Liquid polybutadiene, its production method and use, as well as compositions, polymeric coatings, adhesives and crosslinkers

The controlled anionic polymerization of 1,3-butadiene with specific modifiers and initiators produces liquid polybutadiene with targeted molecular properties, addressing the challenges of existing methods by enhancing adhesion and coating performance while reducing metal impurities.

JP7571158B2Active Publication Date: 2024-10-22CHINA PETROLEUM & CHEMICAL CORP +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2022571236
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-21
Filing Date
2020-10-28
Publication Date
2024-10-22
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

Existing liquid polybutadiene production methods face challenges in achieving high vinyl content, narrow molecular weight distribution, and suitable molecular weight and kinematic viscosity, leading to issues such as low peel strength and poor weather resistance due to wide molecular weight distribution and metal impurities.

Method used

A method involving anionic polymerization of 1,3-butadiene with a structure modifier and organolithium initiator in a solvent at controlled temperatures, using specific ether and amine compounds, results in liquid polybutadiene with a targeted molecular weight, narrow distribution, and high vinyl content, achieving a molecular weight of 2500 to 5500, a distribution index of 1 to 1.2, and kinematic viscosity of 100 to 500 poise.

Benefits of technology

The produced liquid polybutadiene exhibits excellent fluidity, film-forming properties, and coating properties with high adhesion to substrates, suitable for polymer coatings and adhesives, and low metal content, making it suitable for crosslinking agents and electrical insulation materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571158000001
    Figure 0007571158000001
  • Figure 0007571158000002
    Figure 0007571158000002
  • Figure 0007571158000003
    Figure 0007571158000003
Patent Text Reader

Abstract

A liquid polybutadiene, its production method, and use, which has a number average molecular weight of 2500 to 5500, a molecular weight distribution index of 1 to 1.2, a 1,2-structural unit content of 85 to 95 wt% based on the total weight, a 1,4-structural unit content of 5 to 15 wt%, a molar ratio of cis-1,4-structural units to trans-1,4-structural units of 1 to 2:1, and a kinematic viscosity at 45°C of 100 to 500 P. The liquid polybutadiene has excellent fluidity, film-forming properties, and coatability, and the formed coating has improved adhesion to substrates.
Need to check novelty before this filing date? Find Prior Art

Description

Detailed Description of the Invention

[0001] [CROSS REFERENCE TO RELATED APPLICATIONS] This application claims the benefit of Chinese patent application No. 202010436914.8, filed on May 21, 2020, the contents of which are incorporated herein by reference. [Technical field] The present invention relates to liquid polybutadiene, its preparation method and use. The present invention also relates to compositions containing said liquid polybutadiene. The present invention further relates to polymer coatings, adhesives and crosslinkers containing said liquid polybutadiene and said compositions. [Background technology] Liquid polybutadiene is a viscous, fluid polymer with a number-average molecular weight of 500 to 10,000, which is an oily liquid at room temperature and is widely used in paints, inks, surfactants, polymer modifiers, etc.

[0002] According to the microstructure, liquid polybutadienes can be divided into 1,4-adducts (cis and trans isomers) and 1,2-adducts, and according to the vinyl content, 1,2-adducts can be divided into medium vinyl liquid polybutadienes and high vinyl liquid polybutadienes.

[0003] High-vinyl liquid polybutadiene is a liquid polybutadiene with a 1,2-structure content of 65% by weight or more, and is generally produced using iron-, cobalt-, or molybdenum-based catalysts. However, the above catalyst systems have the following drawbacks: (1) It is difficult to produce low-molecular-weight liquid polybutadiene. (2) The molecular weight distribution is wide, and the peel strength is low. (3) Since it contains variable valence metals, the weather resistance is poor. Therefore, there is a need to develop liquid polybutadiene with high vinyl content and narrow molecular weight distribution. [Summary of the invention] [Problem to be solved by the invention] It is an object of the present invention to provide a liquid polybutadiene having not only high vinyl content and narrow molecular weight distribution, but also suitable molecular weight and kinematic viscosity. [Means for solving the problem] According to a first aspect of the present invention, there is provided a liquid polybutadiene having a number average molecular weight of 2500 to 5500, a molecular weight distribution index of 1 to 1.2, a 1,2-structural unit content of 85 to 95 wt % and a 1,4-structural unit content of 5 to 15 wt % based on the total amount, a molar ratio of cis-1,4-structural units to trans-1,4-structural units of 1 to 2:1, and a kinetic viscosity at 45°C of 100 to 500 P.

[0004] According to a second aspect of the present invention, the present invention includes a step of contacting 1,3-butadiene with a structure-controlling agent and an organolithium initiator in a polymerization solvent under anionic polymerization reaction conditions to obtain a polymerization reaction mixture containing polybutadiene, the contacting being carried out at a temperature of -10°C to 20°C, the structure-controlling agent includes component A and component B, the component A is one or more selected from ethers and amines, the component B is one or more selected from alkali metal alkoxides, the molar ratio of the organolithium initiator:component A:component B is 1:0.05-0.3:0.03-0.2, the organolithium initiator is calculated as lithium, The component A is one or more compounds selected from the group consisting of the compounds represented by formula I and the compounds represented by formula II.

[0005] [ka]

[0006] (In formula I, R1 and R2 are the same or different and each independently represents a hydrogen atom or a C1-C6 alkyl group; R3 and R4 are the same or different and each independently represents a C1-C6 alkyl group; n is an integer from 1 to 5.

[0007] [ka]

[0008] (In formula II, R5 and R6 are the same or different and each independently represents a hydrogen atom or a C1-C6 alkyl. R7 and R8 are the same or different and each independently represents a C1 to C6 alkylene; R9 and R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 are the same or different and each independently represents a hydrogen atom or a C1-C6 alkyl, m is an integer from 1 to 5. According to a third aspect of the invention, the present invention provides a liquid polybutadiene produced by the process according to the second aspect of the invention.

[0009] According to a fourth aspect of the present invention, there is provided a composition comprising a liquid polybutadiene and at least one additive, said liquid polybutadiene being as defined in the first or third aspect of the present invention.

[0010] According to a fifth aspect of the invention, the present invention provides a polymeric coating comprising a liquid polybutadiene according to the first or third aspect of the invention, or a composition according to the fourth aspect of the invention.

[0011] According to a sixth aspect of the present invention, there is provided a pressure sensitive adhesive comprising the liquid polybutadiene according to the first or third aspect of the present invention, or the composition according to the fourth aspect of the present invention. According to a seventh aspect of the present invention, the present invention provides a crosslinker comprising a liquid polybutadiene according to the first or third aspect of the present invention, or a composition according to the fourth aspect of the present invention. According to an eighth aspect of the present invention, there is provided the use of a liquid polybutadiene according to the first or third aspect of the present invention, or a composition according to the fourth aspect of the present invention, as a crosslinking agent, an adhesive or an electrical insulating material.

