Metal oxynitride thin film and capacitor element

A metal oxynitride thin film with specific compositions and structural regions addresses the challenge of achieving high Curie temperature and dielectric constant, providing ferroelectricity with low dielectric loss.

JP7569698B2Active Publication Date: 2024-10-18TDK CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021010987
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-01-31
Filing Date
2021-01-27
Publication Date
2024-10-18
Estimated Expiration
2041-01-27

AI Technical Summary

Technical Problem

Existing dielectric materials face challenges in achieving high Curie temperature (Tc) and dielectric constant simultaneously, with methods for orienting nitrogen atoms in the c-axis direction requiring additional steps or being unsuitable for industrial use, and existing oxynitrides having high dielectric loss.

Method used

A metal oxynitride thin film with a perovskite structure is developed, comprising specific compositions of barium, strontium, lanthanum, tantalum, and titanium, exhibiting regions of centrosymmetric and non-centrosymmetric diffraction, allowing for ferroelectricity with low dielectric loss.

Benefits of technology

The metal oxynitride thin film achieves ferroelectricity with reduced dielectric loss, suitable for applications requiring high dielectric properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569698000002
    Figure 0007569698000002
  • Figure 0007569698000003
    Figure 0007569698000003
  • Figure 0007569698000004
    Figure 0007569698000004
Patent Text Reader

Abstract

To provide a metal oxynitride thin film having a ferroelectricity and a small dielectric loss.SOLUTION: A metal oxynitride thin film containing a metal oxynitride expressed by a general equation of ABOxNy where 2.000≤x≤3.275,0.150≤y≤1.000, A is one or more selected from Ba, Sr, and La, and B is Ta and / or Ti. Assuming that an ionic valence of A is a when A occupies an A-site of a perovskite structure, and an ionic valence of B is b when B occupies a B site of the perovskite structure, 6.7≤a+b≤7.3. The metal oxynitride has an area where a diffraction showing a center symmetry is generated and an area where a diffraction showing a non-center symmetry is generated.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a metal oxynitride thin film and a capacitor element. [Background technology]

[0002] As digital devices become more sophisticated, the dielectrics that make up electronic components that utilize dielectric properties are required to have a high Curie temperature (Tc) and a high dielectric constant. However, it is difficult to achieve both at the same time. For example, barium titanate, which has excellent dielectric properties, has a low Tc because it uses a structural phase transition to achieve its high dielectric constant.

[0003] Metal oxynitrides with a perovskite structure, represented as ABO2N, have attracted attention as dielectric materials, and exhibit high Tc due to their crystal structure. However, although various proposals have been made regarding the mechanism by which the dielectric properties of these metal oxynitrides are expressed, the mechanism has not been clarified.

[0004] For example, Patent Document 1 describes a tetragonal perovskite oxynitride in which nitrogen atoms are oriented in the c-axis direction. Patent Document 1 describes that the orientation of nitrogen atoms in the c-axis direction causes the tetragonal perovskite oxynitride to exhibit ferroelectricity and have good piezoelectric properties.

[0005] Furthermore, Non-Patent Document 1 describes a method in which nitrogen atoms are oriented in the c-axis direction by epitaxially growing an oxynitride thin film on a substrate, utilizing lattice mismatch with the substrate.

[0006] Moreover, Patent Document 2 describes a dielectric ceramic composition having a main composition of a perovskite-type oxynitride and a polycrystalline body exhibiting ferroelectricity. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2010-143788 A [Patent Document 2] International Publication No. 2017 / 135298 [Non-patent literature]

[0008] [Non-Patent Document 1] Daichi Oka, et al., "Possible ferroelectricity in perovskite oxynitride SrTaO2N epitaxial thin films", SCIENTIFIC REPORTS 4, DOI: 10.1038 / srep04987 Summary of the Invention [Problem to be solved by the invention]

[0009] However, in order to orient the nitrogen atoms in the c-axis direction, Patent Document 1 requires an orientation process for orienting the anisotropic-shaped particles. That is, an extra process is required. In addition, the method described in Non-Patent Document 1 is a special method and is not suitable for industrial use. The oxynitride described in Patent Document 2 is composed of a ferroelectric material, and has a problem of high dielectric loss.

[0010] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a metal oxynitride thin film that has ferroelectricity and small dielectric loss. [Means for solving the problem]

[0011] The inventors have discovered that a metal oxynitride having a region that produces centrosymmetric diffraction and a region that produces non-centrosymmetric diffraction can be obtained, which has ferroelectricity as a whole metal oxynitride while having small dielectric loss due to its paraelectric structure.

[0012] In order to achieve the above object, the present invention is embodied as follows.

[0013] [1] General formula ABO x N y A metal oxynitride thin film comprising a metal oxynitride having a perovskite structure, A is at least one selected from the group consisting of barium, strontium, and lanthanum, and B is at least one selected from the group consisting of tantalum and titanium; When the ionic valence indicated when A occupies the A site in the perovskite structure is a and the ionic valence indicated when B occupies the B site in the perovskite structure is b, a and b satisfy the relationship 6.7≦a+b≦7.3; In the general formula, x and y are 2.000≦x≦3.275, The relationship 0.150≦y≦1.000 is satisfied, The metal oxynitride is a metal oxynitride thin film that has regions that produce centrosymmetric diffraction and regions that produce non-centrosymmetric diffraction.

