Binder resin composition for toner
The binder resin composition for toner, featuring a polyester resin with alkylene oxide adducts and amine-based polymer compounds, addresses the challenges of low-temperature fixing and hot offset resistance, while enhancing scratch and bending resistance, ensuring durable image quality.
Patent Information
- Application Number
- JP2020205928
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-11
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-12-11
AI Technical Summary
Existing electrophotographic toner binder resins face challenges in achieving both low-temperature fixing properties and hot offset resistance while maintaining excellent scratch resistance and bending resistance, with conventional approaches either compromising on flexibility or durability.
A binder resin composition for toner is developed, comprising a polyester resin with a softening point between 120°C and 150°C, containing alkylene oxide adducts of bisphenol A, aromatic dicarboxylic acid compounds, and trivalent or higher valent alcohol and carboxylic acid compounds, along with an amine-based polymer compound to introduce a crosslinked structure, enhancing flexibility and hardness.
The composition achieves excellent low-temperature fixing properties, hot offset resistance, scratch resistance, and bending resistance, providing a wide fixable temperature range and improved durability of images.
Smart Images

Figure 0007572225000001 
Figure 0007572225000002 
Figure 0007572225000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a binder resin composition for a toner used for developing a latent image formed in an electrophotographic method, an electrostatic recording method, an electrostatic printing method or the like, a method for producing the binder resin composition, and a toner for electrophotography containing the binder resin composition. [Background technology]
[0002] In the field of electrophotography, with the development of electrophotographic systems, there is a demand for the development of toners that can handle higher image quality and higher speeds. For example, Patent Document 1 describes a binder resin composition for toner that contains a resin composition obtained by condensing an amorphous polyester resin having an acid group with a polyalkyleneimine, for the purpose of providing a binder resin composition for toner that exhibits excellent storage stability of the toner and excellent pigment dispersibility. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-20866 A Summary of the Invention [Problem to be solved by the invention]
[0004] With the increasing need for higher image quality and higher speed in electrophotographic systems, in addition to excellent low-temperature fixing ability and hot offset resistance to obtain a wide fixable temperature range, improvements in performance such as abrasion resistance and folding resistance, which indicate the durability of the formed image, are also required. In particular, in order to ensure abrasion resistance, the polyester resin used as the binder resin for toner needs to have sufficient hardness, but simply increasing the molecular weight reduces the low-temperature fixing ability. On the other hand, when a crosslinked structure using a trivalent monomer such as trimellitic anhydride is introduced into a polyester resin to increase the molecular weight of the polyester resin, the molecular weight distribution is broadened and low-temperature fixability can be maintained even when the molecular weight is increased, so that low-temperature fixability and abrasion resistance can be achieved to a certain extent. However, the abrasion resistance is still insufficient to meet the requirements, and further, when a crosslinked structure using a trivalent monomer such as trimellitic anhydride is introduced into a polyester resin, image deterioration is confirmed during a bending test, and it has been found that the durability of the image is not sufficient just by increasing the molecular weight of the polyester resin. In Patent Document 1, although the storage stability and pigment dispersibility of the toner are improved, it is found that there is room for improvement in terms of achieving both excellent low-temperature fixing property and hot offset resistance, and excellent abrasion resistance and folding resistance. The present invention relates to a binder resin composition for toners which has excellent low-temperature fixing property and hot offset resistance while also having excellent abrasion resistance and folding resistance, a method for producing the binder resin composition, and an electrophotographic toner containing the binder resin composition. [Means for solving the problem]
[0005] The present inventors have found that the above-mentioned problems can be solved by providing a binder resin composition for toner containing a polyester resin having a softening point within a predetermined range, the polyester resin being a polycondensate of raw material monomers including at least one trivalent or higher raw material monomer selected from an alkylene oxide adduct of bisphenol A, an aromatic dicarboxylic acid compound, a trivalent or higher alcohol, and a trivalent or higher carboxylic acid compound, and an amine polymer compound.
[0006] That is, the present invention relates to the following embodiments [1] to [3]. [1] A toner binder resin composition containing a polyester resin (A) having a softening point of 120° C. or more and 150° C. or less, The polyester-based resin (A) is a polycondensate of raw material monomer (a) containing at least one trivalent or higher raw material monomer selected from an alkylene oxide adduct of bisphenol A, an aromatic dicarboxylic acid compound, a trivalent or higher alcohol, and a trivalent or higher carboxylic acid compound, and an amine-based polymer compound. [2] A method for producing the binder resin composition for toner according to the above [1], comprising the following step A: Step A: A step of polycondensing an alcohol component (a-al) and a carboxylic acid component (a-ac) constituting the polyester resin (A) other than the trivalent or higher raw monomer, adding the trivalent or higher raw monomer to polycondense, and then adding an amine polymer compound to polycondense. [3] A toner for electrophotography, comprising the binder resin composition according to [1] above. Effect of the Invention
[0007] According to the present invention, it is possible to provide a binder resin composition for a toner which has excellent low-temperature fixing property and hot offset resistance while also having excellent abrasion resistance and folding resistance, a method for producing the binder resin composition, and a toner for electrophotography containing the binder resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] [Binder resin composition for toner] The binder resin composition for toner of the present invention (hereinafter also simply referred to as "the binder resin composition of the present invention") contains a polyester resin (A) having a softening point of 120°C or higher and 150°C or lower. The polyester resin (A) is a polycondensate of raw material monomer (a) including an alkylene oxide adduct of bisphenol A, an aromatic dicarboxylic acid compound, a trivalent or higher alcohol, and a trivalent or higher carboxylic acid compound (hereinafter simply referred to as a "trivalent or higher raw material monomer"), and an amine polymer compound. The binder resin composition of the present invention exhibits excellent low-temperature fixing property and hot offset resistance of the toner, as well as excellent abrasion resistance and folding resistance.
[0009] The reason why the present invention has an effect is not clear, but is thought to be as follows. The binder resin composition of the present invention contains a polyester resin having a softening point in a predetermined range, and the polyester resin is a polycondensate of raw material monomer (a) containing an alkylene oxide adduct of bisphenol A, an aromatic dicarboxylic acid compound, a raw material monomer having a valence of three or more, and an amine polymer compound. In addition to the introduction of a crosslinked structure by the raw material monomer having a valence of three or more, the polyester resin further contains a crosslinked structure using an amine polymer compound as a crosslinking agent. Since the amine polymer compound has high flexibility, it is possible to achieve both the hardness and flexibility of the polyester resin while maintaining excellent low-temperature fixing property and hot offset resistance, and it is considered that the abrasion resistance and folding resistance can be improved.
