the antireflection layer when heated in a folded state due to compressive and tensile stresses, leading to decreased visibility.
An antireflection film with a hard coat layer containing fine particles and a primer layer, combined with a laminate structure of high and low refractive index layers, including niobium oxide thin films, enhances bending resistance and prevents cracking.
The antireflection film maintains integrity even when heated in a bent state, suitable for foldable displays by reducing stress-induced cracking.
Smart Images

Figure 0007569352000002 
Figure 0007569352000003 
Figure 0007569352000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an antireflection film having an antireflection layer on a hard coat layer of a hard coat film, and a manufacturing method thereof.Furthermore, the present invention relates to an image display device having the antireflection film. [Background technology]
[0002] Anti-reflection films are used on the viewing side surfaces of image display devices such as liquid crystal displays and organic EL displays for the purposes of preventing deterioration of image quality due to reflection of external light, improving contrast, etc. Anti-reflection films have an anti-reflection layer made of a laminate of multiple thin films with different refractive indices on a transparent film.
[0003] For example, Patent Document 1 discloses an antireflection film having a SiO primer layer on a hard coat film, and an antireflection layer thereon consisting of an alternating laminate of a niobium oxide (Nb2O5) layer as a high refractive index layer and a silicon oxide (SiO2) layer as a low refractive index layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2009-47876 A Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, foldable image display devices (foldable displays) equipped with organic EL panels using foldable substrates (flexible substrates) such as resin films have been put to practical use. As the cover window of a foldable display, an anti-reflection film having an anti-reflection layer provided on a flexible film substrate is used.
[0006] Foldable displays are generally stored in a folded state. In the folded state, compressive stress is applied to the inside of the folding point (bending point), and tensile stress is applied to the outside. When the display is folded with the display surface on the inside, the anti-reflection film is folded with the surface on which the anti-reflection layer is formed on the inside. If the display is heated to a high temperature in this state, fine cracks may occur in the anti-reflection layer, causing a decrease in the visibility of the display.
[0007] In view of the above, an object of the present invention is to provide an antireflection film that is unlikely to develop cracks in the antireflection layer and has excellent flex resistance even when heated to high temperatures in a folded (bent) state. [Means for solving the problem]
[0008] The anti-reflection film includes a hard coat film having a hard coat layer on one main surface of a transparent film substrate, and an anti-reflection layer provided on the hard coat layer. The hard coat layer may contain fine particles having an average primary particle size of 10 to 100 nm in addition to a binder resin. A primer layer made of an inorganic oxide may be provided between the hard coat layer and the anti-reflection layer. An antifouling layer may be provided on the anti-reflection layer.
[0009] The antireflection layer includes at least one high refractive index layer and at least one low refractive index layer. The antireflection layer may include two or more high refractive index layers, or may include two or more low refractive index layers. The antireflection layer is preferably an alternating laminate of a plurality of high refractive index layers and a plurality of low refractive index layers.
[0010] The high refractive index layer of the antireflection layer is a thin film mainly composed of niobium oxide, and the high refractive index layer disposed farthest from the hard coat layer has a film thickness of 40 nm or less and a film density of 4.47 g / cm 3 When the antireflection layer contains multiple high refractive index layers (niobium oxide thin films), the thickness of each high refractive index layer is 40 nm or less, and the film density is 4.47 g / cm 3 It is preferable that it is less than 1000 .mu.m.
[0011] The arithmetic mean surface height of the antireflection layer is preferably 2.5 nm or more. When an antifouling layer is provided on the antireflection layer, the arithmetic mean surface height of the antifouling layer is preferably 2.5 nm or more. Effect of the Invention
[0012] The antireflection film of the present invention is unlikely to develop cracks in the antireflection layer even when heated in a bent state with the surface on which the antireflection layer is formed facing inward, and can be suitably used for foldable displays. [Brief description of the drawings]
[0013] [Figure 1] FIG. 2 is a cross-sectional view showing a lamination form of an anti-reflection film. [Diagram 2] FIG. 2 is a cross-sectional view showing the configuration of a sample used in a bending resistance test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] FIG. 1 is a cross-sectional view showing an example of a laminated structure of an antireflection film according to one embodiment of the present invention. The antireflection film 101 includes an antireflection layer 5 on a hard coat layer 11 of a hard coat film 1. The hard coat film 1 includes a hard coat layer 11 on one main surface of a transparent film substrate 10. The antireflection layer 5 is a laminate of two or more thin layers having different refractive indices, and includes at least one high refractive index layer and at least one low refractive index layer. A primer layer 3 may be provided between the hard coat layer 11 and the antireflection layer 5. An antifouling layer 7 may be provided on the antireflection layer 5.
[0015] [Hard coat film] The hard coat film 1 has a hard coat layer 11 on one main surface of a transparent film substrate 10. By providing the hard coat layer 11 on the surface on which the antireflection layer 5 is formed, the mechanical properties such as surface hardness and scratch resistance of the antireflection film can be improved.
[0016] <Transparent film substrate> The visible light transmittance of the transparent film substrate 10 is preferably 80% or more, more preferably 90% or more. The resin material constituting the transparent film substrate 10 is preferably a resin material having excellent transparency, mechanical strength, and thermal stability. Specific examples of the resin material include cellulose-based resins such as triacetyl cellulose, polyester-based resins, polyethersulfone-based resins, polysulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, cyclic polyolefin-based resins (norbornene-based resins), polyarylate-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, and mixtures thereof.
