Method and device for evaluating performance of elastic material
The method and apparatus enhance the accuracy of evaluating elastic material performance by applying strain, detecting low-density regions, and calculating distribution width, addressing the limitations of existing evaluation techniques.
Patent Information
- Application Number
- JP2021034670
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-04
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-03-04
AI Technical Summary
Existing methods for evaluating the performance of elastic materials, such as the Lambourn abrasion tester, lack the necessary accuracy for precise evaluation of properties like wear resistance.
A method and apparatus that applies strain to a test piece made of elastic material, captures X-ray images to detect low-density regions, determines the relationship between density and frequency of these regions, and calculates the distribution width using the full width at half maximum (FWHM) to evaluate performance accurately.
Enables high-accuracy evaluation of elastic material performance, particularly wear resistance, by analyzing the distribution width of low-density regions, improving evaluation precision over existing methods.
Abstract
Description
[Technical field]
[0001] The present invention relates to a method and an apparatus for evaluating the performance of an elastic material. [Background technology]
[0002] A method for evaluating the performance of an elastic material is proposed in the following Patent Document 1. This method includes a step of applying strain to a test piece made of an elastic material, a step of irradiating the test piece with X-rays and taking a projection image, and an evaluation step of evaluating the performance of the elastic material based on the density distribution of the elastic material measured from the projection image. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-83182 A Summary of the Invention [Problem to be solved by the invention]
[0004] While the above method is effective as a new evaluation technique to replace the Lambourn abrasion tester, there is still room for improvement in terms of evaluation accuracy.
[0005] The present invention has been devised in view of the above circumstances, and has as its main object to provide a method and apparatus capable of evaluating the performance of an elastic material with high accuracy. [Means for solving the problem]
[0006] The present invention is a method for evaluating the performance of an elastic material including rubber or an elastomer, and is characterized by comprising the steps of: a strain imparting step of imparting strain to a test piece made of the elastic material; an imaging step of irradiating the strained test piece with X-rays to obtain a projection image of the test piece; a detection step of detecting low-density regions of the test piece, which are regions in which the density of the elastic material is lower than before the strain was applied, based on the projection image; a relationship acquisition step of determining the relationship between the density of the low-density regions and the frequency of the low-density regions based on the detection result of the low-density regions; and a distribution width calculation step of calculating a distribution width specified by a full width at half maximum (FWHM) when the relationship is approximated to a normal distribution.
[0007] The performance evaluation method according to the present invention may further include an evaluation step of evaluating the performance of the elastic material based on the distribution width.
[0008] In the performance evaluation method of the present invention, the evaluation step may include a step of comparing the distribution width with a predetermined threshold value, and a step of evaluating the performance of the elastic material as good when the distribution width is equal to or greater than the threshold value.
[0009] In the performance evaluation method according to the present invention, in the relationship, the density of the low-density region may be defined as a ratio to the density of the elastic material before the strain is applied, and the threshold value may be 0.2.
[0010] In the performance evaluation method according to the present invention, the performance of the elastic material may be abrasion resistance performance.
[0011] In the performance evaluation method according to the present invention, the detection step may include a step of constructing a tomographic image of the test piece using the projection image, and a step of measuring a density distribution of the elastic material from the tomographic image.
[0012] In the performance evaluation method according to the present invention, the strain may be an extensional strain.
[0013] In the performance evaluation method according to the present invention, the tensile strain may be 20% or more.
[0014] In the performance evaluation method according to the present invention, the elastic material may be a rubber obtained by using one or more kinds of conjugated diene compounds.
[0015] In the performance evaluation method according to the present invention, the rubber may be rubber for tires.
[0016] In the performance evaluation method according to the present invention, the luminance (photons / s / mrad) of the X-rays is 2 / mm 2 / 0.1%bw) is 10 10 It may be more than that.
[0017] In the performance evaluation method according to the present invention, the luminance may be 10 12 or more.
[0018] The present invention is an apparatus for evaluating the performance of an elastic material including rubber or an elastomer, and is characterized by including a strain imparting unit that imparts strain to a test piece made of the elastic material, an imaging unit that irradiates the strained test piece with X-rays to obtain a projection image of the test piece, a detection unit that detects low-density regions of the test piece, which are regions in which the density of the elastic material is lower than before the strain was applied, based on the projection image, a relationship acquisition unit that determines the relationship between the density of the low-density regions and the frequency of the low-density regions based on the detection result of the low-density regions, and a distribution width calculation unit that calculates a distribution width specified by a full width at half maximum (FWHM) when the relationship is approximated to a normal distribution.
