Dielectric composition and electronic component

A dielectric composition with strontium and tantalum as main components, free of titanium and niobium, addresses the challenge of maintaining high dielectric constant and resistivity over a wide temperature range, achieving stable capacitance and low loss.

JP7569695B2Active Publication Date: 2024-10-18TDK CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2021007206
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-20
Publication Date
2024-10-18
Estimated Expiration
2041-01-20

AI Technical Summary

Technical Problem

Existing dielectric compositions do not exhibit a high dielectric constant over a wide temperature range, and often contain titanium, niobium, alkali metals, and lead, leading to issues such as oxygen defects, composition deviation, and contamination.

Method used

A dielectric composition comprising strontium and tantalum as main components, with optional barium, and being substantially free of titanium, niobium, and lead, which maintains high resistivity and low dielectric loss over a wide temperature range.

Benefits of technology

The composition achieves a dielectric constant of 75 or more in a temperature range of -55 to 150°C and -70 to 180°C, with a capacitance change rate within ±22%, and exhibits high density, high relative permittivity, and low dielectric loss.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569695000005
    Figure 0007569695000005
  • Figure 0007569695000006
    Figure 0007569695000006
  • Figure 0007569695000007
    Figure 0007569695000007
Patent Text Reader

Abstract

To provide a dielectric composition having high relative permittivity in a wide range of temperatures.SOLUTION: A dielectric composition includes strontium and tantalum as the main components.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a dielectric composition and an electronic component. [Background technology]

[0002] In recent years, in the field of electronic components for in-vehicle applications, etc., there has been a demand for dielectric compositions that exhibit a high relative dielectric constant over a wide temperature range. Summary of the Invention [Problem to be solved by the invention]

[0003] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a novel dielectric composition having a high relative dielectric constant over a wide temperature range. [Means for solving the problem]

[0004] The dielectric composition according to the present invention contains strontium and tantalum as main components.

[0005] The dielectric composition according to the present invention can exhibit a high relative dielectric constant over a wide temperature range.

[0006] It is further preferable that the main component is barium.

[0007] The dielectric composition according to the present invention is preferably substantially free of titanium, niobium, alkali metals and lead.

[0008] Dielectric compositions that exhibit a high dielectric constant include BaTiO3, which is mainly composed of titanium (Ti), (Sr,Ba)Nb2O6, which is mainly composed of niobium (Nb), (Na,K)NbO3, which contains alkali metals, and Pb(Zr,Ti)O3, which contains Pb.

[0009] The dielectric composition according to the present invention is substantially free of titanium and niobium, and therefore oxygen defects are unlikely to occur. In other words, the change in valence is suppressed. Therefore, even if the dielectric composition is simultaneously fired with a base metal and subjected to reduction firing, the valence is unlikely to change, the decrease in resistivity is suppressed, and it is believed that the dielectric composition can exhibit high resistivity over a wide temperature range. Also, for the same reason, it is believed that the dielectric composition can exhibit low dielectric loss.

[0010] Furthermore, since the dielectric composition according to the present invention is substantially free of alkali metals, it is possible to prevent deviation in composition of the dielectric composition and contamination of the furnace due to evaporation of alkali metals.

[0011] Furthermore, although the use of lead is restricted by the RoHS (Restriction of Hazardous Substances Directive) and the like, the dielectric composition according to the present invention is substantially free of lead.

[0012] The main component is {Ba x Sr (1-x)} m Ta4O 12 where x is preferably 0.75 or less, which leads to a higher relative dielectric constant, higher density and resistivity, and lower dielectric loss.

[0013] It is more preferable that x is 0.1 to 0.75, which further increases the relative dielectric constant.

[0014] It is preferable that m is 1.9 to 2.1, which leads to a higher relative dielectric constant, higher density and resistivity, and lower dielectric loss.

[0015] The crystal system of the main component is preferably a tetragonal system.