[0010] The definitions of various terms used in this specification are given below. The crystallinity of a resin is represented by a crystallinity index defined as the ratio of the softening point to the maximum endothermic peak temperature measured by a differential scanning calorimeter (DSC), that is, "softening point / maximum endothermic peak temperature." The term "crystalline resin" refers to a resin having a crystallinity index of 0.6 or more, preferably 0.7 or more, more preferably 0.9 or more, and 1.4 or less, preferably 1.2 or less. The term "amorphous resin" refers to a resin in which no endothermic peak is observed by differential scanning calorimetry (DSC), or, if an endothermic peak is observed, the resin has a crystallinity index of less than 0.6 or more than 1.4. The maximum endothermic peak temperature refers to the temperature of the endothermic peak with the largest peak area among the endothermic peaks observed under the conditions of the measurement method described in the Examples. The crystallinity of the resin can be adjusted by the types and ratios of the raw material monomers, and the production conditions (e.g., reaction temperature, reaction time, cooling rate), etc. The "polyester resin" may include a polyester resin that has been modified to such an extent that its properties are not substantially impaired. Examples of modified polyester resins include amide-modified polyester resins in which a polyester resin is modified with an amide bond, urethane-modified polyester resins in which a polyester resin is modified with a urethane bond, and epoxy-modified polyester resins in which a polyester resin is modified with an epoxy bond. "Bisphenol A" means 2,2-bis(4-hydroxyphenyl)propane. The "carboxylic acid compound" includes, for example, carboxylic acids, their anhydrides, and alkyl esters having 1 to 3 carbon atoms. The term "binder resin composition" refers to a binder resin component in a toner that contains a polyester resin (A).
[0011] <Polyester resin (A)> The polyester-based resin (A) (hereinafter, also simply referred to as "resin (A)") is a polycondensate of raw material monomer (a) containing an amine-based polymer compound and at least one trivalent or higher raw material monomer selected from the group consisting of an alkylene oxide adduct of bisphenol A, an aromatic dicarboxylic acid compound, a trivalent or higher alcohol, and a trivalent or higher carboxylic acid compound, from the viewpoint of improving abrasion resistance and folding resistance while maintaining low-temperature fixing property and hot offset resistance. From the same viewpoint as above, the polyester resin (A) is preferably an amorphous polyester resin.
[0012] (Alkylene oxide adduct of bisphenol A) The raw material monomer (a) constituting the polyester resin (A) includes an alkylene oxide adduct of bisphenol A. The alkylene oxide adduct of bisphenol A (hereinafter also referred to as "BPA-AO") is preferably a compound represented by the formula (I): [ka] [In the formula, OR 11 and R12 O is an alkyleneoxy group, R 11 and R 12 each independently represents an alkylene group having 1 to 4 carbon atoms (preferably an ethylene group or a propylene group), x and y represent the average number of moles of alkylene oxide added, each independently being a positive number, and the average value of the sum of x and y is preferably 1 to 4.
[0013] BPA-AO is preferably a propylene oxide adduct of bisphenol A (hereinafter also referred to as "BPA-PO") or an ethylene oxide adduct of bisphenol A (hereinafter also referred to as "BPA-EO"). These BPA-AOs may be used alone or in combination of two or more.
[0014] The amount of BPA-AO in the alcohol component (a-al) (hereinafter also referred to as "alcohol component (a-al)") constituting the polyester resin (A) is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, even more preferably 98 mol% or more, and is 100 mol% or less, even more preferably 100 mol%.
[0015] (Aromatic dicarboxylic acid compounds) The raw material monomer (a) constituting the polyester resin (A) includes an aromatic dicarboxylic acid compound. Examples of aromatic dicarboxylic acid compounds include phthalic acid, isophthalic acid, and terephthalic acid. Among these, isophthalic acid and terephthalic acid are preferred, and terephthalic acid is more preferred. The amount of aromatic dicarboxylic acid compounds in the carboxylic acid component (a-ac) (hereinafter also referred to as "carboxylic acid component (a-ac)") constituting the polyester resin (A) is preferably 40 mol % or more, more preferably 50 mol % or more, even more preferably 60 mol % or more, and preferably 95 mol % or less, more preferably 90 mol % or less, even more preferably 80 mol % or less.
[0016] (Trivalent or higher raw monomers) The raw material monomer (a) constituting the polyester resin (A) contains at least one kind of raw material monomer having a valence of three or more selected from a trivalent or higher alcohol and a trivalent or higher carboxylic acid compound. Examples of trihydric or higher polyhydric alcohols include glycerin, pentaerythritol, trimethylolpropane, sorbitol, and sorbitan. Examples of the trivalent or higher polyvalent carboxylic acid compound include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, and pyromellitic acid.
[0017] The tri- or higher valent raw material monomer is preferably a tri- or higher valent carboxylic acid compound, more preferably trimellitic acid or its anhydride. When a trivalent or higher carboxylic acid compound is used as the trivalent or higher raw monomer, the amount of the trivalent or higher carboxylic acid compound in the carboxylic acid component (a-ac) constituting the polyester resin (A) is preferably 3 mol % or more, more preferably 5 mol % or more, even more preferably 10 mol % or more, even more preferably 15 mol % or more, even more preferably 20 mol % or more, and preferably 50 mol % or less, more preferably 45 mol % or less, even more preferably 40 mol % or less.
[0018] The raw material monomer (a) may contain an alcohol component or a carboxylic acid compound other than BPA-AO, an aromatic dicarboxylic acid compound, and a raw material monomer having a valence of three or more.
[0019] Examples of the other alcohol component include diols other than BPA-AO, such as aliphatic diols and alicyclic diols. The aliphatic diol preferably has 2 or more carbon atoms and preferably has 18 or less carbon atoms. Examples of the aliphatic diol include ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, neopentyl glycol, 1,4-butenediol, 1,2-pentanediol, 1,4-pentanediol, 2,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, and the like. Examples of the dimethyl-1,2-butanediol include 1,5-hexanediol, 2,5-hexanediol, 1,6-hexanediol, 3,3-dimethyl-1,2-butanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, 1,13-tridecanediol, and 1,14-tetradecanediol. Examples of the alicyclic diol include hydrogenated bisphenol A and adducts of hydrogenated bisphenol A with alkylene oxides having 2 to 4 carbon atoms (average number of moles added: 2 to 12). From the viewpoint of adjusting the molecular weight and softening point of the resin, the raw material monomer (a) may contain a monohydric alcohol as another alcohol component. These other alcohol components may be used alone or in combination of two or more. The amount of other diols in the alcohol component (a-al) constituting the polyester resin (A) is preferably 10 mol % or less, more preferably 5 mol % or less, even more preferably 1 mol % or less, and even more preferably 0 mol %.
[0020] Other carboxylic acid compounds include, for example, linear, branched, or cyclic aliphatic dicarboxylic acid compounds. Examples of linear or branched aliphatic dicarboxylic acid compounds include oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid, pentanedioic acid, adipic acid, sebacic acid, dodecanedioic acid, azelaic acid, and succinic acid substituted with an aliphatic hydrocarbon group having from 1 to 20 carbon atoms. An example of the alicyclic dicarboxylic acid compound is cyclohexanedicarboxylic acid. These other carboxylic acid compounds may be used alone or in combination of two or more. The amount of aliphatic dicarboxylic acid compounds in the carboxylic acid component (a-ac) constituting the polyester resin (A) is preferably 10 mol % or less, more preferably 5 mol % or less, even more preferably 1 mol % or less, and even more preferably 0 mol %.
