Laminated fiber sheet and method of using same

The laminated fiber sheet addresses the issue of stickiness and permeability in ultrafine fiber sheets by integrating inner and outer sheets with different diameters, ensuring a moist state on the inner surface and a dry state on the outer surface, thereby improving adhesion and reducing stuffiness.

JP7569466B2Active Publication Date: 2024-10-17KAO CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2024022028
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2023-02-22
Filing Date
2024-02-16
Publication Date
2024-10-17
Estimated Expiration
2044-02-16

AI Technical Summary

Technical Problem

Fiber sheets containing ultrafine fibers are prone to high liquid permeability, leading to stickiness and transfer of liquid to surrounding objects, and existing solutions like vinyl cause stuffiness, limiting their effective wearing time.

Method used

A laminated fiber sheet with an inner sheet and an outer sheet, where the inner sheet has a median fiber diameter of 0.3 μm to 5 μm and the outer sheet has a larger diameter, integrated to prevent liquid transfer to the outer surface while maintaining a moist state on the inner surface.

Benefits of technology

The laminated fiber sheet effectively prevents stickiness on the outer surface and maintains a continuous moist state on the inner surface, enhancing adhesion and liquid retention while reducing stuffiness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569466000004
    Figure 0007569466000004
  • Figure 0007569466000005
    Figure 0007569466000005
  • Figure 0007569466000006
    Figure 0007569466000006
Patent Text Reader

Abstract

To provide a laminated fiber sheet capable of preventing stuffiness and outside stickiness while simultaneously producing a sustainable wet state of liquid material, and also to provide a method for using the same.SOLUTION: A method for using a laminated fiber sheet moisturizes a laminated fiber sheet having an inner sheet laminated on one surface of an outer sheet with a liquid material. The inner sheet and the outer sheet of the laminated fiber sheet is non-soluble in the liquid material. The median fiber diameter of the inner sheet is 0.3 μm or more and 5 μm or less. The median fiber diameter of the outer sheet is larger than that of the inner sheet. The inner sheet and the outer sheet are integrated. The method for using the laminated fiber sheet includes a step to apply the laminated fiber sheet by making the inner sheet face toward an object and a step to apply the liquid material.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a laminated fiber sheet and a method for using the same. [Background technology]

[0002] Among sheets containing fibers (hereinafter referred to as fiber sheets), there are ones made by depositing ultrafine fibers (fiber diameter of 5 μm or less, for example), which have been attracting attention in recent years. As an example of a spinning technique for uniformly producing a fiber sheet made of such fine fibers, for example, an electric field spinning method (electrospinning method) is used. Such fiber sheets containing ultrafine fibers are expected to be used for various purposes in the future, and intensive research is being conducted for industrialization.

[0003] For example, Patent Document 1 describes a nanofiber sheet having a base layer releasably disposed on one side of a nanofiber layer made of nanofibers with a circle equivalent diameter of 3000 nm or less. It describes that the nanofiber sheet is brought into contact with the surface of an object, and then the base layer is peeled off to transfer the nanofiber layer to the surface of the object. In this case, it is said that the transfer can be performed successfully by keeping the surface of the nanofiber layer or the surface of the object in a moist state. In the nanofiber sheet described in Patent Document 2, the nanofiber layer has a gradation region in which the thickness gradually increases from the peripheral edge toward the inside. It is described that the base layer is peeled off from the nanofiber sheet, and the remaining nanofiber layer is attached to an object for use. When the nanofiber layer is attached to an object, the gradation region makes the outer edge of the nanofiber layer less noticeable and difficult to see. Patent Document 3 describes a cosmetic sheet in which cosmetics or cosmetic ingredients are held in a mesh structure made of nanofibers of 2000 nm or less. Patent Document 4 describes a hand mask made of a material with liquid-retaining properties as an item for holding liquid such as cosmetics. There is no mention of nanofibers as described above, and general nonwoven fabrics, paper, absorbent cotton, etc. are listed as the material with liquid-retaining properties. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2010-167780 A [Patent Document 2] JP 2020-90097 A [Patent Document 3] JP 2008-179629 A [Patent Document 4] JP 2017-137585 A Summary of the Invention [Problem to be solved by the invention]

[0005] The above-mentioned sheet containing ultrafine fibers is useful for creating a continuous and uniform wet state of liquid, as described in Patent Document 3. However, such an ultrafine fiber sheet has high liquid permeability, so when used alone, not only the surface facing the object but also the outer surface on the opposite side is likely to become wet. Therefore, when the ultrafine fiber sheet holding the liquid is attached to the object, the outside becomes sticky, and the liquid may be transferred to surrounding objects. In this regard, as described in Patent Document 4, a material with liquid-proof properties such as vinyl can be placed on the outside. However, taking into consideration the possibility of stuffiness caused by vinyl, etc., there is a limit to the time the mask can be worn. Patent Documents 1 and 2 do not mention this issue.

[0006] In view of the above, the present invention relates to a laminated fiber sheet that can prevent stuffiness and suppress stickiness on the outside, while at the same time creating a sustained wet state for liquid materials. [Means for solving the problem]

[0007] The present invention provides a method for using a laminated fibrous sheet, which comprises an inner sheet laminated on one side of an outer sheet, to wet the laminated fibrous sheet with a liquid. The inner sheet and the outer sheet are preferably insoluble in liquids. The inner sheet preferably has a median fiber diameter of 0.3 μm or more and 5 μm or less. The outer sheet preferably has a larger median fiber diameter than the inner sheet. It is preferable that the inner sheet and the outer sheet are integral with each other. A method for using the laminated fiber sheet preferably includes the steps of applying the laminated fiber sheet with the inner sheet facing an object, and applying the liquid material.

[0008] The present invention also provides a laminated fibrous sheet comprising an inner sheet laminated to one side of an outer sheet. The laminated fiber sheet preferably has the above-described structure of the inner sheet and the outer sheet. It is preferable that the laminated fiber sheet contains a liquid material, and the liquid material is unevenly distributed in the inner sheet. Effect of the Invention

[0009] The laminated fiber sheet of the present invention is capable of preventing stuffiness and suppressing stickiness on the outside, while at the same time creating a sustained moist state for liquid materials. [Brief description of the drawings]

[0010] [Figure 1] 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a laminated fiber sheet according to the present invention. [Diagram 2]Photograph (A) is a drawing substitute photograph showing the inner sheet alone being pinched between fingers, and photograph (B) is a drawing substitute photograph showing the laminated fiber sheet of the present invention being pinched between fingers. [Diagram 3] FIG. 4 is an explanatory diagram illustrating fusion-bonding points at intersections between ultrafine fibers of the inner sheet. [Figure 4] FIG. 4 is a photograph substituted for a drawing, showing an example of an observation image used when measuring the ratio of the number of fusion-bonded points to the number of fiber intersections. [Diagram 5] 1A and 1B are schematic diagrams showing an example in which fusion points are included at the intersections between the fibers of the inner sheet and the outer sheet at the interface between the sheets, where (A) shows the sheet before stretching and (B) shows the sheet in the stretched state. [Figure 6] FIG. 1 is an explanatory diagram illustrating a schematic diagram of an example of the laminated fiber sheet of the present invention in a state where it is applied to an object. [Figure 7] In Example 1, (A) is a photograph substituting a drawing showing the result of transfer of a liquid from an outer sheet to a filter paper, and (B) is a photograph substituting a drawing showing the result of transfer of a liquid from an inner sheet to a filter paper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, a preferred embodiment of the laminated fiber sheet of the present invention will be described with reference to the drawings.

[0012] The laminated fiber sheet 10 of the present invention preferably includes an inner sheet 1 laminated on one surface of an outer sheet 2. The inner sheet 1 is preferably arranged on one surface side 10T of the front and back surfaces of the laminated fiber sheet 10, and the outer sheet 2 is preferably arranged on the other surface side 10B opposite to the one surface side 10T. In the method of use, the laminated fiber sheet 10 of the present invention is typically applied with the inner sheet 1 facing an object described below. Application to an object means that the laminated fiber sheet 10 is brought into contact with the surface of the object. The laminated fiber sheet 10 is preferably attached to the object by the action of its wetting.

[0013] The laminated fiber sheet 10 of the present invention may further include another fiber layer in the inner sheet 1 and the outer sheet 2. In this case, from the viewpoint of making the properties of the inner sheet 1, which will be described later, more effective and not impairing the cooperation between the inner sheet 1 and the outer sheet 2, it is preferable that the other fiber layer is located on the other surface side 10B of the outer sheet 2. That is, in either case, it is preferable that the inner sheet 1 and the outer sheet 2 are adjacent to each other.

[0014] In the method of use, the laminated fiber sheet 10 of the present invention is typically made to contain a liquid and be in a wet state. More specifically, the inner sheet 1 (particularly the surface of the inner sheet 1 facing the object) is made to be in a wet state with the liquid. The "wet state" or "wet state" refers to a state in which the laminated fiber sheet 10 is moistened with the liquid, i.e., a state in which the liquid is present. The method of use of the laminated fiber sheet 10 and the action of the laminated fiber sheet 10 in response to the liquid in the method of use will be described later. In addition, the amount of liquid to be applied to the laminated fiber sheet 10 to make it wet is preferably 0.2 mg / cm. 2 More preferably, it is 0.3 mg / cm or more. 2 More preferably, it is 0.4 mg / cm 2 or more, preferably 10 mg / cm 2 More preferably, it is 7 mg / cm or less. 2 and even more preferably 5 mg / cm 2 and even more preferably 4 mg / cm 2 The following is the result.

[0015] The "liquid" means a substance that is liquid at 20° C. In addition, in the present invention, the "liquid" refers to a substance that is wetted into the laminated fiber sheet. Examples of the liquid include liquids such as water, aqueous solutions and aqueous dispersions, gels thickened with a thickener, oils that are liquid or solid at 20° C., oil agents containing 10% by mass or more of the oil, and emulsions (O / W emulsions, W / O emulsions) containing the oil and a surfactant such as a nonionic surfactant.

