Coating: Peeling of aluminum-containing coating
The described method uses an aluminum-containing intermediate layer and NaOH solution for selective stripping of AlCrN coatings, addressing non-selectivity and substrate damage issues, enabling efficient and damage-free stripping of complex substrates.
Patent Information
- Application Number
- JP2021509802
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2018-08-21
- Filing Date
- 2019-08-21
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2039-08-21
AI Technical Summary
Existing methods for stripping aluminum-containing coatings, such as AlCrN, using oxidizing agents like KMnO4 are non-selective and can damage the substrate, requiring precise timing and additional masking steps, and are ineffective for substrates with varying coating thickness.
A method involving an aqueous alkaline solution with 30-50 wt.% NaOH at 80-160°C, utilizing an aluminum-containing intermediate layer deposited via PVD, which acts as a breaking point for selective stripping without damaging the substrate, and optionally using a sacrificial anode to prevent cobalt leaching.
The method achieves selective and efficient stripping of aluminum-containing coatings without substrate damage, allowing for complex shapes and varying thicknesses without masking or mechanical treatment, and prevents cobalt dissolution.
Smart Images

Figure 0007570594000001 
Figure 0007570594000002 
Figure 0007570594000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for stripping a coating from a substrate surface, the coating comprising aluminum (Al). In particular, the method of the present invention is useful for stripping a coating comprising AlCrN (aluminum chromium nitride), and more particularly for stripping a coating comprising at least one layer comprising or consisting of AlCrN (aluminum chromium nitride). [Background technology]
[0002] (Prior Art) Andreoli et al., in US patent application Ser. No. 12 / 989,727, describe a process for wet-chemical stripping (hereinafter also referred to as wet-chemical delaminating) of coated substrates. They recommend using an alkaline aqueous solution to dissolve the coating from the substrate by introducing the coated substrate into the alkaline aqueous solution. They recommend using a solution containing 3-8% by weight of KMnO4 and at the same time having an alkaline fraction of 6-15% by weight, this alkaline fraction being preferably formed by KOH or NaOH, and the pH of the solution being greater than 13. They further propose using this solution for wet-chemical stripping of coatings of any one of the following types: metallic AlCr, TiAlCr, other AlCr alloys; nitrides, carbides, borides, or oxides thereof; and combinations thereof.
[0003] However, the use of oxidizing agents such as KMnO4 has the drawback that the chemical attacks not only the coating but also the substrate, so the decoated substrate surface (after stripping) often requires mechanical treatment such as microblasting or polishing to obtain a suitable substrate surface after the stripping process that can be successfully utilized for reapplication of the coating (hereafter also referred to as recoating).
[0004] If the coated substrate is left in the stripper solution for a long time, the substrate will be partially dissolved in the surface substrate area. This can result in shape changes that can be fatal for different tools or parts that are intended to be reused. For example, a cutting tool may lose precision because part of the tool surface is dissolved.
[0005] Therefore, when using such oxidizing agents, the stripping time must be carefully controlled so that it is long enough to completely dissolve the coating, but short enough not to cause too much damage to the substrate surface: the longer the substrate remains in the solution, the greater the damage to the substrate.
[0006] In particular, coated substrates (tools or parts) that have coating thickness variations along the coated surface, due to, for example, geometric shading in the PVD coating process, pose a major challenge.
[0007] The stripping time must be long enough so that the most heavily coated areas are stripped, but the thinner coated areas will strip in less time due to greater attack of the substrate.
[0008] A further disadvantage of methods using oxidizing agents is that they are non-selective stripping methods, which means that the uncoated surfaces of the substrate to be decoated must be masked with any material that inhibits chemical attack of these uncoated surfaces of the substrate.
[0009] For example, a polymeric material cover must be used to mask the uncoated areas before exposure to the chemical stripping solution. This also applies to parts of the substrate that should not be attacked, such as inscriptions or markings. The process of applying and removing the masking or shielding adds an additional work step, is time-consuming and can increase costs.
[0010] Object of the Invention The object of the present invention is to provide a decoating solution that is able to overcome at least some of the drawbacks of non-selective stripping methods mentioned above, in particular those methods involving wet chemical stripping using aqueous solutions containing an oxidizing agent such as KMnO4. Summary of the Invention
[0011] Description of the Invention The object of the invention is achieved by carrying out a method for stripping a coating from a coated surface of a substrate according to the main claim.
