Curable composition comprising an ethylene polymer, a monoperoxycarbonate, and a t-alkyl hydroperoxide

A curable ethylene polymer composition with a controlled monoperoxycarbonate and t-alkyl hydroperoxide ratio prevents scorching during extrusion, ensuring uniformity and high crosslinking density for solar panel encapsulants.

JP7570810B2Active Publication Date: 2024-10-22ARKEMA FRANCE SA
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2019513374
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2017-09-08
Publication Date
2024-10-22
Estimated Expiration
2037-09-08

AI Technical Summary

Technical Problem

Ethylene/vinyl acetate (EVA) compositions used in solar panels are prone to premature crosslinking in extruders, leading to uneven products and process interruptions, which is not adequately addressed by existing solutions that either slow down crosslinking rates or cause undesirable yellowing.

Method used

A curable composition comprising ethylene polymers with a specific weight ratio of monoperoxycarbonate to t-alkyl hydroperoxide, within the range of 0.4-4%, effectively prevents scorching during extrusion while maintaining high crosslinking rates and densities.

Benefits of technology

The composition allows for high-speed extrusion of ethylene polymers without scorching, resulting in uniform films with no air bubbles and improved crosslinking density, suitable for encapsulating materials in solar panels.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570810000001
    Figure 0007570810000001
  • Figure 0007570810000002
    Figure 0007570810000002
  • Figure 0007570810000003
    Figure 0007570810000003
Patent Text Reader

Abstract

The present invention relates to a curable composition comprising (a) at least one ethylene polymer, (b) up to 2 parts by weight of at least one monoperoxycarbonate per 100 parts by weight of component (a), and (c) from 0.4 to 4 parts by weight of at least one t-alkyl hydroperoxide per 100 parts by weight of component (b). The present invention also relates to a method for preventing scorch in a curable composition comprising an ethylene polymer by adding a specific amount of t-alkyl hydroperoxide, and a method for producing a material protected from scorch.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to curable compositions containing ethylene polymers, such as ethylene / vinyl acetate copolymers, and further to a method for preventing scorching of curable compositions containing such ethylene polymers. [Background technology]

[0002] Ethylene / vinyl acetate (EVA) is a widely used copolymer, particularly in solar panels, as an encapsulant and electrical insulator to protect the solar cells (and especially the semiconductors contained within them) from outdoor environmental elements, especially moisture and UV radiation. EVA has good transparency, excellent adhesion to the substrates of photovoltaic (PV) modules, high resistivity and excellent moisture barrier properties. These properties can also be used in the manufacture of laminated glass.

[0003] To improve the thermal stability of EVA copolymers, especially creep strength, adhesion to substrates and weathering resistance, EVA copolymers are generally crosslinked. For this purpose, various crosslinking agents are used in the manufacture of EVA. These crosslinking agents are generally peroxides, such as dicumyl peroxide (DCP), peroxyesters, peroxyketals, peroxycarbonates and mixtures thereof. An example of a monoperoxycarbonate used for this purpose is OO-t-butyl-O-2-ethylhexyl-monoperoxycarbonate (TBEC). This peroxide has a lower crosslinking temperature than DCP and has been shown to produce products that do not yellow, and is used in the manufacture of photovoltaic modules (see K. Thaworn et al, Open Journal of Polymer Chemistry, 2012, 2, 77-85).

[0004] The applicant has shown that the addition of OO-t-amyl-O-2-ethylhexyl monoperoxycarbonate (TAEC) to TBEC can shorten the reaction time and improve the crosslink density of EVA, thereby increasing the tensile strength and high modulus of products made from the crosslinked EVA (Patent Document 1 (International Publication No. WO2010 / 007315, Parflet)).

[0005] In the lamination process of a PV module, the EVA composition is first coated on a front sheet, the solar cells are placed on it, coated on top again, and then a back sheet is attached to form a PV module, which is heated at a predetermined elevated temperature under pressure for a predetermined time to cure the EVA composition.

[0006] It has been found that EVA compositions are prone to premature crosslinking in the barrel or head die of the extruder in which they are processed before forming the laminate. This phenomenon is called "burning" and makes the formed EVA sheet non-uniform, impairing the appearance and properties of the PV module. It may also cause the pressure in the extruder to increase, making it necessary to interrupt the extrusion process. This is particularly observed when the EVA has a relatively low melt flow index and / or a relatively narrow molecular weight distribution (US Pat. No. 4,015,058). However, on the other hand, in order to achieve commercially viable processing speeds, it is also necessary to heat the molded EVA sheet above the thermal decomposition temperature of the peroxide and crosslink as quickly as possible to improve the economy of the process and minimize side reactions.

[0007] This premature crosslinking phenomenon has also been observed when polyolefin elastomer (POE) was used instead of EVA.