[0017] The thickness of the transparent film substrate is not particularly limited, but from the viewpoints of strength, workability such as handleability, thin layer property, etc., it is preferably about 5 to 300 μm, more preferably 10 to 250 μm, and even more preferably 20 to 200 μm.
[0018] <Hard coat layer> A hard coat film 1 is formed by providing a hard coat layer 11 on the main surface of a transparent film substrate 10. The hard coat layer is a cured resin layer, and is formed by applying a composition containing a curable resin onto the transparent film substrate and curing the resin component. The hard coat layer may contain fine particles in addition to the cured resin.
[0019] (curable resin) As the curable resin (binder resin) of the hard coat layer 11, a curable resin such as a thermosetting resin, a photocurable resin, or an electron beam curable resin is preferably used. Types of the curable resin include polyester-based, acrylic-based, urethane-based, acryl urethane-based, amide-based, silicone-based, silicate-based, epoxy-based, melamine-based, oxetane-based, and acryl urethane-based. Among these, acrylic resins, acryl urethane resins, and epoxy resins are preferred because of their high hardness and the ability to be photocured, and among these, acryl urethane resins are preferred.
[0020] The photocurable resin composition contains a polyfunctional compound having two or more photopolymerizable (preferably ultraviolet-polymerizable) functional groups. The polyfunctional compound may be a monomer or an oligomer. As the photopolymerizable polyfunctional compound, a compound containing two or more (meth)acryloyl groups in one molecule is preferably used.
[0021] Specific examples of polyfunctional compounds having two or more (meth)acryloyl groups in one molecule include tricyclodecane dimethanol diacrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, trimethylolpropane triacrylate, pentaerythritol tetra(meth)acrylate, dimethylolpropane tetraacrylate, dipentaerythritol hexa(meth)acrylate, 1,6-hexanediol (meth)acrylate, 1,9-nonanediol diacrylate, 1,10-decanediol (meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, dipropylene glycol diacrylate, isocyanuric acid tri(meth)acrylate, ethoxylated glycerin triacrylate, ethoxylated pentaerythritol tetraacrylate, and oligomers or prepolymers thereof. In this specification, "(meth)acrylic" means acrylic and / or methacrylic.
[0022] The polyfunctional compound having two or more (meth)acryloyl groups in one molecule may have a hydroxyl group. By using a polyfunctional compound containing a hydroxyl group, the adhesion between the transparent film substrate and the hard coat layer tends to be improved. Examples of the compound having a hydroxyl group and two or more (meth)acryloyl groups in one molecule include pentaerythritol tri(meth)acrylate and dipentaerythritol penta(meth)acrylate.
[0023] The acrylic urethane resin contains a urethane (meth)acrylate monomer or oligomer as a polyfunctional compound. The number of (meth)acryloyl groups in the urethane (meth)acrylate is preferably 3 or more, more preferably 4 to 15, and even more preferably 6 to 12. The molecular weight of the urethane (meth)acrylate oligomer is, for example, 3000 or less, preferably 500 to 2500, and more preferably 800 to 2000. The urethane (meth)acrylate can be obtained, for example, by reacting a hydroxy (meth)acrylate obtained from (meth)acrylic acid or a (meth)acrylic acid ester and a polyol with a diisocyanate.
[0024] The content of the polyfunctional compound in the composition for forming the hard coat layer is preferably 50 parts by weight or more, more preferably 60 parts by weight or more, and even more preferably 70 parts by weight or more, based on 100 parts by weight of the total of the resin components (monomers, oligomers and prepolymers that form the binder resin by curing). If the content of the polyfunctional monomer is within the above range, the hardness of the hard coat layer tends to be increased.
[0025] (fine particles) When the hard coat layer 11 contains fine particles, fine irregularities are formed on the surface, which tends to improve the adhesion and flex resistance of the antireflection layer.
[0026] As the fine particles, inorganic oxide fine particles such as silica, alumina, titania, zirconia, calcium oxide, tin oxide, indium oxide, cadmium oxide, and antimony oxide, glass fine particles, and crosslinked or uncrosslinked organic fine particles made of transparent polymers such as polymethyl methacrylate, polystyrene, polyurethane, acrylic-styrene copolymer, benzoguanamine, melamine, and polycarbonate can be used without any particular limitation.
[0027] The average particle size (average primary particle size) of the fine particles is preferably about 10 nm to 10 μm. The average primary particle size is the weight average particle size measured by the Coulter count method. Depending on the particle size, the fine particles can be roughly divided into fine particles having a particle size of about 0.5 μm to 10 μm, submicron or μm order (hereinafter sometimes referred to as "microparticles"), fine particles having a particle size of about 10 nm to 100 nm (hereinafter sometimes referred to as "nanoparticles"), and fine particles having a particle size intermediate between microparticles and nanoparticles.
[0028] By including nanoparticles in the hard coat layer 11, fine irregularities are formed on the surface, and the adhesion between the hard coat layer 11 and the primer layer 3 and the antireflection layer 5 tends to be improved. As the nanoparticles, inorganic fine particles are preferred, and inorganic oxide fine particles are particularly preferred. Among them, silica particles are preferred because they have a low refractive index and can reduce the difference in refractive index with the binder resin.
