Powder device component and manufacturing method thereof
The powder device member with a DLC film texture and ta-C coating addresses adhesion issues by enhancing surface adhesion prevention and maintaining structural integrity, achieving effective powder handling.
Patent Information
- Application Number
- JP2020174811
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-10-16
AI Technical Summary
Existing powder molding technologies face challenges in preventing adhesion of powder to contact surfaces, particularly at high molding pressures, where diamond-like carbon (DLC) films alone are insufficient.
A powder device member with a contact surface coated in a DLC film featuring a texture of grooves with an opening width smaller than the average powder particle diameter, formed using femtosecond laser processing, and a ta-C film applied via ion beam assisted filtered arc deposition (IBA-FAD) to enhance adhesion prevention.
Effectively prevents powder adhesion, reduces cleaning burden, and maintains surface integrity under pressure, with ta-C film exhibiting higher hardness, density, and wear resistance.
Smart Images

Figure 0007570881000003 
Figure 0007570881000004 
Figure 0007570881000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a powder device component and a method for making the same. [Background technology]
[0002] As one of the powder device members, a powder molding die used for compressing and molding powder is known. For example, Patent Document 1 discloses a powder molding die having a molding space formed by the inner peripheral surface of a rubber mold, the outer peripheral surface of a mandrel, and the outer surface of a bottom punch. The outermost surface of the mandrel is coated with a diamond carbon (DLC) film. This allows the mandrel to The adhesion of ceramic powder can be effectively prevented. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent No. 5147484 Summary of the Invention [Problem to be solved by the invention]
[0004] The above-mentioned Patent Document 1 describes the effect of suppressing adhesion in isostatic molding using a mandrel, particularly in cases where the molding pressure is as high as 200 MPa. Clay When handling DLC, if the molding pressure or pressure at which adhesion is attempted is low, the DLC film alone may not be sufficient to suppress adhesion.
[0005] The present invention has been made to solve the above problems, and has as its main object to effectively prevent the powder from adhering to the surface of a contact member that comes into contact with the powder. [Means for solving the problem]
[0006] The powder device member of the present invention is A powder device member that contacts and handles a powder, A contact member that contacts the powder; a DLC film covering a surface of the contact member; Equipped with the surface of the DLC film has a texture composed of a plurality of grooves; The opening width of the groove is smaller than the average particle size of the powder. It is something.
[0007] In this powder device member, the surface of the contact member that comes into contact with the powder is coated with a DLC film. The surface of the DLC film has a texture composed of a plurality of grooves, and the opening width of the groove is approximately the same as the interval between the banks that form the grooves and is smaller than the average particle size of the powder being handled. Therefore, it is possible to effectively prevent the powder from adhering to the surface of the DLC film. This reduces the burden of cleaning the DLC film, and prevents the powder adhering to the DLC film from peeling off, resulting in uneven products. The powder device member may be of either a dry or wet type.
[0008] The adhesion of powder is caused by the adhesive force between the particles constituting the powder and the powder contact surface of the powder processing device member that comes into contact with the powder. In dry compaction, the adhesive force depends on the surface energy, and in wet compaction, it is said to also depend on the meniscus force of the liquid.
[0009] In the powder device member of the present invention, the texture may be composed of striped grooves. The striped grooves can be formed relatively easily by femtosecond laser processing. Since the tops of the stripes are not flat, the opening width is the same as the period of the stripes.
[0010] In the powder device member of the present invention, the DLC film is preferably a tetrahedral amorphous carbon (ta-C) film. DLC films are classified into hydrogen-free DLC films and hydrogen-containing DLC films. Hydrogen-free DLC films exhibit higher values in hardness, density, heat resistance, and refractive index than hydrogen-containing DLC films. Therefore, hydrogen-free DLC films are preferred. Hydrogen-free DLC films are sp 3 Structure-rich ta-C film and sp 2 It is classified into ta-C film and amorphous carbon (aC) film, which has a rich structure. ta-C film has higher hardness, density, and heat resistance than aC film. In addition, ta-C film has lower adhesion, lower friction, and higher wear resistance than aC film.
[0011] In the powder device member of the present invention, the ta-C film may be doped with nitrogen atoms. A ta-C film having texture and doped with nitrogen atoms is less likely to have powder adhere thereto than a ta-C film having texture and not doped with nitrogen atoms. The doping amount of nitrogen atoms is not particularly limited, but may be, for example, in the range of 15 atm% or less.