[0008] Various solutions have been proposed to prevent scorching of EVA compositions. For example, it has been proposed to add a polymerization inhibitor to the EVA composition, but this leads to undesirable yellowing. [Patent Document 2] (US Pat. No. 4,015,058) proposes adding at least 1% by weight of cumene hydroperoxide and / or tert-butyl hydroperoxide to dicumyl peroxide (DCP). However, in the manufacture of PV modules, the crosslinking rate obtained with this system is not fast enough for industrial applications due to the presence of DCP. Also, the problem of yellowing due to the aromatic structure of DCP remains.

[0009] Another solution is presented in [Patent Document 3] (JP 2011-140588 A) which is described as being suitable for the manufacture of PV modules. In this patent, 4 to 50 parts by weight of a hydroperoxide, for example t-butyl hydroperoxide, are added for 100 parts by weight of an organic peroxide selected from monoperoxycarbonate, dialkyl peroxide, peroxyketals and peroxyesters. Although this solution makes it possible to overcome the drawbacks associated with the use of DCP, it can be seen from [Patent Document 3] (JP 2011-140588 A) that said amount of hydroperoxide has a negative effect on the crosslink density of EVA. In this regard, this patent proposes to increase the total amount of monoperoxycarbonate and peroxide while keeping the ratio of hydroperoxide to monoperoxycarbonate constant, i.e. around 20% (see Table 1). [Prior art documents] [Patent documents]

[0010] [Patent Document 1] International Publication No. WO2010 / 007315 [Patent Document 2] US Pat. No. 4,015,058 [Patent Document 3] JP 2011-140588 A [Non-patent literature]

[0011] [Non-Patent Document 1] K. Thaworn et al, Open Journal of Polymer Chemistry, 2012, 2, 77-85 Summary of the Invention [Problem to be solved by the invention]

[0012] Surprisingly, the inventors have found that the crosslink density of EVA or POE can be improved by controlling the weight ratio of hydroperoxide to monoperoxycarbonate within a specific range, i.e., 0.4 to 4% by weight or less. Furthermore, contrary to what would be expected from the description in [Patent Document 3] (JP Patent Publication 2011-140588), the inventors have found that the scorch prevention effect of hydroperoxide is significantly increased at the above-mentioned low weight ratio, even if the amount of crosslinker is reduced, without impairing the rate of the crosslinking reaction. Moreover, it has been observed that a sufficient film (film formation) uniformity is obtained, and it is practically bubble-free. In this regard, it is important to note that at extrusion temperatures above 100°C, the encapsulated water in the film evaporates, causing bubbles, which become surface defects and adversely affect the resistivity of the formed film. This phenomenon is particularly detrimental when the film is used as an encapsulant for PV modules.

[0013] Thus, the present invention allows compositions containing ethylene polymers such as EVA and the peroxides described above to be processed in an extruder at high output speeds without scorching.

[0014] It should further be noted that monoperoxycarbonates are also useful for crosslinking other ethylene polymers, such as polyolefin elastomers, such as polydiene elastomers, including ethylene-propylene-diene (EPDM) elastomers, and polyethylene, including low and high density polyethylene. These materials are used in the manufacture of wire and cable insulation, pipes and hoses (including, for example, automobile radiators, drinking water and underfloor heating pipes), roller covers, rotational molded articles and foamed articles. Thus, the compositions of the present invention are useful for preventing scorching in applications where the compositions are extruded as insulating coatings on electrical conductors. [Means for solving the problem]

[0015] Specifically, the present invention relates to a curable composition comprising: (a) at least one ethylene polymer; (b) up to 2 parts by weight per 100 parts by weight of component (a) of at least one monoperoxycarbonate; (c) 0.4 to 4 parts by weight or less per 100 parts by weight of component (b) of at least one t-alkyl hydroperoxide. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] The ethylene polymers used as component (a) in the present invention are homopolymers of ethylene or copolymers of ethylene, preferably copolymers of ethylene. For example, ethylene copolymers are composed of ethylene monomers and at least one other monomer, which is selected from hydrocarbons having at least one unsaturated group, such as methylene, propylene, butene, pentene, hexene, heptene, octene, butadiene, isoprene and styrene; acrylic monomers, such as acrylic acid, methacrylic acid, alkyl methacrylates and alkyl acrylates, the alkyl group being selected from, for example, methyl, ethyl, propyl or butyl; vinyl monomers, such as vinyl acetate. Generally, these copolymers contain at least 30% by weight of ethylene and up to 70% by weight of other monomers.

[0017] In a preferred embodiment, the ethylene-based copolymer is an ethylene / vinyl acetate (EVA) copolymer. The EVA copolymer may contain 15-60% by weight, preferably 25-45% by weight, of vinyl acetate (VA) monomer. Examples of EVA copolymers are available from ARKEMA under the trade names "EVATANE® 18-150" and "EVATANE® 40-55".

