Consumer products with bridged carbon nanotube sensors and systems and methods including same - Patents.com
Crosslinked carbon nanotube sensors integrated into consumer products enable high sensitivity and selectivity for gas monitoring and control, addressing the need for efficient gas management in consumer products.
Patent Information
- Application Number
- JP2023528041
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-12-08
- Filing Date
- 2021-12-07
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-12-07
AI Technical Summary
There is a need for gas sensor devices that achieve high sensitivity and selectivity with small dimensions and low power requirements, suitable for integration into consumer products to monitor and control gas levels in spaces.
A system comprising crosslinked carbon nanotube sensors integrated into consumer products, connected to a central communication unit, which can receive and transmit signals to control the operation of these products based on gas concentration, using a crosslinked carbon nanotube network with a conjugated linker system for enhanced sensitivity and selectivity.
The system provides highly sensitive and selective gas detection, allowing for precise control of gas levels in consumer products, enhancing or mitigating target gases through automated operations.
Smart Images

Figure 0007572553000018 
Figure 0007572553000019 
Figure 0007572553000020
Abstract
Description
[Technical field]
[0001] SUMMARY The present disclosure relates to consumer products comprising bridged carbon nanotube sensors, as well as systems and methods including same. [Background technology]
[0002] The mass availability of data is changing the way people live, with great benefits resulting from the ability to monitor gases present in the surrounding environment, both industrially and at home. Thus, there is currently a well-documented need for gas sensor devices that achieve high sensitivity and selectivity, yet have small dimensions, low power requirements, and affordable manufacturing routes.
[0003] Furthermore, people are using data to automate the operation of various consumer products and appliances in their homes and businesses. Thus, there is a need for gas sensor devices that achieve high sensitivity and selectivity to be incorporated into consumer products, systems and methods comprising the same, etc., that can reduce or enhance the levels of target gases in a space. Summary of the Invention [Means for solving the problem]
[0004] combination: A. A system for utilizing a consumer product, comprising: a central communication unit capable of receiving incoming signals and transmitting outgoing instructions, communicatively connected to a memory configured to store an algorithm; a sensor communicatively connectable to a central communication unit and configured to transmit an incoming signal to the central communication unit alerting the central communication unit of an identity and concentration of a target gas of interest, the sensor comprising a crosslinked carbon nanotube network including a plurality of carbon nanotubes and at least one linker covalently linking adjacent carbon nanotubes; and a consumer product capable of enhancing or mitigating a target gas of interest. B. The system of paragraph A, wherein the consumer product is communicatively connectable to a central communication unit via a wireless communication link, and the algorithm controls the consumer product using incoming signals transmitted from the sensor to the central communication unit. C. The system of paragraph A or B, wherein the consumer product is selected from the group consisting of air freshener devices, air purification devices, toothbrushes, razors, diapers, feminine care products, cleaning implements, and combinations thereof. D. The system of any of paragraphs A-C, wherein the plurality of carbon nanotubes are single-walled carbon nanotubes. E. The system of any of paragraphs A-D, wherein the plurality of carbon nanotubes are bonded into a series of parallel layers, and optionally the bridged carbon nanotube has an in-plane electrical conductivity greater than the through-thickness electrical conductivity. F. The linker has the structure * -A- * and A is a bivalent conjugated system comprising one or more aryl or heteroaryl rings; * The system of any of paragraphs A-E, wherein is a point of attachment to the carbon nanotube. GA,
[0005] [ka] and During the ceremony, each ring B is independently an optionally substituted aryl or heteroaryl; Ring C is an optionally substituted porphyrin ring; n is an integer from 1 to 5; * but, Carbon Nanotubes indicates the point of attachment to Optionally, each ring B is independently
[0006] [ka] and / or
[0007] [ka] may be The system of paragraph F, wherein M is Zn, Cu, Ni, or Co, each of which is optionally substituted. H. One or more aryl or heteroaryl rings are C 1 ~C 20 Alkyl, amino (including alkylamino and dialkylamino), carboxylic acid, amino-C 1 ~C 6 Alkyl, C 1 ~C 6 Alkyl-COOH and -NHC(S)(NH 2 ), or a substituent comprising a precious metal nanoparticle, a porphyrin, a calix[4]arene, or a crown ether. I. The linker has the structure:
[0008] [ka] wherein M is Zn, Cu, Ni, or Co. J. Linker, structure * -Y- * wherein Y is a multivalent rigid linker; * The system of any of paragraphs AI, wherein is a point of attachment to a carbon nanotube. The system of paragraph J, wherein the KY comprises a cycloalkyl group or a polyoctahedral silsesquioxane. L. The system of any of paragraphs A-K, wherein the plurality of carbon nanotubes form a film, and the film is provided on a substrate. M. The system of paragraph L, wherein the film has a thickness of about 1 nm to about 500 nm. N. The system of any of paragraphs A-M, wherein the wireless communication link is selected from the group consisting of Wi-Fi, Bluetooth, ZigBee, 6 LoWPAN, Thread, a mesh network, or a combination thereof. O. A consumer product comprising a sensor, the sensor comprising a crosslinked carbon nanotube network comprising a plurality of carbon nanotubes and at least one linker covalently linking adjacent carbon nanotubes. P. The consumer product of paragraph O, wherein the consumer product is selected from the group consisting of air freshener devices, air purification devices, toothbrushes, razors, diapers, feminine care products, cleaning implements, and combinations thereof. Q. The consumer product of paragraph O or paragraph P, wherein the plurality of carbon nanotubes are single-walled carbon nanotubes. R. The consumer product of any of paragraphs O-Q, wherein the plurality of carbon nanotubes are bonded in a series of parallel layers, and optionally the bridged carbon nanotubes have an in-plane conductivity greater than the through-thickness conductivity. S. The linker has the structure * -A- * wherein A is a bivalent conjugated system comprising one or more aryl or heteroaryl rings; * The consumer product of any of paragraphs O-R, wherein is a point of attachment to the carbon nanotube. The TA,
[0009] [ka] and During the ceremony, each ring B is independently an optionally substituted aryl or heteroaryl; Ring C is an optionally substituted porphyrin ring; n is an integer from 1 to 5; * but, Carbon Nanotubes indicates the point of attachment to Optionally, each ring B is independently
[0010] [ka] and / or
[0011] [ka] may be The consumer product of paragraph S, wherein M is Zn, Cu, Ni, or Co, each of which may be optionally substituted. U. One or more aryl or heteroaryl rings are C 1 ~C 20 Alkyl, amino (including alkylamino and dialkylamino), carboxylic acid, amino-C 1 ~C 6 Alkyl, C 1 ~C 6 Alkyl-COOH and -NHC(S)(NH 2 ), or a substituent comprising a precious metal nanoparticle, a porphyrin, a calix[4]arene, or a crown ether. V. The linker has the structure:
[0012] [ka] wherein M is Zn, Cu, Ni, or Co. W. Linker has the structure * -Y- * wherein Y is a multivalent rigid linker; * The consumer product of any of paragraphs O-V, wherein is a point of attachment to the carbon nanotube. The consumer product of paragraph W, wherein XY comprises a cycloalkyl group or a polyoctahedral silsesquioxane. Y. The consumer product of any of paragraphs O-X, wherein the plurality of carbon nanotubes form a film, and the film is provided on a substrate. Z. The consumer product of paragraph Y, wherein the film has a thickness of about 1 nm to about 500 nm. AA. A method of controlling the operation of a consumer product based on an incoming signal from a sensor, the incoming signal identifying a concentration of a target gas, the sensor and the consumer product each communicatively connectable to a central communication unit, the central communication unit communicatively connected to a memory capable of storing a set point, the sensor comprising a crosslinked carbon nanotube network comprising a plurality of carbon nanotubes and at least one linker covalently linking adjacent carbon nanotubes, the linker comprising a conjugated system directly conjugated to the carbon nanotubes, and the method comprising: setting a concentration set point for the target gas in a memory; identifying a target gas using a sensor and measuring a concentration of the target gas; transmitting an incoming signal from the sensor to a central communication unit, the incoming signal including a concentration measurement of the target gas; comparing the concentration measurement to a concentration set point for the target gas; and identifying one or more consumer products for mitigating or enhancing the target gas. BB. The method of paragraph AA, further comprising adjusting operation of the consumer product if the concentration measurement differs from the concentration set point for the target gas. CC. The method of paragraph AA or paragraph BB, wherein the sensors are configured as an array capable of identifying and measuring multiple target gases. DD. The method of any of paragraphs AA-CC, further comprising the step of informing a user about how to use a consumer product that can enhance or mitigate the target gas. EE. A method according to claim 1, wherein a central communication unit communicates with two or more consumer products, the method comprising: setting in the memory a second concentration set point for a second target gas different from the first target gas; identifying a second target gas with a sensor and measuring a concentration of the second target gas; transmitting a second incoming signal from the sensor to a central communication unit, the incoming signal including a second concentration measurement of a second target gas; comparing a second concentration measurement of the target gas to a second concentration set point; The method of any of paragraphs AA-DD, further comprising the step of sending a second outgoing command to the second consumer product to turn on, turn off, or adjust the operation of the second consumer product if the second concentration measurement differs from a second concentration set point for the second target gas. [Brief description of the drawings]
[0013] [Figure 1] 1 shows a system having a central communication unit, a sensor, and a consumer product. [Diagram 2] 1 shows the placement of consumer products and sensors in different rooms than the placement of the CCU (Central Communication Unit). [Diagram 3] 2 shows several possible flows of sensor measurements. [Figure 4(a)] Schematic diagram of (a) reductive dissolution and crosslinking of single-walled carbon nanotubes with conjugated linker precursors, and (b) molecular layer deposition of alternating layers of carbon nanotubes and linkers. [Figure 4(b)] Schematic diagram of (a) reductive dissolution and crosslinking of single-walled carbon nanotubes with conjugated linker precursors, and (b) molecular layer deposition of alternating layers of carbon nanotubes and linkers. [Diagram 5] 1 illustrates an exemplary CCU having a processor and memory disposed within a housing. [Figure 6] 4 illustrates several exemplary flows of incoming signals to a remote memory. [Figure 7] 1 illustrates an exemplary algorithm for incorporating the operation of a consumer product and / or smart device with measurements from sensors. [Figure 8] 1 illustrates an example system having two or more user interfaces. [Figure 9(a)](a) Schematic of the crosslinking and deposition process; (b) digital photograph of the aerogel film deposited on a glass substrate; (c) UV-visible spectrum of the aerogel thin film; (d, e) atomic force microscope height images of the scarred edge of the aerogel film and the corresponding height profile. [Figure 9(b)] (a) Schematic of the crosslinking and deposition process; (b) digital photograph of the aerogel film deposited on a glass substrate; (c) UV-visible spectrum of the aerogel thin film; (d, e) atomic force microscope height images of the scarred edge of the aerogel film and the corresponding height profile. [Figure 9(c)] (a) Schematic of the crosslinking and deposition process; (b) digital photograph of the aerogel film deposited on a glass substrate; (c) UV-visible spectrum of the aerogel thin film; (d, e) atomic force microscope height images of the scarred edge of the aerogel film and the corresponding height profile. [Figure 9(d)] (a) Schematic of the crosslinking and deposition process; (b) digital photograph of the aerogel film deposited on a glass substrate; (c) UV-visible spectrum of the aerogel thin film; (d, e) atomic force microscope height images of the scarred edge of the aerogel film and the corresponding height profile. [Figure 9(e)] (a) Schematic of the crosslinking and deposition process; (b) digital photograph of the aerogel film deposited on a glass substrate; (c) UV-visible spectrum of the aerogel thin film; (d, e) atomic force microscope height images of the scarred edge of the aerogel film and the corresponding height profile. [Figure 10(a)] (a) Statistical Raman spectroscopy and (b) thermogravimetric analysis of monolithic aerogels. [Figure 10(b)] (a) Statistical Raman spectroscopy and (b) thermogravimetric analysis of monolithic aerogels. [Figure 11(a)](a) Full XPS survey of as-received HiPco SWCNT and aerogel thin films, (b) high-resolution scan