Molded body
The method addresses the limitations of high-pressure molding by using controlled water content and low-pressure lamination to produce large, uniformly rigid cellulose microfibril-based molded articles efficiently and cost-effectively.
Patent Information
- Application Number
- JP2022160768
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-10-05
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-09-30
AI Technical Summary
Existing methods for manufacturing cellulose microfibril-based materials face challenges in producing large-sized, thick, and uniformly rigid molded articles due to the need for high pressure molding, which limits equipment size and complexity, and results in non-uniform thickness and boundaries between laminated sheets.
A method involving the preparation of microfibrillated cellulose compositions with controlled water content, laminating sheets, and sandwiching them between nonwoven fabrics for heating and pressing at low pressures to form a single plate-shaped molded product, eliminating boundaries and ensuring uniformity in thickness.
This method enables efficient production of large-sized, high-rigidity molded articles with uniform thickness and isotropic properties, reducing the need for large-scale equipment and minimizing material crushing, while using environmentally friendly materials.
Smart Images

Figure 0007569361000002 
Figure 0007569361000003 
Figure 0007569361000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a molded body. [Background technology]
[0002] A technology relating to a material containing cellulose microfibrils is disclosed in Japanese Patent No. 3641690 (Patent Document 1). In addition, a technology relating to a method for producing a molded body of microfibrillated cellulose is disclosed in JP 2018-100466 A (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 3641690 [Patent Document 2] JP 2018-100466 A Summary of the Invention [Problem to be solved by the invention]
[0004] Recently, in order to use materials derived from natural substances such as wood materials in a wide range of applications, materials with high rigidity are required in addition to being lighter than metal materials. When manufacturing materials with high rigidity, it is of course preferable to be able to manufacture them efficiently. In addition, when considering application to various applications, materials with high rigidity are required to have a large planar size. Furthermore, it is desirable for the materials to have a certain degree of thickness in order to obtain rigidity.
[0005] Patent Document 1 discloses a high-strength material that is made of cellulose microfibrils with a solid content of 65-100% by weight and 0-35% by weight of an additive, and has a bending strength of 200 MPa to 400 MPa when measured by a three-point support centrally concentrated load method under conditions of room temperature and relative humidity of 60%. Patent Document 1 discloses a method for producing a material made only of microfibrils, in which a suspension of microfibrils with a solid content of 10% is molded to produce a microfibril sheet, which is then dehydrated until the moisture content of the sheet is about 40%, dried at 70°C for 24 hours, and then heated and pressed at 100 MPa and 150°C for 30 minutes.
[0006] However, in such a manufacturing method, an extremely high pressure of 100 MPa must be applied during molding. In that case, even if it is possible to obtain a small-sized molded body, a large-scale facility is required to obtain a molded body of a certain size. In other words, the size of the molded body obtained with the facility is restricted. Therefore, it is difficult to obtain a molded body of a desired size with such a manufacturing method. In addition, the thickness of the obtained molded body is restricted, for example, to be a thin plate, because the molding is performed under an extremely high pressure. Therefore, it is difficult to obtain a molded body that is thick in the thickness direction.
[0007] Patent Document 2 discloses a method for producing a molded body of microfibrillated cellulose, which comprises preparing a microfibrillated cellulose suspension in which microfibrillated cellulose is dispersed in water, an organic solvent, or a mixed solvent of water and an organic solvent, pre-dehydrating the microfibrillated cellulose suspension in a sealed state, and then molding the suspension under heat and pressure.
[0008] However, in the preliminary dehydration in Patent Document 2, it is necessary to form a sealed space using a bag or a sealing tape. Therefore, from the viewpoint of the complexity of the work, it is difficult to efficiently manufacture a molded body. In addition, in order to obtain a molded body that is thick in the thickness direction, it is possible to stack multiple sheets of the obtained microfibrillated cellulose dispersion and perform hot and pressure molding to obtain a thick molded body. However, with this method, the microfibrillated cellulose does not bond to each other at the boundary portion of each sheet in the thickness direction, and a molded body of uniform material in the thickness direction cannot be obtained. On the other hand, it is also possible to make the thickness of the microfibrillated cellulose dispersion before hot and pressure molding to a certain extent in advance in order to eliminate the occurrence of the boundary between each sheet when stacked. However, the preliminary dehydration to obtain such a thick microfibrillated cellulose dispersion requires a lot of time. From this viewpoint as well, an efficient method for manufacturing a molded body is required.