[0018] Other ethylene polymers that can be used in the present invention are disclosed, for example, in [Patent Document 4]. [Patent Document 4] These ethylene polymers consist of functionalized polyolefins, which may be homopolymers of ethylene or copolymers of ethylene with alkyl (meth)acrylates or vinyl acetates, functionalized by grafting or copolymerization with maleic anhydride or glycidyl methacrylate, which may optionally be mixed with ethylene / vinyl carboxylate copolymers, such as EVA.

[0019] In a preferred embodiment, the ethylene polymers of the present invention are polyolefin elastomers.

[0020] A "polyolefin" is a polymer derived from an olefin, such as ethylene, propylene, butene, hexene, octene. "Derived from" means that the units in the polymer backbone and / or in the polymer branches are the result of polymerization or copolymerization of the monomers from which the polymer is made. Preferably, the polyolefin is a polyolefin elastomer.

[0021] The term "polyolefin elastomer" (POE) means an elastomeric polymer derived from olefins such as ethylene, propylene, butene, hexene, and octene.

[0022] "Elastomer" means a polymer that is capable of uniaxial deformation at ambient temperature, preferably of at least 20% uniaxial deformation in 15 minutes, and of recovering its original dimensions after removal of the stress, preferably with a residual deformation of no more than 5% of its original dimensions.

[0023] It is preferred that the α-olefin content of the polyolefin elastomer is at least 15% by weight, preferably at least 20% by weight, and even more preferably at least 25% by weight of the polymer.

[0024] It is preferred that the α-olefin content of the polyolefin elastomer be no more than 50% by weight of the polymer, preferably no more than 45%, more preferably no more than 40%, and even more preferably no more than 35%.

[0025] The alpha-olefin content was determined according to Randall (Rev. Macromol Chem. Phys., C29 (2 and 3)). 13 It can be measured by C nuclear magnetic resonance (NMR) spectroscopy.

[0026] The α-olefin is preferably a linear, branched or cyclic α-olefin having 3 to 20 carbon atoms.

[0027] Examples of α-olefins having 3 to 20 carbon atoms include propene, 1-butene, 4-methyl-1-pentene, 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, 1-hexadecene, and 1-octadecene. The α-olefins can contain a cyclic structure, such as cyclohexane or cyclopentane, and can be α-olefins such as 3-cyclohexyl-1-propene (allylcyclohexane) and vinylcyclohexane.

[0028] For purposes of this invention, some cyclic olefins, such as norbornene and related olefins, can be considered α-olefins and can be used in place of some or all of the above α-olefins.

[0029] Polyolefin elastomers include ethylene / propylene, ethylene / 1-butene, ethylene / 1-hexene, and in particular very low density polyethylene (VLDPE) (e.g., FLEXOMER® ethylene / 1-hexene polyethylene from Dow Chemical Company), ethylene / 1-octene, ethylene / styrene, ethylene / propylene / 1-octene, ethylene / propylene / 1-butene, ethylene / 1-butene / 1-octene, and ethylene / 1-butene / styrene.

[0030] More preferred polyolefin copolymers are the homogeneously branched linear and substantially linear ethylene copolymers. Substantially linear ethylene copolymers are especially preferred and are described in the following patents: US Pat. [Patent Document 5] U.S. Pat. No. 5,272,236 [Patent Document 6] U.S. Patent No. 5,278,272 [Patent Document 7] U.S. Pat. No. 5,986,028

[0031] Examples of homogeneously branched linear ethylene / α-olefin copolymers are TAFMER® from Mitsui Petrochemical Co., Ltd., EXACT® from Exxon Chemical Company, AFFINITY® and ENGAGE® from Dow Chemical Company.

[0032] The polyolefin elastomers of the present invention include copolymers based on propylene, 1-butene and other alkenes, such as copolymers containing a majority of units derived from propylene with minority units derived from other alpha-olefins, including ethylene. Exemplary polypropylenes useful in the practice of the present invention include VERSIFY® polymers available from The Dow Chemical Company and VISTAMAXX® polymers available from Exxon Mobil Chemical Company.

[0033] The polyolefin elastomer of the present invention has a glass transition temperature (Tg) of -35°C or less, preferably -40°C or less, more preferably -45°C or less, and even more preferably -50°C or less, as measured by differential scanning calorimetry (DSC) according to the procedure of ASTM standard D-3418-03.

[0034] The melt index (MI (190°C / 2.16 kg) of the polyolefin elastomer of the present invention, measured according to the procedure of ASTM standard D-1238, is 100 g / 10 min or less, preferably 75 g / 10 min or less, more preferably 50 g / 10 min or less, and even more preferably 35 g / 10 min or less.

[0035] The polyolefin elastomers of the present invention have a melt index of at least 1 g / 10 min, preferably at least 5 g / 10 min.

[0036] The density of the polyolefin elastomers of the present invention is 0.90 g / cc or less, preferably 0.89 g / cc or less, more preferably 0.885 g / cc or less, even more preferably 0.88 g / cc or less, and even more preferably 0.875 g / cc or less.

[0037] The density of the polyolefin elastomer of the present invention is 0.85 g / cc or more, more preferably 0.86 g / cc or more.

