Method for obtaining chlorine leachate from platinum group metal-containing material

By adding a reducing agent like hydrazine or sodium sulfite to the slurry before solid-liquid separation in the chlorine leaching process, the method addresses high gold content issues, enhancing operational efficiency and reducing solvent extraction loads in platinum group element recovery.

JP7571501B2Active Publication Date: 2024-10-23SUMITOMO METAL MINING CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020197148
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-27
Publication Date
2024-10-23
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

Conventional methods for recovering platinum group elements from copper electrolytic slime face challenges such as high energy consumption, environmental contamination, and inefficiencies due to high gold content in the leachate, which increases the load on subsequent solvent extraction processes and reduces operational efficiency.

Method used

A method involving chlorine leaching of platinum group element-containing materials with a reducing agent added to the slurry before solid-liquid separation to reduce gold content, using agents like hydrazine or sodium sulfite, optimizing the amount based on redox potential or fixed volume, to form a precipitate and separate it effectively.

Benefits of technology

Effectively reduces gold content in the leachate, preventing decreases in operational efficiency and solvent extraction load, while maintaining high recovery rates of platinum group elements.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571501000009
    Figure 0007571501000009
  • Figure 0007571501000001
    Figure 0007571501000001
  • Figure 0007571501000002
    Figure 0007571501000002
Patent Text Reader

Abstract

To provide a method for effectively reducing the gold which is usually included in a leachate obtained by chlorine-bleeding a platinum group-including material including at least gold as an impurity element, for example, capable of preventing deterioration of the operation efficiency of a solvent extraction treatment in a post-process.SOLUTION: Disclosed is a method for obtaining a chlorine leachate by making chlorine leach from the platinum group element-including material containing gold as an impurity element and then carrying out a solid-liquid separation treatment. The method includes reducing the gold included in a slurry obtained by chlorine leaching by adding a reducer to the slurry prior to the solid-liquid separation treatment, and separating the chlorine leachate from a leach residue including the precipitate of reduced gold by the solid-liquid separation treatment. Hydrazine or sodium sulfite can be used for example, as the reducer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for subjecting a platinum group element-containing material containing gold as an impurity element to chlorine leaching and then obtaining a chlorine leachate by solid-liquid separation treatment. More specifically, the present invention relates to a method for obtaining a chlorine leachate in which the gold content is effectively reduced. [Background technology]

[0002] Conventionally, a method for recovering precious metal elements from copper electrolytic slime has been carried out by removing copper from the copper electrolytic slime using a wet method, separating selenium, antimony, lead, tin, bismuth, tellurium, etc. using a dry method, and finally obtaining an alloy of gold, silver, and platinum group metals, which is then electrolytically operated. However, such conventional methods have problems such as a long time until the precious metals are recovered, which increases the interest burden during the retention period in the system, a large amount of energy consumption, difficulty in automating the process because solid materials must be transported for each process, pollution of the working environment due to exhaust gas, and low adaptability to the composition of slime and the form of the compound.

[0003] In response to this, for example, Patent Document 1 proposes a method for selectively recovering gold, platinum group elements, selenium, and tellurium from copper electrolytic slime with a high yield by simple wet processing alone. The method disclosed in Patent Document 1 can effectively solve the problems of the conventional method.

[0004] Furthermore, as an improvement over the method disclosed in Patent Document 1, Patent Document 2 proposes a method in which, after recovering most of the gold, a step of concentrating the platinum group elements using an ion exchange resin is added to obtain a platinum group element concentrate (hereinafter also referred to as "PGM concentrate"; PGM: Platinum Group Metals), and the platinum group elements are preferentially recovered.

[0005] Specifically, a method is carried out in which PGM concentrate is used as the starting material, chlorine leaching is carried out under conditions that facilitate the leaching of the platinum group elements, and a PGM leachate (hereinafter also referred to as "chlorine leachate") and a residue (leach residue) are obtained in a solid-liquid separation process. Since the platinum group elements have been preferentially leached from the obtained PGM leachate by the chlorine leaching, the platinum group elements can be effectively recovered by further processing in a post-process. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2001-207223 A [Patent Document 2] JP 2013-104064 A Summary of the Invention [Problem to be solved by the invention]

[0007] In the method disclosed in the above-mentioned Patent Document 2, it is known that the PGM leachate obtained by chlorine leaching contains a small amount of gold, for example, about 0.2 g / L or less. This is because most of the gold is recovered in the PGM concentrate, which is the starting material, and gold inevitably remains in the PGM leachate obtained by leaching the PGM concentrate. For this reason, gold has traditionally been extracted in a post-process using a solvent extraction method (Au·Sb-SX). The extracted gold is recovered as reduced gold powder by reduction stripping from an organic solvent, and is then repeatedly processed in the pre-process, the copper electrolytic slime leaching process.

