Low dielectric material glass cloth, prepreg, and printed wiring board
Treating glass cloth with an alkoxy group-containing organopolysiloxane composition addresses adhesion and dielectric property issues, enhancing the reliability and performance of printed wiring boards for high-frequency applications.
Patent Information
- Application Number
- JP2019220561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2019-12-05
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2039-12-05
AI Technical Summary
Existing glass cloths for printed wiring boards face challenges in adhesion and adhesion with matrix resins, tensile strength, and dielectric properties, particularly in high-frequency applications, due to the presence of silanol groups and poor wettability, which affect the reliability and performance of electronic components.
Treating the glass cloth surface with an alkoxy group-containing organopolysiloxane composition reduces silanol groups and improves adhesion and tensile strength, enhancing dielectric properties, making it suitable for high-frequency applications.
The treated glass cloth exhibits improved adhesion and adhesion with matrix resins, resulting in highly reliable printed wiring boards with excellent dielectric properties, suitable for high-frequency electronic components.
Smart Images

Figure 0007569616000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a glass cloth for low dielectric materials, and a prepreg and a printed wiring board using said glass cloth. [Background technology]
[0002] With the remarkable development of digital technology, electronic devices such as tablet computers and smartphones are becoming lighter, thinner, smaller, and more functional. For example, printed wiring boards, which are one of the important components of these devices, need to be highly densely mounted and lighter, thinner, smaller, and more compact. To meet this demand, there is a strong demand for improved properties of glass cloth, which is an essential component used as a reinforcing material for printed wiring boards.
[0003] In addition, with the advancement of high speed and high frequency in computers, mobile devices, and communication infrastructure, the glass cloth used in printed wiring boards is required to have improved dielectric properties to reduce transmission loss, as well as low thermal expansion and high tensile rigidity. Furthermore, there is an increasing demand for thinner glass cloth to meet the demands for lighter, thinner, smaller, and multi-layered structures.
[0004] As a method for producing thin glass cloth, silica glass systems, in which the filament diameter is easier to control, are being investigated. For example, Patent Document 1 discloses a method for producing a silica glass cloth having a thickness of 27 μm. Patent Document 2 introduces a thin silica glass cloth having a thickness of 6 μm to 45 μm. However, since the thin silica glass cloth has poor tensile strength, it is necessary to improve the tensile strength by surface treatment or the like.
[0005] On the other hand, in the manufacture of substrates, the adhesion and bonding between glass cloth and thermosetting resin such as epoxy resin is important, and poor wettability between glass cloth and matrix resin leads to poor adhesion, and the inclusion of moisture at the interface and the influence of silanol groups present in the glass cloth cause a decrease in dielectric properties. For this reason, the surface of the glass cloth is treated with a silane coupling agent.
[0006] As an example of the use of a silane coupling agent, Patent Document 3 describes the use of a silane coupling agent for surface treatment of low dielectric glass cloth containing B2O3, but only mentions the improvement of moisture absorption resistance.
[0007] Patent Documents 4 to 6 list silazane compounds as surface treatment agents for glass fiber films and glass cloths, but these compounds are insufficient in reducing the silanol groups contained in the glass cloth. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2006-282401 A [Patent Document 2] JP 2009-263824 A [Patent Document 3] International Publication No. 2016 / 175248 Brochure [Patent Document 4] JP 2015-174937 A [Patent Document 5] JP 2015-155196 A [Patent Document 6] JP 2011-017113 A Summary of the Invention [Problem to be solved by the invention]
[0009] As described above, there is a demand for further improvements in adhesion and bonding with the matrix resin used in printed wiring boards, as well as in the strength and reliability of the wiring boards. In particular, there is a demand for a reduction in the number of silanol groups contained in the glass cloth in order to improve dielectric properties.
[0010] The present invention has been made to solve the above problems, and has an object to provide a glass cloth for use as a low dielectric material which has improved strength and excellent dielectric properties and is suitable for use in highly reliable printed wiring boards. [Means for solving the problem]
[0011] In order to achieve the above object, the present invention provides a glass cloth for low dielectric materials, which has a glass cloth substrate whose surface is treated with an alkoxy group-containing organopolysiloxane composition, wherein the alkoxy group-containing organopolysiloxane contained in the alkoxy group-containing organopolysiloxane composition has an average of 2 to 10 silicon atoms.
[0012] Moreover, the glass cloth for low dielectric materials of the present invention is preferably used for printed wiring boards for 5G / IoT and high frequency applications.