[0038] The density is preferably measured according to the procedure of ASTM standard D-792.

[0039] The ethylene polymer is mixed with at least one monoperoxycarbonate. This peroxide compound can be an OO-t-alkyl-O-alkyl monoperoxycarbonate, preferably selected from the group consisting of OO-t-butyl-O-2-ethylhexyl monoperoxycarbonate (TBEC), OO-t-butyl-O-2-isopropyl monoperoxycarbonate (TBIC), OO-t-amyl-O-2-ethylhexyl monoperoxycarbonate (TAEC), OO-t-amyl-O-2-isopropyl monoperoxycarbonate (TAIC) and mixtures thereof. These monoperoxycarbonates are commercially available from the company ARKEMA under the trade name Luperox® or Lupersol®.

[0040] Preferred monoperoxycarbonates are TAEC, TBEC and mixtures thereof, and mixtures of TAEC and TAIC. More preferred monoperoxycarbonates are TAEC and TBEC. In an embodiment of the present invention, a mixture of TBEC and TAEC is used as component (b).

[0041] When a mixture of O,O-tert-butyl-O-(2-ethylhexyl) monoperoxycarbonate (TBEC) and O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) is used, the mass ratio of O,O-tert-butyl-O-(2-ethylhexyl) monoperoxycarbonate (TBEC) to O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) is preferably 0.1:99 to 60:40, preferably 1:99.9 to 50:50, more preferably 10:90 to 30:70, more preferably 15:85 to 25:75, and more preferably about 20:80. Alternatively, the ratio can be about 50:50.

[0042] When a mixture of O,O-tert-amyl-O-2-isopropyl monoperoxycarbonate (TAIC) and O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) is used, the mass ratio of O,O-tert-amyl-O-2-isopropyl monoperoxycarbonate (TAIC) to O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) is preferably in the range of 20:80 to 99:1, preferably 30:70 to 80:20, more preferably 50:50 to 70:30, even more preferably 55:45 to 65:35, and even more preferably about 60:40. Alternatively, the ratio can be about 50:50.

[0043] The amount of component (b) in the composition of the present invention is in the range of 0.1 to 2 parts by weight or less, preferably 0.2 to 1.5 parts by weight, more preferably 0.3 to 1 part by weight, more preferably 0.4 to 1 part by weight, more preferably 0.4 to 0.7 parts by weight, and even more preferably about 0.5 parts by weight, per 100 parts by weight of component (a).

[0044] The third component (c) of the composition of the present invention is a t-alkyl hydroperoxide which may be selected from the group consisting of t-butyl hydroperoxide (TBHP), t-amyl hydroperoxide (TAHP), t-hexyl hydroperoxide (THHP), 1,1,3,3-tetramethylbutyl hydroperoxide (TOHP), perhydroperoxide (PMHP), 2,5-dimethyl-2,5-dihydroperoxide (2,5 to 2,5) and mixtures thereof. Preferably, the t-alkyl hydroperoxide is TAHP.

[0045] The amount of component (c) in the composition of the present invention is in the range of 0.4 to 4 parts by weight, preferably 0.5 to 3.5 parts by weight, preferably 0.5 to 3 parts by weight, preferably 0.5 to 2 parts by weight, and even more preferably about 1 part by weight of at least one t-alkyl hydroperoxide, per 100 parts by weight of component (b).

[0046] The compositions of the present invention may further include a coagent that is not an organic peroxide.

[0047] Advantageously, the coagent contains at least one carbamate, maleimide, acrylate, methacrylate or allyl functional group. Allyl carboxylates can also be used, which can be selected from the group of the allyl, diallyl and triallyl types.

[0048] The above auxiliary agents include divinylbenzene, diisopropenylbenzene, α-methylstyrene, α-methylstyrene dimer, ethylene glycol dimethacrylate, phenylene dimethacrylate, diethylene glycol dimethacrylate, triethylene glycol dimethacrylate, tetraethylene glycol dimethacrylate, polyethylene glycol 200 dimethacrylate, polyethylene glycol 400 dimethacrylate, 1,3-butanediol dimethacrylate, 1,4-butanediol dimethacrylate, 1,6-hexanediol dimethacrylate, 1,12-dodecanediol dimethacrylate, 1,3-glycerol dimethacrylate, diurethane methacrylate, trimethylolpropane trimethacrylate, bisphenol A epoxy diacrylate, dipropylene glycol diacrylate, tripropylene glycol diacrylate, polyethylene glycol 600 diacrylate, acrylate, ethylene glycol diacrylate, diethylene glycol diacrylate, triethylene glycol diacrylate, tetraethylene glycol diacrylate, neopentyl glycol ethoxylate diacrylate, butanediol diacrylate, hexanediol diacrylate, aliphatic urethane diacrylate, trimethylolpropane triacrylate, trimethylolpropane ethoxylate triacrylate, trimethylolpropane propoxylate triacrylate, glycerol propoxylate triacrylate, aliphatic urethane triacrylate, trimethylolpropane triacrylate, dipentaerythritol pentaacrylate, triallyl cyanurate (TAC), triallyl isocyanurate (TAIC), N,N'-phenylenedimaleimide, butadiene, chloroprene and isoprene.

