Substrate with conductive film, reflective mask blank, reflective mask, and method for manufacturing semiconductor device

A laminated conductive film with an amorphous lower and crystalline upper layer addresses the need for chemical resistance and low roughness in EUV lithography masks, enhancing the durability and accuracy of semiconductor manufacturing.

JP7569428B2Active Publication Date: 2024-10-17HOYA CORPORATION
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023148295
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-09-13
Publication Date
2024-10-17
Estimated Expiration
2039-08-30

AI Technical Summary

Technical Problem

Reflective masks used in EUV lithography require a conductive film with excellent chemical resistance and low surface roughness to withstand repeated cleanings with acidic or alkaline solutions and prevent particle generation due to friction during electrostatic chucking.

Method used

A conductive film structure with a laminated amorphous lower layer and crystalline upper layer, containing chromium and nitrogen, is developed, which enhances chemical resistance and reduces surface roughness.

Benefits of technology

The conductive film achieves improved chemical resistance and low surface roughness, preventing film deterioration and particle generation, ensuring accurate and reliable semiconductor device manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569428000003
    Figure 0007569428000003
  • Figure 0007569428000004
    Figure 0007569428000004
  • Figure 0007569428000005
    Figure 0007569428000005
Patent Text Reader

Abstract

To provide a substrate with an electroconductive film for the production of a reflective mask, said substrate having an electroconductive film with excellent chemical resistance and a low surface roughness (Rms).SOLUTION: A substrate with an electroconductive film is provided with an electroconductive film on one of the two main surfaces of a substrate, and this substrate with an electroconductive film is characterized in that: the electroconductive film contains chromium; the electroconductive film has a structure in which a lower layer and an upper layer are stacked in this order from the substrate side; the lower layer is amorphous; and the upper layer is crystalline.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective mask for use in EUV lithography, and a substrate with a conductive film and a reflective mask blank for manufacturing the reflective mask. The present invention also relates to a method for manufacturing a semiconductor device using a reflective mask. [Background technology]

[0002] In recent years, in the semiconductor industry, with the increasing integration of semiconductor devices, fine patterns exceeding the transfer limit of conventional photolithography using ultraviolet light are required. To enable the formation of such fine patterns, EUV lithography, an exposure technology using extreme ultraviolet (hereinafter referred to as "EUV") light, is considered promising. Here, EUV light refers to light in a wavelength band in the soft X-ray region or the vacuum ultraviolet region, specifically light with a wavelength of about 0.2 to 100 nm. A reflective mask has been proposed as a transfer mask used in this EUV lithography. In such a reflective mask, a multilayer reflective film for reflecting exposure light is formed on a substrate, and a pattern-forming thin film for absorbing the exposure light is formed in a pattern on the multilayer reflective film.

[0003] A reflective mask is manufactured from a reflective mask blank having a substrate, a multilayer reflective film formed on the substrate, and a thin film for pattern formation formed on the multilayer reflective film, by forming a pattern in the thin film for pattern formation by a photolithography method or the like.

[0004] In general, when a reflective mask is set on a mask stage of an exposure tool, the reflective mask is fixed by an electrostatic chuck. Therefore, a conductive film (back conductive film) is formed on the back main surface (the main surface opposite to the main surface on which the multilayer reflective film and the like are formed) of an insulating reflective mask blank substrate such as a glass substrate in order to facilitate fixing of the substrate by the electrostatic chuck.

[0005] Patent Document 1 describes a mask substrate including a substrate made of a low thermal expansion material, at least one material layer on the front side of the substrate, and at least one material layer on the back side of the substrate. Patent Document 1 also describes that the material on the back side is a metal selected from the group consisting of Mo and Cr.

[0006] Patent Document 2 describes a substrate with a conductive film used for manufacturing a reflective mask blank for EUV lithography. Patent Document 2 describes that the conductive film contains chromium (Cr) and nitrogen (N), that the average concentration of N in the conductive film is 0.1 at% or more and less than 40 at%, that the crystalline state of at least the surface of the conductive film is amorphous, that the sheet resistance value of the conductive film is 27 Ω / □ or less, and that the surface roughness (Rms) of the conductive film is 0.5 nm or less. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Special table number 2003-501823 [Patent Document 2] International Publication No. 2008 / 072706 Summary of the Invention [Problem to be solved by the invention]

[0008] In the manufacturing process of a reflective mask blank, wet cleaning is performed using an acidic aqueous solution (chemical solution) such as SPM cleaning (SPM: sulfuric acid and hydrogen-peroxide mixture) or an alkaline aqueous solution (chemical solution) such as SC-1 cleaning before applying a resist film on a thin film for pattern formation. In addition, in the manufacturing process of a reflective mask, after forming a pattern on a thin film for pattern formation, wet cleaning is performed using an acidic or alkaline aqueous solution (chemical solution) for removing a resist pattern, etc. Furthermore, in the manufacturing of semiconductor devices, wet cleaning using a chemical solution is performed to remove foreign matter attached to the reflective mask during exposure. Since a reflective mask is usually used repeatedly, these cleanings are performed at least several times. Therefore, the reflective mask is required to have sufficient cleaning resistance. A chemical solution (an acidic or alkaline aqueous solution, for example, sulfuric acid / hydrogen peroxide solution in the case of SPM cleaning) is used to clean the reflective mask. Therefore, the conductive film used in the reflective mask needs to have resistance to chemicals such as chemical solutions (referred to as "chemical resistance" in this specification).

[0009] On the other hand, when manufacturing semiconductor devices using a reflective mask, the reflective mask is fixed to an exposure tool by an electrostatic chuck. In order to prevent the generation of particles due to friction between the conductive film and the electrostatic chuck, the surface roughness (Rms) of the conductive film must be small.

[0010] Therefore, an object of the present invention is to obtain a substrate with a conductive film for manufacturing a reflective mask, the substrate having a conductive film with excellent chemical resistance and small surface roughness (Rms).An object of the present invention is also to obtain a reflective mask blank and a reflective mask, the substrate having a conductive film with excellent chemical resistance and small surface roughness (Rms). [Means for solving the problem]

[0011] As a result of intensive research, the present inventors have found that the chemical resistance of a conductive film can be increased by increasing the crystallinity of the conductive film. On the other hand, the surface roughness of the conductive film can be reduced by making the crystalline state of the conductive film amorphous. That is, in order to reduce the surface roughness of a conductive film, it is necessary to reduce the crystallinity of the conductive film, as opposed to increasing the chemical resistance of the conductive film. As a result of intensive research, the present inventors have found that a conductive film having excellent chemical resistance and small surface roughness (Rms) can be obtained by having a conductive film with a predetermined lower layer and upper layer, and have arrived at the present invention. The present invention has the following configuration.

[0012] (Configuration 1) Configuration 1 of the present invention is a conductive-film-coated substrate having a conductive film on one of two main surfaces of a substrate, the conductive film containing chromium, and the conductive film having a structure in which a lower layer and an upper layer are laminated in this order from the substrate side, the lower layer being amorphous, and the upper layer being crystalline.

[0013] (Configuration 2) A second aspect of the present invention is the conductive film-attached substrate according to the first aspect, wherein the upper layer is made of a material containing nitrogen.

[0014] (Configuration 3) A third aspect of the present invention is the conductive film-attached substrate according to the first or second aspect, wherein the lower layer is made of a material containing oxygen.

[0015] (Configuration 4) A fourth aspect of the present invention is the substrate with a conductive film according to any one of the first to third aspects, wherein the upper layer has a higher chromium content than the lower layer.

[0016] (Configuration 5) Configuration 5 of the present invention is the conductive film-coated substrate according to any one of Configurations 1 to 4, characterized in that when the upper layer is subjected to measurement of diffracted X-ray intensity versus diffraction angle 2θ by X-ray diffraction, a peak is detected in the diffraction angle 2θ range of 41 degrees or more and 47 degrees or less.

[0017] (Configuration 6) A sixth aspect of the present invention is the conductive film-attached substrate according to the fifth aspect, wherein the upper layer has a peak detected in the range of the diffraction angle 2θ of 56 degrees or more and 60 degrees or less.

[0018] (Configuration 7) A seventh aspect of the present invention is the conductive film-coated substrate according to the fifth or sixth aspect, wherein in the upper layer, no peak is detected within the range of the diffraction angle 2θ of 35 degrees or more and 38 degrees or less.

[0019] (Configuration 8) Configuration 8 of the present invention is a conductive-film-coated substrate, characterized in that a multilayer reflective film, in which high refractive index layers and low refractive index layers are alternately stacked, is formed on the main surface of the conductive-film-coated substrate of any one of configurations 1 to 7, opposite the side on which the conductive film is formed.

[0020] (Configuration 9) A ninth aspect of the present invention is the conductive film-coated substrate according to the eighth aspect, further comprising a protective film formed on the multilayer reflective film.

[0021] (Configuration 10) Configuration 10 of the present invention is a reflective mask blank having a structure in which a multilayer reflective film and a thin film for pattern formation are laminated in this order on one main surface of a substrate, and further comprising a conductive film on the other main surface of the substrate, the conductive film containing chromium, the conductive film having a structure in which a lower layer and an upper layer are laminated in this order from the substrate side, the lower layer being amorphous, and the upper layer being crystalline.

[0022] (Configuration 11) An eleventh aspect of the present invention is the reflective mask blank of the tenth aspect, wherein the upper layer is made of a material containing nitrogen.

[0023] (Configuration 12) A twelfth aspect of the present invention is the reflective mask blank according to the tenth or eleventh aspect, wherein the lower layer is made of a material containing oxygen.

[0024] (Configuration 13) A thirteenth aspect of the present invention is the reflective mask blank according to any one of the tenth to twelfth aspects, wherein the chromium content of the upper layer is greater than the chromium content of the lower layer.

[0025] (Configuration 14) Structure 14 of the present invention is the reflective mask blank of any of structures 10 to 13, characterized in that when the diffracted X-ray intensity versus diffraction angle 2θ of the upper layer is measured by X-ray diffraction method, a peak is detected in the diffraction angle 2θ range of 41 degrees or more and 47 degrees or less.

[0026] (Configuration 15) A fifteenth aspect of the present invention is the reflective mask blank according to the fourteenth aspect, wherein the upper layer has a peak detected in the range of the diffraction angle 2θ of 56 degrees or more and 60 degrees or less.

