Method for determining the oxygen absorption capacity of oxygen absorbers

The use of an oxygen absorbing composition with glycerin, copper sulfate, and an alkaline compound, combined with inorganic fine particles, enhances the oxygen absorption capacity of particulate scavengers, achieving effective oxygen scavenging.

JP7571392B2Active Publication Date: 2024-10-23TOPPAN HOLDINGS INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020089220
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-21
Publication Date
2024-10-23
Estimated Expiration
2040-05-21

AI Technical Summary

Technical Problem

Existing particulate oxygen scavengers have limited oxygen absorption capacity, necessitating an improvement in their performance.

Method used

An oxygen absorbing composition comprising glycerin, copper sulfate, and an alkaline compound, with composite particles having a sedimentation rate of 2 mm/sec or more, and inorganic fine particles attached to enhance oxygen absorption.

Benefits of technology

The composition achieves improved oxygen absorption capacity, as evidenced by a sedimentation rate of 2 mm/sec or more, resulting in effective oxygen scavenging.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571392000001
    Figure 0007571392000001
  • Figure 0007571392000002
    Figure 0007571392000002
Patent Text Reader

Abstract

To provide a granular deoxidant where oxygen absorption capacity is further improved.SOLUTION: A deoxidant is powders containing a plurality of composite particles having a granulated material including a porous carrier and an oxygen absorbing composition carried by the carrier and inorganic fine particles stuck on the surface of the granulated material. The oxygen absorbing composition contains glycerol, copper sulfate and an alkaline compound. The sedimentation rate of the composite particles in an aqueous solution containing glycerol and copper sulfate is 2 mm / s or more per one particle.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an oxygen absorber and a method for producing the same.The present invention also relates to an oxygen absorber package and a food package containing the oxygen absorber. [Background technology]

[0002] In order to preserve food for a long period of time, oxygen absorbers are sometimes enclosed in food packaging containers. Conventional oxygen absorbers are generally granular materials in which a liquid oxygen absorbing substance is granulated together with a carrier (for example, Patent Documents 1 to 3). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 4821692 [Patent Document 2] JP 2003-144112 A [Patent Document 3] Patent No. 3541859 Summary of the Invention [Problem to be solved by the invention]

[0004] A main object of the present invention is to further improve the oxygen absorbing capacity of a granular oxygen absorber. [Means for solving the problem]

[0005] One aspect of the present invention is An oxygen absorbing composition comprising glycerin, copper sulfate, and an alkaline compound. Porous support On the body Supported Tazo Granules and inorganic fine particles attached to the surface of the granulated material and A powder containing a plurality of composite particles, Method for determining oxygen absorption capacity of And , G In an aqueous solution containing lycerol and copper sulfate Measure the settling velocity of the composite particles. The settling velocity is 2 mm / sec or more per particle. In this case, the oxygen absorber is judged to have the oxygen absorption capacity to reduce the oxygen concentration in a sealed gas barrier bag containing 2.0 g of oxygen absorber and 500 mL of air to 8% or less after 24 hours. Oxygen absorber Method for determining oxygen absorption capacity of It is.

[0007] The oxygen absorbing composition contains glycerin, copper sulfate, and an alkaline compound, and inorganic fine particles are attached to the surface of the granulated material so that the settling speed of the composite particles in an aqueous solution containing glycerin and copper sulfate is 2 mm / sec or more per particle, thereby allowing the inherent oxygen absorbing properties of glycerin to be exerted, resulting in an oxygen scavenger with improved oxygen absorbing capacity.

[0008] The present invention also provides an oxygen absorber package comprising the oxygen absorber and a breathable packaging material containing the oxygen absorber.The present invention further provides a food package comprising the oxygen absorber package and a food packaging container in which the oxygen absorber package is enclosed. Effect of the Invention

[0009] The present invention can provide a granular oxygen scavenger having improved oxygen absorbing capacity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, several embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.