[0012] The liquid polybutadiene according to the present invention has not only a high vinyl content, but also a narrow molecular weight distribution, and an appropriate molecular weight and kinematic viscosity. The liquid polybutadiene according to the present invention has excellent fluidity, film-forming property and coating property, and is particularly suitable for forming polymer coatings, and the polymer coatings thus formed have improved adhesion to substrates. The liquid polybutadiene according to the present invention is expected to have a promising future in the fields of crosslinking agents, binders and electrical insulating materials. [Mode for carrying out the invention] The endpoints of the ranges and any values ​​disclosed herein are not limited to the exact ranges or values, but should be understood to include the values ​​close to these ranges or values. In the case of ranges of numerical values, the endpoints of the ranges, the endpoints of the ranges and the individual point values, and the individual point values ​​may be combined to form one or more new numerical ranges, which numerical ranges are to be considered as specifically disclosed herein.

[0013] For the purposes of this invention, the term "liquid polybutadiene" is a polybutadiene that is flowable at a temperature of 25°C.

[0014] According to a first aspect of the present invention, there is provided a method for producing ... composition comprising the steps of: The liquid polybutadiene has a number average molecular weight of 2500 to 5500, a molecular weight distribution index of 1 to 1.2, a 1,2-structural unit content of 85 to 95% by weight, a 1,4-structural unit content of 5 to 15% by weight, a molar ratio of cis-1,4-structural units to trans-1,4-structural units of 1 to 2:1, and a kinetic viscosity at 45°C of 100 to 500 P.

[0015] According to the liquid polybutadiene of the present invention, the number average molecular weight (M n ) is 2500 to 5500. Preferably, the number average molecular weight of the liquid polybutadiene is 2800 to 5000. More preferably, the number average molecular weight of the liquid polybutadiene is 3000 to 4500.

[0016] According to the liquid polybutadiene of the present invention, the molecular weight distribution index (M w / M n ) is 1 to 1.2. According to the liquid polybutadiene of the present invention, the molecular weight distribution index of the liquid polybutadiene is preferably 1.01 to 1.09, more preferably 1.02 to 1.06.

[0017] In the present invention, the molecular weight and molecular weight distribution index of liquid polybutadiene are measured by gel permeation chromatography analysis, and a Tosoh HLC-8320 type gel permeation chromatograph is used for the gel permeation chromatography analysis, the column is TSKgel SuperMultiporeHZ-N, the standard column is TSKgel SuperMultiporeHZ, the solvent is chromatographically pure tetrahydrofuran (THF), the standard sample is narrow-distribution polystyrene, the polymer sample is prepared as a tetrahydrofuran solution with a mass concentration of 1 mg / mL, the sample injection amount is 10.00 μL, the flow rate is 0.35 mL / min, and the test temperature is 40.0°C.

[0018] According to the liquid polybutadiene of the present invention, the content of 1,2-structural units in the liquid polybutadiene is 85 to 95% by weight based on the total amount of the liquid polybutadiene. Preferably, the content of 1,2-structural units in the liquid polybutadiene is 87% by weight or more based on the total amount of the liquid polybutadiene, and may be, for example, 87 to 94% by weight. More preferably, the content of 1,2-structural units in the liquid polybutadiene is 90% by weight or more, preferably 90 to 93% by weight, for example, 90, 90.1, 90.2, 90.3, 90.4, 90.5, 90.6, 90.7, 90.8, 90.9, 91, 91.1, 91.2, 91.3, 91.4, 91.5, 91.6, 91.7, 91.8, 91.9, 92, 92.1, 92.2, 92.3, 92.4, 92.5, 92.6, 92.7, 92.8, 92.9 or 93% by weight, based on the total amount of the liquid polybutadiene.

[0019] According to the liquid polybutadiene of the present invention, the content of 1,4-structural units in the liquid polybutadiene is 5-15% by weight. According to the liquid butadiene of the present invention, the molar ratio of cis 1,4-structural units to trans 1,4-structural units in the liquid polybutadiene is 1-2:1, preferably 1.3-1.9:1. According to one preferred example of the liquid polybutadiene of the present invention, the molar ratio of trans 1,4-structural units to cis 1,4-structural units in the liquid polybutadiene is 1.65-1.75:1. The polymer coating formed with the liquid polybutadiene according to the preferred example has higher adhesion to a substrate and exhibits higher peel strength.

[0020] In the present invention, the term "1,2-structural unit" refers to a structural unit formed by butadiene in a 1,2-polymerization manner, and the content of the 1,2-structural unit may be referred to as the vinyl content. In the present invention, the term "1,4-structural unit" refers to a structural unit formed by butadiene in a 1,4-polymerization manner.

[0021] In the present invention, the term "cis 1,4-structural unit" refers to a structural unit formed by butadiene in a 1,4-polymerization manner and having a cis configuration, i.e., a structural unit shown in the following formula:

[0022] [ka]

[0023] In the present invention, the term "trans 1,4-structural unit" refers to a structural unit formed by butadiene in a 1,4-polymerization manner and having a trans configuration, i.e., a structural unit shown in the following formula:

[0024] [ka]

[0025] In the present invention, the contents of 1,2-structural unit, 1,4-structural unit, cis-1,4-structural unit, and trans-1,4-structural unit are all measured by nuclear magnetic resonance spectroscopy, and the specific test method is as follows: Testing is performed using a Bruker AVANCE400 type superconducting nuclear magnetic resonance apparatus; 1 The resonance frequency of H nucleus is 300.13 MHz, the spectral width is 2747.253 Hz, the pulse width is 5.0 μs, the data points are 16 K, the sample tube diameter is 5 mm, the solvent is deuterated chloroform (CDCl3), the sample concentration is 15 mg / mL, the test temperature is room temperature, the number of scans is 16, and the tetramethylsilane chemical shift is calibrated to 0 ppm.

[0026] According to the liquid polybutadiene of the present invention, the kinetic viscosity of the liquid polybutadiene at 45°C is 100 to 500 poise (P), and the liquid polybutadiene has excellent fluidity and is particularly suitable for paints and adhesives. Preferably, the kinetic viscosity of the liquid polybutadiene of the present invention at 45°C is 150 to 350 P. More preferably, the kinetic viscosity of the liquid polybutadiene of the present invention at 45°C is 170 to 300 P. Even more preferably, the kinetic viscosity of the liquid polybutadiene of the present invention at 45°C is 180 to 250 P.