[0013] Such glass cloth for low dielectric materials has improved tensile strength and wettability with matrix resins, and therefore provides prepregs with excellent adhesion and bonding with matrix resins, and printed wiring boards with improved strength and excellent reliability. In particular, the amount of silanol groups present on the glass cloth surface can be reduced to improve the dielectric properties, making it suitable for 5G / IoT and high-frequency printed wiring boards.
[0014] It is also preferable that the alkoxy group-containing organopolysiloxane composition further contains a silane coupling agent made of an alkoxysilane.
[0015] Such a material can further reduce the number of silanol groups present on the surface of the glass cloth substrate, providing a printed wiring board with improved dielectric properties.
[0016] It is also preferable that the alkoxy group-containing organopolysiloxane composition further contains water.
[0017] Such a composition reduces the use of organic solvents, thereby protecting the safety of workers and protecting the global environment, and since the alkoxy group-containing organopolysiloxane is hydrolyzed and its reactivity increases, it can be applied uniformly to the surface of a glass cloth substrate, resulting in a printed wiring board with improved dielectric properties.
[0018] The glass cloth substrate has a dielectric loss tangent of 1×10 at 10 GHz. -4 ~1×10 -2 It is preferable that the glass cloth substrate is made of glass having the following properties:
[0019] If this is the case, the glass cloth for low dielectric materials will provide a printed wiring board with improved dielectric properties.
[0020] In this case, the glass is preferably at least one type selected from the group consisting of E glass, L glass, L2 glass, NE glass, NE2 glass, S glass, T glass, UT glass, LU glass, D glass, and silica glass.
[0021] In the present invention, a glass cloth substrate made of such glass can be used.
[0022] The present invention also provides a prepreg comprising the above-mentioned glass cloth for low dielectric materials and a matrix resin impregnated into the glass cloth.
[0023] Such a prepreg has excellent adhesion and bonding between the low dielectric material glass cloth and the matrix resin, and has improved strength, providing a highly reliable printed wiring board with excellent dielectric properties.
[0024] In this case, the matrix resin is preferably one or more resins selected from the group consisting of epoxy resins, silicone resins, polyimide resins, bismaleimide resins, polyphenylene ether resins, and polytetrafluoroethylene resins.
[0025] Such a prepreg provides a printed wiring board with improved dielectric properties.
[0026] The present invention further provides a printed wiring board comprising the above prepreg.
[0027] Such a printed wiring board has excellent dielectric properties and can be suitably used for electronic components having circuits for transmitting electrical signals of 10 GHz or more. Effect of the Invention
[0028] According to the present invention, the glass cloth for low dielectric materials, the surface of which is treated with an alkoxy group-containing organopolysiloxane composition, has improved tensile strength and wettability with matrix resin, and has excellent adhesion and bonding with matrix resin, and provides prepregs and printed wiring boards with improved strength and higher reliability. In particular, the amount of silanol groups present on the glass cloth surface is reduced, improving the dielectric properties, and the glass cloth is suitable for use in high frequency printed wiring boards for electronic components having circuits that transmit electric signals of 10 GHz or more. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] As described above, there has been a demand for the development of a glass cloth for use as a low dielectric material which has improved strength, excellent dielectric properties, and can be suitably used for highly reliable printed wiring boards.
[0030] As a result of extensive investigations into the above-mentioned problems, the present inventors have found that glass cloth the surface of which is treated with a specific alkoxy group-containing organopolysiloxane composition has excellent tensile strength and good dielectric properties and can be suitably used for high-frequency printed wiring boards used in electronic components having circuits for transmitting electrical signals of 10 GHz or more, and have completed the present invention.
[0031] That is, the present invention relates to a glass cloth for low dielectric materials, the surface of which is treated with an alkoxy group-containing organopolysiloxane composition, and the alkoxy group-containing organopolysiloxane contained in the alkoxy group-containing organopolysiloxane composition has an average of 2 to 10 silicon atoms.
[0032] The following describes an embodiment of the present invention, but this is shown by way of example only, and it goes without saying that various modifications are possible without departing from the technical concept of the present invention.
[0033] <Glass cloth for low dielectric materials> The glass cloth for low dielectric materials of the present invention is a glass cloth for low dielectric materials in which the surface of a glass cloth substrate is treated with an alkoxy group-containing organopolysiloxane composition, and the alkoxy group-containing organopolysiloxane contained in the alkoxy group-containing organopolysiloxane composition has an average of 2 to 10 silicon atoms.