[0021] The equivalent ratio of the carboxyl group (COOH group) of the carboxylic acid component (a-ac) to the hydroxyl group (OH group) of the alcohol component (a-al) [COOH group / OH group] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less.
[0022] (Amine polymer compounds) The amine-based polymer compound is a polymer compound that can be incorporated into the molecular skeleton of the resin (A) by polycondensation reaction with the acid group of the carboxylic acid component (a-ac) constituting the resin (A) from the viewpoint of improving the abrasion resistance and folding resistance while maintaining the low-temperature fixing property and hot offset resistance. In the present invention, the molecular weight of the amine-based polymer compound is 500 or more.
[0023] From the viewpoint of further improving the abrasion resistance and folding resistance while maintaining the low-temperature fixing property and hot offset resistance, the amine-based polymer compound preferably contains a repeating unit including an amino group and an alkylene group having 2 to 6 carbon atoms. The amine-based polymer compound contains a repeating unit including an alkylene group having from 2 to 6 carbon atoms, and is therefore considered to have high flexibility, and to be able to maintain excellent low-temperature fixing property and hot offset resistance while achieving both hardness and flexibility of the resin, thereby enabling further improvement in abrasion resistance and bending resistance. From the viewpoint of reactivity with the carboxylic acid component (a-ac), the amino group contained in the repeating unit preferably contains at least one type selected from a primary amino group and a secondary amino group, more preferably contains at least a primary amino group, and even more preferably is a primary amino group. The amino group contained in the amine polymer compound may be present in the main chain or in the side chain. The polymer structure of the amine polymer compound may be a linear or branched structure. The amine-based polymer compounds may be used alone or in combination.
[0024] From the viewpoint of further improving the abrasion resistance and folding resistance while maintaining the low-temperature fixing property and hot offset resistance, the repeating unit is preferably a unit derived from at least one selected from allylamine, diallylamine, vinylamine, and ethyleneimine, and more preferably a unit derived from at least one selected from allylamine and ethyleneimine. Examples of the amine-based polymeric compound include polyallylamine and polyalkyleneimine.
[0025] Examples of polyallylamine include polymers having amino groups on the side chains, such as homopolymers or copolymers of allylamine compounds such as allylamine and diallylamine. Among these, homopolymers of allylamine compounds are preferred. From the viewpoint of further improving abrasion resistance and folding resistance while maintaining low-temperature fixing property and hot offset resistance, the weight average molecular weight of the polyallylamine is preferably 800 or more, more preferably 3,000 or more, even more preferably 5,000 or more, and is preferably 30,000 or less, more preferably 20,000 or less, even more preferably 10,000 or less. The value of the weight average molecular weight is determined by the method described in the Examples.
[0026] The polyalkyleneimine is preferably a polyalkyleneimine having an alkylene group with 2 or more and 6 or less carbon atoms, more preferably a polyalkyleneimine having an alkylene group with 2 or more and 4 or less carbon atoms, even more preferably polyethyleneimine or polypropyleneimine, and even more preferably polyethyleneimine. The polymer structure of the polyalkyleneimine may be a linear or branched structure, and among these, a branched structure is preferred from the viewpoint of further improving abrasion resistance and folding resistance while maintaining low-temperature fixing property and hot offset resistance. When the polyalkyleneimine has a branched structure, the structure may contain, in addition to a secondary amino group (imino group), a tertiary amino group and a primary amino group. When the polyalkyleneimine has a branched structure, the total proportion of primary amino groups and secondary amino groups in the amino groups of the alkyleneimine is preferably 50% or more, more preferably 60% or more, even more preferably 70% or more, and preferably 100% or less. The total ratio of the primary amino group and the secondary amino group is 13 It is determined by C-NMR.
[0027] From the viewpoint of further improving abrasion resistance and folding resistance while maintaining low-temperature fixing property and hot offset resistance, the number average molecular weight of the polyalkyleneimine is preferably 500 or more, more preferably 800 or more, and even more preferably 1,000 or more, and is preferably 10,000 or less, more preferably 5,000 or less, even more preferably 3,000 or less, and even more preferably 2,000 or less. The value of the number average molecular weight is determined by the method described in the Examples.
[0028] Among these, from the viewpoint of further improving abrasion resistance and folding resistance while maintaining low-temperature fixing property and hot offset resistance, the amine-based polymer compound is preferably one or more selected from polyallylamine and polyalkyleneimine having an alkylene group with 2 to 6 carbon atoms, more preferably one or more selected from polyallylamine and polyethyleneimine, and even more preferably polyallylamine.
[0029] From the viewpoint of further improving abrasion resistance and folding resistance while maintaining low-temperature fixing property and hot offset resistance, the amount of the amine-based polymer compound in the raw material monomer (a) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, even more preferably 2% by mass or more, and is preferably 10% by mass or less, more preferably 7% by mass or less, even more preferably 5% by mass or less, even more preferably 4% by mass or less.
[0030] (Physical properties of resin (A)) From the viewpoint of improving abrasion resistance and folding resistance while maintaining low-temperature fixing property and hot offset resistance, the softening point of the resin (A) is 120°C or higher, preferably 125°C or higher, more preferably 130°C or higher, and even more preferably 135°C or higher, and is 150°C or lower, preferably 145°C or lower, and more preferably 140°C or lower.
[0031] The glass transition temperature of resin (A) is preferably 40°C or higher, more preferably 45°C or higher, even more preferably 50°C or higher, and preferably 90°C or lower, more preferably 80°C or lower, even more preferably 70°C or lower, even more preferably 60°C or lower.
[0032] The acid value of the resin (A) is preferably 2 mgKOH / g or more, more preferably 5 mgKOH / g or more, even more preferably 10 mgKOH / g or more, and preferably 40 mgKOH / g or less, more preferably 30 mgKOH / g or less, even more preferably 25 mgKOH / g or less, even more preferably 20 mgKOH / g or less.
[0033] The softening point, glass transition temperature, and acid value of the resin (A) can be appropriately adjusted by the type and ratio of the raw material monomer (a), as well as production conditions such as reaction temperature, reaction time, and cooling rate. These values are determined by the method described in the Examples below. When two or more types of resin (A) are used in combination, it is preferable that the physical properties of the mixture are each within the above-mentioned range.
[0034] The content of the resin (A) in the binder resin composition of the present invention is preferably 40% by mass or more, more preferably 50% by mass or more, even more preferably 60% by mass or more, even more preferably 70% by mass or more, and is preferably 100% by mass or less, more preferably 95% by mass or less, even more preferably 90% by mass or less, even more preferably 85% by mass or less.