[0014] [2] In the X-ray diffraction pattern obtained by powder X-ray diffraction using Cu-Kα radiation as an X-ray source or by powder X-ray diffraction simulation for a perovskite metal oxynitride consisting only of regions that produce centrosymmetric diffraction and having the same composition as the metal oxynitride thin film, the strongest diffraction peak among the diffraction peaks that appear within the diffraction angle 2θ range of 20° to 25° and that belong to the perovskite structure is defined as P1, the strongest diffraction peak among the diffraction peaks that appear within the diffraction angle 2θ range of 44° to 50° and that belong to the perovskite structure is defined as P2, and the intensity ratio of P1 to the intensity of P2 is defined as IR. r In the X-ray diffraction pattern of a metal oxynitride thin film obtained by perpendicular X-ray diffraction and in-plane X-ray diffraction using Cu-Kα radiation as an X-ray source, the intensity ratio of P1 to the intensity of P2 is defined as IR. r The metal oxynitride thin film according to [1], wherein a ratio A of IR to IR is 0% or more and 80% or less, and the metal oxynitride thin film has remanent polarization.

[0015] [3] The metal oxynitride thin film according to [1] or [2], wherein the region exhibiting centrosymmetric diffraction and the region exhibiting non-centrosymmetric diffraction have different ranges of anion configuration order.

[0016] [4] The metal oxynitride thin film according to [3], wherein the region exhibiting centrosymmetric diffraction and the region exhibiting non-centrosymmetric diffraction have the same cation.

[0017] [5] x and y are 2.450≦x≦3.275, The metal oxynitride thin film according to any one of [1] to [4], which satisfies the relationship 0.150≦y≦0.700.

[0018] [6] A capacitive element comprising the metal oxynitride thin film according to any one of [1] to [5]. Effect of the Invention

[0019] According to the present invention, it is possible to provide a metal oxynitride thin film that has ferroelectricity and small dielectric loss. [Brief description of the drawings]

[0020] [Figure 1] FIG. 1 is a schematic cross-sectional view of a thin film capacitor as an example of a capacitive element according to this embodiment. [Diagram 2] FIG. 2 is a perspective view showing the crystal structure of ABO2N. [Figure 3A] FIG. 3A is a schematic diagram showing a BO4N2 octahedron in which the nitrogen in ABO2N is in the cis configuration. [Figure 3B] FIG. 3B is a schematic diagram showing a BO4N2 octahedron in which the nitrogen in ABO2N is in the trans configuration. [Figure 4] FIG. 4 is a schematic diagram showing that BO4N2 octahedra in which nitrogen is in a cis configuration form octahedral chains in the c-axis direction. [Diagram 5] FIG. 5 is a schematic diagram showing the polarization treatment pattern performed on the sample of the example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will now be described in detail based on specific embodiments in the following order. 1. Thin film capacitor 1.1. Overall structure of thin film capacitor 1.2. Metal oxynitride thin film 1.2.1. Metal oxynitrides 2. Manufacturing method of thin film capacitor 2.1.Method of manufacturing metal oxynitride thin films 3. Summary of this embodiment

[0022] (1. Thin film capacitor) In this embodiment, a thin film capacitor having the metal oxynitride thin film according to this embodiment as a dielectric is described as an example of a capacitive element. Examples of capacitive elements other than thin film capacitors include thermistors, filters, diplexers, resonators, oscillators, antennas, piezoelectric elements, transistor gate materials, ferroelectric memories, etc.

[0023] (1.1. Overall structure of thin film capacitor) As shown in FIG. 1, a thin film capacitor 1 as an example of a capacitive element according to this embodiment has a configuration in which a substrate 51, a first electrode 52, a metal oxynitride thin film 53, and a second electrode 54 are laminated in this order.

[0024] The first electrode 52, the metal oxynitride thin film 53, and the second electrode 54 form a capacitor portion. When the first electrode 52 and the second electrode 54 are connected to an external circuit (not shown) and a voltage is applied, the metal oxynitride thin film 53, which is a dielectric, exhibits a predetermined capacitance and can function as a capacitor.

[0025] 1 is not particularly limited as long as it is made of a material that can suitably form the first electrode 52, the metal oxynitride thin film 53, and the second electrode 54 thereon. Examples of such materials include single crystal and amorphous materials, and in this embodiment, it is preferable to use a Si single crystal substrate.

[0026] 1, the first electrode 52 and the second electrode 54 are formed in the form of thin films, sandwiching the metal oxynitride thin film 53. There are no particular limitations on the material constituting the first electrode 52 and the second electrode 54 as long as it is a conductive material. Examples of the material include metals such as platinum (Pt), ruthenium (Ru), rhodium (Rh), palladium (Pd), iridium (Ir), gold (Au), silver (Ag), copper (Cu), and nickel (Ni), and alloys thereof.

[0027] (1.2. Metal oxynitride thin film) As will be described later, the metal oxynitride thin film according to this embodiment is composed of a metal oxynitride having a predetermined composition and a perovskite structure.

[0028] In this embodiment, the metal oxynitride thin film is a thin film formed by a known film formation method. Such a thin film is usually formed by depositing atoms on a substrate, so the metal oxynitride thin film is preferably a metal oxynitride deposited film. Therefore, the metal oxynitride thin film according to this embodiment does not include a fired body (obtained by a solid-phase reaction) obtained by firing a compact formed by molding a dielectric raw material powder.

[0029] The thickness of the metal oxynitride thin film is not particularly limited and can be set arbitrarily depending on the desired characteristics, applications, etc. In this embodiment, the thickness is preferably 10 nm or more and 2 μm or less.

