Positive electrode additive and positive electrode for lithium secondary battery containing the same
A two-layer positive electrode structure with distinct binders and a specific additive addresses structural instability and adhesive issues, enhancing lithium secondary battery performance and longevity.
Patent Information
- Application Number
- JP2023514814
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-06-03
- Filing Date
- 2022-05-06
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-05-06
AI Technical Summary
Current lithium secondary battery additives are structurally unstable and prone to decomposition under high temperature and humidity, leading to gas generation that causes volumetric expansion and reduces battery stability, while excessive binder use can decrease capacity and conductivity.
A positive electrode structure with a two-layer composite material layer, using a rubber-based resin binder for the first layer and a fluororesin binder for the second layer, with controlled water affinity differences to enhance adhesive strength and minimize additive damage, incorporating a specific positive electrode additive with a chemical formula Li p Co (1-q) M 1 q O 4.
Improves adhesive strength between the electrode collector and composite layers, reduces additive damage, and enhances electrical performance and lifespan by maintaining structural integrity and preventing side reactions.
Smart Images

Figure 0007570759000001 
Figure 0007570759000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a positive electrode additive for a lithium secondary battery and a positive electrode for a lithium secondary battery containing the same.
[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0071880 dated June 3, 2021, and all contents disclosed in the documents of that Korean patent application are incorporated herein by reference. [Background technology]
[0003] With the development of technology and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. Among such secondary batteries, lithium secondary batteries, which have high energy density and working potential, long cycle life, and low self-discharge rate, have been commercialized and are widely used.
[0004] Recently, as lithium secondary batteries are used as power sources for medium- to large-sized devices such as electric vehicles, there is an increasing demand for high capacity, high energy density, and low cost of lithium secondary batteries, and the irreversible additives used in electrodes are also required to have higher irreversible capacity. However, there is currently a limit to the development of positive electrode additives having such high irreversible capacity.
[0005] Conventional irreversible additives such as Li6CoO4 are generally prepared by reacting cobalt oxide with an excess amount of lithium oxide. The irreversible additives prepared in this way are structurally unstable and may be decomposed and lose their irreversible activity when the positive electrode is prepared under high temperature and / or high humidity conditions. As charging proceeds, they generate large amounts of gases such as oxygen gas (O2) and carbon dioxide (CO2). The generated gases not only induce volume expansion of the electrode assembly, reducing the stability of the battery, but also carbon oxides such as carbon dioxide (CO2) induce a side reaction that causes decomposition with the electrolyte, which can act as a major factor in reducing battery performance.
[0006] Meanwhile, a binder is used in the positive electrode mixture layer to ensure adhesion between the positive electrode active material and the irreversible additive and adhesion between the positive electrode active material and the current collector. However, the adhesive strength of the binder may be reduced depending on the type of positive electrode active material, the surface condition of the current collector, etc., and when the content of the binder is increased to prevent this, there is a limit to the capacity and electrical conductivity of the electrode being reduced due to the excessive amount of binder.
[0007] Therefore, there is a need to develop a lithium secondary battery that has excellent electrical performance and life span by minimizing damage to the positive electrode additive contained in the positive electrode and improving the adhesive strength between the positive electrode current collector and the composite layer provided in the positive electrode. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Korean Patent Publication No. 10-2019-0078392 Summary of the Invention [Problem to be solved by the invention]
[0009] Accordingly, an object of the present invention is to provide a positive electrode for a lithium secondary battery, which includes a non-reversible additive in a positive electrode mixture layer provided in a positive electrode, and which can minimize damage to the non-reversible additive and improve adhesion between the positive electrode mixture layer and a positive electrode current collector, thereby improving the electrical performance and lifespan of the battery, and a lithium secondary battery including the same. [Means for solving the problem]
[0010] To solve the above problems, In one embodiment, the present invention comprises: A positive electrode current collector, a first mixture layer, and a second mixture layer are laminated in this order, The first mixture layer includes a first binder made of a rubber-based resin, The second mixture layer provides a positive electrode for a lithium secondary battery, which contains a second binder made of a fluorine-based resin derived from a fluorine (F)-containing monomer.
[0011] In this case, the difference between the static water contact angle of the first mixture layer and the static water contact angle of the second mixture layer may be 5° or more, and specifically, may be 10° to 30°.
[0012] The rubber-based resin may include at least one selected from the group consisting of styrene-butadiene rubber, nitrile-butadiene rubber, methyl methacrylate-butadiene rubber, chloroprene rubber, carboxy-modified styrene-butadiene rubber, and modified polyorganosiloxane polymer.
[0013] The fluorine-based resin may also contain a resin derived from one or more monomers selected from the group consisting of vinylidene fluoride (VDF or VF2), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), chlorotrifluoroethylene (CTFE), hexafluoropropene (HFP), vinyl fluoride (VF), hexafluoroisobutylene (HFIB), perfluorobutylethylene (PFBE), pentafluoropropene, 3,3,3-trifluoro-1-propene, and 2-trifluoromethyl-3,3,3-trifluoropropene.
[0014] In addition, the content of the first binder may be 0.5 to 5 parts by weight per 100 parts by weight of the first composite layer, the content of the second binder may be 0.5 to 10 parts by weight per 100 parts by weight of the second composite layer, and the total content of the first binder and the second binder may be 0.1 to 5 parts by weight per 100 parts by weight of the entire composite layer.
[0015] In addition, at least one of the first mixture layer and the second mixture layer may contain a positive electrode additive represented by the following Chemical Formula 1:
[0016] [Chemical formula 1] Li p Co(1-q) M 1 q O4
[0017] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0018] Here, the positive electrode additive may be contained in an amount of 0.1 to 5 parts by weight per 100 parts by weight of each positive electrode mixture layer.
[0019] The positive electrode additive may have a tetragonal structure with a space group of P42 / nmc.