[0027] The liquid polybutadiene according to the present invention has a large change in kinetic viscosity with molecular weight, and can exhibit an appropriate kinetic viscosity within a wide range. According to the liquid polybutadiene of the present invention, in one preferred example, the number average molecular weight of the liquid polybutadiene is 2500-4000, preferably 3000-4000, and the kinetic viscosity of the liquid polybutadiene at 45°C is 100-280 P, preferably 150-260 P. In this preferred example, the molecular weight distribution index of the liquid polybutadiene may be 1-1.05.

[0028] According to the liquid polybutadiene of the present invention, in another preferred example, the number average molecular weight of the liquid polybutadiene is more than 4000 and not more than 5500, and the kinematic viscosity of the liquid polybutadiene at 45° C. is more than 280 P and not more than 500 P, preferably 280 to 480 P. In this preferred example, the molecular weight distribution index of the liquid polybutadiene may be 1 to 1.08.

[0029] In the present invention, the kinematic viscosity is measured with reference to the capillary method defined in GBT10247-2008, where it is measured at a temperature of 45° C. using an Ubbelohde viscometer with size number 4B.

[0030] According to the liquid polybutadiene of the present invention, the glass transition temperature (T g ) is -32°C to -12°C, preferably -29°C to -15°C, and more preferably -27°C to -17°C.

[0031] In the present invention, the glass transition temperature is measured by differential scanning calorimetry, and the specific test method is as follows: Use a TA-2980 DSC differential scanning calorimeter to measure according to the method specified in "GB / T 29611-2013, glass transition temperature of raw rubber", and the heating rate is 20°C / min.

[0032] According to the liquid polybutadiene of the present invention, the weight content of metal elements in the liquid polybutadiene may be 200 ppm or less, preferably 100 ppm or less, more preferably 50 ppm or less, and even more preferably 20 ppm or less, based on the total amount of the liquid polybutadiene.

[0033] In the present invention, the content of metal elements in liquid polybutadiene is measured by plasma method, and the test method is specifically as follows: Using Optima 8300 type direct reading full spectrum ICP spectrometer manufactured by PerkinElmer (PE) of the United States, equipped with echelle diffraction grating, solid detector, ultraviolet zone and visible light zone double optical path double solid detector, adopting flat plate plasma technology, the operation parameters of the instrument are as follows: high frequency power 1300W, plasma gas flow rate 15L / min, atomization gas flow rate 0.55L / min, auxiliary gas flow rate 0.2L / min, peristaltic pump speed 1.50mL / min, integration time 10s, plasma is observed in the axial direction. The preparation method of the sample is as follows: Put 2,000g of sample accurately into a porcelain crucible, put it into a high-temperature resistance furnace and gradually heat it to 500℃. After it is completely incinerated, take it out, add 5mL of 10% by volume dilute nitric acid, slowly heat it on an electric heating plate to completely dissolve it, evaporate the solution to dryness, add 1mL of concentrated nitric acid (concentration 68% by volume), transfer it to a 50mL measuring flask and add water to the constant volume. At the same time, prepare a reagent blank solution.

[0034] According to a second aspect of the present invention, there is provided a method for producing liquid polybutadiene, the method comprising the steps of contacting 1,3-butadiene with a structure modifier and an organolithium initiator in a polymerization solvent under anionic polymerization reaction conditions to obtain a polymerization reaction mixture containing polybutadiene, said contacting being conducted at a temperature below 40°C.

[0035] According to the production method of the present invention, the structure-controlling agent contains component A and component B, wherein component A is one or more selected from ethers and amines, and component B is one or more selected from alkali metal alkoxides.

[0036] According to the production method of the present invention, the component A is one or more compounds selected from the compounds represented by formula I and the compounds represented by formula II.

[0037] [ka]

[0038] (In formula I, R1 and R2 are the same or different and each independently represents a hydrogen atom or a C1-C6 alkyl group; R3 and R4 are the same or different and each independently represents a C1-C6 alkyl group; n is an integer from 1 to 5, and may be, for example, 1, 2, 3, 4, or 5.

[0039] [ka]

[0040] (In formula II, R5 and R6 are the same or different and each independently represents a hydrogen atom or a C1-C6 alkyl. R7 and R8 are the same or different and each independently represents a C1 to C6 alkylene; R9 and R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 are the same or different and each independently represents a hydrogen atom or a C1-C6 alkyl, m is an integer from 1 to 5, and may be, for example, 1, 2, 3, 4, or 5. In formula I and formula II, C1-C6 alkyl includes C1-C6 linear alkyl and C3-C6 branched alkyl, and specific examples thereof may include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, isobutyl, t-butyl, n-pentyl, isopentyl, t-pentyl, neopentyl, and n-hexyl.

[0041] In one preferred embodiment, in formula I, R1 and R2 are all hydrogen atoms, and R3 and R4 are the same and are methyl, ethyl, n-propyl or n-butyl.

[0042] In one preferred embodiment, in formula II, R5 and R6 are all hydrogen atoms, R7 and R8 are C2-C4 alkylene, and R9 and R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 are all hydrogen atoms.

[0043] According to the production method of the present invention, preferred examples of the component A may include, but are not limited to, one or more of diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol di-n-propyl ether, diethylene glycol di-n-butyl ether, and 1,2-dipiperidylethane.

[0044] The alkali metal alkoxide is preferably one or more selected from the compounds represented by formula III.

[0045] [ka]

[0046] (In formula III, R 17 is C1~C 20 Alkyl, C6-C 30 Aryl or C4-C 20 Cycloalkyl, preferably C2-C 10 Alkyl or C6-C 12 cycloalkyl, more preferably C2-C6 alkyl; M is an alkali metal atom, for example Li, Na or K, preferably Na. In formula III, C1~C 20 Alkyl is C1-C 20 Straight chain alkyl and C3-C 20Including branched alkyl, specific examples of which may include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, isobutyl, t-butyl, n-pentyl and its isomers, n-hexyl and its isomers, n-heptyl and its isomers, n-octyl and its isomers, n-nonyl and its isomers, n-decyl and its isomers, undecyl and its isomers, dodecyl and its isomers, tridecyl and its isomers, tetradecyl and its isomers, pentadecyl and its isomers, hexadecyl and its isomers, heptadecyl and its isomers, octadecyl and its isomers, nonadecyl and its isomers, and eicosyl and its isomers.

[0047] In formula III, C4~C 20 Cycloalkyl includes cyclopropyl, cyclopentyl, cyclohexyl, 4-methylcyclohexyl, 4-ethylcyclohexyl, 4-n-propylcyclohexyl, 4-n-butylcyclohexyl or 2-isopropyl-5-methylcyclohexyl.