[0019] The performance evaluation device according to the present invention may further include an evaluation unit that evaluates the performance of the elastic material based on the distribution width.
[0020] In the performance evaluation device according to the present invention, the imaging section may have a phosphor for converting X-rays into visible light, and a decay time of the phosphor may be 100 ms or less. Effect of the Invention
[0021] The method for evaluating the performance of an elastic material of the present invention employs the above steps, making it possible to evaluate the performance of an elastic material with high accuracy. [Brief description of the drawings]
[0022] [Figure 1] FIG. 2 is a perspective view of an apparatus for evaluating the performance of an elastic material according to the present embodiment. [Diagram 2] FIG. 2 is a block diagram of a computer according to the present embodiment. [Diagram 3] 4 is a flowchart showing the processing steps of a method for evaluating the performance of an elastic material according to the present embodiment. [Figure 4] (a) and (b) are cross-sectional images of two types of test specimens made of elastic materials with different compositions. [Diagram 5] 4 is a flowchart showing a processing procedure of a detection step according to the present embodiment. [Figure 6] 2(a) and 2(b) are graphs showing the relationship between the density of low-density regions and the frequency of low-density regions for two types of test pieces made of elastic materials with different compositions. [Figure 7] 4 is a flowchart showing a processing procedure of an evaluation step according to the present embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. It should be understood that the drawings include exaggerated expressions and expressions different from the dimensional ratio of the actual structure in order to help understand the contents of the invention. Furthermore, the same or common elements are given the same reference numerals throughout the embodiments, and duplicated explanations are omitted. Furthermore, the specific configurations shown in the embodiments and drawings are for understanding the contents of the present invention, and the present invention is not limited to the specific configurations shown in the drawings.
[0024] In the method for evaluating the performance of an elastic material according to the present embodiment (hereinafter, sometimes simply referred to as the "performance evaluation method"), the performance of an elastic material containing rubber or an elastomer is evaluated. Any elastic material can be used as appropriate. An example of the elastic material according to the present embodiment is rubber obtained by using one or more conjugated diene compounds. In addition, an example of the rubber (elastic material) is rubber for tires. An example of the performance evaluated by the method according to the present embodiment is wear resistance.
[0025] [Elastic material performance evaluation device] The performance evaluation method of this embodiment uses an elastic material performance evaluation device (hereinafter, sometimes simply referred to as "performance evaluation device") 1. Fig. 1 is a perspective view of the elastic material performance evaluation device 1 of this embodiment.
[0026] The performance evaluation device 1 is for evaluating the performance of an elastic material. The performance evaluation device 1 of this embodiment includes a distortion applying unit 2, an imaging unit 3, a detection unit 4, a relationship acquisition unit 5, and a distribution width calculation unit 6. Furthermore, the performance evaluation device 1 of this embodiment includes an evaluation unit 7.
[0027] [Distortion section] The strain applying unit 2 of this embodiment is for applying strain to the test piece 10 made of an elastic material. The strain applying unit 2 of this embodiment has a pair of jigs 21, 22 to which the test piece 10 is fixed, and a drive unit 23 that applies strain to the test piece 10 by moving the jigs 21 and 22 relatively to each other.
[0028] While fixing one jig 21, the driving unit 23 moves the other jig 22 in a direction in which the other jig 21 and 22 move away from each other. The driving unit 23 in this embodiment moves the other jig 22 in the axial direction of the cylindrical test piece 10. As a result, the test piece 10 is stretched in its axial direction, and strain is imparted to it.
[0029] The strain or load applied to the test piece 10 is detected by a load cell (not shown) or the like. The position and type of the load cell are arbitrary. A predetermined strain or load is applied to the test piece 10 by such a strain applying unit 2. The driving unit 23 of this embodiment is configured to be capable of rotating the test piece 10 and the jigs 21, 22 around the axis of the test piece 10.
[0030] [Imaging unit] The imaging unit 3 of this embodiment is for irradiating the strained test piece 10 with X-rays to obtain a projection image of the test piece 10. The imaging unit 3 of this embodiment is configured to include an X-ray tube 31 that irradiates X-rays, and a detector 32 that detects the X-rays and converts them into an electrical signal. Such imaging unit 3 can obtain projection images of the test piece 10 over the entire circumference by capturing a plurality of projection images while the test piece 10 is rotated around its axis.