of SWCNT-aniline, (c) SWCNT-phenyl C1s peak and corresponding peak fitting, (d) high-resolution scan of the N1s peak of the SWCNT-aniline aerogel film, and (e) the I3d peak of SWCNT-phenyl. [Figure 11(b)] (a) Full XPS survey of as-received HiPco SWCNT and aerogel thin films, (b) high-resolution scan of SWCNT-aniline, (c) SWCNT-phenyl C1s peak and corresponding peak fitting, (d) high-resolution scan of the N1s peak of the SWCNT-aniline aerogel film, and (e) the I3d peak of SWCNT-phenyl. [Figure 11(c)] (a) Full XPS survey of as-received HiPco SWCNT and aerogel thin films, (b) high-resolution scan of SWCNT-aniline, (c) SWCNT-phenyl C1s peak and corresponding peak fitting, (d) high-resolution scan of the N1s peak of the SWCNT-aniline aerogel film, and (e) the I3d peak of SWCNT-phenyl. [Figure 11(d)] (a) Full XPS survey of as-received HiPco SWCNT and aerogel thin films, (b) high-resolution scan of SWCNT-aniline, (c) SWCNT-phenyl C1s peak and corresponding peak fitting, (d) high-resolution scan of the N1s peak of the SWCNT-aniline aerogel film, and (e) the I3d peak of SWCNT-phenyl. [Figure 11(e)] (a) Full XPS survey of as-received HiPco SWCNT and aerogel thin films, (b) high-resolution scan of SWCNT-aniline, (c) SWCNT-phenyl C1s peak and corresponding peak fitting, (d) high-resolution scan of the N1s peak of the SWCNT-aniline aerogel film, and (e) the I3d peak of SWCNT-phenyl. [Figure 12(a)] N2 adsorption / desorption isotherms for (a) pristine SWCNT powder and (b-d) crosslinked aerogel monoliths (pore size distribution inset). [Figure 12(b)] N2 adsorption / desorption isotherms for (a) pristine SWCNT powder and (b-d) crosslinked aerogel monoliths (pore size distribution inset). [Figure 12(c)] N2 adsorption / desorption isotherms for (a) pristine SWCNT powder and (b-d) crosslinked aerogel monoliths (pore size distribution inset). [Figure 12(d)] N2 adsorption / desorption isotherms for (a) pristine SWCNT powder and (b-d) crosslinked aerogel monoliths (pore size distribution inset). [Figure 13(c)] Scanning electron microscope images of aerogel films (c) without crosslinking and (d, e) with crosslinking are shown. [Figure 13(d)] Scanning electron microscope images of aerogel films (c) without crosslinking and (d, e) with crosslinking are shown. [Figure 13(e)] Scanning electron microscope images of aerogel films (c) without crosslinking and (d, e) with crosslinking are shown. [Figure 14a)] Helium ion microscope images of SWCNT thin films consisting of a) one layer, b) two layers without crosslinking, and c) two layers with a reductive crosslinking step are shown. [Figure 14b)] Helium ion microscope images of SWCNT thin films consisting of a) one layer, b) two layers without crosslinking, and c) two layers with a reductive crosslinking step are shown. [Figure 14c)] Helium ion microscope images of SWCNT thin films consisting of a) one layer, b) two layers without crosslinking, and c) two layers with a reductive crosslinking step are shown. [Figure 15a)] 1 shows pixel thresholding of a helium ion microscope image. [Figure 15b)] 1 shows pixel thresholding of a helium ion microscope image. [Figure 15c)] 1 shows pixel thresholding of a helium ion microscope image. [Figure 16a)] AFM images and corresponding height profiles of a) monolayer, b) bilayer (non-crosslinked), and c) crosslinked bilayer films are shown. [Figure 16b)]AFM images and corresponding height profiles of a) monolayer, b) bilayer (non-crosslinked), and c) crosslinked bilayer films are shown. [Figure 16c)] AFM images and corresponding height profiles of a) monolayer, b) bilayer (non-crosslinked), and c) crosslinked bilayer films are shown. [Figure 17a)] a) UV-Vis absorption of monolayer and bilayer films, b) multilayer films from 1 to 10 layers, and c) corresponding plots of transmittance versus number of layers. [Figure 17b)] a) UV-Vis absorption of monolayer and bilayer films, b) multilayer films from 1 to 10 layers, and c) corresponding plots of transmittance versus number of layers. [Figure 17c)] a) UV-Vis absorption of monolayer and bilayer films, b) multilayer films from 1 to 10 layers, and c) corresponding plots of transmittance versus number of layers. [Figure 18a)] a) Single point Raman spectrum of a SWCNT film and b) statistical analysis of a 25 point Raman map scan. [Figure 18b)] a) Single point Raman spectrum of a SWCNT film and b) statistical analysis of a 25 point Raman map scan. [Figure 19(a)] Response of crosslinked carbon nanotube networks to different volatile amines: (a) ammonia, (b) DMEA, and (c) TEA, where the shaded areas indicate exposure to the gas analytes. [Figure 19(b)] Response of crosslinked carbon nanotube networks to different volatile amines: (a) ammonia, (b) DMEA, and (c) TEA, where the shaded areas indicate exposure to the gas analytes. [Figure 19(c)] Response of crosslinked carbon nanotube networks to different volatile amines: (a) ammonia, (b) DMEA, and (c) TEA, where the shaded areas indicate exposure to the gas analytes. [Figure 20(a)] (a) Sensor response to high concentrations of AcOH, (b) response to lower concentrations of AcOH, and (c) IVA in the ppb range. [Figure 20(b)](a) Sensor response to high concentrations of AcOH, (b) response to lower concentrations of AcOH, and (c) IVA in the ppb range. [Figure 20(c)] (a) Sensor response to high concentrations of AcOH, (b) response to lower concentrations of AcOH, and (c) IVA in the ppb range. [Figure 21] The dynamic range of resistance change versus concentration for each gas (dynamic range) is shown. [Figure 22] (Left) Schematic of the aniline cross-linked MND film and (right) the linear range and sensing response (inset) of the six-layer film to increasing concentrations of AcOH vapor, with the theoretical limit of detection (LoD) shown. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] Although the consumer products, systems, and methods of the present disclosure will now be described more completely, it should be understood at the outset of the following description that those skilled in the art may modify the methods and systems described herein while still achieving the preferred results described in this disclosure. Thus, the following description is a broad teaching disclosure aimed at those skilled in the art, and should not be understood as limiting the present disclosure.
[0015] The systems, methods, and devices of the present invention comprise highly selective and sensitive sensors. The sensors may be used to detect the presence of a target gas. The target gas may be an undesirable gas that a user may wish to mitigate by either masking, removing, or reducing the presence of one or more consumer products, such as an air freshener device or an air cleaning device. The target gas may be a desirable gas, such as a volatile fragrance ingredient, that a user wishes to enhance or increase the presence of a consumer product, such as an air freshener device. The sensor may be integral with the consumer product, or may exist as a separate component that wirelessly communicates with a controller, a user or a user interface, and / or a consumer product.
[0016] The consumer product may be a smart consumer product that can communicate with the CCU or directly with the sensors. The consumer product may also require user intervention when the sensors inform the user that a condition has been met.
[0017] The systems and methods may include a central communication unit (CCU) communicatively connectable to one or more consumer products 104 and / or one or more sensors. The CCU may be in the form of a smartphone, computer, tablet, thermostat, etc. FIGURE 1 illustrates an exemplary, non-limiting system 100 including a central communication unit 102, one or more consumer products 104, and one or more sensors 106, each in communication with the CCU 102 via a wireless communication link 107.
[0018] For example, the sensor 106 may send an incoming signal to the CCU 102. In response to the incoming signal from the sensor 106, the CCU may send an outgoing command to the consumer product 104 to turn the consumer product on or off or adjust the operation of the consumer product. For example, if the sensor 106 sends an incoming signal to the CCU regarding the presence and concentration of a particular target gas, and the CCU compares the value of the incoming signal regarding the target gas to a set point for that particular target gas, the CCU may send an outgoing command to the consumer product 104 to reduce or increase the level of that particular target gas depending on whether the value of the incoming signal is higher or lower than the set point for the target gas.
[0019] As discussed in more detail below, the CCU may include a memory capable of storing set points and algorithms, and a processor capable of executing the algorithms and accessing the stored set points from the memory. Various algorithms may be programmed depending on the desired results.
[0020] The sensors and consumer products may be located anywhere inside or outside the building. The sensors and consumer products may be located in the same room as other components of the system, or the components of the system may be located in one or more different rooms. With reference to FIG. 2, in a non-limiting illustrative example, the consumer product 104 may be located in the same room as the sensor 106, or in a different location than the CCU 102. The consumer product 104 and / or the sensor 106 may be movable to different rooms depending on the user's convenience. The system may include multiple sensors positioned at various locations or rooms within the building. The system may also include multiple consumer products.
[0021] The system may also include additional smart devices 109 located in the building, such as appliances (refrigerators, washers, dryers, stoves, microwaves), fans, lights, electrical outlets, switches, televisions, HVAC systems, speakers, security systems, baby monitors, garage door openers, doorbells, cameras, wearables such as smart watches or baby sleep monitors.
[0022] Sensors The system 100 may include a sensor 106. The sensor 106 may be configured to measure the presence and concentration of a target gas of interest. A target gas of interest may be an undesirable target gas that a user may wish to reduce, or a target gas of interest may be a desirable one that a user may wish to enhance or maintain at a desired concentration. It may be desirable to be able to detect undesirable target gases and distinguish them from desirable target gases. Target gases of interest may include amines such as trimethylamine (e.g., from urine, fish odors), aldehydes / ketones such as 2-nonenal, nonanal, octanal, formaldehyde, 1-octen-3-one, and 3-octanone (e.g., from fragrance ingredients), acids such as acetic acid, isovaleric acid, and myristic acid (e.g., from body odor, tobacco / cigar smoke, bacon grease, and pet odors), alcohols such as 1-dodecanal, 1-octanol, 1-octyldodecyl ... 1-phenyl-3-ol, 3-methyl-1-butanol, and 2-methylisoborneol (e.g., from mold / powdery mildew), sulfur, e.g., dimethyl disulfide (e.g., from garbage, bathrooms, pets), aromatic hydrocarbons, e.g., benzene, naphthalene, and geosmin (e.g., from tobacco / cigar smoke and bacon grease), alkenes, e.g., 1-pentadecene, lactones, e.g., 5-H-furan-2-one, undecalactone, NO 2 The desired target gases may include harmful air quality gases such as aldehydes, ketones, esters, alcohols, etc. The desired target gases of interest may be used as markers to measure the concentration of the fragrance mixture in the air, i.e., measurements of the target gases of interest may be used to calculate the total concentration of the fragrance mixture in the air.
[0023] The system may also be equipped with sensors that measure temperature, relative humidity, indoor air quality, outdoor air quality, noise, human presence, movement, indoor air velocity, airborne particle concentrations, allergens, and / or other airborne substances that affect human health.
[0024] It has been shown that by combining data from any and / or all of these sensor sources, as well as target gas sensors or arrays of target gas sensors (multiple sensors each detecting a unique target gas), a more accurate prediction of the composition of the air can be made. For example, by detecting human movement and listening to the sound of cooking on the stove along with rising temperature / humidity, a stored knowledge-based algorithm along with unique target gas sensing and particle sensing can accurately predict when a person is cooking and what odors or chemicals are in the air associated with cooking. This sensor data can then give the user more accurate information or suggestions on how to manage a particular odor or air quality event. In another non-limiting example, detecting higher airflow indoors and outdoor sounds combined with target gas and particulate sensing can determine that a window is open and a particular event is occurring (e.g., forest fire smoke) or that unique outdoor pollution is entering the indoor space.
[0025] Particular sounds of interest that may be recognized by the sensor include, but are not limited to, cooking on a stove, oven, or microwave, pets (e.g., barking), flushing a toilet, street noise (e.g., cars / traffic), presence and number of people, doors opening and closing, fan operation, television or radio, HVAC operation. In particular, humans have the ability to recognize the presence of a person or what they are saying, but algorithms can be designed to protect privacy by not actually using voice recognition or recording what a person is saying. This can be done by monitoring the type of sound but not monitoring or deciphering what is being said.
[0026] In another example, airflow sensing can be used to determine if a window is open, a door is open, a ceiling fan is running, or to determine when an HVAC unit or room air circulation fan is running. Additionally, data about outdoor air quality for a home or location, such as data available from companies like Breezometer, can be leveraged to predict the outdoor air quality, pollen levels, temperature, and humidity of the air outside any particular home or business.
