Proton conductors, membrane electrode assemblies, electrochemical cells and fuel cell stacks
The optimized Ba a Zr 1-x-y Yb x Cu y O 3-δ proton conductor addresses the conductivity issues in PCFCs by optimizing Cu substitution, enhancing proton conductivity and power generation efficiency.
Patent Information
- Application Number
- JP2024539643
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-05-15
- Filing Date
- 2024-02-27
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2044-02-27
AI Technical Summary
Existing proton conductors in proton conducting ceramic fuel cells (PCFCs) suffer from reduced proton conductivity and performance issues due to the addition of CuO, which compromises the sinterability and conductivity, limiting high power generation efficiency and output.
A proton conductor with the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ is developed, where 0.95≦a≦1.05, 0.1≦x≦0.4, 0.01
The optimized proton conductor exhibits enhanced proton conductivity, enabling PCFCs to achieve higher power generation efficiency and output by maintaining high fuel utilization rates and reducing internal resistance.
Smart Images

Figure 0007569473000002 
Figure 0007569473000003 
Figure 0007569473000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to proton conductors, membrane electrode assemblies, electrochemical cells and fuel cell stacks. [Background technology]
[0002] A solid oxide fuel cell (hereinafter referred to as "SOFC") is a fuel cell that uses a solid oxide as the electrolyte that constitutes the electrolyte membrane. Oxide ion conductors such as stabilized zirconia are widely used as the solid oxide electrolyte, and SOFCs have the advantage of having higher power generation efficiency than solid polymer electrolyte fuel cells (PEFCs).
[0003] Proton-conducting ceramic fuel cells (hereinafter referred to as "PCFC"), a type of SOFC, are characterized by the use of a proton-conducting solid oxide as the electrolyte that constitutes the electrolyte membrane. In a typical SOFC, water vapor is generated on the fuel electrode side due to the power generation reaction. For this reason, in an operating environment with a high fuel utilization rate, the hydrogen fuel is diluted by the water vapor, reducing the electromotive force of the fuel cell and increasing the risk of cell deterioration due to fuel starvation. Therefore, a typical SOFC cannot achieve a sufficiently high fuel utilization rate.
[0004] On the other hand, in PCFCs that use a proton conductor as the electrolyte, the generation of water vapor from the power generation reaction proceeds on the air electrode side, suppressing the dilution of hydrogen at the fuel electrode. This makes it possible to maintain a high electromotive force of the fuel cell even when operated at a high fuel utilization rate, and also reduces the risk of fuel starvation, making it advantageous for operation at a high fuel utilization rate. Since the power generation efficiency of a fuel cell is expressed as the product of the cell voltage and the fuel utilization rate, PCFCs, which can achieve both a high fuel utilization rate and a high electromotive force, are expected to have particularly high power generation efficiency among SOFCs. Furthermore, the ability to maintain a high electromotive force also means that the fuel cell can be operated at a higher current density, which is advantageous in terms of increasing output.
[0005] In order to achieve high power generation efficiency and high output of PCFCs, it is important to reduce the internal resistance of the cell during power generation, and to do so, it is important to improve the proton conductivity of the proton conductor used as the electrolyte.
[0006] A typical proton conductor is BaZrO, which has a perovskite structure. 3 , BaCeO 3 , and Ba(Ce,Zr)O 3 In these materials, materials are used in which the Zr or Ce sites are partially replaced with metal elements having a valence of +3, such as yttrium (Y) or ytterbium (Yb). These materials are known to have relatively high proton conductivity. In particular, BaZrO 3 The proton conductor in the system is CO contained in the fuel gas of the fuel cell or in the air. 2 It has been attracting attention because of its relatively high chemical stability against BaZrO 3 In the case of proton conductors based on this system, when Y is used as a replacement element, the NiO used in the anode and the by-product BaY 2 NiO 5-δ (δ is the amount of oxygen vacancies) is easily generated. Note that δ represents the amount of oxygen vacancies. BaY 2 NiO 5-δ The formation of BaZrO leads to a decrease in the performance and reliability of the fuel cell. On the other hand, when Yb is used as a replacement element, it has the advantage that by-products are less likely to be generated. 3 Materials that use Yb as a substitution element in proton conductors based on this system are considered to be promising materials for practical use. Yb-substituted BaZrO 3 If the proton conductivity can be further improved based on this, it will be advantageous for realizing fuel cells with high power generation efficiency or high power density.
[0007] In Non-Patent Document 1, Yb-substituted BaZrO 3 According to Non-Patent Document 1, Yb-substituted BaZrO 3 By adding 1.0mol% CuO to Yb-substituted BaZrO 3The effect of promoting sintering has been obtained.
Prior Art Documents
Non-Patent Documents
[0008]
Non-Patent Document 1
Summary of the Invention
Problems to be Solved by the Invention
[0009] According to Non-Patent Document 1, by adding 1.0 mol% of CuO, the sinterability of Yb-substituted BaZrO 3 is improved, but the proton conductivity of Yb-substituted BaZrYbO substituted with 1.0 mol% Cu obtained thereby 3 is lower than that of the one不含 Cu.
[0010] An object of the present disclosure is to provide a proton conductor applicable to a PCFC and having improved proton conductivity.
Means for Solving the Problems
[0011] The proton conductor of the present disclosure is a compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ and includes where 0.95 ≦ a ≦ 1.05, 0.1 ≦ x ≦ 0.4, 0.01 < y < 0.20, and 0 < δ ≦ 0.65 are satisfied.