[0009] An object of the present disclosure is to provide a method for producing a molded article that can efficiently produce a molded article that has high rigidity and is large in size. [Means for solving the problem]
[0010] The method for producing a molded body according to the present disclosure is a method for producing a molded body containing microfibrillated cellulose. The method for producing a molded body includes the steps of preparing a dispersion liquid in which microfibrillated cellulose is dispersed in water at a predetermined concentration, filtering the dispersion liquid to form a sheet-shaped microfibrillated cellulose-containing composition so that the moisture content is 65% by mass or more and 85% by mass or less, preparing a plurality of sheets of the microfibrillated cellulose-containing composition, stacking the plurality of sheets of the microfibrillated cellulose-containing composition in the thickness direction, sandwiching the stacked plurality of sheets of the microfibrillated cellulose-containing composition between nonwoven fabrics arranged on both sides in the thickness direction, and performing heat and pressure molding by heating the plurality of sheets of the microfibrillated cellulose-containing composition sandwiched between the nonwoven fabrics while applying pressure in the thickness direction at a pressure of 0.1 MPa to 4.0 MPa to form a sheet-shaped molded body. Effect of the Invention
[0011] According to the method for producing a molded article having such a configuration, a molded article having high rigidity and large size can be efficiently produced. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a schematic perspective view showing the appearance of a molded plate according to one embodiment of the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an enlarged portion of the molded plate shown in FIG. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a molded article according to another embodiment. [Figure 4] FIG. 4 is a flow chart showing typical production steps in a method for producing a microfibrillated cellulose-containing composition according to one embodiment of the present disclosure. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing the obtained microfibrillated cellulose-containing composition. [Figure 6] FIG. 6 is a flow chart showing typical manufacturing steps in the method for manufacturing the molded article according to the embodiment of the present disclosure shown in FIGS. [Figure 7] FIG. 7 is a schematic cross-sectional view showing each member when hot-press molding is performed to obtain the molded article shown in FIGS. [Figure 8] FIG. 8 is a flow chart showing typical manufacturing steps in the method for manufacturing the molded article shown in FIG. [Figure 9] FIG. 9 is a schematic cross-sectional view showing each member when hot-press molding is performed to obtain the molded body shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Description of the embodiments of the present disclosure] First, the embodiments of the present disclosure will be listed and described. The method for producing a molded body according to the present disclosure is a method for producing a molded body containing microfibrillated cellulose (hereinafter, sometimes simply abbreviated as "MFC (Microfibrillated cellulose)"). The method for producing a molded body includes the steps of preparing a dispersion liquid in which microfibrillated cellulose is dispersed in water at a predetermined concentration, filtering the dispersion liquid so that the moisture content is 65% by mass or more and 85% by mass or less to form a sheet-shaped microfibrillated cellulose-containing composition, preparing multiple sheets of the microfibrillated cellulose-containing composition, stacking the multiple sheets of the microfibrillated cellulose-containing composition in the thickness direction, sandwiching the stacked multiple sheets of the microfibrillated cellulose-containing composition between nonwoven fabrics arranged on both sides in the thickness direction, and performing heat and pressure molding by heating the multiple sheets of the microfibrillated cellulose-containing composition sandwiched between the nonwoven fabrics while applying pressure in the thickness direction at a pressure of 0.1 MPa to 4.0 MPa to form a sheet-shaped molded body.
[0014] The present inventors have investigated a method for producing a molded body having high rigidity from a naturally derived material such as a wood material, which is required to be lighter than a metal material in order to be used in a wide range of applications. First, the inventors considered using microfibrillated cellulose as a naturally derived material such as a wood material. Furthermore, when producing a molded body using microfibrillated cellulose, the inventors have conducted extensive research to avoid high pressure during hot and pressure molding from the viewpoint of efficient production of large molded bodies, and to obtain a molded body having high rigidity, and have completed the present invention.
[0015] The method for producing a molded article according to the present disclosure includes a step of forming a sheet-shaped microfibrillated cellulose-containing composition by filtering the dispersion so that the moisture content is 65% by mass or more and 85% by mass or less. Therefore, when forming the sheet-shaped microfibrillated cellulose-containing composition, it is not necessary to prepare a bag or a sealing tape to provide a sealed space. Therefore, the microfibrillated cellulose-containing composition can be produced efficiently. In other words, when producing multiple sheets of the microfibrillated cellulose-containing composition, it can be produced in a short time with little effort.
[0016] As described above, the microfibrillated cellulose-containing composition obtained by filtration has a relatively rough surface. The present inventors have found that the surface properties of a sheet-shaped microfibrillated cellulose-containing composition from which water has been removed to a certain extent by filtration become like this. The present inventors have further found that, for a molded body obtained by stacking multiple sheets of such a microfibrillated cellulose-containing composition and hot-pressing molding, the microfibrillated cellulose located on the surface side of the multiple stacked sheets of microfibrillated cellulose-containing composition can be moderately entangled in the thickness direction to eliminate the boundary in the thickness direction, and the material in the thickness direction can be made uniform. Thus, by configuring in this way, a molded body of any thickness can be obtained. In addition, the microfibrillated cellulose-containing composition obtained by filtration can densely entangle the microfibrillated cellulose. Therefore, the rigidity of the obtained molded body can be increased. In addition, the molded body obtained in this way has isotropy because the microfibrillated cellulose is not aligned in one direction but is randomly arranged. That is, for example, when the molded body is in the shape of a plate, the rigidity in both the vertical direction and the horizontal direction can be made large.
[0017] In the hot and pressure molding of a plurality of laminated sheets of the microfibrillated cellulose-containing composition, a plate-shaped molded body can be obtained by pressing at a pressure of 0.1 MPa to 4.0 MPa. Therefore, since molding can be performed at a relatively low pressure during hot and pressure molding, large-scale equipment is not required, and the size of the molded body is less subject to restrictions imposed by the equipment. In addition, it is possible to prevent the material from being crushed in the thickness direction by high pressure. Therefore, a molded body of a certain size can be manufactured with a relatively simple equipment configuration. In addition, it is easy to obtain a laminate of the desired thickness.
[0018] As described above, according to the above-mentioned method for producing a molded article, a molded article having high rigidity and large size can be efficiently produced.
[0019] The method for producing the molded body may further include a step of preparing a sheet-shaped pulp-containing composition composed of water and pulp, and a step of sandwiching the pulp-containing composition between a plurality of sheets of the microfibrillated cellulose-containing composition. Since pulp is a versatile material, the pulp-containing composition having the above-mentioned structure can be produced more inexpensively than the microfibrillated cellulose-containing composition. Since layers composed of microfibrillated cellulose are disposed on both sides of the thickness direction of the obtained molded body, the decrease in rigidity can be suppressed. Therefore, according to such a method for producing a molded body, a molded body having high rigidity and a desired thickness can be obtained inexpensively.