[0008] However, depending on the raw material conditions, the PGM concentrate may contain more gold than before, and in conventional operations, for example, about 2 to 4 g / L of gold (more than 10 times the conventional amount) may remain in the PGM leachate. This increases the load on the post-processing process using solvent extraction, and may reduce operational efficiency. For example, the amount of processing liquid per unit time may be reduced to about one-tenth, which is not within the range that can be solved by adjusting the solvent extraction conditions, and it may become necessary to increase the number of solvent extraction devices, increasing operational costs.

[0009] The present invention has been proposed in light of the above-mentioned circumstances, and has as its object to provide a method which can effectively reduce the amount of gold contained in a leachate obtained by chlorine leaching of a platinum group element-containing material which contains at least gold as an impurity element, and which can prevent a decrease in the operational efficiency of, for example, a solvent extraction treatment in a downstream process. [Means for solving the problem]

[0010] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result have found that, after subjecting a platinum group element-containing material including gold to chlorine leaching, the gold can be reduced by adding a reducing agent to the resulting slurry prior to solid-liquid separation treatment, thereby efficiently precipitating and removing the reduced gold and effectively reducing the gold content in the leachate, which led to the completion of the present invention.

[0011] (1) The first aspect of the present invention is a method for subjecting a platinum group element-containing material containing gold as an impurity element to chlorine leaching, followed by a solid-liquid separation treatment to obtain a chlorine leachate, in which a reducing agent is added to a slurry obtained by the chlorine leaching prior to the solid-liquid separation treatment to reduce the gold contained in the slurry, and the chlorine leachate is separated from a leach residue containing a precipitate of the reduced gold by the solid-liquid separation treatment.

[0012] (2) A second aspect of the present invention is the method according to the first aspect of the present invention, wherein the reducing agent contains hydrazine.

[0013] (3) A third aspect of the present invention is the method according to the second aspect of the present invention, wherein the hydrazine is added in an amount within the range of 0.1% by volume to 0.3% by volume per 1000 L of the supernatant liquid of the slurry.

[0014] (4) A fourth aspect of the present invention is the method according to the first aspect of the present invention, wherein the reducing agent contains sodium sulfite.

[0015] (5) A fifth aspect of the present invention is the method according to the fourth aspect of the present invention, wherein the amount of sodium sulfite added is controlled based on an oxidation-reduction potential of the slurry. Effect of the Invention

[0016] According to the present invention, the gold content in the resulting leachate can be effectively reduced, and this can prevent a decrease in the operational efficiency of the subsequent solvent extraction process. [Brief description of the drawings]

[0017] [Figure 1] FIG. 1 is a process diagram showing an example of the flow of a method according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] A specific embodiment of the present invention (hereinafter, also referred to as "the present embodiment") will be described in detail below. Note that the present invention is not limited to the following embodiment, and can be implemented with appropriate modifications within the scope of the present invention.

[0019] The method according to the present embodiment is a method in which a platinum group element-containing material containing gold as an impurity element is subjected to chlorine leaching, and then a chlorine leachate is obtained by a solid-liquid separation process.

[0020] The platinum group element-containing material is not particularly limited, and a platinum group element concentrate (hereinafter referred to as "PGM concentrate") containing various impurity elements obtained from by-products of non-ferrous metal smelting such as copper, nickel, cobalt, and various used waste catalysts such as automobile exhaust gas treatment catalysts can be used. The PGM concentrate used in this method contains at least gold as an impurity element. Other impurity elements include main metals such as copper, nickel, cobalt, and iron, and other constituent elements such as silver, lead, tin, selenium, tellurium, arsenic, antimony, and bismuth. Examples of such platinum group element-containing materials containing at least gold as an impurity element include those obtained by treating anode slime to concentrate precious metals (PGMconc).

[0021] For example, as disclosed in Patent Document 2, in the separation and recovery of platinum group elements, a PGM concentrate is subjected to chlorine leaching to obtain a leachate from which the platinum group elements have been leached (PGM leachate, chlorine leachate).