Effects of the Invention
[0012] The present disclosure provides a proton conductor that is applicable to PCFCs and has improved proton conductivity. [Brief description of the drawings]
[0013] [Figure 1] FIG. 1 shows a cross-sectional view of an electrolyte membrane according to the second embodiment. [Diagram 2] FIG. 2 shows a cross-sectional view of a membrane electrode assembly according to a third embodiment. [Diagram 3] FIG. 3 shows a cross-sectional view of an electrochemical cell according to embodiment 4. [Figure 4] FIG. 4 shows a fuel cell system including a fuel cell stack according to a fifth embodiment. [Diagram 5] FIG. 5 is a flow chart showing a method for producing pellets of proton conductor according to the examples and comparative examples. [Figure 6] FIG. 6 shows a procedure for producing the electrochemical cell of Example 6 using the proton conductor of Example 2. [Figure 7] FIG. 7 is a graph showing the current-voltage characteristics and current output characteristics of the electrochemical cell of Example 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] [How one embodiment of the present disclosure was achieved] In Non-Patent Document 1, by adding 1.0 mol% CuO, Yb-substituted BaZrO 3 However, the sinterability of the resulting BaZrO2 alloy, which is Yb-substituted with 1.0 mol% Cu, is improved. 3 The proton conductivity of the Cu-free film is decreased compared to that of the Cu-free film.
[0015] Therefore, as a result of intensive studies on the substitution amount of Cu, it was found that when the substitution amount of Cu is a small amount of 1.0 mol%, the proton conductivity decreases, whereas by increasing the substitution amount further, it is possible to improve the proton conductivity, that is, the inventors found that there is an optimal range for the substitution amount of Cu. As a result, the present disclosure described below has been achieved.
[0016] [Embodiments of the Present Disclosure] Hereinafter, embodiments of the present disclosure will be described with reference to the drawings.
[0017] (Embodiment 1) The proton conductor according to Embodiment 1 contains a compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ Here, in the above chemical formula, 0.95 ≦ a ≦ 1.05, 0.1 ≦ x ≦ 0.4, 0.01 < y < 0.20, and 0 < δ ≦ 0.65 are satisfied.
[0018] As demonstrated in Examples 1 to 5 described later, the proton conductor according to Embodiment 1 has improved proton conductivity. Specifically, the proton conductor according to Embodiment 1 has a higher proton conductivity than a compound in which Cu is not contained in the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ that is, a compound where y = 0. Therefore, when the proton conductor according to Embodiment 1 is applied to a PCFC, it is possible to achieve higher power generation efficiency and higher output of the PCFC.
[0019] The chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δIn the above, 0.04≦y≦0.16 may be satisfied. By including such a compound, the proton conductor according to the first embodiment has further improved proton conductivity. As a result, when the proton conductor according to the first embodiment is applied to a PCFC, it is possible to realize further high power generation efficiency and high output of the PCFC.
[0020] Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ In the above, 0.125≦y≦0.16 may be satisfied. By including such a compound, the proton conductor according to the first embodiment has further improved proton conductivity. As a result, when the proton conductor according to the first embodiment is applied to a PCFC, it is possible to realize further high power generation efficiency and high output of the PCFC.
[0021] Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ In the above, 0.125≦y≦0.15 may be satisfied. By including such a compound, the proton conductor according to the first embodiment has further improved proton conductivity. As a result, when the proton conductor according to the first embodiment is applied to a PCFC, it is possible to realize further high power generation efficiency and high output of the PCFC.
[0022] Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ In this case, y=0.15 may be satisfied. By including such a compound, the proton conductor according to the first embodiment has particularly improved proton conductivity. As a result, when the proton conductor according to the first embodiment is applied to a PCFC, it is possible to realize a PCFC with even higher power generation efficiency and higher output.
[0023] The proton conductor according to embodiment 1 can be synthesized by the citrate complex method, the solid-phase sintering method, the co-precipitation method, the nitrate method, or the spray granulation method.
[0024] The proton conductor according to the first embodiment has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to the first embodiment may contain a compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to the first embodiment may contain a compound represented by the chemical formula Ba in a molar ratio of 5% or more, or 20% or more. a Zr 1-x-y Yb x Cu y O 3-δ By containing the compound represented by the formula: the proton conductor according to embodiment 1 can exhibit high proton conductivity.
[0025] The proton conductor according to the first embodiment has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to the first embodiment may be composed of a compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ "Comprised of a compound represented by the chemical formula Ba" means that in the proton conductor according to embodiment 1, a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to the first embodiment contains a compound represented by the chemical formula Ba in an amount of 80% or more by mole. a Zr 1-x-y Yb x Cu y O 3-δWhen the proton conductor according to embodiment 1 is composed of a compound represented by the formula:
[0026] As an example, the proton conductor according to embodiment 1 has the formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to the first embodiment may be substantially composed of a compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The term "comprised of a compound represented by the chemical formula Ba" means that the proton conductor according to embodiment 1 is made of a compound represented by the chemical formula Ba, excluding components contained as unavoidable impurities. a Zr 1-x-y Yb x Cu y O 3-δ In this case, in the proton conductor according to the first embodiment, the proton conductor is composed only of a compound represented by the chemical formula BaZr (1-x-y) Yb x Sc y O 3-δ The compound represented by the formula (I) may account for 95% or more in terms of molar ratio.
[0027] The proton conductor according to the first embodiment has the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ The proton conductor according to the first embodiment may further contain other components in addition to the compound represented by the formula (I). The proton conductor according to the first embodiment may further contain, as other components, for example, impurities generated in the process of synthesizing the above-mentioned compound.