[0012] In the powder device member of the present invention, the thickness of the ta-C film is preferably 500 nm or more, so that the texture is less likely to be destroyed when the contact member comes into contact with the powder.
[0013] The method for producing a powder device member of the present invention comprises the steps of: 1. A method of manufacturing a powder equipment component for contacting and manipulating a powder, comprising the steps of: (1) forming a texture on a surface of a contact member that comes into contact with the powder, the texture being composed of a plurality of grooves, the opening width of the grooves being smaller than an average particle size of the powder; (2) forming a DLC film on the surface of the contact member on which the texture is formed; or (1') forming a DLC film on a surface of a contact member that contacts the powder; (2') forming a texture on the surface of the DLC film, the texture being composed of a plurality of grooves, the opening width of the grooves being smaller than the average particle size of the powder; It includes.
[0014] In this manufacturing method, in steps (1) and (2'), the texture is preferably formed by, for example, mechanical processing or femtosecond laser processing, and more preferably by femtosecond laser processing. Femtosecond laser processing makes it easy to form a texture composed of grooves, particularly a texture composed of striped grooves of the same order of magnitude as the laser wavelength. In steps (2) and (1'), the DLC film is preferably formed by, for example, PVD or CVD, and more preferably by ion beam assisted filtered arc deposition (IBA-FAD), which is a type of PVD. IBA-FAD makes it possible to efficiently eliminate non-ionized carbon clusters and form a ta-C film that is hard and free of droplets or other adhering portions. In particular, in step (2), the DLC film is formed on a surface on which a texture composed of multiple grooves is formed, so there is a risk that the grooves will be filled during film formation, but IBA-FAD does not fill the grooves. [Brief description of the drawings]
[0015] [Figure 1] FIG. 2 is a plan view of a powder compacting die 10. [Diagram 2] Cross section AA of Figure 1 [Diagram 3] FIG. 2 is a cross-sectional view showing a state in which ceramic powder 50 is compression molded in a powder molding die 10. [Figure 4] FIG. 2 is a cross-sectional view for explaining an outline of a roll press machine 60. [Diagram 5] FIG. 1 is a schematic diagram of an IBA-FAD device 100. [Figure 6] SEM image of the surface of a ta-C film formed on a thin circular sheet. [Figure 7] Cross-sectional profile of a ta-C film formed on a thin circular sheet. [Figure 8] Schematic diagram of adhesion evaluation test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] A preferred embodiment of the present invention will be described below with reference to the drawings. In this embodiment, a powder molding die 10 will be described as an example of a powder device member of the present invention. FIG. 1 is a plan view of the powder molding die 10, and FIG. 2 is a cross-sectional view taken along line AA in FIG. 1. Note that the terms "upper", "lower", "left" and "right" used in the following description are terms that indicate relative positional relationships, not absolute positional relationships.
[0017] The powder molding die 10 is a die used in dry press molding, and includes a die 12, a lower punch 20, a lower sheet 26, an upper punch 30, and an upper sheet 36. The die 12, the lower punch 20, and the upper punch 30 are made of, for example, an iron-based material, graphite, boron nitride, or the like. As the iron-based material, SUS material, SKD material (die steel), SKH material (high speed steel), or the like is preferable. As the SUS material, for example, iron-chromium-based SUS410, SUS430, SUS440, or the like can be mentioned. As the SKD material, for example, SKD11, SKD61, or the like can be mentioned. As the SKH material, for example, SKH2, SKH10, SKH51, SKH55, or the like can be mentioned.
[0018] The die 12 is a thick-walled cylindrical member, and has a through hole 14 along the central axis. The die 12 is fixed onto a work table 40 by a support member (not shown).
[0019] The lower punch 20 has a lower circular plate 24 provided on the lower surface of a lower cylindrical body 22. The lower cylindrical body 22 has a two-stage structure consisting of a large diameter section 22a and a small diameter section 22b, and the large diameter section 22a is inserted into the through hole 14 of the die 12 from below. The lower circular plate 24 is integrated with the lower surface of the small diameter section 22b and is placed on a work table 40.
[0020] The lower sheet 26 is a release sheet, and is placed on the upper surface of the lower cylindrical body 22. The lower sheet 26 is formed by covering the upper surface of a thin circular sheet 27 with a coating film 28. The thin circular sheet 27 is made of the same material as the lower punch 20.