[0016] Moreover, an electronic device according to the present invention includes the above-mentioned dielectric composition. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a schematic cross-sectional view of a multilayer ceramic capacitor according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a thin film capacitor according to one embodiment of the present invention. [Diagram 3] FIG. 3 is a graph showing the relationship between the measurement temperature and the relative dielectric constant of Samples Nos. 1 to 5. [Figure 4] FIG. 4 is a graph showing the relationship between density and relative dielectric constant of a dielectric composition. [Diagram 5] FIG. 5 is a graph showing the relationship between density and dielectric loss of a dielectric composition. [Figure 6] FIG. 6 is a graph showing the relationship between density and resistivity of a dielectric composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] [ First embodiment ] < Multilayer Ceramic Capacitors > FIG. 1 shows a multilayer ceramic capacitor 1 as an example of an electronic component according to this embodiment. The multilayer ceramic capacitor 1 has an element body 10 in which dielectric layers 2 and internal electrode layers 3 are alternately laminated. A pair of external electrodes 4 are formed on both ends of the element body 10, and are electrically connected to the internal electrode layers 3 arranged alternately inside the element body 10. There is no particular restriction on the shape of the element body 10, but it is usually a rectangular parallelepiped. There is also no particular restriction on the dimensions of the element body 10, and the dimensions may be appropriate depending on the application.

[0019] < Dielectric Layer > The dielectric layer 2 is made of a dielectric composition according to the present embodiment, which will be described later.

[0020] The thickness per layer of the dielectric layer 2 (interlayer thickness) is not particularly limited and can be set according to the desired characteristics, applications, etc. In general, the interlayer thickness is preferably 30 μm or less, more preferably 15 μm or less, and further preferably 10 μm or less.

[0021] < internal electrode layer > In this embodiment, the internal electrode layers 3 are laminated so that their ends are alternately exposed on the surfaces of two opposing end faces of the element body 10.

[0022] The conductive material contained in the internal electrode layer 3 is not particularly limited. Examples of precious metals used as conductive materials include palladium (Pd), platinum (Pt), and silver (Ag)-Pd alloys. Examples of base metals used as conductive materials include nickel (Ni), Ni-based alloys, copper (Cu), and Cu-based alloys. Note that Ni, Ni-based alloys, Cu, or Cu-based alloys may contain various trace components such as phosphorus (P) and / or sulfur (S) at about 0.1 mass% or less. The internal electrode layer 3 may be formed using a commercially available electrode paste. The thickness of the internal electrode layer 3 may be appropriately determined depending on the application, etc.

[0023] < external electrode > There is no particular limitation on the conductive material contained in the external electrodes 4. For example, known conductive materials such as nickel (Ni), copper (Cu), tin (Sn), Ag, Pd, Pt, gold (Au), or alloys of these, conductive resins, etc. may be used. The thickness of the external electrodes 4 may be appropriately determined depending on the application, etc.

[0024] < Dielectric Composition > The dielectric composition constituting the dielectric layer 2 according to the present embodiment contains strontium (Sr) and tantalum (Ta) as main components. The dielectric composition according to the present embodiment preferably further contains barium (Ba) as a main component.

[0025] The main component of the dielectric composition according to this embodiment is {Ba x Sr (1-x)} m Ta4O 12 It is expressed as:

[0026] x is preferably 0.75 or less, and more preferably 0.1 to 0.75.

[0027] m is preferably from 1.8 to 2.2, and more preferably from 1.9 to 2.1.

[0028] The crystal system of the main component of the dielectric composition according to this embodiment is not particularly limited, but is preferably a tetragonal or orthorhombic system, and more preferably a tetragonal system.

[0029] The main component is a component that occupies 80 to 100 parts by mol, and preferably 90 to 100 parts by mol, when the elements other than oxygen contained in the dielectric composition are taken as 100 parts by mol.