[0011] The oxygen scavenger according to one embodiment is a composite particle mainly composed of a granulated material containing a porous support and an oxygen absorbing composition supported on the support, and inorganic fine particles adhering to the surface of the granulated material.

[0012] The support may be any porous particle capable of supporting the oxygen absorbing composition. Usually, the oxygen absorbing composition is supported on the support by impregnating the support with the oxygen absorbing composition. The support may be selected from the group consisting of activated carbon, zeolite particles, bentonite particles, activated alumina particles, activated clay, calcium silicate particles, and diatomaceous earth.

[0013] The oxygen absorbing composition contains glycerin, copper sulfate, and an alkaline compound.

[0014] The amount of glycerin is usually 80 to 200 parts by mass, and may be 100 to 180 parts by mass, relative to 100 parts by mass of the support. When the amount of glycerin is within this range, it tends to be easy to obtain an oxygen scavenger having an appropriate oxygen absorption capacity.

[0015] The presence of water may be preferable for the oxygen absorption reaction. Therefore, 30 to 85 parts by mass of water, particularly 30 to 70 parts by mass of water may be added to 100 parts by mass of glycerin. When the amount of water is within this range, it is easy to obtain an oxygen scavenger having an appropriate oxygen absorption capacity.

[0016] The alkaline compound is a compound that forms an alkaline aqueous solution when dissolved in water. The alkaline compound ionizes the hydroxyl group of glycerin, activating the oxygen absorption reaction. In the state of the oxygen absorbing composition, a part of the alkaline compound is often dissolved in glycerin. The alkaline compound may be a hydroxide, carbonate, hydrogen carbonate, triphosphate, or diphosphate of an alkali metal or an alkaline earth metal. The alkaline compound may be one or more compounds selected from the group consisting of lithium hydroxide, sodium hydroxide, potassium hydroxide, rubidium hydroxide, cesium hydroxide, beryllium hydroxide, magnesium hydroxide, calcium hydroxide, strontium hydroxide, radium hydroxide, lithium carbonate, sodium carbonate, calcium carbonate, magnesium carbonate, potassium carbonate, potassium hydrogen carbonate, sodium hydrogen carbonate, lithium hydrogen carbonate, trisodium phosphate, trisodium potassium phosphate, disodium phosphate, and disodium potassium phosphate.

[0017] The amount of the alkaline compound is usually 100 to 300 parts by mass, and may be 150 to 250 parts by mass, relative to 100 parts by mass of the support. When the amount of the alkaline compound is within this range, it tends to be easy to obtain an oxygen scavenger having an appropriate oxygen absorption capacity.

[0018] Copper sulfate is added to promote the oxygen absorption reaction of glycerin. In the state of the oxygen absorbing composition, copper sulfate is often dissolved in glycerin. The copper sulfate may be any copper sulfate, and may be anhydride, pentahydrate, or other hydrates. Moreover, regardless of the oxidation number, it may be copper sulfate (I) or copper sulfate (II).

[0019] The amount of copper sulfate, calculated as an anhydride, is 15 to 30 parts by mass, and may be 18 to 26 parts by mass, per 100 parts by mass of glycerin. When the amount of the transition metal compound is within this range, it tends to be easy to obtain an oxygen scavenger having an appropriate oxygen absorption capacity.

[0020] The support or the oxygen absorbing composition may contain a binder so that the granules can be easily formed. Specific examples of the binder include gum arabic, polyvinyl alcohol, sodium alginate, gelatin, and cellulose. The amount of the binder is usually 0 to 30 parts by mass, and may be 10 to 20 parts by mass, based on 100 parts by mass of the support.

[0021] The oxygen absorbing composition may further contain other substances. Examples of the other substances include catechol-based compounds. The amount of the other substances is usually about 30 parts by mass or less per 100 parts by mass of the support.