[0016] The liquid preferably contains a polyol that is liquid at 20° C. This makes it difficult for the liquid to lose its transparent state due to evaporation. The polyol may include, for example, one or more selected from ethylene glycol, propylene glycol, 1,3-butanediol, dipropylene glycol, polyethylene glycol having a mass average molecular weight of 2000 or less, glycerin, and diglycerin.

[0017] The liquid material may contain an oil that is liquid at 20° C. The oil may contain one or more oils selected from the group consisting of hydrocarbon oils, esters of linear or branched fatty acids, linear or branched alcohols or polyhydric alcohols, ester oils, and silicone oils. The hydrocarbon oil may include one or more selected from liquid paraffin, squalane, squalene, n-octane, n-heptane, cyclohexane, light isoparaffin, and liquid isoparaffin. The ester of a straight-chain or branched-chain fatty acid and a straight-chain or branched-chain alcohol or polyhydric alcohol may include one or more selected from octyldodecyl myristate, myristyl myristate, isocetyl stearate, isocetyl isostearate, cetearyl isononanoate, diisobutyl adipate, di-2-ethylhexyl sebacate, isopropyl myristate, isopropyl palmitate, diisostearyl malate, neopentyl glycol dicaprate, and alkyl benzoate (having 12 to 15 carbon atoms). The ester oil may include one or more selected from triglycerin fatty acid esters (triglycerides). Triglycerol fatty acid esters can include tri(caprylic acid / capric acid)glycerol and the like. The silicone oil may include one or more selected from dimethylpolysiloxane, dimethylcyclopolysiloxane, methylphenylpolysiloxane, methylhydrogenpolysiloxane, and higher alcohol-modified organopolysiloxane.

[0018] The liquid may contain an oil that is solid at 20° C. The oil may contain one or more oils selected from the group consisting of petrolatum, cetanol, stearyl alcohol, and ceramide.

[0019] Such liquids preferably do not contain pharmaceutical agents and are used for cosmetic or aesthetic purposes.

[0020] The "subject" to which the laminated fiber sheet 10 is applied may include various objects, such as, but not limited to, human skin, human nails, teeth, gums, and hair, the skin, nails, teeth, gums, and plant surfaces such as branches and leaves of non-human mammals, and the like.

[0021] The method of using the laminated fiber sheet 10 by wetting it with the liquid and applying it to the object may, for example, be intended to cosmetically and aesthetically improve the surface condition of the object. For example, when the object is human skin, the method is preferably used for the purpose of enhancing the barrier function or moisturizing function of the skin, whitening the skin, concealing wrinkles or blemishes, applying makeup, or otherwise beautifying the appearance. The method of use preferably does not include a method of surgery, treatment, or diagnosis of a human being by a doctor or a person under the instruction of a doctor.

[0022] The inner sheet 1 and the outer sheet 2 of the laminated fiber sheet 10 of the present invention are preferably insoluble in the liquid. Insoluble in the liquid means that no reduction or change in fiber diameter due to dissolution is observed. Specifically, it means that a 50 mm square laminated fiber sheet is immersed in the liquid equivalent to 10 times its mass in an environment of 1 atmosphere and 23°C, and after 24 hours, the median fiber diameter of each layer after immersion is equal to or greater than the median fiber diameter before immersion. The measurement method is based on the method of measuring the median fiber diameter described below. The above-mentioned measuring method can be applied to any type of liquid, so long as it is capable of wetting the laminated fiber sheet. For example, when the liquid is water, the above measurement is carried out using deionized water.

[0023] The inner sheet 1 preferably contains fibers (also called nanofibers) with a median fiber diameter (P1) of 0.3 μm to 5 μm. These fibers are also called ultrafine fibers or nanofibers, and can be formed, for example, by electrospinning. In such an inner sheet 1, the fineness of the fibers reduces the unevenness of the individual fibers compared to conventional fiber layers such as nonwoven fabrics, and the contact area with the target surface (for example, the skin surface) is increased, resulting in high adhesion to the target surface. The outer sheet 2 preferably has a larger median fiber diameter than the inner sheet 1. Examples of such an outer sheet 2 include nonwoven fabrics obtained by a spunbonding method (hereinafter, also referred to as spunbonded nonwoven fabrics). In addition, it is preferable that the inner sheet 1 and the outer sheet 2 are integrated together. Specifically, it is preferable that the inner sheet 1 and the outer sheet 2 are adjacent to each other and integrated together by fusion of the fibers constituting the inner sheet 1 and the fibers constituting the outer sheet 2. As a result, a very strong capillary force acts from the outer sheet 2 to the inner sheet 1 in the thickness direction of the laminated fiber sheet 10. In addition, the inner sheet 1 has a high liquid retention capacity due to the extremely large specific surface area of ​​the ultrafine fibers described above, and is excellent in preventing liquid from returning to the outer sheet 2, which is a fiber layer laminated thereon.

[0024] (Method of measuring median fiber diameter) (1) The laminated fiber sheet 10 is peeled between the fiber layers to take out the fiber layer to be measured. This fiber layer is cut to 10 mm x 10 mm. This is attached to a sample stage for a scanning electron microscope (manufactured by Oken Shoji Co., Ltd.) via conductive carbon double-sided tape (manufactured by Oken Shoji Co., Ltd.). (2) The sample stage with the fiber layer attached is placed in a sputtering device (Ion Sputter E-1030, Hitachi High-Tech Corporation). The pressure is reduced to 6 Pa under an argon gas atmosphere, and platinum-palladium (Pt-Pd) deposition is performed. The distance between the fiber layer mounting surface and the Pt-Pd electrode is 30 mm, the deposition time is 80 seconds, and the current value during deposition is 30 mA. (3) The sample stage is placed in a scanning electron microscope (SEM) (Hitachi High-Tech Corporation, S-4300SE / N) and images are obtained in high-resolution mode (accelerating voltage: 5 kV, work distance: 10 mm, observation magnification 500x or 1000x). Images are obtained from a total of 15 locations on the same sample by changing the observation location. (4) From the observation image acquired in (3), the fiber diameter of the fiber layer is measured using image analysis software (WinRooF2015 manufactured by Mitani Shoji Co., Ltd.). From the measured fiber diameters of a total of 600 fibers, the number average diameter, the number 10% diameter (D10) (from the thin diameter side), the number 50% diameter (median diameter), and the number 90% diameter (D90) are tallied. Of these, the median diameter is taken as the representative value of the fiber diameter.

[0025] Due to the above action, when the laminated fiber sheet 10 contains the liquid during use, the liquid exhibits the ability to migrate from the outer sheet 2 to the inner sheet 1. Not only when the liquid is applied from the surface side (the other surface side 10B) of the outer sheet 2 of the laminated fiber sheet 10, but also when the liquid is contained throughout the laminated fiber sheet 10, the liquid is likely to migrate to the inner sheet 1. In addition, the inner sheet 1 acts to push back or retain the liquid that attempts to return to the outer sheet 2 in the inner sheet 1. Furthermore, the inner sheet 1, containing the liquid, becomes a liquid-retaining layer, forming a uniform liquid film between the inner sheet 1 and the surface of the object, and can retain the liquid film for a long period of time. This is due to the above-mentioned action as well as the fact that the inner sheet 1 has a fiber structure made of ultrafine fibers, which reduces the unevenness of individual fibers as in the past, thereby contributing to excellent smoothness on the object surface. In this way, the laminated fiber sheet 10 of the present invention, through the cooperative action of the outer sheet 2 and the inner sheet 1, forms a uniform liquid film (uniformly wet state) of the liquid on the inner sheet 1, dramatically increasing the adhesion between the liquid and the surface of the object compared to conventional methods, and can maintain that state for a long time. This allows the liquid to act uniformly on the object for a long time.

[0026] This allows the laminated fiber sheet 10 to contain the liquid and have the liquid unevenly distributed on the inner sheet 1 in a wet state, and this state is easily maintained. As a result, the surface side of the outer sheet 2 (the other surface side 10B) of the laminated fiber sheet 10 is easily brought into a dry state, and this state is easily maintained. In other words, the laminated fiber sheet 10 can be brought into a state in which stickiness due to the liquid is suppressed even when the surface side of the outer sheet 2 (the other surface side 10B) is touched. The "uneven distribution" is determined by comparing the ratio (mass ratio) of the mass of the liquid material in the inner sheet 1 divided by the sheet mass (not containing any liquid material) of the inner sheet 1 to the ratio (mass ratio) of the mass of the liquid material in the outer sheet 2 divided by the sheet mass (not containing any liquid material) of the outer sheet 2. For example, if the mass ratio of the inner sheet 1 is greater than the mass ratio of the outer sheet 2, it can be said that the liquid material is unevenly distributed on the inner sheet 1 side. As for this "uneven distribution", it is preferable that the inner sheet 1 is in a wet state and the outer sheet 2 is in a dry state. The "dry state" refers to a state in which the mass ratio is 1.5 or less. On the other hand, the "wet state (moist state)" refers to a state in which the mass ratio is more than 1.5.

[0027] (Method of determining uneven distribution) (1) 0.15 g of a liquid material is applied to a 50 mm square laminated fiber sheet 10 from the outer sheet 2 side. (2) After application, the laminated fiber sheet 10 is allowed to stand and then collected after 10 minutes. (3) The inner sheet 1 and the outer sheet 2 are separated, the mass of each is measured, and the mass of the liquid is calculated from the difference with the sheet mass before the liquid is applied. Because it is not possible to measure the sheet mass by separating the inner sheet 1 and the outer sheet 2 before the liquid is applied, a value converted from the basis weight is used. (4) Calculate the ratio (mass ratio) by dividing the mass of the liquid material in the inner sheet 1 by the sheet mass of the inner sheet 1 before the liquid material is applied, and calculate the mass ratio in the same manner for the outer sheet 2. Comparing the mass ratio of the inner sheet 1 with the mass ratio of the outer sheet 2, the larger value is determined to be in an uneven distribution state.