[0030] Furthermore, the dielectric composition according to this embodiment is substantially free of titanium (Ti), niobium (Nb), alkali metals, and lead (Pb). "Substantially free of titanium, niobium, alkali metals, and lead" means that the total amount of "titanium, niobium, alkali metals, and lead" is 10 molar parts or less, and preferably 5 molar parts or less, when the elements other than oxygen contained in the dielectric composition are taken as 100 molar parts.

[0031] The dielectric composition according to this embodiment may contain vanadium (V), aluminum (Al), magnesium (Mg), silicon (Si), calcium (Ca), manganese (Mn), chromium (Cr), rare earth elements, etc. as accessory components.

[0032] The density of the dielectric composition according to this embodiment is 5.72 g / cm 3 It is preferable that the content is 5.75 to 7.85 g / cm or more. 3 It is more preferable that the density of the dielectric composition is within the above range. The method for adjusting the density of the dielectric composition to the above range is not particularly limited, and examples thereof include a method of adjusting the firing temperature of the dielectric composition, a method of adjusting the particle size of the calcined powder, and a method of adding a sintering aid. In order to adjust the density to the above range, it is preferable that the firing temperature is 1380 to 1600°C.

[0033] < Manufacturing method of multilayer ceramic capacitor> Next, an example of a method for manufacturing the multilayer ceramic capacitor 1 shown in FIG. 1 will be described.

[0034] In this embodiment, a calcined powder of the main components constituting the dielectric composition is prepared. The raw materials of the elements constituting the main components are not particularly limited, and oxides of the respective elements can be used. In addition, various compounds that can obtain oxides of the respective elements by firing can be used.

[0035] After weighing out the raw materials of the main components in a predetermined ratio, wet mixing is performed for a predetermined time using a ball mill or the like. After drying the mixed powder, heat treatment is performed in the range of 700 to 1300°C in the atmosphere to obtain calcined powder of the main components. The calcined powder may also be pulverized for a predetermined time using a ball mill or the like.

[0036] Next, a paste for producing a green chip is prepared. The calcined powder of the main component is kneaded with a solvent to form a paste, and a dielectric layer paste is prepared. Known binders and solvents may be used.

[0037] The dielectric layer paste may contain additives such as a plasticizer and a dispersant, if necessary.

[0038] The internal electrode layer paste is obtained by kneading the above-mentioned conductive material, a binder, and a solvent. The binder and the solvent may be known. The internal electrode layer paste may contain additives such as a co-material and a plasticizer as necessary.

[0039] The external electrode paste can be prepared in the same manner as the internal electrode layer paste.

[0040] Using each of the obtained pastes, green sheets and internal electrode patterns are formed, and these are laminated to obtain a green chip.

[0041] The obtained green chip is subjected to a binder removal treatment as necessary. The binder removal treatment conditions are, for example, a holding temperature of preferably 200 to 350°C.

[0042] After the binder removal process, the green chip is fired to obtain the element body 10. In this embodiment, the atmosphere during firing is not particularly limited, and may be air or a reducing atmosphere. In this embodiment, the holding temperature during firing is, for example, 1380 to 1600°C.

[0043] After firing, the obtained element body 10 is subjected to a reoxidation treatment (annealing) as necessary. The annealing conditions are preferably, for example, an oxygen partial pressure during annealing higher than that during firing, and a holding temperature of 1150° C. or less.

[0044] The dielectric composition constituting the dielectric layer 2 of the element body 10 obtained as described above is the dielectric composition described above. The end faces of this element body 10 are polished, and an external electrode paste is applied and baked to form the external electrodes 4. Then, if necessary, a coating layer is formed on the surface of the external electrodes 4 by plating or the like.

[0045] In this manner, the multilayer ceramic capacitor 1 according to this embodiment is manufactured.

[0046] According to this embodiment, by containing strontium and tantalum as main components, it is possible to obtain a dielectric composition having a constant and high relative dielectric constant in a wide temperature range. Specifically, according to the dielectric composition of this embodiment, it is possible to exhibit a relative dielectric constant of 75 or more in a temperature range of -55 to 150°C, and a relative dielectric constant of 70 or more in a temperature range of -70 to 180°C.