[0012] The present invention comprises the steps of:
[0013] As a first step, which may be performed long before the second step, a strippable substrate is produced by depositing an aluminum-containing coating directly onto the substrate surface to be stripped. The substrate surface to be stripped is the surface of the substrate that is "decoated" or "bare" by the stripping and should not be attacked by the stripping. An additional coating may or may not be deposited on top of this coating.
[0014] Then, as soon as it is time to strip, the substrate to be stripped is introduced, meaning washed with or preferably immersed in an alkaline aqueous solution, which has the effect of chemically stripping the coating from the substrate.
[0015] According to the invention, the aqueous alkaline solution contains NaOH in a concentration by weight of 30 wt.% to 50 wt.%. Preferably, the concentration range includes the boundaries of 30 wt.% NaOH and 50 wt.% NaOH, respectively.
[0016] The inventors have discovered and for the first time systematically exploited the effect that aluminum, constituted by a layer deposited directly on the surface to be stripped, forms a kind of "predefined breaking point" which breaks under attack by NaOH. In this way, layers deposited directly on said surface can be rapidly stripped.
[0017] Preferably, the layer comprising aluminum deposited directly on the substrate surface to be stripped is: Metal interlayer, or a wurtzite aluminium nitride layer (which may also be deposited as an intermediate layer), or a layer comprising wurtzite aluminium nitride (which may also be deposited as an intermediate layer), or An aluminium oxide layer (which may also be deposited as an intermediate layer).
[0018] Preferably, the chemical stripping is carried out by maintaining said aqueous alkaline solution at a temperature corresponding to a value in the range of 80° C. to 160° C., including the limits of 80° C. and 160° C., respectively.
[0019] According to a preferred embodiment of the method according to the invention, the layer deposited directly on the substrate surface to be decoated is deposited using a physical vapor deposition process (PVD), and before carrying out the deposition process, a blasting medium containing alumina is used to blast (also called sandblasting in the context of the present invention) one or more cathodes used as a coating material source for depositing the layer deposited directly on the substrate. These blasted cathodes or cathodes create different deposition conditions during the first stage of the PVD deposition process, resulting in the formation of a thin first coating layer (or a kind of intermediate layer), which facilitates chemical stripping of the coating by an alkaline NaOH aqueous solution (generally, the formation of said kind of intermediate layer in this way does not result in a deterioration of the coating performance). The inventors suggest that in this case, one possible explanation for this effect is that the blasting media first cleans the surface of the cathode (e.g., removes cathode material that has reacted with reactive gases such as nitrogen or oxygen) and then, perhaps, immerses into the target surface in such a way that the formation of a first or intermediate layer produced by the used blasted cathode is influenced by the immersed blasting media on the cathode surface, resulting in this positive effect (leading to the formation of a first or intermediate layer that facilitates chemical stripping with alkaline NaOH aqueous solution).
[0020] In view of the above aspects of the invention, one preferred embodiment of the invention is a method for stripping a coating from a surface of a substrate, comprising the steps of: a) using a blasting medium comprising alumina for blasting a cathode which will be used as a coating material source for depositing at least a first coating layer of a coating to be deposited on a substrate surface by using a physical vapor deposition (PVD) process; b) activating the cathode for depositing the first coating layer after blasting the cathode as shown in step a); c) depositing a first coating layer, during the deposition of the first coating layer an intermediate layer is formed directly on the substrate surface, the intermediate layer may contain alumina coming from the blasting media used in step a); d) Chemical stripping of the coating from the substrate, where the substrate with the coating is introduced into an aqueous solution comprising NaOH (with the aqueous solution properties during chemical stripping as described below).
[0021] According to a preferred embodiment of the present invention, the concentration of NaOH in the alkaline aqueous solution is a value in the concentration range of 40 wt.% to 50 wt.%, the concentration range including the boundaries of 40 wt.% and 50 wt.%, respectively. If the content of NaOH in the solution is more than 50 wt.%, the solution may become saturated, which may result in the precipitation of solid NaOH, which is unfavorable for the process. If the content of NaOH in the solution is less than 30 wt.%, it may result in an inefficient stripping process.
[0022] Preferably, the temperature of the aqueous alkaline solution is selected to be in the range of 100° C. to 140° C., the range including the boundaries of 100° C. and 140° C., respectively.