[0028] The proton conductor according to embodiment 1 contains a compound of the formula Ba a Zr 1-x-y Yb x Cu y O 3-δThe average crystal grain size of the compound represented by the formula (I) is, for example, 0.1 μm or more and 10 μm or less. Even if the average crystal grain size is within the above range, or even if it is smaller than 0.1 μm, the proton conductor according to the first embodiment can achieve high proton conductivity. Here, the average crystal grain size can be determined, for example, by using the median diameter (volume basis) obtained from the measurement of particle size distribution.
[0029] (Embodiment 2) 1 shows a cross-sectional view of an electrolyte membrane 10 according to embodiment 2. The proton conductor contained in the electrolyte membrane 10 is the proton conductor described in embodiment 1.
[0030] The proton conductor contained in the electrolyte membrane 10 according to embodiment 2 has improved proton conductivity as described in embodiment 1. Therefore, the electrolyte membrane 10 according to embodiment 2 can have high proton conductivity. As a result, when the electrolyte membrane 10 according to embodiment 2 is applied to the electrolyte membrane of a PCFC, it can achieve high power generation efficiency and high output of the PCFC.
[0031] The electrolyte membrane 10 contains the proton conductor described in the first embodiment as an electrolyte material. a Zr 1-x-y Yb x Cu y O 3-δ The proton conductive material may further contain other compounds that exhibit proton conductivity other than the compound represented by the formula BaZr 1-x1 M1 x1 O 3-δ The compound represented by the chemical formula BaCe 1-x2 M2 x2 O 3-δ Compounds represented by the formula BaZr 1-x3-y3 Ce x3 M3 y3 O 3-δIt is a compound represented by [here, M1, M2, and M3 each contain at least one selected from the group consisting of Pr, Nd, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Y, Sc, In, and Lu, and 0 < x1 < 1, 0 < x2 < 1, 0 < x3 < 1, 0 < y3 < 1, and 0 < δ < 0.5 are satisfied]. The electrolyte membrane 10 may further contain an electrolyte material other than the proton conductor.
[0032] The thickness of the electrolyte membrane 10 according to Embodiment 2 is not particularly limited and can be appropriately determined according to the application. As an example, the thickness of the electrolyte membrane 10 can be, for example, from 1 to 500 μm, and can be from 1 to 50 μm.
[0033] The electrolyte membrane 10 is produced, for example, by a tape casting method, a spin coating method, a dip coating method, sputtering, or PLD (Pulse Laser Deposition).
[0034] (Embodiment 3) FIG. 2 shows a cross-sectional view of the membrane electrode assembly 20 according to Embodiment 3. The membrane electrode assembly 20 includes an electrolyte membrane 21 and an electrode 22 provided on the electrolyte membrane 21. The electrolyte membrane 21 in the membrane electrode assembly 20 is the electrolyte membrane 10 described in Embodiment 2.
[0035] The electrolyte membrane 21 in the membrane electrode assembly 20 according to Embodiment 3 contains a proton conductor having improved proton conductivity as described in Embodiment 2. Therefore, the electrolyte membrane 21 can have high proton conductivity. Thereby, when the membrane electrode assembly 20 according to Embodiment 3 is applied to the electrodes and electrolyte membrane of the PCFC, high power generation efficiency and high output of the PCFC can be realized.
[0036] As described above, since the electrolyte membrane 21 is the electrolyte membrane 10 described in Embodiment 2, a detailed description of the electrolyte membrane 21 is omitted here.
[0037] The material constituting the electrodes 22 can be selected appropriately depending on the application to which the membrane electrode assembly 20 is to be applied.
[0038] The membrane electrode assembly 20 may be used, for example, as an electrode and electrolyte membrane of a fuel cell, or as an electrode and electrolyte membrane of a PCFC. Thus, for example, the electrode 22 may function as a fuel electrode or as a cathode.
[0039] When the electrode 22 in the membrane electrode assembly 20 is applied, for example, to an anode of a fuel cell, particularly an anode of a PCFC, the electrode 22 may mainly contain, for example, at least one of the following compounds. (i) A mixture of an electrolyte material contained in the electrolyte membrane 21, one or more metals selected from the group consisting of Co, Fe, Pt, and Pd, and Ni (i.e., a cermet). (ii) Lanthanum-containing composite oxides (iii) Barium-containing composite oxides (iv) Strontium-containing composite oxides
[0040] When the electrode 22 mainly contains a certain compound, it means that the mass ratio of that compound in the electrode 22 is the largest.
[0041] When the electrode 22 in the membrane electrode assembly 20 is applied to, for example, an air electrode of a fuel cell, particularly an air electrode of a PCFC, the electrode 22 includes, for example, a composite compound. In this case, the electrode 22 may mainly include, for example, lanthanum strontium cobalt oxide, lanthanum strontium cobalt iron oxide, lanthanum barium cobalt oxide, barium strontium cobalt iron oxide, or the like. In this case, the electrode 22 may be formed on the electrolyte membrane 21 by, for example, a screen printing method.
[0042] The electrode 22 has a thickness of, for example, 1 μm to 1000 μm. When the electrode 22 also serves as a support for the cell, the electrode 22 desirably has a thickness of 100 μm to 700 μm. When a component other than the electrode 22 serves as a support for the cell, the electrode 22 desirably has a thickness of 10 μm to 50 μm.
[0043] 2, the electrolyte membrane 21 and the electrode 22 are in contact with each other, but another layer may be provided between the electrolyte membrane 21 and the electrode 22. An example of the another layer is a functional layer. The functional layer is a layer that promotes the movement of electrons or protons between the electrolyte membrane 21 and the electrode 22. The functional layer is made of, for example, a composite of a cermet and a complex oxide.