[0020] In the above-mentioned method for producing a molded article, the step of forming the microfibrillated cellulose-containing composition may include a step of suction filtering the dispersion. In this way, the filtration can be performed in a short time. Therefore, the molded article can be produced more efficiently.
[0021] In the above-mentioned method for producing a molded article, the nonwoven fabric may be a glass nonwoven fabric. During the heating and pressurizing of a multi-layered microfibrillated cellulose-containing composition, the water in the microfibrillated cellulose-containing composition is pressurized and moves mainly in the thickness direction, and then is discharged from the side of the nonwoven fabric arranged on both sides in the thickness direction. Here, by using a glass nonwoven fabric using glass fibers as the nonwoven fabric, a water passage in the nonwoven fabric can be sufficiently secured, and water can be discharged smoothly. Therefore, a molded article having high rigidity and large size can be produced more efficiently.
[0022] In the above-mentioned method for producing a molded article, the step of hot-press molding may include a step of heating a plurality of laminated sheets of microfibrillated cellulose-containing composition to a temperature of 100° C. to 150° C. and maintaining the temperature at a pressure of 0.1 MPa to 4.0 MPa for a period of 30 minutes to 120 minutes. By performing hot-press molding within the above-mentioned temperature range, pressure range and time range during hot-press molding of a plurality of laminated sheets of microfibrillated cellulose-containing composition, a molded article having high rigidity and large size can be produced more reliably and efficiently.
[0023] In the above-mentioned method for producing a molded article, the step of performing hot and pressure molding may include a step of applying pressure by gradually increasing the pressure from 0.1 MPa to 4.0 MPa. In this way, deformation of the molded article during hot and pressure molding can be suppressed, and water in the microfibrillated cellulose-containing composition can be efficiently removed. Therefore, a molded article having high rigidity and large size can be produced more reliably and efficiently.
[0024] The molded article according to the present disclosure is made of only microfibrillated cellulose and has a flexural modulus of 11.0 GPa or more. Since such a molded article is made of only microfibrillated cellulose and does not contain resins, metal materials, etc., it is good from the viewpoint of the global environment. In addition, since the flexural modulus is 11.0 GPa or more, it can be effectively used as a member that requires rigidity, such as an electronic material or a building material.
[0025] The molded body according to the present disclosure is plate-shaped and includes a first layer made of only microfibrillated cellulose, a second layer made of only pulp and disposed on the first layer, and a third layer made of only microfibrillated cellulose and disposed on the second layer on the opposite side of the first layer in the thickness direction, and has a flexural modulus of 11.0 GPa or more. Such a molded body has a configuration in which the second layer made of only pulp is sandwiched between the first and third layers made of only microfibrillated cellulose. The second layer made of only pulp can be manufactured relatively inexpensively. Therefore, the molded body can be manufactured inexpensively while having a certain thickness as a whole. In this case, the first and third layers made of only microfibrillated cellulose are disposed on both sides of the second layer made of only pulp in the thickness direction. The first and third layers are homogeneous in the thickness direction and have high rigidity. Therefore, the flexural modulus is set to 11.0 GPa or more, and the rigidity of the molded body can be increased. Therefore, such a molded body can also be effectively used in cases where a certain degree of thickness and rigidity are required.
[0026] The molded body may be plate-shaped and have a thickness of 2.0 mm or more. Since such a molded body has a thickness of 2.0 mm or more, it can be effectively used when a certain thickness is required as a member requiring rigidity. Here, when obtaining a molded body having a certain thickness, a plurality of thin plate-shaped molded bodies obtained by the technology disclosed in Patent Document 1 or the technology disclosed in Patent Document 2 may be stacked and bonded to each other, for example, by an adhesive. However, such a configuration requires a lot of effort for bonding in the manufacturing process. In addition, many boundaries between the adhesive and the molded body are generated, making it difficult to ensure the homogeneity of the material in the thickness direction. Here, according to the molded body of the present disclosure, the effort for bonding can be simplified and the homogeneity of the material in the thickness direction can be ensured. In addition, in the molded body of the present disclosure composed only of the above-mentioned microfibrillated cellulose, the material in the thickness direction is uniform, so the risk of cracking, chipping, peeling, etc. at the boundary portion is reduced compared to a molded body obtained by stacking and bonding a plurality of sheets. Therefore, it can be effectively used as a member requiring rigidity.
[0027] In the above molded body, the density is 1.30 g / cm 3 More than 1.55g / cm 3 Such a molded article can be more reliably made to have high rigidity.
[0028] In the above molded article, the fiber diameter of the microfibrillated cellulose may be 10 nm or more and 1000 nm or less. By doing so, the microfibrillated cellulose in the molded article can be more densely entangled, and therefore the rigidity can be increased.
[0029] A method for producing a microfibrillated cellulose-containing composition according to the present disclosure includes the steps of preparing a dispersion in which microfibrillated cellulose is dispersed in water at a predetermined concentration, and filtering the dispersion to form a sheet-like microfibrillated cellulose-containing composition having a water content of 65% by mass or more and 85% by mass or less.
[0030] According to such a method for producing a microfibrillated cellulose-containing composition, when forming a sheet-like microfibrillated cellulose-containing composition, it is not necessary to prepare a bag or a sealing tape to provide a sealed space. Therefore, the microfibrillated cellulose-containing composition can be produced efficiently. That is, when producing multiple sheets of the microfibrillated cellulose-containing composition, it can be produced in a short time with little effort. Furthermore, when multiple sheets of the microfibrillated cellulose-containing composition obtained in this manner are laminated and subjected to heat and pressure molding to form a molded product, the boundaries in the thickness direction of the molded product are eliminated, and the material in the thickness direction can be made uniform. Therefore, a molded product with high rigidity can be obtained.