[0027] (Configuration 16) A sixteenth aspect of the present invention is the reflective mask blank according to the fourteenth or fifteenth aspect, wherein in the upper layer, no peak is detected within the range of the diffraction angle 2θ of 35 degrees or more and 38 degrees or less.

[0028] (Configuration 17) A seventeenth aspect of the present invention is the reflective mask blank according to any one of the tenth to sixteenth aspects, further comprising a protective film formed between the multilayer reflective film and the pattern-forming thin film.

[0029] (Configuration 18) An eighteenth aspect of the present invention is a reflective mask blank according to any one of the tenth to seventeenth aspects, wherein a transfer pattern is provided on the pattern-forming thin film.

[0030] (Configuration 19) Structure 19 of the present invention is a method for producing a semiconductor device, comprising the step of exposing and transferring a transfer pattern to a resist film on a semiconductor substrate using the reflective mask of Structure 18. Effect of the Invention

[0031] According to the present invention, it is possible to obtain a substrate with a conductive film for manufacturing a reflective mask, which has a conductive film with excellent chemical resistance and small surface roughness (Rms). Also, according to the present invention, it is possible to obtain a reflective mask blank and a reflective mask, which have a conductive film with excellent chemical resistance and small surface roughness (Rms). [Brief description of the drawings]

[0032] [Figure 1] 1 is a schematic cross-sectional view showing an example of a configuration of a conductive film-attached substrate according to an embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view showing an example of a configuration of a multilayer reflective film-coated substrate (substrate with conductive film) according to an embodiment of the present invention. [Diagram 3] FIG. 1 is a schematic cross-sectional view showing an example of the configuration of a reflective mask blank (substrate with conductive film) according to an embodiment of the present invention. [Figure 4] 1 is a schematic cross-sectional view showing an example of a reflective mask according to an embodiment of the present invention. [Diagram 5] FIG. 2 is a schematic cross-sectional view showing another example of the configuration of a reflective mask blank according to an embodiment of the present invention. [Figure 6] 1A to 1C are schematic cross-sectional views illustrating steps of producing a reflective mask from a reflective mask blank. [Figure 7] 1 is a diagram (diffracted X-ray spectrum) showing the diffracted X-ray intensity (counts / second) versus the X-ray diffraction angle (2θ) in Example 1. [Figure 8] 1 is a diagram (diffracted X-ray spectrum) showing diffracted X-ray intensity (counts / second) versus X-ray diffraction angle (2θ) in Comparative Example 1. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Hereinafter, embodiments of the present invention will be described in detail with reference to the drawings. Note that the following embodiments are forms for embodying the present invention, and are not intended to limit the scope of the present invention.

[0034] 1 shows an example of a conductive film-attached substrate 50 of this embodiment. The conductive film-attached substrate 50 of this embodiment has a predetermined conductive film 23 on at least one of the two main surfaces of a mask blank substrate 10 (sometimes simply referred to as "substrate 10").

[0035] In this specification, of the main surfaces of the mask blank substrate 10, the main surface (sometimes simply referred to as the "rear surface") on which the conductive film 23 (sometimes referred to as the "rear surface conductive film") is formed is referred to as the "rear main surface". Also, in this specification, the main surface of the conductive film-coated substrate 50 on which the conductive film 23 is not formed is referred to as the "front main surface". On the front main surface of the mask blank substrate 10, a multilayer reflective film 21 is formed in which high refractive index layers and low refractive index layers are alternately laminated.

[0036] 1 illustrates an example of a conductive-film-attached substrate 50 in which a predetermined conductive film 23 is disposed on one main surface (the back main surface) of a substrate 10, and no thin film is formed on the front main surface. In this specification, the conductive-film-attached substrate 50 refers to at least a mask blank substrate 10 in which a conductive film 23 is formed on the back main surface, and also includes a substrate with a multilayer reflective film 21 formed on the other main surface (substrate with a multilayer reflective film 20), a substrate with a pattern-forming thin film 24 further formed (reflective mask blank 30), and the like.

[0037] Fig. 2 shows a multilayer reflective film-coated substrate 20 of this embodiment having a conductive film 23 formed on its back main surface. The multilayer reflective film-coated substrate 20 shown in Fig. 2 includes a predetermined conductive film 23 on its back main surface. Therefore, the multilayer reflective film-coated substrate 20 shown in Fig. 2 is a type of conductive film-coated substrate 50 of this embodiment.

[0038] Fig. 3 is a schematic diagram showing an example of a reflective mask blank 30 of this embodiment. The reflective mask blank 30 of Fig. 3 has a multilayer reflective film 21, a protective film 22, and a thin film for pattern formation 24 on the front main surface of a mask blank substrate 10. The reflective mask blank 30 of Fig. 3 also includes a predetermined conductive film 23 on its back main surface. Therefore, the reflective mask blank 30 shown in Fig. 3 is a type of conductive film-coated substrate 50 of this embodiment.

[0039] FIG. 5 is a schematic diagram showing another example of the reflective mask blank 30 of this embodiment. The reflective mask blank 30 shown in FIG. 5 includes the multilayer reflective film 21 and the thin film for pattern formation 24, the protective film 22 formed between the multilayer reflective film 21 and the thin film for pattern formation 24, and the etching mask film 25 formed on the surface of the thin film for pattern formation 24. The reflective mask blank 30 of this embodiment includes a predetermined conductive film 23 on its rear main surface. Therefore, the reflective mask blank 30 shown in FIG. 5 is a type of the substrate with conductive film 50 of this embodiment. When using a reflective mask blank 30 having an etching mask film 25, the etching mask film 25 may be peeled off after a transfer pattern is formed on the thin film for pattern formation 24, as described later. In addition, in the reflective mask blank 30 without the etching mask film 25, the thin film for pattern formation 24 may have a laminated structure of multiple layers, and the materials constituting the multiple layers may have different etching properties, so that the thin film for pattern formation 24 has an etching mask function.

[0040] In this specification, "having a predetermined thin film (e.g., conductive film 23) on the main surface of the mask blank substrate 10" means that the predetermined thin film is disposed in contact with the main surface of the mask blank substrate 10, and also includes the case where another film is disposed between the mask blank substrate 10 and the predetermined thin film. The same applies to films other than the predetermined thin film. For example, "having film B on film A" means that film A and film B are disposed so as to be in direct contact with each other, and also includes the case where another film is disposed between film A and film B. In addition, in this specification, for example, "film A is disposed in contact with the surface of film B" means that film A and film B are disposed so as to be in direct contact with each other, without another film being interposed between film A and film B.

[0041] Next, the surface roughness (Rms) which is a parameter indicating the surface morphology of the mask blank substrate 10 and the surface morphology of the thin film constituting the reflective mask blank 30 or the like will be described.

[0042] Rms (Root Mean Square), a typical index of surface roughness, is the square root of the average of the squares of the deviations from the average line to the measured curve. Rms is expressed by the following formula (1).

[0043]

number

[0044] Rms has conventionally been used to control the surface roughness of the mask blank substrate 10, and allows the surface roughness to be grasped numerically.

[0045] [Substrate with conductive film 50] Next, the conductive-layer-coated substrate 50 of the embodiment will be specifically described. First, the mask blank substrate 10 (sometimes simply referred to as "substrate 10") used in the conductive-layer-coated substrate 50 will be described.

[0046] <Mask blank substrate 10> In order to prevent distortion of a transfer pattern (thin film pattern 24a of pattern-forming thin film 24 described below) due to heat during exposure to EUV light, a material having a low thermal expansion coefficient within the range of 0±5 ppb / ° C. is preferably used as the mask blank substrate 10. Materials having a low thermal expansion coefficient within this range include, for example, SiO2-TiO2-based glass and multi-component glass ceramics.

[0047] The front main surface of the substrate 10 on which the transfer pattern is formed is surface-processed to have a high flatness from the viewpoint of obtaining at least pattern transfer accuracy and positional accuracy. In the case of EUV exposure, the flatness is preferably 0.1 μm or less, more preferably 0.05 μm or less, and even more preferably 0.03 μm or less in a 132 mm×132 mm area of ​​the main surface of the substrate 10 on which the transfer pattern is formed. The back main surface opposite to the front main surface is a surface that is electrostatically chucked when set in an exposure device. The back main surface is preferably 0.1 μm or less, more preferably 0.05 μm or less, and even more preferably 0.03 μm or less in a 132 mm×132 mm area. The flatness of the back main surface of the reflective mask blank 30 is preferably 1 μm or less, more preferably 0.5 μm or less, and even more preferably 0.3 μm or less in a 142 mm×142 mm area.

[0048] The surface smoothness of the substrate 10 is also an extremely important item. The surface roughness of the front main surface of the transfer pattern forming thin film 24 on which the thin film pattern 24a is formed is preferably 0.1 nm or less in root mean square roughness (Rms). The surface smoothness can be measured by an atomic force microscope.

[0049] Furthermore, the substrate 10 preferably has high rigidity to prevent deformation due to film stress of films (such as the multilayer reflective film 21) formed thereon. In particular, the substrate 10 preferably has a high Young's modulus of 65 GPa or more.

[0050] <Conductive film 23> Next, the conductive film 23 included in the conductive film-coated substrate 50 of this embodiment will be described.

[0051] As shown in FIG. 1, a conductive film 23 for electrostatic chuck is formed on the back main surface of the substrate 10 (the main surface opposite to the main surface on which the multilayer reflective film 21 is formed).

[0052] The predetermined conductive film 23 of the conductive-film-coated substrate 50 of the present embodiment contains chromium. The predetermined conductive film 23 preferably contains nitrogen. When the predetermined conductive film 23 contains chromium and nitrogen, the chemical resistance of the predetermined conductive film 23 can be further improved.

[0053] The conductive film 23 of the conductive-film-coated substrate 50 of this embodiment contains chromium. When a given conductive film 23 contains chromium, it is possible to impart conductivity to the conductive film 23.

[0054] The conductive film 23 included in the conductive-film-attached substrate 50 of this embodiment includes a lower layer 231 and an upper layer 232. Specifically, the conductive film 23 of the conductive-film-attached substrate 50 of this embodiment has a structure in which the lower layer 231 and the upper layer 232 are laminated in this order from the substrate side.