[0021] The upper punch 30 has an upper circular plate 34 provided on the upper surface of an upper cylindrical body 32. The upper cylindrical body 32 has a two-stage structure consisting of a large diameter section 32a and a small diameter section 32b, and the large diameter section 32a is inserted from above into the through hole 14 of the die 12. The upper circular plate 34 is integrated with the upper surface of the small diameter section 32b, and a downward load can be applied thereto by a pressurizer (not shown).
[0022] The upper sheet 36 is placed on the lower surface of the upper cylinder 32. The upper sheet 36 is a release sheet, and is formed by covering the lower surface of a thin circular sheet 37 with a coating film 38. The thin circular sheet 37 is made of the same material as the upper punch 30. The molding space between the lower sheet 26 and the upper sheet 36 is filled with ceramic powder 50 (see FIG. 3).
[0023] The coating films 28, 38 are ta-C films (a type of DLC film). The surface of the ta-C film (the surface that comes into contact with the ceramic powder 50) has a texture composed of a plurality of grooves, and the opening width of the grooves is smaller than the average particle size of the ceramic powder 50 to be molded. The plurality of grooves are formed in a striped pattern. The opening width of the grooves is not particularly limited, but is preferably, for example, 0.1 μm or more and 10 μm or less. The depth of the valley forming the groove is preferably 100 nm or more. The thickness of the ta-C film is preferably 500 nm or more. However, when the pressing force is low, it may be less than 500 nm. For example, when almost no pressing force is applied, it may be less than 200 nm.
[0024] Next, a description will be given of a method for manufacturing the lower sheet 26 used in the powder molding die 10 of this embodiment. Note that the method for manufacturing the upper sheet 36 is the same as the method for manufacturing the lower sheet 26, so the description will be omitted.
[0025] A first manufacturing example for manufacturing the lower sheet 26 will be described. First, a thin circular sheet 27 is prepared. Next, a texture consisting of a plurality of grooves (striped grooves) is formed on one side of the thin circular sheet 27. When forming the texture, the opening width of the groove is set to be smaller than the average particle diameter of the ceramic powder to be compression molded. The texture can be formed, for example, by mechanical processing or femtosecond laser processing, among which femtosecond laser processing is preferable. With femtosecond laser processing, striped grooves of the same order as the laser wavelength can be easily formed. Therefore, by setting the laser wavelength according to the opening width of the groove, the opening width of the groove can be controlled to a desired width. Next, a ta-C film is formed on the surface of the thin circular sheet 27 on which the texture is formed. The ta-C film can be formed, for example, by PVD or CVD, among which ion beam assisted filtered arc deposition (IBA-FAD), which is a type of PVD, is preferable. With IBA-FAD, non-ionized carbon clusters can be efficiently eliminated, and a ta-C film that is hard and free of adhesion portions such as droplets can be formed. In addition, IBA-FAD allows deposition without filling the grooves of the texture. This makes it possible to obtain a lower sheet 26 having a coating film 28 (a ta-C film having striped grooves on its surface) on one side of a thin circular sheet 27. IBA-FAD is also sometimes called FCVA.
[0026] A second manufacturing example for manufacturing the lower sheet 26 will be described. First, a thin circular sheet 27 is prepared. Next, a ta-C film is formed on one side of the thin circular sheet 27. The ta-C film can be formed by, for example, PVD or CVD. Next, a texture consisting of a plurality of grooves is formed on the surface of the ta-C film. When forming the texture, the opening width of the groove is set to be smaller than the average particle diameter of the ceramic powder to be compression molded. The texture can be formed by, for example, mechanical processing or femtosecond laser processing, among which femtosecond laser processing is preferable. With femtosecond laser processing, striped grooves of the same order as the laser wavelength can be easily formed. Therefore, by setting the laser wavelength according to the opening width of the groove, the opening width of the groove can be controlled to a desired width. As a result, a lower sheet 26 having a coating film 28 (a ta-C film having striped grooves on the surface) on one side of the thin circular sheet 27 can be obtained.