[0020] The first mixture layer may include a first positive electrode active material, a first conductive material, a positive electrode additive, and a first binder, and the second mixture layer may include a second positive electrode active material, a second conductive material, and a second binder.
[0021] Meanwhile, the first and second positive electrode active materials may each include a lithium metal composite oxide represented by the following Chemical Formula 2:
[0022] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0023] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0.01<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0024] Furthermore, the first conductive material and the second conductive material may each contain one or more materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon nanotubes, graphene, and carbon fibers.
[0025] The content of each of the first conductive material and the second conductive material may be 0.5 to 5 parts by weight per 100 parts by weight of the positive electrode mixture layer.
[0026] Moreover, in one embodiment, the present invention provides forming a first mixture layer containing a first binder made of a rubber-based resin on a positive electrode current collector; forming a second mixture layer on the first mixture layer, the second mixture layer containing a second binder made of a fluorine-based resin derived from a fluorine (F)-containing monomer.
[0027] Here, at least one of the first mixture layer and the second mixture layer may contain a positive electrode additive represented by the following Chemical Formula 1:
[0028] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0029] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0030] In addition, the step of forming the first composite layer may be performed through a step of dry-mixing a first positive electrode active material, a positive electrode additive represented by Chemical Formula 1, a first conductive material, and a first binder composed of a rubber-based resin to prepare a composite composition, and a step of coating the prepared composite composition on a positive electrode current collector. Effect of the Invention
[0031] The positive electrode for a lithium secondary battery according to the present invention has a structure in which a positive electrode current collector, a first composite layer, and a second composite layer are sequentially laminated, and a binder that is more hydrophobic than the binder contained in the second composite layer is used in the first composite layer at a position adjacent to the positive electrode current collector, thereby improving the adhesion between the positive electrode current collector and the composite layer, thereby improving the durability of the positive electrode. In addition, when the first composite layer contains a positive electrode additive, the first binder, which has low affinity for water, can minimize damage to the positive electrode additive during the manufacture of the positive electrode, thereby providing an advantage in that the electrical performance and lifespan of the lithium secondary battery can be further improved. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0032] While the present invention may be modified in many ways and have various embodiments, a specific embodiment will be described in detail in the detailed description.
[0033] It should be understood, however, that this is not intended to limit the invention to the particular embodiment, but rather to include all modifications, equivalents, or alternatives falling within the spirit and scope of the invention.
[0034] In the present invention, the terms "comprise" or "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, and should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.
[0035] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "located on" may include not only the case where it is located at the top, but also the case where it is located at the bottom.
[0036] In addition, in the present invention, a "major component" means 50% by weight or more, 60% by weight or more, 70% by weight or more, 80% by weight or more, 90% by weight or more, 95% by weight or more, or 97.5% by weight or more of the total weight of the composition or specific component, and in some cases, it can also mean 100% by weight when it constitutes the entire composition or specific component.
[0037] In the present invention, "Ah" is a unit of capacity of a lithium secondary battery, and is called "ampere-hour" and means the amount of current per hour. For example, if a battery capacity is "3000mAh", it means that it can be discharged at a current of 3000mA for one hour.
[0038] In addition, in the present invention, the "contact angle" refers to the angle formed between the liquid surface and the solid wall when the liquid comes into contact with the solid surface.
[0039] The present invention will now be described in more detail.
[0040] <Positive electrodes for lithium secondary batteries> In one embodiment, the present invention comprises: A current collector, a first composite layer, and a second composite layer are laminated in this order. The first mixture layer includes a first binder made of a rubber-based resin, The second mixture layer includes a second binder composed of a fluorine-based resin derived from a fluorine (F)-containing monomer, The present invention provides a positive electrode for a lithium secondary battery, the positive electrode additive being represented by the following Chemical Formula 1, in at least one of the first and second composite layers:
[0041] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0042] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0043] The positive electrode for a lithium secondary battery according to the present invention has a structure including a two-layer composite layer on a positive electrode current collector, and in this case, the composite layers forming the two-layer structure, specifically the first composite layer and the second composite layer, may contain different types of binders having different affinities for water.
[0044] For example, the first mixture layer contains a binder made of a rubber-based resin having low affinity for water as a first binder. Such a first binder may include one or more selected from the group consisting of styrene-butadiene rubber, nitrile-butadiene rubber, methyl methacrylate-butadiene rubber, chloroprene rubber, carboxy-modified styrene-butadiene rubber, and modified polyorganosiloxane polymer.
[0045] The second mixture layer contains, as a second binder, a binder composed of a fluorine-based resin derived from a fluorine (F)-containing monomer having a higher affinity for water. Such a second binder may contain a resin derived from one or more monomers selected from the group consisting of vinylidene fluoride (VDF or VF2), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), chlorotrifluoroethylene (CTFE), hexafluoropropene (HFP), vinyl fluoride (VF), hexafluoroisobutylene (HFIB), perfluorobutylethylene (PFBE), pentafluoropropene, 3,3,3-trifluoro-1-propene, and 2-trifluoromethyl-3,3,3-trifluoropropene.
[0046] The second binder may have a crystalline phase and / or an amorphous phase in the positive electrode mixture layer, and specifically, may have both a crystalline phase and an amorphous phase, in which the amorphous phase may occupy 51% or more or 55% or more of the entire crystalline phase. As an example, the second binder may contain 51 to 95%, 51 to 90%, 51 to 85%, 51 to 80%, 51 to 75%, 51 to 70%, 51 to 65%, or 51 to 55% of the entire crystalline phase. The second binder has different affinity to water depending on the crystalline phase in the mixture layer, and among them, when the crystalline form is an amorphous phase, the affinity to water is high. In the present invention, the second binder contains more than 50% of the amorphous phase in the entire crystalline phase of the second binder, thereby improving the wettability of the second mixture layer to the electrolyte.