[0044] (Embodiment 4) FIG. 3 shows a cross-sectional view of an electrochemical cell 30 according to a fourth embodiment.
[0045] The electrochemical cell 30 according to the fourth embodiment includes a first electrode 31, a second electrode 32, and an electrolyte membrane 33. The electrolyte membrane 33 is provided between the first electrode 31 and the second electrode 32. In other words, as shown in Fig. 3, in the electrochemical cell 30, the first electrode 31, the electrolyte membrane 33, and the second electrode 32 are provided in this order. The electrolyte membrane 33 in the electrochemical cell 30 is the electrolyte membrane 10 described in the second embodiment.
[0046] The electrolyte membrane 33 in the electrochemical cell 30 according to the embodiment 4 includes a proton conductor having improved proton conductivity as described in the embodiment 2. Therefore, the electrolyte membrane 33 can have high proton conductivity. As a result, when the electrochemical cell 30 according to the embodiment 4 is used as, for example, a PCFC, it can realize high power generation efficiency and high output of the PCFC.
[0047] As described above, the electrolyte membrane 33 in the electrochemical cell 30 is the electrolyte membrane 10 described in embodiment 2. Therefore, a detailed description of the electrolyte membrane 33 will be omitted here.
[0048] The electrochemical cell 30 according to the fourth embodiment may be used, for example, as a fuel cell or a PCFC. Thus, for example, the first electrode 31 may function as a fuel electrode, and the second electrode 32 may function as a cathode.
[0049] When first electrode 31 functions as a fuel electrode of a fuel cell such as a PCFC, the material used for first electrode 31 is the same as that described in the third embodiment as the material used when electrode 22 is used as a fuel electrode.
[0050] When second electrode 32 functions as an air electrode of a fuel cell such as a PCFC, the material used for second electrode 32 is the same as that described in the third embodiment as the material used when electrode 22 is used as an air electrode.
[0051] 3, the first electrode 31 and the second electrode 32 are provided in contact with the electrolyte membrane 33. However, another layer may be provided between the first electrode 31 and the electrolyte membrane 33. Also, another layer may be provided between the second electrode 32 and the electrolyte membrane 33. An example of the another layer is, for example, a functional layer. The functional layer is the same as the functional layer described in the third embodiment.
[0052] The electrochemical cell 30 may be used in fuel cells, electrochemical hydrogen pumps, hydrogen sensors and water electrolysis devices.
[0053] (Embodiment 5) FIG. 4 shows a fuel cell system 1000 including a fuel cell stack 40 according to a fifth embodiment.
[0054] The fuel cell stack 40 includes a plurality of electrochemical cells 30. The plurality of electrochemical cells 30 are stacked together to form the fuel cell stack 40. The electrochemical cells 30 are described in the fourth embodiment.
[0055] In the fuel cell system 1000 according to the fifth embodiment, the electrochemical cell 30 is used as a fuel cell. Therefore, in this case, the first electrode 31 functions as a fuel electrode, and the second electrode 32 functions as a cathode.
[0056] The fuel cell system 1000 further includes a raw material gas supply path 1023 and an oxidizing gas supply path 1024. The raw material gas supply path 1023 is connected to the first electrode 31 and the raw material supplier 1022. The oxidizing gas supply path 1024 is connected to the second electrode 32 and the oxidizing gas supplier 1021.
[0057] As described in the third embodiment, the electrochemical cell 30 can achieve high power generation efficiency and high output of the PCFC, and therefore the fuel cell stack 40 can achieve high power generation efficiency and high output as a fuel cell stack.
[0058] The fuel cell stack 40 is housed in a housing 1014, for example.
[0059] The housing 1014 may be made of a heat insulating material.
[0060] An oxidant gas is supplied to the second electrodes 32 of the stacked electrochemical cells 30. Specifically, the oxidant gas is supplied from an oxidant gas supplier 1021 through an oxidant gas supply path 1024 to the second electrodes 32 (i.e., cathodes) of the multiple electrochemical cells 30.
[0061] At the second electrode 32, the following reaction (1) proceeds. O 2 +4H + +4e - →2H 2 O (1)
[0062] The oxidant gas is, for example, air.
[0063] The raw material is supplied from a raw material supplier 1022 through a raw material gas supply path 1023 to the first electrodes 31 of the multiple electrochemical cells 30 .
[0064] In the first electrode 31, the following reaction (2) proceeds. 2H 2 →4H + +4e - (2)
[0065] The raw material is, for example, a hydrogen molecule.
[0066] Hydrogen may be generated by a reforming reaction. Alternatively, hydrogen may be generated by water electrolysis.
[0067] In this way, the fuel cell system 1000 operates. Then, the fuel cell system 1000 generates electricity.
[0068] [Other Embodiments] (Appendix) According to the description of the above embodiments, the following technology is disclosed.
[0069] (Technology 1) A compound represented by the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ is included, where 0.95 ≦ a ≦ 1.05, 0.1 ≦ x ≦ 0.4, 0.01 < y < 0.20, and 0 < δ ≦ 0.65 are satisfied, a proton conductor.
[0070] With this configuration, the proton conductor according to Technology 1 has improved proton conductivity. Therefore, when the proton conductor according to Technology 1 is applied to a PCFC, high power generation efficiency and high output of the PCFC can be realized.
[0071] (Technology 2) In the above chemical formula, 0.04 ≦ y ≦ 0.16 is satisfied, the proton conductor according to Technology 1.
[0072] With this configuration, when the proton conductor according to Technology 2 is applied to a PCFC, it can realize even higher power generation efficiency and higher output of the PCFC.