[0022] The particle size (maximum width) of the granulated material before the inorganic fine particles are attached is not particularly limited, but may be, for example, 0.3 mm or more, 8.0 mm or less, 4.5 mm or less, 1.8 mm or less, or 1.5 mm or less. The shape of the granulated material is not particularly limited, but may be, for example, cylindrical or spherical. In the case of a cylindrical granulated material, the length of the side may be 0.3 mm or more, and 4.5 mm or less. The diameter of the cylindrical bottom may be 0.3 mm or more, 1.8 mm or less, or 1.5 mm or less. When the particle size or size of the granulated material is small, a higher oxygen absorption capacity tends to be obtained.

[0023] The granulated material composed of the support and the oxygen absorbing composition can be obtained by granulating a mixture containing the support and the components constituting the oxygen absorbing composition. The components constituting the oxygen absorbing composition may be mixed together or separately. The mixer for mixing is not particularly limited, and may be, for example, a container rotation type mixer such as a cylindrical type or a V type, or a container fixed type mixer such as a ribbon type, a horizontal screw type, a paddle type, or a planetary motion type.

[0024] The granulated material can be obtained by granulation, for example, extrusion granulation, stirring granulation, fluidized bed granulation, rolling granulation, or compression granulation. Extrusion granulation can be performed, for example, using a screen having a predetermined opening. Granulated materials obtained by extrusion granulation are often cylindrical.

[0025] The inorganic fine particles are water-insoluble particles containing an inorganic substance as a main component. The inorganic fine particles usually contain 50 parts by mass or more of the inorganic substance based on the total mass of the inorganic fine particles. The inorganic substance may be, for example, at least one selected from the group consisting of silicon dioxide, calcium silicate hydrate, and magnesium oxide. By attaching the inorganic fine particles to the surface of the granulated product, the surface area of ​​the granulated product can be increased, and the oxygen absorption performance can be improved.

[0026] The faster the inorganic fine particles attached to the granules absorb the oxygen absorbing composition, the faster the oxygen absorbing composition contained inside the granules can be transferred to the inorganic fine particles, and the more improved the oxygen absorbing performance can be. The speed at which the oxygen absorbing composition is absorbed is determined by the affinity between the inorganic fine particles and the aqueous solution containing glycerin and copper sulfate.

[0027] The affinity between inorganic fine particles and the aqueous solution can be understood as the settling speed of composite particles in the aqueous solution. Granulated materials to which inorganic fine particles are not attached have a lower density than the aqueous solution, and do not settle because of the low affinity between the granulated material surface and the aqueous solution. On the other hand, composite particles in which inorganic fine particles having a high affinity with the aqueous solution are attached to the surface of the granulated material settle because the inorganic fine particles on the surface absorb the aqueous solution and the composite particles become heavier. The higher the affinity between inorganic fine particles and the aqueous solution, the faster the aqueous solution is absorbed, and therefore the faster the settling speed. The affinity can be evaluated using the settling speed to evaluate the oxygen absorption speed.

[0028] The concentration of the aqueous solution is 15 to 30 parts by mass, or may be 18 to 26 parts by mass, of copper sulfate calculated as an anhydride, relative to 100 parts by mass of glycerin. Furthermore, the amount of water is 30 to 85 parts by mass, or may be 30 to 70 parts by mass, relative to 100 parts by mass of glycerin. The concentration of the aqueous solution is preferably the same as the concentration of the oxygen absorbing composition contained in the granulated product. When the concentrations of the aqueous solution and the oxygen absorbing composition are the same, the ease of migration of the oxygen absorbing composition to the inorganic fine particle portion can be more accurately quantified.

[0029] When the settling velocity of the composite particles is 2 mm / sec or more per composite particle, a high oxygen absorption capacity tends to be obtained. From the same viewpoint, the settling velocity of each composite particle may be 2.5 mm / sec or more, 5 mm / sec or more, or 10 mm / sec or more. There is no particular upper limit to the settling velocity. In addition, the mass of each composite particle may be, for example, 0.3 to 10.0 mg.