[0048] According to the production method of the present invention, preferred examples of the alkali metal alkoxide include, but are not limited to, one or more of sodium t-butoxide, sodium t-amyloxy, sodium menthol, sodium ethoxide, and sodium-n-hexyloxide.

[0049] According to the production method of the present invention, the molar ratio of organolithium initiator:component A:component B is 1:0.05-0.3:0.03-0.2, and the organolithium initiator is calculated as lithium. Preferably, the molar ratio of organolithium initiator:component A:component B is 1:0.08-0.25:0.04-0.18, and the organolithium initiator is calculated as lithium. More preferably, the molar ratio of organolithium initiator:component A:component B is 1:0.1-0.2:0.05-0.15, and the organolithium initiator is calculated as lithium. According to the production method of the present invention, the molar ratio of component B:component A is preferably 0.4-1.5:1, more preferably 0.5-1:1.

[0050] According to the process of the present invention, the organolithium initiator is preferably an organomonolithium compound, more preferably a compound as shown in formula IV. R 18 Li (Formula IV) (In formula IV, R 18 is C1-C6 alkyl, C3-C 12 Cycloalkyl, C7-C 14 Aryl alkyl or C6-C 12 It is aryl. In formula IV, C1-C6 alkyl includes C1-C6 linear alkyl and C3-C6 branched alkyl, and specific examples thereof may include, but are not limited to, methyl, ethyl, n-propyl, isopropyl, n-butyl, s-butyl, isobutyl, t-butyl, n-pentyl, isopentyl, t-pentyl, neopentyl, and n-hexyl.

[0051] In formula IV, C3~C 12 Examples of cycloalkyl can include, but are not limited to, cyclopropyl, cyclopentyl, cyclohexyl, 4-methylcyclohexyl, 4-ethylcyclohexyl, 4-n-propylcyclohexyl, and 4-n-butylcyclohexyl.

[0052] In formula IV, C7~C 14 Examples of arylalkyl can include, but are not limited to, phenylmethyl, phenylethyl, phenyl n-propyl, phenyl n-butyl, phenyl t-butyl, phenylisopropyl, phenyl n-pentyl, and phenyl n-butyl.

[0053] In formula IV, C6~C 12 Examples of aryl can include, but are not limited to, phenyl, naphthyl, 4-methylphenyl, and 4-ethylphenyl.

[0054] According to the manufacturing method of the present invention, specific examples of the organolithium initiator may include, but are not limited to, one or more of ethyllithium, n-propyllithium, isopropyllithium, n-butyllithium, s-butyllithium, t-butyllithium, phenyllithium, 2-naphthyllithium, 4-butylphenyllithium, 4-tolyllithium, cyclohexyllithium, and 4-butylcyclohexyllithium. Preferably, the organolithium initiator is n-butyllithium and / or s-butyllithium, and more preferably, the organolithium initiator is n-butyllithium.

[0055] The amount of the organolithium initiator used may be determined according to the expected molecular weight of the liquid polybutadiene. Preferably, the amount of the organolithium initiator used is such that the number average molecular weight of the produced liquid polybutadiene is 2500 to 5500, preferably 2800 to 5000, more preferably 3000 to 4500. The method of determining the specific amount of the organolithium initiator used according to the expected molecular weight of the polymer is known to those skilled in the art, and will not be described in detail in this specification.

[0056] According to the production method of the present invention, the polymerization solvent may be any of various organic substances, such as hydrocarbon solvents, that function as a reaction medium and allow the polymerization reaction to be carried out under solution polymerization conditions. The polymerization solvent may be one or more selected from cyclohexane, n-hexane, n-pentane, n-heptane, benzene, and raffinate. The raffinate is a distillate oil remaining after aromatic hydrocarbons are extracted from catalytic reforming products rich in aromatic hydrocarbons during petroleum refining. The polymerization solvent may be used alone or in combination.

[0057] According to the production method of the present invention, the content of 1,3-butadiene (i.e., monomer content) may be 1 to 15% by weight, preferably 2 to 12% by weight, and more preferably 4 to 10% by weight, based on the total amount of the polymerization solvent and 1,3-butadiene. In the present invention, the monomer content is the weight percentage content of 1,3-butadiene determined based on the total amount of the polymerization solvent and 1,3-butadiene before carrying out the polymerization reaction.

[0058] According to the production method of the present invention, 1,3-butadiene is contacted with a structure modifier and an organolithium initiator in a polymerization solvent at a temperature of -10°C to 20°C to carry out an anionic polymerization reaction, for example, 1,3-butadiene is contacted with a structure modifier and an organolithium initiator at a temperature of -10°C, -9°C, -8°C, -7°C, -6°C, -5°C, -4°C, -3°C, -2°C, -1°C, 0°C, 1°C, 2°C, 3°C, 4°C, 5°C, 6°C, 7°C, 8°C, 9°C, 10°C, 11°C, 12°C, 13°C, 14°C, 15°C, 16°C, 17°C, 18°C, 19°C or 20°C. More preferably, 1,3-butadiene is contacted with a structure modifier and an organolithium initiator at a temperature of 10°C or less, for example, at a temperature of -5°C to 10°C.

[0059] According to the production method of the present invention, the anionic polymerization reaction is carried out at a pressure of 0.005 to 1.5 MPa, more preferably at a pressure of 0.1 to 1 MPa. In the present invention, the pressures all refer to gauge pressures. According to the production method of the present invention, the time of the anionic polymerization reaction may be determined depending on the temperature of the polymerization reaction, and may generally be 30 to 240 min, and is preferably 40 to 120 min.

[0060] According to the production method of the present invention, the anionic polymerization reaction is carried out in an atmosphere of an inert gas, which is a gas that does not chemically interact with any of the reactants, reaction products, and solvent under the polymerization conditions, such as nitrogen gas and / or a Group 0 element gas (e.g., argon gas).

[0061] According to the production method of the present invention, the production method may further include a step of removing at least a portion of the metal ions in the polymerization reaction mixture to obtain a purified polymerization reaction mixture. At least a portion of the metal ions may be removed by washing the polymerization reaction mixture.

[0062] In one preferred embodiment, the method for removing at least a portion of the metal ions in the polymerization reaction mixture comprises mixing the polymerization reaction mixture with a washing liquid and separating an oil phase from the mixture, the washing liquid being water or an aqueous solution containing an acid. In this preferred embodiment, the acid is preferably an inorganic acid, more preferably one or more of sulfuric acid, nitric acid, hydrochloric acid and carbonic acid. When the acid is carbonic acid, carbonic acid is formed by introducing carbon dioxide gas into a mixture of the polymerization reaction mixture and water and / or adding dry ice to the polymerization reaction mixture.