[0031] The detector 32 has a phosphor 32a for converting X-rays into visible light. The decay time of the phosphor 32a can be set appropriately. If the decay time of the phosphor 32a exceeds 100 ms, when a plurality of projection images are continuously captured while rotating the test piece 10 or the like around an axis, the afterimage of the previously captured projection image may affect the projection image captured later. From this viewpoint, the decay time of the phosphor 32a is preferably 100 ms or less, more preferably 50 ms or less, and even more preferably 10 ms or less.
[0032] [Detection section, Relationship acquisition section, Distribution width calculation section, Evaluation section] The detection unit 4, the relationship acquisition unit 5, the distribution width calculation unit 6, and the evaluation unit 7 of this embodiment are configured by a computer 8. Fig. 2 is a block diagram of the computer 8 of this embodiment.
[0033] The computer 8 of this embodiment is configured to include an input unit 11 as an input device, an output unit 12 as an output device, and an arithmetic processing unit 13.
[0034] For example, a keyboard or a mouse is used as the input unit 11. For example, a display device or a printer is used as the output unit 12. The arithmetic processing device 13 includes a calculation unit (CPU) 13A that performs various calculations, a storage unit 13B that stores data, programs, etc., and a working memory 13C.
[0035] The storage unit 13B is a non-volatile information storage device formed of, for example, a magnetic disk, an optical disk, an SSD, etc. The storage unit 13B includes a data section 16 and a program section 17.
[0036] The data section 16 of this embodiment includes a projection image input section 16A, a detection result input section 16B, a relationship input section 16C, and a distribution width input section 16D. The data input to these sections will be explained in the processing procedure of the performance evaluation method described later.
[0037] The program section 17 of this embodiment is configured as a computer program. The program section 17 of this embodiment includes a detection program 17A, a relationship acquisition program 17B, a distribution width calculation program 17C, and an evaluation program 17D. These programs 17A to 17D are executed by the calculation section 13A, so that the computer 8 can function as the detection section 4, the relationship acquisition section 5, the distribution width calculation section 6, and the evaluation section 7. These functions will be explained in the processing procedure of the performance evaluation method described later.
[0038] [Method of evaluating the performance of elastic materials] Next, the procedure of the performance evaluation method of this embodiment will be described with reference to Fig. 3, which is a flow chart showing the procedure of the performance evaluation method of this embodiment.
[0039] [Process of fixing the test specimen] In the performance evaluation method of this embodiment, first, as shown in Fig. 1, a test piece 10 is fixed to jigs 21 and 22 (step S1). The above-mentioned elastic material having a uniform density distribution is used for the test piece 10 of this embodiment. The test piece 10 is formed in a cylindrical shape, similar to Patent Document 1. Details of the test piece 10 and the procedure for fixing the test piece 10 to the jigs 21 and 22 are as described in Patent Document 1.
[0040] [Strain imparting process] Next, in the performance evaluation method of this embodiment, strain is applied to the test piece 10 (strain application step S2). In the strain application step S2 of this embodiment, the driving unit 23 of the strain application unit 2 relatively moves the jigs 21 and 22 of the strain application unit 2 in directions in which the jigs move away from each other in the axial direction of the cylindrical test piece 10. Thereby, in the strain application step S2, the test piece 10 can be elongated, and an elongation strain can be applied to the test piece 10.
[0041] In the strain imparting step S2 of the present embodiment, a stress is generated inside the test piece 10 by imparting a strain to the test piece 10, and a bias occurs in the density of the elastic material. As a result, a low-density region is generated inside the test piece 10.
[0042] 4(a) and (b) are tomographic images of two types of test pieces 10A and 10B made of elastic materials with different compositions. These tomographic images are acquired in an imaging step S3 described below. These tomographic images show a cross section of the test piece 10 cut along an arbitrary plane that perpendicularly intersects with the axial direction of the test piece 10 shown in FIG. 1. The low-density regions 15 (voids 15a and low-density rubber portions 15b) are shown in black.
[0043] The low-density region 15 is a region of the test piece 10 where the density of the elastic material is lower than that before strain is applied. In this embodiment, a region having a density that is 0.0 to 0.8 times the density of the elastic material before strain is applied is defined as the low-density region 15.