[0027] Next, an example of use of the powder molding die 10 of this embodiment will be described. FIG. 3 is a cross-sectional view showing a state in which ceramic powder 50 is compression molded by the powder molding die 10. First, the lower punch 20 is inserted from below into the through hole 14 of the die 12 of the powder molding die 10. Next, the lower sheet 26 is placed on the upper surface of the lower punch 20 with the coating film 28 facing up, and a predetermined amount of ceramic powder 50 is placed on top of it. The ceramic powder 50 has an average particle size larger than the opening width of the groove formed in the coating film 28. Next, the upper sheet 36 is placed on the ceramic powder 50 with the coating film 38 facing down, and the upper cylindrical body 32 of the upper punch 30 is inserted into the through hole 14 of the die 12 on top of it. As a result, the ceramic powder 50 is filled in the molding space between the coating film 28 of the lower sheet 26 and the coating film 38 of the upper sheet 36. In this state, a downward load is applied to the upper punch 30 by a pressurizer (not shown) to compress the ceramic powder 50 and obtain a compact of a predetermined shape. Thereafter, the powder compacting die 10 is disassembled and the compact is taken out.
[0028] The upper surface of the thin circular sheet 27 of the lower sheet 26 is covered with a coating film 28, and the lower surface of the thin circular sheet 37 of the upper sheet 36 is covered with a coating film 38. Therefore, it is the coating films 28, 38 that are in direct contact with the ceramic powder 50. The above-mentioned grooves are formed on the surfaces of the coating films 28, 38 (the surfaces that come into contact with the ceramic powder 50). Due to these grooves, most of the particles that make up the ceramic powder 50 do not adhere to the coatings 28, 38. The thin circular sheets 27, 37 correspond to the contact members of the present invention.
[0029] According to the powder molding die 10 of the present embodiment described above, the upper surface of the thin circular sheet 27 and the lower surface of the thin circular sheet 37 that come into contact with the powder are covered with a ta-C film, which is a type of DLC film. The surface of the ta-C film has a texture composed of a plurality of grooves, and the opening width of the grooves is smaller than the average particle size of the powder to be compressed. Therefore, it is possible to effectively prevent the powder from adhering to the surface of the ta-C film. This reduces the burden of cleaning the ta-C film, and it is possible to prevent the powder adhering to the ta-C film from peeling off, resulting in an uneven product.
[0030] The texture is made up of stripe-shaped grooves, which can be formed relatively easily by femtosecond laser processing.
[0031] Furthermore, the coating films 28, 38 are ta-C films, which have higher hardness, density, and heat resistance than aC films. In addition, the ta-C film has excellent low adhesion, low friction, and high wear resistance. The thickness of the ta-C film is preferably 500 nm or more. This makes it difficult for the texture to be broken when compressing powder using this powder molding die 10.
[0032] It goes without saying that the present invention is not limited to the above-described embodiment, and can be embodied in various forms within the technical scope of the present invention.
[0033] For example, in the above-mentioned embodiment, the coating films 28, 38 are used as DLC films, but the present invention is not limited thereto. For example, an aC film may be used as the DLC film. However, the ta-C film is preferable because it is superior in terms of functionality. In addition, when using a ta-C film, a ta-C film doped with nitrogen atoms may be used. The doping amount of the nitrogen atoms is not particularly limited, but may be more than 0 atm% and 15 atm% or less. When doped with nitrogen atoms, depending on the type of powder, the powder may be less likely to adhere to the coating films 28, 38. Therefore, it is preferable to set the doping amount of the nitrogen atoms according to the type of powder.
[0034] In the above-described embodiment, striped grooves are given as an example of the multiple grooves formed in the texture, but this is not particularly limited, and grooves of other shapes (such as lattice-shaped grooves) may also be used.
[0035] In the above-described embodiment, the lower surface (surface on which the coating film 28 is not formed) of the thin circular sheet 27 of the lower sheet 26 may be integrated with the upper surface of the lower cylindrical body 22 of the lower punch 20 by bonding or joining. In this case, the member obtained by integrating the lower punch 20 and the thin circular sheet 27 corresponds to the contact member of the present invention. Similarly, the upper surface (surface on which the coating film 38 is not formed) of the thin circular sheet 37 of the upper sheet 36 may be integrated with the lower surface of the upper cylindrical body 32 of the upper punch 30 by bonding or joining. In this case, the member obtained by integrating the upper punch 30 and the thin circular sheet 37 corresponds to the contact member of the present invention.