[0034] Moreover, the glass cloth for low dielectric materials of the present invention is preferably used for printed wiring boards for 5G / IoT and high frequency applications.
[0035] Note that "5G / IoT" here refers to the fifth generation mobile communications system (5G) and the Internet of Things (IoT) that utilizes it, and "for 5G / IoT" refers to materials that have the properties required for high-speed, large-capacity communications, etc. Specific required properties include low dielectric constant and low transmission loss, and specific applications include computers, mobile terminals, and high-frequency printed wiring boards for communications infrastructure.
[0036] The glass cloth for low dielectric materials of the present invention has an improved tensile strength and wettability with a matrix resin by treating the surface of the glass cloth substrate with an alkoxy group-containing organopolysiloxane composition, and when producing a prepreg as described below, it has the effect of improving the adhesion and bondability between the glass cloth and the matrix resin, thereby providing a printed wiring board with improved strength.
[0037] Furthermore, the glass cloth for low dielectric materials of the present invention has the effect of improving the dielectric properties by surface-treating the glass cloth substrate with a composition containing an alkoxy group-containing organopolysiloxane having an average of 2 to 10 silicon atoms, whereby the alkoxy groups react with silanol groups on the surface of the glass cloth substrate to reduce the amount of silanol groups.
[0038] <Glass cloth substrate> The glass cloth substrate to be surface-treated with the alkoxy group-containing organopolysiloxane composition used in the glass cloth for low dielectric materials of the present invention will be described below.
[0039] The glass cloth substrate is not particularly limited, but has a dielectric loss tangent of 1×10 at 10 GHz. -4 ~1×10 -2 It is preferable that the glass cloth is made of a glass having a dielectric loss tangent of 5×10 at 10 GHz. Examples of the glass cloth substrate include one or more types of glass cloth selected from the group consisting of E glass, L glass, L2 glass, NE glass, NE2 glass, S glass, T glass, UT glass, LU glass, D glass, and silica glass. In terms of dielectric properties, it is preferable that the glass cloth is selected from L glass, L2 glass, NE glass, NE2 glass, LU glass, and silica glass. In particular, it is preferable that the dielectric loss tangent at 10 GHz is 5×10 -3 Less than or equal to 2 x 10 -4 ~2×10 -3 More preferred is a glass cloth made of silica glass.
[0040] In the present invention, the dielectric loss tangent at 10 GHz refers to a value measured by the method described in JIS R 1641:2007 (Method of measuring microwave dielectric properties of fine ceramic substrates).
[0041] In addition, it is preferable to remove organic matter such as a sizing agent adhering to the surface of the glass cloth substrate before surface treatment with the alkoxy group-containing organopolysiloxane composition, since this allows the surface of the glass cloth substrate to be treated evenly with the alkoxy group-containing organopolysiloxane composition. Methods for removing organic matter include heat cleaning treatment, corona treatment, and hot water washing.
[0042] The thickness of the glass cloth substrate is preferably 6 μm to 200 μm, more preferably 10 μm to 100 μm, and the mass per unit area is preferably 5 g / m 2 ~200g / m 2 and more preferably 10 g / m 2 ~100g / m 2 The glass cloth substrate is
[0043] <Alkoxy Group-Containing Organopolysiloxane Composition> The alkoxy group-containing organopolysiloxane composition used in the present invention will now be described.
[0044] <Alkoxy group-containing organopolysiloxane> The alkoxy group-containing organopolysiloxane composition used in the present invention essentially comprises a low molecular weight alkoxy group-containing organopolysiloxane having an average of 2 to 10 silicon atoms, preferably an average of 3 to 5. If the number of silicon atoms exceeds 10, many unreacted alkoxy groups remain when the surface of the glass cloth substrate is treated with the alkoxy group-containing organopolysiloxane composition, which may deteriorate the dielectric properties. If the number of silicon atoms is less than 2, the tensile strength of the glass cloth cannot be increased. In the present invention, the term "alkoxy group-containing organopolysiloxane" refers to an organopolysiloxane containing an alkoxy group directly bonded to a silicon atom, and examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, and an n-butoxy group. Of these, a methoxy group, an ethoxy group, and an isopropoxy group are preferred.