[0073] (Technology 3) In the above chemical formula, 0.125≦y≦0.16 is satisfied. The proton conductor according to claim 2.
[0074] With this configuration, when the proton conductor according to Technology 3 is applied to a PCFC, it can realize even higher power generation efficiency and higher output of the PCFC.
[0075] (Technology 4) In the above chemical formula, 0.125≦y≦0.15 is satisfied. The proton conductor according to claim 3.
[0076] With this configuration, when the proton conductor according to Technology 4 is applied to a PCFC, it can realize even higher power generation efficiency and higher output of the PCFC.
[0077] (Technology 5) In the above chemical formula, y=0.15 is satisfied. The proton conductor according to claim 4.
[0078] With this configuration, when the proton conductor according to Technology 5 is applied to a PCFC, it can realize even higher power generation efficiency and higher output of the PCFC.
[0079] (Technology 6) The proton conductor according to any one of techniques 1 to 5 is included. Electrolyte membrane.
[0080] With this configuration, when the electrolyte membrane according to Technology 6 is applied to the electrolyte membrane of a PCFC, it is possible to realize high power generation efficiency and high output of the PCFC.
[0081] (Technology 7) The electrolyte membrane according to claim 6, and an electrode provided on the electrolyte membrane. Membrane electrode assembly.
[0082] With this configuration, when the membrane electrode assembly according to Technology 7 is applied to the electrodes and electrolyte membrane of a PCFC, it can realize high power generation efficiency and high output of the PCFC.
[0083] (Technology 8) A first electrode; A second electrode; The electrolyte membrane according to technology 6 is provided between the first electrode and the second electrode. Electrochemical cell.
[0084] With this configuration, when the electrochemical cell according to Technology 8 is used as, for example, a PCFC, it can realize high power generation efficiency and high output of the PCFC.
[0085] (Technology 9) A plurality of electrochemical cells according to the technique of claim 8, Fuel cell stack.
[0086] With this configuration, the fuel cell stack according to Technology 9 can achieve high power generation efficiency and high output. EXAMPLES
[0087] The present disclosure will now be described in more detail with reference to the following examples and comparative examples.
[0088] <Proton conductor> As described below, proton conductors were prepared in Examples 1 to 5 and Comparative Examples 1 to 5. The proton conductivity of each proton conductor was evaluated.
[0089] [Example 1] (Preparation of pellets for evaluation of proton conductors) 5 is a flow chart showing a method for producing pellets of proton conductors according to examples and comparative examples.The production of pellets for evaluation of proton conductors will be described with reference to FIG.
[0090] The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.076 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO 3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.004 mol
[0091] The above starting materials were added to and dissolved in 1000 mL of distilled water to obtain a mixed liquid, and the mixed liquid was stirred (S11).
[0092] Next, 0.3 mol of citric acid (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) and 0.3 mol of ethylenediaminetetraacetic acid (manufactured by Fuji Film Wako Pure Chemical Industries, Ltd.) were added to the mixed solution (S12). Hereinafter, "ethylenediaminetetraacetic acid" will be referred to as "EDTA".
[0093] Next, ammonia water (28% by mass, manufactured by Kishida Chemical Co., Ltd.) was added to the mixture, and the pH of the mixture was adjusted to 10 using a pH meter (manufactured by Horiba, Ltd.) (S13).
[0094] Next, the mixture was stirred at a temperature of 90° C. (S14).
[0095] The temperature of the mixture was raised to 370°C using a hot stirrer to evaporate the water (solvent) and to remove the fat (S15), resulting in a black solid.
[0096] The obtained solid was transferred into a crucible and calcined in air at 900° C. for 10 hours (S16).
[0097] The calcined powder was pulverized (S17). The pulverized powder was then transferred to a plastic container together with zirconia balls.
[0098] Then, 100 g of ethanol (manufactured by Kanto Chemical Co., Ltd.) was added to the plastic container. The mixture thus obtained was pulverized for 72 hours using a ball mill (S18).
[0099] After grinding with a ball mill, the mixture was dried using a lamp to remove the ethanol from the mixture (S19). In this way, a powder was obtained.
[0100] Next, the obtained powder was pressed into a cylindrical shape using a hydraulic pump (made by Enerpac Co., Ltd.) and a powder molding die with a diameter of 20 mm, and further molded into a pellet at a pressure of 250 MPa using a cold isostatic press (made by Sansho Industry Co., Ltd.). The obtained circular pellet was sintered in an oxygen atmosphere at 1500°C for 10 hours (S20). As a result, a sintered pellet of the proton conductor was obtained.
[0101] The obtained sintered pellets were cut into disks with a thickness of approximately 500 μm using a low-speed cutter (Isomet 4000). In this way, pellets for evaluation were obtained. Ethanol was dropped onto #500 emery paper, and both sides of the pellets for evaluation were polished.
[0102] Then, Ag paste (manufactured by Tanaka Kikinzoku Kogyo Co., Ltd.) was applied to both polished surfaces of the evaluation pellet by screen printing. The applied Ag paste had a diameter of 8 mm.
[0103] Then, the evaluation pellets coated with the Ag paste were fired in an air atmosphere for 1 hour at 900° C. In this manner, the evaluation pellets according to Example 1 were produced.
[0104] (Evaluation of proton conductivity) The proton conductivity of the proton conductor was calculated from the resistance and thickness of the pellet using the evaluation pellet according to Example 1. The resistance of the pellet was measured based on the AC impedance method. The method for determining the proton conductivity is as follows.