[0036] In the above-described embodiment, the lower sheet 26 provided with the coating film 28 is disposed on the upper surface of the lower punch 20, and the upper sheet 36 provided with the coating film 38 is disposed on the lower surface of the upper punch 30, but the coating film 28 may be directly formed on the upper surface of the lower punch 20 and the coating film 38 may be directly formed on the lower surface of the upper punch 30 without using the lower and upper sheets 26, 36. In this case, the lower punch 20 and the upper punch 30 each correspond to the contact member of the present invention. The coating films 28, 38 can be formed in the same manner as in the above-described embodiment. Also, in this manner, the same effects as in the above-described embodiment can be obtained.
[0037] In the above-mentioned embodiment, the powder molding die 10 is exemplified as one of the powder device members, but the present invention is not particularly limited to a powder molding die, and may be applied to, for example, a roll press machine 60 as shown in FIG. 4. The roll press machine 60 has a pair of rollers 62 (contact members) whose surfaces are covered with a coating film 64 made of a ta-C film, and a texture composed of grooves similar to those in the above-mentioned embodiment is formed on the surface of the coating film 64. Clay The thickness of the tape 70 is adjusted when it passes through the gap between the coating films 64 of the pair of rollers 62 from left to right in Fig. 4. In this case as well, the same effects as those of the above-mentioned embodiment can be obtained. EXAMPLES
[0038] EXAMPLES The present invention will be described below with reference to examples, but the present invention is not limited to the following examples in any way.
[0039] 1.Dry molding [Example 1] The lower sheet 26 and the upper sheet 36 of the powder molding die 10 were prepared as follows. First, a thin circular sheet made of SKD-11 with a diameter of 16 mm and a thickness of 1.5 mm was prepared. Next, a texture consisting of striped grooves was formed on one side of this thin circular sheet by femtosecond laser processing. Specifically, the femtosecond laser was set to a wavelength of 800 nm, a pulse width of 250 fs, an output of 1 W, and a beam diameter of 4 mm. The period of the striped grooves was 800 nm, the same as the laser wavelength, the groove opening width was also 800 nm, and the groove depth was 230 nm.
[0040] Next, a ta-C film was formed on one side of the textured thin circular sheet by IBA-FAD. FIG. 5 is a schematic diagram of an IBA-FAD device 100. A rotatable stage 104 is arranged in a film formation chamber 102 of the IBA-FAD device 100. Four workpieces W can be fixed to the stage 104 at 90° intervals. An ion gun 106 and a T-shaped duct 108 are attached to the film formation chamber 102. A graphite cathode 110, an anode 112, and a trigger 114 are arranged at one end of the duct 108. The trigger 114 generates an arc discharge toward the graphite cathode 110. The carbon ion beam generated from the graphite cathode 110 by the arc discharge from the trigger 114 is bent at a right angle from one end of the duct 108 by an electromagnetic field generated by a coil and introduced into the film formation chamber 102 (see the hatched arrow). On the other hand, non-ionized carbon clusters (droplets) travel in a straight line from one end of the duct 108 to the other end (see white arrow) and are captured by the collection film 116. The nitrogen ion beam emitted from the ion gun 106 is introduced into the film formation chamber 102 at an angle of 90° to the carbon ion beam (see black arrow). When a ta-C film not doped with nitrogen atoms is formed on the workpiece W, a nitrogen ion beam is not used, whereas when a ta-C film doped with nitrogen atoms is formed on the workpiece W, a nitrogen ion beam is used.
[0041] In Example 1, the ta-C film was formed without using a nitrogen ion beam, and the discharge voltage was set to 1 kV, the arc discharge current value to 50 A, and the negative bias applied to the workpiece W (thin circular sheet) to 100 V. The deposition time was set to 40 minutes, and the stage rotation speed to 10 rpm. As a result, the texture composed of striped grooves was covered by the ta-C film. The striped grooves were reflected as they were on the surface of the ta-C film. The thickness of the ta-C film was 600 mm. nm The period of the striped grooves that appeared on the ta-C film was 800 nm, the groove opening width was also 800 nm, and the depth was 230 nm. The ta-C film formed by IBA-FAD hardly filled the grooves of the texture. This is due to the characteristic of IBA-FAD, which provides a strongly rectified linear carbon ion beam and leads to the accumulation of carbon atoms from one direction. Figure 6 shows an example of a scanning electron microscope (SEM) image of the surface of the ta-C film formed on a thin circular sheet. Figure 7 shows an example of a cross-sectional profile when the ta-C film is cut on a plane perpendicular to the extension direction of the grooves. In this way, a release sheet was obtained in which one side of the thin circular sheet was covered with a ta-C film (having a surface texture composed of striped grooves). The surface energy of the ta-C film was measured by the sessile drop method using pure water and diiodomethane. The results are shown in Table 1.