[0028] The laminated fiber sheet 10 of the present invention is easy to dissipate heat due to the ventilation spaces between the fibers of the dry outer sheet 2. In this regard, when the liquid is applied, the fiber diameter of the outer sheet 2 adjacent to the inner sheet 1 is large while the inner sheet 1 maintains a wet state, and the liquid is more likely to volatilize than the inner sheet 1 with a small fiber diameter, so that an endothermic reaction is likely to occur when the liquid evaporates. For example, the endothermic reaction may make the liquid feel cold immediately after application. This phenomenon may be a factor that promotes the transfer of heat under conditions combined with the liquid. In addition, part of the liquid in the outer sheet 2 may volatilize along with the transfer of heat, making the above-mentioned "uneven distribution" and "dry state" even more likely to occur over time.

[0029] As described above, the laminated fiber sheet 10, by utilizing the combined action of the inner sheet 1 and the outer sheet 2, is able to prevent stuffiness and suppress stickiness on the outside, while at the same time creating a sustained moist state for liquid materials.

[0030] In the laminated fiber sheet 10, from the viewpoint of enabling a clearer and more rapid expression of the aforementioned liquid migration properties, the ratio (P2 / P1) of the median fiber diameter (P2) of the outer sheet 2 to the median fiber diameter (P1) of the inner sheet 1 is preferably 1.5 or more, more preferably 10 or more, and even more preferably 20 or more. Moreover, the ratio (P2 / P1) is preferably 170 or less, more preferably 150 or less, and even more preferably 100 or less, from the viewpoint of maintaining the softness of the entire sheet.

[0031] In addition, from the viewpoint of more clearly expressing the migration of the liquid material, the uneven distribution of the liquid material, and further enhancing adhesion to the object, the median fiber diameter (P1) of the inner sheet 1 is preferably 5 μm or less, more preferably 3 μm or less, even more preferably 2 μm or less, and particularly preferably 1 μm or less. From the viewpoint of improving productivity, the median fiber diameter (P1) of the inner sheet 1 is preferably 0.3 μm or more, more preferably 0.4 μm or more, and even more preferably 0.5 μm or more.

[0032] The outer sheet 2 preferably contains fibers having a median fiber diameter (P2) of 5 μm or more and 50 μm or less. By containing fibers having the above median fiber diameter, the outer sheet 2 can further improve the dry state and heat release properties described above, impart strength and rigidity to the entire laminated fiber sheet 10, and increase resistance to tearing and abrasion without impairing the above-mentioned adhesive properties of the inner sheet 1. Such an outer sheet 2 can be obtained by appropriately setting the median fiber diameter using a method commonly used for this type of article. The median fiber diameter (P2) of the fibers contained in the outer sheet 2 is more preferably 50 μm or less, even more preferably 30 μm or less, and even more preferably 25 μm or less, from the viewpoint of maintaining the softness of the entire sheet. From the viewpoint of further increasing resistance to tearing and abrasion, the median fiber diameter (P2) of the fibers contained in the outer sheet 2 is more preferably 5 μm or more, even more preferably 10 μm or more, and even more preferably 15 μm or more.

[0033] In the laminated fiber sheet 10, the basis weight (M1) of the inner sheet 1 is 1 g / m 2 More than 8g / m 2The following is preferable. By having the basis weight (M1) of the inner sheet 1 within this range, the inner sheet 1 can more easily maintain the aforementioned softness, adhesion to the surface of the object, and uniformity of the liquid film of the liquid material, and can be made strong without impairing these properties. In addition, in an inner sheet 1 whose basis weight is suppressed within the above range, the number of ultrafine fibers with the aforementioned median fiber diameter is reduced accordingly, and the number of fiber voids is also reduced. This suppresses light scattering due to the presence of the fiber voids, and the inner sheet 1 is more likely to become transparent. In particular, when the liquid material is applied, the fiber voids are filled with the liquid material to form a uniform film, making it even more difficult for the light scattering to occur and providing greater transparency. From the viewpoint of further enhancing the above-mentioned effects and further increasing the strength, the basis weight (M1) of the inner sheet 1 is set to 1 g / m 2 More than 1.5 g / m is preferable. 2 More preferably, 2 g / m 2 The above is more preferable. From the viewpoint of further improving the softness and adhesion to the object, the basis weight (M1) of the inner sheet 1 is set to 8 g / m 2 Less than 6 g / m is preferable. 2 Less than 5 g / m is more preferable. 2 The following is even more preferred:

[0034] In the laminated fiber sheet 10, the basis weight (M2) of the outer sheet 2 is 8 g / m 2 More than 50g / m 2 The following is preferred. With the basis weight (M2) of the outer sheet 2 in this range, the dry state and heat release properties of the outer sheet 2 can be further improved, and the strength of the entire laminated fiber sheet 10 can be further increased to further improve resistance to tearing and abrasion. Furthermore, in an outer sheet 2 having a basis weight in the above range, the number of fibers with the above-mentioned median fiber diameter is reduced. This makes the outer sheet 2 more likely to be transparent, and particularly highly transparent when a formulation is applied. The basis weight (M2) of the outer sheet 2 is set to 8 g / m2 from the viewpoint of further increasing the strength of the entire laminated fiber sheet 10. 2 More than 15g / m is preferable. 2 More preferably, 17 g / m 2 The above is more preferable. The basis weight (M2) of the outer sheet 2 is set to 50 g / m from the viewpoint of further enhancing the dry state and heat release property of the outer sheet 2 and from the viewpoint of not impairing the softness and adhesion to the skin surface of the inner sheet 1. 2 Less than 40 g / m is preferable. 2 Less than 30 g / m is more preferable. 2 The following is even more preferred:

[0035] The ratio (M2 / M1) of the basis weight (M2) of the outer sheet 2 to the basis weight (M1) of the inner sheet 1 is preferably 1 or more, more preferably 1.6 or more, and even more preferably 2 or more, from the viewpoints of preventing the migration of liquid substances, uneven distribution of liquid substances in the inner sheet 1, and further improving the dry state and heat release properties of the outer sheet 2. The ratio (M2 / M1) is preferably 50 or less, more preferably 34 or less, and even more preferably 25 or less, from the viewpoint of maintaining the aforementioned softness of the inner sheet 1 and its adhesiveness to the surface of the object.

[0036] In the laminated fiber sheet 10, the thickness of the inner sheet 1 is preferably 3 μm or more, more preferably 4 μm or more, and even more preferably 5 μm or more, from the viewpoint of favorably forming a liquid film of the liquid material. From the viewpoint of improving the aforementioned softness and adhesion of the inner sheet 1 to the surface of the object, the thickness of the inner sheet 1 is preferably 50 μm or less, more preferably 40 μm or less, and even more preferably 30 μm or less. From the viewpoint of further increasing the strength of the entire laminated fiber sheet 10, the thickness of the outer sheet 2 is preferably 10 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more. The thickness of the outer sheet 2 is preferably 500 μm or less, more preferably 300 μm or less, and even more preferably 200 μm or less, from the viewpoint of further enhancing the dry state and heat release properties of the outer sheet 2, and of not impairing the softness and adhesion to the skin surface, etc. of the inner sheet 1.

[0037] In the laminated fiber sheet 10, from the viewpoint of further enhancing the unity between the inner sheet 1 and the outer sheet 2, it is preferable that the inner sheet 1 and the outer sheet 2 contain the same material. The same material is a material in which the repeating unit (monomer structure) has the same polymer structure. Specifically, the same material is selected from olefin resins, diene resins, urethane resins, and copolymers thereof. Since the inner sheet 1 and the outer sheet 2 contain the same material, the molecular structures of the resin components are similar and the fibers are highly compatible with each other, which makes it easier for the inner sheet 1 and the outer sheet 2 to be firmly fused together, enhancing the integrity of the laminated fiber sheet 10.

[0038] It is preferable that the laminated fiber sheet 10 has elasticity. This improves the fit and conformability of the laminated fiber sheet 10 to the object, and further improves the adhesion of the liquid film of the liquid material formed on the inner sheet 1 to the object.

[0039] With regard to the stretchability, it is preferable that the inner sheet 1 and the outer sheet 2 have stretchability by containing an elastomer of the same material selected from the aforementioned olefin-based resins, diene-based resins, urethane-based resins, and copolymers thereof.

[0040] (Method of measuring whether inner sheet 1 and outer sheet 2 contain the same material) The method for determining whether the inner sheet 1 and the outer sheet 2 contain the same material is to peel the sheets apart and measure the resin composition contained in each sheet. The resin composition is subjected to various analyses such as nuclear magnetic resonance (NMR) analysis and infrared spectroscopy (IR) analysis, and the molecular skeleton structure and the functional group structure at the end of the molecular structure are identified based on the positions of each signal and spectrum obtained by these analyses. This identifies and specifies the type of resin contained in each sheet. The resin compositions specified for each sheet are compared to determine whether they contain the same material.

[0041] In the laminated fiber sheet 10 of the present invention, the adjacent inner sheet 1 and outer sheet 2 are both stretchable, but have high integrity, so that peeling is unlikely to occur at the interface between the inner sheet 1 and the outer sheet 2 during stretching. By suppressing peeling, the laminated fiber sheet 10 as a whole is given sheet strength or rigidity, and the entire sheet becomes stiff. The inner sheet 1 is more likely to stretch together with the outer sheet 2. As a result, the laminated fiber sheet 10 as a whole has durability that can withstand repeated stretching operations. That is, the laminated fiber sheet 10 of the present invention is designed to stretch with the inner sheet 1 and the outer sheet 2 having high integrity and with high overall sheet strength or rigidity. Therefore, the inner sheet 1 is less likely to twist or be rubbed during the stretching behavior of the laminated fiber sheet 10. In addition, shedding of the inner sheet 1 due to rubbing is also suppressed. Thus, the laminated fiber sheet 10 as a whole has improved elasticity and sheet strength, and even if elasticity is exhibited, resistance to tearing and abrasion is increased. Furthermore, the elasticity of the entire laminated fiber sheet 10 enables the inner sheet 1 to follow the shape of the object surface and various changes (movements), and the aforementioned adhesive properties can be fully exhibited even under such changes.