[0044] The low-density region 15 of this embodiment includes a void 15a and a low-density rubber portion 15b. The void 15a of this embodiment is defined as a region having a density of 0.0 to 0.1 times (or less than) the density of the elastic material before the application of strain. On the other hand, the low-density rubber portion 15b is defined as a region having a density of 0.1 to 0.8 times the density of the elastic material before the application of strain.
[0045] In the strain imparting process S2 of this embodiment, an tensile strain is imparted to the test piece 10, so that a low-density region 15 can be generated more efficiently inside the elastic material (test piece 10) than when, for example, other strains (e.g., compressive strain or shear strain) are imparted.
[0046] In order to effectively exert the above-mentioned action, the tensile strain is preferably 20% or more. By having the tensile strain of 20% or more, a low-density region 15 with a sufficient volume is generated inside the elastic material, and the evaluation accuracy of the performance of the elastic material is improved. On the other hand, if the tensile strain is larger than necessary, the test piece 10 may be destroyed. For this reason, the tensile strain is preferably 100% or less. In this embodiment, the tensile strain is a ratio obtained by dividing the deformation length of the test piece 10 after strain application (change in the elongation direction from before strain application) by the height of the test piece 10 before strain application (length in the elongation direction), expressed as a percentage.
[0047] The magnitude of the stress applied to the test piece 10 can be set as appropriate. If the stress is too small, there is a risk that the low-density region 15 (shown in FIGS. 4(a) and (b)) may not be formed in the test piece 10. From this perspective, it is desirable to apply a stress of preferably 0.5 MPa or more to the test piece 10. On the other hand, if the stress is greater than necessary, there is a risk that the test piece 10 may be significantly damaged. From this perspective, it is desirable to apply a stress of preferably 2.0 MPa or less to the test piece 10.
[0048] [Imaging process] Next, in the performance evaluation method of the present embodiment, as shown in Fig. 1, the strained test piece 10 is irradiated with X-rays to obtain a projection image of the test piece 10 (imaging step S3). The imaging step S3 of the present embodiment is performed by a computer tomography method.
[0049] In the imaging step S3 of this embodiment, first, as shown in FIG. 1, X-rays are irradiated onto the test piece 10 from the X-ray tube 31. The X-rays pass through the test piece 10 and are detected by the detector 32. The detected X-rays are converted into an electrical signal. The electrical signal is output to the computer 8. The electrical signal is processed by the computer 8 to obtain a projection image of the test piece 10.
[0050] In the imaging step S3 of this embodiment, a plurality of projection images (rotation series images) are acquired by rotating the test piece 10 around its axis. Then, in the imaging step S3, the plurality of projection images (rotation series images) are reconstructed by a computer tomography method, and a three-dimensional tomographic image of the test piece 10 (shown in FIG. 4(a) as an example) is acquired. The projection image of the test piece 10 is input to a projection image input unit 16A (shown in FIG. 2) of the computer 8.
[0051] The brightness of the X-rays can be set appropriately. The brightness of the X-rays is closely related to the S / N ratio of the X-ray scattering data. If the brightness of the X-rays is low, the signal strength tends to be weaker than the statistical error of the X-rays, and it may be difficult to obtain data with a sufficiently good S / N ratio even if the measurement time is extended. From this perspective, the brightness of the X-rays (photons / s / mrad) 2 / mm 2 / 0.1%bw) is preferably 10 10 More preferably, it is 10 12 That's all.
[0052] The decay time of the phosphor 52a for converting X-rays into visible light can be appropriately set. As in the above-mentioned Patent Document 1, the decay time of the phosphor 52a is preferably 100 ms or less, more preferably 50 ms or less, and further preferably 10 ms or less, from the viewpoint of preventing an afterimage of a previously captured projection image from affecting a subsequently captured projection image.
[0053] [Detection process] Next, in the performance evaluation method of this embodiment, low-density regions 15 (shown in Figure 4(a)), which are regions of the test piece 10 where the density of the elastic material is lower than before it was strained, are detected based on the projection image (detection process S4).
[0054] In the detection step S4 of this embodiment, first, as shown in Fig. 2, a projection image (not shown) of the test piece 10 inputted to the projection image input unit 16A and a detection program 17A are read into the working memory 13C. Then, the detection program 17A is executed by the calculation unit 13A, whereby the computer 8 can function as the detection unit 4 for detecting the low-density region 15 (shown in Figs. 3(a) and (b)) based on the projection image. Fig. 5 is a flowchart showing the processing procedure of the detection step S4 of this embodiment.