[0027] When these different sources of sensor data (e.g., noise, airflow, air quality) are combined with the target gas sensor, a more informed recommendation can be made to the consumer or another device for any corrective actions needed. Non-limiting examples of corrective actions could be for the consumer to turn on the kitchen vent, turn on the air cleaner, change the air cleaner or HVAC filter, open a window, turn on the fan / HVAC, spray an air freshener, or any number of actions based on the various sensor data from all these sources, and combinations thereof. The sensor 106 may include a wireless communication module so as to be communicatively connectable with the CCU and / or various components of the system through wireless communication links.
[0028] The sensor 106 may be powered by a power source. The sensor 106 may be powered independently of the consumer product or through the same power source of the consumer product. The sensor 106 may be powered independently. The sensor may be battery powered or may be powered via an electrical outlet.
[0029] The sensors may be configured to transmit sensor measurements in the form of incoming signals to the CCU. The sensor measurements can be used in a variety of ways. For example, the sensor measurements can be viewed as raw data and compared to set points, such as target gas concentration set points for controlling air treatment devices, or can be stored in a database for further analysis to recommend optimal set points taking into account comfort and energy efficiency.
[0030] 3 illustrates several possible flows of signals from components to the CCU. Sensor measurements can flow from components through the CCU to a user interface for raw local sensor measurements. Sensor measurements may also pass from the sensors through the CCU to a destination server on the Internet where they are stored in memory or analyzed by a processor for sending instructions to various components, including but not limited to the consumer product 104 and / or smart devices. Sensor measurements may also pass from the sensors through the CCU to the consumer product 104.
[0031] The sensor may be configured in a variety of different ways. The sensor may be a standalone device or unit that is movable throughout space. The sensor may be integrated into another device, such as a consumer product or a smart device.
[0032] Reductive dissolution is sp 2This provides a route to highly individualized carbon nanotube solutions with high mass loadings without damaging the π-system. (Clancy, AJ et al. Charged Carbon Nanomaterials: Redox Chemistry of Fullerenes, Carbon Nanotubes, and Graphenes. Chem. Rev. 118, 7363-7408 (2018), the entire contents of which are incorporated herein by reference). Such solutions can be grafted with, for example, alkyl and aryl halides, allowing for efficient attachment of binding sites. For example, biaryl halides may be utilized to crosslink adjacent carbon nanotubes, resulting in free-standing three-dimensional networks exhibiting high specific surface areas with well-defined pore structures (Figure 4).
[0033] As described herein, crosslinking chemistry was adapted to achieve crosslinked carbon nanotube aerogel thin films. The thin aerogel structure provides a sensor material with a large active surface area with rapid access to the available porosity. Through this strategy, lower limits of detection for both gases (such as volatile acids and amines) were demonstrated.
[0034] Thin film aerogel structures are hypothesized to be ideally suited for gas sensing applications due to their high surface area and accessible porosity.
[0035] Additional enhancements can be imparted through surface functionalization. The reported unique structures may be further applied to the specific sensing of other gas molecules through deliberate surface modification.
[0036] Accordingly, the present invention provides a process for preparing a cross-linked carbon nanotube network, comprising: Providing a plurality of reduced carbon nanotubes; reacting the reduced carbon nanotubes with a conjugated linker precursor to covalently form a crosslinked carbon nanotube network comprising carbon nanotubes covalently linked by a linker formed from the conjugated linker precursor, the linker comprising a conjugated system directly bonded to the carbon nanotube to which it is covalently linked.
[0037] Methods for preparing reduced carbon nanotubes are known to those skilled in the art, for example, methods are described in Clancy, AJ et al. Charged Carbon Nanomaterials: Redox Chemistry of Fullerenes, Carbon Nanotubes, and Graphenes. Chem. Rev. 118, 7363-7408 (2018).
[0038] Reduced carbon nanotubes can be prepared by treating parent carbon nanotubes with a reducing agent.
[0039] The reducing agent may include a Group I or Group II metal. Group I metals (alkali metals) may be used to prepare reduced carbon nanotubes. The alkali metals may include lithium, sodium, potassium or alloys thereof. The carbon nanotubes react to form reducing species with associated counterions. The metals may be introduced as vapor, molten metal, amalgam, eutectic alloy or plasma. Group II metals (alkaline earth metals) may also be used.
[0040] Solvation reduction may also be used, i.e., the carbon nanotubes may be treated with a reducing agent in the presence of a solvent, for example, an alkali metal may be dissolved in liquid ammonia for the Birch reduction.
[0041] The reducing agent may further include a charge transfer agent. The charge transfer agent is an agent that supports electride formation. The charge transfer agent may include an aromatic. Examples of such charge transfer agents are naphthalene, anthracene, phenanthrene, 4,4'-di-tert-butylbiphenyl, azulene, or combinations thereof. Preferably, the charge transfer agent is naphthalene.
[0042] The solvent used for the reduction may preferably be aprotic, such as an ether, amide or amine solvent, or a mixture thereof. The ether may include an alkyl or cycloalkyl ether. Exemplary ethers include tetrahydrofuran (THF), dioxane, diethyl ether, diisopropyl ether, di-n-butyl ether, di-sec-butyl ether, methyl t-butyl ether, 1,2-dimethoxyethane, 1,2-dimethoxypropane, 1,3-dimethoxypropane, 1,2-diethoxyethane, 1,2-diethoxypropane, 12-crown-4 ether, 15-crown-5 ether, 18-crown-6 ether, or a combination thereof. Amine solvents may be used and may include tertiary amines. Useful amines may include tertiary alkyl or cycloalkyl amines. Exemplary amines include tertiary amines including n-methylpiperidine, n-methylmorpholine, N,N,N',N'-tetramethyl-1,2-diaminoethane, or a combination thereof. Amide solvents may be used. Exemplary amides include dimethylformamide, N-methyl-2-pyrrolidone, and N,N-dimethylacetamide. The amide solvent should preferably be inert to alkali metals. The solvent should also be stable in the presence of both the charge transfer agent and the reduced carbon nanotubes (formed by treatment with a reducing agent). Preferred amide-based solvents include N,N-dimethylacetamide.
[0043] Organometallics (e.g., n-BuLi and C 3 H 7NHLi) may be used to reduce carbon nanotubes and simultaneously functionalize them with organic groups to allow for the attachment of different surface moieties. The reducing agent may therefore be an organometallic, preferably an alkali metal organometallic, as defined herein.
[0044] The reduction of the carbon nanotubes can alternatively be carried out electrochemically, which has the advantage of simultaneously reducing the carbon nanotubes and dissolving the reduced carbon nanotubes if a suitable solvent (e.g., N,N-dimethylformamide, DMF) is used.
[0045] Preferably, the reduced carbon nanotubes are provided in a solution. Preferably, the solvent is a polar aprotic solvent as described above. Suitable solvents include N-N-dimethylacetamide, N,N-dimethylformamide (DMF), N-cyclohexyl-2-pyrrolidone (CHP), N-methylpyrrolidone (NMP), dimethylsulfoxide (DMSO) and dimethylacetamide (DMAc). Simultaneous reduction and dissolution of the carbon nanotubes, i.e., reductive dissolution, can be advantageous. Reductive dissolution is the preferred method for producing films of crosslinked nanotubes, since the electrical properties of the nanotubes are preserved during the process. See FIG. 4(a). Reductive dissolution can achieve high reduced carbon nanotube concentrations while retaining outstanding properties.
[0046] N-N-dimethylacetamide is a preferred solvent, especially in the case of reductive dissolution, since it can stabilize the reduced carbon nanotubes.
[0047] The term carbon nanotubes according to the present invention refers to substantially sp 2Carbon nanotubes refer to nanoscale tubes made of bonded carbon atoms and have a structure based on the graphite basal plane that is wrapped or curled into a tube. Carbon nanotubes can be any type of nanotube, i.e., any hollow tubular structure that has at least one dimensional measurement on the nanometer scale.
[0048] The carbon nanotubes may be single-walled carbon nanotubes (SWCNTs), double-walled carbon nanotubes or multi-walled carbon nanotubes (MWCNTs) having three or more walls, preferably SWCNTs or double-walled carbon nanotubes. Preferably, the carbon nanotubes are SWCNTs, and thus the reduced carbon nanotube species are nanotubes (SWCNTs). n- ).
[0049] Carbon nanotubes used in the nanotubes of the present invention may have a minimum inner diameter measurement of about 0.5 nm to about 50 nm, e.g., about 0.5 nm to about 20 nm, about 0.7 nm to about 10 nm, e.g., about 0.8 nm to about 2 nm. Small diameter carbon nanotubes are defined herein as carbon nanotubes having a diameter of at most about 3 nm, regardless of the number of walls. Nanotubes may be of any length. For example, nanotubes may have a length of about 5 nm to about 500 μm, preferably about 10 nm to about 100,000 nm, preferably about 100 nm to about 10,000 nm. Preferably, greater than 75% by weight of the nanotubes in the networks prepared herein have dimensions in the ranges described immediately above.
[0050] The dimensions of the carbon nanotubes may be determined by microscopy (e.g., atomic force microscopy (AFM) or transmission electron microscopy (TEM) or spectroscopy, e.g., Raman spectroscopy or absorbance / fluorescence spectroscopy). The carbon nanotubes may be dispersed in any suitable manner that does not affect the distribution measured. For example, reductive dissolution may be used. Once dissolved and deposited on a substrate (e.g., a silicon wafer), the length distribution may be confirmed by imaging the sample with AFM and directly measuring the length of the imaged CNTs. Similarly, the diameter distribution may be measured by imaging the sample with TEM and determining the diameter of the species present. The diameters may be measured by AFM (using height measurements), by Raman spectroscopy (via the so-called "breathing mode" frequency) or inferred from absorbance / fluorescence spectroscopy in the visible / near infrared range.
[0051] The reduced carbon nanotubes are reacted with a conjugated linker precursor to form a covalently crosslinked carbon nanotube network. The carbon nanotube network comprises carbon nanotubes covalently linked to one another by a linker formed from the conjugated linker precursor. The linker comprises a conjugated system directly bonded to the carbon nanotube. The linker is directly bonded to the carbon nanotube such that there is no unconjugated portion between the linker and the carbon nanotube. Thus, the two conjugated systems (the linker and the carbon nanotube covalently bonded thereto) are directly adjacent.
[0052] The conjugated linker precursor contains at least two functional groups capable of reacting with the walls of a reduced carbon nanotube to form a C-C covalent bond, thus forming a covalently crosslinked network. Preferably, the at least two functional groups are located on different atoms of the linker molecule, and more preferably some distance apart, to maximize the opportunity to react with two different nanotubes.
[0053] As will be appreciated, the conjugated linker precursor reacts with the reduced carbon nanotube to form a linker without functional groups. The linker is directly bonded to the carbon nanotube via a C-C bond to form a contiguous conjugated system with the carbon nanotube to which the linker is covalently bonded. Thus, the linker is a multivalent moiety.
[0054] In a direct bond, there is no intervening moiety. For example, a conjugated linker precursor reacts with a reduced carbon nanotube to form a direct C-C bond with no intervening moiety.
[0055] The functional group may be a suitable leaving group that allows the linker precursor to react directly with the sidewall of a reduced nanotube, for example, by electrophilic substitution as shown in Scheme 1.
[0056] Scheme 1: Reaction between reduced carbon nanotubes and conjugated linker precursors (R-Br) to form covalently functionalized carbon nanotubes.
[0057] [ka]
[0058] Direct attachment of conjugated linkers to the nanotube sidewalls is particularly suitable for creating conjugated networks that aid in electrical conductivity. The linker is conjugated such that when it is directly attached to a nanotube, two conjugated systems are adjacent, so that some degree of conjugation can be maintained between adjacent nanotubes.
[0059] The conjugated linker precursor (and thus the linker) comprises a continuous conjugation between each of the functional groups. The conjugated linker precursor may comprise non-conjugated substituents around the continuous conjugation between each of the functional groups. Preferably, the conjugated linker precursor is entirely conjugated between each of the functional groups.
[0060] The linker is a polyvalent (e.g., divalent) conjugated system, e.g., containing one or more optionally substituted aryl or heteroaryl rings. The one or more aryl or heteroaryl rings may be directly bonded to each other or may be bonded to a trivalent sp 2 The bond may be via a carbon group.