[0047] In the present invention, the first mixture layer adjacent to the positive electrode current collector contains a rubber-based resin as a first binder, and the second mixture layer contains a fluorine-based resin derived from a fluorine (F)-containing monomer as a second binder. In this case, the rubber-based resin as the first binder has a lower affinity for water than the fluorine-based resin as the second binder.
[0048] As an example, when measuring the static water contact angle for a first composite layer containing the above-mentioned first binder and a second composite layer containing the second binder, the difference between the static water contact angle of the first composite layer and the static water contact angle of the second composite layer may be 5° or more due to the difference in affinity for water between the first binder and the second binder, and specifically may be 10° or more, 15° or more, 20° or more, 5° to 30°, 10° to 30°, 15° to 30°, 20° to 30°, 5° to 20°, 5° to 15°, 8° to 15°, 10° to 16°, 14° to 19°, or 5° to 10°. By controlling the difference in static water contact angle between the first composite layer and the second composite layer within the above range, the present invention can improve the adhesive strength between the positive electrode current collector and the first composite layer, and the adhesive strength between the first composite layer and the second composite layer, and at the same time, improve the wettability of the second composite layer to the electrolyte.
[0049] For example, the first composite layer has a relatively lower affinity for water than the second composite layer, and therefore has excellent adhesion to the metal positive electrode current collector. Specifically, the positive electrode manufactured according to the present invention has an adhesion strength between the positive electrode current collector and the composite layer that is at least 1.5 times, more specifically, at least 1.8 times, at least 2 times, at least 2.2 times, or at least 2.5 times stronger than when the first composite layer and the second composite layer are made of a binder (i.e., a second binder) made of a fluorine-based resin such as PVDF.
[0050] Here, the content of the first binder may be 0.5 to 5 parts by weight per 100 parts by weight of the first composite layer, the content of the second binder may be 0.5 to 10 parts by weight per 100 parts by weight of the second composite layer, and the total content of the first binder and the second binder may be 0.1 to 5 parts by weight per 100 parts by weight of the entire composite layer.
[0051] Specifically, the content of the first binder may be 0.5 to 4 parts by weight, 0.5 to 3 parts by weight, 0.5 to 2 parts by weight, 1 to 3 parts by weight, 2 to 5 parts by weight, or 1.5 to 2.5 parts by weight, per 100 parts by weight of the first composite layer, and the content of the second binder may be 0.5 to 8 parts by weight, 0.5 to 6 parts by weight, 0.5 to 5 parts by weight, 0.5 to 3 parts by weight, 0.5 to 2 parts by weight, 1 to 3 parts by weight, or 2 to 4 parts by weight, per 100 parts by weight of the second composite layer.
[0052] The total content of the first binder and the second binder may be 0.5 to 4 parts by weight, 0.5 to 3 parts by weight, 0.5 to 2 parts by weight, 1 to 3 parts by weight, 2 to 5 parts by weight, or 1.5 to 2.5 parts by weight, based on 100 parts by weight of the entire composite layer.
[0053] In the present invention, by controlling the contents of the first binder and the second binder contained in the first composite layer and the second composite layer, respectively, as described above, it is possible to easily improve the adhesive strength between the positive electrode current collector and the first composite layer, and between the first composite layer and the second composite layer.
[0054] Meanwhile, the positive electrode according to the present invention may contain a positive electrode additive represented by the following Chemical Formula 1 in at least one of the first mixture layer and the second mixture layer:
[0055] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0056] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0057] The positive electrode additive contains an excess of lithium and can provide lithium to replace lithium consumption that occurs due to irreversible chemical and physical reactions at the negative electrode during initial charging, thereby increasing the charging capacity of the battery and reducing the irreversible capacity, thereby improving the life characteristics.
[0058] Among them, the positive electrode additive represented by the above formula 1 has a higher lithium ion content than nickel-containing oxides commonly used in the industry, and therefore can replenish lithium ions lost in irreversible reactions during initial activation of the battery, thereby significantly improving the charge / discharge capacity of the battery. Also, compared to iron- and / or manganese-containing oxides commonly used in the industry, there is no side reaction caused by the elution of transition metals during charging and discharging of the battery, and therefore the battery has excellent stability. Examples of lithium cobalt oxides represented by the formula 1 include Li6CoO4, Li6Co 0.5 Zinc 0.5 O4, Li6Co 0.7 Zinc 0.3 It may also include O4.
[0059] The average particle size of the lithium cobalt oxide represented by the above chemical formula 1 may be 0.1 to 10 μm, specifically, 0.1 to 8 μm, 0.1 to 5 μm, 0.1 to 3 μm, 0.5 to 2 μm, 0.1 to 0.9 μm, 0.1 to 0.5 μm, 0.6 to 0.9 μm, 1 to 4 μm, 4 to 6 μm, or 6 to 9 μm. By controlling the average particle size of the lithium cobalt oxide within the above range, the present invention can enhance the irreversible activity of the lithium cobalt oxide and prevent the powder electrical conductivity of the lithium cobalt oxide from decreasing.
[0060] In addition, the lithium cobalt oxide represented by the formula 1 may have a tetragonal crystal structure, and may be included in the space group P42 / nmc having a distorted tetrahedral structure formed by cobalt and oxygen atoms. The positive electrode additive having a distorted tetrahedral structure has a distorted tetrahedral structure formed by cobalt and oxygen atoms, and is structurally unstable, so that it may be damaged by a side reaction with moisture (H2O) in the air during the preparation of the positive electrode, and thus the electrical performance of the battery may be deteriorated. However, the present invention uses a binder having low affinity for water as a binder for the composite layer to minimize the damage to the positive electrode additive, and therefore the electrical performance and life of the lithium secondary battery may be improved.