[0022] In an operation to obtain a PGM leachate from such a PGM concentrate as a starting material, the gold content of the PGM leachate obtained by chlorine leaching may be high, for example, when the copper electrolytic slime contains a high gold content, or when the PGM concentrate is mixed with miscellaneous raw materials such as residues and solids containing platinum group elements recovered from other processes. The reason why the gold content of the copper electrolytic slime is high is because there is a business requirement to increase gold production, which may increase the gold content in the gold ore that is the raw material for copper smelting. Also, there is a business requirement to recover platinum group elements from miscellaneous raw materials, which may contain high concentrations of gold.

[0023] Conventionally, the gold content in the PGM leachate obtained by chlorine leaching is about 0.2g / L, and gold was separated and recovered by a subsequent solvent extraction process, but due to the above-mentioned circumstances, if the gold content in the PGM leachate increases to about 2-4g / L, the load required to separate the gold using the solvent extraction process (Au·Sb-SX) will exceed its limit. In other words, there is too much gold and it will not be able to be processed by solvent extraction, and measures such as reducing the amount of processing solution will be required.

[0024] It is easy to imagine that the solution to this problem would be to reduce the gold concentration in the PGM leachate, but due to the business requirements mentioned above, it is not possible to choose a method to reduce the gold content in the raw materials upstream of the process. Therefore, appropriate measures must be taken in the process after chlorine leaching of the PGM concentrate (which may contain a mixture of miscellaneous raw materials). In order to reduce the gold concentration in the liquid phase (supernatant) of the slurry immediately after chlorine leaching, it is possible to consider a method of suppressing the leaching level of the PGM concentrate, but this method is not an option because it would also reduce the leaching rate of the platinum group elements. Therefore, it is necessary to effectively reduce the gold content in the resulting PGM leachate under conditions that allow the platinum group elements to be preferentially leached to the maximum extent from the PGM concentrate.

[0025] Therefore, in the method according to the present embodiment, a platinum group element-containing material containing gold as an impurity element is subjected to chlorine leaching, and then a chlorine leachate is obtained by solid-liquid separation. In this method, a reducing agent is added to the slurry obtained by chlorine leaching to reduce the gold contained in the slurry (the leachate in the slurry).

[0026] Fig. 1 is a process diagram showing the flow of the method according to this embodiment. As shown in the process diagram in Fig. 1, after the chlorine leaching treatment (chlorine leaching step), a reducing agent is added to the slurry obtained by the leaching treatment (slurry containing a liquid phase leachate and leach residue) to reduce gold (de-gold removal step). Then, the slurry is subjected to a solid-liquid separation process by filtration or the like to separate the chlorine leachate from the leach residue containing precipitates of reduced gold (solid-liquid separation step). Note that "reduced gold" refers to gold (gold powder) produced by reducing gold ions in the slurry.

[0027] In this way, even if the gold concentration in the liquid phase of the slurry immediately after chlorine leaching becomes high, for example, to about 2 to 4 g / L or more, due to the raw material conditions as described above, the gold content in the resulting PGM leachate can be effectively reduced by adding a reducing agent to the slurry to reduce gold (de-gold treatment), and a decrease in the operational efficiency of the solvent extraction treatment in the subsequent process can be effectively prevented.

[0028] Here, as a demetalization process for reducing the gold content in the PGM leachate, it is possible to separate the slurry obtained by chlorine leaching (leach slurry) into solid and liquid, and to treat the leachate recovered by separating it from the leach residue. In addition, in the case of a method in which a reducing agent is added to the leachate after solid-liquid separation, compared to a case in which a reducing agent is added to the leach slurry, the reducing agent acts only on the liquid phase, which has the advantage of saving the amount of reducing agent consumed by the leach residue when the reducing agent is added to the slurry containing the leach residue.

[0029] However, in the case of a method in which a reducing agent is added to the separated and recovered leachate after solid-liquid separation to perform demetalization, the reduction reaction causes gold-containing precipitates to form in the leachate, making it necessary to separate the leachate into solid and liquid again (requiring a separate solid-liquid separation process).This increases the processing costs even more than the increased amount of reducing agent used, and also causes a significant decrease in operating efficiency.

[0030] For this reason, the method according to the present embodiment is characterized in that the slurry obtained by chlorine leaching is the target of demetalization treatment, and a reducing agent is added to the slurry before solid-liquid separation treatment (before the solid-liquid separation step) to reduce gold. This method makes it possible to carry out efficient treatment without the need to provide an additional solid-liquid separation step for removing precipitates mainly composed of reduced gold that are generated as a result of the effective reduction of the gold concentration in the leachate.