[0042] This release sheet was used as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to compression mold the ceramic powder. The molding was performed under different conditions as shown in Tests 1 to 3 below. Test 1 Alumina (Al2O3) powder with an average particle size of 2.0 μm was used as the ceramic powder, and molding was performed at a molding pressure of 5 MPa, a temperature of 23°C, and a humidity of <20% RH. Test 2 Silica (SiO2) powder with an average particle size of 1.5 μm was used as the ceramic powder, and molding was performed at a molding pressure of 20 MPa, a temperature of 23°C, and a humidity of <20% RH. Test 3 Alumina (Al2O3) powder with an average particle size of 0.46 μm was used as the ceramic powder, and molding was performed at a molding pressure of 5 MPa, a temperature of 23°C, and a humidity of <20% RH. Note that Test 3 is a reference test because the opening width of the texture grooves is larger than the average particle size of the ceramic powder.
[0043] In each test, the amount of powdery matter adhering to the upper sheet 36 after molding was measured with an electronic balance, and this value was taken as the amount of adhesion. The results are shown in Table 1.
[0044] [Example 2] In forming the ta-C film, the same conditions as in Example 1 were adopted except that nitrogen gas was added to the ion gun 106 in FIG. 5 at a flow rate of 10 sccm, and the ta-C film doped with nitrogen atoms was formed. The thickness of the ta-C film was 600 mm. nm The period of the striped grooves that appeared in the ta-C film was 800 nm, the opening width of the grooves was 800 nm, and the depth was 230 nm. The ta-C film formed with IBA-FAD hardly filled the grooves of the texture. The ta-C film contained 8 atm% nitrogen atoms. The nitrogen atom content (doping amount) was measured by X-ray photoelectron spectroscopy (XPS) (same below). The surface energy of the ta-C film doped with nitrogen atoms was determined in the same manner as in Example 1. In addition, the obtained release sheet was used as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to mold ceramic powder under the conditions of the above-mentioned test 2, and the adhesion amount per sheet was determined. The results are shown in Table 1.
[0045] [Example 3] In forming the ta-C film, the same conditions as in Example 1 were adopted except that nitrogen gas was added to the ion gun 106 in FIG. 5 at a flow rate of 20 sccm, and the ta-C film doped with nitrogen atoms was formed. The thickness of the ta-C film was 600 mm. nmThe period of the striped grooves that appeared in the ta-C film was 800 nm, the groove opening width was 800 nm, and the depth was 230 nm. The ta-C film formed with IBA-FAD hardly filled the grooves of the texture. The ta-C film contained 12 atm% nitrogen atoms. The surface energy of the ta-C film doped with nitrogen atoms was determined in the same manner as in Example 1. In addition, the obtained release sheet was used as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to mold ceramic powder under the conditions of the above-mentioned Test 2, and the adhesion amount per sheet was determined. The results are shown in Table 1.
[0046] [Comparative Example 1] A release sheet was obtained by forming a texture on a thin circular sheet made of SKD-11 in the same manner as in Example 1, but without forming a ta-C film. The surface energy of the thin circular sheet on which the texture was formed but the ta-C film was not formed was determined in the same manner as in Example 1. The obtained release sheet was used as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to mold ceramic powder under the conditions of the above-mentioned Test Examples 1 to 3, and the adhesion amount per sheet was determined. The results are shown in Table 1.
[0047] [Comparative Example 2] A ta-C film was formed on a thin circular sheet made of SKD-11 in the same manner as in Example 1 without forming a texture, to obtain a release sheet. The thickness of the ta-C film was 600 mm. nm The surface energy of the ta-C film without texture was determined in the same manner as in Example 1. The resulting release sheets were used as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to mold ceramic powder under the conditions of the above-mentioned Test Examples 1 to 3, and the adhesion amount per sheet was determined. The results are shown in Table 1.
[0048] [Comparative Example 3] A ta-C film was formed on a thin circular sheet made of SKD-11 in the same manner as in Example 2 without forming a texture, to obtain a release sheet. The thickness of the ta-C film was 600 mm. nmThe ta-C film contained 8 atm % nitrogen atoms. The surface energy of the ta-C film doped with 8 atm % nitrogen atoms and not having texture was determined in the same manner as in Example 1. The resulting release sheets were used as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to mold ceramic powder under the conditions of the above-mentioned Test Example 2, and the adhesion amount per sheet was determined. The results are shown in Table 1.