[0049] More preferably, the coagent is selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, N,N'-m-phenylenedimaleimide, triallyl trimellitate, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate, preferably from the group consisting of triallyl cyanurate (TAC), triallyl isocyanurate (TAIC), trimethylolpropane triacrylate (TMPTA) and trimethylolpropane trimethacrylate (TMPTMA), even more preferably trimethylolpropane triacrylate (TMPTA).

[0050] The above auxiliaries may be present in an amount of from 0.05% to 30% by weight, preferably from 0.1 to 10% by weight, based on the total weight of the composition.

[0051] The main purpose of using the co-agent in the composition of the present invention is to increase the crosslinking level, which can also reduce the emission of residual gas during the decomposition of the same peroxide, ultimately reducing the number of bubbles in the sealing film.

[0052] The mass ratio of the auxiliary to the organic peroxide is in the range of 1:10 to 10:1, preferably 1:3 to 3:1.

[0053] The composition of the present invention may further comprise additives such as coupling agents, UV stabilizers, UV absorbers, fillers, plasticizers, flame retardants, antioxidants, dyes and mixtures thereof. Examples of coupling agents are monoalkyl titanates, (vinyl)trichlorosilanes and (vinyl)trialkoxysilanes, which may be present in a proportion of 0.01-5% by weight relative to the weight of the ethylene polymer. The UV absorbers may be selected from hindered amine light stabilizers (HALS), and the UV stabilizers may be selected from, for example, benzophenones, triazines and benzotriazoles. These compounds may be present in a proportion of 0.01-3% by weight relative to the weight of the ethylene polymer. Inorganic fillers may be added to increase the mechanical strength, such as silicon dioxide, alumina, talc, calcium carbonate. Nanometric clays are preferably added to improve transparency. Examples of plasticizers are peraffinic or aromatic mineral oils, phthalates, azelaic acid, adipic acid, etc. Examples of antioxidants are phenolic, phosphorus or sulfur antioxidants. Alternatively, quinolines such as 1,2-dihydro-2,2,4-trimethylquinoline can be used as antioxidants.

[0054] In a preferred embodiment of the present invention, the composition does not contain an aromatic peroxide, such as dicumyl peroxide.

[0055] In a preferred embodiment of the invention, the composition does not contain any peroxide other than the at least one monoperoxycarbonate (b) and the at least one t-alkyl hydroperoxide (c).

[0056] In a preferred embodiment of the invention, the total amount of peroxide in the composition is no more than 2 parts by weight per 100 parts by weight of component (a), more preferably no more than 1.5 parts by weight per 100 parts by weight of component (a).

[0057] More preferably, the composition of the present invention comprises components (a), (b) and (c) above, and optionally at least one of the following additives: coupling agents, UV stabilizers, UV absorbers, fillers, plasticizers, flame retardants, antioxidants, dyes, auxiliaries and mixtures thereof.

[0058] In another aspect, the present invention also relates to a process for the preparation of the composition defined above, which comprises the step of mixing components (a), (b) and (c) as defined above, which is advantageously carried out in conventional equipment, such as continuous mixers and extruders, preferably at a temperature below the decomposition temperature of the peroxide of the present invention.

[0059] The present invention further relates to the use of a t-alkyl hydroperoxide to inhibit scorch in a curable composition comprising (a) at least one ethylene polymer and (b) at least one monoperoxycarbonate, in which the amount of t-alkyl hydroperoxide is 0.4 to 4 parts by weight or less per 100 parts by weight of component (b), and preferably 0.5 to 3.5 parts by weight, preferably 0.5 to 3 parts by weight, more preferably 0.5 to 2 parts by weight, and even more preferably about 1 part by weight of component (c) per 100 parts by weight of component (b).

[0060] The present invention further relates to a method for preventing scorch in a curable composition comprising (a) at least one ethylene polymer and (b) at least one monoperoxycarbonate, the method comprising the step of adding to the composition at least one tertiary alkyl hydroperoxide in a ratio of from 0.4 to 4 parts by weight or less, preferably from 0.5 to 3.5 parts by weight, preferably from 0.5 to 3 parts by weight, more preferably from 0.5 to 2 parts by weight, per 100 parts by weight of portion (b), and even more preferably about 1 part by weight of at least one tertiary alkyl hydroperoxide.

[0061] In another aspect, the present invention also relates to a method for the preparation of a scorch protection material comprising an ethylene polymer, in particular selected from the group consisting of encapsulants or sealants, especially solar cell encapsulants or sealants, wire and cable insulation, pipes and hoses (including e.g. automotive radiator lines, drinking water and underfloor heating), roller coverings, rotational mouldings and foamed products, which method comprises a step (a) as defined above of curing the composition. Preferably, the scorch protection material is a solar cell encapsulant or sealant.