[0031] In the method for producing a microfibrillated cellulose-containing composition, the step of preparing a dispersion may include a step of preparing a dispersion in which microfibrillated cellulose is dispersed in water at a concentration of 10% by mass, which makes it possible to more efficiently obtain a microfibrillated cellulose-containing composition.
[0032] [Details of the embodiment of the present disclosure] Hereinafter, embodiments of the present disclosure will be described. In the following drawings, the same or corresponding parts are designated by the same reference numerals, and description thereof will not be repeated.
[0033] Fig. 1 is a schematic perspective view showing the appearance of a molded plate according to an embodiment of the present disclosure. Fig. 2 is a schematic cross-sectional view showing an enlarged portion of the molded plate shown in Fig. 1. Fig. 2 is a cross-sectional view taken along the line II-II shown in Fig. 1.
[0034] 1 and 2, the molded body 11 according to one embodiment of the present invention is a flat plate with the thickness direction being the Z direction. The molded body 11 is rectangular with the Y direction as the longitudinal direction and the X direction as the short side direction when viewed in the thickness direction. The thickness S1 of the molded body 11, i.e., the length from one surface 13a to the other surface 13b in the Z direction of the molded body 11, the length S2 in the X direction and the length S3 in the Y direction are arbitrarily determined depending on the application, the location of use, etc. Specifically, the length S2 in the X direction is preferably 100 mm or more and 1200 mm or less, and the length S3 in the Y direction is preferably 100 mm or more and 2400 mm or less. Of course, the molded body 11 of such a size can also be efficiently manufactured using, for example, the manufacturing method of the molded body 11 described later.
[0035] The thickness S1 of the molded body 11 is 1.0 mm or more and 100.0 mm or less. Specifically, the thickness S1 of the molded body 11 is, for example, 2.0 mm. It is more preferable to use the thickness S1 of the molded body 11 of, for example, 2.0 mm or more. It is also more preferable to use the thickness S1 of the molded body 11 of, for example, 4.0 mm or more and 100.0 mm or less. Of course, the molded body 11 having such a thickness can also be efficiently manufactured by using, for example, the manufacturing method of the molded body 11 described later.
[0036] The molded body 11 is composed only of the microfibrillated cellulose 12. Specifically, the molded body 11 is in the form of a flat plate in which the microfibrillated cellulose 12 is aggregated.
[0037] The microfibrillated cellulose 12 is also called cellulose nanofiber, and is a microfibrillated cellulose fiber. The raw material of the microfibrillated cellulose 12 may be, for example, a plant-derived material, an animal-derived material, or a microorganism-derived material. Furthermore, a chitin-derived material or a chitosan-derived material may be used.
[0038] The fiber diameter of the microfibrillated cellulose 12 may be 10 nm or more and 50 nm or less. This allows the microfibrillated cellulose 12 to be more densely entangled within the molded body 11. This allows the rigidity to be increased.
[0039] The flexural modulus of the molded body 11 is 11.0 GPa or more. Such a molded body 11 can be applied to various applications requiring high rigidity. The flexural modulus of the molded body 11 is measured by a method conforming to JIS-K6911. In the molded body 11, the microfibrillated cellulose 12 is not aligned in one direction but is arranged randomly. Therefore, the molded body 11 has isotropy. That is, for example, when the molded body 11 is formed into a plate shape, the rigidity in the vertical direction (X direction) and the rigidity in the horizontal direction (Y direction) are both high.
[0040] In the above molded body 11, the density is 1.30 g / cm 3 More than 1.55g / cm 3 Such a molded body 11 can be more reliably made to have high rigidity. 3 More than 1.55g / cm 3 By setting it to the following, it is possible to more reliably achieve high rigidity.
[0041] The molded article may be in the form of a plate, and may include a first layer made of only microfibrillated cellulose, a second layer made of only pulp and disposed on the first layer, and a third layer made of only microfibrillated cellulose and disposed on the second layer on the opposite side in the thickness direction to the side on which the first layer is disposed. The molded article may have a flexural modulus of 11.0 GPa or more.
[0042] FIG. 3 is a schematic cross-sectional view showing a molded body according to another embodiment. Referring to FIG. 3, the molded body 21 includes a first layer 22, a second layer 23, and a third layer 24. The first layer 22 and the third layer 24 are composed only of microfibrillated cellulose. The second layer 23 is composed only of pulp. The second layer 23 is disposed on the first layer 22. Specifically, one surface 25a in the thickness direction of the first layer 22 is exposed, and the other surface 25b in the thickness direction of the first layer 22 is in contact with one surface 26a in the thickness direction of the second layer 23. In addition, one surface 27a in the thickness direction of the third layer 24 is in contact with the other surface 26b in the thickness direction of the second layer 23, and the other surface 27b in the thickness direction of the third layer 24 is exposed. The thickness S4 of the molded body 21, that is, the length in the Z direction from one surface 25a of the first layer 22 to the other surface 27b of the third layer 24, can be arbitrarily changed depending on, for example, the required thickness of the molded body.
[0043] The molded body 21 has a structure in which a second layer 23 made of only pulp is sandwiched between a first layer 22 and a third layer 24 made of only microfibrillated cellulose. The second layer 23 made of only pulp can be manufactured relatively inexpensively. Therefore, the molded body 21 as a whole can be manufactured inexpensively while having a certain degree of thickness. In this case, the first layer 22 and the third layer 24 made of only microfibrillated cellulose are disposed on both sides in the thickness direction of the second layer 23 made of only pulp. The first layer 22 and the third layer 24 are homogeneous in the thickness direction and have high rigidity. Therefore, the rigidity of the molded body 21 can be increased by setting the flexural modulus to 11.0 GPa or more. Therefore, such a molded body 21 can be effectively used when a certain degree of thickness and high rigidity are required.