[0029] From the viewpoint of forming an uneven surface on the hard coat layer 11 that provides excellent adhesion to the antireflection layer, the average primary particle size of the nanoparticles is preferably 20 to 80 nm, more preferably 25 to 70 nm, and even more preferably 30 to 60 nm.
[0030] The amount of nanoparticles in the hard coat layer 11 may be about 1 to 150 parts by weight relative to 100 parts by weight of the binder resin. From the viewpoint of forming a surface shape on the surface of the hard coat layer 11 that has excellent adhesion to an antireflection layer, the content of nanoparticles in the hard coat layer 11 is preferably 20 to 100 parts by weight, more preferably 25 to 90 parts by weight, and even more preferably 30 to 80 parts by weight, relative to 100 parts by weight of the binder resin.
[0031] (Formation of hard coat layer) The hard coat layer forming composition contains the above-mentioned binder resin component, and if necessary, contains a solvent capable of dissolving the binder resin component. As described above, the hard coat layer forming composition may contain fine particles. When the binder resin component is a photocurable resin, it is preferable that a photopolymerization initiator is contained in the composition. In addition to the above, the hard coat layer forming composition may contain additives such as a leveling agent, a thixotropic agent, an antistatic agent, an antiblocking agent, a dispersant, a dispersion stabilizer, an antioxidant, an ultraviolet absorber, an antifoaming agent, a thickener, a surfactant, and a lubricant.
[0032] A hard coat layer is formed by applying a composition for forming a hard coat layer on a transparent film substrate, and removing the solvent and curing the resin as necessary. Any suitable method such as bar coating, roll coating, gravure coating, rod coating, slot orifice coating, curtain coating, fountain coating, and comma coating may be adopted as a method for applying the composition for forming a hard coat layer. The heating temperature after application may be set to an appropriate temperature depending on the composition of the composition for forming a hard coat layer, and is, for example, about 50°C to 150°C. When the binder resin component is a photocurable resin, photocuring is performed by irradiating it with active energy rays such as ultraviolet rays. The integrated light amount of the irradiated light is preferably 100 to 500 mJ / cm. 2 That's about it.
[0033] The thickness of the hard coat layer 11 is not particularly limited, but from the viewpoint of realizing high hardness and appropriately controlling the surface shape, it is preferably about 1 to 10 μm, more preferably 2 to 9 μm, and even more preferably 3 to 8 μm.
[0034] (Surface treatment of hard coat layer) Before forming the anti-reflection layer 5 on the hard coat layer 11, the hard coat layer 11 may be subjected to a surface treatment. Examples of the surface treatment include surface modification treatments such as corona treatment, plasma treatment, frame treatment, ozone treatment, glow treatment, alkali treatment, acid treatment, and treatment with a coupling agent. The surface treatment may be a vacuum plasma treatment. The surface roughness of the hard coat layer can also be adjusted by the vacuum plasma treatment. For example, when the hard coat layer 11 contains inorganic fine particles in addition to the binder resin component (resin cured product), the resin component on the hard coat layer surface is likely to be selectively etched by the vacuum plasma treatment, and the inorganic particles are hardly etched and remain, so that the ratio of inorganic oxide particles present on the hard coat layer surface and in its vicinity increases, and the arithmetic average height Sa1 of the hard coat layer surface tends to increase.
[0035] The atmospheric gas in the vacuum plasma treatment is preferably an inert gas such as helium, neon, argon, krypton, xenon, or radon, of which argon is the most preferable. The effective power density in the vacuum plasma treatment is 0.01 W min / m cm 2 More than 0.03 W min / m cm is preferable. 2 More than 0.05W min / m cm 2 More than 0.07W min / m cm 2 or more than 0.1 W min / m cm 2 The effective power density is the power density of the plasma output (W / cm 2 ) divided by the conveying speed (m / min). The higher the effective power density, the larger the arithmetic mean height Sa1 of the hard coat layer surface becomes, and accordingly, the adhesion and flex resistance of the antireflection layer formed on the hard coat layer tend to improve.
[0036] On the other hand, if the effective power density is too high, the etching of the binder resin proceeds excessively, which may lead to the roughness of the hard coat layer surface becoming larger and the adhesion being reduced due to the falling off of fine particles. Therefore, the effective power density should be 0.6 W min / m cm 2 Less than 0.43 W min / m cm is preferable.2 Less than or equal to 0.22 W min / m cm 2 It may be the following.
[0037] (Surface shape of hard coat layer) As described above, the hard coat layer 11 contains fine particles (nanoparticles), so that fine irregularities are formed on the surface. In addition, by carrying out a surface treatment such as a plasma treatment on the hard coat layer containing fine particles, the irregularities tend to become large, and the arithmetic mean height Sa1 tends to become large. The arithmetic mean height Sa is calculated according to ISO 25178 from an observation image of 1 μm square using an atomic force microscope (AFM).
[0038] The arithmetic mean height Sa1 of the surface of the hard coat layer 11 is preferably 2.5 nm or more, more preferably 3.0 nm or more, and may be 3.5 nm or more, 4.0 nm or more, 4.5 nm or more, 5.0 nm or more, 5.3 nm or more, or 5.5 nm or more. The larger the arithmetic mean height Sa1 of the hard coat layer 11, the more the adhesion of the antireflection layer tends to improve. In addition, when the arithmetic mean height Sa1 of the hard coat layer that serves as the film formation base of the antireflection layer 5 is large, the antireflection layer 5 is more likely to grow in a columnar shape during sputtering film formation, and the bending resistance tends to improve.