[0061] In addition, the positive electrode additive may be included in an amount of 0.1 to 5 parts by weight relative to 100 parts by weight of each positive electrode mixture layer, specifically, 0.1 to 4 parts by weight, 0.1 to 3 parts by weight, 0.1 to 2 parts by weight, 0.1 to 1 part by weight, 0.5 to 2 parts by weight, 1 to 3 parts by weight, 2 to 4 parts by weight, 1.5 to 3.5 parts by weight, 0.5 to 1.5 parts by weight, or 1 to 2 parts by weight.
[0062] As an example, the positive electrode additive may be included in an amount of 0.1 to 0.5 parts by weight with respect to 100 parts by weight of the first mixture layer, and 0.2 to 0.6 parts by weight with respect to 100 parts by weight of the second mixture layer.
[0063] As another example, the positive electrode additive may be contained only in the first mixture layer. In this case, the amount contained in the first mixture layer may be 0.5 to 2 parts by weight with respect to 100 parts by weight of the entire mixture layer.
[0064] In addition, the first mixture layer may include a first positive electrode active material, a first conductive material, and a first binder, and the second mixture layer may include a second positive electrode active material, a second conductive material, and a second binder, and the positive electrode additive may be included in either one of the first mixture layer or the second mixture layer.
[0065] For example, the first mixture layer may include a first positive electrode active material, a first conductive material, a positive electrode additive, and a first binder, and the second mixture layer may include a second positive electrode active material, a second conductive material, and a second binder. The present invention has an advantage that, by including the positive electrode additive in the first mixture layer, damage to the positive electrode additive caused by high temperature and / or high humidity during the manufacture of the positive electrode can be minimized, thereby further improving the electrical performance and lifespan of the lithium secondary battery.
[0066] In this case, the first positive electrode active material and the second positive electrode active material may be a lithium composite transition metal oxide containing two or more elements selected from the group consisting of nickel (Ni), cobalt (Co), manganese (Mn), aluminum (Al), zinc (Zn), titanium (Ti), magnesium (Mg), chromium (Cr) and zirconium (Zr). For example, the first positive electrode active material and the second positive electrode active material may each contain a lithium metal composite oxide capable of reversible intercalation and deintercalation, as represented by the following Chemical Formula 2:
[0067] [Chemical formula 2] Li x [Ni y Co z Mn w M 2 v ]O u
[0068] In the above chemical formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w, v, and u are within the range of 1.0≦x≦1.30, 0.1≦y<0.95, and 0.01, respectively. <z≦0.5、0.01<w≦0.5、0≦v≦0.2、1.5≦u≦4.5である。
[0069] The lithium metal composite oxide represented by the above chemical formula 2 is a composite metal oxide containing lithium, nickel, cobalt and manganese, and in some cases, other transition metals (M 2 For example, the first positive electrode active material and the second positive electrode active material may each be doped with LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.8 Co 0.1 Mn 0.05 Al 0.05 O2 and LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2. As an example, the first positive electrode active material and the second positive electrode active material are each a lithium metal composite oxide represented by Chemical Formula 2, LiNi 0.6 Co 0.2 Mn 0.2 O2 and LiNi 0.8 Co 0.1 Mn 0.1 O2 can be used alone or in combination.
[0070] In addition, the first conductive material and the second conductive material can be used to improve the performance of the positive electrode, such as the electrical conductivity, and each may contain one or more materials selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon nanotubes, graphene, and carbon fibers.
[0071] Here, the content of the first conductive material and the second conductive material may be 0.5 to 5 parts by weight relative to 100 parts by weight of each composite layer, specifically, 0.5 to 4 parts by weight, 0.5 to 3 parts by weight, 0.5 to 1 part by weight, 0.5 to 2 parts by weight, 1 to 3 parts by weight, 2 to 4 parts by weight, 1.5 to 3.5 parts by weight, 0.5 to 1.5 parts by weight, or 1 to 2 parts by weight.
[0072] Moreover, the average thickness of the first composite layer and the second composite layer is not particularly limited, but may be specifically 50 μm to 200 μm, 50 μm to 150 μm, 50 μm to 100 μm, 50 μm to 80 μm, 70 μm to 120 μm, or 60 μm to 110 μm, respectively. In addition, the total thickness of these layers may be 50 μm to 300 μm, more specifically 100 μm to 200 μm, 80 μm to 150 μm, 120 μm to 170 μm, 150 μm to 300 μm, 200 μm to 300 μm, or 150 μm to 190 μm.
[0073] In addition, the positive electrode can be a positive electrode current collector having high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. can be used, and in the case of aluminum or stainless steel, those surface-treated with carbon, nickel, titanium, silver, etc. can be used. In addition, the positive electrode current collector can be formed with fine irregularities on the surface to increase the adhesive force of the positive electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the positive electrode current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the positive electrode to be manufactured.
[0074] <Method of manufacturing positive electrode for lithium secondary battery> In one embodiment, the present invention provides a method for producing a composition comprising: forming a first mixture layer containing a first binder made of a rubber-based resin on a positive electrode current collector; forming a second mixture layer on the first mixture layer, the second mixture layer including a second binder composed of a fluorine-based resin derived from a fluorine (F)-containing monomer; The present invention provides a method for manufacturing a positive electrode for a lithium secondary battery, the method comprising the steps of:
[0075] [Chemical formula 1] Li p Co (1-q) M 1 q O4
[0076] In the above chemical formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
[0077] The method for manufacturing a positive electrode for a lithium secondary battery according to the present invention may be carried out through a process of forming a two-layered composite layer on a positive electrode composite layer. Specifically, the method is carried out by sequentially forming a first composite layer and a second composite layer on a positive electrode current collector, and the first composite layer and the second composite layer may contain a first binder and a second binder, respectively, having different affinities to water, and a positive electrode additive may be contained in at least one of the first composite layer and the second composite layer.
[0078] Here, the first composite layer can be manufactured by dry-mixing the first positive electrode active material constituting the composite layer, the positive electrode additive represented by Chemical Formula 1, the first conductive material, and the first binder composed of a rubber-based resin at a speed of 1000 to 4000 rpm at room temperature (e.g., 22±3°C) to manufacture a composite composition, and applying the manufactured composite composition to a positive electrode current collector.