[0045] The alkoxy group-containing organopolysiloxane reacts with silanol groups on the surface of the glass cloth substrate to reduce the amount of said silanol groups, so that the glass cloth for low dielectric materials of the present invention has the effect of providing a printed wiring board with improved dielectric properties and enhanced reliability. The glass cloth for low dielectric materials of the present invention is particularly suitable for high-frequency printed wiring boards used in electronic components having circuits that transmit electric signals of 10 GHz or more.
[0046] The average number of silicon atoms referred to in this specification is determined from the number average molecular weight measured by gel permeation chromatography (GPC) under the following conditions using polystyrene as a standard substance.
[0047] [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.6mL / min Detector: UV detector Column: TSK Guardcolumn SuperH-L TSKgel SuperMultiporeHZ-M (4.6mm I.D. x 15cm x 4) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 3 μL (THF solution with a concentration of 0.5% by mass)
[0048] The alkoxy-containing organopolysiloxane may also contain functional groups other than alkoxy groups. The functional groups other than alkoxy groups may be the same or different functional groups in combination. Specific examples include alkyl groups such as methyl, ethyl, n-propyl, hexyl, octyl, and decyl; fluoroalkyl groups such as trifluoropropyl; aryl groups such as phenyl, methylphenyl, dimethylphenyl, and trimethylphenyl; alkenyl groups such as vinyl, allyl, 4-vinylbutyl, and 8-vinyloctyl; alicyclic unsaturated hydrocarbon groups such as 3-cyclohexenyl and norbornenyl; alkynyl groups such as ethynyl and 2-propynyl; aromatic unsaturated hydrocarbon groups such as styryl; unsaturated ester groups such as acrylic and methacrylic groups; unsaturated cyclic imide groups such as N-propylmaleimide; and amino groups such as methylamino, 3-aminopropyl, and N-2-(aminoethyl)-3-aminopropyl. Among these, alkenyl groups and unsaturated ester groups having a structure similar to that of the unsaturated groups contained in the thermosetting resin, which is the matrix resin, are preferred, and vinyl and methacrylic groups, which are particularly excellent in reactivity and adhesiveness, are more preferred.
[0049] By containing an organic group having a carbon-carbon unsaturated bond, the reactivity with the unsaturated group-containing thermosetting resin used as the matrix resin is improved, and the dielectric properties are improved due to improved adhesive strength, wettability, and adhesion.
[0050] The alkoxy group-containing organopolysiloxane may contain D units or T units that do not have an alkoxy group in the molecule, and organopolysiloxanes containing a branched structure, cyclic structure, or cage structure can also be used.
[0051] In addition, two or more alkoxy-containing organopolysiloxanes with different structures can be used in combination. The use of multiple oligomers in combination is preferable because it improves the tensile strength of the glass cloth and the adhesion to the resin for the substrate, and also provides excellent processability.
[0052] As a method for treating glass cloth using two or more different oligomers in combination, two or more oligomers having different structures may be used for surface treatment in any order multiple times, or two or more oligomers having different structures may be mixed in advance and surface treated simultaneously.
[0053] <Silane coupling agent> The alkoxy-containing organopolysiloxane composition used in the present invention may contain a silane coupling agent made of an alkoxysilane. By containing a silane coupling agent, the coating property and the reactivity with the silanol groups present on the surface of the glass cloth are improved, which is preferable.
[0054] Examples of the silane coupling agent include methyltrimethoxysilane, methyltriethoxysilane, phenyltrimethoxysilane, phenyltriethoxysilane, hexyltrimethoxysilane, decyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, and N-(vinylbenzyl)-2-aminoethyl-3-aminopropyltriethoxysilane hydrochloride. Vinyltrimethoxysilane and 3-methacryloxypropyltrimethoxysilane are preferred because they have excellent reactivity and adhesion with the unsaturated groups contained in the thermosetting resin, which is the matrix resin.
[0055] The silane coupling agent may be added alone or in any combination of two or more kinds at any ratio. The mixing ratio of the oligomer (alkoxy group-containing organopolysiloxane) to the silane coupling agent is preferably in the range of 0.1 / 99.9 to 99.9 / 0.1, more preferably 1 / 99 to 99 / 1, and further preferably 10 / 90 to 90 / 10, by mass ratio.
[0056] <Solvent> The alkoxy-containing organopolysiloxane composition (oligomer-containing composition) used in the present invention may be diluted with a solvent. The solvent may be either water-based or organic solvent-based, but by using water as the main solvent, the use of organic solvents can be reduced, making it possible to protect the safety of workers and the global environment. In addition, the oligomer is hydrolyzed and its reactivity increases, making it possible to apply the composition uniformly to the surface of the glass cloth, which is preferable.