[0061] The conjugated linker precursor has the structure: X-A'-X may be a compound of wherein A' is a divalent conjugated system and each X is independently a suitable leaving group. X may comprise a halide, sulfoxide, or tosylate. Alternatively, X may be a peroxide or disulfide moiety.
[0062] The conjugated linker precursor has the structure: XAX may be a compound of wherein A is a divalent conjugated system containing one or more aryl or heteroaryl rings, A is optionally substituted, and each X is independently a suitable leaving group. X may include a halide, sulfoxide, or tosylate.
[0063] A may contain two or more aryl or heteroaryl rings, each of which may be directly bonded to each other or may be trivalent sp 2 The bond may be via a carbon group (eg, methine).
[0064] A is a ring having one or more aryl or heteroaryl rings and an optional triple valency sp 2 It may consist essentially of carbon groups and any optional substituents present on the one or more aryl or heteroaryl rings.
[0065] A is a conjugated moiety that includes one or more aryl or heteroaryl rings. A has the structure:
[0066] [ka] and wherein each ring B is independently an optionally substituted aryl or heteroaryl; and n is an integer from 1 to 5; * indicates the point of attachment to each X.
[0067] A may include a porphyrin ring. For example, A may have the structure:
[0068] [ka] and During the ceremony, each ring B is independently an optionally substituted aryl or heteroaryl; Ring C is an optionally substituted porphyrin ring; n is an integer from 1 to 5; * indicates the point of attachment to each X.
[0069] As will be appreciated, the conjugated linker precursor reacts with the sidewalls of the reduced nanotubes to bridge adjacent nanotubes, and the nanotubes have the structure * -A- * (In the formula, * are attached by a conjugated linker having a leaving group X (which indicates the point of attachment to each nanotube, i.e., to the linker precursor structure) absent.
[0070] The linker portion of the conjugated linker precursor (e.g., group A) may be substituted. It is not necessary that such substitutions are conjugated. If the network is used in gas sensing applications, the substituents can be adjusted according to the target gas. The substituents can be selected to adjust the binding affinity to the target gas.
[0071] For example, amino substituents may increase binding affinity for volatile acidic gases. Substituents containing carboxylic acid groups may increase binding to amines. Thiourea groups may increase binding of ketones. Noble metal nanoparticles may improve hydrogen sensing. Metallated porphyrin substituents may increase binding to CO or amines. Calix[4]arenes may be used for the selective detection of aromatic and chlorinated hydrocarbons. Long alkyl chains (e.g., C 1 ~C 20 Alkyl) may be used to increase the adsorption of aliphatic hydrocarbons. Crown ether groups may be used to enhance the binding of alcohols through hydrogen bonding basicity.
[0072] Possible substituents include C 1 ~C 20 Alkyl, amino (including alkylamino and dialkylamino), carboxylic acid, amino-C 1 ~C 6 Alkyl, C 1 ~C 6 Alkyl-COOH and -NHC(S)(NH 2 ), or substituents including noble metal nanoparticles, porphyrins, calix[4]arenes, or crown ethers.
[0073] Substituents that provide additional functional groups capable of reacting with the surface of the reduced carbon nanotubes, such as suitable leaving groups, may also be used.
[0074] The group A, which contains one or more aryl or heteroaryl rings, may be optionally substituted. A may be optionally substituted with a substituent as defined herein, including one or more suitable leaving groups, such as a halide.
[0075] As will be appreciated, when the conjugated linker precursor (e.g., A) is optionally substituted with one or more suitable leaving groups (such as halides), the suitable leaving group substituents may function as functional groups capable of reacting with the surface of the reduced carbon nanotubes.
[0076] The conjugated linker precursor may have three or more functional groups capable of reacting with the surface of the reduced carbon nanotube. For example, the conjugated linker precursor may have the structure: A-(-X) m may be a compound of wherein A and X are as defined herein, and m is an integer of 2 or greater, e.g., 3 or 4.
[0077] A combination of conjugated linker precursors may be used in the process of the invention.
[0078] Linkers in crosslinked carbon nanotube networks can provide, for example, increased sensitivity to target gas analytes when the networks are used in gas sensing applications. Selection of the linker structure and substitutions on the linker allows for tuning of binding affinities for different gases.
[0079] Varying the linking moieties can significantly affect the resulting film morphology, allowing for tuning of properties. Additionally, the crosslinking reaction provides a useful route to incorporate additional functional groups into the crosslinked carbon nanotube network.
[0080] The crosslinking reaction between the reduced carbon nanotubes and the conjugated linker precursor can be carried out in solution, for example, a polar aprotic solvent such as that used to dissolve the reduced carbon nanotubes.
[0081] The crosslinking process may be carried out at any reasonable temperature and left for any length of time required to complete the reaction, so long as the reaction is carried out at a temperature below the boiling point of the reaction solvent, for example. The reaction is carried out at a temperature between 10° C. and 60° C., preferably between 15° C. and 30° C. The reaction time is preferably between 0.1 hours and 50 hours or more.
[0082] During the course of the reaction, the carbon nanotubes crosslink to form a gel phase. "Gel" refers to a composition that retains its shape during a drying process and is known to those skilled in the art. The gel phase is formed by a continuous network of covalently bonded nanotubes in a solvent.
[0083] By carrying out the covalent cross-linking process in the gel phase, the resulting carbon nanotubes are able to retain their structural integrity during removal of the solvent. The cross-linking reaction can be advantageously carried out in a saturated solvent environment to avoid solvent evaporation, which can result in capillary collapse of the microporous structure and a reduction in the available surface area.
[0084] The process may further include depositing a cross-linked carbon nanotube network on a surface of the substrate.
[0085] Reacting the cross-linking reaction may include contacting a plurality of reduced carbon nanotubes with a conjugated linker precursor in a single step.
[0086] Alternatively, the cross-linking reaction may involve two or more steps, in which the reduced carbon nanotubes are contacted with a conjugated linker precursor, followed by contact with additional reduced carbon nanotubes to form a cross-linked carbon nanotube network. Providing a substrate; depositing reduced carbon nanotubes on a surface of a substrate; contacting the reduced carbon nanotubes with a conjugated linker precursor to form a covalently functionalized carbon nanotube; The method may include a layer-by-layer deposition process comprising: contacting the covalently functionalized carbon nanotubes with additional reduced carbon nanotubes to covalently form a cross-linked carbon nanotube network comprising carbon nanotubes covalently linked by linkers formed from conjugated linker precursors, the linkers comprising a conjugated system directly bonded to the carbon nanotubes.
[0087] Each contacting step may be repeated to build up a three-dimensional cross-linked carbon nanotube network. The method may further include reacting the crosslinked carbon nanotube network with additional conjugated linker precursors and then reacting the resulting material with additional reduced carbon nanotubes.
[0088] A layer-by-layer deposition (also described as molecular layer deposition) process for single-walled carbon nanotubes (SWCNTs) is shown in Figure 4(b). A first SWCNT layer is deposited (e.g., by spin coating) of nanotubes onto a substrate (e.g., silanized glass). This charged layer is then immersed in a bath of linker precursor, monofunctionalizing the available surface until the surface charge is depleted. This results in the formation of covalently functionalized carbon nanotubes. Residual leaving group moieties (e.g., halides) are available on the covalently functionalized carbon nanotubes for grafting to the next SWCNT layer. The yield from monografted linkers to bigrafted linkers is speculated to be high due to the very high concentration of crosslinker molecules, which allows for a fast reaction rate for the first grafting. The deposited SWCNTs may be advantageously anchored to the substrate as a result of covalent interactions due to the functionalization of the substrate (e.g., an iodopropylsilane layer). This steric restriction may help ensure that the linker precursor does not crosslink SWCNTs within the same layer. Following deposition of a layer of mono-grafted linker, excess reagent can be removed by immersion in a suitable solvent (such as DMAc) before the next layer of SWCNTs is added. The charged nanotubes in solution react with residual leaving groups remaining from the linker precursor. This reaction forms a second, separate layer of SWCNTs, which are covalently attached to the previous SWCNT layer by the linker. SWCNTs are deposited until the leaving groups are exhausted, limiting the deposition to a single layer. The cycle is repeated for the addition of each subsequent crosslinked layer, depositing a film with controllable thickness and transparency.
[0089] By using a molecular layer deposition process, a layer-by-layer structure can be created in the crosslinked carbon nanotube network such that the carbon nanotube bonds (i.e., crosslinkers) are connected in a series of parallel layers. Molecular layer deposition allows a high level of control over the thickness and transparency of the resulting crosslinked carbon nanotube network film, as observed by AFM and UV-Vis spectroscopy. The crosslinked carbon nanotube network can be described as an anisotropic network (organized in layers), unlike any previously known process. It allows a large number of molecular bonds to be linked in parallel. If these bonds "switch on" in the presence of analyte, high sensitivity is expected. If they "switch off" in the presence of analyte, additional layers provide sensitivity. The ability to adjust the balance of serial and parallel molecular bonds (and any of the probes) is an advantage of the present invention.
[0090] In an alternative embodiment, a conjugated crosslinker precursor may be deposited on the surface of a substrate and a crosslinked carbon nanotube network may be constructed therefrom.
[0091] The cross-linked carbon nanotube network is deposited on a substrate. The deposition can be carried out, for example, by drop casting or spin coating. The deposition can be carried out for any amount of time required. By carrying out the cross-linking reaction in the presence of the substrate, the cross-linked carbon nanotube network may be deposited as it is formed. Thus, the deposition can occur simultaneously with the cross-linking reaction.
[0092] Preferably, the deposition occurs during the cross-linking reaction such that the bridged carbon nanotubes are formed on the surface of the substrate. This can be accomplished by carrying out the cross-linking reaction in the presence of the substrate, which allows the formation of a homogenous film.
[0093] Advantageously, the layer-by-layer deposition process allows for the in-situ formation of a cross-linked carbon nanotube network on the surface of a substrate forming a homogeneous film in a highly controlled manner.
[0094] Any suitable substrate may be used. The substrate may be an inert substrate. For example, the substrate may be a glass substrate. The substrate may be a silicon wafer or a non-conductive metal oxide substrate, such as an alumina substrate.
[0095] The substrate is preferably a non-conductive substrate.
[0096] However, it is also possible to use top-to-bottom transport measurements, where the aerogel is deposited on a metal contact (e.g., a metal substrate or a conducting oxide such as indium tin oxide). Such conducting substrates may be particularly suitable for multilayer structures, where measurements through the thickness use intended parallel mode coupling. In this case, source and drain electrodes are positioned at the top and bottom of the thin film, allowing through-layer transport to be measured.
[0097] The substrate may be functionalized prior to deposition, for example to aid in wetting of the substrate by the cross-linked carbon nanotube network. Substrate functionalization may also aid in the homogeneity of the deposited cross-linked carbon nanotube network. The substrate may be functionalized, i.e. silanized, with a silane material. Suitable silane materials include halo-alkoxysilanes or (3-aminopropyl)triethoxysilane (APTES). Preferably, the silane material is a halo-alkoxysilane, such as 3-iodopropoxysilane or (3-bromopropyl)trimethoxysilane. Alternatively, functionalization may be performed with a thiol.
[0098] The substrate may be saturated with the reduced carbon nanotubes prior to deposition to aid wetting. For example, the process may include an initial step prior to deposition in which the substrate is contacted with the reduced carbon nanotubes for a suitable time to ensure adsorption of the reduced carbon nanotubes to the substrate, either directly or via functionalization on the substrate surface. Alternatively, the substrate may be saturated with a crosslinker precursor. This is particularly advantageous when a layer-by-layer deposition process is used.
[0099] The processes described herein may be carried out under any suitable conditions. For example, the processes may be carried out under inert conditions, such as under argon gas.
[0100] The processes described herein may be used to form films for a variety of potential applications ranging from photovoltaic devices, sensors and catalysts to conductive inks and coatings.
[0101] Also provided herein is a bridged carbon nanotube network prepared by the process of the present invention. a plurality of carbon nanotubes as described herein; and at least one linker as described herein that covalently links adjacent carbon nanotubes, the linker comprising a conjugated system directly bonded to the carbon nanotube.
[0102] The bridged carbon nanotube networks provided herein have a high degree of individualization achieved by reduction chemistry, providing a large available surface area for adsorption. This is in contrast to other methods reported to result in bundled networks. The crosslinking reaction provides a defined open pore structure, allowing diffusion through the open network. The pore structure can be tailored by altering the structure of the linker.