[0047] Moreover, according to the dielectric composition of this embodiment, the capacitance change rate can be kept within ±22% in the temperature range of −55 to 150° C. with the reference temperature set to 25° C., so that the X8S characteristic can be satisfied. Furthermore, in the temperature range of −70 to 180° C., the capacitance change rate can be kept within ±22% with the reference temperature set to 25° C.

[0048] Furthermore, according to this embodiment, it is possible to obtain a dielectric composition that is substantially free of titanium, niobium, alkali metals and lead, and that exhibits high density, high dielectric constant, low dielectric loss and high resistivity.

[0049] The dielectric composition according to the present embodiment contains tantalum, and is substantially free of niobium and titanium. On the other hand, the conventional dielectric composition does not contain tantalum, and contains niobium and titanium. The dielectric composition according to the present embodiment tends to exhibit a higher resistivity and a lower dielectric loss than the conventional dielectric composition. The reason for this is considered to be that tantalum oxide (Ta2O5) is less likely to cause oxygen defects than niobium oxide (Nb2O5) and titanium oxide (TiO2).

[0050] Dielectric properties are properties that are premised on the fact that the material is an insulator. Therefore, it is required that the dielectric composition has high resistance so that it does not become a semiconductor or a conductor. As described above, tantalum oxide (Ta2O5) is less likely to develop oxygen defects than niobium oxide (Nb2O5) and titanium oxide (TiO2). In other words, the change in valence is controlled. For this reason, it is believed that the decrease in resistivity is suppressed and high resistivity can be exhibited over a wide temperature range. For the same reason, it is believed that low dielectric loss can be exhibited.

[0051] [ Second embodiment ] < Thin Film Capacitor > A schematic diagram of a thin film capacitor 11 according to this embodiment is shown in Fig. 2. In the thin film capacitor 11 shown in Fig. 2, a lower electrode 112 and a dielectric thin film 113 are formed in this order on a substrate 111, and an upper electrode 114 is provided on the surface of the dielectric thin film 113.

[0052] Although there is no particular limitation on the material of the substrate 111, a Si single crystal substrate is easy to obtain and inexpensive to use as the substrate 111. When flexibility is important, Ni foil or Cu foil can also be used as the substrate.

[0053] There is no particular limit to the material of the lower electrode 112 and the upper electrode 114, as long as it functions as an electrode. Examples include Pt, Ag, and Ni. There is no particular limit to the thickness of the lower electrode 112, and it is, for example, 0.01 to 10 μm. There is also no particular limit to the thickness of the upper electrode 114, and it is, for example, 0.01 to 10 μm.

[0054] The composition of the dielectric composition constituting the dielectric thin film 113 according to this embodiment and the crystal system of the main component are the same as those in the first embodiment.

[0055] There is no particular limit to the thickness of the dielectric thin film 113, but it is preferably 10 nm to 1 μm.

[0056] < Manufacturing method of thin film capacitor > Next, a method for manufacturing the thin film capacitor 11 will be described.

[0057] There is no particular limitation on the method for forming the thin film that will ultimately become the dielectric thin film 113. Examples include vacuum deposition, sputtering, PLD (pulsed laser deposition), MO-CVD (metal organic chemical vapor deposition), MOD (metal organic decomposition), sol-gel, and CSD (chemical solution deposition).

[0058] In addition, the raw materials used in film formation may contain minute impurities or secondary components, but this is not a problem as long as the amount does not significantly impair the performance of the thin film. The dielectric thin film 113 according to this embodiment may also contain minute impurities or secondary components to the extent that the performance is not significantly impaired.

[0059] In this embodiment, a film formation method using PLD method will be described.