[0105] Using an LCR meter (HIOKI: IM2526), an AC signal was applied to the pellet with an amplitude of 10 mV in the frequency range of 8 MHz to 4 Hz. This measurement was performed in a 1.9% humidified, 1% hydrogen, nitrogen diluted gas atmosphere at 700°C. A Cole-Cole plot was then output. Based on the arc of the output Cole-Cole plot, the intersection point between the arc and the real axis was determined. The real axis is the axis where the Y-axis value in the Cole-Cole plot graph is 0. The intersection point on the high frequency side of the arc was taken as the resistance of the pellet.
[0106] Based on the measured resistance and the thickness of the pellet, the proton conductivity of the proton conductor was calculated.
[0107] [Example 2] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.075 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.005 mol
[0108] The subsequent procedures were the same as in Example 1.
[0109] (Evaluation of proton conductivity) The proton conductor of Example 2 was evaluated in the same manner as in Example 1.
[0110] [Example 3] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.0675 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO 3 ) 2 3H 2 O (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) 0.0125 mol
[0111] The subsequent procedures were the same as in Example 1.
[0112] (Evaluation of proton conductivity) The proton conductor of Example 3 was evaluated in the same manner as in Example 1.
[0113] [Example 4] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.065 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO 3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.015 mol
[0114] The subsequent procedures were the same as in Example 1.
[0115] (Evaluation of proton conductivity) The proton conductor of Example 4 was evaluated in the same manner as in Example 1.
[0116] [Example 5] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.064 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO 3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.016 mol
[0117] The subsequent procedures were the same as in Example 1.
[0118] (Evaluation of proton conductivity) The proton conductor of Example 5 was evaluated in the same manner as in Example 1.
[0119] [Comparative Example 1] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.08 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol
[0120] The pellets were fired at a temperature of 1650° C. The rest of the procedure was the same as in Example 1.
[0121] (Evaluation of proton conductivity) The proton conductor of Comparative Example 1 was evaluated in the same manner as in Example 1.
[0122] [Comparative Example 2] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.079 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO 3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.001 mol
[0123] The subsequent procedures were the same as in Example 1.
[0124] (Evaluation of proton conductivity) The proton conductor of Comparative Example 2 was evaluated in the same manner as in Example 1.
[0125] [Comparative Example 3] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.06 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Cu(NO 3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.02 mol
[0126] The subsequent procedures were the same as in Example 1.
[0127] (Evaluation of proton conductivity) The proton conductor of Comparative Example 3 was evaluated in the same manner as in Example 1.
[0128] [Comparative Example 4] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.0725 mol Yb(NO3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Ni(NO 3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.0075 mol
[0129] The subsequent procedures were the same as in Example 1.
[0130] (Evaluation of proton conductivity) The proton conductor of Comparative Example 4 was evaluated in the same manner as in Example 1.
[0131] [Comparative Example 5] (Preparation of pellets for evaluation of proton conductors) The following materials were prepared as starting materials for the proton conductor. Ba(NO 3 ) 2 (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.1mol ZrO(NO 3 ) 2 2H 2 O (Kanto Chemical Co., Ltd.) 0.065 mol Yb(NO 3 ) 3 3H 2 O (Mitsuwa Chemical Co., Ltd.) 0.02 mol Ni(NO 3 ) 2 3H 2 O (Fujifilm Wako Pure Chemical Industries, Ltd.) 0.015 mol
[0132] The subsequent procedures were the same as in Example 1.
[0133] (Evaluation of proton conductivity) The proton conductor of Comparative Example 5 was evaluated in the same manner as in Example 1.
[0134] The proton conductivities measured for Examples 1 to 5 and Comparative Examples 1 to 5 are summarized in Table 1.
[0135]
Table 1
[0136] The proton conductivities of the proton conductors in Examples 1 to 5 were 0.012 S / cm, 0.013 S / cm, 0.013 S / cm, 0.019 S / cm, and 0.010 S / cm, respectively. Also, in Comparative Example 1, the proton conductivity was 0.008 S / cm. From this, it was found that the proton conductivity was improved in the proton conductors of Examples 1 to 5.
[0137] Also, in the case where the addition amount y of Cu shown in Comparative Example 2 was 0.01, the proton conductivity was 0.007 S / cm. Therefore, when the addition amount y of Cu was 0.01, the proton conductivity would be lower than when no Cu was added. This result reproduced the result of Non-Patent Document 1. It was found that an effect of improving the proton conductivity can be obtained by making the value of y, which is the addition amount of Cu, larger than 0.01.
[0138] Also, in the case where the addition amount y of Cu shown in Comparative Example 3 was 0.20, the proton conductivity was 0.007 S / cm. Therefore, also when the addition amount y of Cu was 0.20, the proton conductivity would be lower than when no Cu was added. It was found that an effect of improving the proton conductivity can be obtained by making the value of y, which is the addition amount of Cu, smaller than 0.20.
[0139] That is, it was found that there is an optimal range for the addition amount y of Cu to improve the proton conductivity. Specifically, in the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ it was found that the compound in which Cu was added so that 0.01 < y < 0.20 was satisfied had an improved proton conductivity. In particular, when y = 0.15 shown in Example 4, it was found that the proton conductivity was high.
[0140] In Comparative Example 4 and Comparative Example 5, Ni was used instead of Cu as an additive element. In Comparative Example 4 and Comparative Example 5, the amount of Ni added was y=0.075 and y=0.15, respectively. The proton conductivity in Comparative Example 4 and Comparative Example 5 was 0.001 S / cm and 0.004 S / cm, respectively, which was lower than the case where Ni was not added (i.e., Comparative Example 1). It was found that y=0.075 and y=0.15 are the ranges of the amount of addition in which the proton conductivity is improved when Cu is added, but the proton conductivity is not improved when Ni is used. Therefore, it was found that the effect of improving the proton conductivity is unique to the case where Cu is added.