[0057] In addition to water as a solvent, one, two or more organic solvents may be added in any ratio. Examples of the organic solvent include aliphatic alcohols such as methanol, ethanol, and isopropyl alcohol, aliphatic ketones such as acetone and methyl ethyl ketone, saturated chain aliphatic hydrocarbons such as n-pentane, i-pentane, n-hexane, i-hexane, n-heptane, i-heptane, n-octane, i-octane, 2,2,4-trimethylpentane (isooctane), n-nonane, i-nonane, n-decane, i-decane, and 2,2,4,6,6-pentamethylheptane (isododecane), saturated cyclic aliphatic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, p-menthane, and decahydronaphthalene, and saturated cyclic aliphatic hydrocarbons such as benzyl alcohol, butyl ... Examples of the solvent include aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene; alkyl ethers such as diethyl ether, dipropyl ether, dibutyl ether, dipentyl ether, dihexyl ether, methyl tertiary butyl ether, and butoxyethyl ether; aryl ethers such as anisole and diphenyl ether; and ester compounds such as n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, isoamyl acetate, and ethyl caproate. Among these, aliphatic alcohols such as methanol are preferably used because of their good solubility in water.
[0058] The mixing ratio of the solvent to the alkoxy group-containing organopolysiloxane is preferably in the range of 99.99 / 0.01 to 90 / 10, more preferably 99.95 / 0.05 to 95 / 5, and even more preferably 99.9 / 0.1 to 99 / 1, in terms of mass ratio. A ratio within this range is preferable because it provides good storage stability, coatability, and the like.
[0059] <Other additives> The alkoxy group-containing organopolysiloxane composition used in the present invention may contain added pH adjusters, surfactants, and silazane structure-containing compounds for the purposes of improving storage stability, coatability, and adhesion and adhesiveness to the matrix resin.
[0060] Examples of pH adjusters include hydrochloric acid, acetic acid, ammonia, and sodium hydroxide, with acetic acid and ammonia being preferred from the standpoint of safety and volatility.
[0061] As the surfactant, any of anionic surfactants, cationic surfactants and nonionic surfactants can be used, but nonionic surfactants are preferred in terms of workability, properties, etc. Examples include polyoxyethylene octyl ether, polyoxyethylene second alkyl ether, polyoxyethylene octylphenyl ether, polyoxyethylene nonylphenyl ether, polyoxyethylene phenyl ether, alkylcarbonyloxypolyoxyethylene, aliphatic polyhydric alcohol polyoxyethylene, aliphatic sucrose ester, etc.
[0062] Examples of compounds containing a silazane structure include low molecular weight silazane compounds such as 1,1,3,3-tetramethyldisilazane, hexamethyldisilazane, 1,3-divinyl-1,1,3,3-tetramethyldisilazane, octamethyltrisilazane, 1,1,3,3,5,5-hexamethylcyclotrisilazane, and 1,1,3,3,5,5-trimethyltrivinylcyclotrisilazane.
[0063] The amount of the other components added is preferably 1 to 500 parts by mass, and more preferably 10 to 200 parts by mass, per 100 parts by mass of the alkoxy group-containing organopolysiloxane.
[0064] <Prepreg> The present invention also provides a prepreg (glass cloth-containing prepreg for low dielectric materials) containing the above-mentioned glass cloth for low dielectric materials and a matrix resin impregnated into the glass cloth.
[0065] Such a prepreg has excellent adhesion and bonding between the low dielectric material glass cloth and the matrix resin, and has improved strength, providing a highly reliable printed wiring board with excellent dielectric properties.
[0066] <Matrix resin> The glass cloth surface-treated with the alkoxy group-containing organopolysiloxane composition of the present invention is preferably used for producing a prepreg by impregnating the glass cloth with a matrix resin. In order to produce a prepreg for a high-frequency substrate having excellent dielectric properties, it is preferable that the matrix resin also has excellent dielectric properties.
[0067] The matrix resin in the present invention is impregnated into the above-mentioned glass cloth for low dielectric materials to form a prepreg, and can be either a thermosetting resin or a thermoplastic resin. In particular, a resin having low dielectric properties is preferred, and more preferably one or more resins selected from epoxy resin, silicone resin, polyimide resin, bismaleimide resin, polyphenylene ether resin, and polytetrafluoroethylene resin. The matrix resin may be used alone or in combination of two or more resins.