[0030] (1.2.1. Metal oxynitride) The composition of the metal oxynitride constituting the metal oxynitride thin film according to this embodiment is represented by the general formula ABO x N yIn the general formula, x represents the proportion of oxygen in the metal oxynitride, and y represents the proportion of nitrogen in the metal oxynitride.

[0031] In this embodiment, x satisfies the relationship 2.000≦x≦3.275, and y satisfies the relationship 0.150≦y≦1.000. When x and y are within the above ranges, it becomes easy to obtain a metal oxynitride thin film that has ferroelectricity and small dielectric loss.

[0032] x is preferably 2.450 or more, and more preferably 2.750 or more. x is preferably 3.200 or less, and more preferably 2.900 or less.

[0033] Furthermore, y is preferably 0.200 or more, and more preferably 0.400 or more.Y is preferably 0.700 or less, and more preferably 0.500 or less.

[0034] In the general formula, A is at least one selected from the group consisting of barium (Ba), strontium (Sr) and lanthanum (La), and preferably contains at least one selected from the group consisting of barium and strontium. In the formula, B is at least one selected from the group consisting of tantalum (Ta) and titanium (Ti).

[0035] Therefore, the above composition formula ABO x N y (Ba 1-p-q Sr p La q )(Ta 1-r Ti r )O x N y Here, p and q satisfy the relationships 0≦p≦1.0 and 0≦q≦1.0. Also, r satisfies the relationship 0≦r≦1.0. Preferably, the composition formula ABO x N y (Ba 1-p Sr p ) 1-q Laq (Ta 1-r Ti r )O x N y Here, it is preferable that p and q satisfy the relationships 0≦p≦1.0 and 0≦q≦0.30.

[0036] Moreover, the metal oxynitride has a perovskite structure. The perovskite structure is shown in FIG. 2. As shown in FIG. 2, in the perovskite structure, anions (11, 12) occupy six vertices, and octahedra 15 with a B-site atom 13 at the center share the vertices to form a three-dimensional network, with A-site atoms 14 disposed in the gaps of this network. As described above, the A-site atom is at least one selected from the group consisting of barium, strontium, and lanthanum, and the B-site atom is at least one selected from the group consisting of tantalum and titanium.

[0037] In this embodiment, if the ionic valence indicated when A occupies the A site in the perovskite structure is a, and the ionic valence indicated when B occupies the B site in the perovskite structure is b, a and b satisfy the relationship 6.7≦a+b≦7.3.

[0038] The ionic valence a and ionic valence b are each expressed as an average valence. The average valence is a value obtained by averaging the valences of ions present in the A site or B site according to their abundance ratio. For example, a case will be described in which Sr and La are present in the A site at a molar ratio of 4:1. The valence of the Sr ion in the perovskite structure is 2, and the valence of the La ion in the perovskite structure is 3. Therefore, the average valence a of the A site is calculated by the following (Formula 1), and a is 2.2. (Formula 1) (Average valence a in the above case) = 2 (valence of Sr ions) × 4 / 5 (abundance ratio of Sr ions) + 3 (valence of La ions) × 1 / 5 (abundance ratio of La ions) =8 / 5+3 / 5 =11 / 5 =2.2…(1)

[0039] Similarly, we consider the case where Ta and Ti exist in the B site in a molar ratio of 4:1. The valence of the Ta ion in the perovskite structure is 5, and the valence of the Ti ion in the perovskite structure is 4. Therefore, the average valence b of the B site is calculated by the following (Equation 2), and b is 4.8. (Formula 2) (Average valence b in the above case) = 5 (valence of Ta ions) × 4 / 5 (abundance ratio of Ta ions) + 4 (valence of Ti ions) × 1 / 5 (abundance ratio of Ti ions) =20 / 5+4 / 5 =24 / 5=4.8…(2)

[0040] The above average valence is a valence calculated when the molar ratio of the ion present at the A site to the ion present at the B site is 1:1. On the other hand, the average valence may be a valence calculated when the molar ratio of the ion present at the A site to the ion present at the B site is not 1:1.

[0041] For example, if the molar ratio of Sr ions present at the A site to Ta ions present at the B site is 1:1.02, then using the above formulas (1) and (2), a will have a valence of 2 and b will have a valence of 5.1. (average valence a) =2×1=2 (average valence b) =5×1.02=5.1

[0042] When the sum of the average valence a of the A site and the average valence b of the B site satisfies the above range, it becomes easy to obtain a metal oxynitride thin film having ferroelectricity and small dielectric loss.

[0043] On the other hand, the anion is a metal oxynitride ABO x N y The oxygen and nitrogen in the ABO are distributed according to their composition ratio. x N yWhen x=2 and y=1 in the formula (1), the octahedron is a BO4N2 octahedron, in which nitrogen ions 12 occupy two of the six vertices occupied by anions, as shown in FIG.

[0044] In this embodiment, the metal oxynitride has ferroelectricity. Ferroelectricity is a property in which the direction of spontaneous polarization is reversed by an external electric field and the polarization remains even after the external electric field is removed. Spontaneous polarization is a bias in the distribution of electric charges caused by the relative change in the positions of cations and anions in a crystal.

[0045] Therefore, a ferroelectric material has a structure that causes a bias in the charge distribution. For example, barium titanate (BaTiO3), known as a perovskite-type ferroelectric, has a tetragonal crystal structure at room temperature, with the lattice length in the c-axis direction being longer than the lattice lengths in the a-axis and b-axis directions. Therefore, spontaneous polarization occurs in the unit lattice due to an arrangement in which the position of the titanium ion is shifted from the center of gravity of the oxygen ion. This arrangement does not have centrosymmetricity. Whether or not such spontaneous polarization occurs can be evaluated, for example, by whether or not the metal oxynitride exhibits a piezoelectric response.