[0055] First, the lower layer 231 of the conductive film 23 of the conductive film-attached substrate 50 of this embodiment will be described. The crystalline state of the lower layer 231 of this embodiment is preferably amorphous. In this specification, the lower layer 231 being amorphous means that when the lower layer 231 is measured by a predetermined X-ray diffraction method, no peak is observed in the diffracted X-ray spectrum. The diffracted X-ray spectrum and peaks will be described later. The crystalline state of the lower layer 231 can also be specified from an electron beam diffraction image obtained by a transmission electron microscope (TEM) or the like. That is, a cross-sectional sample of the conductive film-attached substrate 50 is prepared, and an electron beam is irradiated from the cross-sectional direction to the lower layer 231 to obtain an electron beam diffraction image. From the electron beam diffraction image, it is possible to specify whether the lower layer 231 is amorphous or crystalline.

[0056] Since the crystal state of the lower layer 231 of the conductive film 23 is amorphous, the surface roughness of the lower layer 231 can be reduced. In the conductive film-attached substrate 50 of this embodiment, the surface roughness of the lower layer 231 is small, so when a predetermined upper layer 232 is further disposed on the surface of the lower layer 231, the surface roughness of the upper layer 232 can be reduced. Since the conductive film 23 of the conductive film-attached substrate 50 of this embodiment has a small surface roughness (Rms), it is possible to prevent the generation of particles due to friction between the conductive film 23 of the reflective mask 40 obtained by the conductive film-attached substrate 50 of this embodiment and the electrostatic chuck. The reason why the surface roughness of the upper layer 232 is reduced by stacking the crystalline upper layer 232 on the lower layer 231 in an amorphous bonded state is presumed to be due to the following action. Note that the following presumption is based on the presumption of the present inventors at the time of filing the application, and does not limit the scope of the present invention in any way.

[0057] In a crystalline film, surface roughness occurs due to the size of the crystal grains that compose the film. On the other hand, in an amorphous film, the crystal planes inside the film are arranged in a long-range order, so the crystal grains are finer, and the surface roughness is suppressed compared to a crystalline film. In the combination of an amorphous lower layer 231 and a crystalline upper layer 232, mixing occurs between the lower layer 231 and the upper layer 232 during the process of forming the upper layer 232 by a sputtering method, and the crystal grains are finer. It is presumed that this suppresses the coarsening of the crystal grains in the initial film growth process of the upper layer 232, thereby reducing the surface roughness.

[0058] The lower layer 231 of the conductive film 23 of the conductive film-coated substrate 50 of this embodiment is preferably made of a material containing oxygen. When the material of the lower layer 231 contains chromium and oxygen, the crystalline state of the lower layer 231 can be easily made amorphous. In order to make it easier to make the crystalline state of the lower layer 231 amorphous, the oxygen content of the lower layer 231 is preferably 1 atomic % or more and 20 atomic % or less, and more preferably 3 atomic % or more and 15 atomic % or less.

[0059] The lower layer 231 of the conductive film 23 of the conductive film-coated substrate 50 of this embodiment may further contain elements other than chromium and oxygen, provided that the effect of this embodiment is not impaired. For example, the lower layer 231 may further contain nitrogen. Examples of elements further contained in the lower layer 231 include highly conductive metals such as Ag, Au, Cu, Al, Mg, W, Ru, and Co. However, in order not to prevent the crystal state of the lower layer 231 from being made amorphous, the content of components other than chromium and oxygen is preferably 30 atomic % or less, and more preferably 15 atomic % or less.

[0060] Next, the upper layer 232 of the conductive film 23 of the conductive film-attached substrate 50 of this embodiment will be described. The upper layer 232 of the conductive film 23 of the conductive film-attached substrate 50 of this embodiment is preferably crystalline. In this specification, "the upper layer 232 has crystallinity" means that when the upper layer 232 is measured by a predetermined X-ray diffraction method, at least one peak is observed in the diffracted X-ray spectrum. The diffracted X-ray spectrum and peaks will be described later. The crystalline state of the upper layer 232 can also be specified from an electron beam diffraction image obtained by a transmission electron microscope (TEM) or the like. That is, a cross-sectional sample of the conductive film-attached substrate 50 is prepared, and an electron beam is irradiated from the cross-sectional direction to the upper layer 232 to obtain an electron beam diffraction image. From the electron beam diffraction image, it is possible to specify whether the upper layer 232 is amorphous or crystalline.

[0061] The upper layer 232 of the conductive film 23 has a crystalline state, so that the chemical resistance of the upper layer 232 disposed on the outermost surface of the conductive film 23 can be increased. Therefore, the conductive film 23 includes the upper layer 232 having a crystalline state, so that the chemical resistance of the conductive film 23 can be increased. Therefore, when the reflective mask 40 manufactured using the conductive-film-coated substrate 50 of this embodiment is repeatedly washed with a chemical such as a chemical solution, deterioration of the conductive film 23 can be suppressed.

[0062] The upper layer 232 of the conductive film-coated substrate 50 of this embodiment is preferably made of a material containing nitrogen. By containing chromium and nitrogen in the material of the upper layer 232, the mechanical strength of the upper layer 232 can be increased compared to the case where the upper layer 232 is formed only from chromium. In general, a chromium nitride film becomes a non-crystalline (amorphous) film when the nitrogen content is within a predetermined range. A chromium nitride film with a nitrogen content below the predetermined range becomes a metallic film having crystallinity, and a chromium nitride film with a nitrogen content above the predetermined range becomes a highly nitrided film having crystallinity. Therefore, in order to make the upper layer 232 crystalline while further increasing the conductivity, the nitrogen content of the upper layer 232 is preferably 1 atomic % or more and 15 atomic % or less, and more preferably 2 atomic % or more and 10 atomic % or less.

[0063] In order to further increase the chemical resistance of the upper layer 232 of the predetermined conductive film 23, the upper layer 232 of the predetermined conductive film 23 of the conductive-film-coated substrate 50 of this embodiment preferably consists of only chromium and nitrogen, excluding impurities that inevitably get mixed in. Note that in this specification, even if it is simply stated that "the thin film consists of only chromium and nitrogen," this means that the thin film can contain impurities that inevitably get mixed in other than chromium and nitrogen.

[0064] The upper layer 232 of the conductive film 23 of the conductive film-coated substrate 50 of this embodiment may further contain elements other than chromium and nitrogen to the extent that the effect of this embodiment is not impaired. For example, elements further contained in the upper layer 232 may include highly conductive metals such as Ag, Au, Cu, Al, Mg, W, Ru, and Co. However, in order not to prevent the crystal state of the upper layer 232 from being made crystalline, the content of components other than chromium and nitrogen is preferably 30 atomic % or less, and more preferably 15 atomic % or less.

[0065] The chromium content of the upper layer 232 of the conductive film-coated substrate 50 of this embodiment is preferably greater than the chromium content of the lower layer 231. The greater the chromium content in the thin film, the lower the sheet resistance. By making the chromium content of the upper layer 232 relatively large, fixation by an electrostatic chuck can be made more reliable.

[0066] The upper layer 232 of the predetermined conductive film 23 of the conductive film-coated substrate 50 of this embodiment preferably has a predetermined crystallinity. Specifically, as described below, when the upper layer 232 is measured by an X-ray diffraction method, it is preferable that the upper layer 232 exhibits a diffracted X-ray spectrum in which a peak is detected at a predetermined diffraction angle 2θ (hereinafter, such a diffracted X-ray spectrum may be referred to as a "predetermined diffracted X-ray spectrum"). The detection of a peak in the diffracted X-ray spectrum means that the upper layer 232 to be measured has crystallinity.

[0067] The upper layer 232 of the predetermined conductive film 23 of the conductive film-coated substrate 50 of this embodiment is CuK α When the diffracted X-ray intensity versus diffraction angle 2θ is measured by an X-ray diffraction method using 100 nm ray, it is preferable that a peak is detected in the range of diffraction angle 2θ of 41 degrees or more and 47 degrees or less. FIG. 7 shows a diffracted X-ray spectrum (diffracted X-ray intensity versus diffraction angle 2θ) obtained by measuring the diffracted X-ray intensity for the upper layer 232 of a given conductive film 23 of this embodiment. As shown in FIG. 7, in the diffracted X-ray spectrum of Example 1, a peak is detected in the range of diffraction angle 2θ of 41 degrees or more and 47 degrees or less. It is presumed that this peak corresponds to the peak of the (111) plane of Cr2N or the (200) plane of CrN, but the present invention is not bound by this presumption. The detection of a peak in the range of diffraction angle 2θ of 41 degrees or more and 47 degrees or less means that the upper layer 232 to be measured has crystallinity, and the detection of the peak makes it possible to more reliably obtain a conductive film-attached substrate 50 having a conductive film 23 (upper layer 232) with excellent chemical resistance.

[0068] In this specification, the peak detected by the X-ray diffraction method is CuK αThe diffraction angle 2θ of the peak can be defined as the diffraction angle 2θ that indicates the maximum value of the peak when the background is subtracted from the measurement data (diffracted X-ray spectrum).

[0069] The upper layer 232 of the predetermined conductive film 23 of the conductive film-coated substrate 50 of this embodiment is CuK α When the diffracted X-ray intensity versus diffraction angle 2θ is measured by an X-ray diffraction method using 1000 nm radiation, it is preferable that a peak is detected at a diffraction angle 2θ in the range of 56 degrees or more and 60 degrees or less. As shown in Fig. 7, in the diffracted X-ray spectrum of the upper layer 232 of Example 1, which has excellent chemical resistance, a peak is detected at a diffraction angle 2θ in the range of 56 degrees or more and 60 degrees or less. This peak is presumed to correspond to the peak of the (112) plane of Cr2N, but the present invention is not limited to this presumption.

[0070] The present inventors have found that a thin film having a crystal structure in which a peak is detected in the range of a diffraction angle 2θ of 56 degrees or more and 60 degrees or less in the upper layer 232 of the conductive film 23 has excellent chemical resistance. Therefore, when a reflective mask 40 is manufactured using a conductive-film-coated substrate 50 including a conductive film 23 having such an upper layer 232, deterioration of the thin film of the reflective mask 40 can be suppressed even if the reflective mask 40 is repeatedly washed with a chemical such as a chemical solution.

[0071] The upper layer 232 of the predetermined conductive film 23 of the conductive film-coated substrate 50 of this embodiment is CuK αWhen the diffracted X-ray intensity versus diffraction angle 2θ is measured by an X-ray diffraction method using 1000 nm 400 nm 450 nm 1000 nm 1500 nm 1000 nm, it is preferable that no peak is detected in the diffraction angle 2θ range of 35 degrees or more and 38 degrees or less. As shown in Fig. 7, in the diffracted X-ray spectrum of Example 1, no peak is detected in the diffraction angle 2θ range of 35 degrees or more and 38 degrees or less. Note that the peak in this diffraction angle range is presumed to correspond to the peak of the (111) plane of CrN, but the present invention is not bound by this presumption.