[0039] On the other hand, if the surface irregularities of the hard coat layer become too large, sufficient adhesion may not be achieved. Therefore, the arithmetic mean height Sa1 of the hard coat layer surface is preferably 10 nm or less, more preferably 8.0 nm or less, and even more preferably 7.5 nm or less, and may be 7.0 nm or less or 6.5 nm or less.
[0040] [Anti-reflective film] An antireflection layer 5 is formed on the hard coat layer 11 of the hard coat film 1, optionally with a primer layer 3 interposed therebetween, thereby forming an antireflection film.
[0041] <Primer layer> A primer layer 3 is preferably provided between the hard coat layer 11 and the anti-reflection layer 5 of the hard coat film 1. Examples of materials for the primer layer 3 include metals such as silicon, nickel, chromium, tin, gold, silver, platinum, zinc, titanium, indium, tungsten, aluminum, zirconium, and palladium; alloys of these metals; and oxides, fluorides, sulfides, or nitrides of these metals. Among these, the material for the primer layer is preferably an inorganic oxide, and silicon oxide or indium oxide is particularly preferred. The inorganic oxide constituting the primer layer 3 may be a composite oxide such as indium tin oxide (ITO).
[0042] The thickness of the primer layer 3 is, for example, about 1 to 20 nm, and preferably 3 to 15 nm. If the thickness of the primer layer is within the above range, both the adhesion to the hard coat layer 11 and high light transmittance can be achieved.
[0043] <Anti-reflection layer> The antireflection layer 5 is a laminate of multiple thin films with different refractive indices, and includes at least one high refractive index layer and at least one low refractive index layer. In general, the optical thickness (product of refractive index and film thickness) of the thin films of the antireflection layer is adjusted so that the inverted phases of the incident light and the reflected light cancel each other out. The multi-layer laminate of multiple thin films with different refractive indices can reduce the reflectance in a wide wavelength range of visible light.
[0044] In the antireflection film 101 shown in FIG. 1, the antireflection layer 5 includes four layers, namely, a high refractive index layer 51, a low refractive index layer 52, a high refractive index layer 53, and a low refractive index layer 54, in this order from the hard coat film 1 side. .this The anti-reflection layer 5 , 2 layers High refractive index layer and 2 Layer It is an alternating laminate of low refractive index layers. In order to reduce reflection at the air interface, the thin film 54 provided as the outermost layer (the layer farthest from the hard coat film 1) of the antireflection layer 5 is preferably a low refractive index layer.
[0045] The high refractive index layers 51 and 53 are thin films mainly composed of niobium oxide. Since niobium oxide has a high refractive index, it is possible to efficiently reduce reflected light by laminating it with a low refractive index layer. The refractive index of the high refractive index layer is 2.0 or more, and preferably 2.2 or more. The high refractive index layer may contain a metal oxide other than niobium oxide, but the content of niobium oxide is 90% by weight or more, and preferably 99% by weight or more.
[0046] The thickness of the niobium oxide thin film as the high refractive index layer is preferably 40 nm or less. When the antireflection layer includes a plurality of niobium oxide thin films 51, 53, it is preferable that at least the thickness of the niobium oxide thin film as the high refractive index layer 53 arranged farthest from the hard coat layer is 40 nm or less, and the thickness of all the high refractive index layers (niobium oxide thin films) is 40 nm or less. Since the thickness of the niobium oxide thin film is small, the antireflection layer has excellent bending resistance, and cracks are unlikely to occur in the antireflection layer even if the antireflection film is heated in a bent state. The thickness of the niobium oxide thin film is more preferably 35 nm or less, and may be 32 nm or less or 30 nm or less.
[0047] The density of the niobium oxide thin film is 4.47 g / cm 3 Less than 4.40 g / cm is preferred. 3 Less than 4.35 g / cm is more preferable. 3 Less than or equal to 4.33g / cm 3 In the case where the antireflection layer includes a plurality of niobium oxide thin films 51, 53, it is preferable that at least the niobium oxide thin film serving as the high refractive index layer 53 disposed farthest from the hard coat layer 11 has a film density in the above range, and it is particularly preferable that all of the plurality of niobium oxide thin films 51, 53 have a film density in the above range. The film density of the niobium oxide thin film is generally 4.0 g / cm 3 More than 4.1g / cm 3 or more than 4.2g / cm 3 The film density is a value measured by the Rutherford backscattering (RBS) method, and the density is calculated using the film thickness obtained by observing a cross section.
[0048] The larger the thickness of the niobium oxide thin film, the higher the film density tends to be. As described above, by making the thickness of the niobium oxide thin film 40 nm or less, the film density of the niobium oxide thin film does not become excessively high, and the occurrence of cracks during bending tends to be suppressed. In addition, the larger the surface unevenness of the base of the niobium oxide thin film (the larger Sa), the smaller the film density of the niobium oxide thin film, and the more the occurrence of cracks tends to be suppressed.