[0049] [Comparative Example 4] A ta-C film was formed on a thin circular sheet made of SKD-11 without forming a texture in the same manner as in Example 3 to obtain a release sheet. The thickness of the ta-C film was 600 mm. nm The ta-C film contained 12 atm % nitrogen atoms. The surface energy of the ta-C film doped with 12 atm % nitrogen atoms and not having texture was determined in the same manner as in Example 1. The resulting release sheets were used as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to mold ceramic powder under the conditions of the above-mentioned Test Example 2, and the adhesion amount per sheet was determined. The results are shown in Table 1.
[0050] [Comparative Example 5] The surface energy of the thin circular sheet itself made of SKD-11 was determined in the same manner as in Example 1. In addition, the thin circular sheets made of SKD-11 were used as they were (i.e., neither texture nor ta-C film was formed) as the lower sheet 26 and the upper sheet 36 of the powder molding die 10 to mold ceramic powder under the conditions of the above-mentioned Test Examples 1 to 3, and the adhesion amount per sheet was determined. The results are shown in Table 1.
[0051] [Table 1]
[0052] As can be seen from the results of Test 1, in molding alumina powder with an average particle size of 2 μm, Example 1, which had a ta-C film with a texture formed thereon, had a higher powder adhesion prevention effect than Comparative Example 1, which had a texture formed but no ta-C film, Comparative Example 2, which had a ta-C film without texture, and Comparative Example 5, which had neither texture nor a ta-C film.
[0053] As can be seen from the results of Test 2, in molding silica powder with an average particle size of 1.5 μm, Examples 1 to 3 having a ta-C film with texture formed thereon had a higher powder adhesion prevention effect than Comparative Example 1 having a texture but no ta-C film, Comparative Examples 2 to 4 having a ta-C film without texture, and Comparative Example 5 having neither a texture nor a ta-C film. In addition, Examples 2 and 3 having a ta-C film doped with nitrogen atoms had a higher powder adhesion prevention effect than Example 1 having a ta-C film not doped with nitrogen atoms. On the other hand, when no texture was formed, Comparative Examples 3 and 4 having a ta-C film doped with nitrogen atoms had a lower powder adhesion prevention effect than Comparative Example 2 having a ta-C film not doped with nitrogen atoms.
[0054] As can be seen from the results of Test 3 (Reference Test), in molding alumina powder with an average particle size of 0.46 μm, Example 1 had a higher powder adhesion prevention effect than Comparative Examples 1 and 5, but the effect was inferior to Comparative Example 2, in which the surface was covered with a ta-C film without texture. The reason for this is thought to be that in Example 1, the opening width of the striped grooves was larger than the average particle size of the alumina powder, so the alumina particles entered the grooves and adhered.
[0055] In addition, in Example 1, even if the molding pressure in Test 1 was changed from 5 MPa to 20 MPa, no change was observed in the powder adhesion prevention effect. nm From 200 nm (deposition time was changed from 40 min to 10 min), there was no problem at 5 MPa, but the texture was destroyed at 20 MPa.
[0056] 2.Wet molding [Example 4] A thin circular sheet made of SKD-11 with a diameter of 16 mm and a thickness of 1.5 mm was prepared, and a texture consisting of striped grooves was formed on one side of the plate in the same manner as in Example 1, and then a ta-C film was formed to obtain a contact member of Example 4. The following adhesion evaluation test was carried out using the obtained contact member.
[0057] Adhesion evaluation test A schematic diagram of the adhesion evaluation test is shown in Figure 10. An organic binder and a solvent were added to ceramic powder and kneaded to produce a clay-like material ( Clay ) was obtained. Clay The plate is then shaped into a rectangular plate, and a die is used to cut out a piece with a diameter of 10 mm and a thickness of about 1.4 mm. Clay A disk 82 was obtained. Clay The disk 82 is placed on a chrome-plated base 84, Clay The contact member of Example 4 is attached to the disk 82 with a ta-C film. Clay In this state, the contact member was lowered by the elevator 86 at a speed of 0.5 mm / min. Clay The disk 82 was compressed until its thickness became about 0.7 mm, and then the contact member was raised at a speed of 0.5 mm / min. This operation was carried out three times, and the lower surface of the contact member that was raised in each of the three times was Clay The number of times that the disk 82 adhered and was lifted was counted. The results are shown in Table 2.