[0042] The laminated fiber sheet 10 of the present invention is provided with rigidity due to the unity of the inner sheet 1 and the outer sheet 2, and handleability is improved. That is, stiffness is obtained compared to a fiber sheet having only the inner sheet 1 made of ultrafine fibers (FIGS. 2(A) and (B)), and handling is facilitated. For example, when a single laminated fiber sheet 10 is taken out from a state in which multiple laminated fiber sheets 10 are stacked or from a state in which the laminated fiber sheet 10 is stored in a packaging bag or container, etc., and used (for example, attached to the surface of the object), stiffness significantly affects the ease of taking out the sheet. In addition, when taken out, the laminated fiber sheet 10 of the present invention is less likely to curl than a fiber sheet having only the inner sheet 1 (for example, FIG. 2(A)), and handleability is improved. This allows the sheet to be neatly attached to an object such as the skin surface without wrinkles.

[0043] The above-mentioned homogeneous material is preferably an olefin-based resin from the viewpoint of increasing the integrity of the inner sheet 1 and the outer sheet 2 and increasing the stretchability of the laminated fiber sheet 10 including them. By using an olefin-based resin, the inner sheet 1 and the outer sheet 2 are less likely to peel off when the laminated fiber sheet 10 is stretched. From the same viewpoint, the inner sheet 1 preferably contains a low-crystalline olefin resin. The term "low-crystalline" means that the crystallinity is 10.5% or less, and can be measured by the following method. When the inner sheet 1 contains a low-crystalline olefin resin, the inner sheet 1 itself becomes more flexible. When the inner sheet 1 contains a low-crystalline olefin-based resin, the mass proportion of the low-crystalline olefin-based resin in the inner sheet 1 is preferably 70 mass% or more, more preferably 80 mass% or more, even more preferably 90 mass% or more, even more preferably 92 mass% or more, and even more preferably 94 mass% or more.

[0044] (Method for measuring whether the inner sheet 1 contains a low-crystalline olefin resin) The resin composition constituting the inner sheet 1 is subjected to various analyses such as NMR analysis and IR analysis, and the molecular skeleton structure and the terminal functional group structure of the molecular structure are identified based on the positions of the signals and spectra obtained by these analyses, thereby identifying and specifying the type of resin contained. Next, regarding crystallinity, low crystallinity can be confirmed using differential scanning calorimetry. The total heat of fusion obtained when the sample is heated is divided by the heat of fusion of perfect crystals. If this value is less than 10.5%, it is determined that the sample contains low-crystalline olefin resin.

[0045] From the viewpoint of enhancing the integrity of the inner sheet 1 and the outer sheet 2 and enhancing the stretchability of the laminated fiber sheet 10 including them, specific examples of the above-mentioned homogeneous material include the following. That is, examples of olefin resins include polypropylene (hereinafter referred to as PP) and polyethylene. Examples of low-crystalline olefin resins include α-olefins, such as polypropylene with controlled stereoregularity (polypropylene polymerized with controlled stereoregularity using a metallocene catalyst). Examples of the diene resin include polybutadiene and polyisoprene. The urethane resin includes polyurethane. Copolymers of olefin resins, diene resins, and urethane resins include ethylene-propylene copolymers, ethylene-1-butene copolymers, ethylene-1-octene copolymers, propylene-1-butene copolymers, propylene-1-octene copolymers, ethylene-isoprene copolymers, ethylene-butadiene copolymers, propylene-isoprene copolymers, propylene-butadiene copolymers, ethylene-propylene-isoprene copolymers, and ethylene-propylene-butadiene copolymers.

[0046] In the laminated fiber sheet 10, it is preferable that the inner sheet 1 and the outer sheet 2 are both elastic and integrated. Here, "elastic" means that the sheet can be stretched, and when the force is released from a state in which the sheet is stretched 50% of its original length (which becomes 150% of the original length), the sheet returns to a length of 125% or less of its original length. In the laminated fiber sheet 10 of the present invention, it is preferable that the elongation rate in one direction Y (also called Y direction) in the planar direction is 20% to 100%, and the elongation rate in a direction X (also called X direction) perpendicular to the one direction Y is 0% to 30%. The difference in elongation rate between these two mutually perpendicular directions gives the laminated fiber sheet 10 directional elasticity. The one direction Y and the direction X perpendicular to the one direction Y are appropriately determined according to the intended use of the laminated fiber sheet 10. For example, the longitudinal direction of the laminated fiber sheet 10 may be the one direction Y, and the width direction may be the direction X perpendicular to the one direction Y. In this case, it is preferable that the longitudinal direction of the laminated fiber sheet 10 is aligned with the elastic direction required for the article to which it is applied.

[0047] (Method of measuring elongation rate) The above-mentioned elongation percentage of the laminated fiber sheet 10 refers to the elongation of a test piece having a width of 20 mm and a length of 70 mm, fixed with a gripping distance of 50 mm, when a tensile load of 1.2 N is applied, expressed as a percentage (%) of the gripping distance of 50 mm. More specifically, the length of the gripping distance of the test piece before the elongation test is taken as L0, and the length of the gripping distance of the test piece at the time of the breaking elongation is taken as LB, and the elongation percentage (%) can be calculated as 100×(LB−L0) / L0. The measurement is performed along any two mutually perpendicular directions in the sheet plane of the laminated fiber sheet 10, for example, along the longitudinal direction and the width direction perpendicular to the longitudinal direction.

[0048] By providing the laminated fiber sheet 10 with directional elasticity due to the difference in the elongation percentages, it is possible to suitably control the elasticity according to the intended use, and reduce excessive stretching in directions where elasticity is not required and excessive loads associated with stretching, thereby more effectively preventing twisting, chafing, and tearing of the inner sheet 1. For example, when the laminated fiber sheet 10 is made into a glove, it is preferable to make the elasticity large in the length direction of the fingers and small in the width direction perpendicular to the length direction, which makes it possible to provide a glove that fits closely to the tips of the fingers and webs of the user. On the other hand, when the laminated fiber sheet 10 is made into gloves, it is also preferable to make the elasticity of the fingers small in the length direction and large in the width direction perpendicular to the length direction. This makes it possible to provide gloves that have a high adhesion according to the thickness of the user's fingers when wearing the gloves made of the laminated fiber sheet 10.

[0049] From the viewpoint of further enhancing the above-mentioned effects, the elongation percentage (T1) of the laminated fiber sheet 10 in one direction Y is preferably 20% or more, more preferably 25% or more, and even more preferably 30% or more. The elongation percentage (T1) of the laminated fiber sheet 10 in one direction Y is preferably 100% or less, more preferably 80% or less, and even more preferably 60% or less, from the viewpoint of processing and mounting the laminated fiber sheet 10 into any shape. From the viewpoint of continuously transporting the laminated fiber sheet 10, the extensibility (T2) of the laminated fiber sheet 10 in the direction X perpendicular to the direction Y is preferably 0% or more. From the viewpoint of continuously transporting the laminated fiber sheet 10, the elongation percentage (T2) in the direction X perpendicular to the direction Y of the laminated fiber sheet 10 is preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less.

[0050] The absolute value |T1-T2| of the difference between the elongation rate (T1) of the laminated fiber sheet 10 in one direction Y and the elongation rate (T2) of the laminated fiber sheet 10 in the direction X perpendicular to the one direction Y is preferably 0 or more, more preferably 10 or more, and even more preferably 20 or more, from the viewpoint of clarifying the directionality of the elasticity of the laminated fiber sheet 10 and more effectively suppressing twisting, abrasion, and tearing of the inner sheet 1. From the viewpoint of improving the fit of the laminated fiber sheet 10 to an object such as the skin, the absolute value of the difference |T1-T2| is preferably equal to or less than 70, more preferably equal to or less than 60, and even more preferably equal to or less than 50. Thereby, for example, when the laminated fiber sheet 10 is applied to gloves, the elongation rates in two perpendicular directions in the gloves can be balanced to make the gloves easier to put on.

[0051] The directionality of the stretchability of the laminated fiber sheet 10 is determined mainly by the outer sheet 2 rather than the inner sheet 1. The inner sheet 1 contains the ultrafine fibers described above, and is formed by directly spinning and depositing a resin solution or a resin melt using, for example, an electrospinning method, so that it is difficult to form a directionality of stretchability. Therefore, it is preferable that the directionality of the stretchability of the laminated fiber sheet 10 is mainly imparted by the outer sheet 2. In addition, since the directionality of the stretchability of the laminated fiber sheet 10 is mainly determined by the outer sheet 2, it is possible to suitably control the outer sheet 2 to stop stretching before the inner sheet 1 breaks when the laminated fiber sheet 10 is stretched. The directionality of the stretchability of the outer sheet 2 can be determined, for example, by stretching in the conveying direction and cooling and solidifying during the conveying process to form an outer sheet 2 that does not have stretchability in the conveying direction but has stretchability in the perpendicular direction.

[0052] From the viewpoint of further increasing the strength of the inner sheet 1 itself in the laminated fiber sheet 10, the ratio of the number of fusion points (for example, fusion points 31 at the intersections of ultrafine fibers 11, 11 in FIG. 3, and the enclosed areas with symbols D4, D14, and D1 in FIG. 4) to the number of fiber intersections in a field of view of 0.128 mm × 0.096 mm in the SEM image of the inner sheet 1 is preferably 50% or more, more preferably 70% or more. As a result, each ultrafine fiber of the inner sheet 1 is fixed at the intersections to increase the strength. That is, the integrity of the inner sheet 1 itself is strengthened. For example, when the surface of the inner sheet 1 on one side 10T of the laminated fiber sheet 10 is traced with a finger, the fibers are less likely to fluff and the fibers are suppressed from falling off. In addition, since the bonding area is suppressed at the fusion points at the fiber intersections, the excessive increase in the rigidity of the inner sheet 1 itself is suppressed and the softness is maintained compared to surface fusion, and the above-mentioned adhesive properties are easily expressed.

