Positive electrodes for lithium-ion secondary batteries
The positive electrode for lithium ion secondary batteries, featuring controlled tungsten valence through XAFS analysis, addresses high resistance issues by enhancing conductivity and lithium ion diffusion, thereby improving battery performance.
Patent Information
- Application Number
- JP2021196620
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-12-03
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-12-03
AI Technical Summary
Lithium ion secondary batteries face high cell resistance due to the use of hexavalent tungsten, which has low conductivity and increases resistance when used as a positive electrode active material, despite conventional efforts to improve cycle characteristics.
A positive electrode for lithium ion secondary batteries is developed with a tungsten content that satisfies a specific X-ray absorption fine structure analysis (XAFS) criterion, ensuring a valence between tetravalent and hexavalent tungsten, thereby reducing cell resistance.
The electrode design with controlled tungsten valence significantly lowers cell resistance by enhancing conductivity and facilitating lithium ion diffusion, thus improving battery performance.
Smart Images

Figure 0007571714000003 
Figure 0007571714000004 
Figure 0007571714000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a positive electrode for a lithium-ion secondary battery. [Background technology]
[0002] Lithium-ion secondary batteries are increasingly being put to practical use not only as small power sources for mobile phones and notebook computers, but also as medium- and large-sized power sources for automobiles and power storage.
[0003] In order to improve the performance of lithium-ion secondary batteries, research has been conducted focusing on the positive electrode active material. For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery having a low initial resistance and suppressing an increase in resistance during repeated charging and discharging, which is made of porous particles of a lithium composite oxide having a specific porosity and containing two or more specific voids, and which has tungsten oxide (WO 3、 A non-aqueous electrolyte secondary battery is disclosed that includes a positive electrode that includes, as a positive electrode active material, porous particles having a coating that contains hexavalent tungsten and lithium tungstate. Patent Document 2 discloses a positive electrode active material for lithium secondary batteries that contains a lithium composite metal compound composed of secondary particles and has a specific pore distribution, as a positive electrode active material for lithium secondary batteries in which particle cracking after cycling is significantly suppressed, and in which lithium-containing tungsten oxide is present at least in the gaps between the primary particles. Patent Document 2 discloses that the lithium-containing tungsten oxide is at least one of Li2WO4 (hexavalent tungsten) and Li4WO5 (hexavalent tungsten).
[0004] Patent Document 3 discloses a positive electrode active material that reduces the amount of gas generated when a non-aqueous electrolyte secondary battery is stored at high temperature, the positive electrode active material having a core particle of a lithium transition metal composite oxide having a layered structure containing nickel, and a surface layer containing boron, tungsten, and oxygen in a specific state on the surface of the core particle. In Patent Document 3, tungsten oxide (WO3、 Hexavalent tungsten) is used. Patent Document 4 discloses a method for producing a nickel-cobalt composite hydroxide that contains tungsten homogeneously inside and on the surface of primary particles. In Patent Document 4, a hexavalent tungsten raw material is used. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2021-018895 [Patent Document 2] JP 2018-098183 A [Patent Document 3] JP 2019-106379 A [Patent Document 4] JP 2019-073436 A Summary of the Invention [Problem to be solved by the invention]
[0006] Conventionally, as the tungsten raw material used for the positive electrode active material, a hexavalent tungsten raw material that is highly stable, inexpensive, and easily available has been used. However, the lithium tungstate coated on the surface of the porous particles of the lithium composite oxide disclosed in Patent Document 1 does not have the effect of lowering the activation energy, and tungsten oxide (WO 3、 Since hexavalent tungsten has low electrical conductivity, increasing the coverage rate to improve cycle characteristics results in an increase in resistance. Lithium ion secondary batteries using positive electrodes such as those disclosed in Patent Documents 1 to 4 still have high cell resistance, and further reduction in resistance is required.
[0007] The present disclosure has been made in view of the above-mentioned circumstances, and has as its main object to provide a positive electrode that reduces the cell resistance of a lithium-ion secondary battery when used in the secondary battery. [Means for solving the problem]
[0008] The positive electrode for a lithium ion secondary battery of the present disclosure is a positive electrode for a lithium ion secondary battery including a positive electrode active material including tungsten, The positive electrode has a spectrum at the rising position (10200 eV to 10205 eV) of the peak at the L absorption edge of tungsten measured by X-ray absorption fine structure analysis (XAFS), Formula (1): (ab) / (cb)≦0.86 [In formula (1), a represents the energy (eV) at which the spectral slope is greatest in the range of 10200 eV to 10205 eV, When the spectral intensity at a (eV) is A, b represents the energy (eV) at which the spectral intensity of WO2 (tungsten (IV) oxide) becomes A in the range of 10200 eV to 10205 eV, c represents the energy (eV) at which the spectral intensity of WO3 (tungsten (VI) oxide) becomes A in the range of 10200 eV to 10205 eV. This is a positive electrode for lithium-ion secondary batteries.