[0063] In a more preferred example of this preferred embodiment, the washing liquid includes a first washing liquid and a second washing liquid, the first washing liquid is an aqueous solution containing an acid I, the second aqueous solution is an aqueous solution containing an acid II, the acid I is one or more of sulfuric acid, hydrochloric acid, and nitric acid, and the acid II is carbonic acid, and the method for removing at least a portion of the metal ions in the polymerization reaction mixture includes the steps of mixing the polymerization reaction mixture with the first washing liquid to obtain a first mixture, separating a first oil phase from the first mixture, removing at least a portion of the polymerization solvent in the first oil phase, and obtaining a crude liquid polybutadiene, and mixing the first oil phase with water in the presence of carbon dioxide to obtain a second mixture, separating the second oil phase from the second mixture, removing at least a portion of the volatile components in the second oil phase, and obtaining liquid polybutadiene. In this more preferred example, the weight ratio of the first cleaning solution to 1,3-butadiene is preferably 0.5 to 5:1, more preferably 2 to 4:1, and the molar ratio of acid I to the organolithium initiator in the first cleaning solution is preferably 0.1 to 1.5:1, more preferably 0.2 to 1:1, and even more preferably 0.3 to 0.6:1. The acid I is H +The weight ratio of the second cleaning solution to 1,3-butadiene is 1 to 2: 1. The molar ratio of the acid II to the organolithium initiator in the second cleaning solution is preferably 0.1 to 1.5: 1, more preferably 0.2 to 1: 1, and further preferably 0.3 to 0.6: 1. The acid I is H + It is a conversion.

[0064] According to a third aspect of the invention, the present invention provides a liquid polybutadiene produced by the process according to the second aspect of the invention.

[0065] The liquid polybutadiene produced by the method according to the second aspect of the present invention has a high vinyl content and a narrow molecular weight distribution, as well as an appropriate molecular weight and kinematic viscosity. The liquid polybutadiene according to the present invention has excellent fluidity, film-forming properties and applicability, and in particular, the coating formed from the paint containing the liquid polybutadiene according to the present invention has improved adhesion to the substrate.

[0066] According to a fourth aspect of the present invention, there is provided a composition comprising a liquid polybutadiene and at least one additive, said liquid polybutadiene being a liquid polybutadiene according to the first aspect of the present invention.

[0067] The additive may be a substance that can impart new properties to the composition and / or improve the existing properties of the composition. In a preferred embodiment, the additive includes an antioxidant. The antioxidant may be a common antioxidant, for example, the antioxidant may be a phenolic and / or amine antioxidant. Specifically, the antioxidant may be one or more of 4,6-bis(octylthiomethyl)-6-methylphenol, pentaerythritol tetrakis[3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (i.e., antioxidant 264), tri(2,4-di-t-butylphenyl)phosphite (i.e., antioxidant 168), n-octadecyl 3-(3,5-di-t-butyl-4-hydroxyphenyl)propionate (i.e., antioxidant 1076), 2,6-di-t-butyl-p-cresol, t-butylcatechol, and 2,2'-methylene-bis(4-methyl-6-t-butylphenol). The content of the antioxidant may be 0.005 to 2 parts by weight, and is preferably 0.01 to 1 part by weight, relative to 100 parts by weight of liquid polybutadiene.

[0068] According to a fifth aspect of the invention, the present invention provides a polymeric coating comprising a liquid polybutadiene according to the first or third aspect of the invention, or a composition according to the fourth aspect of the invention.

[0069] The polymeric coating of the present invention has high adhesion to the substrate.

[0070] According to a sixth aspect of the present invention, there is provided a pressure sensitive adhesive comprising the liquid polybutadiene according to the first or third aspect of the present invention, or the composition according to the fourth aspect of the present invention.

[0071] According to a seventh aspect of the present invention, the present invention provides a crosslinker comprising a liquid polybutadiene according to the first or third aspect of the present invention, or a composition according to the fourth aspect of the present invention.

[0072] According to an eighth aspect of the present invention, there is provided the use of a liquid polybutadiene according to the first or third aspect of the present invention, or a composition according to the fourth aspect of the present invention, as a crosslinking agent, an adhesive or an electrical insulating material.

[0073] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these.

[0074] Unless otherwise specified, normal temperature and room temperature refer to 25±3°C.

[0075] In the following examples and comparative examples, the content of 1,2-structural units in the liquid polybutadiene was measured using a Bruker AVANCE 400 superconducting nuclear magnetic resonance spectrometer. 1 The resonance frequency of H nucleus is 300.13 MHz, the spectral width is 2747.253 Hz, the pulse width is 5.0 μs, the data points are 16 K, the sample tube diameter is 5 mm, the solvent is deuterated chloroform (CDCl3), the sample concentration is 15 mg / mL, the test temperature is room temperature, the number of scans is 16, and the tetramethylsilane chemical shift is calibrated to 0 ppm.

[0076] In the following examples and comparative examples, the molecular weight and molecular weight distribution index of liquid polybutadiene are measured by gel permeation chromatography analysis, and a Tosoh HLC-8320 type gel permeation chromatograph is used for the gel permeation chromatography analysis, the column is TSKgel SuperMultiporeHZ-N, the standard column is TSKgel SuperMultiporeHZ, the solvent is chromatographically pure tetrahydrofuran (THF), the standard sample is narrow-distribution polystyrene, the polymer sample is prepared as a tetrahydrofuran solution with a mass concentration of 1 mg / mL, the sample injection amount is 10.00 μL, the flow rate is 0.35 mL / min, and the test temperature is 40.0°C.

[0077] In the following examples and comparative examples, the glass transition temperature of liquid polybutadiene is measured using a TA-2980 DSC differential scanning calorimeter according to the method specified in "GB / T 29611-2013 Raw rubber, glass transition temperature", and the heating rate is 20°C / min.

[0078] In the following examples and comparative examples, the content of metal elements in liquid polybutadiene is measured by plasma method, and the test method is specifically as follows: Using Optima 8300 type direct reading full spectrum ICP spectrometer manufactured by PerkinElmer (PE) of the United States, equipped with echelle diffraction grating, solid detector, ultraviolet zone and visible light zone double optical path double solid detector, adopting flat plate plasma technology, the operation parameters of the instrument are as follows: high frequency power 1300W, plasma gas flow rate 15L / min, atomization gas flow rate 0.55L / min, auxiliary gas flow rate 0.2L / min, peristaltic pump speed 1.50mL / min, integration time 10s, plasma is observed in the axial direction. The preparation method of the sample is as follows: Put 2.000g of sample accurately into a porcelain crucible, put it into a high-temperature resistance furnace and gradually heat it to 500℃. After it is completely incinerated, take it out, add 5mL of 10% (V%) dilute nitric acid, slowly heat it on an electric heating plate to completely dissolve it, evaporate the solution to dryness, add 1mL of concentrated nitric acid (concentration 68% by volume), transfer it to a 50mL measuring flask and add water to the constant volume. At the same time, prepare a reagent blank solution.