[0103] The surface area of the bridged carbon nanotube network may be measured by the BET method. Ideally, the bridged carbon nanotube network is formed in a bulk monolithic form to measure the surface area. The process described herein allows for the provision of bulk monolithic networks in addition to thin film forms. Surface area may also be measured electrochemically from capacitance measurements.
[0104] The bridged carbon nanotube network is approximately 500 Sm -1 More than 600Sm, preferably about 600Sm -1 More than 700 Sm, preferably about 700 Sm -1 More than 800 Sm, preferably about 800 Sm -1 More than 900Sm, preferably about 900Sm -1 More than 1000 Sm, preferably about 1000 Sm -1 The electrical conductivity may be up to about 1,000,000 Sm -1 may be also possible.
[0105] The electrical conductivity of the bridged carbon nanotube network can be anisotropic.
[0106] The bridged carbon nanotube networks prepared by the molecular layer deposition process described herein have electrical conductivities of approximately 10 Sm -1 It may be more than that.
[0107] Conductivity may be determined by measuring the film resistance using a four-point probe. In this method, the film may be contacted with four wires and a current applied to the outer two wires. The voltage drop between the two inner wires is then measured and used to determine the sheet resistance. Conductivity can then be calculated from the sheet resistance.
[0108] As will be appreciated, greater electrical conductivity can be achieved by using longer carbon nanotubes, aligning CNTs, and chemical doping. An important electrical feature of the crosslinked carbon nanotube network film is the presence of molecular elements, i.e., linker groups, at the carbon nanotube-to-carbon nanotube junctions that modulate electrical transport upon exposure to different analytes. In sensor applications, modulation can be important. Higher baseline electrical conductivity can help provide cheaper electronics. The crosslinked carbon nanotube network films described herein provide high sensitivity and high selectivity. This can be achieved by having selective binding sites at the junctions that aid in electron transport through the network.
[0109] This can be described as tying together a large number of molecular bonds. In molecular electronics, molecular bonds are intriguing but difficult to measure. A practical method for measuring large numbers of molecular bonds is described herein.
[0110] The physical properties of the crosslinked carbon nanotube networks described herein can be distinct from other thin films in the degree of individualization of carbon species and fine filament structure. The prominent van Hove bands (distinct peaks / bumps) in UV-Vis indicate that the majority of the carbon nanotubes remain as individual species and small bundles in the solid state. This is a direct result of the reductive dissolution and crosslinking process described herein. Scanning electron microscopy provides further evidence of the fine carbon nanotube scaffold structure, with few large bundles or aggregates observed. The high level of individualization and fine pore structure indicates a large active surface area, a property ideally suited for gas sensing applications.
[0111] Advantageously, the cross-linked carbon nanotube network is formed using a molecular layer deposition process such that the carbon nanotubes are connected in a series of parallel layers. This can be determined by comparing the in-plane conductivity to the through-thickness conductivity. The in-plane conductivity may be measured by making both contacts on the same surface of the film, while a through-thickness measurement requires one contact on the top surface of the film and the other on the bottom surface. An in-plane conductivity significantly greater than the through-thickness conductivity indicates that the carbon nanotubes are arranged in separate layers with alternating layers of cross-linker. It is expected that the through-thickness conductivity will decrease with each subsequent layer, while the in-plane conductivity will increase.
[0112] After deposition of the crosslinked carbon nanotube network, the solvent may be removed, for example, the network may be dried.
[0113] The removal of the solvent may, for example, include a first step of solvent exchange with at least one solvent having a lower surface tension than the initial solvent. The term "surface tension" as used herein refers to the attractive force in any liquid exerted by molecules below the surface on molecules at the surface / air interface, which force tends to inhibit the liquid from flowing. As used herein, the term "low surface tension" may refer to a liquid having a surface tension of about 30 mN / m or less, measured at 25° C. and atmospheric pressure. After the solvent exchange, the carbon nanotube network may be dried.
[0114] Some networks may be dried without solvent exchange, others require very low surface tension. Whether a particular network requires such solvent exchange depends on the individual properties of the network, i.e., the gel. Low density, high surface area networks have more desirable properties but tend to be less robust and may require solvent exchange or other controlled drying techniques well known to those skilled in the art. The properties of the network vary depending on the dimensions and crosslink density of the carbon nanotubes.
[0115] The crosslinked carbon nanotube network according to the present invention is preferably an aerogel. As used herein, the term "aerogel" refers to a low density, highly porous material prepared by forming a gel and then removing the liquid from the gel while substantially retaining the gel structure. Preferably, the "aerogel" according to the present invention comprises a carbon nanotube network in which the volume change upon drying of the gel is less than about 30%, preferably less than about 20%, preferably less than about 10%, preferably less than about 5%. Aerogels have an open-cell microporous or mesoporous structure. Typically, they have pore sizes of less than about 1000 nm and a density of less than about 100 m per gram. 2 Preferably, they have a pore size of less than about 200 nm and a surface area of less than about 400 nm per gram. 2 They often have low densities, e.g., about 1000 mg / cm 3 to about 1 mg / cm 3 to about 15 mg / cm 3 ~500mg / cm 3 Exceptionally, and unlike other existing aerogels, aerogels made from carbon nanotubes may have low density, high surface area, but large pore size.
[0116] Pore size may be measured by mercury porosimetry, which is suitable for larger macropores (diameter >50 nm). For smaller mesopores (approximately 2-50 nm) and micropores (<2 nm), nitrogen porosimetry may be used. The specific surface area can be determined by applying the Brunauer-Emmett-Teller (BET) theory to the adsorption-desorption isotherms. The pore size distribution is then calculated from the experimental isotherms using further analysis such as the Barrett-Joyner-Halenda (BJH) method or density functional theory (DFT).
[0117] Preferably, the aerogel is a material in which liquid has been removed from a gel under supercritical conditions.
[0118] Drying of the deposited network may be carried out by supercritical drying or freeze drying, preferably to form an aerogel. The most common method of supercritical drying involves the removal of the solvent with supercritical carbon dioxide, which may be used in the present invention. Critical point drying removes the solvent without crossing the liquid-gas boundary, potentially avoiding forces that may exert forces on the network microstructure that could cause rebundling of the carbon nanotubes.
[0119] Drying of the deposited network may be carried out at room temperature and / or at ambient pressure. The network may be dried in a stream of inert gas (N 2 The drying may be carried out by, for example, a stream of water.
[0120] This process uses supercritical CO 2 It may be a more versatile procedure for producing aerogels, since it does not require a freeze-vacuum process. Aerogels can be obtained by simply drying the gel. The aim is to evaporate the solvent, which results in a minimal volume reduction when obtaining the aerogel from the gel.
[0121] The aerogels prepared according to the present invention allow the gel to be cast into a given shape. The idea is to control the final shape by controlling the shape in the gel phase. The process of the present invention also allows the formation of large gels to form large aerogels.
[0122] It is desirable that the resulting carbon nanotube network contains as few impurities as possible. Such impurities include residual reagents, surfactants, additives, polymer binders, etc. The presence of these impurities can lead to an increase in the density of the carbon nanotube network and a decrease in the electrical conductivity and surface area of the carbon nanotube aerogel. The impurities may be removed during the solvent exchange process. The process according to the invention does not require the use of significant amounts of such additives or reagents, which are often difficult to remove, and therefore allows for the attainment of carbon nanotube networks with high electrical conductivity, large surface area, and low density. The total amount of impurities present in the carbon nanotube network may be less than 5% by weight, and even more preferably less than 1% by weight, preferably measured after the solvent has been removed.
[0123] Preferably, each carbon nanotube used in the present invention has a high electrical conductivity, greater than 10 MA / cm 2 Greater than 100 MA / cm 2 It is possible to pass electric current at a higher current density. Therefore, it is believed that the carbon nanotube network exhibits superior electrical conductivity and current density compared to existing carbon aerogels.
[0124] In addition, carbon nanotubes have desirable inherent mechanical properties, including high strength, stiffness, and flexibility at low density, which make them desirable for many industrial applications and impart desirable properties to the resulting aerogel networks.
[0125] The shape of the aerogel or xerogel can be controlled by controlling the shape of the container used during the gelation step. The density of the final aerogel can be controlled by varying the volume fraction of nanotubes within the initial gel.
[0126] The bridged carbon nanotube network may be provided (eg, deposited) on a substrate as described herein. The bridged carbon nanotube network may be provided as a film on the substrate.
[0127] Also provided herein is a film comprising a crosslinked carbon nanotube network, the film having a thickness of from about 1 nm to about 10 μm, for example, from about 1 nm to about 500 nm.
[0128] The thickness of the film can be measured by cutting a scar or step into the film. The height difference between the substrate and the film surface can be precisely determined by AFM for very thin films (<1 μm) and with a surface profiler for thicker films. Alternatively, electron microscopy can be used to measure the thickness of the film cross section.
[0129] Also provided herein is a layer-by-layer deposition process (molecular layer deposition process) for forming a cross-linked nanotube network, the process comprising: depositing reduced carbon nanotubes on a surface of a substrate as described herein; contacting the reduced carbon nanotubes with a linker precursor to form covalently functionalized carbon nanotubes; and contacting the covalently functionalized carbon nanotubes with additional reduced carbon nanotubes to covalently form a cross-linked carbon nanotube network comprising carbon nanotubes covalently linked by linkers formed from the linker precursor.
[0130] Each contacting step may be repeated to build up a three-dimensional cross-linked carbon nanotube network. The method may further include reacting the crosslinked carbon nanotube network with additional linker precursors and then reacting the resulting material with additional reduced carbon nanotubes.
[0131] A linker is a multivalent (eg, divalent) moiety that contains at least two functional groups capable of reacting with the walls of a reduced carbon nanotube to form a CC covalent bond and thus a crosslinked network.
[0132] Preferably, the linker is a rigid linker, which is rigid enough to avoid "backbiting", whereby the leaving group reacts with the same carbon nanotube, as shown in Scheme 2 below.
[0133] Scheme 2: Backbiting of a non-rigid linker
[0134] [ka]
[0135] As will be understood, the rigid linker must be sufficiently rigid to avoid the appearance of the leaving group on the same side of the rigid linker. Thus, as used herein, "rigid" means that the conformational constraints and steric hindrance of the linker molecule favors binding to two carbon nanotubes, rather than forming two bonds to a single carbon nanotube. Preferably, at least two functional groups are located on different atoms of the linker molecule, more preferably some distance apart, to maximize the chance of reacting with two different nanotubes.
[0136] It is understood that the rigid linker precursor may be a conjugated linker precursor, such that the process follows the process described above and the covalently crosslinked carbon nanotube network comprises carbon nanotubes covalently linked by conjugated linkers formed from the conjugated linker precursor, however, the process need not be limited to conjugated linker precursors.
[0137] The rigid linker precursor has the structure: XYX may be a compound of wherein Y is a polyvalent rigid system and each X is independently a suitable leaving group as described herein.
[0138] The rigidity of the linker may be provided by one or more cycloalkyl or aryl groups.
[0139] Y may comprise a cycloalkyl group. Y may consist essentially of a cycloalkyl group. Exemplary cycloalkyl groups include cyclohexyl and adamantane. Y may comprise (and preferably consist essentially of) a polyoctahedral silsesquioxane.
[0140] Y is of the structure * -Y'-CH 2 -Y'- * may be a group wherein each Y' is independently C 6 ~C 10 a monocyclic or bicyclic aryl ring or a 5- to 10-membered monocyclic or bicyclic heteroaryl ring; * indicates the point of attachment to each X. Each Y may independently be phenyl or thiophenyl.
[0141] The rigid linker precursor may be 1,4-dihalocyclohexane, for example 1,4-diiodocyclohexane. The rigid linker precursor may be bis(4-bromophenyl)methane or 5,5-dibromo-2,2-dithienylmethane.
[0142] A combination of rigid linker precursors may be used in the process of the invention.
[0143] As will be appreciated, the rigid linker precursor reacts with the sidewalls of the reduced nanotubes to bridge adjacent nanotubes, resulting in nanotubes having the structure * -Y- * (In the formula, * are attached by a rigid linker having a leaving group X absent (denoting the point of attachment to each nanotube, i.e., the rigid linker precursor structure).
[0144] The rigid linker moiety of the rigid linker precursor (e.g., group Y) may be substituted as described herein. As will be appreciated, when the rigid linker precursor (e.g., Y) is optionally substituted with one or more suitable leaving groups (such as halides), the suitable leaving group substituents may function as functional groups capable of reacting with the surface of the reduced carbon nanotubes.