[0049] The low refractive index layers 52, 54 have a refractive index of 1.6 or less, preferably 1.5 or less. Examples of low refractive index materials include silicon oxide, titanium nitride, magnesium fluoride, barium fluoride, calcium fluoride, hafnium fluoride, and lanthanum fluoride. Among these, silicon oxide is preferred because it has a low refractive index, high hardness, and can efficiently reduce reflectance by laminating with a niobium oxide high refractive index layer. The low refractive index layers 52, 54 preferably have a silicon oxide content of 90% by weight or more, more preferably 99% by weight or more. The silicon oxide thin film has a film density of 2.20 g / cm. 3 Less than 2.15 g / cm is preferred. 3 Less than or equal to 2.10g / cm 3 It may be the following.
[0050] When the low refractive index layer 54, which is the outermost layer of the antireflection layer, is a silicon oxide layer, its thickness is preferably greater than 85 nm. When the low refractive index layer 54, which is the outermost layer of the antireflection layer 5, is a silicon oxide layer having a thickness greater than 85 nm, the surface hardness of the antireflection layer 5 is increased, the scratch resistance of the antireflection layer is increased, and the abrasion resistance of the antifouling layer 7 formed thereon tends to be improved.
[0051] The thickness of the low refractive index layer 54 is preferably 87 nm or more, more preferably 90 nm or more, and may be 92 nm or more, 94 nm or more, or 95 nm or more. If the thickness of the low refractive index layer 54 is excessively large, it may cause cracks to occur or may be difficult to achieve an optical design with low reflectance and excellent anti-reflection properties. Therefore, the thickness of the low refractive index layer 54 is preferably 200 nm or less, more preferably 150 nm or less, and may be 130 nm or less, 120 nm or less, 115 nm or less, 110 nm or less, or 105 nm or less.
[0052] In one embodiment, the antireflection layer 5 is an alternating laminate of four layers in total, including, from the hard coat film 1 side, a first layer: a niobium oxide thin film as a high refractive index layer 51, a second layer: a silicon oxide thin film as a low refractive index layer 52, a third layer: a niobium oxide thin film as a high refractive index layer 53, and a fourth layer: a silicon oxide thin film as a low refractive index layer 54. In another embodiment, the antireflection layer is an alternating laminate of six layers in total, including three niobium oxide thin films as high refractive index layers and three silicon oxide thin films as low refractive index layers.
[0053] When the antireflection layer 5 is an alternating laminate of four layers in total, consisting of two high refractive index layers 51, 53 and two low refractive index layers 52, 54, an example of a configuration having, from the hard coat film 1 side, a niobium oxide thin film 51 having a thickness of 10 to 20 nm, a silicon oxide thin film 52 having a thickness of 35 to 45 nm, a niobium oxide thin film 53 having a thickness of 25 to 35 nm, and a silicon oxide thin film 54 having a thickness of 90 to 105 nm, in that order.
[0054] (Deposition of primer layer and anti-reflection layer) The method for forming the thin films constituting the primer layer 3 and the anti-reflection layer 5 is not particularly limited, and may be either a wet coating method or a dry coating method. Dry coating methods such as vacuum deposition, CVD, sputtering, and electron beam vapor deposition are preferred because they can form thin films with a uniform thickness. Among these, sputtering is preferred because it has excellent uniformity in thickness and is easy to form dense films.
[0055] In the sputtering method, a thin film can be continuously formed while a long hard coat film is transported in one direction (longitudinal direction) by a roll-to-roll method, so that the productivity of the antireflection film can be improved. In order to improve the productivity of the antireflection film, it is preferable to form all the thin films constituting the antireflection layer 5 by the sputtering method.
[0056] In the sputtering method, the film is formed while introducing an inert gas such as argon, and if necessary, a reactive gas such as oxygen, into the chamber. The formation of the oxide layer by the sputtering method can be carried out by either a method using an oxide target or reactive sputtering using a metal target. In order to form a metal oxide film at a high rate, reactive sputtering using a metal target is preferred.
[0057] The film density of the anti-reflection layer can be adjusted by adjusting the sputtering film formation conditions. For example, when the discharge voltage during sputtering film formation is low, the kinetic energy of the sputtered particles is low and diffusion on the substrate surface is suppressed, which promotes columnar growth and tends to reduce the film density.
[0058] Moreover, when the pressure during film formation is high, the mean free path of the sputtered particles becomes small, and the directivity of the sputtered particles decreases, making them more likely to diffuse, which tends to result in a lower film density. In order to form a niobium oxide thin film with a low film density, the pressure during sputtering film formation is preferably 0.5 Pa or more, and may be 0.55 Pa or more or 0.6 Pa or more. On the other hand, if the film formation pressure is excessively high, the film formation rate is low and productivity is poor, so the film formation pressure is preferably 1.5 Pa or less, and may be 1 Pa or less or 0.9 Pa or less.
[0059] When a thin film is formed by a dry process such as a sputtering method, a thin film (initially formed) is strongly influenced by the base, and as the film thickness increases, it tends to have bulk-like characteristics. In particular, when the hard coat layer 11 has surface irregularities and Sa1 is large, the film density tends to be small in the initial stage of film formation due to the influence of the base irregularities, but as the film thickness increases, it approaches the bulk characteristics and the film density tends to increase.
[0060] When an anti-reflection film including a thick niobium oxide thin film as a high refractive index layer is heated in a bent state with the anti-reflection layer-forming surface facing inward, cracks may occur in the anti-reflection layer. Even when the thickness of a low refractive index layer such as silicon oxide is thick, the occurrence of cracks is suppressed when the thickness of the niobium oxide thin film is small, and therefore the occurrence of cracks is considered to be due to the thick niobium oxide thin film.