[0079] In the following examples and comparative examples, the kinematic viscosity of liquid polybutadiene at 45°C is measured with reference to the capillary method specified in GBT10247-2008, where it is measured at a temperature of 45°C using an Ubbelohde viscometer with size number 4B.

[0080] The following examples and comparative examples refer to the following chemical reagents:

[0081] Antioxidant 264, antioxidant 168 and antioxidant 1076: purchased from Sino-Yaoxin Reagent Company; Cyclohexane: purchased from Sinopharma Reagents Co., purity >99.9%, soaked in molecular weight sieve for 15 days, water content less than 5ppm (weight content); 1,3-Butadiene: polymerization grade, purchased from Yanshan Petrochemical Company; n-Butyllithium: purchased from Bailingwei Reagent Co., Ltd., 1.6 mol / L hexane solution; Diethylene glycol dimethyl ether (2G, molecular weight 134): purchased from Bailingwei Reagent Co., Ltd., analytically pure; Diethylene glycol diethyl ether: purchased from Bailingwei Reagent Co., Ltd., analytically pure; Diethylene glycol dibutyl ether: purchased from Bailingwei Reagent Co., Ltd., analytically pure; 1,2-Dipiperidylethane (DPE, molecular weight 196): purchased from Bai Lingwei Reagent Co., Ltd., analytically pure; t-Amyloxy sodium (STA, molecular weight 110): purchased from Bailingwei Reagent Co., Ltd., 1.4 mol / L tetrahydrofuran solution; Sodium menthol (SMT, molecular weight 178): provided by Innochem Reagents Co., Ltd., 1.0 mol / L tetrahydrofuran solution; Sodium ethoxylate (SEO, molecular weight 68): purchased from Bailingwei Reagent Co., Ltd., purity 96%, prepared as a 0.2 mol / L tetrahydrofuran solution; N,N,N',N'-Tetramethylethylenediamine (TMEDA): purchased from Bai Lingwei Reagent Co., Ltd., analytically pure; Methylmorpholine: purchased from Sino-Yaoxin Reagent Co., Ltd., analytically pure; Sulfuric acid: purchased from Bailingwei Reagent Company, concentration 98% by weight, prepared as a 20% by weight solution with water; Nitric acid: purchased from Sino-Yaoxin Reagents Co., Ltd., concentration 68% by weight, prepared as a 20% by weight solution using water.

[0082] Example 1 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0083] (1) Under nitrogen gas protection, cyclohexane, structure modifier 1, structure modifier 2, and 1,3-butadiene (types and amounts used are shown in Table 1, and all amounts used in the table are calculated based on pure compounds) were added to a 5 L reactor, the reactor temperature was lowered to 10°C or lower, a predetermined amount of n-butyllithium (amounts used are shown in Table 1, and all amounts used in the table are calculated based on pure compounds) was added to the 5 L reactor, and an anionic polymerization reaction was carried out at the temperature and reaction pressure shown in Table 1, to obtain a polymerization reaction mixture containing polybutadiene.

[0084] (2) Water and an acid (specific amounts and types of acids used are shown in Table 2, and the amounts used in the table are all calculated based on pure compounds) were added to the polymerization reaction mixture obtained in step (1), and the mixture was stirred for 15 minutes, allowed to stand for stratification, the aqueous phase was separated, and the obtained oil phase was distilled under reduced pressure to remove the liquid polybutadiene crude product.

[0085] (3) Water was added to the liquid polybutadiene crude product obtained in step (2), carbon dioxide gas (specific amounts of water and carbon dioxide used are shown in Table 2) was introduced with stirring, and then the mixture was allowed to stand to form layers, the aqueous phase was separated, and the oil phase was distilled under reduced pressure, and an antioxidant (specific amount and type used are shown in Table 2) was added to the distillation residue to obtain composition PB1 containing liquid polybutadiene according to the present invention. The structure and property parameters of the produced liquid polybutadiene are shown in Table 3.

[0086] Examples 2 to 7 Examples 2-7 illustrate the liquid polybutadiene of the present invention and its method of manufacture.

[0087] In Examples 2 to 7, liquid polybutadiene was produced by the same method as in Example 1, except that compositions PB2 to PB7 containing the liquid polybutadiene according to the present invention were produced under the conditions shown in Table 1, and the structure and property parameters of the produced liquid polybutadienes are shown in Table 3.

[0088] Example 8 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0089] Except for the addition of 50 mmol of n-butyllithium, the liquid polybutadiene was prepared in the same manner as in Example 1 to obtain the liquid polybutadiene-containing composition PB8 according to the present invention, and the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0090] Example 9 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0091] Except for using 200g of water in step (2), the liquid polybutadiene was produced in the same manner as in Example 1 to obtain a composition PB9 containing the liquid polybutadiene according to the present invention, and the structure and property parameters of the produced liquid polybutadiene are shown in Table 3.

[0092] Example 10 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0093] Except for using 30 mmol of sulfuric acid in step (2), the liquid polybutadiene was prepared in the same manner as in Example 1 to obtain the liquid polybutadiene-containing composition PB10 according to the present invention, and the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0094] Example 11 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0095] Except for not carrying out step (3), the liquid polybutadiene was prepared by the same method as in Example 1, and the composition PB11 containing the liquid polybutadiene of the present invention was obtained, in which the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0096] Example 12 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0097] The acid used in step (2) is nitric acid, H + In terms of conversion, the molar amount of nitric acid used is the same as that of sulfuric acid used in Example 1, but the same method as in Example 1 is used to produce liquid polybutadiene, and a composition PB12 containing liquid polybutadiene according to the present invention is obtained, and the structure and property parameters of the produced liquid polybutadiene are shown in Table 3.

[0098] Example 13 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0099] In step (1), except that the structure control agent 1 is diethylene glycol diethyl ether, the liquid polybutadiene is prepared in the same manner as in Example 1 to obtain the liquid polybutadiene-containing composition PB13 according to the present invention, in which the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0100] Example 14 This example illustrates the liquid polybutadiene of the present invention and its method of manufacture.