[0046] On the other hand, a material that loses its polarization when the external electric field is removed is called a paraelectric. At high temperatures, barium titanate transitions to a cubic crystal structure, and the lattice length in the c-axis direction becomes the same as the lattice length in the a-axis and b-axis directions. As a result, barium titanate loses its ferroelectricity and becomes a paraelectric. In other words, the center of gravity of the oxygen ions and the center of gravity of the titanium ions are aligned, and the spontaneous polarization disappears as the structure transitions to one in which there is no bias in the charge distribution. This type of arrangement is a centrosymmetric arrangement.

[0047] Normally, a substance having ferroelectricity has only a region in which a configuration having no centrosymmetric property (a non-centrosymmetric configuration) is repeated in an orderly manner. However, in this embodiment, the metal oxynitride has a region that produces centrosymmetric diffraction and a region that produces non-centrosymmetric diffraction, and can exhibit ferroelectricity due to the region that produces non-centrosymmetric diffraction.

[0048] In this embodiment, both the region that produces centrosymmetric diffraction and the region that produces non-centrosymmetric diffraction are configured with a non-centrosymmetric arrangement. However, the region that produces centrosymmetric diffraction and the region that produces non-centrosymmetric diffraction have different ranges in which the arrangement order of anions (oxygen ions and nitrogen ions) is maintained.

[0049] In the region where the diffraction exhibits centrosymmetric properties, the arrangement of the anions is non-centrosymmetric, but the arrangement is random throughout the crystal grain, and the non-centrosymmetric arrangement is about the size of the unit cell, so that the range affected by the polarization caused by the non-centrosymmetric properties is small. Therefore, since the polarization direction is omnidirectional in the region, the region as a whole does not have a polarization oriented in a specific direction, and can be considered to have centrosymmetric properties. As a result, when the metal oxynitride according to the present embodiment is analyzed by a diffraction method, the region is a region where the diffraction exhibits centrosymmetric properties, and is not detected as a region where the diffraction exhibits non-centrosymmetric properties as a second phase.

[0050] On the other hand, in a region where non-centrosymmetric configurations are arranged in an orderly manner, the configuration order is repeated in a specific direction, and the non-centrosymmetric nature is strengthened in that direction. When such a region has a certain size, the diffraction occurring in this region may affect the centrosymmetric diffraction. As will be described later, when non-centrosymmetric diffraction occurs, the centrosymmetric diffraction is affected, and a diffraction pattern different from the diffraction pattern exhibited by a metal oxynitride composed only of regions where centrosymmetric diffraction occurs is obtained.

[0051] In metal oxynitrides that produce such diffraction patterns, the regions where anions are ordered are large, which serve as the origin of ferroelectricity, while the metal oxynitrides have regions where diffraction occurs with centrosymmetric properties, which reduces dielectric loss.

[0052] In the BO4N2 octahedron, there are two configurations (cis configuration) in which two nitrogen (N) ions 12 are adjacent to each other as shown in Figure 3A, and there are two configurations (trans configuration) in which two nitrogen ions (N) 12 are not adjacent to each other as shown in Figure 3B. Both the cis configuration and the trans configuration are non-centrosymmetric configurations because the bond lengths of the oxygen ions and the nitrogen ions are different.

[0053] In this embodiment, the non-centrosymmetric configuration is preferably a cis configuration. Therefore, the region that produces centrosymmetric diffraction and the region that produces non-centrosymmetric diffraction are preferably configured in a cis configuration.

[0054] In the cis-configured BO4N2 octahedron shown in Figure 3A, nitrogen ions are present in the a-axis and c-axis directions, but the BO4N2 octahedrons with nitrogen ions in the a-axis and b-axis directions and the BO4N2 octahedrons with nitrogen ions in the b-axis and c-axis directions are also cis-configured. Therefore, these BO4N2 octahedra are randomly present and share vertices, weakening the non-centrosymmetric property and forming regions that produce diffraction that shows centrosymmetric properties.

[0055] In contrast, a structure in which the cis configuration exists in an orderly manner is shown in FIG. 4. In FIG. 4, in the cis-configuration ordered structure, nitrogen is arranged at one of the sites (4a) in the c-axis direction and one of the sites (8h) on the plane parallel to the a-axis and b-axis among the vertices of the octahedron. As a result, the BO4N2 octahedra form an octahedral chain in which the octahedra are linked in a state tilted from the axis connecting B (c-axis in FIG. 3). In this embodiment, such an ordered structure formed by linking octahedra in which nitrogen is in the cis configuration affects the diffraction pattern due to the region in which the BO4N2 octahedra exist randomly (the order range of the BO4N2 octahedra is narrow).

[0056] The types of cations in the region producing centrosymmetric diffraction and the region producing non-centrosymmetric diffraction may be the same or different. In this embodiment, it is preferable that the types of cations are the same. By reducing the number of types of elements constituting the metal oxynitride, contamination can be suppressed and the load on the manufacturing process can be reduced.