[0060] First, a Si single crystal substrate is prepared as the substrate 111. Next, SiO2, TiO x Then, Pt is deposited in this order to form the lower electrode 112. There are no particular limitations on the method for forming the lower electrode 112. For example, sputtering or CVD may be used.

[0061] Next, the dielectric thin film 113 is formed by PLD on the lower electrode 112. In order to expose a part of the lower electrode 112, a metal mask may be used to form an area where the thin film is not formed.

[0062] In the PLD method, first, a target containing the constituent elements of the desired dielectric thin film 113 is placed in a film formation chamber. Next, a pulsed laser is irradiated onto the surface of the target. The surface of the target is instantly evaporated by the strong energy of the pulsed laser. The evaporated material is then deposited on a substrate placed opposite the target to form the dielectric thin film 113.

[0063] There is no particular limitation on the type of target, and in addition to a metal oxide sintered body containing the constituent elements of the dielectric thin film 113 to be produced, an alloy or the like can be used. In addition, it is preferable that each element is distributed evenly in the target, but the distribution may vary within a range that does not affect the quality of the obtained dielectric thin film 113.

[0064] The number of targets does not necessarily have to be one, and it is also possible to prepare and use a plurality of targets for film formation, each containing some of the constituent elements of the dielectric thin film 113. There is also no limitation on the shape of the target, and it is sufficient if the shape is suitable for the film formation apparatus to be used.

[0065] In addition, in the PLD method, it is preferable to heat the substrate 111 with an infrared laser during film formation in order to crystallize the dielectric thin film 113 to be formed. The heating temperature of the substrate 111 varies depending on the constituent elements and composition of the dielectric thin film 113 and the substrate 111, but the film is formed by heating to, for example, 600 to 800° C. By keeping the temperature of the substrate 111 at an appropriate temperature, the dielectric thin film 113 is easily crystallized and cracks that occur during cooling can be prevented.

[0066] Finally, the thin film capacitor 11 can be manufactured by forming the upper electrode 114 on the dielectric thin film 113. There is no particular limit to the material of the upper electrode 114, and Ag, Au, Cu, etc. can be used. There is also no particular limit to the method of forming the upper electrode 114. For example, it can be formed by vapor deposition or sputtering.

[0067] Although the embodiments of the present invention have been described above, the present invention is not limited to these embodiments, and it is of course possible to implement the present invention in various different forms without departing from the spirit of the present invention.

[0068] In the above-described embodiment, the electronic component according to the present invention has been described as a multilayer ceramic capacitor or a thin film capacitor, but the electronic component according to the present invention is not limited to a multilayer ceramic capacitor or a thin film capacitor, and may be any electronic component having the above-described dielectric composition.

[0069] For example, it may be a single-plate type ceramic capacitor in which a pair of electrodes is formed on a single-layer dielectric substrate made of the above-mentioned dielectric composition.

[0070] Moreover, the electronic component according to the present invention may be a filter, a diplexer, a resonator, an oscillator, an antenna, or the like in addition to a capacitor. EXAMPLES

[0071] The present invention will be described in more detail below using examples and comparative examples, although the present invention is not limited to the following examples.

[0072] [ Experiment 1 ] < Sample No. 1-5 > For samples 1 to 5, starting materials for the dielectric compositions were prepared that would become the components shown in Table 1 when fired. The prepared starting materials (powders) were weighed out so as to obtain the metal element ratios in the composition formulas shown in Table 1.

[0073] Next, the weighed powders were wet-mixed in a ball mill using ion-exchanged water as a dispersion medium, and the mixture was dried to obtain a mixed raw material powder. The mixed raw material powder was then heat-treated in air at a holding temperature of 900°C for a holding time of 2 hours to obtain a calcined powder of the main components.

[0074] The obtained calcined powder of the main component was wet-pulverized in a ball mill using ion-exchanged water as a dispersion medium, and then dried to obtain a dielectric material.

[0075] To 100 parts by mass of the obtained dielectric raw material, 10 parts by mass of an aqueous solution containing 6 parts by mass of polyvinyl alcohol resin as a binder was added and granulated to obtain a granulated powder.