[0053] (The ratio of the number of fusion points to the number of fiber intersections) The same operations as those in (1), (2), and (3) in the above section (Method of measuring median fiber diameter) are performed to obtain SEM observation images of the fiber layer to be measured at a magnification of 1000 times. The same sample is measured at a total of five locations by changing the observation location. A total of five observation images are obtained by focusing on the sample surface side for each location. The image quality is 0.128 mm in width and 0.096 mm in height. From the obtained observation images, the fiber intersections are marked using image analysis software (WinRooF2015 made by Mitani Shoji Co., Ltd.), and the number of fusion points at the fiber intersections is recorded. The ratio of the number of fusion points to the total number of fiber intersections is calculated using the following formula (I). This evaluation is performed by two people, an observer and a recorder. The number of fiber intersections is tallied by the observer's manual marking process on the above image analysis software. Regarding the fusion points, the recorder tallies the fiber intersections that the observer has determined to be fusion points according to the definition of fusion points below. Percentage of fusion points [%] = Number of fusion points / Total number of fiber intersections × 100 (Formula (I)) The fiber intersections and the fusion points of the fiber intersections are defined as follows. (Fiber intersection) In the SEM observation image of the fiber layer to be measured, the image itself is enlarged three times (300%) on a 410 mm × 260 mm monitor. In this case, a focused image is selected within a range in which the width between the boundaries of the fiber shape (fiber width confirmed in the observation image) does not exceed 1 mm. The fiber intersections are defined as the points where they cross, or the points where they do not cross but are in contact (contact), or the points where one fiber branches off in the middle (e.g., the boxed areas D4, D14, and D1 in Figure 4). If two or more fibers shown in the image are in contact with each other in the whole or part of the image capture area over the longitudinal direction to form a fiber bundle, these are also defined as fiber intersections (e.g., the boxed area D5 in Figure 4). For example, if there is a point in the observation image where four fibers are lined up without any gaps, the number of fiber intersections is determined to be three. In addition, due to the characteristics of the fiber layer, there is a depth due to the thickness of the fiber layer on the side closer to the detector (surface side in the specimen thickness direction) and the side farther away (sample stage side in the specimen thickness direction) in SEM observation. Therefore, even if the fibers appear to cross in the observation image, they may not be in contact with each other. As described above, when the image itself is enlarged three times (300%) on a 410 mm x 260 mm monitor, multiple fibers that are in focus within a range where the width of the boundary line of the fiber shape does not exceed 1 mm are considered to be in the same positional relationship in the thickness direction (depth) of the specimen. The intersections of the fibers selected in this way are considered to be fiber intersections according to the above definition. (Fusion points at fiber intersections) Among the intersections defined above, (i) a point where the boundary line between two or more fibers related at the intersection is not clearly visible (e.g., the area enclosed by reference symbol D4 in FIG. 4), and (ii) a point where the width between the boundary lines of one or more fibers related at the intersection is wider than the width between the boundary lines at the other points (e.g., the area enclosed by reference symbol D16 in FIG. 4) are defined as fusion points at fiber intersections. When the sheet is in a laminated state, the fiber layers are peeled off, and the fiber layer to be measured is taken out and subjected to the above operation.

[0054] The laminated fiber sheet 10 preferably has a high strength and has an integral structure between the inner sheet 1 and the outer sheet 2. The strength of this integral structure is preferably sufficient to withstand the above-mentioned stretchability. This strength is indicated as breaking strength. In relation to the above-mentioned stretchability and the resistance of the inner sheet 1 to abrasion and tearing during stretching behavior, the breaking strength is preferably set within the following range in the two directions X and Y which show the above-mentioned elongation. The breaking strength in the Y direction is preferably 1 N / 20 mm or more, more preferably 2 N / 20 mm or more, and even more preferably 2.5 N / 20 mm or more, from the viewpoint of obtaining resistance to elongation. The breaking strength in the X direction is preferably 1 N / 20 mm or more, more preferably 3 N / 20 mm or more, and even more preferably 5 N / 20 mm or more, from the viewpoint of facilitating transport of the laminated fiber sheet 10. (Method of measuring breaking strength of laminated fiber sheet 10) The breaking strength of the laminated fiber sheet 10 is measured by fixing a test piece 20 mm wide and 70 mm long with a gripping distance of 50 mm and stretching it at a tensile speed of 300 mm / min, and measuring the maximum load until the sheet breaks. The measurement temperature is 23°C.

[0055] In the laminated fiber sheet 10, it is preferable from the viewpoint of improving the integrity that the fibers of both sheets at the interface between the inner sheet 1 and the outer sheet 2 are fused to each other (for example, fused points 32 in FIG. 5(A)). Moreover, it is preferable from the viewpoint of preventing the rigidity of the laminated fiber sheet 10 from being excessively increased that the fibers at the interface are bonded to each other at fused points at the intersections of both sheets while maintaining the fiber shapes. The fusion means that the resin components contained in the inner sheet 1 and the outer sheet 2 are melted by heat and bonded (thermal bonding, etc.). Since the inner sheet 1 and the outer sheet 2 contain the same material with high compatibility as described above, the fusion at the interface becomes stronger. This can further improve the integration of the inner sheet 1 and the outer sheet 2 while maintaining the softness and adhesion to the skin surface, etc. on one side 10T of the inner sheet 1 itself. In particular, peeling at the interface between the inner sheet 1 and the outer sheet 2 during the stretching behavior of the laminated fiber sheet 10 can be more effectively suppressed, and the followability of both layers can be improved (for example, Figure 5 (A) to (B)). This can more reliably express the migration of the liquid from the outer sheet 2 to the inner sheet 1. In addition, if the inner sheet 1 and the outer sheet 2 are integrated at the fusion points at the fiber intersections of both sheets, the gaps between the fibers at the interface between the two sheets are more likely to be maintained, and the above-mentioned liquid migration can be more reliably and smoothly expressed. Furthermore, due to the further improvement in the integrity, the handling properties of the laminated fiber sheet 10 described above become even better.

[0056] From the viewpoint of further improving the above-mentioned action, the fusion strength at the interface is preferably 0.01 N / 20 mm or more, more preferably 0.1 N / 20 mm or more, and even more preferably 0.2 N / 20 mm or more. Furthermore, the strength of the fusion at the interface is practically 10N / 20mm or less. If the thickness falls within the above range, the laminated fiber sheet 10 is integrated.

[0057] (Method of measuring strength of fusion at interface between inner sheet 1 and outer sheet 2) It is measured by the following means. An adhesive tape is applied to the surface of the inner sheet 1 of the laminated fiber sheet 10, and the tape is T-peeled using a tensile tester. This makes it possible to measure the strength of fusion between the fibers of the inner sheet 1 and the outer sheet 2 at the interface between the two sheets. The greater the number of fusion points at the interface between the inner sheet 1 and the outer sheet 2, the greater the resistance to T-peel. After attaching an adhesive tape (adhesive strength: 4.4 N / 10 mm) to the surface side of the inner sheet 1, a test piece 20 mm wide and 100 mm long is prepared. The end of the tape on the longitudinal side is peeled off, and the end of the tape and the laminated fiber sheet 10 are pulled with a gripping distance of 50 mm and a pulling speed of 100 mm / min, and the test force at which the tape peels off from the laminated fiber sheet 10 is measured. Of the test forces obtained, the average value of the test forces where the gripping tool travels a distance of 30 mm or more and 80 mm or less from the initial position is taken as the strength of the fusion, i.e., the fusion force.

[0058] The above-mentioned fusion points at the fiber intersections in the inner sheet 1 and the fusion points between the fibers of the inner sheet 1 and the outer sheet 2 at the interface between the two sheets are easily formed when the inner sheet 1 and the outer sheet 2 contain the same material as described above. The fusion points can be formed as follows. On the surface of the outer sheet 2, a resin solution or resin melt using the same material as described above is discharged from a nozzle by, for example, electrospinning. The spun fibers (constituent fibers of the inner sheet 1) formed by the discharge are collected on the outer sheet 2 in a state of high temperature and fluidity. As a result, the spun fibers can be collected in a state where they are fused at their intersections, and the spun fibers and the fibers of the outer sheet 2 are integrated in a fused state. By collecting such spun fibers, the inner sheet 1 is formed in which a network having fusion points at the above-mentioned fiber intersections is formed. At the same time, fusion points between the fibers of both the inner sheet 1 and the outer sheet 2 at the interface between them can be formed. The temperature at which the spun fibers are made to have fluidity is appropriately set depending on the resin raw material used. For example, when a low-crystallinity PP resin is used as the resin raw material of the inner sheet 1, it is preferable to collect the spun fibers in a range of 40°C to 70°C at which the spun fibers change to a rubber state. In addition, it is preferable to heat and maintain such a temperature for the outer sheet 2, which serves as a receiver for the collected fibers. In addition to the above-mentioned methods, the above-mentioned fusion points can also be formed by heat sealing. From the viewpoint of preventing the thermal shrinkage of the elastomer of the fiber and the film formation due to the melting of the resin, as described above, fusion during spinning, which requires less time and fewer exposures to heat, is more preferable.

[0059] Next, a method for using the laminated fiber sheet 10 of the present invention will be described below. In a method of using the laminated fiber sheet 10, the laminated fiber sheet 10 is moistened with the liquid. Specifically, the method includes a step of applying the laminated fiber sheet 10 with the inner sheet 1 facing the object, and a step of applying the liquid material. It is preferable that the laminated fiber sheet 10 exhibits the ability to transfer the liquid from the outer sheet 2 to the inner sheet 1 through the above two steps.