[0009] In the positive electrode for a lithium ion secondary battery of the present disclosure, the content of the tungsten relative to the positive electrode active material may be 0.015% by mass to 3.1% by mass.
[0010] In the positive electrode for a lithium ion secondary battery of the present disclosure, the positive electrode may be one in which (ab) / (cb) in formula (1) satisfies 0.15 or more and 0.65 or less. Effect of the Invention
[0011] According to the present disclosure, it is possible to provide a positive electrode for a lithium ion secondary battery that reduces the cell resistance of the lithium ion secondary battery. [Brief description of the drawings]
[0012] [Figure 1]FIG. 1 is a diagram showing XAFS measurement spectra of an example of a positive electrode for a lithium ion secondary battery (positive electrode sample) of the present disclosure, WO2, and WO3. [Diagram 2] FIG. 2 is a schematic diagram for explaining formula (1) of the present disclosure, in which the rising positions of the peaks at the L absorption edge of tungsten in the XAFS measurement spectra of the positive electrode sample, WO2, and WO3 are partially enlarged. [Diagram 3] FIG. 3 is a cross-sectional view that diagrammatically illustrates a portion of the layered structure of an electrode body of a lithium-ion secondary battery according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] Hereinafter, embodiments of the present disclosure will be described. Note that matters other than those specifically mentioned in this specification and necessary for implementing the present disclosure (for example, the general configuration and manufacturing process of a lithium ion secondary battery that does not characterize the present disclosure) can be understood as design matters of a person skilled in the art based on the prior art in the field. The present disclosure can be implemented based on the contents disclosed in this specification and the technical common sense in the field. Furthermore, the dimensional relationships (length, width, thickness, etc.) in the drawings do not reflect the actual dimensional relationships. In this specification, the use of "to" indicating a numerical range means that the numerical values before and after it are included as the lower limit and upper limit. Furthermore, any combination of upper and lower limits in a numerical range can be used.
[0014] [Positive electrodes for lithium-ion secondary batteries] The positive electrode for a lithium ion secondary battery of the present disclosure is a positive electrode for a lithium ion secondary battery including a positive electrode active material including tungsten, The positive electrode has a spectrum at the rising position (10200 eV to 10205 eV) of the peak at the L absorption edge of tungsten measured by X-ray absorption fine structure analysis (XAFS), Formula (1): (ab) / (cb)≦0.86 [In formula (1), a represents the energy (eV) at which the spectral slope is greatest in the range of 10200 eV to 10205 eV, When the spectral intensity at a (eV) is A, b represents the energy (eV) at which the spectral intensity of WO2 (tungsten (IV) oxide) becomes A in the range of 10200 eV to 10205 eV, c represents the energy (eV) at which the spectral intensity of WO3 (tungsten (VI) oxide) becomes A in the range of 10200 eV to 10205 eV. This is a positive electrode for lithium-ion secondary batteries.
[0015] Fig. 1 is a diagram showing XAFS measurement spectra of an example of a positive electrode for a lithium ion secondary battery (positive electrode sample) of the present disclosure, WO2, and WO3. Fig. 1 shows spectra including the rising position (10200 eV to 10205 eV) of the peak at the L absorption edge of tungsten by XAFS measurement of an example of a positive electrode for a lithium ion secondary battery (positive electrode sample) of the present disclosure, WO2 (tungsten oxide (IV)), and WO3 (tungsten oxide (VI)) (hereinafter, sometimes simply referred to as the tungsten spectrum of the XAFS measurement). FIG. 2 is a schematic diagram for explaining formula (1) of the present disclosure, in which the rising positions of the peaks at the L absorption edge of tungsten in the XAFS measurement spectra of the positive electrode sample, WO2, and WO3 are partially enlarged. The rising position of the peak of the L absorption edge of tungsten in the XAFS measurement spectrum represents the valence of the element tungsten. In the present disclosure, the energy (eV) at which the spectrum slope is maximum at the rising position (10200 eV to 10205 eV) of the peak of the L absorption edge of tungsten in the XAFS measurement spectrum of the positive electrode sample is a, and is used as an index of the peak rising position. a can be specified as the energy of the peak top of the derivative obtained by differentiating the spectrum in the range of 10200 eV to 10205 eV. When the spectrum intensity at a (eV) is A, the energy (eV) at which the spectrum intensity becomes A in the range of 10200 eV to 10205 eV of WO2 (tungsten oxide (IV)) is b, and the energy (eV) at which the spectrum intensity becomes A in the range of 10200 eV to 10205 eV of WO3 (tungsten oxide (VI)) is c. Here, WO2 is used as a standard sample of tetravalent tungsten, and WO3 is used as a standard sample of hexavalent tungsten.