[0044] Here, the molded article shown in Figures 1 and 2 can be produced, for example, by using a microfibrillated cellulose-containing composition having the following configuration: Figure 4 is a flowchart showing typical production steps in a method for producing a microfibrillated cellulose-containing composition according to one embodiment of the present disclosure.
[0045] Referring to FIG. 4, first, a dispersion liquid in which microfibrillated cellulose is dispersed in water at a predetermined concentration is prepared (step S11 in FIG. 4, hereinafter, "step" is omitted). Next, the dispersion liquid is diluted with water to a desired concentration of microfibrillated cellulose (S12). Specifically, for example, the dispersion liquid is diluted so that the concentration of microfibrillated cellulose is about 1% by mass. Next, the dispersion liquid is molded into a sheet while being dehydrated (S13). In this case, the dispersion liquid is filtered and molded into a sheet. In this way, the dispersion liquid is filtered so that the moisture content is 65% by mass or more and 85% by mass or less to form a sheet-like microfibrillated cellulose-containing composition. In addition to natural filtration, the filtration may be performed by pressure filtration in which filtration is performed by applying pressure, or by vacuum filtration or centrifugal filtration, or by suction filtration. That is, the step of forming the microfibrillated cellulose-containing composition may include a step of suction filtration of the dispersion liquid. By doing so, the filtration can be performed in a short time. Therefore, a molded body can be produced more efficiently.
[0046] Thus, the method for producing a microfibrillated cellulose-containing composition according to the present disclosure includes a step of forming a sheet-shaped microfibrillated cellulose-containing composition by filtering the dispersion so that the moisture content is 65% by mass or more and 85% by mass or less. Therefore, when forming the sheet-shaped microfibrillated cellulose-containing composition, it is not necessary to prepare a bag or sealing tape to provide a sealed space. Therefore, the microfibrillated cellulose-containing composition can be produced efficiently. In other words, when producing multiple sheets of the microfibrillated cellulose-containing composition, it can be produced in a short time with little effort.
[0047] Fig. 5 is a schematic cross-sectional view showing the obtained microfibrillated cellulose-containing composition. Referring to Fig. 5, the microfibrillated cellulose-containing composition 14 contains microfibrillated cellulose 12 and water 15. The microfibrillated cellulose-containing composition 14 is in a state in which the water 15 is dispersed and mixed in a large amount of aggregated microfibrillated cellulose 12. The microfibrillated cellulose-containing composition 14 is in a state similar to so-called sake lees. The microfibrillated cellulose-containing composition 14 is in a sheet form. The thickness S5 of the microfibrillated cellulose-containing composition 14, i.e., the length from one surface 16a to the other surface 16b of the microfibrillated cellulose-containing composition 14, is, for example, 0.5 mm or more and 2.5 mm or less.
[0048] Next, an outline of a method for producing a molded article according to an embodiment of the present disclosure will be described. Fig. 6 is a flow chart showing typical steps in the method for producing a molded article according to an embodiment of the present disclosure shown in Figs.
[0049] Referring to Fig. 6, a plurality of sheets of the microfibrillated cellulose-containing composition obtained by the above-mentioned production method shown in Fig. 4 are prepared (S21). In this case, sheets having the same length in the X direction and the Y direction are prepared. Then, the prepared plurality of sheets of the microfibrillated cellulose-containing composition are laminated (S22). That is, the plurality of sheets of the microfibrillated cellulose-containing composition are stacked in the thickness direction.
[0050] Thereafter, the laminated multiple sheets of microfibrillated cellulose-containing composition are sandwiched between nonwoven fabrics arranged on both sides in the thickness direction (S23). In this case, glass nonwoven fabric is used as the nonwoven fabric. Next, the multiple sheets of microfibrillated cellulose-containing composition sandwiched between the nonwoven fabrics are heated and pressed in the thickness direction at a pressure of 0.1 MPa to 4.0 MPa, and then subjected to heat and pressure molding to form a sheet-like molded product (S24). Specifically, stainless steel metal plates are placed on both sides of the glass nonwoven fabric, and pressure is applied in the thickness direction.
[0051] Fig. 7 is a schematic cross-sectional view showing each member when performing one-step heating and press molding to obtain the molded body 11 shown in Fig. 1 and Fig. 2. Referring to Fig. 7, glass nonwoven fabrics 32a and 32b are arranged on both sides in the thickness direction of four laminated microfibrillated cellulose-containing compositions 31a, 31b, 31c, and 31d. That is, the laminated microfibrillated cellulose-containing compositions 31a, 31b, 31c, and 31d are sandwiched between the glass nonwoven fabrics 32a and 32b. Furthermore, metal plates 33a and 33b made of stainless steel or the like are arranged on both sides in the thickness direction of the glass nonwoven fabrics 32a and 32b. The microfibrillated cellulose-containing compositions 31a, 31b, 31c, and 31d laminated via the metal plates 33a and 33b are heated and pressurized in the direction indicated by the arrow D1 to be molded. During the hot and pressure molding, water contained in the microfibrillated cellulose-containing compositions 31a, 31b, 31c, and 31d first moves in the thickness direction as shown by the arrow D2, and then is discharged from the side of the glass nonwoven fabrics 32a and 32b.
[0052] In this manner, the microfibrillated cellulose-containing compositions 31a, 31b, 31c, and 31d are heated while being pressed in the thickness direction at a pressure of 0.1 MPa or more and 4.0 MPa or less to form a plate-like molded body as shown in Figures 1 and 2.