[0061] When an anti-reflective film is bent so that the surface on which the anti-reflective layer is formed faces inward, a compressive strain is generated in the anti-reflective layer. When heated in this state, the film substrate expands thermally, and a tensile strain (a force that tries to stretch the film) is generated on the surface of the thin film on the hard coat layer side. When the niobium oxide thin film is thick, the difference in strain between the front and back of the thin film becomes large, and the high film density makes it difficult to relax the strain within the film, which is thought to be one of the causes of cracks in the anti-reflective layer.
[0062] In particular, the niobium oxide thin film 53 on the front side of the antireflection layer 5 is more likely to cause cracks because it is subject to greater strain when bent than the niobium oxide thin film 51 located closer to the hard coat layer 11. In an antireflection film in which niobium oxide thin films as high refractive index layers and silicon oxide thin films as low refractive index layers are alternately laminated, a configuration in which the niobium oxide thin film on the front side of the antireflection layer is made thick is adopted as an optical design for reducing reflectance.
[0063] In contrast, in the present invention, since the thickness of the niobium oxide thin film 53 is 40 nm or less, even if the antireflection film is heated in a bent state, the distortion of the niobium oxide thin film is small, and it is believed that the occurrence of cracks is suppressed. In addition, since the hard coat layer contains fine particles and fine irregularities are formed on the surface of the hard coat layer, columnar growth is promoted when a thin film is formed thereon, and the film density of the niobium oxide thin film is reduced, which is also believed to contribute to the improvement of bending resistance (suppression of cracks).
[0064] The arithmetic mean height Sa of the surface of the antireflection layer 5 is preferably 2.5 nm or more, more preferably 2.8 nm or more, even more preferably 3.0 nm or more, and may be 3.5 nm or more or 4.0 nm or more. The arithmetic mean height Sa of the antireflection layer 5 is preferably 8 nm or less, more preferably 7.5 nm or less, even more preferably 7 nm or less, and may be 6 nm or less or 5.5 nm or less.
[0065] <Anti-stain layer> The antireflection film preferably has an antifouling layer 7 as an outermost layer (topcoat layer) on the antireflection layer 5. By providing the antifouling layer on the outermost surface, the influence of contamination from the external environment (fingerprints, hand dirt, dust, etc.) can be reduced and contaminants attached to the surface can be easily removed.
[0066] In order to maintain the antireflection properties of the antireflection layer 5, it is preferable that the antifouling layer 7 has a small difference in refractive index from the low refractive index layer 54 which is the outermost layer of the antireflection layer 5. The refractive index of the antifouling layer 7 is preferably 1.6 or less, more preferably 1.55 or less.
[0067] The material of the antifouling layer 7 is preferably a fluorine-containing compound. The fluorine-containing compound not only imparts antifouling properties but also contributes to lowering the refractive index. Among them, a fluorine-based polymer containing a perfluoropolyether skeleton is preferable because it has excellent water repellency and can exhibit high antifouling properties. From the viewpoint of enhancing antifouling properties, perfluoropolyether having a main chain structure that can be rigidly arranged in parallel is particularly preferable. As a structural unit of the main chain skeleton of perfluoropolyether, a perfluoroalkylene oxide having 1 to 4 carbon atoms that may have a branch is preferable, and examples thereof include perfluoromethylene oxide (-CF2O-), perfluoroethylene oxide (-CF2CF2O-), perfluoropropylene oxide (-CF2CF2CF2O-), and perfluoroisopropylene oxide (-CF(CF3)CF2O-).
[0068] The antifouling layer 7 can be formed by a wet method such as a reverse coating method, a die coating method, or a gravure coating method, or a dry method such as a CVD method. The thickness of the antifouling layer is usually about 2 to 50 nm. The larger the thickness of the antifouling layer 7, the more the antifouling property tends to improve. In addition, the larger the thickness of the antifouling layer 7, the more the deterioration of the antifouling property due to abrasion tends to be suppressed. The thickness of the antifouling layer is preferably 5 nm or more, more preferably 7 nm or more, and even more preferably 8 nm or more. On the other hand, from the viewpoint of forming a surface shape reflecting the uneven shape of the hard coat layer surface on the surface of the antifouling layer and imparting slipperiness, the thickness of the antifouling layer is preferably 30 nm or less, more preferably 20 nm or less.
[0069] The arithmetic mean height Sa2 of the surface of the antifouling layer 7 is preferably 2.5 nm or more, more preferably 2.8 nm or more, even more preferably 3.0 nm or more, and may be 3.5 nm or more, 3.7 nm or more, 3.9 nm or more, or 4.0 nm or more. The arithmetic mean height Sa2 of the antifouling layer 7 is preferably 8 nm or less, more preferably 7.5 nm or less, even more preferably 7 nm or less, and may be 6.5 nm or less, 6 nm or less, or 5.5 nm or less.
[0070] Since the surface shape of the antifouling layer 7 reflects the surface shapes of the hard coat layer 11 and the antireflection layer 5 provided thereon, the greater the arithmetic mean height Sa1 of the hard coat layer 11, the greater the arithmetic mean height Sa2 of the antifouling layer 7 tends to be. In addition, if the antireflection layer 5 grows columnarly during deposition, the unevenness increases, and the arithmetic mean height Sa2 of the antifouling layer 7 tends to be greater.