[0079] In the present invention, the first composite layer is formed by the dry method as described above, which can omit the process of drying the solvent when the wet method is used, thereby improving productivity, and preventing the binder and conductive material from migrating to the surface of the composite layer during the solvent drying process. In addition, the dry mixing method performed at a high speed of 1000 to 4000 rpm realizes an effect of uniformly coating the surface of each particle with the first binder, thereby improving the adhesive strength between particles and / or between the current collector and the composite layer, and when a positive electrode additive is contained in the first composite layer, it can effectively prevent the positive electrode additive from being damaged by moisture during the manufacture of the positive electrode.
[0080] In addition, the method for manufacturing a positive electrode for a lithium secondary battery includes a process of forming a second composite layer on the formed first composite layer, and the method for forming the second composite layer is not particularly limited and can be applied. Specifically, the second composite layer can be formed by a wet method in which a positive electrode slurry is prepared by mixing a second positive electrode active material, a second conductive material, a second binder, etc. in a solvent, and in some cases, the second composite layer can be formed by a dry method in the same manner as the first composite layer.
[0081] In this case, when the second composite layer is formed by a wet method, the usable solvent may contain one or more polar aprotic solvents selected from N-methyl-2-pyrrolidone (NMP), dimethylacetamide (DMAc), dimethylformamide (DMF), dimethylsulfoxide (DMSO), acetonitrile (ACN), dimethylformamide (DMF), acetone, and ethyl acetate. In the present invention, when the second composite layer contains a positive electrode additive, the above-mentioned solvent is used in a wet method when the second composite layer is formed, thereby minimizing damage to the positive electrode additive and allowing the positive electrode additive to be uniformly mixed with the second positive electrode active material, the second conductive material, and the second binder.
[0082] In addition, when the step of forming the second mixture layer is performed by a wet method, the positive electrode slurry applied on the positive electrode current collector may be dried in a vacuum at a temperature of 140°C or less, specifically, at 130°C or less, 120°C or less, 110°C or less, 100°C or less, 80°C or less, 70°C or less, 60°C or less, 50°C or less, 40°C or less, 20°C to 140°C, 20°C to 120°C, 20°C to 100°C, 20°C to 90°C, 20°C to 70°C, 20°C to 50°C, 40°C to 90°C, 60°C to 140°C, 90°C to 140°C, or 100°C to 130°C.
[0083] In the present invention, by drying the positive electrode slurry under the above-mentioned conditions, the proportion of the amorphous phase in the crystalline phase of the fluorine-based resin as the second binder can be easily controlled to be 51% or more.
[0084] The method for manufacturing a positive electrode for a lithium secondary battery according to the present invention has the advantages of minimizing damage to the positive electrode additive manufactured by the above-mentioned configuration, improving wettability to an electrolyte, thereby improving electrical performance of the battery, and improving adhesion of the positive electrode for a lithium secondary battery, thereby improving the life of the battery.
[0085] <Lithium secondary battery> Further, in one embodiment, the present invention provides There is provided a lithium secondary battery including the above-described positive electrode according to the present invention, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.
[0086] The lithium secondary battery according to the present invention includes the positive electrode of the present invention as described above, and thus the adhesion between the positive electrode current collector and the composite layer can be further improved, thereby improving the durability of the positive electrode, and damage to the positive electrode additive during the manufacture of the positive electrode can be minimized, thereby advantageously improving the electrical performance and lifespan of the lithium secondary battery.
[0087] The lithium secondary battery of the present invention has a structure including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.
[0088] Here, the negative electrode is manufactured by applying a negative electrode active material onto a negative electrode current collector, followed by drying and pressing, and may further include the same conductive material, organic binder polymer, additives, etc. as the positive electrode, as necessary.
[0089] The negative electrode active material may include, for example, a carbon material and a silicon material. The carbon material means a carbon material mainly composed of carbon atoms, and examples of such carbon materials include graphite having a perfect layered crystal structure like natural graphite, soft carbon having a low crystalline layered crystal structure (graphene structure; a structure in which hexagonal honeycomb-shaped carbon planes are arranged in layers), and hard carbon in which such a structure is mixed with a non-crystalline portion, artificial graphite, expanded graphite, carbon fiber, non-graphitizable carbon, carbon black, acetylene black, ketjen black, fullerene, activated carbon, graphene, carbon nanotubes, etc., and preferably, may include one or more selected from the group consisting of natural graphite, artificial graphite, graphene, and carbon nanotubes. More preferably, the carbon material includes natural graphite and / or artificial graphite, and may include at least one of graphene and carbon nanotubes together with the natural graphite and / or artificial graphite. In this case, the carbon substance may contain 50 to 95 parts by weight of graphene and / or carbon nanotubes per 100 parts by weight of the total carbon substance, and more specifically, may contain 60 to 90 parts by weight, or 70 to 80 parts by weight of graphene and / or carbon nanotubes per 100 parts by weight of the total carbon substance.
[0090] The silicon substance is a particle containing silicon (Si) as a metal component as a main component, and is a silicon (Si) particle and a silicon oxide (SiO X , 1≦X≦2) particles. As an example, the silicon material may include silicon (Si) particles, silicon monoxide (SiO) particles, silicon dioxide (SiO2) particles, or a mixture of these particles.
[0091] In addition, the silicon material may have a mixed form of crystalline particles and amorphous particles, and the ratio of the amorphous particles may be 50 to 100 parts by weight, specifically 50 to 90 parts by weight, 60 to 80 parts by weight, or 85 to 100 parts by weight, based on 100 parts by weight of the total silicon material. By controlling the ratio of the amorphous particles contained in the silicon material within the above range, the present invention can improve thermal stability and flexibility without deteriorating the electrical properties of the electrode.