[0060] Specifically, the above-mentioned two steps include cases where the steps are carried out in any of the following procedures (I) to (III). In any procedure, the laminated fiber sheet 10 exhibits the ability to transfer the liquid from the outer sheet 2 to the inner sheet 1, creating a wet state of the liquid on the inner sheet 1 (particularly the surface of the inner sheet 1 facing the object). This makes it possible to keep the outer sheet 2 in a dry state. The amount of the liquid to be applied in the step of applying the liquid is preferably within the range shown as "amount of liquid to be applied to create a wet state" above. (I) After the liquid has been applied to the object, the laminated fiber sheet 10 is applied with the inner sheet 1 facing the object. (II) After the liquid is applied to the laminated fiber sheet 10, the laminated fiber sheet 10 is applied with the inner sheet 1 facing the target object. (III) The laminated fiber sheet 10 is applied with the inner sheet 1 facing the target object, and then the liquid material is applied to the laminated fiber sheet 10.

[0061] The expression of the liquid migration property from the outer sheet 2 to the inner sheet 1 is not limited to the migration of the liquid in the outer sheet 2 to the inner sheet 1, but also includes the pushing back of the liquid that is flowing back from the inner sheet 1 to the outer sheet 2, or the liquid that has flowed back, to the inner sheet 1. FIG. 6 shows an example of the migration of the liquid in a state where the laminated fiber sheet 10 is applied to an object W. The arrows F1, F2, and F3 indicate only the rough direction of the migration of the liquid, and the actual migration form of the liquid may be more complicated than this. The migration directions of the liquid indicated by the arrows F1, F2, and F3 are shown as different locations and different steps for the convenience of explanation. However, in reality, they may occur in the same location and in the same step, and may occur not necessarily at the same time but at different times.

[0062] In the step (I), the liquid is applied to the object before the laminated fiber sheet 10 applies the inner sheet 1 toward the object. The liquid can be applied to the object by various commonly used methods such as spraying. In this case, the liquid is initially present at the interface between the inner sheet 1 and the object. At this time, the inner sheet 1 sucks up the liquid by its own extremely strong capillary force. Since the inner sheet 1 and the outer sheet 2 are integrated and the inner sheet 1 is an extremely thin layer of the ultrafine fibers, the liquid can gradually migrate to the outer sheet 2. However, in such a wet state, the laminated fiber sheet 10 acts to push back the liquid that migrates from the inner sheet 1 to the outer sheet 2 to the inner sheet 1 due to the high liquid retention capacity of the ultrafine fibers of the inner sheet 1 in addition to the capillary force (for example, arrow F1 in FIG. 6). This allows the liquid to remain on the inner sheet 1.

[0063] In the above-mentioned step (II), the laminated fiber sheet 10 is in a wet state by applying the liquid in advance. The liquid can be applied by immersing the laminated fiber sheet 10 in a solution of the liquid or by using a coating method such as spraying. In this case, the liquid may be applied to both the inner sheet 1 and the outer sheet 2 of the laminated fiber sheet 10, or to either one of them. In any case, the laminated fiber sheet 10 in a wet state transfers the liquid from the outer sheet 2 to the extremely thin inner sheet 1 (for example, arrow F2 in FIG. 6) due to the high liquid retention ability of the inner sheet 1 due to the ultrafine fibers described above in addition to the above-mentioned capillary force, so that the liquid remains on the inner sheet 1.

[0064] In the step (III), the liquid is applied to the laminated fiber sheet 10 applied to the object. More specifically, the liquid is applied to the surface side (the other surface side 10B) of the outer sheet 2 while the surface side (one surface side 10T) of the inner sheet 1 of the laminated fiber sheet 10 is in contact with the object. In this case, the laminated fiber sheet 10 transfers the liquid that has soaked in from the outside to the inner sheet 1 (for example, arrow F3 in FIG. 6 ) due to the high liquid retention capacity of the ultrafine fibers of the inner sheet 1 in addition to the capillary force described above, so that the liquid remains on the inner sheet 1.

[0065] As described above, regardless of the order of the above two steps (I) to (III), the laminated fiber sheet 10 forms a uniform liquid film (uniformly wet state) of the liquid on the inner sheet 1 by the cooperation of the outer sheet 2 and the inner sheet 1, and the adhesion between the liquid and the surface of the object is dramatically improved compared to the conventional case, and the state can be maintained for a long time. This allows the liquid to act uniformly on the object for a long time. As a result, the liquid is unevenly distributed on the inner sheet 1, and the state is easily maintained. In addition, the surface side (other surface side 10B) of the outer sheet 2 of the laminated fiber sheet 10 is easily kept in a dry state, and the state is easily maintained. In other words, even if the surface side (other surface side 10B) of the outer sheet 2 of the laminated fiber sheet 10 is touched, stickiness due to the liquid is suppressed.

[0066] In the method of using the laminated fiber sheet 10, since the inner sheet 1 contains ultrafine fibers and is extremely thin, it is easy to break, and it is preferable that friction is as small as possible when applying it to an object. From this viewpoint, it is preferable to apply the liquid to the object after applying the laminated fiber sheet 10 to the object as in the above-mentioned (III) rather than applying the liquid to the object or the laminated fiber sheet 10 first as in the above-mentioned (I) and (II) procedures and then applying the laminated fiber sheet 10 to the object. In particular, when the laminated fiber sheet 10 is glove-shaped and worn on a human finger, the wearing can be smoothly performed while avoiding resistance from the liquid, and the liquid can be quickly delivered to the inner sheet 1 while worn. In addition, as described above, a uniform liquid film is formed on the inner sheet 1, and the surface side of the outer sheet 2 (the other surface side 10B) becomes dry, so that when the laminated fiber sheet 10 is worn on a human finger, the user can continue to operate electronic devices such as smartphones and various other daily activities while wearing it.

[0067] In the method of using the laminated fiber sheet 10, as shown in FIG. 6, it is preferable that at the interface between the outer sheet 2 and the inner sheet 1, which have different median fiber diameters, there is a mixture of a contact region 21 where the constituent fibers of the outer sheet 2 contact the fiber layer of the inner sheet 1 and a void region (non-contact region) L where the constituent fibers of the outer sheet 2 do not contact the fiber layer of the inner sheet 1. This makes it possible to more effectively realize the above-mentioned transfer of liquid from the outer sheet 2 to the inner sheet 1, the formation of a uniform liquid film of the liquid on the inner sheet 1, and the realization of a dry state of the outer sheet 2. In addition, when the inner sheet 1 and the outer sheet 2 are bonded at the fusion points of the fiber intersections as described above, a certain strength is obtained, there is no floating at the interface, and capillary force is more easily expressed. Therefore, a uniform wet state is more easily generated in the inner sheet 1, and liquid retention is further improved.

[0068] The method of using the laminated fiber sheet 10 may include a step of applying the liquid material, which has already been applied once, to the surface side of the outer sheet 2 of the laminated fiber sheet 10. In other words, the liquid material can be reapplied while the laminated fiber sheet 10 is still applied to the object. In this case as well, due to the capillary force and the high liquid retention capacity of the ultrafine fibers of the inner sheet 1, the liquid material can be transferred to and unevenly distributed in the inner sheet 1, keeping the outer sheet 2 dry. Therefore, the above step can be performed any number of times.

[0069] In the method of using the laminated fiber sheet 10, it is preferable that the fibers constituting the laminated fiber sheet 10 maintain their fibrous shape even when the laminated fiber sheet 10 contains the liquid. This is possible because the inner sheet 1 and the outer sheet 2 are insoluble in the liquid, as described above. This makes it possible to more significantly affect the action of the fiber structure of the laminated fiber sheet 10 on the liquid, and to more significantly distribute the liquid unevenly in the inner sheet 1. In addition, the application of the additional liquid can be more effectively performed. The handleability of the laminated fiber sheet 10 is also improved.

[0070] In the method of using the laminated fiber sheet 10, it is preferable that the content by weight of the liquid be 50% or more of the basis weight of the laminated fiber sheet 10. This makes it easier to form a uniform film of the liquid, and improves the above-mentioned migration of the liquid from the outer sheet 2 to the inner sheet 1, the formation of a uniform liquid film of the liquid on the inner sheet 1, and the realization of a dry state of the outer sheet 2.

[0071] (Method for measuring the ratio of the basis weight of the liquid content to the basis weight of the laminated fiber sheet) (1) The mass of the laminated fiber sheet before the liquid is applied is measured. (2) After the liquid has been applied, the mass of the laminated fiber sheet containing the liquid is measured. (3) The basis weight of the liquid is calculated from the difference between (2) and (1) above, and the ratio of this basis weight to the basis weight of the laminated fiber sheet before the liquid is applied in (1) above is calculated.

[0072] In the method of using the laminated fiber sheet 10, the laminated fiber sheet 10 can be used for various articles and shapes. For example, the laminated fiber sheet 10 can be used for bandages and dressings that are used by contacting the skin surface. The laminated fiber sheet 10 can also be used in a cylindrical or glove-like shape. Specific examples of the cylindrical body include a supporter and a finger cot. In such an article, it is preferable that the laminated fiber sheet 10 has unidirectional stretchability, that is, the laminated fiber sheet 10 is preferably applied to the article such that the laminated fiber sheet 10 stretches along the unidirectional stretch direction Y. The "unidirectional stretchability" refers to the direction in which the difference in elongation between two mutually perpendicular directions, measured by applying a load of 1.2 N to a sample based on the above-mentioned (method of measuring elongation), is 20% or more and the elongation is large. In the laminated fiber sheet 10, these two mutually perpendicular directions are the one direction Y and the direction X perpendicular to the one direction Y.

[0073] In relation to the above-mentioned embodiment, the present invention further discloses the following laminated fiber sheet and a method for using the same.

[0074] <1> A method for using a laminated fiber sheet, comprising wetting a liquid onto the laminated fiber sheet, the method comprising the steps of: Regarding the laminated fiber sheet, the inner sheet and the outer sheet are insoluble in liquids; The inner sheet has a median fiber diameter of 0.3 μm or more and 5 μm or less, the outer sheet has a larger median fiber diameter than the inner sheet; The inner sheet and the outer sheet are integrated, applying the laminated fiber sheet with the inner sheet facing an object; and applying said liquid to said laminated fiber sheet.