[0030] The settling velocity of the composite particles can be determined by placing an aqueous solution containing glycerin and copper sulfate in a container with a certain volume, gently placing one composite particle on the liquid surface, and measuring the time it takes for the settling composite particle to reach the bottom of the container and the distance from the bottom of the container to the liquid surface. Details of the method for measuring the settling velocity will be described in the Examples below.

[0031] The inorganic fine particles may have an average particle size of 150 μm or less. By making the inorganic fine particles have an average particle size of 150 μm or less, the oxygen absorption capacity of the oxygen scavenger can be further improved. The surface of the granulated material usually has fine irregularities, and inorganic fine particles having a small particle size tend to enter the recesses on the surface of the granulated material. This results in a significant increase in the surface area of ​​the granulated material, which is thought to contribute to improving the oxygen absorption capacity. From the same perspective, the inorganic fine particles may have an average particle size of 100 μm or less, or 50 μm or less. The lower limit of the average particle size is not particularly limited, but since nano-sized fine particles are expensive and difficult to handle, it may be, for example, 0.1 μm or more. The average particle size here is the value of the secondary particle size measured by a laser diffraction method.

[0032] The pore volume of the inorganic fine particles may be 0.5 mL / g or more. When the pore volume of the hydrophilic inorganic fine particles is 0.5 mL / g or more, the oxygen absorption capacity of the oxygen scavenger can be further improved. It is considered that inorganic fine particles having a large pore volume are likely to absorb the oxygen absorbing composition near the surface of many granules. When the oxygen absorbing composition is absorbed into the inorganic fine particles, the contact area between the oxygen absorbing composition and oxygen in the environment increases, and as a result, it is presumed that the oxygen absorption capacity is improved. From the same viewpoint, the pore volume of the inorganic fine particles may be 0.8 mL / g or more, or 1.2 mL / g or more. The upper limit of the pore volume is not particularly limited, but may be, for example, 10 mL / g or less. The pore volume here is a value measured by a nitrogen adsorption method or a mercury intrusion method. It is sufficient that the pore volume measured by at least one of the nitrogen adsorption method and the mercury intrusion method is within the above numerical range.

[0033] The inorganic fine particles having the above-mentioned average particle diameter and pore volume can be produced by a conventional method, or can be obtained by appropriately selecting from among commercially available products.

[0034] The amount of inorganic fine particles attached to the surface of the granulated material (adhesion amount) may be 0.1 parts by mass or more, 0.5 parts by mass or more, 1 part by mass or more, 2 parts by mass or more, or 3 parts by mass or more, based on 100 parts by mass of the granulated material. When the adhesion amount of inorganic fine particles is within these ranges, the oxygen absorbing ability of the oxygen scavenger is easily obtained. The upper limit of the adhesion amount of inorganic fine particles is not particularly limited, but may be 30 parts by mass or less, 25 parts by mass or less, 15 parts by mass or less, 10 parts by mass or less, or 8 parts by mass or less, from the viewpoint of granulation property, etc. Inorganic fine particles not attached to the granulated material may be mixed with the particles of the oxygen scavenger, but the amount of inorganic fine particles alone is not included in the above adhesion amount.

[0035] The volume ratio of the granulated material based on the entire oxygen scavenger may be more than 60%. When the volume ratio of the granulated material is in an appropriate range, a particularly high oxygen absorption capacity is easily obtained. From the same viewpoint, the volume ratio of the granulated material may be 70% or more, or 80% or more, or may be 98% or less.

[0036] The inorganic fine particles are usually attached over the entire surface of the granulated product. However, it is not always necessary for the surface of the granulated product to be completely covered with the inorganic fine particles, and the inorganic fine particles may be distributed over the entire surface of the granulated product with spaces between them.

[0037] The oxygen scavenger can be obtained by a method including a step of adhering inorganic fine particles to a granulated material containing a carrier and an oxygen absorbing composition. For example, the granulated material and inorganic fine particles are mixed, and the obtained powder mixture is shaken to allow the inorganic fine particles to adhere to the granulated material.