[0071] [Usage of anti-reflective film] Antireflection films are used by being disposed on the surface of image display devices such as liquid crystal displays, organic EL displays, etc. For example, by disposing an antireflection film on the viewing side surface of a panel including an image display medium such as a liquid crystal cell or an organic EL cell, the reflection of external light can be reduced and the visibility of the image display device can be improved.
[0072] The antireflection film of the present invention has excellent bending resistance, and even if it is held in a bent state with the antireflection layer-forming surface on the inside, cracks in the antireflection layer are unlikely to occur at the bent portion, and therefore it can be suitably used for a foldable display. EXAMPLES
[0073] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following specific examples.
[0074] [Preparation of hard coat film] An organosilica sol (Nissan Chemical Industries, Ltd., MEK-ST-L; average primary particle diameter of silica particles: 50 nm, particle diameter distribution of silica particles: 30 nm to 130 nm, solid content 30% by weight) was added to and mixed with an ultraviolet-curable acrylic resin composition (manufactured by DIC, product name "GRANDIC PC-1070") so that the amount of silica particles was 40 parts by weight per 100 parts by weight of the resin component, to prepare a composition for forming a hard coat layer.
[0075] The above composition was applied to one side of a triacetyl cellulose film (FUJITAC, manufactured by FUJIFILM Corporation) having a thickness of 80 μm so that the thickness after drying would be 4 μm, and dried at 80° C. for 3 minutes. Thereafter, the composition was exposed to a high-pressure mercury lamp with an accumulated light amount of 200 mJ / cm 2 The coating layer was cured by irradiation with ultraviolet light of 1000 ohms to form a hard coat layer.
[0076] [Example 1] (Surface treatment of hard coat layer) While transporting the hard-coated film in a vacuum atmosphere of 0.5 Pa, the effective power density was 0.014 W min / m cm 2 The surface of the hard coat layer was subjected to argon plasma treatment at 100° C. The arithmetic mean height Sa1 of the hard coat layer after the argon plasma treatment was 4.9 nm.
[0077] (Formation of primer layer) The hard coat film after plasma treatment was introduced into a roll-to-toll sputtering deposition device, and the inside of the chamber was heated to 1×10-4 After reducing the pressure to 10 Pa, argon gas and oxygen gas were introduced at a volume ratio of 98:2 while running the film so that the pressure became 0.5 Pa, and an ITO primer layer with a thickness of 2 nm was formed by sputtering under the conditions of power supply: MFAC, input power: 6 kW. A sintered target containing indium oxide and tin oxide in a weight ratio of 90:10 was used as the target material for forming the ITO primer layer.
[0078] (Formation of anti-reflection layer) Following the formation of the ITO primer layer, the following layers were deposited by reactive sputtering in order to form an anti-reflection layer: 1st layer: 14 nm Nb2O5 layer (refractive index: 2.32), 2nd layer: 40 nm SiO2 layer (refractive index: 1.46), 3rd layer: 29 nm Nb2O5 layer, and 4th layer: 94 nm SiO2 layer. For the deposition of the Nb2O5 layers (first and third layers), a Nb target was used, and argon gas and oxygen gas were introduced in a volume ratio of 90:10 to achieve a pressure of 0.6 Pa, and sputtering was performed at an input power of 30 kW. For the deposition of the SiO2 layers (second and fourth layers), a Si target was used, and argon gas and oxygen gas were introduced in a volume ratio of 70:30 to achieve a pressure of 0.5 Pa, and sputtering was performed at an input power of 20 kW.
[0079] (Formation of antifouling layer) A fluorine-based anti-fouling coating agent ("SHIN-ETSU SUBELYN KY1903-1" manufactured by Shin-Etsu Chemical Co., Ltd.) was dried and solidified and used as the deposition source to form an anti-fouling layer with a thickness of 7 nm on the anti-reflection layer by vacuum deposition at a heating temperature of 260°C.
[0080] [Example 2] The discharge power during plasma treatment was changed to an effective power density of 0.14 W min / m cm 2 Otherwise, the plasma treatment of the hard coat layer, the formation of the antireflection layer, and the formation of the antifouling layer were performed in the same manner as in Example 1 to prepare an antireflection film. The arithmetic mean height Sa1 of the hard coat layer after the argon plasma treatment was 5.7 nm.
[0081] [Comparative Example 1] In forming the antireflection layer, the film thickness of each layer was changed as shown in Table 1. Otherwise, the plasma treatment of the hard coat layer, the formation of the antireflection layer, and the formation of the antifouling layer were carried out in the same manner as in Example 1 to prepare an antireflection film.
[0082] [Comparative Example 2] In forming the antireflection layer, the pressure during deposition of the first and third Nb2O5 layers was changed to 0.4 Pa. Otherwise, the plasma treatment of the hard coat layer, the formation of the antireflection layer, and the formation of the antifouling layer were performed in the same manner as in Example 1 to produce an antireflection film.