[0092] The negative electrode active material may include a carbon material and a silicon material, and may be included in an amount of 1 to 20 parts by weight relative to 100 parts by weight of the negative electrode composite layer. Specifically, the negative electrode active material may be included in an amount of 5 to 20 parts by weight, 3 to 10 parts by weight, 8 to 15 parts by weight, 13 to 18 parts by weight, or 2 to 7 parts by weight relative to 100 parts by weight of the negative electrode composite layer.
[0093] By adjusting the contents of the carbon material and silicon material contained in the negative active material within the above ranges, the present invention can reduce the lithium consumption and irreversible capacity loss during the initial charge and discharge of the battery, and improve the charge capacity per unit mass.
[0094] For example, the negative electrode active material may include 95±2 parts by weight of graphite and 5±2 parts by weight of a mixture of silicon monoxide (SiO) particles and silicon dioxide (SiO2) particles uniformly mixed, relative to 100 parts by weight of the negative electrode composite layer. By adjusting the contents of the carbon material and silicon material contained in the negative electrode active material within the above ranges, the present invention can reduce lithium consumption and irreversible capacity loss during initial charging and discharging of the battery, and improve the charging capacity per unit mass.
[0095] The negative electrode mixture layer may have an average thickness of 100 μm to 200 μm, specifically, 100 μm to 180 μm, 100 μm to 150 μm, 120 μm to 200 μm, 140 μm to 200 μm, or 140 μm to 160 μm.
[0096] In addition, the negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and for example, copper, stainless steel, nickel, titanium, calcined carbon, etc. can be used. In the case of copper or stainless steel, it is also possible to use a material that has been surface-treated with carbon, nickel, titanium, silver, etc. In addition, the negative electrode current collector can be formed with fine irregularities on the surface in the same manner as the positive electrode current collector to strengthen the binding force with the negative electrode active material, and can be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc. In addition, the average thickness of the negative electrode current collector can be appropriately applied to 3 to 500 μm in consideration of the conductivity and total thickness of the negative electrode to be manufactured.
[0097] The separator is a thin insulating membrane having high ion permeability and mechanical strength, which is interposed between the positive and negative electrodes. The separator is not particularly limited as long as it is one commonly used in the industry. Specifically, a sheet or nonwoven fabric made of chemically resistant and hydrophobic polypropylene, glass fiber, or polyethylene may be used. In some cases, a composite separator made of a porous polymer substrate such as the sheet or nonwoven fabric and inorganic particles / organic particles coated with an organic binder polymer may be used. When a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte may also serve as the separator. The pore diameter of the separator may be an average of 0.01 to 10 μm, and the thickness may be an average of 5 to 300 μm.
[0098] Meanwhile, the positive and negative electrodes may be wound in a jelly roll form and housed in a cylindrical battery, a prismatic battery, or a pouch battery, or may be housed in a pouch battery in a folded or stack-and-folded form, but is not limited thereto.
[0099] The lithium salt-containing electrolyte according to the present invention may be composed of an electrolyte and a lithium salt. The electrolyte may be a non-aqueous organic solvent, an organic solid electrolyte, or an inorganic solid electrolyte.
[0100] Examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydrofuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.
[0101] Examples of the organic solid electrolyte that can be used include polyethylene derivatives, polyethylene oxide derivatives, polypropylene oxide derivatives, phosphate polymers, polyagitation lysine, polyester sulfide, polyvinyl alcohol, polyvinylidene fluoride, and polymeric materials containing ionic dissociation groups.
[0102] Examples of the inorganic solid electrolyte that can be used include nitrides, halides, and sulfates of Li, such as Li3N, LiI, Li5NI2, Li3N-LiI-LiOH, LiSiO4, LiSiO4-LiI-LiOH, Li2SiS3, Li4SiO4, Li4SiO4-LiI-LiOH, and Li3PO4-Li2S-SiS2.
[0103] The lithium salt is a substance that is easily dissolved in a non-aqueous electrolyte, and examples of the lithium salt include LiCl, LiBr, LiI, LiClO4, LiBF4, and LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, (CF3SO2)2NLi, lithium chloroborane, lithium lower aliphatic carboxylates, lithium 4-phenylboronate, imides, etc. can be used.
[0104] In addition, for the purpose of improving charge / discharge characteristics, flame retardancy, etc., the electrolyte may contain, for example, pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, n-glyme, hexaphosphoric acid triamide, nitrobenzene derivatives, sulfur, quinoneimine dyes, N-substituted oxazolidinones, N,N-substituted imidazolidines, ethylene glycol dialkyl ethers, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, etc. In some cases, in order to impart non-flammability, a halogen-containing solvent such as carbon tetrachloride or trifluoroethylene may be further contained, and in order to improve high-temperature storage characteristics, carbon dioxide gas may be further contained, and FEC (Fluoro-Ethylene Carbonate), PRS (Propene sultone, propene sultone, etc. may be further contained.
[0105] The present invention will now be described in more detail with reference to examples and experimental examples.
[0106] However, the following examples and experimental examples are merely illustrative of the present invention, and the content of the present invention is not limited to the following examples and experimental examples.
[0107] <Examples 1 to 3 and Comparative Examples 1 to 2. Production of Positive Electrodes for Lithium Secondary Batteries> The homo mixer contains LiNi as the first positive electrode active material. 0.6 Co 0.2 Mn 0.2 A composite material composition was prepared by weighing and adding 47.7 parts by weight of O2 (average particle size: 1±0.5 μm), 40.8 parts by weight of Li6CoO as a positive electrode additive, 0.5 parts by weight of carbon black (average particle size: 2±0.5 μm) as a first conductive material, and 1 part by weight of styrene-butadiene rubber (SBR) as a first binder at room temperature and 3,000±500 rpm for 50 to 70 minutes.