[0055] [Compose the tomographic image] In the detection step S4 of this embodiment, first, a tomographic image 33 (shown in FIG. 4(a)) of the test piece 10 is constructed using the projection image (step S41). In step S41 of this embodiment, a plurality of tomographic images 33 (shown in FIG. 4(a) as an example) of the test piece 10 cut on an arbitrary plane intersecting perpendicularly to the axial direction of the test piece 10 are acquired using the projection image of the test piece 10. The tomographic images 33 of this embodiment are acquired at arbitrary intervals (for example, 10 to 30 μm) between one end (not shown) and the other end 10b of the axial direction of the test piece 10 shown in FIG. 1. The number of tomographic images 33 acquired in this embodiment is 150 to 300.
[0056] [Measurement of density distribution] Next, in the detection step S4 of this embodiment, the density distribution of the elastic material is measured from the tomographic image 33 (shown in FIG. 4(a) as an example) (step S42). In step S42 of this embodiment, first, in the area of the test piece 10 displayed in each tomographic image 33, the brightness value of the tomographic image 33 is acquired for each minute area (in this example, pixel) constituting the tomographic image 33. In this embodiment, the brightness value is the lowest in the gap 15a. Furthermore, the higher the brightness value, the higher the density of the elastic material. In this way, a proportional relationship is established between the brightness value and the density.
[0057] Next, in step S42 of this embodiment, the luminance value of the elastic material before strain is applied (i.e., the portion without low-density region 15) is set to 1.0, and the luminance value where no elastic material is present (the lowest luminance value) is set to 0.0, and the luminance value ratio of each minute region (pixel in this example) is calculated. Such a luminance value ratio is defined as a normalized density (i.e., the ratio to the density of the elastic material before strain is applied).
[0058] As described above, the density of the low-density region 15 is 0.0 to 0.8 times the density of the elastic material before the strain is applied. Therefore, in step S42, an area displayed as a minute area (pixel) with a luminance value ratio (normalized density) of 0.0 to 0.8 is detected as the low-density region 15.
[0059] In this embodiment, an area displayed as a minute area (pixel) where the brightness value ratio (normalized density) is 0.0 to less than 0.1 is detected as a gap 15a. Also, an area displayed as a minute area (pixel) where the brightness value ratio (normalized density) is 0.1 to 0.8 is detected as a low-density rubber part 15b.
[0060] In step S42 of the present embodiment, low-density regions 15 are detected in each tomographic image 33. Commercially available image processing software (e.g., Photoshop (registered trademark) manufactured by Adobe Systems) or the like is used to detect the low-density regions 15. The detection results of the low-density regions 15 are input to the detection result input unit 16B.
[0061] [Relationship Acquisition Process] Next, in the performance evaluation method of this embodiment, the relationship between the density of the low-density regions 15 and the frequency of the low-density regions 15 is obtained based on the detection results of the low-density regions 15 (shown in Figure 4(a) as an example) (relationship acquisition process S5).
[0062] In the relationship acquisition step S5 of this embodiment, first, the detection result of the low-density area 15 input to the detection result input unit 16B and the relationship acquisition program 17B are read into the working memory 13C as shown in Fig. 2. Then, the relationship acquisition program 17B is executed by the calculation unit 13A, thereby causing the computer 8 to function as the relationship acquisition unit 5 that obtains the relationship between the density of the low-density area and the frequency of the low-density area.
[0063] In the relationship acquisition step S5 of this embodiment, first, for the low-density regions 15 displayed in all tomographic images 33 (shown in FIG. 4(a) as an example), the number of micro-regions (pixels in this example) is tallied for each normalized density (ratio of brightness values). Next, in the relationship acquisition step S5, the number of micro-regions with a density of 1.0 is set to "1.0", and the ratio of the number of micro-regions with other densities is calculated. Such a ratio of numbers is defined as a normalized frequency.
[0064] Next, in the relationship acquisition step S5 of the present embodiment, the normalized frequency is plotted for each normalized density, with the normalized density (ratio of brightness values) on the horizontal axis and the normalized frequency (ratio of numbers) on the vertical axis. This makes it possible to obtain the relationship between the density of low-density regions and the frequency of low-density regions in the relationship acquisition step S5.