[0057] In a metal oxynitride, whether or not there is a region that produces centrosymmetric diffraction and a region that produces non-centrosymmetric diffraction can be evaluated, for example, as follows. Such structures determined by the positions of atoms are often evaluated by XRD diffraction. However, as described above, in the above metal oxynitride, whether a region produces centrosymmetric diffraction or a non-centrosymmetric diffraction depends on the difference in the arrangement of anions (oxygen and nitrogen). The intensity of the diffraction peaks reflecting the positions of light elements such as oxygen and nitrogen is weaker than the intensity of the diffraction peaks reflecting the positions of metal elements (A and B), and it is difficult to directly evaluate the diffraction peaks reflecting the positions of light elements.

[0058] However, differences in the arrangement of anions can affect the intensity of diffraction peaks observed by XRD diffraction, so in this embodiment, the presence or absence of regions that produce centrosymmetric diffraction and regions that produce non-centrosymmetric diffraction in the metal oxynitride is evaluated based on the ratio of the intensity of a diffraction peak reflected by a given plane to the intensity of a diffraction peak reflected by another plane.

[0059] First, a measurement result or a simulation result of powder XRD diffraction for a perovskite metal oxynitride composed only of regions that produce diffraction exhibiting centrosymmetricity is obtained. When the X-ray source is Cu-Kα radiation, an intensity ratio IR is calculated from the intensity of the strongest diffraction peak P1 among the diffraction peaks that appear within a diffraction angle 2θ range of 20° to 25° and the intensity of the strongest diffraction peak P2 among the diffraction peaks that appear within a diffraction angle 2θ range of 44° to 50°. r (P1 intensity / P2 intensity) is calculated and used as a reference. XRD diffraction simulation can be performed using known software.

[0060] Next, XRD diffraction measurement is performed on a metal oxynitride having the same composition as the reference to obtain a diffraction peak pattern. In the obtained diffraction peak pattern, the intensity ratio IR (intensity of P1 / intensity of P2) is calculated from the intensity of the diffraction peak P1 and the intensity of the diffraction peak P2, and the ratio A (IR / IR r ) can be used to evaluate whether or not there are regions in the metal oxynitride that produce centrosymmetric diffraction and regions that produce non-centrosymmetric diffraction.

[0061] The intensity ratio of the diffraction peaks also changes depending on the orientation, but since the above intensity ratio IR is not due to orientation, the intensity ratio IR (P1 intensity / P2 intensity) shows the same relationship for diffraction peaks measured from both the out-of-plane direction and the in-plane direction. For example, P1 intensity / P2 intensity < 1 is maintained. On the other hand, when oriented, the relationship is reversed in the out-of-plane direction and the in-plane direction. For example, P1 intensity / P2 intensity > 1 in the out-of-plane direction, while P1 intensity / P2 intensity < 1 in the in-plane direction.

[0062] In this embodiment, when the ratio A is equal to or greater than 0% and equal to or less than 80%, it is determined that the metal oxynitride contains a region that produces centrosymmetric diffraction and a region that produces non-centrosymmetric diffraction.

[0063] It is preferable that the metal oxynitride thin film according to this embodiment is non-oriented. In this embodiment, whether or not the thin film is non-oriented is determined as follows. First, two orthogonal planes are selected in the metal oxynitride crystal. XRD measurements are performed on the metal oxynitride thin film from both in-plane and out-of-plane directions, and the peak with the greater intensity in the in-plane XRD measurement is used as a reference, and the ratio B1 of the smaller peak intensity to the reference peak intensity of 100% (<100% since it is the smaller one) is calculated. Next, in the out-of-plane XRD measurement, the ratio B2 of the other peak intensity to the peak intensity of 100% at the position used as a reference in the in-plane XRD measurement is calculated. Then, if the difference between the two (|B1-B2|) is within 80%, the thin film is determined to be non-oriented.

[0064] As a specific example, if in-plane XRD measurement shows that the peak intensity of the (220) plane is 100% and that of the (002) plane is 80%, while in out-of-plane XRD measurement shows that the peak intensity of the (002) plane is 120% and that of the (220) plane is 100%, then the difference in peak intensity of the (002) plane is 40% (120%-80%). Therefore, in this case, the metal oxynitride thin film is determined to be non-oriented.

[0065] In addition, the positions of light elements can be evaluated by neutron diffraction. In the crystal structure refined by neutron diffraction measurements, when ABO2N is SrTaO2N or (SrLa)TaO2N, it is known that the centrosymmetric structure belongs to the space group I4 / mcm (Table No. 140), and the non-centrosymmetric structure due to the cis-ordered structure belongs to the space group Pmc21 (Table No. 26).

[0066] When ABO2N is BaTaO2N or (BaLa)TaO2N, the structure with centrosymmetric structure belongs to the space group Pm-3m (Table No. 221), and the structure with non-centrosymmetric structure due to the cis-ordered structure belongs to the space group Pmc21 (Table No. 26).

[0067] (2. Manufacturing method of thin film capacitor) Next, an example of a method for manufacturing the thin film capacitor 1 shown in FIG. 1 will be described below.

[0068] First, prepare a substrate 51. When using, for example, a Si single crystal substrate as the substrate 51, an insulating layer (for example, SiO2) is formed on one main surface of the substrate. The insulating layer may be formed by a known film formation method such as a thermal oxidation method or a CVD (Chemical Vapor Deposition) method.

[0069] Next, a thin film of a material constituting the first electrode is formed on the formed insulating layer by a known film formation method, for example, a sputtering method, to form the first electrode 52.

[0070] Next, a metal oxynitride thin film 53 is formed on the first electrode 52 using a known film formation method.