[0141] Although the mechanism behind these phenomena is not clear, since proton conductivity is expressed as the product of the amount of protons, which are the conductive carriers, and the mobility, it means that either or both of them have improved. The amount of protons is the amount of water dissolved in the crystal lattice. Water dissolution proceeds when water molecules fill the oxygen vacancies in the crystal, so it is advantageous for the crystal lattice to have many oxygen vacancies. When Cu is added, Cu has a lower valence than Zr's +4, so the amount of oxygen vacancies increases to balance the charges in the crystal. Therefore, it is thought that the more Cu is added, the more oxygen vacancies there will be. Therefore, theoretically, it is advantageous for proton dissolution, and the amount of proton dissolution may increase.
[0142] However, in Comparative Example 2 and Comparative Example 3, although Cu is added, the proton conductivity is decreased. Alternatively, in Comparative Example 4 and Comparative Example 5, Ni is added. Although Ni is considered to have a lower valence than +4 of Zr and thus increase the amount of oxygen vacancies, the proton conductivity is decreased. It is presumed that the mobility, which is another factor of the proton conductivity, is decreased. The amount of the added element varies in the local strain state or electronic state of the crystal lattice depending on the element species. Since the influence on the mobility such as local trapping of protons changes when the strain state and electronic state are different, it is considered that the proton conductivity is decreased in Comparative Example 2 to Comparative Example 5. For Examples 1 to 5, it is considered that the decrease in mobility is suppressed or the mobility is improved.
[0143] In addition, in Examples 1 to 5, in the chemical formula Ba a Zr 1-x-y Yb x Cu y O 3-δ the effect of adding Cu was confirmed for the case where x = 0.2. In the above chemical formula, a proton conductor that satisfies 0.1 ≦ x ≦ 0.4 and 0.01 < y < 0.20 for y similarly exhibits the effect of improving the proton conductivity.
[0144] <Electrochemical cell> [Example 6] (Fabrication of Electrochemical Cell) With reference to FIG. 6, the fabrication of the electrolyte membrane and the electrochemical cell using the same will be described. FIG. 6 shows the procedure for fabricating the electrochemical cell of Example 6 using the proton conductor of Example 2.
[0145] (1) Fabrication of Electrolyte Green Sheet (see S100 to S102) First, an electrolyte ceramic slurry was prepared. The proton conductor used in the electrolyte ceramic slurry was the proton conductor of Example 2. However, instead of the die molding, CIP, and firing processes of S20 shown in the flow chart of Figure 5, the proton conductor was fired in air at 1200°C for 10 hours. A powder of the proton conductor was obtained by firing in air at 1200°C for 10 hours.
[0146] The proton conductor powder (BaZr 0.75 Yb 0.20 Cu 0.05 O 3-δ The following ingredients were mixed:
[0147] Proton conductor of Example 2 (BaZr 0.75 Yb 0.20 Cu 0.05 O 3-δ ) 50g Polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd.) 5g Butyl benzyl phthalate (Kanto Chemical Co., Ltd.) 1.25g Mixed solvent 40g
[0148] The mixed solvent consisted of butyl acetate (20 g, manufactured by Kanto Chemical Co., Ltd.) and 1-butanol (20 g, manufactured by Kanto Chemical Co., Ltd.) In this manner, an electrolyte ceramic slurry was prepared.
[0149] Next, a film made of the electrolyte ceramic slurry was formed on a support sheet made of a polyethylene terephthalate film having a thickness of about 50 μm by the doctor blade method. The film made of the obtained slurry was heated at a temperature of 80° C. to evaporate the solvent. In this way, an electrolyte green sheet was produced. The electrolyte green sheet had a thickness of about 21 μm.
[0150] (2) Preparation of electrode green sheets (see S200 to S202) An electrode ceramic slurry was prepared by mixing the following materials:
[0151] The proton conductor used in the electrodes was the proton conductor of Comparative Example 1 (BaZr 0.80 Yb 0.20 O 3-δ ) was used. However, instead of the molding, CIP, and sintering processes of S20 shown in the flow chart of Figure 5, sintering was performed in air at 1200°C for 10 hours. Proton conductor powder was obtained by sintering in air at 1200°C for 10 hours.
[0152] Proton conductor BaZr of Comparative Example 1 0.80 Yb 0.20 O 3-δ ) 10g Polyvinyl butyral (manufactured by Sekisui Chemical Co., Ltd.) 5g Butyl benzyl phthalate (Kanto Chemical Co., Ltd.) 1.25g NiO (Sumitomo Metal Mining Co., Ltd.) 40g Mixed solvent 40g
[0153] The mixed solvent consisted of butyl acetate (20 g, Kanto Chemical Co., Ltd.) and 1-butanol (20 g, Kanto Chemical Co., Ltd.).
[0154] Next, a film made of the electrode ceramics slurry was formed on a support sheet made of a polyethylene terephthalate film having a thickness of about 50 μm by the doctor blade method. The film made of the slurry had a thickness of about 30 μm. The film made of the obtained slurry was heated at a temperature of 80° C. In this way, an electrode green sheet was produced.
[0155] (3) Sheet stacking (see S300 to S303) The electrolyte green sheet was cut to obtain one cut electrolyte green sheet. Then, the polyethylene terephthalate film was peeled off from the electrolyte green sheet. The cut electrolyte green sheet had a size of 140 mm x 140 mm. The electrode green sheet was cut to obtain one cut electrode green sheet. The cut electrode green sheet had a size of 140 mm x 140 mm.