[0016] When (ab) / (cb) in the above formula (1) is 1, tungsten in the positive electrode is hexavalent, and when it is 0, tungsten in the positive electrode is tetravalent. When the above formula (1): (ab) / (cb)≦0.86 is satisfied, it is interpreted that the tungsten in the positive electrode is tetravalent or has an average valence between 4 and 6. Tungsten having an average valence between 4 and 6 is considered to be a mixture of 4-valent tungsten and 6-valent tungsten, and has a lower average valence than 6-valent tungsten, and has high conductivity and the effect of lowering activation energy. Therefore, when the tungsten in the positive electrode is 4-valent or has an average valence between 4 and 6, the tungsten exerts high conductivity and the effect of lowering activation energy, and it is considered that the cell resistance can be reduced. In addition, low-valence tungsten is easily dissolved in Ni, Co, Mn, etc., which are used in positive electrode active materials. When dissolved in solid solution, it is thought that the diffusion resistance of lithium ions can be reduced by expanding the crystal axis of the crystal structure of the positive electrode active material. In this way, the spectrum at the rising position of the tungsten L absorption edge peak (10200 eV to 10205 eV) measured by XAFS at the positive electrode is Formula (1): (ab) / (cb)≦0.86 By satisfying the above, it is possible to provide a positive electrode for a lithium ion secondary battery that reduces the cell resistance of the lithium ion secondary battery.
[0017] In order to further reduce the cell resistance of the positive electrode, (ab) / (cb) in the formula (1) may be 0.65 or less, 0.60 or less, 0.55 or less, or 0.50 or less. In order to further reduce the cell resistance of the positive electrode, (ab) / (cb) in the formula (1) may be 0.15 or more. The XAFS measurements of the positive electrode for a lithium ion secondary battery, WO2, and WO3 of the present disclosure for determining (ab) / (cb) in the formula (1) can be performed by the method described in the Examples below.
[0018] (Cathode active material) The positive electrode for a lithium ion secondary battery of the present disclosure includes a positive electrode active material, and the positive electrode active material includes tungsten. The positive electrode active material of the present disclosure may contain a lithium metal composite oxide as an essential component, or may contain a lithium metal composite oxide having a layered structure. Examples of the lithium metal composite oxide include lithium nickel composite oxide, lithium manganese composite oxide, lithium cobalt composite oxide, lithium nickel cobalt aluminum composite oxide, lithium iron nickel manganese composite oxide, lithium nickel cobalt manganese composite oxide, etc. Among these, the lithium nickel cobalt manganese composite oxide may be used because it has more excellent resistance characteristics. In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Si, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. The content of these additional elements is preferably 0.1 mol or less relative to lithium. This also applies to the lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide described above. The positive electrode active material may have a conventionally known shape and may be in the form of particles, and the particle size may be the same as conventionally known particle sizes.
[0019] The tungsten contained in the positive electrode active material of the present disclosure may be present in any part of the positive electrode active material. In the positive electrode active material of the present disclosure, tungsten may be present on the surface of the positive electrode active material, or may be contained inside the lithium metal composite oxide in the positive electrode active material, or may be present in both. The positive electrode active material of the present disclosure may contain tungsten at least on its surface.
[0020] There is no particular limitation on the form in which tungsten is present on the surface of the positive electrode active material. For example, the tungsten compound may cover the entire surface of the positive electrode active material or a part of the surface. In addition, the tungsten compound may be granular, and the granular coating may be scattered on the surface of the positive electrode active material. The positive electrode active material may be a porous particle, and the tungsten compound may be present not only on the outer surface of the positive electrode active material but also on the inner surface (i.e., the surface inside the positive electrode active material). The positive electrode active material may be a secondary particle formed by agglomeration of primary particles of the positive electrode active material, or may be a secondary particle formed by agglomeration of particles of the positive electrode active material and a granular coating, and the tungsten compound may be present on the inner surface of the secondary particle of the positive electrode active material (the surface inside the positive electrode active material). When tungsten is present on the inner surface of the positive electrode active material, tungsten is likely to dissolve in the lithium metal composite oxide, and tungsten is incorporated into the lithium metal composite oxide in the positive electrode active material, widening the crystal axis of the crystal structure of the positive electrode active material, making it easy to reduce the diffusion resistance of lithium ions. In order to reduce cell resistance, the positive electrode active material of the present disclosure may contain tungsten on at least its surface, with some of the tungsten being incorporated into the lithium metal composite oxide, or may contain tungsten on the outer and inner surfaces, with some of the tungsten being incorporated into the lithium metal composite oxide. The locations where tungsten is present in the positive electrode active material of the present disclosure can be analyzed by, for example, transmission electron microscope-energy dispersive X-ray analysis (TEM-EDX).
[0021] The tungsten content in the positive electrode active material is not particularly limited, but from the viewpoint of reducing cell resistance, it may be, for example, 0.010 mass% or more, 0.015 mass% or more, 0.1 mass% or more, 0.4 mass% or more, 4.0 mass% or less, or 3.1 mass% or less. The tungsten content in the positive electrode active material can be determined by elemental analysis using ICP (inductively coupled plasma) emission spectrometry, specifically, by the method described in the Examples below.