[0076] The obtained granulated powder was put into a φ12 mm die and subjected to a pressure of 0.6 ton / cm 2 The material is then pre-press molded at a pressure of 1.2 ton / cm. 2 The mixture was pressed at a pressure of 1000 MPa to obtain a disk-shaped green compact.

[0077] Next, the obtained green molded body was subjected to a binder removal treatment, sintering and annealing under the following conditions to obtain an element body.

[0078] The binder removal treatment conditions were as follows: holding temperature: 400° C., temperature holding time: 2 hours, atmosphere: air.

[0079] The firing conditions were: holding temperature: 1425-1500°C, temperature holding time: 2 hours, atmosphere: humidified N2+H2 mixed gas (oxygen partial pressure 10 -12 A wetter was used to humidify the atmospheric gas during firing.

[0080] The annealing conditions were: holding temperature: 1050°C, temperature holding time: 2 hours, atmospheric gas: humidified N2 gas (oxygen partial pressure: 10 -7 A wetter was used to moisten the atmospheric gas during annealing.

[0081] The dielectric constant, dielectric loss (tan δ), density, resistivity and crystal system of the obtained sintered body (dielectric composition) were examined by the following methods. In order to measure the dielectric constant, dielectric loss and resistivity, an In-Ga electrode was applied to the above-mentioned dielectric composition (sintered body) to obtain a disk-shaped ceramic capacitor sample (capacitor sample).

[0082] < Dielectric constant and dielectric loss (tan δ) > A signal with a frequency of 1 kHz and an input signal level (measurement voltage) of 1 Vrms was input to the capacitor sample at room temperature (20°C) using a digital LCR meter (YHP 4284A) to measure the capacitance C and tan δ. The relative dielectric constant was calculated based on the thickness of the sintered body, the effective electrode area, and the capacitance C obtained as a result of the measurement. The results are shown in Table 1.

[0083] Moreover, the relative dielectric constant was measured at intervals of 10° C. in the temperature range of −70 to 180° C. The results are shown in FIG.

[0084] < density > The density of the dielectric composition was measured as follows. First, the volume V of the dielectric composition was calculated. Next, the mass m of the disk-shaped dielectric composition was measured, and the density of the dielectric composition was obtained by calculating m / V. The results are shown in Table 1.

[0085] < resistivity > The insulation resistance of the capacitor sample was measured at a reference temperature (25°C) using a digital resistance meter (R8340 manufactured by ADVANTEST Co., Ltd.). The resistivity was calculated from the obtained insulation resistance, the effective electrode area, and the thickness of the dielectric composition. The results are shown in Table 1.

[0086] [Table 1]

[0087] Sample numbers 1 to 5 are oxides belonging to the polar point group. As shown in Fig. 3, sample number 1, which contains barium, strontium, and tantalum as main components, has a relative dielectric constant of 100 or more in a wide measurement temperature range (-70 to 180°C), which is higher than the relative dielectric constant of other oxides (sample numbers 2 to 5).

[0088] 3, sample No. 1 satisfies the X8S characteristics because the capacitance change rate is within ±22% when the reference temperature is 25° C. in the temperature range of −55 to 150° C. Furthermore, the capacitance change rate is within ±22% when the reference temperature is 25° C. in the temperature range of −70 to 180° C.

[0089] From Table 1, it was confirmed that sample No. 1, which contains barium, strontium and tantalum as its main components, has a high density, a high relative dielectric constant, a low dielectric loss and a high resistivity compared to the other oxides (sample Nos. 2 to 5).