[0101] In step (1), except that the structure control agent 1 is diethylene glycol dibutyl ether, the liquid polybutadiene is prepared in the same manner as in Example 1 to obtain the liquid polybutadiene-containing composition PB14 according to the present invention, and the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0102] Comparative Example 1 In step (1), the liquid polybutadiene was produced in the same manner as in Example 1, except that the amount of diethylene glycol dimethyl ether used as the structure control agent 1 was 0.4 g, and a liquid polybutadiene-containing composition DPB1 was obtained, and the structure and property parameters of the produced liquid polybutadiene are shown in Table 3.

[0103] Comparative Example 2 In step (1), except that the structure modifier 2, t-amyloxy sodium, was not used, and only the structure modifier 1, diethylene glycol dimethyl ether, was used, the same method as in Example 1 was used to prepare liquid polybutadiene, and a liquid polybutadiene-containing composition DPB2 was obtained, where the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0104] Comparative Example 3 In step (1), the liquid polybutadiene was prepared in the same manner as in Example 1, except that the polymerization reaction temperature was 50°C, and the liquid polybutadiene-containing composition DPB3 was obtained, where the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0105] Comparative Example 4 In step (1), the polymerization temperature was 50°C, and the structure modifier 2, t-amyloxy sodium, was not used, but only the structure modifier 1, diethylene glycol dimethyl ether, was used. The same method as in Example 1 was used to prepare liquid polybutadiene, and a liquid polybutadiene-containing composition DPB4 was obtained. The structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0106] Comparative Example 5 In step (1), polybutadiene was produced in the same manner as in Example 1, except that the amount of n-butyllithium used was 3 mmol, to obtain a polybutadiene-containing composition DPB5, where the structure and property parameters of the produced polybutadiene are shown in Table 3.

[0107] Comparative Example 6 In step (1), except that the amount of n-butyl lithium used was 3 mmol, the amount of diethylene glycol dimethyl ether was 0.08 g, and the amount of t-amyloxy sodium was 0.3 mmol, polybutadiene was produced in the same manner as in Example 1 to obtain a polybutadiene-containing composition DPB6, and the structure and property parameters of the produced polybutadiene are shown in Table 3.

[0108] Comparative Example 7 In step (1), the solvent was tetrahydrofuran, the amount of which was 2300 g, the initiator was sodium naphthalene, the amount of which was 70 mmol, and diethylene glycol dimethyl ether and t-amyloxy sodium were not added. Except for this, the same method as in Example 1 was used to prepare liquid polybutadiene, and polybutadiene-containing composition DPB7 was obtained, and the structure and property parameters of the prepared polybutadiene are shown in Table 3.

[0109] Comparative Example 8 In step (1), except that diethylene glycol dimethyl ether is replaced with an equal amount of TMEDA, and STA is replaced with an equal amount of SMT, liquid polybutadiene is prepared in the same manner as in Example 1 to obtain a liquid polybutadiene-containing composition DPB8, where the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0110] Comparative Example 9 In step (1), except that diethylene glycol dimethyl ether was changed to TMEDA and STA was not added, the liquid polybutadiene was prepared in the same manner as in Example 1 to obtain the liquid polybutadiene-containing composition DPB9, in which the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0111] Comparative Example 10 In step (1), except that diethylene glycol dimethyl ether is replaced with an equal amount of TMEDA, liquid polybutadiene is prepared in the same manner as in Example 1 to obtain a liquid polybutadiene-containing composition DPB10, where the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0112] Comparative Example 11 In step (1), except that the amount of n-butyllithium used was 125 mmol, liquid polybutadiene was prepared in the same manner as in Example 1 to obtain a liquid polybutadiene-containing composition DPB11, where the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0113] Comparative Example 12 338 g of n-hexane was placed in a 1 L flask and cooled to -40°C. A solution of s-butyllithium in cyclohexane (1.0 mol L -1 ) was added, then 84 g of butadiene liquefied at -78°C was added, then 18 g of THF was added to the polymerization liquid, and the mixture was stirred at -20°C for 4 hours to obtain liquid polybutadiene DPB12, the structure and properties of which are shown in Table 3.

[0114] Comparative Example 13 338 g of n-hexane was placed in a 1 L flask and cooled to -40°C. A solution of s-butyllithium in cyclohexane (1.0 mol L -1 ) was added, then 84 g of butadiene liquefied at -78°C was added, then 18 g of THF was added to the polymerization liquid, and the mixture was stirred at -20°C for 120 minutes to obtain liquid polybutadiene DPB13, the structure and properties of which are shown in Table 3.

[0115] Comparative Example 14 338 g of n-hexane was placed in a 1 L flask and cooled to -40°C. A solution of s-butyllithium in cyclohexane (1.0 mol L -1 ) was added, then 84 g of butadiene liquefied at -78°C was added, then 18 g of THF was added to the polymerization liquid, and the mixture was stirred at -20°C for 120 minutes to obtain polybutadiene DPB14, the structure and properties of which are shown in Table 3.

[0116] Comparative Example 15 In step (1), except that 1,2-dipiperidylethane is replaced with an equivalent amount of methylmorpholine, liquid polybutadiene is prepared in the same manner as in Example 7 to obtain a liquid polybutadiene-containing composition DPB15, where the structure and property parameters of the prepared liquid polybutadiene are shown in Table 3.

[0117] [Table 1] JPEG0007571158000009.jpg135169

[0118] [Table 2]

[0119] [Table 3] JPEG0007571158000012.jpg168169

[0120] Test Example The compositions prepared in Examples 1 to 14 were uniformly applied to the surface of copper foil to a coating thickness of 0.6 mm, crosslinked and cured at 120°C for 2 hours, and the peel strength was measured according to the method specified in IPC-TM-650 2.4.08C. The experimental results are shown in Table 4.

[0121] Comparative test examples The peel strength of the compositions prepared in Comparative Examples 1 to 4 and 7 to 15, B3000 and B2000 was measured in the same manner as in the Test Examples. The experimental results are shown in Table 4.

[0122] [Table 4]

[0123] As can be seen from Tables 3 and 4, the liquid polybutadienes according to the present invention not only have a high content of 1,2-structural units and a narrow molecular weight distribution, but also have appropriate molecular weights and kinetic viscosities at 45°C, and have excellent fluidity, coatability and film-forming properties, and the polymer coatings formed by crosslinking and curing have high adhesion to substrates. Among these, the liquid polybutadienes prepared in Comparative Examples 11, 13 and 14 have low kinetic viscosities, poor coatability and film-forming properties, and it is difficult to form polymer coatings with uniform thickness and performance.

[0124] In addition, the liquid polybutadiene according to the present invention has a low metal ion content, and is suitable as a crosslinking agent, an adhesive, or an electrical insulating material.