[0031] In the demetalization treatment, the reducing agent to be added is not particularly limited, but it is preferable to use hydrazine, sodium sulfite, etc. These reducing agents are particularly inexpensive and readily available, and therefore can effectively reduce gold while achieving economically efficient treatment.

[0032] For example, the reducing agent hydrazine is not only an inexpensive and easily available reducing agent as described above, but also a reducing agent that is stable in a liquid state within the range of treatment temperatures. In this respect, by using a reducing agent containing hydrazine, it is possible to perform stable treatment without causing blockage of the supply path when the reducing agent is supplied to the treatment tank holding the slurry.

[0033] However, in the treatment using a reducing agent containing hydrazine, the change in the oxidation-reduction potential (ORP) of the slurry accompanying the addition of hydrazine is gradual. Therefore, when treatment is performed while monitoring the ORP of the slurry, the amount of hydrazine added tends to increase. Since the PGM leachate obtained by chlorine leaching of PGM concentrate naturally contains the platinum group elements to be separated and recovered, the addition of excessive hydrazine reduces the platinum group elements platinum (Pt) and palladium (Pd), which are distributed to the leach residue (leach residue containing precipitates produced by reduction) and become a loss, which can also cause a decrease in the recovery rate of the platinum group elements.

[0034] For this reason, in demetalization treatment using a reducing agent containing hydrazine, it is preferable to add a fixed amount of hydrazine rather than controlling the amount of reducing agent added based on the ORP of the slurry. Specifically, the amount of hydrazine added is not particularly limited, but it is preferable to add a fixed amount in the range of preferably 0.1% by volume to 1.2% by volume, more preferably 0.2% by volume to 0.5% by volume, per 1000 L of the supernatant liquid (liquid phase) of the slurry. By adding a fixed amount in such a range, gold can be preferentially reduced to precipitate, and effective treatment can be achieved while suppressing the reduction of platinum group elements contained in the slurry.

[0035] If the amount of hydrazine added is less than 0.1% by volume, the amount of reducing agent may be too small to effectively reduce the gold contained in the liquid phase of the slurry, whereas if the amount of hydrazine added is more than 1.2% by volume, the amount added is excessive and there is a possibility that platinum group elements such as platinum and palladium may also be reduced, resulting in a decrease in the recovery rate of platinum group elements.

[0036] For example, the reducing agent sodium sulfite is inexpensive and easily available as described above, so it can be easily applied to the treatment process and effectively reduces gold while realizing economically efficient treatment. Sodium sulfite is also an excellent reducing agent in terms of reactivity and responsiveness, and the ORP of the slurry changes appropriately with the addition of sodium sulfite, stabilizing in a short time.

[0037] For this reason, in demetalization treatment using a reducing agent containing sodium sulfite, it is preferable to monitor the ORP of the slurry and control the amount of sodium sulfite added based on the change in the oxidation-reduction potential. This allows gold to be preferentially reduced and precipitated, while preventing the excessive addition of reducing agent, suppressing the reduction of platinum group elements such as platinum and palladium, and preventing a decrease in the recovery rate of these platinum group elements. In addition, since the amount of reducing agent added can be controlled based on the ORP, the treatment can also be automated.

[0038] However, on the other hand, sodium sulfite, being a sodium salt, has the property of crystallizing, and therefore when supplying a reducing agent containing sodium sulfite, there is a possibility that a problem of clogging the piping constituting the supply path may occur, and it is preferable to take care in this regard.

[0039] When adding the above-mentioned reducing agent such as hydrazine or sodium sulfite, for example, the optimal amount to be added only to the liquid phase of the slurry may be determined in advance, and the amount added may be appropriately adjusted while monitoring the amount of gold recovered (the amount of gold removed from the liquid).

[0040] The method for the solid-liquid separation treatment (solid-liquid separation step) of the slurry after the demetalization treatment (after the demetalization step) is not particularly limited as long as it effectively separates the leachate constituting the liquid phase (supernatant) of the slurry from the leach residue containing the precipitate of reduced gold obtained by reduction. For example, this can be done by a process such as filtration.

[0041] Furthermore, as described above, since the demetalization process is performed on the leach slurry obtained by chlorine leaching, the precipitate of reduced gold, which is the reduction product, can be separated by a solid-liquid separation process for separating the leach residue, as in the conventional method. This eliminates the need for a separate solid-liquid separation process to separate the precipitate of reduced gold, as compared with, for example, a case in which the PGM leachate recovered after solid-liquid separation process is used for demetalization, enabling more efficient operation. EXAMPLES

[0042] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.