[0065] 6(a) and (b) are graphs showing the relationship R between the density of the low-density region and the frequency of the low-density region for two types of test pieces 10A and 10B made of elastic materials with different compositions. The relationship R is input to the relationship input unit 16C.
[0066] [Distribution width calculation process] Next, in the performance evaluation method of this embodiment, a distribution width W specified by a full width at half maximum FWHM when the relationship R between the density of the low-density region and the frequency of the low-density region is approximated to a normal distribution is calculated (distribution width calculation step S6).
[0067] In the distribution width calculation step S6 of this embodiment, first, the relationship R between the density of the low-density region and the frequency of the low-density region, which is input to the relationship input unit 16C, and the distribution width calculation program 17C are read into the working memory 13C as shown in Fig. 2. Then, the distribution width calculation program 17C is executed by the calculation unit 13A, whereby the computer 8 can function as the distribution width calculation unit 6 for calculating the distribution width W.
[0068] In the distribution width calculation step S6 of this embodiment, the relationship R between the density of the low-density region 15 and the frequency of the low-density region 15 shown in Figures 6(a) and 6(b) is approximated to a normal distribution D. For the approximation of the normal distribution D, for example, commercially available numerical analysis software (for example, "MATLAB" manufactured by The MathWorks, Inc.) is used.
[0069] Next, in a distribution width calculation step S6 of this embodiment, a distribution width W specified by the full width at half maximum FWHM is calculated based on the normal distribution D approximated to the relationship R. Note that, as shown in Fig. 6(b), when the peak of the normal distribution D approximated to the relationship R ends at a density of 0, the distribution width W (full width at half maximum FWHM) from the density of 0 is obtained. The distribution width W (full width at half maximum FWHM) is specified, for example, using the above-mentioned numerical analysis software.
[0070] The full width at half maximum FWHM is an index showing the spread of the density distribution of the low-density region 15. Therefore, a larger full width at half maximum FWHM indicates that the density of the low-density region 15 is distributed over a wider range. On the other hand, a smaller full width at half maximum FWHM indicates that the density of the low-density region 15 is locally concentrated.
[0071] According to the experiments of the inventors, it was found that there is a certain correlation between the distribution width W specified by the full width at half maximum FWHM and the performance of the elastic material (in this example, the wear resistance performance). That is, it was found that in an elastic material with a large distribution width W, the density of the low-density region 15 is distributed over a wide range, so that the ratio of voids 15a (shown in FIG. 4(a)) having a density of less than 0.0 to 0.1 is reduced, and the performance of the elastic material is improved.
[0072] The distribution width W of the elastic material of the test piece 10A in Fig. 6(a) is larger than the distribution width W of the elastic material of the test piece 10B in Fig. 6(b), and the frequency is small at densities of 0.0 to less than 0.1. Therefore, the elastic material of the test piece 10A can be evaluated as having higher performance (wear resistance in this example) than the elastic material of the test piece 10B.
[0073] On the other hand, in the method of Patent Document 1, the performance (wear resistance) of the elastic material is evaluated based on the density distribution (total volume of low-density region 15) of low-density region 15. However, in such a method, the density distribution (total volume) of the elastic material of test piece 10A and the elastic material of test piece 10B are substantially the same, and it may not be possible to evaluate the difference in performance.
[0074] In this way, in the performance evaluation method of the present embodiment, the performance of the elastic material can be evaluated based on the distribution width W of the low-density region 15, thereby improving the evaluation accuracy. The distribution width W is input to the distribution width input section 16D (shown in FIG. 1).
[0075] [Evaluation process] Next, in the performance evaluation method of the present embodiment, the performance of the elastic material is evaluated based on the distribution width W (evaluation step S7).
[0076] In the evaluation step S7 of this embodiment, first, the distribution width W inputted to the distribution width input section 16D and the evaluation program 17D are read into the working memory 13C as shown in Fig. 2. Then, the evaluation program 17D is executed by the calculation section 13A, whereby the computer 8 can function as the evaluation section 7 that evaluates the performance of the elastic material.