[0035] (Production of Resin (A)) The resin (A) can be obtained by subjecting raw material monomers (a) including BPA-AO, an aromatic dicarboxylic acid compound, a raw material monomer having a valence of three or more, and an amine-based polymer compound to a polycondensation reaction. The order of addition of the raw material monomers of the raw material monomer (a) is not particularly limited, but the resin (A) is preferably produced by a method including the following step A. Step A: A step of polycondensing an alcohol component (a-al) and a carboxylic acid component (a-ac) constituting the polyester resin (A) other than the trivalent or higher raw monomer, adding the trivalent or higher raw monomer to polycondense, and then adding an amine polymer compound to polycondense.
[0036] In the polycondensation reaction of the raw material monomer (a), an esterification catalyst such as tin(II) dioctylate, dibutyltin oxide, or titanium diisopropylate bistriethanolamine may be used in an amount of 0.01 part by mass or more and 5 parts by mass or less per 100 parts by mass of the total amount of the raw material monomer (a); or an esterification promoter such as gallic acid (same as 3,4,5-trihydroxybenzoic acid) may be used in an amount of 0.001 part by mass or more and 0.5 part by mass or less per 100 parts by mass of the total amount of the raw material monomer (a). In addition, when raw material monomers having an unsaturated bond such as fumaric acid are used in the polycondensation reaction, a radical polymerization inhibitor may be used, if necessary, in an amount of preferably 0.001 to 0.5 parts by mass per 100 parts by mass of the total amount of the raw material monomers (a). Examples of the radical polymerization inhibitor include 4-tert-butylcatechol. The temperature of the polycondensation reaction is preferably 120° C. or higher, more preferably 160° C. or higher, and even more preferably 180° C. or higher, and is preferably 260° C. or lower, and more preferably 240° C. or lower. The polycondensation reaction may be carried out in an inert gas atmosphere.
[0037] The amount of the amine polymer compound in the raw material monomer (a) is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, even more preferably 1% by mass or more, even more preferably 2% by mass or more, and is preferably 10% by mass or less, more preferably 7% by mass or less, even more preferably 5% by mass or less, even more preferably 4% by mass or less.
[0038] <Amorphous polyester resin (B)> The binder resin composition of the present invention preferably further contains, in addition to the polyester resin (A), an amorphous polyester resin (B) other than the polyester resin (A) (hereinafter, simply referred to as "resin (B)") from the viewpoint of further improving abrasion resistance and folding resistance while maintaining excellent low-temperature fixing property and hot offset resistance. The resin (B) preferably has a softening point different from that of the aforementioned resin (A), and more preferably has a softening point lower than that of the aforementioned resin (A).
[0039] The resin (B) is preferably an amorphous polyester resin which is a polycondensation product of an alcohol component (b-al) and a carboxylic acid component (b-ac).
[0040] (Alcohol content (b-al)) The alcohol component (b-al) preferably contains BPA-AO. The BPA-AO is preferably BPA-AO represented by the above formula (I). The BPA-AO is preferably BPA-PO or BPA-EO, more preferably BPA-PO. That is, the alcohol component (b-al) preferably contains BPA-PO. These BPA-AOs may be used alone or in combination of two or more. The amount of BPA-AO in the alcohol component (b-al) is preferably 80 mol% or more, more preferably 90 mol% or more, even more preferably 95 mol% or more, even more preferably 98 mol% or more, and is 100 mol% or less, even more preferably 100 mol%. When the alcohol component (b-al) contains BPA-PO, the amount of BPA-PO in the alcohol component (b-al) is preferably 50 mol % or more, more preferably 60 mol % or more, even more preferably 70 mol % or more, and is 100 mol % or less, preferably 90 mol % or less.
[0041] The alcohol component (b-al) may contain other alcohol components different from BPA-AO. Examples of the other alcohol components include aliphatic diols, alicyclic diols, and trihydric or higher polyhydric alcohols. Examples of the aliphatic diol, the alicyclic diol, and the trihydric or higher polyhydric alcohol are the same as those exemplified above. From the viewpoint of adjusting the molecular weight and softening point of the resin, the alcohol component (b-al) may contain a monohydric alcohol. These alcohol components may be used alone or in combination of two or more.
[0042] (Carboxylic acid component (b-ac)) Examples of the carboxylic acid component (b-ac) include dicarboxylic acid compounds and trivalent or higher polyvalent carboxylic acid compounds. Examples of the dicarboxylic acid compound include aromatic dicarboxylic acid compounds, aliphatic dicarboxylic acid compounds, and alicyclic dicarboxylic acid compounds. Examples of the aromatic dicarboxylic acid compound, the linear or branched aliphatic dicarboxylic acid compound, the alicyclic dicarboxylic acid compound, and the trivalent or higher polyvalent carboxylic acid compound are the same as those exemplified above. Among these dicarboxylic acid compounds, the carboxylic acid component (b-ac) preferably contains an aromatic dicarboxylic acid compound, and more preferably contains terephthalic acid. The amount of the aromatic dicarboxylic acid compound in the carboxylic acid component (b-ac) is preferably 50 mol% or more, more preferably 60 mol% or more, even more preferably 65 mol% or more, even more preferably 70 mol% or more, and is 100 mol% or less, even more preferably 100 mol%. The content of the trivalent or higher polyvalent carboxylic acid compound in the carboxylic acid component (b-ac) is preferably 10 mol % or less, more preferably 5 mol % or less, even more preferably 1 mol % or less, and even more preferably 0 mol %. From the viewpoint of adjusting the molecular weight and softening point of the resin, the carboxylic acid component (b-ac) may appropriately contain a monovalent carboxylic acid. These carboxylic acid components may be used alone or in combination of two or more.
[0043] The equivalent ratio of the carboxyl group (COOH group) of the carboxylic acid component (b-ac) to the hydroxyl group (OH group) of the alcohol component (b-al) [COOH group / OH group] is preferably 0.7 or more, more preferably 0.8 or more, and is preferably 1.3 or less, more preferably 1.2 or less, and even more preferably 1.0 or less.
[0044] (Physical properties of resin (B)) From the viewpoint of further improving abrasion resistance and folding resistance while maintaining excellent low-temperature fixing property and hot offset resistance, the softening point of resin (B) is preferably 80° C. or higher, more preferably 90° C. or higher, even more preferably 100° C. or higher, and is preferably less than 120° C., more preferably 115° C. or lower, even more preferably 110° C. or lower. The difference in softening point between resin (A) and resin (B) is preferably 5°C or more, more preferably 10°C or more, even more preferably 20°C or more, even more preferably 30°C or more, and is preferably 60°C or less, more preferably 50°C or less, even more preferably 40°C or less. The glass transition temperature of resin (B) is preferably 40°C or higher, more preferably 50°C or higher, even more preferably 55°C or higher, and preferably 90°C or lower, more preferably 80°C or lower, even more preferably 70°C or lower. The acid value of the resin (B) is preferably 2 mgKOH / g or more, more preferably 3 mgKOH / g or more, even more preferably 4 mgKOH / g or more, and preferably 40 mgKOH / g or less, more preferably 30 mgKOH / g or less, even more preferably 20 mgKOH / g or less.