[0156] A plurality of cut electrode green sheets were laminated to obtain a laminate. The laminate was then hot pressed. The hot pressing was carried out under conditions of 85°C and 13 MPa. In this manner, a first electrode was produced.
[0157] Further, one cut electrolyte green sheet was laminated on one main surface of the first electrode to obtain a laminate. The obtained laminate was then hot pressed. The hot pressing was performed under the conditions of 80°C and 13 MPa. In this manner, a compact was obtained.
[0158] The obtained molded body was further pressed at a pressure of 50 MPa (by Sansho Industry Co., Ltd.) to obtain a laminate. The thickness was almost unchanged and was about 700 μm.
[0159] The laminate was cut to a size of φ25 mm.
[0160] Finally, the cut laminate was sintered in an air atmosphere at 1475° C. for 2 hours. In this manner, a membrane electrode assembly was produced. The membrane electrode assembly was an assembly of an electrolyte membrane and a first electrode.
[0161] (4) Formation of the second electrode (see S304 and S305) Furthermore, a second electrode was provided on the obtained membrane electrode assembly.
[0162] LSC paste (manufactured by Noritake Company Limited, composition La 0.6 Sr 0.4 Chief of Staff 3-δ) was applied by screen printing to one of the main surfaces of the membrane electrode assembly where the electrolyte membrane was exposed. The applied LSC paste had a diameter of 10 mm. In this way, the precursor of the cell was obtained.
[0163] The cell precursor was then sintered in air at 950°C for 2 hours. In this manner, an electrochemical cell was fabricated that included a first electrode, an electrolyte membrane, and a second electrode. The first electrode functions as a fuel electrode. The second electrode functions as an air electrode.
[0164] (Electrochemical cell evaluation) Hydrogen and air were supplied to the electrochemical cell obtained by the above method, and a power generation test of the fuel cell was carried out.
[0165] The electrochemical cell was set in a fuel cell holder (manufactured by Chino Corporation) and placed in an electric furnace. The temperature of the fuel cell holder was raised to 700°C, and the fuel electrode (NiO-BaZr 0.80 Yb 0.20 O 3-δ Hydrogen gas humidified at 20°C was supplied to the anode at 100cc / min, and air gas humidified at 20°C was supplied to the cathode at 100cc / min, respectively, and the reduction of the anode was carried out for 3 hours. After that, the electric furnace temperature was set to 700°C, 600°C, 500°C, 400°C, and 300°C in that order, and after confirming that each temperature was stable, an electrochemical evaluation was carried out using a potentiogalvanostat (MODULAB XM ECS, manufactured by AMETEC).
[0166] In the electrochemical evaluation, the voltage of the fuel electrode and the air electrode was swept from the open circuit voltage to 0.4 V at 4 mV / sec, and a current-voltage curve and a current-output curve were obtained.
[0167] Figure 7 shows the current-voltage curves and current-output curves obtained in the electrochemical evaluation. The maximum output obtained was 0.83 W / cm at 700°C, 600°C, 500°C, 400°C, and 300°C, respectively. 2 , 0.62W / cm 2 , 0.37W / cm 2 , 0.14W / cm 2 , 0.02W / cm2 It was confirmed that the proton conductor according to the present disclosure can be used as an electrolyte in an electrochemical cell to extract a current. [Industrial Applicability]
[0168] The proton conductor according to the present disclosure is suitable for a system using an electrochemical cell of a hydrogen generation system or a fuel cell system. The membrane electrode assembly according to the present disclosure can also be used in an electrochemical hydrogen pump such as a hydrogen purification device or a hydrogen compression device. [Explanation of symbols]
[0169] 10 Electrolyte membrane 20 Membrane electrode assembly 21 Electrolyte membrane 22 electrodes 30 Electrochemical Cell 31 1st electrode 32 2nd electrode 33 Electrolyte membrane 40 Fuel Cell Stack 1000 Fuel Cell System 1014 Case 1021 Oxidant gas supply 1022 Raw material feeder 1023 Raw material gas supply route 1024 Oxidant gas supply route
Claims
1. Chemical formula: Ba a Zr 1-x-y Yb x Cu y O 3-δ The compound represented by the formula: Here, 0.95≦a≦1.05, 0.1≦x≦0.4, 0.01<y<0.20, and 0<δ≦0.65 are satisfied. Proton conductor.
2. In the above chemical formula, 0.04≦y≦0.16 is satisfied. The proton conductor according to claim 1 .
3. In the above chemical formula, 0.125≦y≦0.16 is satisfied. The proton conductor according to claim 2 .
4. In the above chemical formula, 0.125≦y≦0.15 is satisfied. The proton conductor according to claim 3 .
5. In the above chemical formula, y=0.15 is satisfied. The proton conductor according to claim 4.
6. The proton conductor according to any one of claims 1 to 5, Electrolyte membrane.
7. The electrolyte membrane according to claim 6 ; and an electrode provided on the electrolyte membrane. Membrane electrode assembly.
8. A first electrode; A second electrode; and the electrolyte membrane according to claim 6 provided between the first electrode and the second electrode. Electrochemical cell.
9. A plurality of electrochemical cells according to claim 8. Fuel cell stack.
Citation Information
Patent Citations
Electrochemical synthesizer for CO2 in-situ hydro-conversion as well as preparation method and application of electrochemical synthesizer
CN116078314A
Proton conductor and membrane electrode assembly
JP2019106360A
Fuel cell and manufacturing method of fuel cell
JP2020024847A
Electrode catalyst, membrane electrode assembly, electrochemical cell, and fuel cell system