[0038] The inorganic fine particles attached to the granulated material by the above-mentioned method of mixing powders together form a relatively thin layer, and in this respect, the form of the oxygen absorber of this embodiment is generally different from that of a tablet having an outer shell obtained by, for example, tablet compression. Specifically, the inorganic fine particles attached to the surface of the granulated material can form a layer having a thickness of 1 mm or less, or 0.7 mm or less. The fact that the layer of the inorganic fine particles is thin can also be confirmed by detecting elements contained in the material constituting the granulated material (glycerin, alkaline compound, or copper sulfate) when the surface of the composite particle is subjected to elemental analysis by energy dispersive X-ray analysis (EDX analysis). Generally, in the case of the oxygen absorber according to this embodiment, at least one element contained in the material constituting the granulated material is often detected at a concentration of 0.05 atomic % or more, or 0.1 atomic % or more. On the other hand, when a certain thickness of the outer shell containing the granulated material is formed by tablet compression, the elements of the material constituting the granulated material are not substantially detected by EDX analysis.

[0039] The oxygen absorbing package according to one embodiment may be mainly composed of the oxygen absorbing agent according to the above embodiment and a breathable packaging material containing the oxygen absorbing agent. The breathable packaging material may be appropriately selected from those commonly used in the technical field. Specific examples of the breathable packaging material include a bag formed of a base material consisting of a perforated plastic film, a nonwoven fabric, a microporous film, paper, or a combination thereof. The oxygen absorbing agent package may be contained in various food packaging containers and used for the purpose of maintaining the freshness of food, for example.

[0040] The food package according to one embodiment includes the oxygen absorber package and a food packaging container in which the oxygen absorber package is enclosed. The food packaging container can be appropriately selected from those commonly used in the field of food packaging, and a sealable container is preferable. Examples of the food packaging container include a bag, a deep-draw package, a tray package, and a stretch package. EXAMPLES

[0041] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0042] 1. Granulated materials The raw materials shown in Table 1 were uniformly mixed in a sealed state to obtain a mixture containing activated carbon and an oxygen absorbing composition containing an oxygen scavenger supported on the activated carbon, an alkali compound, a transition metal salt, and a binder. The obtained mixture was granulated by an extrusion granulator equipped with a screen with a screen hole diameter of 1.0 mmφ and an aperture ratio of 22.6%, to obtain a granulated powder consisting of granular granulated material. Table 1 shows the blending amount of each raw material in parts by mass.

[0043] [Table 1]

[0044] 2.Inorganic fine particles The following inorganic fine particles were prepared. · Silopage 720 (hydrophilic silicon dioxide powder, manufactured by Fuji Silysia Chemical) NipSeal SS-50B (hydrophobic silicon dioxide powder, made by Tosoh Silica) Calcium hydroxide (Kanto Chemical)

[0045] 3. Oxygen absorbers Example 1 30 g of the granules and 1.5 g of Silopage 720, a hydrophilic silicon dioxide powder, were placed in an oxygen barrier bag, and the bag was heat-sealed. The bag was shaken to form an oxygen absorber in which the granules were covered with inorganic fine particles. The bag was opened and heat-sealed again to expel the air inside, and the oxygen absorber was stored. Example 2 An oxygen scavenger was prepared and stored in the same manner as in Example 1, except that 30 g of the granules and 2.4 g of Silopage 720 were placed in an oxygen barrier bag. Comparative Example 1 An oxygen scavenger was prepared and stored in the same manner as in Example 1, except that 30 g of the granules and 6 g of calcium hydroxide were placed in an oxygen barrier bag. Comparative Example 2 An oxygen scavenger was prepared and stored in the same manner as in Example 1, except that 30 g of the granules and 1.5 g of calcium hydroxide were placed in an oxygen barrier bag. Comparative Example 3 An oxygen scavenger was prepared and stored in the same manner as in Example 1, except that 30 g of the granules and 1.5 g of hydrophobic silicon dioxide were placed in an oxygen barrier bag. Comparative Example 4 30 g of the granulated material was placed in an oxygen barrier bag, and the bag was heat-sealed without adding any inorganic fine particles and stored.