[0071] Examples of known film formation methods include vacuum deposition, sputtering, pulsed laser deposition (PLD), metal-organic chemical vapor deposition (MOCVD), metal organic decomposition (MOD), or the sol-gel method, and chemical solution deposition (CSD).

[0072] Examples of the film-forming raw material include various target materials, deposition materials, organometallic materials, etc. The film-forming raw material may contain a small amount of impurities or subcomponents, but this is not a problem as long as it does not significantly deteriorate the effects of the present invention.

[0073] Among these film formation methods, the well-known vapor phase growth method in which a film formation source material is once separated or excited at an atomic or molecular level and then deposited on a substrate to form a film is preferred. In the following, a method for forming a metal oxynitride thin film using a sputtering method as a vapor phase growth method will be described.

[0074] When forming a metal oxynitride thin film by sputtering, a target having a predetermined composition is used as a film forming raw material. Also, when a part of the A-site atoms of barium and / or strontium is replaced with lanthanum, the perovskite structure is easily distorted. Therefore, by using a target containing a predetermined ratio of lanthanum as the A-site atom, it is easy to reduce the symmetry in a part of the crystal structure and form a region that generates non-centrosymmetric diffraction in a region that generates centrosymmetric diffraction.

[0075] During film formation, it is preferable to heat the substrate in order to crystallize the thin film. The substrate temperature during film formation may be determined according to the constituent elements and composition of the thin film, but in this embodiment, in order to set the intensity ratio within the above range, the substrate temperature is preferably within the range of 500°C to 800°C. If the substrate temperature is too low, the thin film tends not to crystallize, and if the substrate temperature is too high, nitrogen tends to be desorbed.

[0076] In order to keep the intensity ratio within the above range, the high frequency power (applied power) is preferably within the range of 50 W to 300 W. If the high frequency power is too small, the film formation rate tends to decrease significantly. On the other hand, if the high frequency power is too large, the characteristics tend to decrease due to abnormal grain growth.

[0077] When an oxide is used as the target, the atmosphere gas during film formation contains at least oxygen gas and nitrogen gas. By using such an atmosphere gas, the insulating properties of the obtained thin film are ensured, and a thin film as a dielectric is obtained. In this embodiment, in order to set the intensity ratio within the above range, the oxygen gas pressure is preferably in the range of 0.01 Pa or more and 0.1 Pa or less. By setting the oxygen gas pressure within the above range, a decrease in symmetry is easily caused in the crystal, and it becomes easy to set the intensity ratio within the above range. Similarly, the nitrogen gas pressure is preferably in the range of 0.01 Pa or more and 0.1 Pa or less.

[0078] It is also a good idea to introduce an inert gas such as Ar gas separately from the atmospheric gas. Since Ar gas is used to knock atoms out of the target, it is a good idea to introduce the amount necessary to obtain a pressure at which the plasma can be maintained stably. Note that the state at which the plasma can be maintained stably depends on the input voltage and Ar gas pressure, so these can be adjusted according to the size of the chamber and the size of the target.

[0079] In this embodiment, the metal oxynitride may be formed directly on the substrate without passing through a metal oxide thin film, or a metal oxide thin film may be formed and nitrogen may be introduced into the crystal structure of the formed metal oxide thin film to obtain a metal oxynitride thin film. In either case, the nitriding process may be performed by introducing nitrogen radicals into the film formation chamber when forming the metal oxide film, by using reactive sputtering using nitrogen gas or the like, or by using nitrogen activated by plasma nitriding.

[0080] This method is preferable because it is possible to form a metal oxynitride thin film without using toxic gases. It is also possible to use partial oxidation treatment of the metal nitride thin film. In this embodiment, it is preferable to obtain a metal oxynitride by introducing nitrogen for nitridation when forming a film using a metal oxide raw material.

[0081] The metal oxynitride thin film thus obtained is a deposited film that acts as a dielectric.

[0082] Next, in this embodiment, a thin film of a material that constitutes an upper electrode is formed on the formed metal oxynitride thin film 53 by using a known film formation method to form the second electrode 54.

[0083] Through the above steps, a thin film capacitor 1 is obtained in which a capacitor portion (second electrode 52, metal oxynitride thin film 53 and second electrode 54) is formed on a substrate 51, as shown in FIG.

[0084] (3. Summary of the present embodiment) In this embodiment, the metal oxynitride has a region that generates centrosymmetric diffraction and a region that generates non-centrosymmetric diffraction. The region that generates centrosymmetric diffraction is composed of a non-centrosymmetric arrangement, and when viewed microscopically, spontaneous polarization occurs due to the non-centrosymmetric arrangement, but the non-centrosymmetric arrangement exists in a random direction, so the spontaneous polarization that occurs is canceled. As a result, despite being composed of a non-centrosymmetric arrangement, centrosymmetric diffraction occurs. Therefore, since no spontaneous polarization occurs in the entire region, the region is paraelectric.

[0085] On the other hand, the regions where the non-centrosymmetric arrangement is ordered are large enough to generate spontaneous polarization, and in these regions, the spontaneous polarization occurs due to the displacement of two types of anions with different bond lengths. Therefore, these regions are ferroelectric.

[0086] As a result, due to the presence of both regions that produce centrosymmetric diffraction and regions that produce non-centrosymmetric diffraction, the metal oxynitride as a whole exhibits ferroelectricity while having low dielectric loss, making it suitable for applications that utilize ferroelectricity while also providing the low dielectric loss characteristic of paraelectrics.