[0053] According to the above-mentioned manufacturing method of the molded body, the microfibrillated cellulose-containing compositions 31a, 31b, 31c, 31d obtained by filtration as described above have a relatively rough surface. In the molded body obtained by stacking multiple sheets of the microfibrillated cellulose-containing compositions 31a, 31b, 31c, 31d and molding them under heat and pressure, the microfibrillated cellulose-containing compositions 31a, 31b, 31c, 31d located on the surface side of the stacked multiple sheets of the microfibrillated cellulose-containing compositions 31a, 31b, 31c, 31d are appropriately entangled in the thickness direction to eliminate the boundary in the thickness direction, and the material in the thickness direction can be made uniform. Therefore, by configuring in this way, a molded body of any thickness can be obtained. In addition, the microfibrillated cellulose-containing compositions 31a, 31b, 31c, 31d obtained by filtration can densely entangle the microfibrillated cellulose. Therefore, the rigidity of the obtained molded body can be increased. The obtained molded body has isotropy. That is, the rigidity in both the vertical and horizontal directions can be increased. Therefore, for example, when manufacturing by cutting out electronic materials, there is no need to worry about the directionality, and the molded body is extremely valuable.
[0054] In the heat and pressure molding of the laminated microfibrillated cellulose-containing compositions 31a, 31b, 31c, and 31d, a plate-shaped molded body is obtained by pressing at a pressure of 0.1 MPa to 4.0 MPa. Therefore, since molding can be performed at a relatively low pressure during heat and pressure molding, large-scale equipment is not required, and the size of the molded body is less subject to restrictions due to the equipment. In addition, it is possible to prevent the material from being crushed in the thickness direction due to high pressure. Therefore, a large-sized molded body can be manufactured with a relatively simple equipment configuration. In addition, it is easy to obtain a laminate of the desired thickness.
[0055] As described above, according to the above-mentioned method for producing a molded article, a molded article having high rigidity and large size can be efficiently produced.
[0056] Next, there will be described a method for producing the molded article shown in Fig. 3. Fig. 8 is a flow chart showing typical steps in the method for producing the molded article shown in Fig. 3.
[0057] Referring to FIG. 8, a plurality of sheets of the microfibrillated cellulose-containing composition obtained by the above-mentioned manufacturing method shown in FIG. 4 are prepared (S31). A sheet-shaped pulp-containing composition composed of water and pulp is also prepared (S32). The prepared plurality of sheets of the microfibrillated cellulose-containing composition are then stacked to sandwich the pulp-containing composition (S33). That is, in the manufacturing method of the molded body of the present disclosure, the pulp-containing composition is sandwiched between the plurality of sheets of the microfibrillated cellulose-containing composition before the step of sandwiching the stacked plurality of sheets of the microfibrillated cellulose-containing composition between the nonwoven fabrics arranged on both sides in the thickness direction. Specifically, the plurality of sheets of the microfibrillated cellulose-containing composition are stacked so as to sandwich the pulp-containing composition between them.
[0058] Thereafter, the laminated multiple sheets of the microfibrillated cellulose-containing composition and the pulp-containing composition are sandwiched between nonwoven fabrics arranged on both sides in the thickness direction (S34). Next, the multiple sheets of the microfibrillated cellulose-containing composition and the pulp-containing composition sandwiched between the nonwoven fabrics are heated while being pressed in the thickness direction at a pressure of 0.1 MPa to 4.0 MPa, and then subjected to hot-press molding to form a sheet of molded body 21 (S35).
[0059] Fig. 9 is a schematic cross-sectional view showing each member when performing hot and pressure molding to obtain the molded body shown in Fig. 3. Referring to Fig. 9, one sheet of pulp-containing composition 34a is sandwiched between two sheets of laminated microfibrillated cellulose-containing composition 31a, 31b and two sheets of laminated microfibrillated cellulose-containing composition 31c, 31d. Then, glass nonwoven fabrics 32a, 32b are arranged on both sides in the thickness direction. That is, the microfibrillated cellulose-containing composition 31a, 31b, the pulp-containing composition 34a, and the microfibrillated cellulose-containing composition 31c, 31d laminated by the glass nonwoven fabrics 32a, 32b are sandwiched. Then, stainless steel metal plates 33a, 33b are arranged on both sides in the thickness direction of the glass nonwoven fabrics 32a, 32b. The microfibrillated cellulose-containing compositions 31a, 31b, pulp-containing composition 34a, and microfibrillated cellulose-containing compositions 31c, 31d, which are stacked via the metal plates 33a, 33b, are heated and pressurized in the direction indicated by the arrow D1 to be molded. During the heat and pressure molding, water contained in the microfibrillated cellulose-containing compositions 31a, 31b, pulp-containing composition 34a, and microfibrillated cellulose-containing compositions 31c, 31d first moves in the thickness direction, mainly as indicated by the arrow D2. Then, the water is discharged from the side of the glass nonwoven fabrics 32a, 32b.
[0060] In this manner, the microfibrillated cellulose-containing compositions 31a, 31b, the pulp-containing composition 34a, and the microfibrillated cellulose-containing compositions 31c, 31d are heated while being pressed in the thickness direction at a pressure of 0.1 MPa or more and 4.0 MPa or less to form a plate-like molded body as shown in FIG. 3.
[0061] Such a molded body has a structure in which a second layer made of only pulp is sandwiched between a first layer and a third layer made of only microfibrillated cellulose. The second layer made of only pulp can be manufactured relatively inexpensively. Therefore, the molded body can be manufactured inexpensively while having a certain thickness as a whole. In this case, the first layer and the third layer made of only microfibrillated cellulose are disposed on both sides in the thickness direction of the second layer made of only pulp. The first layer and the third layer are homogeneous in the thickness direction and have high rigidity. Therefore, the rigidity of the molded body can be increased by setting the flexural modulus to 11.0 GPa or more. Therefore, such a molded body can be effectively used when a certain thickness and high rigidity are required.