[0058] [Comparative Example 6] In Comparative Example 6, the same thin circular sheet as in Example 4 was prepared and used as it was as the contact member of Comparative Example 6 to carry out an adhesion evaluation test. The results are shown in Table 2.
[0059] [Comparative Example 7] In Comparative Example 7, the same thin circular sheet as in Example 4 was prepared, and a ta-C film was formed in the same manner as in Example 1 without forming a texture on the thin circular sheet to obtain a contact member. An adhesion evaluation test was performed using the contact member. The results are shown in Table 2.
[0060] [Comparative Example 8] In Comparative Example 8, the same thin circular sheet as in Example 4 was prepared, and the texture was formed on the thin circular sheet in the same manner as in Example 1, and then a contact member was obtained without forming a ta-C film. An adhesion evaluation test was performed using the contact member. The results are shown in Table 2.
[0061] [Table 2]
[0062] The contact member of Example 4, in which the lower surface was coated with a ta-C film having a texture, had a higher thermal conductivity than the contact members of Comparative Example 6, which had a lower surface left as is, Comparative Example 7, which was coated with a ta-C film without a texture, and Comparative Example 8, which was not coated with a ta-C film and only had a texture. Clay The adhesion of the disks (powder containing the solvent) could be effectively prevented. [Explanation of symbols]
[0063] 10 Powder device member, 12 Die, 14 Through hole, 20 Lower punch, 22 Lower cylindrical body, 22a Large diameter portion, 22b Small diameter portion, 24 Lower circular plate, 26 Lower sheet, 27 Thin circular sheet, 28 coating film, 30 upper punch, 32 upper cylindrical body, 32a large diameter part, 32b small diameter part, 34 upper circular plate, 36 upper sheet, 37 thin circular sheet, 38 coating film, 40 work table, 50 ceramic powder, 60 roll press machine, 62 roller, 64 coating film, 70 Clay Tape, 82 Clay Disk, 84 base, 86 elevator, 100 FAD device, 102 deposition chamber, 104 stage, 106 ion gun, 108 duct, 110 graphite cathode, 112 anode, 114 trigger, 116 collection film.
Claims
1. A powder device member that contacts and handles a powder, A contact member that contacts the powder; a DLC film covering a surface of the contact member; Equipped with the surface of the DLC film has a texture composed of a plurality of grooves; The opening width of the groove is smaller than the average particle size of the powder, The DLC film is a ta-C film doped with nitrogen atoms. Powder device components.
2. The texture is made up of striped grooves.
2. The powder device member of claim 1.
3. The thickness of the ta-C film is 500 nm or more.
3. A powder device member according to claim 1 or 2.
4. 1. A method of manufacturing a powder equipment component for contacting and manipulating a powder, comprising the steps of: (1) forming a texture on a surface of a contact member that contacts the powder, the texture being composed of a plurality of grooves, the opening width of the grooves being smaller than an average particle size of the powder; (2) forming a ta-C film doped with nitrogen atoms as a DLC film on the surface of the contact member on which the texture is formed; A method for making a powder device member comprising:
5. In the step (1), the texture is formed by femtosecond laser processing; In the step (2), the ta-C film is formed by ion beam assisted filtered arc deposition. A method for producing the powder device member according to claim 4.
6. 1. A method of manufacturing a powder equipment component for contacting and manipulating a powder, comprising the steps of: (1') forming a ta-C film doped with nitrogen atoms as a DLC film on a surface of a contact member that contacts the powder; (2') forming a texture on the surface of the ta-C film, the texture being composed of a plurality of grooves, the opening width of the grooves being smaller than the average particle size of the powder; A method for making a powder device member comprising:
7. In the step (1'), the ta-C film is formed by ion beam assisted filtered arc deposition; In the step (2'), the texture is formed by femtosecond laser processing. A method for producing the powder device member according to claim 6.
Citation Information
Patent Citations
Jugikyunotamamigakidoosokuteisuruhoho narabini sonosochi
JP1976047484A
Manufacture of powder molded body and manufacture of powder sintered body
JP2000052328A
Coating method with diamond-like carbon film and die for plastic working
JP2004084014A
Forming mold and method for manufacturing the same
JP2011098845A
Laser processing method, laser processing apparatus, and material manufacturing method
JP2018144056A