[0023] The first layer of the intermediate layer deposited directly on the substrate surface to be coated in the context of the present invention and subsequently decoated (e.g. after use) should preferably be deposited to have a layer thickness of at least 5 nm, more preferably at least 8 nm or 10 nm. The Al content in this first or intermediate layer should be 30 at.% or more, more preferably 35 at.% or more.
[0024] According to an optional preferred embodiment of the invention, the method includes, prior to introducing the coated substrate into the aqueous solution, an additional step in which the coated substrate is introduced into an acidic solution to weaken the coating in a kinetically controlled reaction using acids and / or oxidizing agents. In this embodiment, it may be necessary to shield all uncoated substrate surfaces that are about to come into contact with the acidic solution in order to prevent chemical attack of these uncoated surfaces of the substrate.
[0025] Preferably the acidic solution is as follows: Mixtures containing or consisting of HNO3, or Mixtures containing or consisting of H2SO4, or Mixtures containing or consisting of HCl.
[0026] The inventors have found that the preferred time of exposure, i.e. reaction time in the acidic solution, corresponds to a value ranging from 1 minute to 10 minutes, with the reaction time range including boundaries of 2 minutes and 10 minutes, respectively.
[0027] Cathodic sandblasting as described above results in the formation of a metallic / partially metallic interlayer (often with a thickness of about 10 nm) between the substrate and the coating, which favors that the coating can be dissolved without damaging the substrate surface; particularly very good results have been observed using a 50-50 wt.% NaOH-water solution at 140°C.
[0028] Instead of sandblasting the cathode, other methods with similar effectiveness may be used.The inventors believe that the better solubility of the coatings produced using the conventionally sandblasted cathode may be due to the content of metallic Al at the interface.
[0029] Possibly, using a cathode with a higher Al content (eg, greater than 70 at.% Al) for producing a metallic interlayer or for producing the first layer (eg, interlayer) may also result in improved solubility.
[0030] The present invention relates to a decoating process (also called a stripping process) that does not use oxidizing agents, which makes the process selective since it only attacks the coating and not the substrate.
[0031] Therefore, stripping time is not critical compared to wet chemical stripping process using KMnO4 as oxidizing agent, because by using the method of the present invention, the substrate will not be damaged if left in the stripping solution after decoating (dissolving or removing the coating) is completed. See examples in Figures 1-3. Substrates with complex shapes such as different tools and parts with different and variable coating thicknesses along the extension of the area to be coated can be easily handled and no masking before the decoating process or mechanical treatment of the decoated substrate surface before recoating is required.
[0032] A further aspect of the present invention relates to the avoidance of cobalt dissolution (hereinafter also referred to as Co-dissolution).
[0033] It is well known that prolonged immersion of cemented carbide materials, and thus substrates made of or containing cemented carbide, in aqueous solutions leads to dissolution of the cobalt binder phase. This phenomenon is known as Co-dissolution. According to the present invention, to prevent Co-dissolution while the cemented carbide substrate is undergoing chemical stripping, the coated cemented carbide substrate may be held using a substrate holder equipped with a sacrificial anode that has a lower electrochemical potential than cobalt.
[0034] For example, a sacrificial anode containing Fe (Fe 2+ Oxidation to E 0 -0.447V) is the dissolution of Co (Co 2+ Oxidation to E 0 This would be effective in preventing a 10V drop (-0.28V) as shown in Figure 4.
[0035] Thus, according to a preferred embodiment of the invention, the method of the invention comprises the use of a sacrificial anode connected to the substrate to be decoated in order to carry out the chemical stripping process without any dissolution of the cobalt binder, when the substrate is made of or comprises a hard metal material, where the material of the sacrificial anode is selected to have a lower electrochemical potential than the material of the substrate to be decoated or to have a lower electrochemical potential than the material components contained in the substrate to be decoated that may be dissolved during chemical stripping. For example, the material of the sacrificial anode for decoating a substrate material such as a hard metal with a cobalt binder phase can be selected to have a lower electrochemical potential than cobalt. And, when using a hard metal substrate with a cobalt binder phase, the sacrificial anode can be made of iron or a material that contains mostly iron.