[0046] 4. Sedimentation velocity The settling velocity of the granulated material (composite particles) to which the inorganic fine particles were attached was measured by the following procedure. (1) An aqueous solution containing 30 parts by mass of copper (II) sulfate pentahydrate and 40 parts by mass of water per 100 parts by mass of glycerin was prepared and designated solution A. This solution A was kept at 25°C. (2) The oxygen scavenger was passed through a sieve with 1 mm mesh, and composite particles remaining on the sieve and having a particle size of 1 mm or more were selected. (3) Solution A was poured into a cylindrical glass bottle with an opening of 30 mm in diameter until it was 50 mm from the bottom. (4) One composite particle obtained in (2) was picked up with tweezers and gently placed on the surface of solution A in (3), and the time it took for the composite particle to settle and reach the bottom of the glass bottle was measured. (5) The settling velocity was calculated using the following formula. The average value of the values ​​measured using five different composite particles was used. Settling speed [mm / s] = 50 [mm] / time to reach bottom [s]

[0047] 5. Oxygen absorption capacity 2.0 g of oxygen absorber was placed in a bag (60 mm long, 60 mm wide) made of perforated packaging material to prepare an oxygen absorber package. A laminated material consisting of polyethylene terephthalate / polyethylene / paper / polyethylene was used as the effective packaging material. The oxygen absorber package was placed in a gas barrier bag together with absorbent cotton (water activity 0.95) soaked in a 44% sucrose aqueous solution. The bag was sealed, 500 mL of air was injected into it, and the bag was left in an atmosphere of 25°C. The oxygen concentration in the bag was measured after 24 hours. An oxygen concentration of 8% or less was judged as "Good", 13% or less was judged as "Good", and more than 13% was judged as "Poor". A low oxygen concentration means a high oxygen absorption capacity.

[0048] 6.Results Table 2 shows the types of inorganic fine particles, the settling speed (average value of n=5) of the composite particles to which the inorganic fine particles are attached, and the evaluation results of the oxygen absorption capacity. In the reference example, the granulated material was not covered with inorganic fine particles, but was used as an oxygen absorber as it is. It was confirmed that oxygen absorbers with a settling speed of 2 mm / sec or more exhibited excellent oxygen absorption capacity.

[0049] [Table 2] [Industrial Applicability]

[0050] The present invention is useful as an oxygen scavenger for food preservation and the like.

Claims

1. A method for determining the oxygen absorbing ability of an oxygen scavenger, which is a powder containing a plurality of composite particles including a granule in which an oxygen absorbing composition containing glycerin, copper sulfate, and an alkaline compound is supported on a porous support, and inorganic fine particles adhering to a surface of the granule, comprising: A method for determining the oxygen absorption capacity of an oxygen absorber, comprising: measuring the settling velocity of the composite particles in an aqueous solution containing glycerin and copper sulfate; and determining that the composite particles have an oxygen absorption capacity that reduces the oxygen concentration after 24 hours to 8% or less in a gas barrier bag sealed with 2.0 g of the oxygen absorber and 500 mL of air.

2. The method for determining the oxygen absorption capacity of an oxygen scavenger according to claim 1, wherein the concentration of the aqueous solution is such that the amount of copper sulfate is 15 to 30 parts by mass, calculated as an anhydride, relative to 100 parts by weight of glycerin, and the amount of water is 30 to 85 parts by mass relative to 100 parts by weight of glycerin.

Citation Information

Patent Citations

  • JP1973021692B1

  • Free-oxygen absorber composition

    JP2003144112A

  • Deoxidant and method for producing the same

    JP2017104845A

  • Deoxidizer and production method of the same

    JP2017104846A

  • Oxygen scavenger and manufacturing method thereof

    JP2017225952A