[0068] Other components may be added to the matrix resin in the present invention in order to accelerate the curing of the resin, increase its strength, etc. Examples of such components include inorganic fillers, flame retardants, additives, and reaction initiators.
[0069] The amount of the other components added is preferably 1 to 900 parts by mass, and more preferably 10 to 500 parts by mass, relative to 100 parts by mass of the matrix resin.
[0070] <Prepreg manufacturing method> The manufacturing method of the prepreg containing the glass cloth for low dielectric materials of the present invention is not particularly limited. A manufacturing method of a general glass cloth-containing substrate, film, prepreg, etc. can be applied. For example, it can be manufactured according to a general method of applying a curable resin composition to glass cloth fibers (coating method).
[0071] Representative coating methods include direct gravure coater, chamber doctor coater, offset gravure coater, single roll kiss coater, reverse kiss coater, bar coater, reverse roll coater, slotter die, air doctor coater, positive rotation roll coater, blade coater, knife coater, impregnation coater, MB coater, and MB reverse coater.
[0072] To improve and ensure the coating property, the matrix resin may be diluted with a solvent. Depending on the solubility property of the matrix resin, the organic solvent may be used alone or in combination of two or more kinds.
[0073] Examples of the organic solvent include aliphatic alcohols such as methanol, ethanol, isopropanol, and n-butanol; aliphatic ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone; glycol ethers such as ethylene glycol and propylene glycol; aliphatic hydrocarbons such as hexane and heptane; aromatic hydrocarbons such as toluene and xylene; and alkyl ethers such as diethyl ether, diisopropyl ether, and dibutyl ether.
[0074] The amount of the matrix resin attached to the glass cloth for low dielectric materials of the present invention is preferably 10 to 80% by mass, more preferably 20 to 70% by mass. Within this range, the amount of the matrix resin attached to the glass cloth for low dielectric materials of the present invention is more appropriate, and there is an effect of improving the adhesion and adhesiveness of the glass cloth to the matrix resin and the strength of the wiring board. If the amount of attachment is 10% by mass or more, when a printed wiring board is produced from the prepreg, the amount of matrix resin attached to the copper foil is not too small, and sufficient peel strength with the copper foil is obtained. In addition, if the amount of attachment is 80% by mass or less, the amount of matrix resin is not too large, and resin flow during pressing is unlikely to occur, which is preferable. The amount of attachment referred to here indicates the mass % of the matrix resin relative to the mass of the entire prepreg.
[0075] Conditions vary depending on the matrix resin used, but an example of a method is to apply, dry, and then heat at 50° C. to 300° C. for 1 minute to 24 hours for curing.
[0076] <Printed wiring board> The present invention also provides a printed wiring board (a printed wiring board containing glass cloth for low dielectric material) that includes the above-mentioned prepreg.
[0077] Such a printed wiring board has excellent dielectric properties and can be suitably used for electronic components having circuits for transmitting electrical signals of 10 GHz or more.
[0078] <Manufacturing method for printed wiring board> The glass cloth-containing printed wiring board for low dielectric materials of the present invention is produced, for example, by heating and curing one or more, preferably 2 to 20, laminated sheets of the above-mentioned glass cloth-containing prepreg. Heat curing conditions include heating at 100 to 250°C for 1 to 600 minutes, and if necessary, applying a pressure of 0.1 to 20 MPa at the same time as heating. EXAMPLES
[0079] The present invention will be specifically described below using examples and comparative examples, but the present invention is not limited to these.
[0080] <Preparation example of alkoxy group-containing organopolysiloxane (oligomer)> Origo-1 to Origo-6, which are organopolysiloxanes containing an alkoxy group, were prepared as follows.
[0081] [Origo-1] As the methyl group-containing oligomer (Origo-1), KC-89R-P (manufactured by Shin-Etsu Chemical Co., Ltd.) was used. The number of silicon atoms in the oligomer was 2.1 on average.
[0082] [Origo-2] As the phenyl group-containing oligomer (Origo-2), KC-103M (manufactured by Shin-Etsu Chemical Co., Ltd.) was used. The number of silicon atoms in the oligomer was 2.5 on average.
[0083] [Origo-3] DC-3055 (manufactured by Dow Corning Corporation) was used as the amino group-containing oligomer (Oligo-3). The average number of silicon atoms in the oligomer was 3.9.