[0022] The tungsten contained in the positive electrode active material of the present disclosure may be tetravalent tungsten or a mixture of tetravalent tungsten and hexavalent tungsten in which the tungsten spectrum in an XAFS measurement satisfies the above formula (1). Examples of the tetravalent tungsten compound contained in the positive electrode active material include WO2, lithium tungstate containing tetravalent tungsten, and lithium nickel cobalt manganese-based composite oxide containing tetravalent tungsten, and from the viewpoint of reducing the cell resistance, WO2 may be contained. Examples of the hexavalent tungsten compound contained in the positive electrode active material include lithium tungstate containing hexavalent tungsten, such as WO3 and Li2WO4, and lithium nickel cobalt manganese-based composite oxides containing hexavalent tungsten. From the viewpoint of reducing cell resistance, at least one of WO3 and Li2WO4 may be contained.
[0023] The method for producing the tungsten-containing positive electrode active material of the present disclosure is not particularly limited as long as the tungsten spectrum of the XAFS measurement satisfies the formula (1). As the method for producing the positive electrode active material, a method capable of producing the positive electrode active material as a final product can be appropriately adopted. The manufacturing method of the tungsten-containing positive electrode active material of the present disclosure can be used with at least a tetravalent tungsten raw material, because it can easily manufacture a positive electrode active material containing tungsten whose tungsten spectrum in XAFS measurement satisfies the formula (1). When a tetravalent tungsten raw material and a hexavalent tungsten raw material are used, the ratio of the tetravalent tungsten raw material and the hexavalent tungsten raw material can be appropriately adjusted so that the tungsten spectrum in XAFS measurement satisfies the formula (1). Examples of tetravalent tungsten raw materials include WO2, WCl4, etc., but may be WO2 in terms of reducing cell resistance. Examples of hexavalent tungsten raw materials include WO3 and lithium tungstate containing hexavalent tungsten such as Li2WO4, but may be at least one of WO3 and Li2WO4 in terms of reducing cell resistance. In addition, tetravalent tungsten can become stable hexavalent tungsten, for example, by firing at high temperatures. Therefore, the ratio of tetravalent tungsten to hexavalent tungsten contained in the manufactured positive electrode active material can be different from the ratio of the tetravalent tungsten raw material to the hexavalent tungsten raw material used in the manufacture of the positive electrode active material.
[0024] Examples of the method for producing a positive electrode active material containing tungsten include a conventionally known method in which a tungsten raw material is added in at least one of the following steps 1 to 3. Among them, a production method in which a tungsten raw material containing at least tetravalent tungsten is added in at least one of the following steps 2 and 3 may be used, since it is possible to easily produce a positive electrode active material containing tungsten whose tungsten spectrum in an XAFS measurement satisfies the above formula (1). Step 1: A step of reacting metal components (raw material compounds) in water under a predetermined temperature condition (for example, room temperature to 60° C.) to prepare a precursor (co-precipitated precursor) composed of a metal compound; Step 2: preparing a mixture containing the precursor and a lithium compound, and calcining the mixture to produce a lithium metal composite oxide. Step 3: Coating the surface of the lithium metal composite oxide with an optional compound.
[0025] For example, in the case where a tungsten raw material containing at least tetravalent tungsten is added in step 2, the step may be a step of preparing a mixture containing the precursor, a lithium compound, and the tungsten raw material, and calcining the mixture to produce a lithium metal composite oxide. The calcination can be carried out in an air atmosphere at a temperature of about 750° C. to 950° C. The calcination time may be about 8 hours to 20 hours. The ratio of tetravalent tungsten and hexavalent tungsten contained in the positive electrode active material can be appropriately adjusted by the calcination temperature and the calcination time. In step 2, the order in which the precursor, the lithium compound, and the tungsten raw material are mixed is not particularly limited.
[0026] For example, in step 3, when a tungsten raw material containing at least tetravalent tungsten is added to form a coating on the surface of the lithium metal composite oxide, a conventional method for forming a coating on an active material can be appropriately adopted. One example of the conventional method is mechanochemical treatment using various mechanochemical devices. For example, a desired mechanochemical reaction can be caused by using a mixing device such as an automatic mortar, and grinding using a ball mill, a planetary mill, a bead mill, or the like, to form a coating on at least a part of the surface of the lithium metal composite oxide. After the mechanochemical treatment, a heat treatment may be performed at a temperature of about 80°C to 300°C for about 0.5 hours to 5 hours.
[0027] The positive electrode for a lithium ion secondary battery of the present disclosure may further contain other components in addition to the positive electrode active material. The positive electrode for a lithium ion secondary battery of the present disclosure may have a positive electrode active material layer on one or both sides of a positive electrode current collector. The positive electrode current collector has a function of collecting the current from the positive electrode active material layer. Examples of the material of the positive electrode current collector include aluminum, SUS, nickel, chromium, gold, zinc, iron, and titanium. Examples of the shape of the positive electrode current collector include a foil shape, a plate shape, and a mesh shape.