[0043] [Common conditions] Slurry (leached slurry) was collected immediately after chlorine leaching from a site where PGM concentrate is leached during operation, and the supernatant of the slurry (liquid phase only) was used as the original liquid for treatment tests. Three different periods were selected for slurry collection based on when the gold concentration in the PGM concentrate was high, and the original liquid shown in Table 1 below was used. Table 1 shows the component composition of the liquid phase (no residue) after chlorine leaching and the oxidation-reduction potential (ORP) as a property.

[0044] [Table 1]

[0045] As the raw liquid to be treated, 1000 L of the liquid after degassing was collected, and the batch test was carried out using the supernatant without any residue. In the degassing process, steam was blown into the raw liquid to remove acid gases. Then, steam was blown into the raw liquid to adjust the liquid temperature to about 60°C.

[0046] In the demetallization treatments in Examples 1 to 7, either the reducing agent [1] or the reducing agent [2] was used and added to the original solution in the amounts shown below. Reducing agent [1]: (Type) Sodium sulfite (powder, anhydrous sodium sulfite) (manufactured by Shinshu Chemical Co., Ltd.) (Amount to add): Monitor the ORP and add until it drops below 560mV. Reducing agent [2]: (Type) Hydrazine (liquid, hydrazine hydrate 60%) (manufactured by Otsuka MGC Chemical Co., Ltd.) (Amount added) Add 0.2, 0.4, 0.6, and 0.8 vol% (= 0.2, 0.4, 0.6, and 0.8 mL, respectively) to 100 mL of liquid phase.

[0047] The metal components in the leachate were analyzed by ICP-AES (measuring device: Agilent, model number 5100).

[0048] [Example 1] In Example 1, original liquid A was subjected to degold removal treatment using sodium sulfite as a reducing agent [1], and the reducing agent was added until the ORP reached 560 mV while monitoring the ORP, reducing the gold (Au) contained in original liquid A to produce and remove precipitates of reduced gold. Table 2 below shows the results of component analysis of the liquid after degold removal treatment (post-gold removal liquid) and the removal rate.

[0049] [Table 2]

[0050] As shown in Table 2, the Au concentration in the degold solution was less than 0.2 g / L (removal rate 96.7%), effectively reducing Au. In addition, the removal rates of platinum (Pt) and palladium (Pd) contained in original solution A were low at less than 1.5%, meaning that there was almost no loss of platinum group elements due to the degold treatment.

[0051] Furthermore, no problems, including an increase in the processing load, occurred in the subsequent solvent extraction treatment of the demetallized liquid.

[0052] [Example 2] In Example 2, the same treatment as in Example 1 was carried out except that in the demetalization treatment, a reducing agent was added until the ORP reached 540 mV. Table 3 below shows the component analysis results and removal rate of the liquid after demetalization.

[0053] [Table 3]

[0054] As shown in Table 3, the Au concentration in the degold solution was less than 0.2 g / L (removal rate of 99.9%), effectively reducing Au. In addition, the removal rate of Pt and Pd contained in original solution A was low at less than 1.7%, meaning that there was almost no loss of platinum group elements due to the degold treatment.

[0055] Furthermore, no problems, including an increase in the processing load, occurred in the subsequent solvent extraction treatment of the demetallized liquid.

[0056] [Example 3] In Example 3, the original liquid B was subjected to a degold removal treatment using hydrazine, a reducing agent [2], by adding 0.2% by volume (2 L) to the volume (1000 L) of the original liquid B, reducing the Au contained in the original liquid B and generating a precipitate of reduced gold, which was then removed. Table 4 below shows the results of the component analysis of the liquid after degold removal and the removal rate.

[0057] [Table 4]

[0058] As shown in Table 4, the Au concentration in the degold solution was less than 0.2 g / L (removal rate of 98.8%), effectively reducing Au. In addition, the removal rate of Pt and Pd contained in original solution B was low at less than 3.5%, meaning that there was almost no loss of platinum group elements due to the degold treatment.

[0059] Furthermore, no problems, including an increase in the processing load, occurred in the subsequent solvent extraction treatment of the demetallized liquid.

[0060] [Example 4] In Example 4, the same treatment as in Example 3 was carried out, except that 0.4% by volume (4 L) of the reducing agent was added to the volume (1000 L) of the original liquid B. Table 5 below shows the component analysis results and removal rate of the liquid after gold removal.