[0045] The softening point, glass transition temperature, and acid value of the resin (B) can be appropriately adjusted by the types and ratios of the raw material monomers, as well as production conditions such as reaction temperature, reaction time, and cooling rate. These values are determined by the method described in the Examples below. When two or more types of resin (B) are used in combination, it is preferable that the physical properties of the mixture are each within the above-mentioned ranges.
[0046] The resin (B) may be produced, for example, by a method including a step B of carrying out a polycondensation reaction of a raw material monomer (b) containing an alcohol component (b-al) and a carboxylic acid component (b-ac). As the conditions for the polycondensation reaction, for example, the conditions shown for the polycondensation reaction for the resin A described above can be applied.
[0047] The content of the resin (B) in the binder resin composition of the present invention is, from the viewpoint of further improving the abrasion resistance and folding resistance while maintaining excellent low-temperature fixing property and hot offset resistance, preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 15% by mass or more, and is preferably 60% by mass or less, more preferably 50% by mass or less, even more preferably 40% by mass or less, even more preferably 30% by mass or less.
[0048] [Electrophotographic toner] The toner for electrophotography of the present invention (hereinafter also referred to as "the toner of the present invention") contains the binder resin composition, and preferably contains a colorant and the binder resin composition. The toner of the present invention contains, for example, toner particles and an external additive. The toner particles contain the binder resin composition, and preferably contain a colorant and the binder resin composition. The toner particles may contain, for example, a colorant derivative, a charge control agent, a release agent such as wax, and other additives. The content of the binder resin composition in the toner is preferably 80% by mass or more, more preferably 85% by mass or more, and further preferably 87% by mass or more, and 100% by mass or less.
[0049] <Coloring agent> The colorant may be either a pigment or a dye. Examples of the pigment include azo pigments, phthalocyanine pigments, condensed polycyclic pigments, and lake pigments. Examples of azo pigments include insoluble azo pigments such as CI Pigment Red 3, soluble azo pigments such as CI Pigment Red 48:1, and condensed azo pigments such as CI Pigment Red 144. Examples of the phthalocyanine pigment include copper phthalocyanine pigments such as CI Pigment Blue 15:3, and polyhalogenated zinc phthalocyanine pigments such as CI Pigment Green 58. Examples of the condensed polycyclic pigments include anthraquinone pigments such as CI Pigment Red 177, perylene pigments such as CI Pigment Red 123, perinone pigments such as CI Pigment Orange 43, quinacridone pigments such as CI Pigment Red 122, naphthol pigments such as CI Pigment Red 269, dioxazine pigments such as CI Pigment Violet 23, isoindolinone pigments such as CI Pigment Yellow 139 and 185, isoindoline pigments such as CI Pigment Orange 66, quinophthalone pigments such as CI Pigment Yellow 138, nickel azo complex pigments such as CI Pigment Yellow 150, indigo pigments such as CI Pigment Red 88, metal complex pigments such as CI Pigment Green 8, and diketopyrrolopyrrole pigments such as CI Pigment Red 254, CI Pigment Red 255, and CI Pigment Orange 71. An example of a lake pigment is CI Pigment Red 57:1.
[0050] Examples of the dyes include azine dyes, anthraquinone dyes, perinone dyes, and rhodamine dyes. More specific examples of the dyes include CI Solvent Black 5, CI Solvent Black 7, Spirit Black SB, Toluidine Blue, CI Solvent Blue 11, CI Solvent Blue 12, CI Solvent Blue 35, CI Solvent Blue 59, CI Solvent Blue 74, 1-aminoanthraquinone, 2-aminoanthraquinone, hydroxyethylaminoanthraquinone, CI Solvent Violet 47, Solvent Orange 60, Solvent Orange 78, Solvent Orange 90, Solvent Violet 29, Solvent Red 135, Solvent Red 162, Solvent Red 179, and Rhodamine-B Base.
[0051] From the viewpoint of the image density of the toner, the content of the colorant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, even more preferably 3 parts by mass or more, relative to 100 parts by mass of the total amount of the binder resin components of the toner, and is preferably 40 parts by mass or less, more preferably 30 parts by mass or less, even more preferably 15 parts by mass or less.
[0052] <Release agent> The toner of the present invention may contain a release agent. Examples of the release agent include polypropylene wax, polyethylene wax, polypropylene-polyethylene copolymer wax, hydrocarbon waxes such as microcrystalline wax, paraffin wax, Fischer-Tropsch wax, and oxides thereof, ester waxes such as carnauba wax, montan wax, and deacidified waxes thereof, and fatty acid ester wax, fatty acid amides, fatty acids, higher alcohols, and fatty acid metal salts. These may be used alone or in combination of two or more. The melting point of the release agent is preferably 60° C. or higher, more preferably 70° C. or higher, and even more preferably 75° C. or higher, and is preferably 150° C. or lower, more preferably 130° C. or lower, and even more preferably 100° C. or lower.
[0053] The content of the release agent is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 0.8 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 5 parts by mass or less, relative to 100 parts by mass of the total amount of the binder resin components of the toner.
[0054] <Charge control agent> The toner of the present invention may contain a charge control agent. The charge control agent may contain either a positively chargeable charge control agent or a negatively chargeable charge control agent. Examples of the positively charged charge control agent include nigrosine dyes such as "Nigrosine Base EX", "Oil Black BS", "Oil Black SO", "Bontron (registered trademark) N-01", "Bontron (registered trademark) N-04", "Bontron (registered trademark) N-07", "Bontron (registered trademark) N-09", and "Bontron (registered trademark) N-11" (all manufactured by Orient Chemical Industry Co., Ltd.); triphenylmethane dyes containing a tertiary amine as a side chain, quaternary ammonium salt compounds such as "Bontron (registered trademark) P-51" (manufactured by Orient Chemical Industry Co., Ltd.), cetyltrimethylammonium bromide, and "COPY CHARGE PX Examples of such resins include "VP435" (manufactured by Clariant), polyamine resins such as "AFP-B" (manufactured by Orient Chemical Industry Co., Ltd.), imidazole derivatives such as "PLZ-2001" and "PLZ-8001" (both manufactured by Shikoku Chemical Industry Co., Ltd.), and styrene-acrylic resins such as "FCA-701PT" (manufactured by Fujikura Chemical Industry Co., Ltd.).
[0055] Examples of the negatively chargeable charge control agent include metal-containing azo dyes such as "Varifast (registered trademark) Black 3804", "Bontron (registered trademark) S-31", "Bontron (registered trademark) S-32", "Bontron (registered trademark) S-34", "Bontron (registered trademark) S-36" (all manufactured by Orient Chemical Industry Co., Ltd.), "Aizen Spiron Black TRH", "T-77" (manufactured by Hodogaya Chemical Industry Co., Ltd.), etc.; metal compounds of benzilic acid compounds such as "LR-147" and "LR-297" (all manufactured by Nippon Carlit Co., Ltd.); metal compounds of salicylic acid compounds such as "Bontron (registered trademark) E-81", "Bontron (registered trademark) E-84", "Bontron (registered trademark) E-88", "Bontron (registered trademark) E-304" (all manufactured by Orient Chemical Industry Co., Ltd.), "TN-105" (manufactured by Hodogaya Chemical Industry Co., Ltd.), etc.; copper phthalocyanine dyes; and quaternary ammonium salts such as "COPY CHARGE PX VP434" (Clariant), nitroimidazole derivatives, etc.; organometallic compounds, etc. These charge control agents may be used alone or in combination of two or more kinds.