[0072] The upper layer 232 of the predetermined conductive film 23 of the conductive-film-coated substrate 50 of this embodiment preferably contains chromium and nitrogen. As described below, the crystal structure of the predetermined thin film (upper layer 232 of the conductive film 23) containing chromium and nitrogen changes depending on the nitrogen content of the predetermined thin film.

[0073] As described above, in this embodiment, by using the conductive film 23 including the predetermined upper layer 232 and the predetermined lower layer 231, it is possible to obtain a conductive film-attached substrate 50 including the conductive film 23 having excellent chemical resistance and small surface roughness (Rms). Therefore, when the reflective mask 40 manufactured using the conductive film-attached substrate 50 of this embodiment is repeatedly washed with a chemical such as a chemical solution, deterioration of the conductive film 23 can be suppressed. In addition, since the surface roughness (Rms) of the conductive film 23 is small, it is possible to prevent the generation of particles due to friction between the conductive film 23 of the reflective mask 40 and the electrostatic chuck. Therefore, the conductive film-attached substrate 50 of this embodiment can be preferably used as the conductive film-attached substrate 50 for manufacturing the reflective mask 40.

[0074] The method of forming the predetermined conductive film 23 (upper layer 232 and lower layer 231) of this embodiment can be any known method as long as the required characteristics can be obtained. As the method of forming the predetermined conductive film 23, sputtering methods such as DC magnetron sputtering, RF sputtering, and ion beam sputtering are generally used. In order to more reliably obtain the required characteristics, reactive sputtering can be used. When the predetermined conductive film 23 (upper layer 232 or lower layer 231) contains chromium and nitrogen, a chromium target is used, nitrogen gas is introduced, and the film is formed by sputtering in a nitrogen atmosphere, thereby forming the predetermined conductive film 23 (upper layer 232 or lower layer 231) containing chromium and nitrogen. When the predetermined conductive film 23 (upper layer 232 or lower layer 231) contains chromium and oxygen, a chromium target is used, oxygen gas is introduced, and the film is formed by sputtering in an oxygen atmosphere, thereby forming the predetermined conductive film 23 (upper layer 232 or lower layer 231) containing chromium and oxygen. Furthermore, by introducing both nitrogen gas and oxygen gas and depositing the film by sputtering, a predetermined conductive film 23 (upper layer 232 or lower layer 231) containing chromium, nitrogen, and oxygen can be formed. Note that by controlling the flow rate of nitrogen gas and / or oxygen gas introduced during sputtering, the upper layer 232 or lower layer 231 of the predetermined conductive film 23 having a diffraction X-ray spectrum can be deposited. In addition to nitrogen gas and / or oxygen gas, an inert gas such as argon gas can be used in combination.

[0075] Specifically, the method of forming the predetermined conductive film 23 (upper layer 232 and lower layer 231) is preferably to form the predetermined conductive film 23 by rotating the substrate 10 on a horizontal plane with the surface of the substrate 10 on which the predetermined conductive film 23 is to be formed facing upward. At this time, it is preferable to form the film at a position where the central axis of the substrate 10 is offset from a straight line that passes through the center of the sputtering target and is parallel to the central axis of the substrate 10. That is, it is preferable to form the predetermined conductive film 23 by inclining the sputtering target to a predetermined angle with respect to the surface on which the film is to be formed. The sputtering target and the substrate 10 are disposed in this manner, and the predetermined conductive film 23 can be formed by sputtering the facing sputtering target. The predetermined angle is preferably an inclination angle of the sputtering target of 5 degrees or more and 30 degrees or less. In addition, the gas pressure during sputtering film formation is preferably 0.03 Pa or more and 0.1 Pa or less.

[0076] Each of the upper layer 232 and the lower layer 231 of the conductive film 23 can be a uniform film in which the concentration of elements (e.g., chromium element and nitrogen element) contained in the thin film is uniform, except for the surface layer affected by surface oxidation. Also, it can be a compositionally graded film in which the concentration of elements contained in the upper layer 232 or the lower layer 231 changes along the thickness direction of the upper layer 232 or the lower layer 231. Also, the upper layer 232 or the lower layer 231 can be a laminated film consisting of multiple layers of multiple different compositions, as long as the effect of this embodiment is not impaired.

[0077] The conductive film-attached substrate 50 of the present embodiment can include, for example, a hydrogen penetration-inhibiting film between the substrate 10 and the conductive film 23, which inhibits hydrogen from penetrating from the substrate 10 (glass substrate) into the conductive film 23. The presence of the hydrogen penetration-inhibiting film can inhibit hydrogen from being taken in by the conductive film 23, and can inhibit an increase in the compressive stress of the conductive film 23.

[0078] The material of the hydrogen penetration suppression film may be any type of material that is difficult for hydrogen to permeate and can suppress the penetration of hydrogen from the substrate 10 (glass substrate) into the conductive film 23. Specific examples of the material of the hydrogen penetration suppression film include Si, SiO2, SiON, SiCO, SiCON, SiBO, SiBON, Cr, CrN, CrO, CrON, CrC, CrCN, CrCO, CrCON, Mo, MoSi, MoSiN, MoSiO, MoSiCO, MoSiON, MoSiCON, TaO, and TaON. The hydrogen penetration suppression film may be a single layer of these materials, or may be a multi-layer or composition-graded film. CrO may be used as the material of the hydrogen penetration suppression film.

[0079] The electrical properties required for the conductive film 23 having conductivity for electrostatic chuck are usually 150Ω / □ (Ω / square) or less, and preferably 100Ω / □ or less. The thickness of the conductive film 23 is not particularly limited as long as it satisfies the function for electrostatic chuck, but is usually 20 nm to 250 nm. The thickness of the lower layer 231 is preferably 5 to 50 nm, and the thickness of the upper layer 232 is preferably 15 to 200 nm. The conductive film 23 also serves to adjust the stress on the back main surface side of the reflective mask blank 30. The conductive film 23 is adjusted to obtain a flat reflective mask blank 30 by balancing the stress from various films formed on the front main surface.

[0080] The conductive film 23 preferably has a film loss of 1 nm or less after one SPM cleaning, so that the sheet resistance, mechanical strength, and / or transmittance required for the conductive film 23 are not impaired even when wet cleaning using an acidic aqueous solution (chemical solution), such as SPM cleaning, is performed in the manufacturing process of the reflective mask blank 30, the reflective mask 40, and / or the semiconductor device.

[0081] SPM cleaning is a cleaning method that uses H2SO4 and H2O2, and is performed using a cleaning solution with a H2SO4:H2O2 ratio of 1:1 to 5:1 at a temperature of 80 to 150°C for a processing time of approximately 10 minutes.

[0082] The cleaning conditions of the SPM, which are the criteria for judging the cleaning resistance in this embodiment, are as follows. Cleaning solution H2SO4:H2O2=2:1 (weight ratio) Washing temperature: 120℃ Washing time: 10 minutes

[0083] Furthermore, a pattern transfer apparatus for manufacturing a semiconductor device is usually equipped with an electrostatic chuck for fixing the reflective mask 40 mounted on a stage. The conductive film 23 formed on the rear main surface of the reflective mask 40 is fixed to the stage of the pattern transfer apparatus by the electrostatic chuck.

[0084] The surface roughness of the conductive film 23 is preferably 0.5 nm or less, and more preferably 0.4 nm or less, in terms of root mean square roughness (Rms) obtained by measuring an area of ​​1 μm × 1 μm with an atomic force microscope. When the surface of the conductive film 23 has a predetermined root mean square roughness (Rms), it is possible to prevent the generation of particles due to friction between the electrostatic chuck and the conductive film 23.

[0085] Furthermore, in the above-mentioned pattern transfer device, if the moving speed of the stage carrying the reflective mask 40 is increased to increase production efficiency, an additional load is applied to the conductive film 23. Therefore, it is desirable for the conductive film 23 to have a higher mechanical strength. The mechanical strength of the conductive film 23 can be evaluated by measuring the crack generation load of the conductive film-coated substrate 50. The mechanical strength needs to be 300 mN or more in terms of the crack generation load. The mechanical strength is preferably 600 mN or more, more preferably greater than 1000 mN, in terms of the crack generation load. When the crack generation load is within a predetermined range, it can be said that the conductive film 23 has the mechanical strength required for the conductive film 23 for an electrostatic chuck.

[0086] Japanese Patent No. 5883249 describes a method for correcting errors in a photolithography mask by using a laser beam. When applying the technique described in Japanese Patent No. 5883249 to a reflective mask 40, it is possible to irradiate a laser beam from the rear main surface of the substrate 10. However, since a conductive film 23 is arranged on the rear main surface of the substrate 10 of the reflective mask 40, a problem occurs in that the laser beam is difficult to transmit through the conductive film 23. When chromium is used as a thin film material, the thin film has a relatively high visible light transmittance at a predetermined wavelength. Therefore, when a thin film containing chromium is used as the conductive film 23 of the reflective mask 40, the defect described in Japanese Patent No. 5883249 can be corrected by irradiating a predetermined light from the rear main surface.

[0087] The thickness of the conductive film 23 can be appropriately selected in relation to the transmittance and electrical conductivity for light with a wavelength of 532 nm. For example, if the electrical conductivity of the material is high, the film thickness can be made thin, and the transmittance can be increased. The thickness of the conductive film 23 of the conductive film-coated substrate 50 of this embodiment, which uses chromium as the thin film material, is preferably 20 nm or more and 50 nm or less. By making the conductive film 23 have a predetermined thickness, it is possible to obtain a conductive film 23 having more appropriate transmittance and electrical conductivity.

[0088] The transmittance of the conductive film 23 at a wavelength of 532 nm is preferably 10% or more, more preferably 20% or more, and even more preferably 25% or more. The transmittance of the conductive film 23 at a wavelength of 632 nm is preferably 25% or more. When the transmittance of light at a predetermined wavelength of the conductive film 23 of the conductive film-coated substrate 50 is within a predetermined range, it is possible to obtain a reflective mask 40 in which misalignment of the reflective mask 40 can be corrected from the rear main surface side by a laser beam or the like.