[0062] Preferably, said step (a) of curing the composition is a lamination step.

[0063] Step (a) is preferably carried out at a temperature of 130 to 180°C, more preferably at a temperature of 140 to 165°C.

[0064] Step (a) preferably lasts for 6 to 25 minutes, more preferably 4 to 30 minutes, or alternatively step (a) may last for 6 to 25 minutes, more preferably 8 to 30 minutes.

[0065] The method of the present invention preferably further comprises a pre- and / or simultaneous step (a') selected from the group consisting of molding, extrusion and injection molding of the composition as defined above. In case the product is an encapsulant or sealant for solar cells, said step (a') is preferably an extrusion step.

[0066] Step (a') can be carried out in such a way that a sheet having a thickness of 50 to 2000 μm is obtained, preferably a sheet having a thickness of, for example, 100 to 1000 μm.

[0067] Step (a') can be carried out using a T-die extruder or a twin-screw extruder in combination with a two-roll mill.

[0068] The step (a') is preferably carried out at a temperature of 80 to 150°C, preferably 90 to 120°C.

[0069] Preferably, no crosslinking takes place during step (a').

[0070] In certain embodiments, steps (a') and (a) are carried out in a single step.

[0071] In another embodiment, the present invention relates to a method for producing a solar cell module, the method comprising the steps of pressing a laminate of the following (1) to (5): (1) A front sheet (e.g., a glass plate or a PMMA sheet), (2) Composition of the Present Invention Includes Seat, (3) at least one solar cell (preferably made of crystalline silicon or organic solar cells); Made ), (4) Composition of the Present Invention Includes Another sheet, (5) A backsheet (such as a multilayer PVDF / PET film or a glass plate or a PMMA sheet).

[0072] The laminate is then heated and / or pressed under vacuum according to conventional techniques, for example at a temperature of 130-180°C, preferably 140-165°C, under vacuum. The curing time may range from 4 to 30 minutes, for example 6 to 25 minutes. Alternatively, step (a) may last from 8 to 30 minutes, more preferably 6 to 25 minutes. The composition according to the invention may be crosslinked during this pressing step. The method according to the invention preferably involves pressing and curing in a single simultaneous step.

[0073] In another aspect, the present invention also relates to a scorch protection material comprising an ethylene polymer obtainable by the process defined above.

[0074] The scorch protection material comprising an ethylene polymer is preferably selected from the group consisting of encapsulants or sealants, especially solar cell encapsulants or sealants, wire and cable insulation, pipes and hoses (including, for example, pipes for automobile radiators, drinking water and underfloor heating), roller coatings, rotational moldings and foam products.

[0075] More preferably, the scorch protection material comprising an ethylene polymer is a film, preferably an EVA film, more preferably an encapsulant or sealant, even more preferably a solar cell encapsulant or sealant.

[0076] The scorch protection material of the present invention, which includes an ethylene polymer, can improve the crosslink density of the ethylene polymer and eliminate or significantly reduce the scorch problem, thereby resulting in a film that is free of surface defects and has excellent resistance.

[0077] In yet another aspect, the present invention also relates to a solar cell module comprising a scorch protection material as defined above, preferably a solar cell encapsulant material.

[0078] The present invention may be better understood by reference to the following examples, which are intended for illustrative purposes only and are not intended to limit the scope of the invention, the scope of which is defined by the claims. EXAMPLES

[0079] Example 1 Scorch prevention effect The composition of the present invention was prepared by mixing ethylene / vinyl acetate (EVA) copolymer (Cosmothene® EVA KA-40, supplied by Sumitomo, containing 28% VA) with OO-t-amyl-O-2-ethylhexyl monoperoxycarbonate (Luperox® TAEC, available from Arkema) and t-amyl hydroperoxide (Luperox® TAHP, available from Arkema) in a Haake internal mixer at a stirring speed of 50 revolutions per minute at 35° C. for 12 minutes. The polymer mixture was then passed through an open mill set at 60° C. to produce sheets of approximately 2 mm thickness.

[0080] Approximately 2-3 g samples of the above compositions were placed on the plate of a GOTECH moving die rheometer (MDR), which contains software capable of measuring the cure characteristics of the samples and analyzing the results. Each sample was placed in a temperature-controlled cavity between two dies, the lower die oscillating to subject the sample to repeated stress or strain, while the upper die was connected to a torque sensor to measure the deformation torque response of the sample. Stiffness was continuously recorded as a function of time. The stiffness of the sample increased as the vulcanization (curing) process progressed.

[0081] This device in particular gives calculated values ​​for ML (minimum torque), MH (maximum torque), tc10 (time to 10% cure) and tc90 (time to 90% cure) as defined in international standards (ASTM standard D5289 and ISO standard 6502).