[0145] The rigid linker precursor may have three or more functional groups capable of reacting with the surface of the reduced carbon nanotube. For example, the rigid linker precursor may have the structure: Y-(-X) m may be a compound of wherein Y, X and m are as defined herein.
[0146] It is not essential that the linker precursor is a rigid linker. Complete backbiting of the linker can be avoided by saturating the surface of the carbon nanotube with the linker precursor to form a saturated covalently functionalized carbon nanotube. Therefore, any linker precursor may be used as long as it contains at least two functional groups that can react with the wall of the reduced carbon nanotube to form a C-C covalent bond.
[0147] Thus, each step of contacting the reduced carbon nanotube with a linker precursor to form a covalently functionalized carbon nanotube may include contacting the reduced carbon nanotube with the linker precursor for a sufficient time such that the carbon nanotube is saturated with the covalent functionalization of the linker, i.e., such that all available sites on the nanotube surface that comply with steric requirements are covalently functionalized, leaving exposed reactive functional groups on the grafted linker molecule. As will be appreciated, the extent to which the carbon nanotube is saturated will vary depending on the steric constraints of the linker molecule.
[0148] The process may be carried out under any suitable conditions, such as under inert conditions, as described above.
[0149] This process may be used to form films for a variety of potential applications, from photovoltaic devices, sensors and catalysts to conductive inks and coatings, as discussed above.
[0150] Also provided herein is a cross-linked carbon nanotube network prepared by this process. The cross-linked carbon nanotube network comprises: a plurality of carbon nanotubes as described herein; and at least one linker, as described herein, that covalently links adjacent carbon nanotubes. A bridged carbon nanotube network is formed using reduced carbon nanotubes, whereby the layer-by-layer approach shares many advantages with respect to porosity, homogeneity and conductance, as discussed above.
[0151] Gas Sensing Applications The cross-linked carbon nanotube networks and films described herein may be used in gas sensing applications. Thus, the cross-linked carbon nanotube networks and films described herein may be used as gas sensors or to sense gases.
[0152] Also provided herein is a gas sensor comprising the carbon nanotube network or film described herein. The gas sensor described herein (e.g., a gas sensor for sensing a target gas) comprises: A first electrode and a second electrode; a carbon nanotube network as described herein (preferably as a film), The first electrode and the second electrode are in electrical contact with the carbon nanotube network.The sensor may be in the form of a sensor array.
[0153] In use, when the gas sensor or sensor array is exposed to a target gas, the target gas is bound by the carbon nanotube network. This changes the impedance of the carbon nanotube network between the first electrode and the second electrode. This change in impedance can be measured and used to determine the concentration or presence of the target gas. Thus, the carbon nanotube network of the gas sensor or sensor array may be a chemiresistor.
[0154] The carbon nanotube network of the gas sensor or sensor array may be a transistor. For example, the sensor or sensor array may be a chemical field effect transistor (ChemFET). The bridged carbon nanotube network may provide a conductive channel between source and drain electrodes in the transistor. In use, a voltage may be applied to the third "gate" electrode, allowing modulation of the conductivity in the source-drain channel. The channel current is measured upon exposure to gas over a range of gate voltages, allowing accurate determination of the concentration or presence of the target gas with high sensitivity.
[0155] Any suitable electrode material may be used. For example, each electrode may be independently a metal electrode such as gold, silver, nickel, or platinum, with some palladium being some of the more commonly used. Gold deposited on chromium may be used as the electrode material. In general, inert, high work function metals are preferred. Bonding between the metal and the carbon nanotube network may contribute to the sensing activity.
[0156] The cross-linked carbon nanotube network may be provided on a substrate as described herein. The substrate may be inert.
[0157] As will be appreciated, the substrate may function as an electrode in a sensor or sensor array and therefore may be formed from any suitable electrode material.
[0158] In the case of a transistor, the substrate may act as a "back gate" and may therefore be formed from a suitable electrode material, however preferably a gate electrode is provided in addition to the substrate.
[0159] The gas sensor or sensor array may further comprise a voltage source configured to apply an electrical potential between the first electrode and the second electrode.
[0160] The gas sensors or sensor arrays described herein may be combined with machine learning to provide a fingerprint of the gases present in a sample, for example, air.
[0161] Also provided herein is a process for sensing a target gas, comprising: exposing a gas sensor or sensor array described herein to a gas sample containing a target gas such that the target gas is bound by the carbon nanotube network; measuring the impedance of the carbon nanotube network layer by applying a potential to the carbon nanotube network; and determining a concentration of the target gas based on the impedance of the carbon nanotube network layer.
[0162] The concentration of the target gas may be measured in parts per million, for example, as partial pressure, weight percentage, volume percentage, moles per unit volume, or moles per unit mass.
[0163] Throughout the description and claims of this specification, the terms "comprises" and "including," as well as variations of these terms, such as "comprises" and "comprises," mean "including / comprises, but are not limited to," and are not intended to (and do not) exclude other elements.
[0164] It is understood that variations to the foregoing embodiments of the invention may be made while still falling within the scope of the invention. Each feature disclosed herein, unless otherwise stated, may be replaced by an alternative feature serving the same, equivalent or similar purpose. Thus, unless otherwise stated, each feature disclosed is only one example of a generic series of equivalent or similar features.
[0165] All of the features disclosed herein may be combined in any combination, except combinations in which at least some of such features and / or steps are mutually exclusive. In particular, preferred features of the invention are applicable to all aspects of the invention and may be used in any combination. Similarly, features described in non-essential combinations may be used separately (not in combination).
[0166] It will be appreciated that many of the features described above, particularly those of the preferred embodiments, are inventive in their own right and not as merely part of an embodiment of the present invention, and independent protection may be sought for these features in addition to, or as an alternative to, any presently claimed invention.
[0167] definition As used herein, alkyl refers to a straight or branched hydrocarbon chain. An alkyl may have 1 to 10 carbon atoms, optionally 1 to 6 carbon atoms. Exemplary alkyl groups include, but are not limited to, methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, s-butyl, t-butyl, 2-methylbutyl, n-pentyl, s-pentyl, n-hexyl, 2-ethylhexyl, n-heptyl, n-octyl, and the like. An alkyl may be unsubstituted or substituted with one or more substituents as defined herein.
[0168] As used herein, aryl refers to an aromatic hydrocarbon ring. As used herein, heteroaryl refers to an aryl ring containing one or more heteroatoms (e.g., O, S, or N). Aryl and heteroaryl groups may be mononuclear, i.e., having only one aromatic ring (e.g., phenyl or phenylene), or polynuclear, i.e., having two or more aromatic rings, which may be fused (e.g., naphthyl or naphthylene), individually covalently bonded (e.g., biphenyl), and / or a combination of both fused and individually bonded aromatic rings. Aryl groups may contain 6 to 20 carbon atoms, or 6 to 12 carbon atoms. Aryl may be fused to one or more aryl or cycloalkyl rings to form a polycyclic ring system. Exemplary aryl groups include, but are not limited to, phenyl, biphenylene, triphenylene, [1,1':3',1"]terphenyl-2'-ylene, naphthalene, anthracene, binaphthylene, phenanthrene, pyrene, dihydropyrene, chrysene, perylene, tetracene, pentacene, benzopyrene, fluorene, indene, indenofluorene, spirobifluorene, and the like. Preferably, the aryl is phenyl. Exemplary heteroaryl groups include, but are not limited to, pyrrolyl, furanyl, thiophenyl, imidazolyl, oxazolyl, thiazolyl, triazolyl, pyrazolyl, pyridinyl, pyrazinyl, pyridazinyl, and pyrimidinyl, and the like. Preferably, the heteroaryl is thiophenyl or pyrrolyl. The aryl or heteroaryl may be unsubstituted or substituted with one or more substituents as defined herein.
[0169] As used herein, cycloalkyl refers to a cyclic alkyl group. Cycloalkyl may have 3 to 20 carbon atoms, or 3 to 15 carbon atoms, or 3 to 10 carbon atoms. Cycloalkyls include bridged, fused, and / or spiro ring systems such as decalin, norbornane, and spiro[5.4]decane. Exemplary cycloalkyl groups include cyclopropyl, cyclobutyl, cyclopentyl, cyclooctyl, decalin, norbornane, and spiro[5.4]decane. Cycloalkyls may be unsubstituted or substituted with one or more substituents as defined herein.
[0170] As used herein, a halide may be selected from the group consisting of -F, -Cl, -Br, -I.
[0171] As used herein, porphyrin is a group containing four pyrrole rings linked through the alpha positions by four methine groups to form an aromatic macrocyclic structure.
[0172] Reference is now made to the following examples, which illustrate the invention in a non-limiting manner.
[0173] consumer products Consumer products of the present invention may include air fresheners, air freshener devices, air purifying devices, air filtering devices, oral care products including toothbrushes and toothpastes, mouthwashes, body washes, shampoos, conditioners, personal care products including antiperspirants and deodorants, absorbent articles including diapers and adult incontinence articles, feminine care products, razors, dish detergents, detergents, fabric softeners, dryer sheets, fabric care products including fragrance enhancers, cleaning implements including dusters and mops, surface cleaners, cleaning wipes, and paper products including paper towels and tissues.
[0174] The consumer product may be a smart consumer product, device, or both wirelessly connected to the controller and / or sensor. The consumer product may be equipped with a wireless communication module to be connected and automated through the system and included in the method of the present disclosure. The consumer product may be communicatively connectable to the CCU. Referring to FIG. 5, the consumer product may be equipped with a wireless communication module 136 to communicate with the CCU and / or the consumer product composition dispenser 104. The smart consumer product may be configured as a toothbrush, a razor, an adsorbent article, a feminine care product, a cleaning implement, an air freshener device, or an air purification device.
[0175] The sensor may be physically located on the consumer product or the sensor may be a separate element of a system that is movable independently of the consumer product. Locating the sensor directly on the consumer product may allow for close proximity to the consumer product to allow for a reading no matter where the consumer product is positioned at any given time, and may allow the sensor and consumer product to be moved simultaneously.
[0176] The consumer product 104 may require user intervention to respond to data generated by the sensor 106. For example, the sensor 106 may send an incoming signal to the CCU. The incoming signal from the CCU may read a high or low level of target gas concentration in the space surrounding the sensor compared to a set point of the target gas concentration. The CCU may alert the user and have the user respond by selecting and using a particular consumer product that can mitigate or enhance the concentration of the particular target gas.
[0177] The consumer product 104 may be in the form of a consumer product composition dispenser. The consumer product composition dispenser may be used to deliver the consumer product composition into the atmosphere or onto an inanimate surface. Such consumer product composition dispensers may be configured in a variety of ways. For example, the consumer product composition dispenser may be configured as an energized dispenser (i.e., powered by electricity, or by a chemical reaction such as a catalytic fuel system, or by solar power, etc.). An exemplary energized consumer product composition dispenser includes a power supply support means that may include a heating element, a piezoelectric element, a thermal inkjet element, a fan assembly, cold air diffusion using an air pump for aerosolization, an automatic sprayer, an automatic aerosol, a hydrogen fuel cell, etc. More specifically, the consumer product composition dispenser may be an electrical wall outlet consumer product composition dispenser, a non-limiting example of an electrical wall outlet consumer product composition dispenser includes a battery (including a rechargeable battery) powered consumer product composition dispenser with heating and / or fan elements as described in U.S. Pat. No. 7,223,361. In an energized device, the consumer product composition dispenser may be located near a power supply support means for dispersing the volatile material. The volatile material may be formulated for optimal diffusion with the supply support means. Exemplary consumer product composition dispensers include air freshening dispensers.
[0178] The consumer product composition dispenser may be configured as a non-energized dispenser. An exemplary non-energized consumer product composition dispenser includes a reservoir and, optionally, a capillary, a wicking means, or an emanation surface to help the volatile material to diffuse passively (i.e., without energized means) into the air. A more specific example of the consumer product composition dispenser includes a supply engine having a liquid reservoir for containing the volatile material and a microporous membrane surrounding the liquid reservoir, as disclosed in U.S. Patent Nos. 8,709,337 and 8,931,711.
[0179] The consumer product composition dispenser 104 may also be configured for use as an aerosol or non-aerosol sprayer. The consumer product composition dispenser 104 may be programmed to automatically dispense the consumer product composition into the atmosphere. The sprayer may be operated manually by a user or automatically by electromechanical means.