[0084] [Origo-4] 5.4g of 0.01N hydrochloric acid was added dropwise to 34.1g of methyltrimethoxysilane, and the mixture was aged at room temperature for 3 hours, neutralized with sodium bicarbonate, and filtered. Methanol and water were then removed to synthesize a methyl-group-containing oligomer (Origo-4). The number of silicon atoms in the resulting oligomer was 15.2 on average.
[0085] [Origo-5] 49.6g of phenyltrimethoxysilane was dripped with 9.0g of 0.1N hydrochloric acid, then aged at room temperature for 3 hours, neutralized with sodium bicarbonate, and filtered. Methanol and water were then removed to synthesize a phenyl-containing oligomer (Origo-5). The average number of silicon atoms in the resulting oligomer was 12.8.
[0086] [Origo-6] 5.4g of 1.0N hydrochloric acid was added dropwise to 44.8g of 3-aminopropyltrimethoxysilane, and the mixture was aged at room temperature for 3 hours, neutralized with sodium bicarbonate, and then filtered. Methanol and water were then removed to synthesize an amino group-containing oligomer (Origo-6). The number of silicon atoms in the resulting oligomer was 11.4 on average.
[0087] <Matrix resin preparation example> The matrix resin used in producing the prepreg was prepared as follows.
[0088] [Matrix resin (BMI)] 122 parts by mass of toluene was added to 100 parts by mass of a bismaleimide compound (BMI-5000P (manufactured by Designer Molecules Inc.)) to prepare a resin concentration of 45% by mass. Then, 2 parts by mass of dicumyl peroxide was added as a curing catalyst to prepare a matrix resin (BMI).
[0089] [Examples 1 to 6, Comparative Examples 2 to 6] An oligomer-containing composition was prepared so as to obtain a 0.1 mass % solution of an oligomer and a silane coupling agent mixed in the mass % ratio shown in Table 1 (mixed solvent of 95 mass % water + 2 mass % methanol).
[0090] The prepared oligomer-containing composition was applied to a silica glass cloth (thickness: 95 μm, mass per unit area: 93 g / m 2 ) and heated and dried at 100℃ for 10 minutes for surface treatment. This surface-treated glass cloth was impregnated with matrix resin (BMI) and heated and dried at 100℃ for 10 minutes to remove the solvent and produce a prepreg. Next, one sheet of prepreg was heated and cured at 180℃ for 60 minutes under a pressure of 5 MPa using a vacuum press to produce a printed wiring board.
[0091] [Example 7, Comparative Example 7] An oligomer-containing composition was prepared so as to give a 0.1% by mass solution (methanol solvent) of the oligomers mixed in the mass percentages shown in Table 1.
[0092] The prepared oligomer-containing composition was applied to a silica glass cloth (thickness: 95 μm, mass per unit area: 93 g / m 2 ) and heated and dried at 100℃ for 10 minutes for surface treatment. This surface-treated glass cloth was impregnated with matrix resin (BMI) and heated and dried at 100℃ for 10 minutes to remove the solvent and produce a prepreg. Next, one sheet of prepreg was heated and cured at 180℃ for 60 minutes under a pressure of 5 MPa using a vacuum press to produce a printed wiring board.
[0093] [Comparative Example 1] Untreated silica glass cloth (thickness: 95 μm, mass per unit area: 93 g / m 2 ) was impregnated with a matrix resin (BMI) in the same manner as in Examples 1 to 7 and Comparative Examples 2 to 7, and heated and dried at 100°C for 10 minutes to remove the solvent and obtain a prepreg. Next, one sheet of prepreg was heated and cured at 180°C for 60 minutes under a pressure of 5 MPa using a vacuum press to produce a printed wiring board.
[0094] <Solubility> The appearance of the oligomer-containing compositions (alkoxy group-containing organopolysiloxane compositions) prepared in Examples 1 to 6 and Comparative Examples 2 to 7 was visually observed. Colorless and transparent compositions were indicated as ◯, and cloudy or separated compositions were indicated as ×. The results are shown in Table 1.
[0095] <Dielectric properties> The dielectric properties of the printed wiring boards of the examples and comparative examples were measured by the following method.
[0096] A rectangular molded piece of 3 cm x 4 cm with a thickness of 0.15 mm was prepared. A network analyzer (Keysight: E5063-2D5) was connected to a strip line (Keycom Co., Ltd.) to measure the dielectric constant and dielectric loss tangent of the molded piece at a frequency of 10 GHz. The results are shown in Table 1.