[0089] In addition, the transmittance in this embodiment was obtained by irradiating light with a wavelength of 532 nm from the conductive film 23 side of the conductive film-coated substrate 50 having the conductive film 23, and measuring the transmitted light that passes through the conductive film 23 and the substrate 10.

[0090] <Substrate 20 with multilayer reflective film and multilayer reflective film 21> Next, the multilayer reflective film coated substrate 20 and the multilayer reflective film 21 of this embodiment will be described below.

[0091] 2, the multilayer reflective film-coated substrate 20 of this embodiment has a multilayer reflective film 21 formed by alternately stacking high refractive index layers and low refractive index layers on a main surface (front main surface) opposite to a main surface (rear main surface) on which the above-mentioned conductive film 23 is formed. The multilayer reflective film-coated substrate 20 of this embodiment has a predetermined conductive film 23 on the rear main surface. Therefore, the multilayer reflective film-coated substrate 20 of this embodiment is a type of conductive film-coated substrate 50. The multilayer reflective film-coated substrate 20 of this embodiment has the predetermined multilayer reflective film 21, and is thereby able to reflect EUV light of a predetermined wavelength.

[0092] In this embodiment, the multilayer reflective film 21 can be formed before forming the conductive film 23. Alternatively, the conductive film 23 may be formed as shown in FIG 1, and then the multilayer reflective film 21 may be formed as shown in FIG 2.

[0093] The multilayer reflective film 21 provides a function of reflecting EUV light in the reflective mask 40. The multilayer reflective film 21 has a multilayer structure in which layers containing elements with different refractive indices as main components are periodically laminated.

[0094] Generally, the multilayer reflective film 21 is a multilayer film in which a thin film (high refractive index layer) of a light element or its compound, which is a high refractive index material, and a thin film (low refractive index layer) of a heavy element or its compound, which is a low refractive index material, are alternately laminated for about 40 to 60 periods. The multilayer film may be laminated in a multi-period of a high refractive index layer / low refractive index layer structure in which a high refractive index layer and a low refractive index layer are laminated in this order from the substrate 10 side, or in a multi-period of a low refractive index layer / high refractive index layer structure in which a low refractive index layer and a high refractive index layer are laminated in this order from the substrate 10 side. Note that the topmost layer of the multilayer reflective film 21 (i.e., the surface layer of the multilayer reflective film 21 on the opposite side to the substrate 10) is preferably a high refractive index layer. In the above-mentioned multilayer film, when a multi-period of a multilayer structure (high refractive index layer / low refractive index layer) in which a high refractive index layer and a low refractive index layer are laminated in this order is laminated on the substrate 10, the topmost layer is a low refractive index layer. The low refractive index layer on the top surface of the multilayer reflective film 21 is easily oxidized, so that the reflectance of the multilayer reflective film 21 decreases. In order to avoid the decrease in reflectance, it is preferable to form a high refractive index layer on the top low refractive index layer to form the multilayer reflective film 21. On the other hand, in the above-mentioned multilayer film, when a laminate structure (low refractive index layer / high refractive index layer) in which a low refractive index layer and a high refractive index layer are laminated in this order on the substrate 10 is defined as one period, and multiple periods are laminated, the top layer becomes the high refractive index layer. In this case, there is no need to further form a high refractive index layer.

[0095] In this embodiment, a layer containing silicon (Si) is used as the high refractive index layer. In addition to simple Si, a Si compound containing boron (B), carbon (C), nitrogen (N), and / or oxygen (O) can be used as the material containing Si. By using a layer containing Si as the high refractive index layer, a reflective mask 40 for EUV lithography with excellent reflectance of EUV light can be obtained. In this embodiment, a glass substrate is preferably used as the substrate 10. Si also has excellent adhesion to the glass substrate. In addition, a simple metal selected from molybdenum (Mo), ruthenium (Ru), rhodium (Rh), and platinum (Pt), or an alloy thereof is used as the low refractive index layer. For example, a Mo / Si periodic laminated film in which Mo films and Si films are alternately laminated for about 40 to 60 periods is preferably used as the multilayer reflective film 21 for EUV light with a wavelength of 13 nm to 14 nm. The high refractive index layer, which is the uppermost layer of the multilayer reflective film 21, can be made of silicon (Si), and a silicon oxide layer containing silicon and oxygen can be formed between this uppermost layer (Si) and the Ru-based protective film 22. By forming the silicon oxide layer, the cleaning resistance of the reflective mask 40 can be improved.

[0096] The reflectance of the multilayer reflective film 21 alone is usually 65% ​​or more, and the upper limit is usually 73%. The thickness and period of each constituent layer of the multilayer reflective film 21 can be appropriately selected according to the exposure wavelength, for example, so as to satisfy the law of Bragg reflection. In the multilayer reflective film 21, there are multiple high refractive index layers and multiple low refractive index layers. The thickness of the multiple high refractive index layers does not need to be the same, and the thickness of the multiple low refractive index layers does not need to be the same. In addition, the film thickness of the Si layer on the outermost surface of the multilayer reflective film 21 can be adjusted within a range that does not reduce the reflectance. The film thickness of the Si (high refractive index layer) on the outermost surface can be 3 nm to 10 nm.

[0097] The method of forming the multilayer reflective film 21 is known. For example, the multilayer reflective film 21 can be formed by depositing each layer by ion beam sputtering. In the case of the Mo / Si periodic multilayer film described above, for example, a Si film having a thickness of about 4 nm is first deposited on the substrate 10 using a Si target by ion beam sputtering, and then a Mo film having a thickness of about 3 nm is deposited using a Mo target. This Si film / Mo film is regarded as one period, and 40 to 60 periods are stacked to form the multilayer reflective film 21 (the outermost layer is a Si layer). In addition, when depositing the multilayer reflective film 21, it is preferable to form the multilayer reflective film 21 by supplying krypton (Kr) ion particles from an ion source and performing ion beam sputtering.

[0098] <Protective film 22> The multilayer reflective film coated substrate 20 (conductive film coated substrate 50) of this embodiment preferably further includes a protective film 22 arranged in contact with the surface of the multilayer reflective film 21 opposite the mask blank substrate 10.

[0099] The protective film 22 is formed on the multilayer reflective film 21 to protect the multilayer reflective film 21 from dry etching and cleaning in the manufacturing process of the reflective mask 40 described later. In addition, the protective film 22 can protect the multilayer reflective film 21 when correcting black defects in a transfer pattern (thin film pattern 24a described later) using an electron beam (EB). The protective film 22 can have a laminated structure of three or more layers. For example, the bottom layer and the top layer of the protective film 22 can be layers made of a material containing Ru, and a metal other than Ru or an alloy of a metal other than Ru can be interposed between the bottom layer and the top layer. The material of the protective film 22 is, for example, composed of a material containing ruthenium as a main component. As the material containing ruthenium as a main component, Ru metal alone or Ru alloys containing metals such as titanium (Ti), niobium (Nb), molybdenum (Mo), zirconium (Zr), yttrium (Y), boron (B), lanthanum (La), cobalt (Co), and / or rhenium (Re) can be used. The material of the protective film 22 can further contain nitrogen. The protective film 22 is effective when the pattern-forming thin film 24 is patterned by dry etching with a Cl-based gas.

[0100] When a Ru alloy is used as the material of the protective film 22, the Ru content of the Ru alloy is 50 atomic % or more and less than 100 atomic %, preferably 80 atomic % or more and less than 100 atomic %, and more preferably 95 atomic % or more and less than 100 atomic %. In particular, when the Ru content of the Ru alloy is 95 atomic % or more and less than 100 atomic %, it is possible to sufficiently ensure the reflectance of EUV light while suppressing the diffusion of the element (silicon) constituting the multilayer reflective film 21 into the protective film 22. Furthermore, this protective film 22 can have a mask cleaning resistance, an etching stopper function when the pattern-forming thin film 24 is etched, and a protective function for preventing the multilayer reflective film 21 from changing over time.

[0101] In the case of EUV lithography, since there are few substances transparent to the exposure light, it is technically not easy to make an EUV pellicle that prevents foreign matter from adhering to the mask pattern surface. For this reason, pellicle-less operation that does not use a pellicle has become mainstream. In addition, in the case of EUV lithography, exposure contamination occurs, such as the deposition of a carbon film on the mask or the growth of an oxide film due to EUV exposure. Therefore, when the EUV reflective mask 40 is used in the manufacture of semiconductor devices, it is necessary to frequently clean the mask to remove foreign matter and contamination on the mask. For this reason, the EUV reflective mask 40 is required to have a mask cleaning resistance that is orders of magnitude higher than that of a transmission mask for optical lithography. If a Ru-based protective film 22 containing Ti is used, the cleaning resistance against cleaning solutions such as sulfuric acid, sulfuric acid / hydrogen peroxide (SPM), ammonia, ammonia / hydrogen peroxide (APM), OH radical cleaning water, and ozone water with a concentration of 10 ppm or less can be particularly increased. Therefore, it is possible to meet the requirements for mask cleaning resistance for the EUV reflective mask 40.

[0102] The thickness of the protective film 22 is not particularly limited as long as it can function as the protective film 22. From the viewpoint of the reflectance of EUV light, the thickness of the protective film 22 is preferably 1.0 nm to 8.0 nm, and more preferably 1.5 nm to 6.0 nm.

[0103] A known film formation method can be used without any particular limitation as the method for forming the protective film 22. Specific examples of the method for forming the protective film 22 include a sputtering method and an ion beam sputtering method.

[0104] The multilayer reflective film coated substrate 20 of this embodiment can have an undercoat film in contact with the main surface of the substrate 10. The undercoat film is a thin film formed between the substrate 10 and the multilayer reflective film 21. By having the undercoat film, charge-up during mask pattern defect inspection using an electron beam can be prevented, and the multilayer reflective film 21 can have fewer phase defects and have high surface smoothness.

[0105] As the material of the undercoat film, a material containing ruthenium or tantalum as a main component is preferably used. Specifically, as the material of the undercoat film, for example, Ru metal alone, Ta metal alone, Ru alloy, or Ta alloy can be used. As the Ru alloy and Ta alloy, those containing metals such as titanium (Ti), niobium (Nb), molybdenum (Mo), zirconium (Zr), yttrium (Y), boron (B), lanthanum (La), cobalt (Co), and / or rhenium (Re) in addition to Ru and / or Ta can be used. The thickness of the undercoat film can be, for example, in the range of 1 nm to 10 nm.