[0087] In addition, since the polarization due to non-centrosymmetric structure is realized by the displacement of two anions, the distortion of the crystal is smaller than that caused by the displacement of cations, and therefore it is easy to achieve both ferroelectricity and dielectric loss.

[0088] Although the embodiment of the present invention has been described above, the present invention is not limited to the above embodiment, and may be modified in various aspects within the scope of the present invention. EXAMPLES

[0089] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to the following examples.

[0090] (Experiment 1) First, strontium carbonate (SrCO3), barium carbonate (BaCO3), lanthanum oxide (La2O3), titanium oxide (TiO2) and tantalum oxide (Ta2O5) were prepared as target materials for film formation. The prepared materials were weighed to have the compositions shown in Table 1 (Examples 1 to 14 and Comparative Examples 1 to 5). The weighed materials were mixed in a wet ball mill with ethanol as a solvent for 16 hours. The resulting mixed slurry was dried in a thermostatic dryer at 80°C for 12 hours. The resulting mixture was lightly crushed in a mortar, placed in a ceramic crucible and heat-treated in an electric furnace at 1000°C in the air for 2 hours to obtain a calcined product.

[0091] The calcined product was ground in a wet ball mill with ethanol as a solvent for 16 hours, and the ground slurry was dried in a thermostatic dryer at 80°C for 12 hours to obtain a ground product. A polyvinyl alcohol solution was added as a binder to the ground product in an amount of 0.6% by weight (based on the solid content in the solution) and mixed to obtain a granulated product. The granulated product was molded into a cylindrical shape with a diameter of approximately 23 mm and a height of approximately 9 mm to obtain a molded product. The molded product was fired in an electric furnace in an air atmosphere at 1400°C for 2 hours to obtain a sintered body. The top and bottom surfaces of the obtained sintered body were mirror-polished to obtain a film-forming target with a height of 5 mm.

[0092] The film formation target obtained as described above was placed in a film formation apparatus, and then a Si substrate with a Pt film as a first electrode was placed on the surface facing the target. A metal oxynitride thin film was formed to a thickness of 500 nm by sputtering with nitrogen radicals. Ar, N2, and O2 were used as atmospheric gases.

[0093] The film formation conditions were a substrate temperature of 600°C, oxygen gas pressure and nitrogen gas pressure of 0.01 Pa, and plasma applied power of 150 W. For Examples 1 to 14 and Comparative Examples 2 to 5, the total pressure adjusted with Ar was 2 Pa or more, and for Comparative Example 1, the total pressure adjusted with Ar was 1 Pa or less.

[0094] Next, a bulk sample was prepared as follows. First, strontium carbonate (SrCO3) powder and tantalum oxide (Ta2O5) powder were prepared as raw material powders. The prepared powders were weighed so as to obtain a metal oxynitride represented by the composition formula SrTaO2N.

[0095] The weighed SrCO3 powder and Ta2O5 powder were wet mixed with ethanol and calcined twice in air at 1200℃ for 10 hours to obtain an oxide precursor containing Sr and Ta by a solid-phase reaction.

[0096] Next, the obtained oxide precursor was subjected to nitriding treatment twice to obtain a metal oxynitride powder represented by the composition formula SrTaO2N. In the nitriding treatment, the NH3 supply rate was 100 ml / min, the heating temperature was 1000°C, and the heating time was 20 hours.

[0097] The obtained metal oxynitride powder was wet-pulverized in a ball mill for 16 hours and dried. 0.6% by mass of polyvinyl alcohol was added as a binder to 100% by mass of the dried metal oxynitride powder, and the mixture was granulated to obtain a granulated powder. The obtained granulated powder was placed in a mold and press-molded to obtain a molded body.

[0098] The obtained compact was sintered in a N2 atmosphere to obtain a bulk metal oxynitride sintered body. The sintering conditions were a holding temperature of 1400°C and a holding time of 16 hours.

[0099] The obtained metal oxynitride thin film and the metal oxynitride fired body were subjected to XRD measurement by the method described below to obtain X-ray diffraction charts. In the obtained X-ray diffraction charts, the strongest diffraction peak appearing within the 2θ range of 20° to 25° was ABO x N y The strongest diffraction peak, which appears within the 2θ range of 44° to 50°, is the (002) diffraction peak of ABO. x N y The diffraction peak intensity (intensity ratio) of the (002) plane to the diffraction peak intensity of the (220) plane was calculated.

[0100] On the other hand, ABO consists only of structures with centrosymmetric structure. x N y In this example, the intensity (intensity ratio) of the diffraction peak of the (002) plane to the intensity of the diffraction peak of the (220) plane was 20.4 / 21.9=0.93, assuming the intensity of the main peak to be 100. Using this value as the reference (100%), the intensity ratio ratio in each example and comparative example was calculated. In this example, when the intensity ratio ratio was 80% or less, ABO x N y It was determined that there existed regions in the sample that exhibited centrosymmetric diffraction and regions that exhibited non-centrosymmetric diffraction. The results are shown in Table 1.

[0101] In addition, the intensity ratio of the bulk sintered metal oxynitride was 100%. In other words, the bulk sintered metal oxynitride was composed only of structures having centrosymmetrical structures. In addition, sintered metal oxynitride bodies were produced by changing the composition of the metal oxynitride, but the intensity ratio of all samples was 100%.

[0102] Subsequently, the dielectric constant and piezoelectric response of the obtained metal oxynitride thin film were measured by the methods described below.