[0082] The MDR involves subjecting the samples to a vibration amplitude (degree of deformation) of 0.5° for 30 minutes at 115°C and 145°C. The scorch time is defined as the time required to reach 10% of the total cure, i.e. tc10.

[0083] Experiments were carried out on the following samples, the amount of monoperoxycarbonate expressed in parts by weight per 100 parts by weight of EVA resin (PHR) and the amount of TAHP expressed in parts by weight per 100 parts by weight of monoperoxycarbonate:

[0084] [Table 1]

[0085] From Table 1, it can be seen that TAHP acts as a scorch inhibitor, since the scorch time (tc10) increases with the amount of TAHP. When the amount of TAHP is below 0.4 wt% with respect to TAEC, crosslinking undesirably starts at 115°C (see MH value). However, the crosslinking time (tc90) increases dramatically, and therefore the crosslinking rate is slow, and the crosslink density (MH) is also low when the amount of TAHP is 4 wt% with respect to TAEC. When the amount of TAHP is below 4 wt% with respect to TAEC, scorch can be effectively prevented while maintaining a good crosslinking rate (tc90), and the crosslink density (MH-ML) is also good.

[0086] Example 2 This experiment was carried out under the same conditions as in Example 1, except that a mixture of 20% O,O-tert-butyl-O-(2-ethylhexyl) monoperoxycarbonate (TBEC) and 80% O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) was used instead of TAEC alone. The results are shown in Table 2.

[0087] [Table 2]

[0088] Similar to Example 1, the crosslinking time (tc90) increases dramatically when the latter reaches 4 wt % relative to TAEC+TBEC.

[0089] Example 3 This experiment was also carried out under the same conditions as in Example 1, but instead of TAEC alone, a mixture of 50% O,O-tert-butyl-O-(2-ethylhexyl) monoperoxycarbonate (TBEC) and 50% O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) was used. The results are shown in Table 3.

[0090] [Table 3]

[0091] Similar to the previous example, the crosslinking time increases dramatically (tc90) when the latter reaches 4 wt % relative to TAEC+TBEC.

[0092] Example 4 This experiment was carried out under the same conditions as in Example 1, except that LUP® TBHP (t-butyl hydroperoxide) was used instead of TAHP. The results are shown in Table 4.

[0093] [Table 4]

[0094] Similar to the previous example, the crosslinking time (tc90) increases dramatically when the latter reaches 4 wt % relative to TAEC.

[0095] Example 5 This experiment was carried out under the same conditions as in Example 4, but instead of TAEC, a mixture of 20% O,O-tert-butyl-O-(2-ethylhexyl) monoperoxycarbonate (TBEC) and 80% O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) was used. The results are shown in Table 5.

[0096] [Table 5]

[0097] Similar to the previous example, the crosslinking time increases dramatically (tc90) when the latter reaches 4 wt % relative to TAEC+TBEC.

[0098] Example 6 This experiment was also carried out under the same conditions as in Example 4, but instead of TAEC, a mixture of 50% O,O-tert-butyl-O-(2-ethylhexyl) monoperoxycarbonate (TBEC) and 50% O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) was used alone. The results are shown in Table 6.

[0099] [Table 6]

[0100] Similar to the previous example, the crosslinking time increases dramatically (tc90) when the latter reaches 4 wt % relative to TAEC+TBEC.

[0101] Example 7 This experiment was carried out under the same conditions as in Example 1, but 0-t-amyl-O-2-isopropyl monoperoxycarbonate (TAIC) was used instead of TAEC. The results are shown in Table 7.

[0102] [Table 7]

[0103] From Table 7, it can be seen that by adding at least 0.4 wt% TAHP to TAEC, scorch can be effectively prevented and a high crosslinking rate (tc90) and good crosslinking density (MH-ML) can be maintained.

[0104] Example 8 The experiment was carried out under the same conditions as in Example 1, but instead of TAEC alone, a mixture of 60% O,Ot-amyl-O-2-isopropyl monoperoxycarbonate (TAIC) and 40% O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) was used. The results are shown in Table 8.

[0105] [Table 8] As can be seen from Table 8, the addition of at least 0.4 wt% TAHP to TAIC can effectively prevent scorch and maintain a high crosslinking rate (tc90) and good crosslinking density (MH-ML).

[0106] Example 9 This experiment was carried out under the same conditions as in Example 1, but a polyolefin elastomer (KJ640T27255C from JAPAN POLYETHYLENE CORPORATION) was used instead of EVA. The results are shown in Table 9.

[0107] [Table 9]

[0108] From Table 9, it can be seen that by adding at least 0.4 wt% TAHP to TAEC, scorch can be effectively prevented, and at the same time, a high crosslinking rate (tc90) and good crosslinking density (MH-ML) can be maintained.

[0109] Example 10 This experiment was carried out under the same conditions as in Example 9, except that O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TBEC) was used instead of O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC). The results are shown in Table 10.