[0036] Further aspects of the invention will now be illustrated and explained in more detail to improve understanding of the invention. The following figures should be helpful in illustrating and understanding the invention. [Brief description of the drawings]
[0037] Figure caption: [Figure 1] Scanning electron micrograph (SEM) of the surface of a cemented carbide abrasive substrate, WC (with 6 wt.% Co) before the application of the coating. [Diagram 2] Scanning electron micrograph (SEM) of the surface of a cemented carbide abrasive substrate after 10 min of immersion in a prior art stripping medium of 4 wt.% KMnO4, 8 wt.% NaOH. The surface is heavily attacked, dissolving the WC grains and leaving the Co-matrix. [Diagram 3] The present invention: Scanning electron micrograph (SEM) of the surface of a cemented carbide abrasive substrate after immersion in a stripping medium of 50 wt.% NaOH for 5 hours at 140° C. The substrate surface is intact. [Figure 4]Schematic diagram of the structure of the stripping process including a sacrificial anode: 1: AlCrN coating, 2: intermediate layer, 3: WC / Co substrate (hard metal substrate), 4: sacrificial anode made of iron having an electrical connection with the substrate to be decoated according to the invention, 5: stripping solution including NaOH according to the invention, 6: oxide layer formed of iron oxide produced by oxidation of the sacrificial anode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0038] In order to explain the present invention in more detail, some examples are described below. The described examples of the present invention should not be understood as limitations of the present invention, but only as showcases of possible, and in most cases preferred, embodiments of the present invention.
[0039] Example 1 (Comparative Example) - Prior Art Stripping Process Conventional PVD coatings, especially Al in atomic percent 70 Cr 30 AlCrN deposited from a target with the composition is stripped using a solution of 4 wt.% KMnO4 and 8 wt.% NaOH. The coated substrate is left in the stripper solution for 20 minutes until the coating is completely dissolved. The substrate surface is attacked and consequently appears highly damaged and rough after the de-coating process.
[0040] Example 2 (Example of the present invention) The process of the present invention is carried out comprising the following steps: I) Coating preparation step - Prior to the PVD coating procedure, the Al in atomic percent used in the PVD process step was 70 Cr 30 The surface of an AlCr target with a composition of was previously sandblasted. The sandblasting media consisted of Al2O3 with grit size 0.25-0.5 mm. A blasting pressure of 1-5 bar, typically 4 bar, was used and the basting time was up to about 30 seconds to cover the surface of one target.
[0041] II) PVD coating of AlCrN is performed using the deposition target prepared in step I. N2 is used as the process gas.
[0042] III) Chemical stripping of the coating was performed by introducing the coated substrate into a 50 wt% NaOH aqueous solution at 130°C. After 4 hours, the coating (3 μm) was completely removed from the substrate. The substrate did not show any damage or degradation of the substrate surface.
[0043] Example 3 (Example of the present invention): A further process of the invention is carried out comprising the steps of:
[0044] I) At the beginning of the coating process, the metal interlayer was deposited using PVD technology, the metal interlayer was deposited directly on the substrate using Al70Cr30 target as the coating material source and Ar gas as the process gas in the coating chamber, typically at 300sccm, for 20s to 5min. The thickness of the metal interlayer ranged from 20nm to 460nm.
[0045] II) A coating layer of AlCrN was deposited on the metallic intermediate layer using a flow of N2 gas as a process gas (also called reactive gas, since it reacts with the AlCr material from the target of composition Al70Cr30 in this case) to form an AlCrN coating layer on the intermediate layer deposited on the substrate to be coated.
[0046] III) Chemical stripping of the coating was performed by introducing the coated substrate into a 50 wt% NaOH aqueous solution at 130°C. After 1.5 hours, the coating was completely removed from the substrate. The substrate showed no damage or degradation of the substrate surface.
[0047] Example 4 (Example of the invention): A further process of the invention is carried out comprising the steps of:
[0048] I) To form an AlCrN coating layer containing wurtzite-AlN, at the beginning of the coating process, an intermediate layer containing wurtzite-AlN was deposited using PVD technique from an AlCr target having elemental composition Al90Cr10 in atomic percent, used as a coating material source in a coating chamber containing a N2 gas flow as a process gas (also called reactive gas, since in this case it reacts with the AlCr material from the target).
[0049] II) To form an AlCrN coating layer on the intermediate layer deposited on the substrate to be coated, a coating layer of AlCrN was deposited on the intermediate layer comprising wurtzite-AlN using PVD technique from an AlCr target having elemental composition Al70Cr30 in atomic percent, used as a coating material source in a coating chamber containing a N2 gas flow as a process gas.