[0056] The content of the charge control agent is preferably 0.01 parts by mass or more, more preferably 0.2 parts by mass or more, even more preferably 0.5 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, relative to 100 parts by mass of the total amount of the binder resin components of the toner.
[0057] <Other additives> The toner particles may further contain, as other additives, additives such as magnetic powder, a flowability improver, a conductivity adjuster, a reinforcing filler such as a fibrous substance, an antioxidant, an antiaging agent, and a cleaning property improver, as appropriate.
[0058] In the toner of the present invention, the content of toner particles is preferably 80% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and is 100% by mass or less, preferably 99% by mass or less.
[0059] The volume median particle size of toner particles (D 50 ) is preferably 2 μm or more, more preferably 3 μm or more, even more preferably 4 μm or more, and is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less. 50 ) means the particle size at which the cumulative volume frequency calculated by volume fraction is 50% calculated from the smallest particle size.
[0060] <External additives> The toner of the present invention may further contain an external additive in order to improve fluidity. Examples of the external additive include inorganic material particles such as silica, alumina, titania, zirconia, tin oxide, and zinc oxide, and organic particles such as resin particles such as melamine resin particles and polytetrafluoroethylene resin particles. These may be used alone or in combination. Among these external additives, silica is preferred, and hydrophobic silica treated with a hydrophobic treatment agent is more preferred.
[0061] Examples of hydrophobic treatment agents include hexamethyldisilazane (HMDS), dimethyldichlorosilane (DMDS), silicone oil, octyltriethoxysilane (OTES), and methyltriethoxysilane. Among these, hexamethyldisilazane is preferred.
[0062] When the toner particles are surface-treated using an external additive, the content of the external additive in the toner of the present invention is, from the viewpoint of the chargeability and flowability of the toner, preferably 0.05 parts by mass or more, more preferably 0.08 parts by mass or more, even more preferably 0.1 parts by mass or more, and is preferably 5 parts by mass or less, more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, relative to 100 parts by mass of the toner particles.
[0063] [Toner manufacturing method] The toner of the present invention may be a toner obtained by any of the known methods such as a melt kneading method, an emulsion phase inversion method, a suspension polymerization method, an emulsion aggregation method, etc., but from the viewpoints of productivity and dispersibility of the colorant, a pulverized toner obtained by a melt kneading method is preferred. In the melt-kneading method, the binder resin composition, the colorant, and, if necessary, a property improver and the like are uniformly dispersed, and then the mixture is melt-kneaded, cooled, crushed, and classified by a known method to obtain a volume median particle size (D 50 ) A toner having a particle size of 2 μm or more and 20 μm or less can be obtained.
[0064] The toner of the present invention is used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing, etc. The toner can be used as a one-component developer, or mixed with a carrier to form a two-component developer. EXAMPLES
[0065] The properties of the raw materials were measured and evaluated by the following methods.
[0066] [measurement] [Softening point of resin] Using a flow tester "CFT-500D" (Shimadzu Corporation), 1 g of sample was heated at a temperature increase rate of 6°C / min, while applying a load of 1.96 MPa with the plunger, and extruding the sample from a nozzle with a diameter of 1 mm and a length of 1 mm. The plunger descent amount of the flow tester was plotted against the temperature, and the temperature at which half of the sample flowed out was taken as the softening point.
[0067] [Maximum endothermic peak temperature] Using a differential scanning calorimeter "Q-20" (manufactured by TA Instruments Japan, Inc.), the sample was cooled from room temperature (20°C) to 0°C at a rate of 10°C / min, maintained at that temperature for 1 minute, and then heated to 180°C at a rate of 10°C / min while measuring the calorific value. The temperature of the peak with the largest peak area among the observed endothermic peaks was determined as the maximum endothermic peak temperature.
[0068] [Glass transition temperature of resin] Using a differential scanning calorimeter "Q-20" (manufactured by TA Instruments Japan Co., Ltd.), 0.01 to 0.02 g of sample was weighed into an aluminum pan, heated to 200°C, and cooled to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min, and the glass transition temperature was determined as the temperature at the intersection of the extension of the baseline below the maximum endothermic peak temperature and the tangent line showing the maximum slope from the rising part of the peak to the top of the peak.
[0069] [Acid value of resin] The acid value was measured according to the method of JIS K0070:1992, except that the measurement solvent was changed from a mixed solvent of ethanol and ether to a mixed solvent of acetone and toluene [acetone:toluene=1:1 (volume ratio)] in the case of an amorphous polyester resin.
[0070] [Weight average molecular weight (Mw) of polyallylamine and number average molecular weight (Mn) of polyalkyleneimine] The molecular weight distribution was measured by the gel permeation chromatography (GPC) method described below to determine the number average molecular weight and the weight average molecular weight. (1) Preparation of sample solution Polyalkyleneimine or polyallylamine was dissolved in 0.15 mol / L of Na to give a concentration of 0.2 g / 100 mL. 2 SO 4 was dissolved in a 1% by mass aqueous solution of acetic acid. Next, this solution was filtered using a fluororesin filter "FP-200" (manufactured by Sumitomo Electric Industries, Ltd.) with a pore size of 0.2 μm to remove insoluble components, and a sample solution was obtained. (2) Molecular weight measurement The following measuring equipment and analytical column were used, and 0.15 mol / L Na was used as the eluent. 2 SO 4 A solution of 1% by mass of pullulan in acetic acid solution was passed through the column at a flow rate of 1 mL per minute, and the column was stabilized in a thermostatic bath at 40°C. 100 μL of the sample solution was injected into the column and measurements were performed. The molecular weight of the sample was calculated based on a calibration curve that had been prepared in advance. The calibration curve used here included several types of standard pullulan "P-5" (5.9 × 10 3 ), "P-50" (4.73 x 10 4 ), "P-200" (2.12 x 10 5 ), "P-800" (7.08 x 10 5 ) (both manufactured by Showa Denko K.K.) were used as standard samples. The numbers in parentheses indicate the molecular weight. Measuring device: "HLC-8320GPC" (Tosoh Corporation) Analytical column: "α" + "α-M" + "α-M" (manufactured by Tosoh Corporation)
[0071] [Melting point of release agent] Using a differential scanning calorimeter "Q-100" (manufactured by TA Instruments Japan Co., Ltd.), 0.02 g of the sample was weighed into an aluminum pan, heated to 200°C, and then cooled from 200°C to 0°C at a rate of 10°C / min. The sample was then heated at a rate of 10°C / min and the calorific value was measured. The maximum endothermic peak temperature obtained was taken as the melting point.