[0108] Separately, N-methylpyrrolidone was poured into a homo mixer, and LiNi as the second positive electrode active material was mixed with 100 parts by weight of the positive electrode slurry solids. 0.6 Co 0.2 Mn 0.2 48.5 parts by weight of O2 (average particle size: 1±0.5 μm), 0.5 parts by weight of carbon black (average particle size: 2±0.5 μm) as a second conductive material, and 1 part by weight of polyvinylidene fluoride (PVDF) as a second binder were weighed and added, and mixed at room temperature at 2,000±500 rpm for 50 to 70 minutes to prepare a positive electrode slurry.
[0109] Then, a prepared composite composition was applied to one side of an aluminum current collector, and the first composite layer was formed by passing it between hot press rollers and rolling it. Then, the positive electrode slurry was continuously applied onto the first composite layer, and the layer was vacuum dried under the temperature conditions shown in Table 1 below, and then rolled to produce a positive electrode for a lithium secondary battery. At this time, the thicknesses of the first composite layer and the second composite layer were 55 μm and 80 μm, respectively, and the total thickness of the produced positive electrode was about 200 μm.
[0110] [Table 1]
[0111] <Comparative Example 3. Production of Positive Electrode for Lithium Secondary Battery> A positive electrode for a lithium secondary battery was manufactured in the same manner as in Example 1, except that polyvinylidene fluoride (PVDF) was used as the first binder, and a positive electrode slurry containing a first positive electrode active material, a positive electrode additive, a first conductive material, and the first binder was manufactured in N-methylpyrrolidone to form a first composite layer.
[0112] <Experimental Example> In order to evaluate the performance of the positive electrode additive according to the present invention, the following experiment was carried out.
[0113] a) Evaluation of static water contact angle of the positive electrode composite layer Positive electrodes were fabricated in the same manner as in Examples 1 to 3 and Comparative Examples 1 to 3, and when the first and second composite layers were formed, the static water contact angle for the surface of each composite layer was measured. Here, the static water contact angle was measured using a sessile drop method. Specifically, the static water contact angle was measured by dropping a drop of purified water onto the surface of each composite layer, capturing an image of the dropped drop, and then analyzing the captured image.
[0114] b) Evaluation of the interfacial adhesion strength of the positive electrode composite layer The positive electrodes manufactured in Examples 1 to 3 and Comparative Examples 1 to 3 were cut to have horizontal and vertical lengths of 25 mm and 70 mm, respectively, and laminated at 70 ° C. and 4 MPa using a press to produce test pieces. The prepared test pieces were attached and fixed to a glass plate using double-sided tape, and the positive electrode current collector was arranged to face the glass plate. The separation membrane portion of the test piece was peeled off at an angle of 90 ° at a speed of 100 mm / min at 25 ° C. using a tensile tester, and the peel force at this time was measured in real time, and the average value was defined as the interfacial adhesion force between the first composite layer and the second composite layer, and then the interfacial adhesion force between the positive electrode current collector and the first composite layer was measured by continuously performing the same method. The results are shown in Table 2 below.
[0115] C) Evaluation of battery charge / discharge capacity First, 84 parts by weight of natural graphite and silicon (SiO x 14 parts by weight of 1≦x≦2) particles and 2 parts by weight of styrene butadiene rubber (SBR) as a binder were prepared, and the negative electrode slurry was prepared in the same manner as the positive electrode slurry. At this time, the graphite used in the manufacture of the negative electrode mixture layer was natural graphite (average particle size: 0.01 to 0.5 μm), and silicon (SiOx) particles having an average particle size of 0.9 to 1.1 μm were used. The prepared negative electrode slurry was applied to one side of a copper current collector, and then dried at 100°C and rolled to manufacture a negative electrode. At this time, the total thickness of the negative electrode mixture layer was 150 μm, and the total thickness of the manufactured negative electrode was about 250 μm.
[0116] The positive and negative electrodes prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were laminated with a separator (thickness: about 16 μm) made of a porous polyethylene (PE) film interposed between them, and E2DVC was injected as an electrolyte to prepare a full cell type lithium secondary battery.
[0117] Here, "E2DVC" refers to a type of carbonate-based electrolyte, a solution in which lithium hexafluorophosphate (LiPF6, 1.0M) and vinyl carbonate (VC, 2% by weight) are mixed with a mixture of ethylene carbonate (EC): dimethyl carbonate (DMC): diethyl carbonate (DEC) = 1:1:1 (volume ratio).
[0118] The fabricated lithium secondary battery was charged at a temperature of 25°C with a charging current of 0.1C to a charge cut-off voltage of 4.2 to 4.25V, and activated by charging until the current density at the cut-off voltage was 0.01C. Thereafter, the battery was discharged at a discharging current of 0.1C to a cut-off voltage of 2V, and the initial charge / discharge capacity per unit mass was measured. The results are shown in Table 2 below.
[0119] [Table 2]
[0120] Referring to Table 2 above, it can be seen that the positive electrode for a lithium secondary battery according to the present invention has excellent adhesion between the positive electrode current collector and the positive electrode mixture layer, and the charging capacity of the battery is high.
[0121] Specifically, in the positive electrode for a lithium secondary battery according to the embodiment of the present invention, the first and second composite layers contain a rubber-based resin and a fluorine-based resin as binders, respectively, to control the affinity of each composite layer for water, and the first composite layer has a lower affinity for water, so that the difference AB in the static water contact angle between the first composite layer A and the second composite layer B is 5° or more. This difference is found to improve the interfacial adhesion between the positive electrode current collector and the first composite layer, and between the first composite layer and the second composite layer, and when a positive electrode additive is used in the first composite layer having a low affinity for water, damage to the positive electrode additive is prevented, resulting in a high initial charge capacity.