[0077] Fig. 7 is a flow chart showing the procedure of the evaluation step S7 of this embodiment. In the evaluation step S7 of this embodiment, first, the distribution width W (shown in Fig. 6(a)) is compared with a predetermined threshold value T (step S71). The threshold value T can be set appropriately according to, for example, the performance required for the elastic material (wear resistance in this embodiment). In the relationship R shown in Fig. 6(a) as in this embodiment, when the density of the low density region 15 is defined as the ratio to the density of the elastic material before the application of strain (0.0 to 0.8 in this example), it is desirable to set it to 0.2.
[0078] In step S71, when the distribution width W is equal to or greater than the threshold value T (0.2 in this example), the performance of the elastic material is evaluated as good (step S72). On the other hand, in step S71, when the distribution width W is less than the threshold value T, the performance of the elastic material is evaluated as poor (step S73). In this case, a new elastic material with a changed composition is produced, and the performance evaluation method of this embodiment is carried out again. This makes it possible to reliably produce an elastic material with excellent performances.
[0079] In the present embodiment, the wear resistance is evaluated, but the present invention is not limited to such an embodiment. For example, the tear resistance or crack resistance of the elastic material may be evaluated based on the distribution width W.
[0080] Although a particularly preferred embodiment of the present invention has been described in detail above, the present invention is not limited to the illustrated embodiment and can be modified in various ways. EXAMPLES
[0081] The wear resistance of elastic materials A to C was evaluated based on the distribution width W (full width at half maximum FWHM) obtained by the method of the present invention, and the correlation with the evaluation of wear resistance by an actual vehicle running test was verified (Example). For comparison, the wear resistance of elastic materials A to C was evaluated using a Lambourn tester, and the correlation with the evaluation of wear resistance by an actual vehicle running test was verified (Comparative Example).
[0082] The reagents used are as follows: 1. Polymer (1): (1 modifying group) 2. Polymer (2): (2 modified groups; different amount of monomer from polymer (1)) 3. Polymer (3): (3 modified groups; different amount of monomers from polymer (1)) 4. SBR: SPRINTAN SLR6430 made by STYRON 5.BR: BR150B manufactured by Ube Industries, Ltd. 6. Modifier: 3-(N,N-dimethylaminopropyl)trimethoxysilane manufactured by Azumax Corporation 7. Anti-aging agent: Nocrac 6C (N-1,3-dimethylbutyl-N'-phenyl-p-phenylenediamine) manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 8. Stearic acid: Stearin manufactured by Nippon Oil & Fats Co., Ltd. 9. Zinc oxide: Ginrei R manufactured by Toho Zinc Co., Ltd. 10. Aromatic oil: Diana Process AH-24 manufactured by Idemitsu Kosan Co., Ltd. 11. Wax: Sunnock Wax manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 12. Sulfur: Powdered sulfur manufactured by Tsurumi Chemical Co., Ltd. 13. Vulcanization accelerator (1): Noccela CZ manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 14. Vulcanization accelerator (2): Noccelaer D manufactured by Ouchi Shinko Chemical Industry Co., Ltd. 15. Silica: Degussa Ultrasil VN3 16. Silane coupling agent: Degussa Si69 17. Carbon black: Diablack LH (N326, N2SA:84m) manufactured by Mitsubishi Chemical Corporation 2 / g)
[0083] The monomers and polymers (1) to (3) were synthesized in the same manner as described in the "Examples" of the above-mentioned Patent Document 1. The test methods were as follows.
[0084] <Distribution width W (full width at half maximum FWHM)> For the elastic materials A to C, cylindrical test pieces with a diameter of 20 mm and an axial length of 1 mm were prepared. The performance of the elastic materials was evaluated according to the procedure shown in FIG. 3. In the strain application step S2, a stress of 0.5 MPa was applied to the test piece, and multiple low-density regions (voids and low-density rubber parts) were formed inside the test piece. Next, in the relationship acquisition step S5, the relationship between the density of the low-density region and the frequency of the low-density region was obtained based on the detection result of the low-density region. Next, in the distribution width calculation step S6, the distribution width W specified by the full width at half maximum FWHM when the relationship obtained in the relationship acquisition step S5 was approximated to a normal distribution was calculated. The larger the distribution width W, the better the wear resistance.
[0085] <Lambourn test> For elastic materials A to C, the amount of wear was measured using a Lambourn abrasion tester under the conditions of room temperature, a load of 1.0 kgf, and a slip ratio of 30%, and the reciprocal was calculated. The results are expressed as an index with elastic material A being 100, and the larger the value, the more excellent the abrasion resistance.