[0110] [Table 10]

[0111] From Table 10, it can be seen that adding at least 0.4 wt% TBHP to TBEC can effectively prevent scorch while maintaining a high crosslinking rate (tc90) and good crosslinking density (MH-ML).

[0112] Example 11 This experiment was also carried out under the same conditions as in Example 9, except that O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAIC) was used instead of O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC). The results are shown in Table 11.

[0113] [Table 11]

[0114] From Table 11, it can be seen that by adding at least 0.4 wt% TAHP to TAIC, scorch can be effectively prevented and a high crosslinking rate (tc90) and good crosslinking density (MH-ML) can be maintained.

[0115] Example 12 This experiment was also carried out under the same conditions as in Example 9, except that O,O-tert-amyl-O-(2-ethylhexyl) monoperoxycarbonate (TAEC) was replaced by O,Ot-butyl-O-2-isopropyl monoperoxycarbonate (TBIC). The results are shown in Table 12.

[0116] [Table 12]

[0117] From Table 12, it can be seen that by adding at least 0.4 wt% TBHP to TBIC, scorch can be effectively prevented while maintaining a high crosslinking rate (tc90) and good crosslinking density (MH-ML).

Claims

1. (a) at least one ethylene polymer; (b) less than 2 parts by weight per 100 parts by weight of component (a) of at least one monoperoxycarbonate; (c) at least 0.4 parts by weight but less than 4 parts by weight of at least one t-alkyl hydroperoxide per 100 parts by weight of component (b); 1. A curable composition comprising:

2. The composition of claim 1 wherein the ethylene polymer is an ethylene / vinyl acetate copolymer.

3. The composition of claim 1 , wherein the ethylene polymer is a polyolefin elastomer.

4. The composition according to any one of claims 1 to 3, wherein the monoperoxycarbonate is an OO-t-alkyl-O-alkyl monoperoxycarbonate.

5. 5. The composition of claim 4, wherein the OO-t-alkyl-O-alkyl monoperoxycarbonate is selected from the group consisting of OO-t-butyl O-2-ethylhexyl monoperoxycarbonate (TBEC), OO-t-butyl O-2-isopropyl monoperoxycarbonate (TBIC), OO-t-amyl O-2-ethylhexyl monoperoxycarbonate (TAEC), OO-t-amyl O-2-isopropyl monoperoxycarbonate (TAIC) and mixtures thereof.

6. The composition according to any one of claims 1 to 5, wherein the monoperoxycarbonate is from 0.1 to less than 2 parts by weight per 100 parts by weight of component (a).

7. 7. The composition of any one of claims 1 to 6, wherein the t-alkyl hydroperoxide is selected from the group consisting of t-butyl hydroperoxide (TBHP), t-amyl hydroperoxide (TAHP), t-hexyl hydroperoxide (THHP), 1,1,3,3-tetramethylbutyl hydroperoxide (TOHP), paramethane hydroperoxide (PMHP), 2,5-dimethyl-2,5-dihydroperoxide (2,5-2,5) and mixtures thereof.

8. The composition according to any one of claims 1 to 7, comprising 0.5 to 3.5 parts by weight of component (c) per 100 parts by weight of component (b).

9. The composition according to claim 1, further comprising one auxiliary selected from the group consisting of triallyl cyanurate, triallyl isocyanurate, N,N'-m-phenylenedimaleimide, triallyl trimellitate, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.

10. 1. Use of a t-alkyl hydroperoxide to inhibit scorch in a curable composition comprising (a) at least one ethylene polymer and (b) less than 2 parts by weight of at least one monoperoxycarbonate per 100 parts by weight of component (a), wherein the t-alkyl hydroperoxide represents from 0.4 to less than 4 parts by weight per 100 parts by weight of (b).

11. 1. A method for preventing scorch in a curable composition comprising (a) at least one ethylene polymer and (b) less than 2 parts by weight per 100 parts by weight of component (a) of at least one monoperoxycarbonate, the method comprising the step of adding to said composition at least 0.4 parts by weight but less than 4 parts by weight per 100 parts by weight of (b) of at least one tertiary alkyl hydroperoxide.

12. A method for producing a scorch protected material comprising an ethylene polymer, the method comprising step (a) curing the composition of any one of claims 1 to 9.

13. The process according to claim 12, comprising a preceding and / or simultaneous step (a') selected from the group consisting of molding, extruding and injecting the composition according to any one of claims 1 to 9.

14. The process according to claim 13, wherein step (a') is carried out at a temperature of from 80 to 150°C.

Citation Information

Patent Citations

  • Ethylene-vinyl acetate copolymer composition and crosslinked product

    JP2011140588A

  • Sealing material for solar cell module

    JP2013170193A

  • US-4015058

  • Mixture of peroxides for crosslinking elastomers

    WO2010007315A2

  • Curable composition comprising an ethylene polymer, a monoperoxycarbonate and a t-alkyl hydroperoxide

    WO2016151385A1