[0075] <2> The laminated fiber sheet exhibits the ability to transfer the liquid from the outer sheet to the inner sheet through the two steps. <1> A method for using the laminated fiber sheet according to claim 1.

[0076] <3> The liquid material is applied from the surface side of the outer sheet while the surface side of the inner sheet is in contact with the object. <1> or <2> A method for using the laminated fiber sheet according to claim 1. <4> After applying the liquid to the object, the laminated fiber sheet is applied with the inner sheet facing the object. <1> or <2> A method for using the laminated fiber sheet according to claim 1. <5> After applying the liquid to the laminated fiber sheet, the laminated fiber sheet is applied with the inner sheet facing the target object. <1> or <2> A method for using the laminated fiber sheet according to claim 1.

[0077] <6> The outer sheet contains fibers having a median fiber diameter of 5 μm or more and 50 μm or less, preferably 10 μm or more and 30 μm or less, and more preferably 15 μm or more and 25 μm or less. <1> ~ <5> 13. A method for using the laminated fiber sheet according to claim 12.

[0078] <7> The inner sheet has a basis weight of 1 g / m 2 More than 8g / m 2 Less than 1.5 g / m 2 More than 6g / m 2 Less than 2 g / m, more preferably 2 More than 5g / m 2 The above-mentioned <1> ~ <6> 13. A method for using the laminated fiber sheet according to claim 12. <8> In the laminated fiber sheet, the outer sheet has a basis weight of 8 g / m 2 More than 50g / m 2 Less than 15 g / m 2 More than 40g / m 2 Less than 17g / m2 More than 30g / m 2 The above-mentioned <1> ~ <7> 13. A method for using the laminated fiber sheet according to claim 12. <9> The laminated fiber sheet has elasticity. <1> ~ <8> 13. A method for using the laminated fiber sheet according to claim 12. <10> The laminated fiber sheet has an elongation rate in one direction in a planar direction of 20% to 100%, and an elongation rate in a direction perpendicular to the planar direction of 0% to 30%. <1> ~ <9> 13. A method for using the laminated fiber sheet according to claim 12.

[0079] <11> The ratio of the basis weight of the liquid to the basis weight of the laminated fiber sheet is 50% or more. <1> ~ <10> 13. A method for using the laminated fiber sheet according to claim 12. <12> The method further comprises the step of applying the liquid to the surface side of the outer sheet of the laminated fiber sheet. <1> ~ <11> 13. A method for using the laminated fiber sheet according to claim 12.

[0080] <13> The liquid is unevenly distributed on the inner sheet. <1> ~ <12> 13. A method for using the laminated fiber sheet according to claim 12. <14> The surface side of the outer sheet of the laminated fiber sheet is kept dry. <1> ~ <13> 13. A method for using the laminated fiber sheet according to claim 12.

[0081] <15> The inner sheet and the outer sheet are adjacent to each other and are integrated by fusing the fibers constituting the inner sheet and the fibers constituting the outer sheet. <1> ~ <14> 13. A method for using the laminated fiber sheet according to claim 12. <16> The ratio (P2 / P1) of the median fiber diameter (P2) of the outer sheet to the median fiber diameter (P1) of the inner sheet is 1.5 or more and 170 or less, preferably 10 or more and 150 or less, more preferably 20 or more and 100 or less. <1> ~ <15> 13. A method for using the laminated fiber sheet according to claim 12. <17> The median fiber diameter (P1) of the inner sheet is 0.3 μm or more and 5 μm or less, preferably 0.4 μm or more and 3 μm or less, more preferably 0.5 μm or more and 2 μm or less, and even more preferably 0.5 μm or more and 1 μm or less. <1> ~ <16> 13. A method for using the laminated fiber sheet according to claim 12. <18> The ratio (M2 / M1) of the basis weight (M2) of the outer sheet to the basis weight (M1) of the inner sheet is 1 or more and 50 or less, preferably 1.6 or more and 34 or less, and more preferably 2 or more and 25 or less. <1> ~ <17> 13. A method for using the laminated fiber sheet according to claim 12. <19> The thickness of the inner sheet is 3 μm or more and 50 μm or less, preferably 4 μm or more and 40 μm or less, and more preferably 5 μm or more and 30 μm or less. <1> ~ <18> 13. A method for using the laminated fiber sheet according to claim 12.

[0082] <20> The amount of the liquid applied in the step of applying the liquid is 0.2 mg / cm 2 More than 10mg / cm 2 Less than 0.3 mg / cm, preferably 0.3 mg / cm 2 More than 7mg / cm 2 Less than 0.4 mg / cm, more preferably 0.4 mg / cm 2 More than 5mg / cm 2 More preferably, 0.4 mg / cm 2 More than 4mg / cm 2 The above-mentioned <1> ~ <19> 13. A method for using the laminated fiber sheet according to claim 12.

[0083] <21> The strength of fusion at the interface between the integrated inner sheet and the outer sheet is 0.01 N / 20 mm or more and 10 N / 20 mm or less, preferably 0.1 N / 20 mm or more and 10 N / 20 mm or less, and more preferably 0.2 N / 20 mm or more and 10 N / 20 mm or less. <1> ~ <20> 13. A method for using the laminated fiber sheet according to claim 12. <22> The liquid contains a polyol that is liquid at 20° C., and preferably the polyol contains one or more selected from ethylene glycol, propylene glycol, 1,3-butanediol, dipropylene glycol, polyethylene glycol having a mass average molecular weight of 2000 or less, glycerin, and diglycerin. <1> ~ <21> 13. A method for using the laminated fiber sheet according to claim 12. <23> Even if the liquid is contained in the laminated fiber sheet, the fibers constituting the laminated fiber sheet maintain their fibrous shape. <1> ~ <22> 13. A method for using the laminated fiber sheet according to claim 12. <24> The laminated fiber sheet is in the form of a bandage, a dressing, a tube, or a glove. <1> ~ <23> 13. A method for using the laminated fiber sheet according to claim 12.

[0084] <25> A laminated fiber sheet comprising an inner sheet laminated on one side of an outer sheet, the inner sheet and the outer sheet are insoluble in liquids; the inner sheet has a median fiber diameter of 0.3 μm or more and 5 μm or less, and the outer sheet has a larger median fiber diameter than the inner sheet, The inner sheet and the outer sheet are integrated, The laminated fiber sheet contains a liquid, the liquid being unevenly distributed in the inner sheet.

[0085] <26> Due to uneven distribution of the liquid, the surface side of the outer sheet becomes dry. <25> The laminated fiber sheet according to claim 1. <27> The outer sheet contains fibers having a median fiber diameter of 5 μm or more and 50 μm or less, preferably 10 μm or more and 30 μm or less, and more preferably 15 μm or more and 25 μm or less. <25> or <26> The laminated fiber sheet according to claim 1. <28> the inner sheet and the outer sheet contain an olefin-based resin, The inner sheet contains a low-crystalline olefin-based resin. <25> ~ <27> 13. The laminated fiber sheet according to claim 12.

[0086] <29> The inner sheet has a basis weight of 1 g / m 2 More than 8g / m 2 Less than 1.5 g / m 2 More than 6g / m 2 Less than 2 g / m, more preferably 2 More than 5g / m 2 The above-mentioned <25> ~ <28> 13. The laminated fiber sheet according to claim 12.

[0087] <30> The inner sheet and the outer sheet are adjacent to each other and are integrated by fusing the fibers constituting the inner sheet and the fibers constituting the outer sheet. <25> ~ <29> 13. The laminated fiber sheet according to claim 12. <31> The laminated fiber sheet is in the form of a bandage, a dressing, a tube, or a glove. <25> ~ <30> 13. The laminated fiber sheet according to claim 12 . EXAMPLES

[0088] The present invention will be described in more detail below based on examples, but the present invention is not limited thereto. In the examples, "parts" and "%" expressing mass are all based on mass unless otherwise specified. "←" means that the content is the same as the column to the left. "-" means that there is no value or the like corresponding to that item.

[0089] Example 1 An outer sheet 2 having the median fiber diameter and basis weight shown in Table 1 was formed by the spunbond method using the resin raw material PP. A resin melt was prepared using the resin raw material PP, and spun by electrospinning. At that time, the space between the spinning nozzle and the collector was heated to 40°C or higher by hot air ejected from the periphery of the spinning nozzle, and the spun fibers were collected on the outer sheet 2 in a fluid state. The distance between the nozzle and the collector was 300 mm. In this way, an inner sheet 1 having the median fiber diameter and basis weight shown in Table 1 was formed, and a laminated fiber sheet sample consisting of the inner sheet 1 and the outer sheet 2 was obtained.

[0090] Comparative Example 1 The outer sheet 2 produced in Example 1 was used alone as a fiber sheet sample of Comparative Example 1. Comparative Example 2 The inner sheet 1 produced in Example 1 was used alone as a fiber sheet sample of Comparative Example 2.