[0061] [Table 5]

[0062] As shown in Table 5, the Au concentration in the demetallized solution was 0g / L (100% removal rate), effectively reducing Au. The removal rate of Pt and Pd contained in original solution B was also at a low level of less than 3.5%, meaning that there was almost no loss of platinum group elements due to the demetallization process. As the Au removal rate was 100%, it can be seen that there was no need to add any further reducing agent.

[0063] Furthermore, no problems, including an increase in the processing load, occurred in the subsequent solvent extraction treatment of the demetallized liquid.

[0064] [Example 5] In Example 5, the original liquid C was used, and the same treatment as in Example 3 was carried out on the original liquid C. Table 6 below shows the component analysis results and removal rate of the liquid after degold removal.

[0065] [Table 6]

[0066] As shown in Table 6, the Au concentration in the degold solution was less than 0.2 g / L (removal rate of 99.7%), effectively reducing Au. In addition, the removal rate of Pt and Pd contained in the original solution C was low at less than 3.0%, meaning that there was almost no loss of platinum group elements due to the degold treatment.

[0067] Furthermore, no problems, including an increase in the processing load, occurred in the subsequent solvent extraction treatment of the demetallized liquid.

[0068] [Example 6] In Example 6, the same treatment as in Example 5 was carried out, except that 0.4% by volume (4 L) of the reducing agent was added to the volume (1000 L) of the original liquid C. Table 7 below shows the component analysis results and removal rate of the liquid after gold removal.

[0069] [Table 7]

[0070] As shown in Table 7, the Au concentration in the liquid after demetalization was 0g / L (100% removal rate), and Au was effectively reduced. In addition, the removal rate of Pt and Pd contained in original liquid C was low at less than 3.6%, and there was almost no loss of platinum group elements due to the demetalization process. Furthermore, since the Au removal rate was 100%, it can be seen that there is no need to add any further reducing agent.

[0071] Furthermore, no problems, including an increase in the processing load, occurred in the subsequent solvent extraction treatment of the demetallized liquid.

[0072] [Example 7] In Example 7, the same treatment as in Example 6 was carried out, except that original liquid D was used and hydrazine, a reducing agent, was added in small amounts up to 0.66 volume % relative to the volume (1000 L) of original liquid D. Table 7 below shows the component analysis results and removal rates of the resulting post-gold depletion liquids (post-gold depletion liquids 1 to 5) for each amount of hydrazine added in small amounts.

[0073] [Table 8]

[0074] As shown in Table 8, the Au concentration in the post-gold removal solution could be reduced more as the amount of hydrazine added was increased. For example, when the amount of reducing agent added was 0.3 vol%, the Au concentration was less than 0.1 g / L (removal rate of 98%), while the removal rate of Pt was kept at 6.5%.

[0075] Furthermore, no problems, including an increase in the processing load, occurred in the subsequent solvent extraction treatment of the post-gold removal liquid obtained by treatment with either added amount.

[0076] [Comparative Example 1] In Comparative Example 1, demetalization was not performed (no demetalization step was provided), and the original liquid A was subjected to solvent extraction. As a result, a problem arose in that the solvent extraction took five times longer than in Examples 1 and 2, possibly due to the Au contained in the original liquid A.

Claims

1. A method for obtaining a chlorine leachate by subjecting a platinum group element-containing material obtained from copper electrolytic slime, which contains gold as an impurity element, to chlorine leaching and then subjecting the material to solid-liquid separation, comprising the steps of: a reducing agent is added to the slurry obtained by the chlorine leaching and having a gold content of 2 g / L or more before the solid-liquid separation treatment to reduce the gold contained in the slurry; The solid-liquid separation process separates the chlorine leachate from a leach residue containing precipitates of reduced gold, and the chlorine leachate is subjected to a step of extracting gold by a solvent extraction method. method.

2. The reducing agent includes hydrazine. The method of claim 1.

3. The hydrazine is added in a quantitative amount in the range of 0.1% by volume to 0.3% by volume per 1000 L of the supernatant of the slurry. The method of claim 2.

4. The reducing agent includes sodium sulfite. The method of claim 1.

5. The amount of sodium sulfite added is controlled based on the oxidation-reduction potential of the slurry. The method according to claim 4.

Citation Information

Patent Citations

  • Production of high purity gold

    JP1999229053A

  • Method for recovering valuable metal from copper electrolytic slime

    JP2001207223A

  • Method for recovering platinum from waste solution containing selenium using hydrazine

    JP2007270250A

  • Method for recovering selenium from copper electrolysis slime

    JP2012126611A

  • Method for separating and recovering platinum group element

    JP2013104064A