[0028] The positive electrode active material layer may contain, in addition to the positive electrode active material, a conductive material, a binder, and the like, as necessary. The conductive material is not particularly limited as long as it can improve the conductivity of the positive electrode active material layer, but examples of the conductive material include carbon black such as acetylene black and ketjen black, carbon nanotubes (CNTs), and carbon nanofibers (CNFs). Examples of the binder include polyvinylidene fluoride (PVdF), polytetrafluoroethylene (PTFE), butylene rubber (BR), and styrene-butadiene rubber (SBR).
[0029] The content of the positive electrode active material in the positive electrode active material layer is not particularly limited, but may be 70% by mass or more, or may be 80% by mass or more. The content of the conductive material in the positive electrode active material layer is not particularly limited, but may be from 1 mass % to 15 mass %, or from 3 mass % to 13 mass %. The content of the binder in the positive electrode active material layer is not particularly limited, but may be from 1% by mass to 15% by mass, or from 1.5% by mass to 10% by mass.
[0030] The thickness of the positive electrode active material layer varies depending on the intended use of the battery, but may be from 10 μm to 250 μm, from 20 μm to 200 μm, or from 30 μm to 150 μm.
[0031] The positive electrode for a lithium ion secondary battery of the present disclosure includes a positive electrode active material containing tungsten, and can be produced by appropriately adopting a conventionally known production method as long as the tungsten spectrum obtained by XAFS measurement satisfies the above formula (1).
[0032] [Lithium-ion secondary battery] The lithium ion secondary battery of the present disclosure may include the positive electrode for lithium ion secondary batteries of the present disclosure, a negative electrode, and a non-aqueous electrolyte.
[0033] 3 is a cross-sectional view that shows a schematic diagram of a portion of the laminated structure of the electrode body of the lithium ion secondary battery of the present disclosure, but the electrode body of the lithium ion secondary battery of the present disclosure is not necessarily limited to this example. The electrode body 100 of the lithium ion secondary battery includes a positive electrode 6 including a positive electrode active material layer 2 and a positive electrode current collector 4, a negative electrode 7 including a negative electrode active material layer 3 and a negative electrode current collector 5, and a separator 1 interposed between the positive electrode 6 and the negative electrode 7. The positive electrode 6 is the positive electrode for a lithium ion secondary battery of the present disclosure. The positive electrode 6 may include a positive electrode lead connected to a positive electrode current collector (not shown). The lithium ion secondary battery of the present disclosure may further include an exterior body (not shown). The electrode assembly 100 and the non-aqueous electrolyte may be housed in the exterior body. The exterior body may be, for example, a metal case. Specific examples of the case shape include a coin type, a flat type, a cylindrical type, and a laminate type. The exterior body may be, for example, a pouch made of an aluminum laminate film.
[0034] The negative electrode 7 includes a negative electrode active material layer 3 containing a negative electrode active material. The negative electrode used in the present disclosure may usually include, in addition to the negative electrode active material layer 3, a negative electrode current collector 5 and a negative electrode lead connected to the negative electrode current collector (not shown). The negative electrode active material is not particularly limited as long as it can absorb and release lithium ions. For example, metallic lithium, lithium alloy, metal oxide containing lithium element, metal sulfide containing lithium element, metal nitride containing lithium element, carbon material such as graphite, hard carbon, soft carbon, Si, etc. can be mentioned, and graphite may be used. Graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.
[0035] The negative electrode active material layer may contain components other than the negative electrode active material, such as a binder or a thickener, if necessary. Examples of the binder include styrene butadiene rubber (SBR) and polyvinylidene fluoride (PVDF). Examples of the thickener include carboxymethyl cellulose (CMC).
[0036] The content of the negative electrode active material in the negative electrode active material layer may be 90% by mass or more, or may be from 95% by mass to 99% by mass. The content of the binder in the negative electrode active material layer may be from 0.1% by mass to 8% by mass, or from 0.5% by mass to 3% by mass. The content of the thickener in the negative electrode active material layer may be from 0.3% by mass to 3% by mass, or from 0.5% by mass to 2% by mass.
[0037] The thickness of the negative electrode active material layer is not particularly limited, but may be, for example, from 10 μm to 100 μm, or from 10 μm to 50 μm. The negative electrode current collector has a function of collecting the current from the negative electrode active material layer. The material of the negative electrode current collector may be SUS, Cu, Ni, Fe, Ti, Co, Zn, or the like. The shape of the negative electrode current collector may be the same as that of the positive electrode current collector described above.