[0072] [Volume median particle size of toner particles (D 50 )〕 The volume median particle size of toner particles (D50 ) was measured as follows. Measurement device: "Coulter Multisizer (registered trademark) III" (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50μm Analysis software: "Coulter Multisizer (registered trademark) III version 3.51" (Beckman Coulter, Inc.) Electrolyte: "Isoton (registered trademark) II" (manufactured by Beckman Coulter, Inc.) Dispersion: "EMULGEN (registered trademark) 109P" (polyoxyethylene lauryl ether, manufactured by Kao Corporation, HLB (hydrophile-lipophile balance, Griffin method) = 13.6) was dissolved in the electrolyte to obtain a dispersion with a concentration of 5% by mass. Dispersion conditions: 10 mg of the measurement sample was added to 5 mL of the dispersion liquid, and dispersed for 1 minute using an ultrasonic disperser. Then, 25 mL of the electrolyte was added, and further dispersed for 1 minute using an ultrasonic disperser to prepare a sample dispersion liquid. Measurement conditions: In a beaker, the sample dispersion is added to 100 mL of the electrolyte to adjust the concentration so that the particle diameters of 30,000 particles can be measured in 20 seconds. Then, 30,000 particles are measured, and the volume median particle diameter (D 50 ) was sought.
[0073] Resin (A) Manufacturing examples A-1~A-6 The alcohol components shown in Table 1 were placed in a 10-liter four-neck flask equipped with a dehydration tube equipped with a nitrogen inlet tube, a stirrer, and a thermocouple, and the temperature was raised to 100°C, and then terephthalic acid shown in Table 1 was added, the temperature was raised to 160°C, and the esterification catalyst and esterification promoter shown in Table 1 were added, and the temperature was raised to 235°C. After reacting at 235°C for 10 hours, polycondensation reaction was carried out at 235°C and 8.0 kPa for 1 hour. After that, it was cooled to 200°C, trimellitic anhydride shown in Table 1 was added, and polycondensation reaction was carried out at 200°C for 1 hour, and it was cooled to 160°C, and an amine-based polymer compound shown in Table 1 was added. The temperature was raised again to 225°C, and polycondensation reaction was carried out at 225°C for 1 hour, and then reaction was carried out at 225°C and 8.0 kPa until the softening point shown in Table 1 was reached, and amorphous polyester resins A1 to A6 were obtained. Various physical properties were measured and shown in Table 1. The details of the amine polymer compounds shown in Table 1 are as follows. Polyethyleneimine 1200: "Polyethyleneimine 1200" manufactured by Junsei Chemical Co., Ltd. (number average molecular weight 1,200, active content 100% by mass) Polyallylamine PAA-01: Nittobo Medical Co., Ltd. "Polyallylamine PAA-01" (weight average molecular weight 1,600, aqueous solution (active content 15% by mass)) Polyallylamine PAA-08: Nittobo Medical Co., Ltd. "Polyallylamine PAA-80" (weight average molecular weight 8,000, aqueous solution (active content 15% by mass)) Polyallylamine PAA-15C: Nittobo Medical Co., Ltd. "Polyallylamine PAA-15C" (weight average molecular weight 15,000, aqueous solution (active content 15% by mass))
[0074] Manufacturing example A-C1 The alcohol components shown in Table 1 were placed in a 10-liter four-neck flask equipped with a dehydration tube equipped with a nitrogen inlet tube, a stirrer, and a thermocouple, and the temperature was raised to 100 ° C., and then terephthalic acid shown in Table 1 was added, the temperature was raised to 160 ° C., and the esterification catalyst and esterification promoter shown in Table 1 were added, and the temperature was raised to 235 ° C., and polycondensation reaction was carried out at 235 ° C. for 10 hours, and then reaction was carried out at 235 ° C. and 8.0 kPa for 1 hour. The mixture was cooled to 200 ° C., trimellitic anhydride shown in Table 1 was added, and the temperature was raised again to 225 ° C., and polycondensation reaction was carried out at 225 ° C. for 1 hour, and then reaction was carried out at 225 ° C. and 8.0 kPa until the softening point shown in Table 1 was reached, and amorphous polyester resin AC1 was obtained. Various physical properties were measured and shown in Table 1.
[0075] [Table 1]
[0076] [Production of Resin (B)] Manufacturing example B-1 The alcohol components shown in Table 2 were placed in a 10-liter four-neck flask equipped with a dehydration tube equipped with a nitrogen inlet tube, a stirrer, and a thermocouple, and the temperature was raised to 100°C, followed by heating to 160°C with terephthalic acid shown in Table 2, and then adding the esterification catalyst and esterification promoter shown in Table 2, heating to 235°C, and carrying out a polycondensation reaction at 235°C for 10 hours, and further reacting at 235°C and 8.0 kPa until the softening point shown in Table 2 was reached, to obtain amorphous polyester resin B1. Various physical properties were measured and are shown in Table 2.
[0077] [Table 2]
[0078] [Toner manufacturing] Examples 1 to 7 and Comparative Example 1 (Toners 1 to 7, 51) 100 parts by mass of the binder resin composition shown in Table 3, 6 parts by mass of a colorant "Fastgen Super Magenta R" (CI Pigment Red 122, manufactured by Dainippon Ink & Chemicals, Inc.), 1 part by mass of a charge control agent "LR-147" (manufactured by Nippon Carlit Co., Ltd.), and 4 parts by mass of a release agent "Carnauba Wax C1" (manufactured by Kato Yoko Co., Ltd., melting point: 80°C) were thoroughly mixed in a Henschel mixer, and then melt-kneaded using a co-rotating twin-screw extruder having a kneading section with a total length of 1560 mm, a screw diameter of 42 mm, and a barrel inner diameter of 43 mm. The screw rotation speed was 200 r / min, the heating temperature setting in the barrel was 100°C, the mixture was fed at a rate of 10 kg / h, and the average residence time was about 18 seconds. The resulting molten kneaded product was cooled and then pulverized in a jet mill to obtain a volume median particle size (D 50 ) 6.5 μm toner particles were obtained. To 100 parts by mass of the obtained toner particles, 2 parts by mass of hydrophobic silica "Aerosil R-972" (manufactured by Nippon Aerosil Co., Ltd., hydrophobic treatment agent: DMDS, average particle size: 16 nm) was added as an external additive, and the particles were mixed in a Henschel mixer at 3600 r / min for 5 minutes to perform external additive treatment, thereby obtaining toners 1 to 7 and 51.