[0106] [Reflective mask blank 30] Next, the reflective mask blank 30 of this embodiment will be described. FIG. 3 is a schematic diagram showing an example of the reflective mask blank 30 of this embodiment. The reflective mask blank 30 of this embodiment has a pattern-forming thin film 24 on the multilayer reflective film 21 or on the protective film 22 of the multilayer reflective film-coated substrate 20 (conductive film-coated substrate 50) described above. That is, the reflective mask blank 30 of this embodiment has a structure in which the multilayer reflective film 21 and the pattern-forming thin film 24 are laminated in this order on one main surface (front main surface) of the substrate 10, and has the above-mentioned predetermined conductive film 23 on the other main surface (rear main surface) of the substrate 10. The reflective mask blank 30 can further have an etching mask film 25 and / or a resist film 32 on the pattern-forming thin film 24 (see FIG. 5 and FIG. 6(a)).

[0107] <Pattern forming thin film 24> The reflective mask blank 30 has a pattern-forming thin film 24 on the multilayer reflective film-coated substrate 20 described above. That is, the pattern-forming thin film 24 is formed on the multilayer reflective film 21 (on the protective film 22 when the protective film 22 is formed). The basic function of the pattern-forming thin film 24 is to absorb EUV light. The pattern-forming thin film 24 may be a pattern-forming thin film 24 intended for absorbing EUV light, or may be a pattern-forming thin film 24 having a phase shift function that takes into account the phase difference of EUV light. The pattern-forming thin film 24 having a phase shift function absorbs EUV light and reflects a part of it to shift the phase. That is, in the reflective mask 40 in which the pattern-forming thin film 24 having a phase shift function is patterned, the portion in which the pattern-forming thin film 24 is formed absorbs and reduces EUV light while reflecting a part of the light at a level that does not adversely affect pattern transfer. In addition, in a region (field portion) where the pattern-forming thin film 24 is not formed, the EUV light is reflected from the multilayer reflective film 21 via the protective film 22. Therefore, a desired phase difference is obtained between the reflected light from the pattern-forming thin film 24 having a phase shift function and the reflected light from the field portion. The pattern-forming thin film 24 having a phase shift function is formed so that the phase difference between the reflected light from the pattern-forming thin film 24 and the reflected light from the multilayer reflective film 21 is 170 degrees to 190 degrees. The light beams having an inverted phase difference of about 180 degrees interfere with each other at the pattern edge portion, thereby improving the image contrast of the projected optical image. The improvement in image contrast leads to an increase in resolution, and various latitudes related to exposure, such as exposure dose latitude and focus latitude, can be increased.

[0108] The pattern-forming thin film 24 may be a single-layer film, or may be a multi-layer film consisting of a plurality of films (for example, a lower-layer pattern-forming thin film and an upper-layer pattern-forming thin film). In the case of a single-layer film, the number of steps during the manufacture of the reflective mask blank 30 can be reduced, and production efficiency can be improved. In the case of a multi-layer film, the optical constants and film thickness of the upper-layer pattern-forming thin film can be appropriately set so that it becomes an anti-reflection film during the mask pattern defect inspection using light. This improves the inspection sensitivity during the mask pattern defect inspection using light. In addition, if a film to which oxygen (O) and nitrogen (N), which improve oxidation resistance, are added is used as the upper-layer pattern-forming thin film, the stability over time is improved. In this way, various functions can be added by making the pattern-forming thin film 24 a multi-layer film. In the case of the pattern-forming thin film 24 having a phase shift function, the range of adjustment on the optical surface can be increased by making it a multi-layer film, so that it becomes easier to obtain a desired reflectance.

[0109] The material of the pattern-forming thin film 24 is not particularly limited as long as it has a function of absorbing EUV light and can be processed by etching or the like (preferably by dry etching with chlorine (Cl) and / or fluorine (F)-based gas). As a material having such a function, tantalum (Ta) alone or a material containing Ta can be preferably used.

[0110] Examples of materials containing Ta include materials containing Ta and B, materials containing Ta and N, materials containing Ta, B and at least one of O and N, materials containing Ta and Si, materials containing Ta, Si and N, materials containing Ta and Ge, materials containing Ta, Ge and N, materials containing Ta and Pd, materials containing Ta and Ru, and materials containing Ta and Ti.

[0111] The pattern-forming thin film 24 can be formed from a material containing at least one selected from the group consisting of, for example, Ni alone, a material containing Ni, Cr alone, a material containing Cr, Ru alone, a material containing Ru, Pd alone, a material containing Pd, Mo alone, and a material containing Mo.

[0112] The pattern-forming thin film 24 can be a thin film similar to the upper layer 232 of the above-mentioned predetermined conductive film 23. That is, the pattern-forming thin film 24 of this embodiment can be a thin film (predetermined thin film) containing chromium (Cr) and having crystallinity. The predetermined thin film can further contain nitrogen. For the predetermined thin film, CuK α When the diffracted X-ray intensity is measured with respect to the diffraction angle 2θ by an X-ray diffraction method using X-rays, the pattern-forming thin film 24 has a predetermined diffracted X-ray spectrum. By containing chromium (Cr) and nitrogen (N) in a predetermined crystal structure having a predetermined diffracted X-ray spectrum, the chemical resistance of the pattern-forming thin film 24, particularly the resistance to SPM cleaning, can be further improved.

[0113] In order to adequately absorb EUV light, the thickness of the pattern-forming thin film 24 is preferably 30 nm to 100 nm.

[0114] The pattern-forming thin film 24 can be formed by a known method, such as magnetron sputtering or ion beam sputtering.

[0115] <Etching mask film 25> An etching mask film 25 may be formed on the pattern-forming thin film 24. The etching mask film 25 is made of a material having a high etching selectivity of the pattern-forming thin film 24 to the etching mask film 25. Here, the "etching selectivity of B to A" refers to the ratio of the etching rate of A, which is a layer that is not to be etched (a layer that serves as a mask), to B, which is a layer that is to be etched. Specifically, it is specified by the formula "etching selectivity of B to A=etching rate of B / etching rate of A". In addition, "high selectivity" refers to a high selectivity value as defined above with respect to a comparative object. The etching selectivity of the pattern-forming thin film 24 to the etching mask film 25 is preferably 1.5 or more, more preferably 3 or more.

[0116] Materials having a high etching selectivity of the pattern-forming thin film 24 to the etching mask film 25 include materials of chromium and chromium compounds. Therefore, when the pattern-forming thin film 24 is etched with a fluorine-based gas, materials of chromium and chromium compounds can be used. Examples of chromium compounds include materials containing Cr and at least one element selected from N, O, C, and H. Also, when the pattern-forming thin film 24 is etched with a chlorine-based gas that does not substantially contain oxygen, materials of silicon and silicon compounds can be used. Examples of silicon compounds include materials containing Si and at least one element selected from N, O, C, and H, as well as materials such as metal silicon (metal silicide) and metal silicon compounds (metal silicide compounds) in which silicon and silicon compounds contain metal. Examples of metal silicon compounds include materials containing metal, Si, and at least one element selected from N, O, C, and H.

[0117] The thickness of the etching mask film 25 is desirably 3 nm or more from the viewpoint of obtaining the function as an etching mask for accurately forming a transfer pattern on the pattern-forming thin film 24. Moreover, the thickness of the etching mask film 25 is desirably 15 nm or less from the viewpoint of making the thickness of the resist film 32 thin.

[0118] The etching mask film 25 can be a thin film similar to the upper layer 232 of the above-mentioned predetermined conductive film 23. That is, the etching mask film 25 of this embodiment can be a thin film (predetermined thin film) containing chromium (Cr) and having crystallinity. The predetermined thin film can further contain nitrogen. For the predetermined thin film, CuK α When the diffracted X-ray intensity is measured with respect to the diffraction angle 2θ by an X-ray diffraction method using X-rays, the etching mask film 25 can have a predetermined diffracted X-ray spectrum. By including chromium (Cr) and nitrogen (N) in a predetermined crystal structure having a predetermined diffracted X-ray spectrum, the chemical resistance of the etching mask film 25, particularly the resistance to SPM cleaning, can be further improved.

[0119] [Reflective mask 40] Next, the reflective mask 40 of this embodiment will be described below. Fig. 4 is a schematic diagram showing the reflective mask 40 of this embodiment. In the reflective mask 40 of this embodiment, a transfer pattern is provided in the pattern-forming thin film 24 of the reflective mask blank 30.

[0120] The reflective mask 40 of the present embodiment has a structure in which the pattern-forming thin film 24 in the above-mentioned reflective mask blank 30 is patterned to form a thin film pattern 24a of the pattern-forming thin film 24 on the multilayer reflective film 21 or on the protective film 22. When the reflective mask 40 of the present embodiment is exposed to exposure light such as EUV light, the exposure light is absorbed in the portions of the surface of the reflective mask 40 where the pattern-forming thin film 24 is present, and the exposure light is reflected by the exposed protective film 22 and multilayer reflective film 21 in the other portions from which the pattern-forming thin film 24 has been removed, and therefore the reflective mask 40 can be used as a reflective mask 40 for EUV lithography.

[0121] According to the reflective mask 40 of this embodiment, by having the thin film pattern 24a on the multilayer reflective film 21 (or on the protective film 22), a predetermined pattern can be transferred onto a transfer target object using EUV light.

[0122] The reflective mask 40 of the present embodiment has a conductive film 23 with excellent chemical resistance. Therefore, even if the reflective mask 40 of the present embodiment is repeatedly cleaned with a chemical such as a chemical solution, deterioration of the reflective mask 40 can be suppressed. Therefore, it can be said that the reflective mask 40 of the present invention can have a highly accurate transfer pattern.

[0123] [Method of manufacturing semiconductor devices] The method for manufacturing a semiconductor device according to this embodiment includes a step of exposing and transferring a transfer pattern to a resist film on a semiconductor substrate using the reflective mask 40 according to this embodiment. That is, by a lithography process using the above-described reflective mask 40 and an exposure apparatus, a transfer pattern such as a circuit pattern based on the thin film pattern 24a of the reflective mask 40 is transferred to a resist film formed on a transfer target such as a semiconductor substrate, and by going through various other steps, a semiconductor device having various transfer patterns formed on a transfer target such as a semiconductor substrate can be manufactured.