[0090] [ Experiment 2 ] < Sample numbers 21-26, 31-34 > In sample numbers 21 to 26 and 31 to 34, the components and amounts of the starting materials for the dielectric composition were as follows, and the sintering temperature was set to 1550°C. Except for this, the dielectric compositions were obtained in the same manner as in experiment 1, and the density, dielectric constant, dielectric loss and resistivity were examined. The crystal system was also examined by the following method. The results are shown in Tables 2 and 3. It was confirmed that in all cases of sample numbers 21 to 26 and 31 to 34, the dielectric constant was 70 or more in the temperature range of -70 to 180°C.

[0091] That is, in Experiment 2, powders of barium carbonate (BaCO3), strontium carbonate (SrCO3) and tantalum oxide (Ta2O5) were prepared as starting materials for the dielectric composition. x Sr (1-x)} m Ta4O 12 The prepared starting materials were weighed out so that the composition represented by the formula (I) was as shown in Table 2 or Table 3.

[0092] < Crystal System > The obtained dielectric composition was subjected to electron diffraction, and the crystal system was analyzed by analyzing the electron diffraction pattern.

[0093] [Table 2]

[0094] [Table 3]

[0095] From Tables 2 and 3, it was confirmed that sample number 26 containing strontium and tantalum as main components, and sample numbers 21 to 25 and 31 to 34 containing barium, strontium and tantalum as main components, had high relative dielectric constants.

[0096] From Table 2, it was confirmed that when x was 0.75 or less (sample numbers 22 to 26), higher density, higher relative dielectric constant, lower dielectric loss and higher resistivity were exhibited than when x was 0.80 (sample number 21).

[0097] From Table 2, it was confirmed that when x was 0.10 to 0.75 (sample numbers 22 to 25), a higher relative dielectric constant was exhibited compared to when x was 0.80 (sample number 21) or when x was 0.00 (sample number 26).

[0098] From Table 3, it was confirmed that when m was 1.9 to 2.1 (sample numbers 32, 24, and 33), the samples exhibited higher density, higher dielectric constant, lower dielectric loss, and higher resistivity than when m was 1.8 (sample number 31) or 2.2 (sample number 34).

[0099] [ Experiment 3 ] < Sample No. 41~45 > For sample numbers 41 to 45, the density, relative dielectric constant, dielectric loss and resistivity of the dielectric composition (sintered body) were measured in the same manner as for sample number 1, except that the firing temperature for each sample was changed within the range of 1375 to 1500° C. The results are shown in Table 4 and Figures 4 to 6.

[0100] [Table 4]

[0101] From Table 4 and Figs. 4 to 6, it was confirmed that when the density exceeds 5.74 (sample numbers 1, 42 to 45), the dielectric loss is lower and the resistivity is higher than when the density is 5.74 (sample number 41). [Explanation of symbols]

[0102] 1. Multilayer ceramic capacitor 10... Element body 2... Dielectric layer 3… Internal electrode layer 4… External electrode 11... Thin film capacitor 111... Circuit board 112… Lower electrode 113... Polycrystalline dielectric thin film 114...Top electrode

Claims

1. The main component is represented by {BaxSr(1-x)}mTa4O12, x is 0.1 to 0.75; m is 1.9 to 2.1; A dielectric composition having a relative dielectric constant of 100 or more.

2. 10. The dielectric composition of claim 1, which is substantially free of titanium, niobium, alkali metals and lead.

3. 3. The dielectric composition according to claim 1, wherein x is 0.1 or more and less than 0.

5.

4. 4. The dielectric composition according to claim 3, wherein x is 0.1 or more and 0.25 or less.

5. 5. The dielectric composition according to claim 1, wherein the crystal system of the main component is a tetragonal system.

6. An electronic component comprising the dielectric composition according to any one of claims 1 to 5.

Citation Information

Patent Citations

  • Preparation method of square crystalloid double perovskite Ba2-xSrxSmTaO6 ceramic material

    CN108395215A

  • Dielectric ceramic composition for high frequence

    JP1983045167A

  • Manufacture of dielectric thin film

    JP1988000905A

  • Manufacture of thin film electric field light emission device

    JP1988000994A

  • Dielectric ceramics

    JP1988037508A