[0103] (Dielectric constant) The dielectric constant was evaluated as follows. First, Ag was evaporated to a diameter of 100 μm on the metal oxynitride thin film of the obtained sample to form an upper electrode. Next, an AC voltage was applied to the sample on which the upper electrode was formed at a reference temperature of 25° C. and a frequency of 1 kHz so that the electric field strength applied to the sample on which the upper electrode was formed was 0.5 Vrms / μm, and the dielectric constant (unitless) was calculated from the capacitance measured and the thickness of the metal oxynitride thin film as a dielectric. In this example, samples with a dielectric constant of 150 or more were judged to be good. The results are shown in Table 1. This is because, for example, when a crystal equivalent to Sr2Ta2O7, which is outside the target composition, is formed in SrTaO2N, the obtained dielectric constant is about 50, and the dielectric constant does not exceed 100 even in consideration of the variation in sample and composition. If the relative dielectric constant is 100 or more, it can be determined that a crystal similar to SrTaO2N has been formed, and if the relative dielectric constant is 150 or more, it can be determined that a particularly desirable crystal structure has been formed.

[0104] (Piezoelectric response) The piezoelectric response was measured using a piezo-response microscope (PRM), which is one of the modes of AFM.

[0105] A predetermined voltage was applied to the surface of the obtained metal oxynitride thin film to polarize the surface, creating the polarization pattern shown in Figure 5. Specifically, a voltage of -1V was applied to X1 = 10 μm square. Then, or simultaneously, a voltage of +1V was applied to the central X2 = 7 μm square. Then, or simultaneously, a voltage of -1V was applied to the central X3 = 5 μm square. Then, or simultaneously, a voltage of +1V was applied to the central X4 = 3 μm square. Then, or simultaneously, a voltage of -1V was applied to the central X5 = 1 μm square.

[0106] Then, a voltage was applied to the polarization pattern shown in Figure 5 under the conditions of a scanning frequency of 0.5 Hz and an excitation voltage (external AC electric field) of -0.3 V to +0.3 V, and it was evaluated whether or not the displacement due to the remnant polarization could be measured by PRM. If the displacement could be measured, the metal oxynitride had a piezoelectric response. The results are shown in Table 1.

[0107] [Table 1]

[0108] From Table 1, it can be seen that when there are regions that produce centrosymmetric diffraction and regions that produce non-centrosymmetric diffraction and the specified composition and average ionic valence are satisfied, the metal oxynitride thin film as a whole has remanent polarization, i.e., has ferroelectricity. [Explanation of symbols]

[0109] 1. Thin film capacitor 51... Circuit board 52... First electrode 53… Metal oxynitride thin film 54... second electrode 15… Octahedron 11. Oxygen 12. Nitrogen 13... B site atom 14… A-site atom

Claims

1. General formula ABO x N y A metal oxynitride thin film comprising a metal oxynitride having a perovskite structure, A is at least one selected from the group consisting of barium, strontium, and lanthanum, and B is at least one selected from the group consisting of tantalum and titanium, When the ionic valence indicated when A occupies the A site in the perovskite structure is a and the ionic valence indicated when B occupies the B site in the perovskite structure is b, the a and b satisfy the relationship 6.7≦a+b≦7.3, In the general formula, x and y are 2.000≦x≦3.275, The relationship 0.150≦y≦1.000 is satisfied, the metal oxynitride has a region that produces centrosymmetric diffraction and a region that produces non-centrosymmetric diffraction, In an X-ray diffraction pattern obtained by powder X-ray diffraction using Cu-Kα radiation as an X-ray source or powder X-ray diffraction simulation for a perovskite metal oxynitride consisting only of regions producing diffraction exhibiting centrosymmetricity and having the same composition as the metal oxynitride thin film, the strongest diffraction peak among the diffraction peaks appearing within a diffraction angle 2θ range of 20° to 25° and attributed to the perovskite structure is defined as P1, the strongest diffraction peak among the diffraction peaks appearing within a diffraction angle 2θ range of 44° to 50° and attributed to the perovskite structure is defined as P2, and the intensity ratio of P1 to the intensity of P2 is defined as IR r . In an X-ray diffraction pattern of the metal oxynitride thin film obtained by perpendicular X-ray diffraction and in-plane X-ray diffraction using Cu-Kα radiation as an X-ray source, when the intensity ratio of P1 to the intensity of P2 is defined as IR, a ratio A of IR to IR of 0% or more and 80% or less, the metal oxynitride thin film having remanent polarization.

2. 2. The metal oxynitride thin film according to claim 1, wherein the region producing centrosymmetric diffraction and the region producing non-centrosymmetric diffraction have different ranges of ordered arrangement of anions.

3. 3. The metal oxynitride thin film of claim 2, wherein the region exhibiting centrosymmetric diffraction and the region exhibiting non-centrosymmetric diffraction have the same cations.

4. The x and y are 2.450≦x≦3.275, 4. The metal oxynitride thin film according to claim 1, which satisfies the relationship: 0.150≦y≦0.

700.

5. A capacitive element comprising the metal oxynitride thin film according to claim 1 .

Citation Information

Patent Citations

  • Oxynitride piezoelectric material and method for producing the same

    JP2010143788A

  • Piezoelectric material, piezoelectric element, liquid discharging head, ultrasonic motor and dust removal device

    JP2013128073A

  • Polycrystal dielectric thin film and capacitive element

    JP2018174305A

  • Metal oxynitride thin film, method for manufacturing the same, and capacitance element

    JP2019091888A

  • Polycrystalline dielectric thin film and capacitor element

    WO2017135294A1