[0124] According to the semiconductor device manufacturing method of this embodiment, the reflective mask 40 having the thin film pattern 24a of the conductive film 2324 with excellent chemical resistance can be used for manufacturing a semiconductor device. Even if the reflective mask 40 is repeatedly cleaned with a chemical such as a chemical solution (for example, sulfuric acid / hydrogen peroxide in the case of SPM cleaning), deterioration of the conductive film 23 and / or the thin film pattern 24a of the reflective mask 40 can be suppressed, so that even if the reflective mask 40 is used repeatedly, a semiconductor device having a fine and highly accurate transfer pattern can be manufactured. EXAMPLES

[0125] Hereinafter, examples will be described with reference to the drawings, but the present invention is not limited to the examples.

[0126] [Example 1] First, a conductive-film-attached substrate 50 according to a first embodiment will be described.

[0127] Substrate 10 for manufacturing conductive film-coated substrate 50 of Example 1 was prepared as follows. That is, a SiO2-TiO2-based glass substrate, which is a low-thermal expansion glass substrate having a 6025 size (approximately 152 mm × approximately 152 mm × 6.35 mm) with both the front main surface and the back main surface polished, was prepared as substrate 10. Polishing was performed, consisting of a rough polishing step, a precision polishing step, a local processing step, and a touch polishing step, so as to obtain a flat and smooth main surface.

[0128] A lower layer 231 made of a CrON film was formed on the rear main surface of the SiO2-TiO2-based glass substrate (mask blank substrate 10) of Example 1, and an upper layer 232 made of a CrN film was formed on the lower layer 231 to form a conductive film 23.

[0129] The CrON film (lower layer 231) was formed to a thickness of 15 nm by reactive sputtering (DC magnetron sputtering) using a Cr target in a mixed gas atmosphere of Ar gas, N2 gas, and O2 gas. The composition (atomic %) of the CrON film was measured by X-ray photoelectron spectroscopy (XPS method), and the atomic ratio was 88 atomic % chromium (Cr), 6 atomic % oxygen (O), and 6 atomic % nitrogen (N).

[0130] Subsequently, an upper layer 232 made of a CrN film was formed on the lower layer 231. The CrN film (upper layer 232) was formed to a thickness of 180 nm by reactive sputtering (DC magnetron sputtering) using a Cr target in a mixed gas atmosphere of Ar gas and N2 gas. The composition (atomic %) of the CrN film was measured by X-ray photoelectron spectroscopy (XPS method), and the atomic ratio was 91 atomic % for chromium (Cr) and 9 atomic % for nitrogen (N).

[0131] For the conductive film 23 of Example 1, CuK α The diffracted X-ray intensity was measured against the diffraction angle 2θ by X-ray diffraction using a Cu-K α Measurements were performed using a radiation source with a diffraction angle 2θ in the range of 30 degrees to 70 degrees, a sampling width of 0.01 degrees, and a scan speed of 2 degrees / min. αX-rays generated by a radiation source were irradiated, and the diffracted X-ray intensity at the diffraction angle 2θ was measured to obtain a diffracted X-ray spectrum. From the obtained diffracted X-ray spectrum, the presence or absence of peaks in the range of the diffraction angle 2θ of 56 degrees or more and 60 degrees or less, the range of 41 degrees or more and 47 degrees or less, and the range of 35 degrees or more and 38 degrees or less was judged. The presence or absence of a peak was judged to be present when the height of the peak when the background was subtracted from the measured diffracted X-ray spectrum was twice or more than the noise level (noise width) of the background near the peak. Since no peak of the CrON film (lower layer 231) was observed in the obtained diffracted X-ray spectrum, it can be said that the diffracted X-ray spectrum obtained by the measurement is the diffracted X-ray spectrum of the CrN film (upper layer 232). This point is the same for the diffracted X-ray spectra of Comparative Examples 1 and 2.

[0132] Fig. 7 shows the diffraction X-ray spectrum of Example 1. As is clear from Fig. 7, the conductive film 23 (upper layer 232) of Example 1 had peaks in the diffraction angle 2θ range of 56 degrees or more and 60 degrees or less and in the range of 41 degrees or more and 47 degrees or less, but had no peaks in the diffraction angle 2θ range of 35 degrees or more and 38 degrees or less. Table 1 shows the presence or absence of peaks in each diffraction angle 2θ range of Example 1.

[0133] In this manner, the conductive layer-attached substrate 50 of Example 1 was manufactured.

[0134] Here, a conductive film was formed on the substrate 10 under the same film forming conditions as described above to prepare a thin film for evaluation in Example 1. The surface roughness (Rms), sheet resistance (Ω / □), and film loss (nm) due to SPM cleaning of the obtained thin film for evaluation in Example 1 were measured. The measurement results are shown in Table 1.

[0135] The amount of film loss (nm) due to SPM cleaning of the conductive film-coated substrate 50 of Example 1 was calculated by measuring the film thickness before and after one SPM cleaning under the cleaning conditions below. Cleaning solution H2SO4:H2O2=2:1 (weight ratio) Washing temperature: 120℃ Washing time: 10 minutes

[0136] In the manner described above, the conductive-layer-attached substrate 50 of Example 1 was manufactured and evaluated.

[0137] [Comparative Example 1] The conductive film-coated substrate 50 of Comparative Example 1 has a conductive film 23 consisting of a lower layer 231 of a CrON film and an upper layer 232 of a CrN film, similar to Example 1. However, the deposition conditions (flow rate of N2 gas) and atomic ratio of the CrN film (upper layer 232) of the conductive film 23 of Comparative Example 1 are different from those of Example 1. The rest is similar to Example 1. The CrN film (upper layer 232) of Comparative Example 1 was deposited to a thickness of 180 nm. The composition (atomic %) of the CrN film (upper layer 232) was measured by X-ray photoelectron spectroscopy (XPS method), and was found to be 84 atomic % chromium (Cr) and 16 atomic % nitrogen (N).

[0138] As in Example 1, the conductive film 23 (upper layer 232) of Comparative Example 1 was coated with CuK α The diffracted X-ray intensity versus diffraction angle 2θ was measured by an X-ray diffraction method using X-rays. FIG. 8 shows the diffracted X-ray spectrum of Comparative Example 1. As is clear from FIG. 8, the upper layer 232 of the conductive film 23 of Comparative Example 1 had no peaks in any of the ranges of diffraction angle 2θ of 56 degrees or more and 60 degrees or less, 41 degrees or more and 47 degrees or less, and 35 degrees or more and 38 degrees or less. From this, it can be said that the conductive film 23 of Comparative Example 1 is a thin film with an amorphous structure. Table 1 shows the presence or absence of peaks in each range of diffraction angle 2θ of Comparative Example 1.

[0139] Here, a thin film for evaluation of Comparative Example 1 was prepared by forming a conductive film on the substrate 10 under the same film forming conditions as those of Comparative Example 1. As in Example 1, the surface roughness (Rms), sheet resistance (Ω / □), and film loss (nm) due to SPM cleaning of the thin film for evaluation of Comparative Example 1 were measured. Table 1 shows the measurement results.

[0140] In the manner described above, the conductive layer-attached substrate 50 of Comparative Example 1 was manufactured and evaluated.

[0141] [Comparative Example 2] The conductive film-attached substrate 50 of Comparative Example 2 differs from the conductive film-attached substrate 50 of Example 1 in that the conductive film 23 is composed only of the upper layer 232 of Example 1. The rest is the same as Example 1. That is, the conductive film 23 of Comparative Example 2 is a CrN film formed to a thickness of 180 nm under the same film-forming conditions as the upper layer 232 of Example 1. The composition (atomic %) of the conductive film (CrN film) 23 was measured by X-ray photoelectron spectroscopy (XPS method), and was found to be 91 atomic % chromium (Cr) and 9 atomic % nitrogen (N).

[0142] As in Example 1, the conductive film 23 of Comparative Example 2 was coated with CuK α The diffracted X-ray intensity was measured with respect to the diffraction angle 2θ by an X-ray diffraction method using X-rays. As a result, the same tendency as in the upper layer 232 of Example 1 was observed.

[0143] Here, a conductive film was formed on the substrate 10 under the same film formation conditions as in Comparative Example 2 to prepare a thin film for evaluation in Comparative Example 2. As in Example 1, the surface roughness (Rms), sheet resistance (Ω / □), and film loss (nm) due to SPM cleaning of the thin film for evaluation in Comparative Example 2 were measured. Table 1 shows the measurement results.

[0144] In the manner described above, the conductive-layer-attached substrate 50 of Comparative Example 2 was manufactured and evaluated.

[0145] [Comparison between Example 1, Comparative Example 1 and Comparative Example 2] As shown in Table 1, the sheet resistance of the conductive film 23 of the conductive film-coated substrate 50 in Example 1 was 150 Ω / □ or less, a satisfactory value for the conductive film 23 of the reflective mask 40. Furthermore, the amount of film loss of the conductive film 23 in Example 1 due to SPM cleaning was 0.1 nm, a satisfactory value for the conductive film 23 of the reflective mask 40. Furthermore, the surface roughness (Rms) of the conductive film 23 in Example 1 was 0.31 nm, which means that it is possible to prevent the generation of particles due to rubbing between the conductive film 23 and the electrostatic chuck.

[0146] As shown in Table 1, the sheet resistance of the conductive film 23 of the conductive-film-coated substrate 50 of Comparative Example 1 was 150 Ω / □ or less, which was a satisfactory value for the conductive film 23 of the reflective mask 40. In addition, the surface roughness (Rms) of the conductive film 23 of Comparative Example 1 was 0.28 nm, which means that it is possible to prevent the generation of particles due to rubbing between the conductive film 23 and the electrostatic chuck. However, the amount of film reduction of the conductive film 23 of Comparative Example 1 due to SPM cleaning was 1.4 nm, which was not a satisfactory value for the conductive film 23 of the reflective mask 40.

[0147] As shown in Table 1, the sheet resistance of the conductive film 23 of the conductive-film-coated substrate 50 of Comparative Example 2 was 150 Ω / □ or less, a satisfactory value for the conductive film 23 of the reflective mask 40. Furthermore, the amount of film loss of the conductive film 23 of Comparative Example 2 due to SPM cleaning was 0.1 nm, a satisfactory value for the conductive film 23 of the reflective mask 40. However, since the surface roughness (Rms) of the conductive film 23 of Comparative Example 2 was 0.71 nm, it can be said that it is difficult to prevent the generation of particles due to rubbing between the conductive film 23 and the electrostatic chuck.