[0083] [evaluation] <Surface shape> The surface shapes of the hard coat layer and the anti-reflection film (anti-soiling layer) were measured using an atomic force microscope (AFM) under the conditions below, and the arithmetic mean surface height Sa was measured in accordance with ISO 25178. Equipment: Bruker Dimemsion 3100, Controller: Nanoscope V Measurement mode: Tapping mode Cantilever: Si single crystal Measurement field of view: 1μm×1μm
[0084] <Thin film thickness and film density> The anti-reflection film was processed using a focused ion beam processing device (Hitachi High-Tech "FB2200") to prepare a sample for cross-sectional observation, and the cross-section was observed using a field emission transmission electron microscope (JEOL "JEM-2800") to measure the thickness of the thin film that constitutes the anti-reflection layer. The film density of the thin film that constitutes the anti-reflection layer was measured using the Rutherford backscattering (RBS) method. The film density was calculated using the film thickness obtained from the cross-sectional observation.
[0085] <Flexibility test> The anti-reflection film was cut into a size of 10 mm wide x 100 mm long, curved 180° so that the surface on the anti-reflection layer side was on the inside, and both ends in the length direction were attached to a spacer of thickness D so that the bending radius was constant at D / 2, as shown in Figure 2. The sample was heated in an oven at 100°C for 30 minutes, then removed and visually confirmed for the presence or absence of cracks (opacity of the anti-reflection layer) in the curved portion. Evaluation was performed when the spacer thickness D was 9.2 mm, 7.8 mm, and 5.2 mm (bending radius D / 2 was 4.6 mm, 3.9 mm, and 2.6 mm), and the minimum bending radius at which no cracks occurred was taken as the bending resistance radius.
[0086] Effective power density of plasma treatment of the hard coat layer of the antireflection film of the examples and comparative examples, arithmetic mean height Sa1 after plasma treatment, and film thickness of each layer constituting the antireflection layer , No. Table 1 shows the film density of the three Nb2O5 layers, the arithmetic mean height Sa2 of the antifouling layer surface, and the bending radius of the antireflection film.
[0087] [Table 1]
[0088] In Comparative Example 1, in which the film thickness of the third layer was 95 nm, the bending resistance radius was 4.6 mm, whereas in Examples 1 and 2, in which the film thicknesses of the Nb2O5 layers (first and third layers) were both 40 nm or less, the bending resistance radius was smaller and bending resistance was superior than that of Comparative Example 1. In Examples 1 and 2, the film density of the third layer was smaller than that of Comparative Example 1, and it is believed that the reduction in film density contributes to the improvement of bending resistance.
[0089] In Comparative Example 2, the bending resistance was inferior even though the film thickness of the third layer was equivalent to that of Examples 1 and 2. In Comparative Example 2, the bending resistance was lower than that of Examples 1 and 2 because the pressure during deposition of the Nb2O5 layer was low and the film density was high.
[0090] Comparing Example 1 and Example 2, Example 2, in which the power during the plasma treatment of the hard coat layer was high, had a smaller bending radius and better bending resistance. In Example 2, in which the discharge power was high, the surface unevenness (arithmetic mean height Sa1) of the hard coat layer was large, which promoted columnar growth and made it difficult for the film density to increase, which is thought to contribute to the improvement in bending resistance. [Explanation of symbols]
[0091] 1. Hard coat film 10 Transparent film substrate 11 Hard coat layer 3 Primer layer 5 Anti-reflection layer 51,53 High refractive index layer (niobium oxide layer) 52,54 Low refractive index layer (silicon oxide layer) 7 Antifouling layer 101 Anti-reflective film
Claims
1. A hard coat film having a hard coat layer on one main surface of a foldable, flexible transparent resin film substrate; and An antireflection film comprising an antireflection layer provided on a hard coat layer of the hard coat film, The antireflection layer is composed of a total of four layers including two high refractive index layers and two low refractive index layers alternately laminated together, the high refractive index layer is a thin film containing niobium oxide as a main component, The high refractive index layer disposed farthest from the hard coat layer has a film thickness of 40 nm or less and a film density of 4.47 g / cm 3 is less than Anti-reflective film.
2. 2. The anti-reflection film according to claim 1, wherein each of the two high refractive index layers is a thin film containing niobium oxide as a main component and having a thickness of 40 nm or less.
3. The antireflection film according to claim 1 , wherein the antireflection layer has an arithmetic mean surface height of 2.5 nm or more.
4. The antireflection film according to claim 1 , further comprising a primer layer made of an inorganic oxide between the hard coat layer and the antireflection layer.
5. 3. The anti-reflection film according to claim 1, wherein the hard coat layer contains a binder resin and fine particles having an average primary particle size of 10 to 100 nm.
6. The antireflection film according to claim 1 , further comprising an antifouling layer on the antireflection layer.
7. The anti-reflection film according to claim 6 , wherein the antifouling layer has an arithmetic mean surface height of 2.5 nm or more.
8. A method for producing the anti-reflection film according to claim 1 or 2, comprising the steps of: The method for producing an antireflection film comprises forming the antireflection layer by a sputtering method.
9. The method for producing an antireflection film according to claim 8 , wherein the pressure during sputtering of the high refractive index layer of the antireflection layer is 0.5 Pa or more.
10. 3. An image display device comprising the anti-reflection film according to claim 1 or 2 disposed on a viewing side surface of an image display medium.
Citation Information
Patent Citations
Method for producing evaporable composition, evaporable composition and method for producing optical component with antireflection film
JP2002169002A
Antireflection film and polarizing plate using the same
JP2009047876A
Plastic spectacle lens
JP2009294661A
Antireflection film
JP2011069995A
Sputtering method
JP2012246540A