[0122] From these results, it can be seen that the positive electrode for a lithium secondary battery according to the present invention has a structure in which a positive electrode current collector, a first composite layer, and a second composite layer are sequentially stacked, and a binder that is more hydrophobic than the binder contained in the second composite layer is used in the first composite layer at a position adjacent to the positive electrode current collector, thereby further improving the adhesion between the positive electrode current collector and the composite layer, thereby improving the durability of the positive electrode; and when the first composite layer contains a positive electrode additive, the first binder, which has low affinity for water, minimizes damage to the positive electrode additive during the manufacture of the positive electrode, thereby further improving the electrical performance and lifespan of the lithium secondary battery.
[0123] Although the present invention has been described above with reference to preferred embodiments thereof, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.
[0124] Therefore, the technical scope of the present invention should not be limited to the contents described in the detailed description of the specification, but should be defined by the claims.
Claims
1. a positive electrode current collector, a first mixture layer, and a second mixture layer are laminated in this order; The first mixture layer includes a first binder made of a rubber-based resin, The second mixture layer includes a second binder composed of a fluorine-based resin derived from a fluorine (F)-containing monomer, At least one of the first mixture layer and the second mixture layer contains a positive electrode additive represented by the following Chemical Formula 1: [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; A positive electrode for a lithium secondary battery, wherein p and q are 5≦p≦7 and 0≦q≦0.5, respectively.
2. 2 . The positive electrode for a lithium secondary battery according to claim 1 , wherein the static water contact angle of the first mixture layer is at least 5° larger than the static water contact angle of the second mixture layer.
3. 2. The positive electrode for a lithium secondary battery according to claim 1, wherein the static water contact angle of the first mixture layer is 10° to 30° larger than the static water contact angle of the second mixture layer.
4. 2. The positive electrode for a lithium secondary battery according to claim 1, wherein the rubber-based resin comprises at least one selected from the group consisting of styrene-butadiene rubber, nitrile-butadiene rubber, methyl methacrylate-butadiene rubber, chloroprene rubber, carboxy-modified styrene-butadiene rubber, and modified polyorganosiloxane polymer.
5. 2. The positive electrode for a lithium secondary battery according to claim 1, wherein the fluorine-based resin comprises a resin derived from one or more monomers selected from the group consisting of vinylidene fluoride (VDF), tetrafluoroethylene (TFE), trifluoroethylene (TrFE), chlorotrifluoroethylene (CTFE), hexafluoropropene (HFP), vinyl fluoride (VF), hexafluoroisobutylene (HFIB), perfluorobutyl ethylene (PFBE), pentafluoropropene, 3,3,3-trifluoro-1-propene, and 2-trifluoromethyl-3,3,3-trifluoropropene.
6. The content of the first binder is 0.5 to 5 parts by weight relative to 100 parts by weight of the first mixture layer; The content of the second binder is 0.5 to 10 parts by weight relative to 100 parts by weight of the second mixture layer, and 2. The positive electrode for a lithium secondary battery according to claim 1, wherein a total content of the first binder and the second binder is 1 to 5 parts by weight with respect to a total of 100 parts by weight of the first mixture layer and the second mixture layer.
7. 2. The positive electrode for a lithium secondary battery according to claim 1, wherein the positive electrode additive is contained in an amount of 0.1 to 5 parts by weight per 100 parts by weight of each composite layer.
8. The positive electrode additive has a space group of P4 2 2. The positive electrode for a lithium secondary battery according to claim 1, having a tetragonal structure in which N is a cubic lattice constant.
9. the first mixture layer includes a first positive electrode active material, a first conductive material, the positive electrode additive, and the first binder; 2 . The positive electrode for a lithium secondary battery according to claim 1 , wherein the second mixture layer comprises a second positive electrode active material, a second conductive material, and the second binder.
10. The first positive electrode active material and the second positive electrode active material each include a lithium metal composite oxide represented by the following Chemical Formula 2: [Chemical formula 2] Li x [Ni yCo z Mn w M 2 v ]O u In the above Chemical Formula 2, M 2 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; 10. The positive electrode for a lithium secondary battery according to claim 9, wherein x, y, z, w, v and u are in the ranges of 1.0≦x≦1.30, 0.1≦y<0.95, 0.01<z≦0.5, 0.01<w≦0.5, 0≦v≦0.2, and 1.5≦u≦4.5, respectively.
11. 10. The positive electrode for a lithium secondary battery according to claim 9, wherein the first conductive material and the second conductive material each include at least one selected from the group consisting of natural graphite, artificial graphite, carbon black, acetylene black, ketjen black, carbon nanotubes, graphene, and carbon fibers.
12. 10. The positive electrode for a lithium secondary battery according to claim 9, wherein the content of the first conductive material and the content of the second conductive material are 0.5 to 5 parts by weight per 100 parts by weight of each mixture layer.
13. forming a first mixture layer containing a first binder made of a rubber-based resin on a positive electrode current collector; forming a second mixture layer on the first mixture layer, the second mixture layer including a second binder composed of a fluorine-based resin derived from a fluorine (F)-containing monomer; At least the first mixture layer of the first mixture layer and the second mixture layer contains a positive electrode additive represented by the following chemical formula 1, [Chemical formula 1] Li p Co (1-q) M 1 q O 4 In the above Chemical Formula 1, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; p and q are 5≦p≦7 and 0≦q≦0.5, respectively; The step of forming the first composite layer includes: preparing a composite composition by dry-mixing a first positive electrode active material, a positive electrode additive represented by Chemical Formula 1, a first conductive material, and a first binder including a rubber-based resin; The method for manufacturing a positive electrode for a lithium secondary battery includes the step of coating the prepared composite composition on a positive electrode current collector.
Citation Information
Patent Citations
Nonaqueous secondary battery
JP1992332480A
Electrode for nonaqueous electrolyte secondary battery and its manufacture
JP1997185960A
Nonaqueous electrolyte battery
JP2002056896A
Nonaqueous secondary battery and its manufacturing method
JP2003163006A
Power storage device
JP2015088268A