[0180] Air freshening devices may be used in individual rooms or small spaces (e.g., bedrooms, bathrooms, automobiles, etc.) and / or whole-house central air conditioning / heating systems (e.g., HVAC) utilizing ionization, filtration, plasma, ultraviolet light (UV light) (e.g., UVC, UVA, UVB) catalytic coatings, metal oxide coatings, and / or hydroxyl radical technologies. In the case of air freshening to sterilize air, the air freshening device may dispense particles such as vaporized or aerosolized droplets of hydrogen peroxide, glycol, triethylene glycol, hydroxyl radicals, hypochlorous acid, essential oils, ozone, quaternary amines, positively and / or negatively charged ions, or other active substances to sterilize or disinfect the air. The air freshening device may also be a ventilation device for a bathroom or kitchen area where it is desired to exhaust the air from that room (i.e., a bathroom exhaust or a kitchen hood over a stove to ventilate the air).
[0181] The consumer product comprising the consumer product composition dispenser and / or air freshening device may also be configured as a mobile robot that can go to locations where the sensor is reading one or more target gases outside of a set point and use one or more available technologies to enhance or reduce the concentration of the target gas at the sensor location. For example, the mobile robot may utilize air freshening, air purification, and / or air sanitation technologies at locations where the sensor is detecting high or low levels of the target gas.
[0182] The system may comprise one or more consumer products. The system may comprise an array of consumer products that may be movable to different rooms within a housing or building. Additionally, the home or building may comprise one or more consumer product composition dispensers positioned in the same room or in different rooms.
[0183] The freshening composition dispenser may be capable of containing and keeping separate two or more consumer product compositions, including at least two different consumer product compositions, or at least two different consumer product compositions, or at least three consumer product compositions.
[0184] The consumer composition may be an air freshening composition comprising a fragrance composition and / or a malodour control composition. The consumer composition may comprise an insect repellent. The consumer composition may comprise a biocide.
[0185] The consumer product composition may include a volatile material. Exemplary volatile materials include fragrance materials, volatile dyes, materials that function as insecticides, essential oils or materials that function to condition, modify, or otherwise modify the environment (e.g., to aid in conditions such as sleep, wakefulness, respiratory health, etc.), deodorants or malodor control compositions (e.g., odor neutralizing materials such as reactive aldehydes (disclosed in U.S. Patent Application Publication No. 2005 / 0124512), odor blocking materials, odor masking materials, or sensory improving materials such as ionones (also disclosed in U.S. Patent Application Publication No. 2005 / 0124512)).
[0186] The consumer product composition may include perfume raw materials of a perfume blend to provide a desired scent in the air. The consumer product composition includes a mixture of volatile aldehydes designed to provide true malodor neutralization (not functioning by simply masking or concealing odors). True malodor neutralization provides sensory and analytically measurable (e.g., gas chromatograph) malodor reduction. Thus, when a consumer product composition provides true malodor neutralization, the consumer product composition reduces malodor in the gas phase and / or liquid phase. The consumer product composition may include a mixture of volatile aldehydes that neutralize malodor in the gas phase and / or liquid phase through chemical reactions. Such volatile aldehydes are also called reactive aldehydes. Reactive aldehydes may react with amine-based odors following the Schiff base formation pathway. Volatile aldehydes may also react with sulfur-based odors to form thiol acetals, hemithiol acetals, and thiol esters in the gas phase and / or liquid phase.
[0187] The consumer product compositions may include a variety of other ingredients, including, but not limited to, surfactants, acid catalysts, polymers, buffers, solubilizers, antimicrobial compounds, preservatives; humectants; aqueous carriers, diluents, and the like, and combinations thereof.
[0188] Central Communication Unit The CCU 102 may be configured in a variety of different ways. The CCU 102 may be configured to receive incoming signals from one or more components of the system 100 and to send outgoing instructions to one or more components of the system 100, such as consumer products and / or smart devices within the system.
[0189] 5, the CCU 102 may be communicatively connectable to various components of the system 100, including the sensors 106, the user interface 108, and the consumer products 104, using a wireless communication link 107. Various wireless communication links may be used, including 802.11 (Wi-Fi), 802.15.4 (ZigBee, 6LoWPAN, Thread, JennetIP), Bluetooth, combinations thereof, and the like. The connection may be via an ad-hoc mesh network protocol. The CCU 102 may include a wireless communication module 116 to establish wireless communication links 107 with the CCU 102 at various components of the system. Any module known in the art may be utilized to establish the communication link.
[0190] The CCU 102 may include a processor 122. The processor 122 may be configured and programmed to perform and / or cause to be performed one or more advantageous functions of the system 100 described herein. The processor 122 may be physically located within the CCU 102 or may be remotely located on a computer, a specialized computer, a smart device such as a phone or tablet, a server, an intranet, a border router, a cloud-based system, or the like, or a combination thereof. The processor 122 may execute algorithms stored in a local memory, a dedicated processor, or an application specific integrated circuit, algorithms executed or managed remotely by a central server or a cloud-based system, such as by executing a Java Virtual Machine that executes instructions provided from a cloud server using asynchronous JavaScript and XML or similar protocols. The algorithms may be repeated periodically, such as at specific time intervals. The algorithms may be repeated hourly, daily, weekly, etc., and may be configured to operate on different schedules at different times of the day or on different days of the week. Different algorithms may be used depending on whether a user is present in the space or not.
[0191] The CCU 102 may include a memory 124. The memory may be configured to store set points, incoming signals such as sensor measurements and status indicators, algorithms, etc. The memory may be local memory within the CCU 102, such as a flash drive, a hard drive, a read-only memory, or a random access memory. Or, the memory may be configured as remote memory on a computer, on a smart device such as a phone or tablet, on a server, or on a cloud-based system. The memory 124 may be accessible to the processor 122 in various ways.
[0192] The processor and / or memory of the CCU 102 may be located within a housing of the CCU 102. The CCU 102 may be connected to or separate from various components of the system 100. For example, the CCU 102 may be physically connected to a consumer product. The CCU 102 may be permanently located in a building in a room or location separate from other components, such as, for example, smart devices and / or consumer products 104. The CCU 102 may be configured as a smart thermostat. A smartphone or tablet may be used as the CCU. The CCU may be communicatively connectable to a computer, smartphone, or tablet.
[0193] The CCU may include the clock or may communicate wirelessly with the clock. The CCU may be communicatively connectable to the clock over a computer, a smart device, or the internet.
[0194] 5 illustrates an example CCU 102 having a processor 122 and a memory 124 disposed within a housing 128. The CCU 102 illustrated in FIG. 5 may be disposed on or within a consumer product 104 or a smart device 109. Although FIG. 5 illustrates the processor 122 and the memory 124 disposed within the housing 128, it should be understood that the processor 122 and / or the memory 124 may be disposed remotely with respect to the CCU 102.
[0195] The incoming signal may be passed through a CCU unit that includes a transmitter that transmits the incoming signal to a remote memory. The incoming signal may also be received directly by a component that is in wireless communication with the component transmitting the signal.
[0196] 6 illustrates several example flows of incoming signals from various components of the system 100 to a remote memory. The incoming signals may flow from the sensor 106, the consumer product 104, the smart device 109, or various other components to the remote memory via a wireless communication link, directly to a computer or smart device, or via a transmitter in the CCU. The processor 122 may access the incoming signals from the memory 124. The processor 122 may access the memory 124 via a wired or wireless communication link.
[0197] The processor 122 may be configured to compare the incoming signal with set points stored in the memory 124. The processor may retrieve the stored set points from the memory 124.
[0198] The system may include a user feedback loop to assist the user in selecting an appropriate set point. For example, the user may not understand what the appropriate level of a particular target gas should be. The user interface or CCU may allow the user to answer questions or select from different prompts related to the user's desired target. Exemplary questions or prompts may relate to the user's preferences regarding scent intensity, identification and quantification of sensitivities the user may have to particular odors, times of day or activities at which the user may desire a particular scent in the air or enhanced cleaning of the air. Based on the response from the user, the CCU may select a particular set point or may modify the set point, such as through machine learning. The user feedback loop allows the user to modify the set point, and subsequent operation of the consumer product may be adjusted in response to the set point modification from the user.
[0199] A consumer feedback loop may occur before the start of operation to aid in algorithm selection, and / or during operation to check that the set points still meet the consumer's needs or interests.
[0200] As discussed above, the CCU may be configured to execute various algorithms to operate one or more consumer products 104 in response to incoming signals from the sensors 106. Figure 7 shows an example algorithm that may be used by the CCU 102 to control the consumer products 104 and / or smart devices 109 based on incoming signals from the sensors 106. The sensors may be configured for one or more target gases of interest. If the sensors detect a target gas, the sensors 106 may identify the target gas and the concentration of the target gas and send those details as an incoming signal to the CCU.
[0201] Continuing with reference to FIG. 7, in an exemplary algorithm, either selected by a user or selected by the processor based on feedback from a user, the processor 122 may be configured to compare an incoming signal from the sensor 106 for a particular target gas to a set point for the target gas stored in the memory 124. If the value of the incoming signal to the CCU 102 is different from the target gas concentration or concentration range set point stored in the memory 124, the processor 122 sends an outgoing command to a particular consumer product 104 or smart device 109 identified by the CCU as being capable of reducing or enhancing the level of the particular target gas. The CCU may send an outgoing command to the selected consumer product 104 to either turn the consumer product 104 on or off, depending on the desired outcome and utility of the particular consumer product 104. If the value of the incoming signal from the sensor 106 is equal or substantially equal to the set point concentration of that particular target gas, the processor 122 sends an outgoing command to the consumer product or smart device to either turn on or off, or sends an outgoing command to the consumer product 104 to change an operational setting of the consumer product, such as flow rate, intensity, etc. Algorithms such as those described may be repeated on a set time schedule, such as hourly, daily, weekly, etc., may be configured to operate on different schedules at different times of the day or different days of the week, and / or may operate differently when a user is present or absent within the space.
[0202] "Substantially equal" may include an acceptable tolerance between the set point and the concentration measured by the sensor, which may be programmed into the algorithm. Thus, a sensor concentration measurement that is substantially equal to the set point may be treated by the processor as being equal to the set point.
[0203] The memory 124 may be configured to store multiple set points. For example, there may be different set points for different times of the day, periods of the day, and different set points for different days of the week. The CCU may use a clock to determine which set point to use at a particular time and / or day of the week.
[0204] The set point may be a desired or acceptable concentration or concentration range for a particular target gas. The memory may store set points for one or more target gases, and one or more sensors may be used to simultaneously identify and measure multiple target gases.
[0205] The algorithm can be programmed to send an outgoing signal to the sensor to take sensor measurements at specific times of the day or at set intervals throughout the day.
[0206] The CCU may be configured to use sensor measurements from different sensors located within the home or building. Different sensors may be used at different times of day and / or on different days of the week, or may take measurements simultaneously.
[0207] Set points may be used to control when a consumer product is turned on and the length of time it is turned on. The duration for which a particular consumer product may be turned on may range from about 5 minutes to about 60 minutes, or from about 10 minutes to about 30 minutes. For example, a set point may be configured as a predetermined duration after the consumer product is turned on, such that the consumer product may be turned off for a preprogrammed duration.
[0208] Upon receiving an incoming signal from the sensor that the target gas is outside the set point, the CCU may be configured to provide a suggested action to the user. For example, the CCU may recognize the type of consumer product connected to the system, or the user may instruct the CCU with a list of consumer products that the user may use at their disposal. Based on that list of consumer products, the CCU may alert the user to certain consumer products that may be useful in mitigating or enhancing a certain target gas. The CCU may automatically send outgoing instructions to one or more wirelessly connected consumer products and / or may send notifications or instructions to the user about manual actions suggested by the user on one or more identified consumer products. The CCU may also send outgoing instructions to the user to open a window or increase ventilation in the house.
[0209] The CCU may be configured as a thermostat, such as the thermostat shown in FIG. 2. The thermostat may include a processor or memory, or the thermostat may be in communication with a remote processor and / or memory. The thermostat may include a user interface. The thermostat may be a NEST® Learning Thermostat, a LUTRON® Thermostat, or the like. The processor may calculate optimal set points from an algorithm based on user preferences for target gas concentrations.