[0038] The separator 1 used in the present disclosure is interposed between the positive electrode and the negative electrode to prevent these electrodes from coming into direct contact. In addition, the separator 1 has a plurality of fine pores that allow lithium ions, which are charge carriers, to pass through, and the charge carriers move through the fine pores during charging and discharging. For the separator 1, for example, insulating resins such as polyethylene (PE), polypropylene (PP), polyester, polyamide, etc. may be used. Also, the separator 1 may be a laminated sheet in which two or more layers of these resins are laminated. An example of such a laminated sheet is a three-layer sheet in which PP, PE, and PP are laminated in this order. The surface of the separator 1 may be provided with a heat-resistant layer (HRL). The thickness of the separator 1 may be, for example, not less than 10 μm and not more than 30 μm.
[0039] The non-aqueous electrolyte typically contains a non-aqueous solvent and a supporting salt. As the non-aqueous solvent, various organic solvents such as carbonates, ethers, esters, nitriles, sulfones, lactones, etc., which are used in the electrolyte of a general lithium ion secondary battery, can be used without any particular limitation. Specific examples include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), monofluoroethylene carbonate (MFEC), difluoroethylene carbonate (DFEC), monofluoromethyl difluoromethyl carbonate (F-DMC), trifluorodimethyl carbonate (TFDMC), etc. Such non-aqueous solvents can be used alone or in appropriate combination of two or more. As the supporting salt, for example, a lithium salt such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF6) can be suitably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.
[0040] A lithium ion secondary battery can be produced by adding the non-aqueous electrolyte to the electrode assembly. Other configurations of the lithium ion secondary battery of the present disclosure can be appropriately selected and adopted from conventionally known configurations, and for example, JP 2021-018895 A and the like can be referenced. EXAMPLES
[0041] EXAMPLES The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.
[0042] [Example 1] (Preparation of Positive Electrode Active Material) A raw material aqueous solution containing nickel sulfate, cobalt sulfate, and manganese sulfate in a molar ratio of 1:1:1 was prepared. Meanwhile, a reaction solution with pH adjusted using sulfuric acid and aqueous ammonia was prepared in a reaction vessel. In addition, an aqueous sodium hydroxide solution was prepared as a pH adjusting solution. The raw material aqueous solution was added to the reaction solution at a predetermined rate under stirring, and neutralized with a pH adjusting solution. The crystallized product was washed with water, filtered, and dried to obtain composite hydroxide particles (precursor particles). The obtained precursor particles were mixed with lithium carbonate so that the molar ratio (Li / Me) of lithium (Li) to the total of nickel, cobalt, and manganese (Me) was 1.1. This mixture was fired at 870°C for 15 hours in an electric furnace. After cooling to room temperature in the furnace, it was crushed to obtain a lithium metal composite oxide (LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2) was obtained. The obtained spherical sintered powder of lithium metal composite oxide was mixed with a predetermined amount of tungsten oxide (IV) (WO2) (W / (lithium metal composite oxide + WO2) = 0.6% by mass), treated in a mechanochemical device at 3000 rpm for 30 minutes, and further heat-treated at 150°C for 1 hour to obtain a positive electrode active material as a lithium metal composite oxide coated with tungsten oxide (IV) (WO2). The obtained positive electrode active material was analyzed by transmission electron microscope-energy dispersive X-ray analysis (TEM-EDX). Granular coatings were scattered on the outer surface of the positive electrode active material. The granular coatings were defined as the outer surface, and the part from the surface of the remaining part excluding the granular coatings to a depth of 10 nm was defined as the inner surface, and point analysis was performed. As a result, it was revealed that tungsten was present on the outer surface and inner surface. The granular coating on the outer surface contained 69 mass% tungsten, and the inner surface contained 0.4 mass% tungsten. The tungsten content here was calculated as W / (total mass within the analysis range) and was calculated as the average value of the measured values at three points. In addition, analysis of the obtained positive electrode active material using a transmission electron microscope-energy dispersive X-ray analysis (TEM-EDX) revealed that tungsten was incorporated into the primary particles of the lithium metal composite oxide.
[0043] (Preparation of positive electrode) The positive electrode active material thus prepared, acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were mixed in N-methylpyrrolidone (NMP) in a mass ratio of positive electrode active material:AB:PVDF=90:8:2 to prepare a paste for forming a positive electrode active material layer. This paste was applied to both sides of an aluminum foil having a thickness of 15 μm, dried, and then pressed to prepare a positive electrode.
[0044] (Preparation of lithium-ion secondary batteries for evaluation) A paste for forming a negative electrode active material layer was prepared by mixing natural graphite (C) as a negative electrode active material, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener in a mass ratio of C:SBR:CMC=98:1:1 in ion-exchanged water. This paste was applied to both sides of a copper foil with a thickness of 10 μm, dried, and pressed to prepare a negative electrode.