[0062] In addition, since pulp is a versatile material, the pulp-containing composition 34a can be manufactured more inexpensively than the microfibrillated cellulose-containing compositions 31a, 31b, 31c, and 31d. Since layers made of microfibrillated cellulose are disposed on both sides of the thickness of the obtained molded body 21, it is possible to prevent the rigidity from decreasing. Therefore, according to this method for manufacturing a molded body, a molded body having a high rigidity and a desired thickness can be obtained inexpensively.
[0063] In the above embodiment, the fiber diameter of the microfibrillated cellulose is 10 nm or more and 1000 nm or less, but this is not limited, and fiber diameters of several nm to several thousand nm can be used depending on the application, cost, etc.
[0064] In the above embodiment, a glass nonwoven fabric is used as the nonwoven fabric, but the present invention is not limited to this, and a nonwoven fabric made of organic fibers or a nonwoven fabric made of inorganic fibers may be used. Of course, the nonwoven fabrics arranged on both sides may not be the same, but different ones may be used. EXAMPLES
[0065] Molded articles were produced according to the compositions and methods shown in Samples 1 to 13, and evaluation tests were carried out. The evaluation results are shown in Table 1. It should be noted that molded articles could not be obtained for Samples 11, 12, and 13, so they are not shown in Table 1. Samples 1 to 8 are within the scope of the present invention. Samples 9 to 13 are outside the scope of the present invention.
[0066] (Sample 1) Microfibrillated cellulose ("BiNFi-S (Binfis) BMa10010" manufactured by Sugino Machine Corp.: fiber diameter 10 nm to 50 nm or less) dispersed in water at a concentration of 10% by mass was prepared. The mixture was then diluted with water to 1% by mass, and the water was then removed by filtration so that the water content was 65% to 85% by mass, to obtain a sheet-like MFC-containing composition with a thickness of 2.5 mm. Here, the water was removed by suction filtration. In this way, two sheets of MFC-containing composition were produced and laminated. Thereafter, the basis weight was 47 g / cm. 2 Two sheets of glass nonwoven fabric were prepared, the laminated MFC-containing composition was sandwiched between them, and the laminate was further sandwiched between two stainless steel metal plates. Then, heat and pressure molding was performed at 150°C for 1 hour. The pressure was increased stepwise from 0.5 MPa, and the final pressure was 4.0 MPa. The thickness of the obtained molded body was 1.0 mm. The flexural modulus, flexural strength, and density of this molded body were measured. The measurements were performed in accordance with JIS-K6911. The same was true for the measurements of the following samples.
[0067] (Sample 2) A molded body according to Sample 2 was obtained in the same manner as Sample 1, except that four sheets of the MFC-containing composition obtained by the manufacturing method shown in Fig. 3 were laminated together. The thickness of the obtained laminate was 2.0 mm.
[0068] (Sample 3) A molded article according to Sample 3 was obtained in the same manner as Sample 1, except that eight sheets of the MFC-containing composition obtained by the manufacturing method shown in Fig. 3 were laminated together. The thickness of the obtained laminate was 4.0 mm.
[0069] (Sample 4) A molded product according to Sample 4 was obtained in the same manner as Sample 1, except that 20 sheets of the MFC-containing composition obtained by the manufacturing method shown in Fig. 3 were laminated together. The thickness of the obtained laminate was 10.0 mm.
[0070] (Sample 5) A molded product according to Sample 5 was obtained in the same manner as Sample 1, except that 100 sheets of the MFC-containing composition obtained by the production method shown in Fig. 3 were laminated. The thickness of the obtained laminate was 50.0 mm.
[0071] (Sample 6) A molded article according to Sample 6 was obtained in the same manner as Sample 1, except that 200 sheets of the MFC-containing composition obtained by the production method shown in Fig. 3 were laminated. The thickness of the obtained laminate was 100.0 mm.
[0072] (Sample 7) A molded product according to Sample 7 was obtained in the same manner as Sample 1, except that the MFC was changed to MFC (Cerish KY-100G manufactured by Daicel FineChem Corporation, fiber diameter: 0.01 to 1 μm). The thickness of the obtained laminate was 100.0 mm.
[0073] (Sample 8) MFC ("BiNFi-S BMa10010" manufactured by Sugino Machine Co., Ltd.) dispersed in water at a concentration of 10% by mass was prepared. Then, it was diluted with water to 1% by mass, and then the water was removed by filtration so that the moisture content was 65% by mass or more and 85% by mass or less, and a sheet-shaped MFC-containing composition having a thickness of 1.2 mm was obtained. Here, the water was removed by suction filtration. In this way, two sheets of MFC-containing composition were manufactured. In addition, as pulp, a dispersion liquid was prepared by disintegrating commercially available toilet paper (for example, Napia roll made of 100% fresh pulp manufactured by Oji Nepia Co., Ltd.) in water at a concentration of 10% by mass. Then, it was diluted with water to 1% by mass, and then the water was removed by filtration so that the moisture content was 65% by mass or more and 85% by mass or less, and a sheet-shaped pulp-containing composition having a thickness of 2.5 mm was obtained. Here, the water was removed by suction filtration. The obtained pulp-containing composition was sandwiched between two sheets of the obtained MFC-containing composition, and then, a sheet-shaped pulp-containing composition having a basis weight of 47 g / cm was obtained. 2 The MFC-containing composition was sandwiched between two sheets of glass nonwoven fabric, and the resulting mixture was then sandwiched between two stainless steel metal plates. Then, the mixture was heated and pressed at 150°C for 1 hour. The pressure was gradually increased from 0.5 MPa, and the final pressure was 4.0 MPa. The thickness of the resulting molded product was 1.0 mm.