[0050] III) Chemical stripping of the coating was performed by introducing the coated substrate into a 50 wt% NaOH aqueous solution at 130°C. After 1.5 hours, the coating was completely removed from the substrate. The substrate showed no damage or degradation of the substrate surface.
[0051] Example 5 (Example of the invention): A further process of the invention is carried out comprising the steps of:
[0052] I) As shown in Example 3, at the beginning of the coating process, a metal intermediate layer was deposited using PVD technology, which was deposited directly on the substrate using an AlCr-target with a composition of Al70Cr30 in atomic percent as the coating material source and Ar gas as the process gas in the coating chamber, typically at 300 sccm, for 20 seconds and up to 5 minutes.
[0053] II) A coating layer of AlCrN was deposited on the metal intermediate layer using a flow of N2 gas as the process gas (in this case also called reactive gas since it reacts with the AlCr material from the same target as that used in step I) to form an AlCrN coating layer on the intermediate layer deposited on the substrate to be coated.
[0054] III) For kinetically controlled reactions, samples were exposed to acids (HNO3, H2SO4, HCl). In particular, one sample (coated substrate as shown in steps I and II above) was exposed to HCl for 2 minutes. Another sample (also coated substrate as shown in steps I and II above) was exposed to H2SO4 for 2 minutes.
[0055] IV) Chemical stripping of the coating was performed by introducing the coated substrates into a 50 wt% aqueous NaOH solution at a temperature of 90° C. (40° C. lower compared to Example 3). After 3 hours, the coating was completely removed from both substrates.
[0056] Examples 6, 7, 8, 9 and 10: These examples all have the same steps I and II, as described below, but are differentiated from each other in the implementation of the chemical stripping process, i.e., step III below.
[0057] I) Before starting the coating process, the surface of the AlCr target that will later be used for deposition was sandblasted. The sandblasting media consisted of Al2O3 with grit size 0.25-0.5 mm. A blasting pressure of 1-5 bar, typically 3 bar, was used and the blasting time was up to about 30 seconds to cover the surface of one target.
[0058] II) Carrying out a coating process, in which a coating layer of AlCrN was deposited on the substrate surface to be coated using PVD technique from an AlCr target having elemental composition Al70Cr30 in atomic percent, used as a coating material source, in a coating chamber containing N2 gas flow as process gas, to form an AlCrN coating layer on the intermediate layer deposited on the substrate to be coated.
[0059] III) Six different samples (substrates coated by directly following steps I and II above) are subjected to chemical stripping of the coating as follows:
[0060] Step III of Example 6: IIIa. LiOH was used as the base in a saturated aqueous solution with a LiOH concentration of 13 wt.%. Partial stripping was observed after 1 h, resulting in a slower stripping rate compared to the chemical stripping process using NaOH 50 wt.% concentration.
[0061] Step III of Example 7: IIIb. KOH was used as the base in a saturated aqueous solution with a KOH concentration of 50 wt.%. Partial stripping was observed after 1.5 h, resulting in a slower stripping rate compared to the chemical stripping process using NaOH 50 wt.% concentration.
[0062] Step III of Example 8: IIIc. CsOH was used in an aqueous solution with a CsOH concentration of 75 wt.%. Partial stripping was observed after 3 h, resulting in a slower stripping rate compared to the chemical stripping process using NaOH 50 wt.% concentration.
[0063] Step III of Example 9: A base / salt mixture of NaOH:KOH in a 1:1 molar ratio was used in a saturated aqueous solution with a NaOH concentration of 50 wt.% and a KOH concentration of 50 wt.%. Partial stripping was observed after 1 hour, resulting in a slower stripping rate compared to the chemical stripping process using NaOH 50 wt.% concentration.
[0064] Step III of Example 10: A base / salt mixture of NaOH:NaCl with a molar ratio of 1:1 was used in a saturated aqueous solution with a NaOH concentration of 50 wt.% and a NaCl concentration of 25 wt.%. Partial stripping was observed after 20 minutes, resulting in a slower stripping rate compared to the chemical stripping process using NaOH 50 wt.% concentration.
[0065] A base / salt mixture of KOH:NaCl with a molar ratio of 1:1 was used in a saturated aqueous solution with a KOH concentration of 50 wt.% and a NaCl concentration of 25 wt.%. Partial stripping was observed, resulting in a slower stripping rate compared to the chemical stripping process using NaOH 50 wt.% concentration.