[0045] In addition, two porous polyolefin sheets having a thickness of 24 μm and a three-layer structure of PP / PE / PP were prepared as separator sheets. The positive and negative electrodes and the two separator sheets were stacked and wound to produce a wound electrode body. Electrode terminals were attached to the positive and negative electrodes of the wound electrode body by welding, and the resulting body was housed in a battery case with a liquid injection port.
[0046] Next, a non-aqueous electrolyte was injected through the inlet of the battery case, and the inlet was hermetically sealed. The non-aqueous electrolyte was a mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 3:4:3, with LiPF6 dissolved as a supporting salt at a concentration of 1.0 mol / L. In this manner, a lithium ion secondary battery for evaluation was obtained.
[0047] [Examples 2, 5, and 6] In the preparation of the positive electrode active material of Example 1, tungsten oxide (IV) (WO2) and tungsten oxide (VI) (WO3) were used instead of tungsten oxide (IV) (WO2), and at least one of the addition ratio of WO2 and WO3, the heat treatment temperature (100°C to 200°C) of WO2 and WO3 and the positive electrode active material, and the heating time (0.5 hours to 2 hours) was changed so that the (ab) / (cb) value of each positive electrode active material would be as shown in Table 1, and positive electrode active materials were prepared in the same manner as in Example 1. Using the obtained positive electrode active material, a positive electrode and a lithium ion secondary battery for evaluation were produced in the same manner as in Example 1.
[0048] [Comparative Example 1] A positive electrode active material was prepared in the same manner as in Example 1, except that tungsten oxide (VI) (WO3) was used instead of tungsten oxide (IV) (WO2). Using the obtained positive electrode active material, a positive electrode and a lithium ion secondary battery for evaluation were produced in the same manner as in Example 1.
[0049] [Example 3] In the preparation of the positive electrode active material of Example 1, composite hydroxide particles (precursor particles) were obtained in the same manner as in Example 1. The obtained precursor particles were mixed with lithium carbonate, tungsten oxide (IV) (WO2), and tungsten oxide (VI) (WO3) in a predetermined amount (W / (lithium metal composite oxide + WO2 + WO3) = 0.45% by mass), and the mixture was fired in an electric furnace at 870°C for 15 hours. The lithium carbonate was mixed so that the molar ratio (Li / Me) of lithium (Li) to the total of nickel, cobalt, and manganese (Me) was 1.1. After cooling to room temperature in the furnace, a crushing treatment was carried out to obtain a positive electrode active material as a spherical sintered powder in which primary particles were aggregated. The obtained positive electrode active material was analyzed by transmission electron microscope-energy dispersive X-ray analysis (TEM-EDX). Granular coatings were scattered on the outer surface of the positive electrode active material. The granular coatings were defined as the outer surface, and the part from the surface of the remaining part excluding the granular coatings to a depth of 10 nm was defined as the inner surface, and point analysis was performed. As a result, it was revealed that tungsten was present on the outer surface and inner surface. The granular coating on the outer surface contained 65 mass% tungsten, and the inner surface contained 0.9 mass% tungsten. The tungsten content here was calculated as W / (total mass within the analysis range) and was calculated as the average value of the measured values at three points. In addition, analysis of the obtained positive electrode active material using a transmission electron microscope-energy dispersive X-ray analysis (TEM-EDX) revealed that tungsten was incorporated into the primary particles of the lithium metal composite oxide. Using the obtained positive electrode active material, a positive electrode and a lithium ion secondary battery for evaluation were produced in the same manner as in Example 1.
[0050] [Examples 4, 7 to 12] In preparing the positive electrode active materials of Example 3, at least one of the ratio of tungsten oxide (IV) (WO2) to tungsten oxide (VI) (WO3) or lithium tungstate (Li2WO4), the amount of tungsten oxide (IV) (WO2), the firing temperature (830°C to 900°C), and the firing time (13 hours to 16 hours) was changed so that the (ab) / (cb) value of each positive electrode active material would be as shown in Table 1 or Table 2, and positive electrode active materials were prepared in the same manner as in Example 3. Using the obtained positive electrode active material, a positive electrode and a lithium ion secondary battery for evaluation were produced in the same manner as in Example 1.
[0051] [evaluation] (Measurement of tungsten content in positive electrode active material) The obtained positive electrode active material was weighed out in an amount of 1 g, and each was heated at 300°C in a mixture of 5 ml of commercially available nitric acid and 10 ml of hydrogen peroxide solution using a heater until complete dissolution was confirmed by visual inspection. The residue was filtered and the volume was adjusted to 100 ml with pure water, and the content (mass%) of tungsten element was measured based on ICP atomic emission spectrometry. The ICP atomic emission spectrometry used was an ICP atomic emission spectrometry device manufactured by Hitachi High-Tech Science Corporation.