[0125] Although the preferred embodiments of the present invention have been described in detail above, the present invention is not limited thereto. Many simple modifications may be made to the technical solution of the present invention without departing from the technical concept of the present invention, including combining each technical feature in any suitable manner, and these simple modifications and combinations should also be considered as the disclosure of the present invention, and all belong to the patent scope of the present invention.

Claims

1. A liquid polybutadiene having a number average molecular weight of 2500 to 5500, a molecular weight distribution index of 1 to 1.2, a 1,2-structural unit content of 85 to 95% by weight, a 1,4-structural unit content of 5 to 15% by weight, a molar ratio of cis-1,4-structural units to trans-1,4-structural units of 1 to 2:1, a kinetic viscosity at 45°C of 100 to 500 P, and fluidity at a temperature of 25°C.

2. 2. The liquid polybutadiene of claim 1, wherein the molar ratio of cis 1,4-structural units to trans 1,4-structural units is 1.3-1.9:

1.

3. 3. The liquid polybutadiene according to claim 1, wherein the content of 1,2-structural units in said liquid polybutadiene is 87 to 94% by weight based on the total weight of said liquid polybutadiene.

4. 2. The liquid polybutadiene according to claim 1, having a number average molecular weight of 2,800 to 5,000.

5. 5. The liquid polybutadiene according to claim 1, having a molecular weight distribution index of 1.01 to 1.

09.

6. 6. The liquid polybutadiene according to claim 5, having a molecular weight distribution index of 1.02 to 1.

06.

7. 7. The liquid polybutadiene according to claim 1, wherein the weight content of metal elements in said liquid polybutadiene is 200 ppm or less based on the total amount of said liquid polybutadiene.

8. 8. The liquid polybutadiene according to claim 7, wherein the weight content of metal elements in said liquid polybutadiene is 20 ppm or less based on the total amount of said liquid polybutadiene.

9. The liquid polybutadiene according to any one of claims 1 to 8, having a glass transition temperature of -32°C to -12°C.

10. The liquid polybutadiene according to any one of claims 1 to 9, having a kinematic viscosity at 45°C of 150 to 350 P.

11. The liquid polybutadiene according to any one of claims 1 to 3, having a number average molecular weight of 2,500 to 4,000 and a kinematic viscosity at 45°C of 100 to 280 P.

12. The liquid polybutadiene according to any one of claims 1 to 3, having a molecular weight distribution index of 1 to 1.

05.

13. The liquid polybutadiene according to any one of claims 1 to 3, having a number average molecular weight of more than 4,000 and not more than 5,500, and a kinematic viscosity at 45°C of more than 280P and not more than 500P.

14. The liquid polybutadiene according to any one of claims 1 to 3, having a molecular weight distribution index of 1 to 1.

08.

15. The method includes contacting 1,3-butadiene with a structure-controlling agent and an organolithium initiator in a polymerization solvent under anionic polymerization reaction conditions to obtain a polymerization reaction mixture containing polybutadiene, the contacting being carried out at a temperature of -10°C to 20°C, the structure-controlling agent containing component A and component B, component A being one or more selected from ethers and amines, and component B being one or more selected from alkali metal alkoxides, the molar ratio of organolithium initiator:component A:component B being 1:0.05-0.3:0.03-0.2, and the organolithium initiator being calculated in terms of lithium, The method for producing liquid polybutadiene according to any one of claims 1 to 14, wherein component A is one or more selected from diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol di-n-propyl ether, diethylene glycol di-n-butyl ether, 1,2-dipiperidylethane, and the compound represented by formula II. 【Chemistry 1】 (In formula II, R 5 and R 6 are the same or different, and each independently represents a hydrogen atom or C 1 ~C 6 is alkyl, R 7 and R 8 are the same or different, and each independently represents 1 ~C 6 alkylene, R 9 , R 10 , R 11 , R 12 , R 13 , R 14 , R 15 and R 16 are the same or different, and each independently represents a hydrogen atom or C 1 ~C 6 is alkyl, m is an integer from 1 to 5.

16. The method according to claim 15, wherein the alkali metal alkoxide is one or more selected from the compounds represented by formula III: 【Chemistry 2】 (In formula III, R 17 is C 1 ~C 20 Alkyl, C 6 ~C 30 Aryl or C 4 ~C 20 is cycloalkyl, M is an alkali metal atom.

17. The method according to claim 15, wherein said component B is one or more selected from the group consisting of sodium t-butoxide, sodium t-amyloxy, sodium menthol, sodium ethoxide and sodium n-hexyloxide.

18. 18. The method of any one of claims 15 to 17, wherein the molar ratio of organolithium initiator: component A: component B is 1:0.1-0.2:0.05-0.15, and the organolithium initiator is calculated as lithium.

19. 19. The method according to any one of claims 15 to 18, wherein the molar ratio of component B:component A is 0.4-1.5:

1.

20. 20. The method of claim 19, wherein the molar ratio of component B to component A is 0.5-1:

1.

21. The method of any one of claims 15 to 20, wherein the amount of organolithium initiator used is such that the number average molecular weight of the liquid polybutadiene produced is 2500 to 5500.

22. The method of any one of claims 15 to 21, wherein the contacting is carried out at a temperature of from -5°C to 10°C.

23. The method according to any one of claims 15 to 22, wherein the content of 1,3-butadiene is 1 to 15% by weight, based on the total amount of the polymerization solvent and 1,3-butadiene.

24. A composition comprising a liquid polybutadiene and at least one additive, said liquid polybutadiene being the liquid polybutadiene according to any one of claims 1 to 14.

25. 25. The composition of claim 24, wherein the additive comprises an antioxidant.

26. A polymeric coating comprising a liquid polybutadiene polymer according to any one of claims 1 to 14, or a composition according to any one of claims 24 and 25.

27. A pressure-sensitive adhesive comprising the liquid polybutadiene according to any one of claims 1 to 14, or the composition according to any one of claims 24 and 25.

28. A crosslinking agent comprising the liquid polybutadiene according to any one of claims 1 to 14, or the composition according to any one of claims 24 and 25.

29. Use of the liquid polybutadiene according to any one of claims 1 to 14, or the composition according to any one of claims 24 and 25, as a crosslinking agent, adhesive or electrical insulating material.

Citation Information

Patent Citations

  • Preparation method of low-molecular-weight liquid polydiolefin

    CN107805288A

  • JP1969027469B

  • Synthesis of high vinyl rubber

    JP2003321510A

  • Ethylene polymer conductor coating fabricated using polybutadiene co-crosslinking agent

    JP2015520916A

  • Process for preparing conjugated diene (CO)polymers in the presence of a catalytic system comprising a pyridyl iron (III) complex

    US20190270832A1