[0148] From the above, it is clear that the conductive film 23 of the reflective mask 40 of Example 1 is a conductive film 23 having excellent chemical resistance and small surface roughness (Rms).

[0149] [Substrate with multilayer reflective film 20] Next, a description will be given of the multilayer reflective film coated substrate 20 of Example 1. The multilayer reflective film coated substrate 20 was manufactured by forming a multilayer reflective film 21 and a protective film 22 on the front main surface of the substrate 10 opposite to the side on which the conductive film 23 of the conductive film coated substrate 50 manufactured as described above was formed. Specifically, the multilayer reflective film coated substrate 20 was manufactured as follows.

[0150] A multilayer reflective film 21 was formed on the front main surface of the substrate 10 opposite to the side on which the conductive film 23 was formed. The multilayer reflective film 21 formed on the substrate 10 was a periodic multilayer reflective film 21 made of Mo and Si in order to make the multilayer reflective film 21 suitable for EUV light with a wavelength of 13.5 nm. The multilayer reflective film 21 was formed by alternately stacking Mo layers and Si layers on the substrate 10 by ion beam sputtering in an Ar gas atmosphere using a Mo target and a Si target. First, a Si film was formed to a thickness of 4.2 nm, and then a Mo film was formed to a thickness of 2.8 nm. This was set as one period, and 40 periods were similarly stacked, and finally a Si film was formed to a thickness of 4.0 nm to form the multilayer reflective film 21. Here, 40 periods were used, but this is not limited thereto, and for example, 60 periods may be used. In the case of 60 periods, the number of steps increases compared to 40 periods, but the reflectance for EUV light can be increased.

[0151] Subsequently, a protective film 22 made of a Ru film was formed to a thickness of 2.5 nm by ion beam sputtering using a Ru target in an Ar gas atmosphere.

[0152] In this manner, the multilayer reflective film coated substrate 20 of Example 1 was produced.

[0153] [Reflective mask blank 30] Next, a description will be given of the reflective mask blank 30 of Example 1. The reflective mask blank 30 was manufactured by forming a thin film 24 for pattern formation on the protective film 22 of the multilayer reflective film coated substrate 20 manufactured as described above.

[0154] A pattern-forming thin film 24 was formed on the protective film 22 of the multilayer reflective film-coated substrate 20 by DC magnetron sputtering. The pattern-forming thin film 24 was a laminated film consisting of two layers, a TaN film as an absorption layer and a TaO film as a low-reflection layer. A TaN film was formed as an absorption layer on the surface of the protective film 22 of the multilayer reflective film-coated substrate 20 by DC magnetron sputtering. This TaN film was formed by placing the multilayer reflective film-coated substrate 20 opposite a Ta target and by reactive sputtering in a mixed gas atmosphere of Ar gas and N2 gas. Next, a TaO film (low-reflection layer) was further formed on the TaN film by DC magnetron sputtering. This TaO film was formed by placing the multilayer reflective film-coated substrate 20 opposite a Ta target and by reactive sputtering in a mixed gas atmosphere of Ar gas and O2 gas, similar to the TaN film.

[0155] The composition (atomic ratio) of the TaN film was Ta:N=70:30, and the thickness was 48 nm.The composition (atomic ratio) of the TaO film was Ta:O=35:65, and the thickness was 11 nm.

[0156] In this manner, the reflective mask blank 30 of Example 1 was produced.

[0157] [Reflective mask 40] Next, a description will be given of a reflective mask 40 of Example 1. The reflective mask 40 was manufactured using the above-mentioned reflective mask blank 30. FIG. 6 is a schematic cross-sectional view of a main part illustrating a process for producing the reflective mask 40 from the reflective mask blank 30.

[0158] A resist film 32 was formed to a thickness of 150 nm on the pattern-forming thin film 24 of the reflective mask blank 30 of Example 1 described above to obtain the reflective mask blank 30 (FIG. 6(a)). A desired pattern was drawn (exposed) on this resist film 32, and then developed and rinsed to form a predetermined resist pattern 32a (FIG. 6(b)). Next, using the resist pattern 32a as a mask, the pattern-forming thin film 24 was dry-etched to form a pattern (thin film pattern 24a) of the pattern-forming thin film 24 (FIG. 6(c)). The TaN film and TaO film of the pattern-forming thin film 24 were both patterned by dry etching using a mixed gas of CF4 and He.

[0159] Thereafter, the resist pattern 32a was removed by ashing or a resist remover. Finally, SPM cleaning was performed under the same cleaning conditions as in the measurement of the amount of film loss by SPM cleaning described above. In this manner, a reflective mask 40 was manufactured (FIG. 6(d)). If necessary, a mask defect inspection can be performed after wet cleaning, and mask defect repair can be performed as appropriate.

[0160] As described in the evaluation of the conductive film-attached substrate 50 of Example 1 above, the conductive film-attached substrate 50 having the conductive film 23 of Example 1 of this embodiment has excellent SPM cleaning resistance. Therefore, the reflective mask 40 having the conductive film 23 of this embodiment also has excellent SPM cleaning resistance. Therefore, even if the reflective mask 40 is subjected to SPM cleaning, the sheet resistance and mechanical strength required for the conductive film 23 are not impaired. Therefore, even if the reflective mask 40 of this embodiment is used for manufacturing a semiconductor device, it can be fixed by an electrostatic chuck without any problems. In addition, the surface roughness (Rms) of the conductive film-attached substrate 50 having the conductive film 23 of Example 1 of this embodiment is small. Therefore, it is possible to prevent the generation of particles due to friction between the conductive film 23 and the electrostatic chuck. Therefore, when the reflective mask 40 of this embodiment is used for manufacturing a semiconductor device, it can be said that a semiconductor device having a fine and highly accurate transfer pattern can be manufactured.

[0161] Each reflective mask 40 produced in Example 1 was set in an EUV exposure device, and EUV exposure was performed on a wafer having a processing film and a resist film formed on a semiconductor substrate. Then, a resist pattern was formed on the semiconductor substrate having the processing film formed thereon by developing the exposed resist film.

[0162] This resist pattern is transferred to the film to be processed by etching, and then various processes such as forming an insulating film and a conductive film, introducing a dopant, and annealing are carried out to manufacture a semiconductor device having the desired characteristics.

[0163] [Table 1] [Explanation of symbols]

[0164] 10 Mask blank substrate 20 Substrate with multilayer reflective film 21 Multilayer reflective film 22 Protective film 23 Conductive Film 24 Thin films for pattern formation 24a Thin film pattern 25 Etching mask film 30 Reflective mask blanks 32 Resist film 32a Resist pattern 40 Reflective mask 50 Conductive film substrate 231 Lower layer 232 Upper layer

Claims

1. A substrate with a conductive film, the substrate having a conductive film on one of two main surfaces thereof, the conductive film has a structure in which a lower layer and an upper layer are laminated in this order from the substrate side, the lower layer is amorphous and the upper layer is crystalline; the upper layer contains chromium and nitrogen, and when diffracted X-ray intensity is measured with respect to a diffraction angle 2θ by an X-ray diffraction method, the upper layer has a peak in a diffraction angle 2θ range of 41 degrees or more and 47 degrees or less; The conductive film has a root mean square roughness (Rms) of 0.5 nm or less.

2. 2. The substrate with a conductive film according to claim 1, wherein the mechanical strength of the conductive film is 300 mN or more in terms of a crack initiation load.

3. 3. The substrate with a conductive film according to claim 1, wherein the upper layer has a peak in the range of the diffraction angle 2θ of 56 degrees or more and 60 degrees or less.

4. 4. The substrate with a conductive film according to claim 1, wherein the nitrogen content of the upper layer is 1 atomic % or more and 15 atomic % or less.

5. 5. The substrate with a conductive film according to claim 1, wherein the upper layer further contains at least one selected from the group consisting of Ag, Au, Cu, Al, Mg, W, Ru, and Co.

6. A substrate with a conductive film, characterized in that a multilayer reflective film formed by alternately stacking high refractive index layers and low refractive index layers is formed on the main surface opposite to the side on which the conductive film of the substrate described in any one of claims 1 to 5 is formed.

7. 7. The substrate with a conductive film according to claim 6, wherein a protective film is formed on the multilayer reflective film.

8. A reflective mask blank having a structure in which a multilayer reflective film and a thin film for pattern formation are laminated in this order on one main surface of a substrate, a conductive film on the other main surface of the substrate; the conductive film has a structure in which a lower layer and an upper layer are laminated in this order from the substrate side, the lower layer is amorphous and the upper layer is crystalline; the upper layer contains chromium and nitrogen, and when diffracted X-ray intensity is measured with respect to a diffraction angle 2θ by an X-ray diffraction method, the upper layer has a peak in a diffraction angle 2θ range of 41 degrees or more and 47 degrees or less; A reflective mask blank, wherein the conductive film has a root mean square roughness (Rms) of 0.5 nm or less.

9. 9. The reflective mask blank according to claim 8, wherein the conductive film has a mechanical strength of 300 mN or more in terms of a crack initiation load.

10. 10. The reflective mask blank according to claim 8, wherein the upper layer has a peak in the range of the diffraction angle 2θ of 56 degrees or more and 60 degrees or less.

11. 11. The reflective mask blank according to claim 8, wherein the nitrogen content of the upper layer is 1 atomic % or more and 15 atomic % or less.

12. 12. The reflective mask blank according to claim 8, wherein the upper layer further contains at least one selected from Ag, Au, Cu, Al, Mg, W, Ru, and Co.

13. 13. The reflective mask blank according to claim 8, wherein a protective film is formed between the multilayer reflective film and the pattern-forming thin film.

14. A reflective mask, characterized in that a transfer pattern is provided in the pattern-forming thin film of the reflective mask blank according to any one of claims 8 to 13.

15. 15. A method for manufacturing a semiconductor device, comprising the step of exposing and transferring a transfer pattern onto a resist film on a semiconductor substrate using the reflective mask according to claim 14.

Citation Information

Patent Citations

  • Coating of reflective mask substrates

    JP2003501823A

  • Fluorescence x-ray spectrometer, and program used therefor

    JP2007139754A

  • WEAR-RESISTANT CrN FILM

    JP2010168603A

  • Reflective mask blank for EUV lithography, substrate with function film for the mask blank, and methods for their production

    JP2015215602A

  • Reflective mask blank for EUV lithography, and substrate with function film for the mask blank

    WO2008072706A1