[0086] <Actual vehicle driving test> A pneumatic tire of size 195 / 65R15 having a tread made of elastic materials A to C was made and fitted to a domestically produced FF vehicle, and the groove depth of the tread after a distance of 8000 km was measured, and the distance traveled per 1 mm of wear of the tread was calculated. The results are expressed as an index with elastic material A being 100, and the higher the value, the better the wear resistance. The test results are shown in Table 1.
[0087] [Table 1]
[0088] As a result of the test, as is clear from Table 1, the method of the embodiment has a good correlation with the actual vehicle running test compared to the comparative example, and it was confirmed that the performance of the elastic material can be evaluated with high accuracy. Furthermore, in the embodiment, elastic materials B and C, which have a distribution width W of equal to or greater than the threshold value T (0.2), were significantly superior in the evaluation in the actual vehicle running test compared to elastic material A, which has a distribution width W less than the threshold value T, and it was confirmed that the performance of the elastic material can be evaluated with high accuracy. [Explanation of symbols]
[0089] S2 Strain imparting process S3 Imaging process S4 Detection process S5 Relationship acquisition process S6 Distribution width calculation process
Claims
1. 1. A method for evaluating the performance of elastic materials, including rubbers or elastomers, comprising: a strain imparting step of imparting strain to a test piece made of the elastic material; an imaging step of irradiating the strained test piece with X-rays to obtain a projection image of the test piece; a detection step of detecting a low-density region of the test piece, the low-density region being a region in which the density of the elastic material is lower than that before the strain is applied, based on the projection image; a relationship acquisition step of determining a relationship between the density of the low-density region and a frequency of the low-density region based on a result of the detection of the low-density region; A distribution width calculation step of calculating a distribution width specified by a full width at half maximum (FWHM) when the relationship is approximated to a normal distribution. Performance evaluation method.
2. The performance evaluation method according to claim 1 , further comprising an evaluation step of evaluating the performance of the elastic material based on the distribution width.
3. The performance evaluation method according to claim 2 , wherein the evaluation step includes the steps of: comparing the distribution width with a predetermined threshold; and evaluating the performance of the elastic material as good when the distribution width is equal to or greater than the threshold.
4. In the relationship, the density of the low density region is defined as a ratio to the density of the elastic material before the strain is applied, The performance evaluation method according to claim 3 , wherein the threshold value is 0.
2.
5. The performance evaluation method according to claim 1 , wherein the performance of the elastic material is abrasion resistance.
6. The detection step includes: constructing a tomographic image of the test piece using the projection images; The performance evaluation method according to claim 1 , further comprising the step of measuring a density distribution of the elastic material from the tomographic image.
7. The performance evaluation method according to claim 1 , wherein the strain is a tensile strain.
8. The performance evaluation method according to claim 7 , wherein the tensile strain is 20% or more.
9. 9. The performance evaluation method according to claim 1, wherein the elastic material is a rubber obtained by using one or more kinds of conjugated diene compounds.
10. The performance evaluation method according to claim 9 , wherein the rubber is a tire rubber.
11. The brightness of the X-rays (photons / s / mrad 2 / mm 2 / 0.1%bw) is 10 10 The performance evaluation method according to any one of claims 1 to 10, wherein
12. The brightness is 10 12 The performance evaluation method according to claim 11 .
13. An apparatus for evaluating the performance of elastic materials, including rubber or elastomers, comprising: A strain applying unit that applies a strain to the test piece made of the elastic material; an imaging unit that irradiates the strained test piece with X-rays to obtain a projection image of the test piece; a detection unit that detects a low-density region of the test piece, the low-density region being a region in which the density of the elastic material is lower than that before the strain is applied, based on the projection image; a relationship acquisition unit that acquires a relationship between a density of the low-density area and a frequency of the low-density area based on a detection result of the low-density area; a distribution width calculation unit that calculates a distribution width specified by a full width at half maximum (FWHM) when the relationship is approximated to a normal distribution, Performance evaluation device.
14. The performance evaluation device according to claim 13 , further comprising an evaluation unit that evaluates performance of the elastic material based on the distribution width.
15. the imaging unit has a phosphor for converting X-rays into visible light; 15. The performance evaluation device according to claim 13, wherein the decay time of the phosphor is 100 ms or less.
Citation Information
Patent Citations
Performance evaluation method and performance evaluation device
JP2017083182A
Method for evaluating performance of elastic material
JP2020008329A