[0091] The samples of each of the Examples and Comparative Examples were subjected to the following tests. (1) Continuous uneven distribution of liquid, wet state on the inside, and dry state on the outside (prevention of stuffiness) in the laminated fiber sheet sample of Example 1 The procedure was carried out according to the following steps (1-1) to (1-4). The results are shown in Table 2. (1-1) 0.15 g of a liquid (Kao Corporation, Curel Beauty Essence Ma, manufactured in 2022) was applied to a 50 mm square laminated fiber sheet sample of Example 1 from the outer sheet 2 side. (1-2) The coated laminated fiber sheet sample was allowed to stand and was collected after the time shown in Table 2 had elapsed since coating. (1-3) The inner sheet 1 and outer sheet 2 of the collected laminated fiber sheet sample were separated, and the mass of each was measured, and the mass of the liquid was calculated from the difference with the sheet mass before the liquid was applied. Since the sheet mass cannot be measured by separating the inner sheet 1 and outer sheet 2 before the liquid is applied, a conversion value from the basis weight was used. (1-4) The ratio (mass ratio) was calculated by dividing the mass of the liquid content of the inner sheet 1 by the sheet mass of the inner sheet 1 before the liquid was applied, and the mass ratio was calculated in the same manner for the outer sheet 2. A mass ratio of 1.5 or less was determined to be a dry state, and a mass ratio exceeding 1.5 was determined to be a non-dry state (wet state). (2) Durability of moist condition The following steps (2-1) to (2-5) were carried out to calculate the mass ratios of the fiber sheet samples of Comparative Examples 1 and 2. The results are shown in Table 3 together with the mass ratios of Example 1. Note that the values ​​in Table 2 were used for the mass ratios of Example 1 in Table 3. (2-1) A 50 mm square sheet was cut out, and the mass of the sheet before application of the liquid was measured. (2-2) 0.15 g of a liquid (Kao Corporation, Curel Beauty Essence Ma, 2022) was applied to one side of a 50 mm square sheet. (2-3) The coated sheet was allowed to stand and collected after the time shown in Table 3 had elapsed since coating. (2-4) The mass of each was measured, and the mass of the liquid material contained was calculated from the difference from the sheet mass before and after the liquid material was applied. (2-5) The ratio was calculated by dividing the mass of the liquid by the mass of the sheet before the liquid was applied.

[0092] (3) Prevents stickiness on the outside In order to confirm whether the wet state on the inside and the suppression of stickiness on the outside could be achieved at the same time, the following steps (3-1) to (3-6) were carried out. The results of (3-5) and (3-6) are shown in Table 3. (3-1) The mass of the filter paper before transfer was measured. (3-2) 0.15 g of a liquid (Kao Corporation, Curel Beauty Essence Ma, 2022) was applied to one side of a 50 mm square sheet. *For the laminated fiber sheet sample of Example 1, the liquid was applied from the outer sheet 2 side. (3-3) The coated sheet was allowed to stand and collected after the time shown in Table 3 had elapsed since coating. (3-4) The fiber sheet samples of each comparative example were placed so that the surface coated with the liquid was at the interface with the filter paper, and a load of 1.5 kg was applied from above for 1 minute. The laminated fiber sheet sample of Example 1 was placed so that the surface on the outer sheet 2 side was at the interface with the filter paper, and a load of 1.5 kg was applied from above for 1 minute. (3-5) The mass of the filter paper after transfer was measured, and the amount of the liquid transferred was calculated from the difference in mass between the filter paper after transfer and the filter paper before transfer to determine the amount of the liquid transferred from the outside. (3-6) In the above (3-1) to (3-5), for (3-4), the fiber sheet samples of each comparative example were placed so that the side opposite to the side on which the liquid was applied was at the interface with the filter paper, and the laminated fiber sheet sample of Example 1 was placed so that the side on the inner sheet 1 side was at the interface with the filter paper. A load of 1.5 kg was applied, and the amount of the liquid transferred in (3-5) was calculated to determine the amount of the liquid transferred from the inside.

[0093] [Table 1]

[0094] [Table 2]

[0095] [Table 3]

[0096] Results of (1) In Example 1, when comparing the mass ratios of the inner sheet 1 and the outer sheet 2 every 10 to 60 minutes in Table 2, it was found that the mass ratio of the inner sheet 1 was large in both cases, and liquid was unevenly distributed in the inner sheet 1. In addition, the mass ratio of the inner sheet 1 exceeded 1.5, and the mass ratio of the outer sheet 2 was below 1.5. Therefore, as defined above, the inner sheet 1 was not dry, and the outer sheet 2 was dry. From the above, the inner sheet 1 continued to be in a non-dry state (wet state) for a long time, and the outer side continued to be in a dry state. In addition, it was found that the laminated fiber sheet sample of Example 1 had good breathability and excellent stuffiness prevention properties because the fiber layer of the outer sheet 2 could continue to be in a dry state even though the inner sheet 1 was in a wet state. Results of (2) and (3) In Example 1, when the amount of liquid transferred at 10 minutes and 20 minutes was checked, the amount of liquid transferred to the outer sheet 2 was smaller than that of the inner sheet 1 at both times. For the outer sheet 2, a small amount of liquid was transferred when the mass ratio was 1.4, which is judged to be dry, as shown in FIG. 7(A). On the other hand, for the inner sheet 1, a large amount of liquid was transferred when the mass ratio was 2.24, which is judged to be not dry, as shown in FIG. 7(B). As described above, it was found that the stickiness of the outer side was prevented when the outer sheet 2 was judged to be dry. At the same time, in Example 1, the inner sheet 1 adjacent to the dry outer sheet 2 was in a wet state and had a large amount of liquid transferred, which indicated that the liquid was likely to act on the object. In comparison with Comparative Example 1, Example 1 was able to maintain the inner moist state based on the transfer amount after 10 minutes and 20 minutes. In comparison with Comparative Example 2, Example 1 was able to suppress the outer stickiness based on the transfer amount after 10 minutes and 20 minutes. Therefore, it was found that by adopting the configuration of Example 1, it is possible to achieve both suppression of outer stickiness and a moist state on the inner side. [Explanation of symbols]

[0097] 1 Inner sheet 2 Outer sheet 10. Laminated fiber sheet

Claims

1. A method for using a laminated fiber sheet, comprising wetting a liquid onto the laminated fiber sheet, the method comprising the steps of: Regarding the laminated fiber sheet, the inner sheet and the outer sheet are insoluble in liquids; The inner sheet has a median fiber diameter of 0.3 μm or more and 5 μm or less, the outer sheet has a larger median fiber diameter than the inner sheet; the inner sheet and the outer sheet are adjacent to each other, and the inner sheet and the outer sheet are integrated by fusion of the fibers constituting the inner sheet and the fibers constituting the outer sheet, applying the laminated fiber sheet with the inner sheet facing an object; A method for using the laminated fiber sheet, comprising the step of applying the liquid.

2. A method for using a laminated fiber sheet, comprising wetting a liquid onto the laminated fiber sheet, the method comprising the steps of: Regarding the laminated fiber sheet, the inner sheet and the outer sheet are insoluble in liquids; The inner sheet has a median fiber diameter of 0.3 μm or more and 5 μm or less, the outer sheet has a larger median fiber diameter than the inner sheet; The inner sheet and the outer sheet are integrated, applying the laminated fiber sheet with the inner sheet facing an object; applying said liquid; A method for using the laminated fiber sheet, comprising the step of further applying the liquid to the surface side of the outer sheet of the laminated fiber sheet while the laminated fiber sheet is applied to the object.

3. A method for using a laminated fiber sheet, comprising the steps of: wetting a liquid material onto the laminated fiber sheet, the method comprising the steps of: Regarding the laminated fiber sheet, the inner sheet and the outer sheet are insoluble in liquids; The inner sheet has a median fiber diameter of 0.3 μm or more and 5 μm or less, the outer sheet has a larger median fiber diameter than the inner sheet; The inner sheet and the outer sheet are integrated, applying the laminated fiber sheet with the inner sheet facing an object; and applying the liquid material from the surface side of the outer sheet while the surface side of the inner sheet is in contact with the object.

4. A method for using a laminated fiber sheet, comprising the steps of: wetting a liquid material onto the laminated fiber sheet, the method comprising the steps of: Regarding the laminated fiber sheet, the inner sheet and the outer sheet are insoluble in liquids; The inner sheet has a median fiber diameter of 0.3 μm or more and 5 μm or less, the outer sheet has a larger median fiber diameter than the inner sheet; The inner sheet and the outer sheet are integrated, The laminated fiber sheet has an elongation rate in one direction in a planar direction of 20% or more and 100% or less, and an elongation rate in a direction perpendicular to the planar direction of the laminated fiber sheet is 0% or more and 30% or less, applying the laminated fiber sheet with the inner sheet facing an object; and applying said liquid to said laminated fiber sheet.

5. 5. A method for using the laminated fiber sheet according to claim 1, 2 or 4, wherein after the liquid is applied to the object, the laminated fiber sheet is applied with the inner sheet facing the object.

6. 5. A method for using the laminated fiber sheet according to claim 1, 2 or 4, wherein after the liquid is applied to the laminated fiber sheet, the laminated fiber sheet is applied with the inner sheet facing an object.

7. A method for using a laminated fiber sheet described in any one of claims 1 to 4, wherein the fusion strength at the interface between the integrated inner sheet and outer sheet is 0.01 N / 20 mm or more and 10 N / 20 mm or less.

8. The method for using the laminated fiber sheet according to any one of claims 1 to 4, wherein the laminated fiber sheet is in the form of a bandage, a dressing, a tube, or a glove.

9. A laminated fiber sheet comprising an inner sheet laminated on one side of an outer sheet, the inner sheet and the outer sheet are insoluble in liquids; the inner sheet has a median fiber diameter of 0.3 μm or more and 5 μm or less, and the outer sheet has a larger median fiber diameter than the inner sheet, the inner sheet and the outer sheet are adjacent to each other, and the inner sheet and the outer sheet are integrated by fusion of the fibers constituting the inner sheet and the fibers constituting the outer sheet, The laminated fiber sheet contains a liquid, the liquid being unevenly distributed in the inner sheet.

10. A laminated fiber sheet as described in claim 9, wherein the fusion strength at the interface between the integrated inner sheet and outer sheet is 0.01 N / 20 mm or more and 10 N / 20 mm or less.

11. The laminated fiber sheet is a laminated fiber sheet as described in claim 9 or 10, wherein the elongation rate in one direction in the planar direction is 20% or more and 100% or less, and the elongation rate in the direction perpendicular to the one direction is 0% or more and 30% or less.

Citation Information

Patent Citations

  • Cosmetic sheet

    JP2008179629A

  • Method for adhering nano-fiber sheet

    JP2010167780A

  • Laminated sheet and method of manufacturing the same

    JP2012214922A

  • Hand mask