[0066] The method according to the invention has also been used successfully for the decoating of substrates coated with many different types of coatings, such as TiAlN-, TiAlSiN-, TiAlN-based coatings and TiAlSiN-based coatings.
[0067] The aqueous solution can be agitated or the substrate to be decoated can be moved during the chemical stripping process. The method according to the invention can also include pre- or post-treatment steps such as rinsing, washing, ultrasonic bathing, drying and heat treatment.
[0068] Independent protection is also claimed for a system of tools with a renewable coating, characterized in that the system is composed of a coated tool carrying an aluminum-containing coating - directly on its surface to be stripped for recoating - and a stripping agent in the form of an aqueous alkaline solution containing NaOH at a concentration of 30 wt.% to 50 wt.% weight percent.
Claims
1. 1. A method of stripping a coating from a coated surface of a substrate, the coating being stripped with an aqueous alkaline solution, the method comprising: preparing a coated substrate to be decoated by providing said substrate with a strippable coating by depositing a coating comprising one or more layers, one layer comprising aluminum being deposited directly on the substrate surface to be decoated; introducing the substrate to be decoated into the alkaline aqueous solution, thereby chemically stripping the coating from the substrate, the alkaline aqueous solution comprising NaOH at a weight percent concentration of 30 wt. % to 50 wt. %, The layer deposited directly on the substrate surface to be decoated comprises: Metal interlayer, or a wurtzite aluminum nitride layer, or a layer comprising wurtzite aluminum nitride, or an aluminum oxide layer; the substrate is connected to a sacrificial anode for carrying out the chemical stripping process, the material of the sacrificial anode being selected to have a lower electrochemical potential than the material of the substrate to be decoated or to have a lower electrochemical potential than material components contained in the substrate to be decoated that may be dissolved during chemical stripping; The layer deposited directly on the substrate surface to be decoated is deposited using a physical vapor deposition process, and prior to carrying out the vapor deposition process, a blasting medium comprising alumina is used to blast one or more cathodes used as a source of coating material for depositing the layer deposited directly on the substrate; The method of claim 1, wherein the layer deposited directly on the substrate surface to be decoated has a thickness of at least 10 nm and an Al content of at least 30 at. %.
2. 2. The method of claim 1, wherein the chemical stripping is performed by maintaining the aqueous alkaline solution at a temperature corresponding to a value in the range of 80°C to 160°C, said temperatures including the boundaries of 80°C and 160°C, respectively.
3. 3. The method according to claim 1, wherein the concentration of NaOH in the alkaline aqueous solution is in the concentration range of 40 wt. % to 50 wt. %, said concentration range including the boundaries of 40 wt. % and 50 wt. %, respectively.
4. 4. The method according to claim 1, wherein the temperature of the aqueous alkaline solution is a value in the range of 100° C. to 140° C., said range including the boundaries of 100° C. and 140° C., respectively.
5. 5. The method according to claim 1, characterized in that, prior to introducing the coated substrate into the aqueous solution, the coated substrate is introduced into an acidic solution for weakening the coating in a kinetically controlled reaction with acids and / or oxidizing agents.
6. The acidic solution is HNO 3 or HNO 3 6. The method of claim 5, wherein the mixture comprises
7. The acidic solution is H 2 SO 4 or H 2 SO 4 6. The method of claim 5, wherein the mixture comprises
8. 7. The method of claim 6, wherein the acidic solution is a mixture consisting of or including HCl.
9. 9. The method according to claim 5, wherein the reaction time in the acidic solution corresponds to a value ranging from 1 minute to 10 minutes, the reaction time range including the limit values of 1 minute and 10 minutes, respectively.
10. 10. The method of claim 1, wherein the sacrificial anode is made of iron or a material containing mostly iron.
11. Method according to any one of the preceding claims, characterized in that the substrate to be decoated is made from a hard metal or the substrate is made from a material which comprises a hard metal.
12. 11. The method according to claim 10, characterized in that the substrate is made of a hard metal having a cobalt binder phase or the substrate to be decoated is made of a material comprising a hard metal having a cobalt binder phase.
Citation Information
Patent Citations
Method for removal of hard coating film in superhard material, and method for production of the superhard material
JP2013064180A
Method for smut removal during stripping of coating
JP2015010279A