[0097] <Tensile strength> The same oligomer-containing composition as in each of the examples and comparative examples was coated with a silica glass cloth (thickness: 31 μm, mass per unit area: 26 g / m 2 The glass cloth was immersed in the above-mentioned solution and then heated and dried at 100°C for 10 minutes for surface treatment. The tensile strength of the glass cloth was measured by the following method.
[0098] The measurements were performed according to the method described in JIS R 3420:2013 (general test method for glass fibers). The results are shown in Table 1.
[0099] <Conventional bending stiffness> The conventional bending stiffness of the glass cloth of each of the Examples and Comparative Examples was measured by the following method.
[0100] Measurement was performed according to the method described in JIS R 3420:2013 (general test method for glass fibers), and the measured value in the warp direction was used. The value of the conventional bending rigidity of the untreated glass cloth (Comparative Example 1) was set to 1, and the value of the conventional bending rigidity of the surface-treated glass cloth was expressed as a multiple. The results are shown in Table 1.
[0101] [Table 1] Cap-1: Methyltrimethoxysilane Cap-2: Phenyltrimethoxysilane Cap-3: 3-aminopropyltrimethoxysilane
[0102] The oligomer-containing compositions containing oligomers composed of an average of 2 to 10 silicon atoms in Examples 1 to 6 are soluble in aqueous solvents and can protect the safety of workers and the global environment, compared to the oligomer-containing compositions containing oligomers composed of an average of 11 or more silicon atoms in Comparative Examples 4 to 6.
[0103] Furthermore, the tensile strength of the glass cloths of Examples 1 to 7, which are glass cloths for low dielectric materials of the present invention, was higher than that of the glass cloth of Comparative Example 1, which was not surface-treated, and the glass cloths of Comparative Examples 2 and 3, which were surface-treated with a silane coupling agent having a silicon atom number of 1. This demonstrates that the glass cloths for low dielectric materials of the present invention provide printed wiring boards with excellent processability and improved strength.
[0104] Furthermore, the dielectric loss tangents at 10 GHz of the printed wiring boards of Examples 1 to 7 made using the glass cloth for low dielectric materials of the present invention were smaller than those of the printed wiring board of Comparative Example 1 made using a glass cloth that had not been surface-treated, and the printed wiring board of Comparative Example 7 made using a glass cloth surface-treated with an oligomer-containing composition containing an oligomer composed of an average of 11.4 silicon atoms. This shows that the glass cloth for low dielectric materials of the present invention has excellent dielectric properties and is suitable for use as a high-frequency printed wiring board.
[0105] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention. [Industrial Applicability]
[0106] The glass cloth for low dielectric materials of the present invention provides prepregs and printed wiring boards which have excellent adhesion and bonding with matrix resins, improved strength, and excellent dielectric properties and are therefore highly reliable. Therefore, the glass cloth can be suitably used as a material for insulating layers and the like of electronic components having circuits for transmitting electrical signals of 10 GHz or more, particularly millimeter waves, for high-speed servers and the like.
Claims
1. A glass cloth for low dielectric materials, the surface of which is treated with an alkoxy group-containing organopolysiloxane composition, the alkoxy group-containing organopolysiloxane contained in the alkoxy group-containing organopolysiloxane composition having an average number of silicon atoms of 2 to 10; A bismaleimide resin impregnated in the glass cloth; A prepreg comprising: It is used for 5G / IoT and high-frequency printed wiring boards. The glass cloth substrate is a glass cloth substrate made of glass having a dielectric loss tangent of 1×10 −4 to 1×10 −2 at 10 GHz, The prepreg is characterized in that the glass is one or more types selected from the group consisting of S glass, T glass, D glass, and silica glass.
2. 2. The prepreg according to claim 1, wherein the alkoxy group-containing organopolysiloxane composition further contains a silane coupling agent made of an alkoxysilane.
3. 3. The prepreg according to claim 1, wherein the alkoxy group-containing organopolysiloxane composition further contains water.
4. A printed wiring board comprising a prepreg according to any one of claims 1 to 3.
Citation Information
Patent Citations
Fiber sheet, method for producing the same, prepreg and laminated sheet
JP2004043984A
Method for producing quartz glass fiber, quartz glass strand, quartz glass yarn and quartz glass cloth
JP2006282401A
Quartz glass cloth
JP2009263824A
Glass cloth, method for producing prepreg, the prepreg and laminated plate
JP2011017113A
Resin composition, fiber sizing agent and molded article
JP2014047283A