[0079] [Toner Evaluation] [Minimum fixing temperature] Each toner was loaded onto a color printer "C612dnw" (manufactured by Oki Data Corporation), and an image was printed without being fixed (printing area: 6 cm x 6 cm, adhesion amount: 0.5 mg / cm 2 ) was performed. The fixing roll temperature was then increased by 5°C from 100°C at a rate of 100 mm / sec using the fixing machine of the printer offline, and the unfixed image was fixed at each temperature. Note that J paper (manufactured by Fuji Xerox Co., Ltd., basis weight: 82 g / m) was used as the fixing paper. 2 , paper thickness: 97 μm) was used. A piece of "UNICEF Cellophane" (manufactured by Mitsubishi Pencil Co., Ltd., width: 18 mm, JIS Z1522) was attached to the fixed image, and the image was passed through a fixing roller set at 30°C, after which the tape was peeled off. The optical reflection density before and after the tape was attached was measured using a reflection densitometer "RD-915" (manufactured by Macbeth Co., Ltd.), and the temperature of the fixing roller at which the ratio of the two (optical reflection density after peeling / optical reflection density before attachment x 100) first exceeded 90% was determined as the minimum fixing temperature. The lower the minimum fixing temperature, the better the low-temperature fixing ability. The results are shown in Table 3.
[0080] [Hot offset temperature] Each toner was loaded onto a copier "AR-505" (manufactured by Sharp Corporation) and an image was printed without fixing (print area: 2 cm × 12 cm, adhesion amount: 0.5 mg / cm 2 The fixing paper is Ncolor104 (Fuji Xerox, 104g / m 2 A 125μm thick film was used. The fixing machine of the copier was used offline to fix the unfixed image at 400mm / sec. The temperature was raised from 160°C to 205°C in 5°C increments, and the fixed image obtained was visually inspected. The lowest temperature of the fixing roll at which hot offset was observed was recorded as the hot offset temperature. The higher the hot offset temperature, the better the hot offset resistance. The results are shown in Table 3. Furthermore, the difference between the minimum fixing temperature and the hot offset temperature was calculated as the fixing temperature range. The wider the fixing temperature range, the wider the usable temperature range can be, and the more energy-saving and high-speed fixing requirements can be met. The results are shown in Table 3. [Abrasion resistance] The evaluation paper was "Business4200" (weighing weight 105g / m 2 (manufactured by Xerox Corporation) was used, and the toner loading amount was 0.50 mg / cm 2The solid image was fixed by passing it through a fixing machine whose temperature was adjusted to 180°C. The fixed image was left for one month in an environment of 40°C and 80% relative humidity. The fixed image after leaving was rubbed five times back and forth with a sand eraser with a bottom surface of 15mm x 7.5mm and a load of 500g, and the optical reflection density before and after rubbing was measured using a reflection densitometer "RD-915" (manufactured by Macbeth Co., Ltd.), and the reduction rate (%) of the optical reflection density was calculated from the following formula, and the rub resistance of the fixed image was evaluated according to the following evaluation criteria. The results are shown in Table 3. Reduction rate of optical reflection density (%) = [1-(optical reflection density after rubbing / optical reflection density before rubbing)] x 100 (Evaluation Criteria) A: The decrease in optical reflection density is less than 15%, and no change in the image due to rubbing is observed. B: The decrease in optical reflection density is 15% or more and less than 20%, and some blurring or the like is observed in the image due to rubbing. C: The decrease in optical reflection density is 20% or more and less than 25%, and blurring or the like is observed on the image due to rubbing. D: The decrease in optical reflection density is 25% or more, and image defects due to abrasion are evident.
[0081] [Bending resistance] The toner was installed in a color printer "C612dnw" (manufactured by Oki Data Corporation), and two types of unfixed images were printed (printing area: 4 cm length x 12 cm width (common), adhesion amount: 1.5 mg / cm 2 and 0.7 mg / cm 2 ) was carried out. The unfixed image was fixed offline using the fixing machine of the printer at 150° C. and 200 mm / sec. The fixing paper was J paper (manufactured by Fuji Xerox, basis weight: 82 g / m 2 , paper thickness: 97 μm) was used. The fixed image was folded in half along a 2 cm vertical line, with the fixed image on the inside, and a 1 kg cylindrical weight "M1CSB-1KA" (manufactured by Ikeda Rika Co., Ltd., bottom diameter 5 cm) was moved back and forth twice on the crease, and then the sheet was opened and the crease was observed, and the folding resistance was evaluated according to the following evaluation criteria. The results are shown in Table 3. (Evaluation Criteria) A: 1.5 mg / cm 2 and 0.7 mg / cm 2 No white spots are observed in either image. B: 1.5 mg / cm 2 In the image, one or more white spots are observed, but the 2 This is not observed in the image. C: 0.7 mg / cm 2 One or more white spots are observed in the image. D: 0.7 mg / cm 2 A white line measuring 5mm or more and less than 1cm is observed in the image. E: 0.7 mg / cm 2 A white line measuring 1cm or more and less than 5cm is observed in the image.
[0082] [Table 3]
[0083] As shown in Table 3, the toner of the embodiment containing a specific resin composition has excellent low-temperature fixing property and hot offset resistance, has a wide fixing temperature range, and is excellent in abrasion resistance and bending resistance, compared to the toner of the comparative example.
Claims
1. A method for producing a binder resin composition for toner containing a polyester resin (A) having a softening point of 120° C. or more and 150° C. or less, comprising the following step A: the polyester-based resin (A) is a polycondensate of a raw material monomer (a) containing an amine-based polymer compound and at least one trivalent or higher raw material monomer selected from an alkylene oxide adduct of bisphenol A, an aromatic dicarboxylic acid compound, a trivalent or higher alcohol, and a trivalent or higher carboxylic acid compound; A method for producing a binder resin composition for toner. Step A: A step of polycondensing the alcohol component (a-al) and the carboxylic acid component (a-ac) constituting the polyester resin (A) other than the trivalent or higher raw monomer, adding the trivalent or higher raw monomer to polycondense the mixture, and then adding an amine polymer compound to polycondense the mixture.
2. A method for producing a binder resin composition for toner as described in claim 1, further comprising a step of incorporating an amorphous polyester resin (B), the softening point of which is 80°C or higher and lower than 120°C.
3. A method for producing a binder resin composition for toner according to claim 1 or 2, wherein the amine-based polymer compound contains a repeating unit including an amino group and an alkylene group having 2 to 6 carbon atoms.
4. A method for producing a binder resin composition for toner according to any one of claims 1 to 3, wherein the amine-based polymer compound is polyallylamine.
5. A method for producing a binder resin composition for toner according to claim 4, wherein the weight average molecular weight of the polyallylamine is 800 or more and 30,000 or less.
6. A method for producing a binder resin composition for toner according to any one of claims 1 to 5, wherein the content of the amine-based polymer compound in the raw material monomer (a) is 0.5 mass % or more and 7 mass % or less.
7. A method for producing a toner for electrophotography, comprising a step of melt-kneading the binder resin composition for toner obtained by the method for producing a toner according to any one of claims 1 to 6 and a colorant.
Citation Information
Patent Citations
Electrostatic charge image developing toner
JP1995128903A
Dry toner, and developing device, process cartridge, image forming apparatus, and image forming method using the same
JP2009217183A
Toner for electrostatic charge image development
JP2019174673A
Binder resin composition for toner
JP2020020866A
Binder resin composition for toner
JP2020024360A