[0052] (XAFS measurement of positive electrode) For the positive electrodes obtained in the respective Examples and Comparative Examples, XAFS measurement was carried out using the following device. XAFS measurements were also performed on standard samples of tungsten oxide (IV) (WO2) and tungsten oxide (VI) (WO3) using the following equipment. The value of (ab) / (cb) in the above formula (1) was determined from the spectrum at the rising position (10200 eV to 10205 eV) of the peak at the L absorption edge of tungsten measured by XAFS. Equipment: Hard X-ray XAFS at Aichi Synchrotron Light Center, Science and Technology Foundation Measurement range: 9897-11297 eV (peak position of the L absorption edge of tungsten) Measurement method: The positive electrode was measured by the fluorescence method, and the tungsten compound was measured by the transmission method. The transmission method for measuring the tungsten compound standard material detects the transmitted X-rays when irradiated with incident X-rays, while the fluorescence method for measuring the positive electrode detects the fluorescent X-rays generated when irradiated with incident X-rays, so even though the measurement methods are different, they can be expressed as the same spectrum. By normalizing the XAFS measurement data using the analysis software Athena, it is possible to compare the tungsten in the tungsten compound standard material with the tungsten in the positive electrode. In order to ensure the reproducibility of formula (1), a standard sample was measured every time a positive electrode sample was measured, and minute deviations were corrected. The results of (ab) / (cb) in the above formula (1) for Examples 1 to 12 and Comparative Example 1 are shown in Table 1 or Table 2.
[0053] (Resistance measurement) The lithium ion secondary batteries for evaluation prepared in each of the Examples and Comparative Examples were placed in an environment of 25° C. Activation (initial charging) was performed using a constant current-constant voltage method, in which each lithium ion secondary battery for evaluation was charged at a constant current of 1 / 3 C up to 4.2 V, and then charged at a constant voltage until the current reached 1 / 50 C, to reach a fully charged state. Thereafter, each lithium ion secondary battery for evaluation was discharged at a constant current of 1 / 3 C up to 3.0 V. The activated lithium ion secondary batteries for evaluation were adjusted to an open circuit voltage of 3.70V. They were placed in a temperature environment of -28°C. They were discharged at a current value of 20C for 8 seconds, and the voltage drop amount ΔV was obtained. Next, the voltage drop amount ΔV was divided by the discharge current value (20C) to calculate the battery resistance, which was defined as the initial resistance. The ratio of the initial resistance of the examples to the initial resistance of Comparative Example 1, which was set to 1.00, was obtained. The results are shown in Table 1 or Table 2.
[0054] [Table 1]
[0055] [Table 2]
[0056] As is clear from the performance evaluation results in Tables 1 and 2, it was confirmed that the positive electrodes for lithium ion secondary batteries of Examples 1 to 12, in which the tungsten spectra obtained by XAFS measurement satisfied the above formula (1): (ab) / (cb)≦0.86, reduced the cell resistance of the lithium ion secondary battery. According to the present disclosure, by using a positive electrode containing tetravalent tungsten or tungsten having an average valence between 4 and 6 as the positive electrode active material so that the tungsten spectrum in the XAFS measurement satisfies the above formula (1): (ab) / (cb)≦0.86, it has become possible to further reduce the cell resistance of a lithium-ion secondary battery. [Explanation of symbols]
[0057] 1 Separator 2 Positive electrode active material layer 3 Negative electrode active material layer 4 Positive electrode current collector 5 Negative electrode current collector 6 Positive electrode 7 Negative electrode 100 Electrode body
Claims
1. A positive electrode for a lithium ion secondary battery, comprising a positive electrode active material containing tungsten, The positive electrode has a spectrum at the rising position (10200 eV to 10205 eV) of the peak at the L absorption edge of tungsten measured by X-ray absorption fine structure analysis (XAFS), Formula (1): 0.15≦(a-b) / (c-b)≦0.65 [In formula (1), a represents the energy (eV) at which the spectral slope is greatest in the range of 10,200 eV to 10,205 eV, When the spectral intensity at a (eV) is A, b is WO 2 represents the energy (eV) at which the spectral intensity becomes A in the range of 10200 eV to 10205 eV of (tungsten (IV) oxide), c is WO 3 (tungsten(VI) oxide) represents the energy (eV) at which the spectral intensity becomes A in the range of 10200 eV to 10205 eV. Positive electrode for lithium-ion secondary batteries.
2. 2. The positive electrode for lithium ion secondary batteries according to claim 1, wherein the content of said tungsten relative to the positive electrode active material is 0.015% by mass to 3.1% by mass.
Citation Information
Patent Citations
Nano-tungsten oxide, one-step vapor phase reduction preparation method of nano-tungsten oxide and application of nano-tungsten oxide
CN104961159A
Electrode composition containing doped tungsten oxide and method of making same
JP2003509829A
Nonaqueous electrolyte, and nonaqueous electrolyte battery
JP2012023034A
Positive electrode active material and lithium ion secondary battery
JP2017183045A
Lithium secondary battery positive-electrode active material, lithium secondary battery positive-electrode and lithium secondary battery
JP2018098183A