[0074] (Sample 9) Using MFC ("BiNFi-S BMa10010" manufactured by Sugino Machine Corp.) dispersed in water at a concentration of 10% by mass, a molded body having a thickness of 1.0 to 4.0 mm was obtained by integral molding based on the manufacturing method described in Patent Document 2.
[0075] (Sample 10) A molded body according to Sample 10 was obtained in the same manner as Sample 9, except that the MFC in Sample 9 was changed to MFC ("Cerish KY-100G" manufactured by Daicel FineChem Corporation). The thickness of the obtained laminate was 1.0 mm.
[0076] (Sample 11) The same procedure was followed as for Sample 1, except that the laminated MFC-containing composition was not sandwiched between glass nonwoven fabrics during production. In this case, the interfaces between the laminated MFC-containing compositions were not bonded, and a molded product could not be obtained.
[0077] (Sample 12) MFC ("BiNFi-S BMa10010" manufactured by Sugino Machine Co., Ltd.: fiber diameter 10 nm to 50 nm or less) dispersed in water at a concentration of 10% by mass was prepared. Then, a sheet-like MFC-containing composition was molded in this state (without dehydration) to a thickness of 5.0 mm, in the same manner as in Sample 1. In this case, the MFC flowed when pressurized, and a molded body of the desired thickness could not be obtained.
[0078] (Sample 13) MFC ("BiNFi-S BMa10010" manufactured by Sugino Machine Co., Ltd.: fiber diameter 10 nm to 50 nm or less) dispersed in water at a concentration of 10% by mass was prepared. The mixture was then diluted with water to 1% by mass, and the water was then removed by filtration so that the water content was less than 65% by mass. The same procedure was followed as for Sample 1, except that a sheet-like MFC-containing composition was used, which was molded to a thickness of 2.0 mm. In this case, the interfaces between the laminated MFC-containing compositions did not bond, and a molded product could not be obtained.
[0079] [Table 1]
[0080] Referring to Table 1, Samples 1, 2, 3, 4, 5 and 6 have a flexural modulus of elasticity of 12.8 GPa, which is a very high value. In other words, the molded bodies have extremely high rigidity. Sample 2 has a thickness of 2.0 mm, and Sample 3 has a thickness of 4.0 mm. Sample 4 has a thickness of 10.0 mm, which is sufficiently thick. Sample 5 has a thickness of 50.0 mm, which is very thick. Sample 6 has a thickness of 100.0 mm, which is extremely thick. Samples 1 to 6 have a density of 1.40 g / cm 3 The bending strength of Samples 1 to 6 was 210 MPa, which is also a high value in terms of strength.
[0081] Sample 7 had a flexural modulus of 11.9 GPa, which is also a considerably high value, and was a molded product with high rigidity. Sample 7 had a density of 1.35 g / cm 3 The bending strength of Sample 7 was 170 MPa, which is a high value in terms of strength.
[0082] Furthermore, sample 8 also has a high flexural modulus of 12.0 GPa, making it a material with high rigidity. Sample 8 has a density of 1.30 g / cm 3 The bending strength of sample 8 was 160 MPa, which is a high value in terms of strength.
[0083] On the other hand, for sample 9, the time required to remove water (dehydration time) was more than 12 hours, which was very inefficient in terms of production. The flexural modulus of the obtained molded body was also small, at 8.8 GPa. The density was also 1.30 g / cm 3 It is.
[0084] For Sample 10, the time required to remove water was 2.5 hours, which was longer than those for Samples 1 to 8. The flexural modulus of the obtained molded body was also 7.3 GPa, which was a very small value. The density was also 1.25 g / cm 3 , which is a fairly low value.
[0085] It should be understood that the embodiments and examples disclosed herein are illustrative in all respects and are not limiting in any respect. The scope of the present invention is defined by the claims, not the above description, and is intended to include all modifications within the meaning and scope of the claims. [Industrial Applicability]
[0086] The method for producing a molded body, and the method for producing a molded body and a microfibrillated cellulose molded body according to the present disclosure are particularly effectively used in cases where efficient production of large-sized molded bodies with high rigidity is required. [Explanation of symbols]
[0087] 11, 21 molded body, 12 microfibrillated cellulose, 13a, 13b, 16a, 16b, 25a, 25b, 26a, 26b, 27a, 27b surfaces, 14, 31a, 31b, 31c, 31d microfibrillated cellulose-containing composition, 15 water, 22 first layer, 23 second layer, 24 third layer, 32a, 32b glass nonwoven fabric, 33a, 33b metal plate, 34a pulp-containing composition.
Claims
1. It is composed only of microfibrillated cellulose. It is plate-shaped and has a thickness of 4.0 mm or more and 100.0 mm or less, The material is uniform in the thickness direction. A molded body having a flexural modulus of 11.9 GPa or more.
2. The molded article according to claim 1 , which is in the form of a plate and has a thickness of 10.0 mm or more.
3. Density is 1.30 g / cm 3 1.55g / cm or more 3 The molded body according to claim 1 or claim 2, wherein:
4. The molded article according to claim 1 , wherein the microfibrillated cellulose has a fiber diameter of 10 nm or more and 1000 nm or less.
Citation Information
Patent Citations
Diaphragm for electroacoustic transducer manufacture therefor
JP1995322390A
Woody base and its manufacturing method
JP2002292608A
Cellulose sheet
JP2012036529A
High-strength material including cellulose nanofiber as main component and method for producing the same
JP2013011026A
Cellulose nanofiber formed body
JP2018062727A