[0210] The machine learning algorithm can learn the user's preferred set points, for example, at different times of the day and / or different days of the week, and / or can be used to program more energy-efficient algorithms. An exemplary learning system is used in the NEST® learning thermostat. An exemplary learning system is also described in U.S. Pat. No. 9,115,908. The processor then transmits the optimal set points to a memory, which then stores the set points. The machine learning algorithm can be used to adjust and calibrate for drift and background levels of the sensor measurements through user feedback and / or calibration to increase sensitivity and selectivity to the target gas.
[0211] Devices in the system, including consumer products, sensors, and smart devices, may interact with each other through the CCU such that an event detected by one device may affect the operation of another device, or such that the current status of one device may affect the operation of another device.
[0212] User Interface The systems and methods of the present disclosure may include one or more user interfaces 108. The user interface 108 may be configured in a variety of different forms. A user may connect sensors 106 through the CCU 102 to interact with the user interface 108 to adjust set points as well as view raw sensor data on the user interface. The CCU 102 may also connect to the Internet or an intranet and pass information such as sensor measurements and set points to a server for remote monitoring on the user interface 108. The user interfaces may be integral to the CCU or may be separate. One or more user interfaces may be connected to the system.
[0213] 8 shows an example system having two or more user interfaces, where a first user interface is connected to the CCU and a second user interface is a remote user interface, which may be in the form of a computer or a handheld smart device.
[0214] If the CCU is configured as a thermostat, the thermostat may include a user interface that allows a user to adjust a temperature setpoint, for example, by pressing a button or turning a dial.
[0215] The user interface may be configured as a program, an HTML website, or a native application accessible by a user through a computer or a handheld smart device. The handheld smart device may include an iPhone, iPad, or an Android or Microsoft based system. The user interface may be accessible on a computer such as a desktop, laptop, or tablet.
[0216] The CCU, the sensors, and / or the user interface may include an indicator light or a series of indicator lights to alert a user that one or more of the sensors is measuring a target gas concentration outside of a set point. The user may respond to the indicator light by selecting and using a consumer product to reduce or enhance the target gas.
[0217] The system of the present disclosure may include a handheld smart device or computer that includes a CCU 102 that includes a processor 122, a memory 124, and / or a user interface 108. EXAMPLES
[0218] Materials and Methods Purified HiPco was purchased from Nanointegris and purified under high vacuum (10 -6 The mixture was degassed at 500°C for 10 h at 375°C and 1000 mbar. Sodium (99.95% ingot), DMAc (anhydrous 99.8%), naphthalene (99%), p-diiodobenzene (99%), and 2,5-dibromoaniline (97%) were purchased from Sigma Aldrich Ltd. (UK). Ethanol (96%) and acetone (99.8%) were purchased from VWR Ltd. (USA). Dry air (O 2 / N 2 20 / 80 v / v) was purchased from BOC. Reductive dissolution and aerogel film deposition were carried out under inert conditions in a glove box (Braun, O 2 <0.1ppm, H 2 O<0.1 ppm).
[0219] measurement TGA was performed using a METTLER Toledo TGA-DSC 1 2 The samples were heated at 100°C in a N 2The sample was heated at 1000° C. for 30 min at a flow rate of 60 mL / min under vacuum, then ramped to 800° C. at 10° C. / min. The XPS spectrometer was equipped with an MXR3 Al Kα monochromated X-ray source (hν=1486.6 eV). The X-ray gun power was set at 72 W (6 mA and 12 kV). Charge compensation was achieved using an FG03 flood gun using a combination of low energy electron and ion flood sources. Argon etching of the sample was performed using a standard EX06 argon ion source, using an accelerating voltage of 500 V and an ion gun current of 1 μA. Survey scans were acquired using a pass energy of 200 eV, a step size of 1 eV and a dwell time of 100 ms (50 ms×2 scans). All high-resolution spectra (C1s and O1s) were acquired using a pass energy of 20 eV, a step size of 0.1 eV and a dwell time of 1 s (50 ms x 20 scans = 1000 ms). Samples were prepared by pressing them onto double-sided sticky carbon-based tape. The pressure during the XPS spectrum measurements was below 1 x 10-8 mbar. Thermo Avance software was used for data interpretation. Data were processed using CASA XPS software (version 2.3.16). Quantitative analysis was performed after subtracting the baseline using Shirley or two-point linear background types. Peaks were fitted using a GL(30) lineshape, a combination of Gaussian (70%) and Lorentzian (30%) functions. All XPS spectra were charge corrected by referencing the fitted contribution of CC graphitic carbon at the C1s signal 284.5 eV.
[0220] Raman spectroscopy was performed with a Renishaw InVia Raman Spectrometer and a 532 nm laser with 1800 lines / mm grating. Statistical D / G measurements were made by comparing the relative intensities of the D and G bands from multiple spectra containing maps with areas >100 μm × 100 μm. Scanning electron microscopy (SEM) was performed on a Zeiss Gemini Sigma300 at an accelerating voltage of 10 keV. Samples were glued to aluminum stubs with carbon tabs and the film was contacted with silver paint. Atomic force microscopy (AFM) was performed in dynamic mode on an hpAFM with an AFM controller (NanoMagnetics Instruments, UK) using a Nanosensor tapping mode probe. Microscopic images were processed with NMI Image Analyzer (v1.4, NanoMagnetics Instruments) utilizing built-in height and line correction and scar removal functions.
[0221] Example 1 - Crosslinking and deposition Reductive dissolution and crosslinking In a typical synthesis, a bulk solution was prepared by adding equimolar amounts of sodium ingot (30 mg, 1.30 mmol) and naphthalene (167 mg) to DMAc (15.0 mL), and 2 mg Na mL DMAc -1 The dark green solution was stirred for 18 hours. Then, sodium naphthalide solution (2.24 mL, 2.24 mmol) was added. Na ) was added to degassed SWCNT powder (40 mg) to give a sodium:carbon stoichiometry of 1:10. The solution was then diluted with additional DMAc to give 1.8 mg SWCNT mL DMAc -1 and an optimal [Na] of 15 mM. The solution was stirred overnight with a glass stir bar to obtain a homogenous solution before use.
[0222] Conjugated linker precursor synthesis BocDBA was synthesized according to Fracaroli, AM et al. Metal-organic frameworks with precisely designed interior for carbon dioxide capture in the presence of water. J. Am. Chem. Soc. 136, 8863-8866 (2014). The procedure was adapted from Fracaroli et al. Briefly, tetrahydrofuran (THF) (20 mL) was degassed by sparging with nitrogen, and then 1,5-dibromoaniline (2.00 g, 8.0 mmol), 4-dimethylaminopyridine (98 mg, 0.8 mmol) and di-tbutyl decarbonate (5.2 g, 24 mmol) were added. The reaction mixture was stirred at 40 °C for 5 h. After removing THF under reduced pressure, MeCN (80 mL) and LiBr (2.14 g, 24.6 mmol) were added. The suspension was stirred at 65° C. for 18 h, then cooled to room temperature and evaporated to dryness. The crude product was dissolved in DCM and purified by flash silica column chromatography eluting with hexane:AcOEt (20:1) to give the product as a pale yellow solid (2.81 g, 35%). 1 HnmR (400MHz, CDCl 3 ),[ppm]:1.54(s,9H),6.99(br s,1H),7.02(dd,J=8.5,2.4Hz,1H),7.34(d,J=8.5Hz,1H),8.40(d,J=2.4Hz,1H).
[0223] Aerogel film deposition Glass microscope slides are cut into squares and soaked in piranha solution (25:75 in H2O). 2 O 2 (30%):H 2 SO 4 (94%)) for 20 min, followed by rinsing three times with HPLC water. The substrate was dried under vacuum, and then excess 3-iodopropyl-trimethoxysilane was drop-cast on top. After 30 min, residual silane was washed off with DMAc and then dried under vacuum.
[0224] Aerogel film: Carbon nanotube (1.8 mg SWCNT mL DMAc -1 ) (150 μL) was added to a vial and an equimolar amount (crosslinker: Na) of crosslinker was added to the nanotubides in solution. 12 μL of this gelled nanotubides was then rapidly drop-cast onto a pre-silanized glass substrate contained in a DMAc-saturated atmosphere for 24 h. The film was then subjected to a series of solvent exchanges (MeOH, MeOH / HCl 0.1M), isopropyl alcohol / H 2 O), followed by acetone for 24 h, followed by liquid CO 2 It was dried under supercritical conditions. Figure 9(a).
[0225] UV-visible spectroscopy of the resulting semitransparent thin films showed that M 11 and S 22 The film shows a pronounced Van Hove singularity peak corresponding to the critical point drying transition (Figure 9(c)). These adsorption bands reveal the presence of individualized SWCNTs and small diameter bundles that are retained in the solid state after critical point drying. The film is low density, with a measured thickness of 240 nm (Figure 9(d,e)), yet retains 35% transparency.
[0226] Functionalization and characterization of cross-linked carbon nanotube networks Aerogel films were fabricated using p-diiodobenzene (DIB) to provide a network without functional binding sites, and Boc-protected 2,5-dibromoaniline (BocDBA) to provide amine binding sites. Statistical Raman spectroscopy (SRS) revealed defect-induced modes (approximately 1350 cm) for both functionalized films when compared to both the uncrosslinked film and the pristine SWCNT material. -1) indicating covalent grafting to the SWCNTs. Higher intensity defect modes are observed for DIB than for BocDBA, which is attributed to the higher reactivity of aryl iodides with the nanotubes. In each case, the increase in the D band is relatively small, especially for the uncrosslinked aerogel films, suggesting that the reductive dissolution pathway is largely dominated by sp 2 X-ray photoelectron spectroscopy (XPS) revealed small amounts of residual iodine and bromine in the p-DIB and BocDBA crosslinked films, respectively, indicating mono-grafted species. The aniline crosslinked network contained 0.84% nitrogen atoms, giving an estimate of one grafted unit per 90 SWCNT carbon atoms. The slight increase in oxygen content of each film indicates that oxygen functional groups were added during the aerogel film synthesis, with the oxygen release step likely being a contributing factor. Further evidence of crosslinker grafting is provided in thermogravimetric analysis (TGA) of the crosslinked networks produced in monolithic form (Figure 10(b)). Larger mass losses of 19% and 14% were observed for the phenyl and aniline crosslinked networks, respectively, reinforcing the evidence from the TGA that p-DIB grafts in higher yield than BocDBA. Only modest mass losses were observed for the non-crosslinked control sample, indicating that the reductive dissolution in isolation does not introduce many additional functional groups.
[0227] Microstructure -X-ray photoelectron spectroscopy (XPS) XPS of the SWCNT sample contains a large C1s peak (285 eV), a smaller O1s peak (532 eV), and additional peaks corresponding to surface functionalization (Figure 11). The C1s scan reveals that the sample is composed mainly of sp2 hybridized carbon, as expected from SWCNT films. The aniline-connected network contains a strong N1s peak at 400 eV, with nitrogen atoms equal to 1.8 at(%), giving an estimate of one grafted crosslinker per 53 SWCNT carbon atoms, confirming the presence of binding sites in the sample. XPS of the crosslinked films reveals small amounts of residual iodine and bromine in the p-DIB and BocDBA functionalized films, respectively, indicating a small number of mono-grafted species present in the sample.
[0228] -N2 isotherm / BET N2 porosimetry revealed that the crosslinked aerogel bulk monoliths were mesoporous materials with characteristic type IV isotherms distinguished by adsorption-desorption hysteresis (Figure 12). The HiPco starting material exhibited a BET specific surface area (SSA) of 443 m2 g-1, significantly smaller than the theoretical limit of 1315 m2 g-1 for closed SWCNTs, reflecting the highly bundled state of the material observed by SEM. An SSA of 657 m2 g-1 was recorded for the non-crosslinked bulk monolith, a substantial increase in active surface relative to the pristine SWCNTs, highlighting the effectiveness of the reductive dissolution pathway in exfoliating the bundles and preserving the open network. The aniline crosslinked network had a BET specific surface area (SSA) of 747 m2 g-1, while the phenyl crosslinked aerogel exhibited a larger SSA of 956 m2 g-1. Both crosslinked networks exhibited a larger active surface than the non-crosslinked aerogels, reiterating the importance of the crosslinking step in preserving the open microstructure. The larger SSA of the phenyl network compared to the aniline network reflects the higher crosslinking yield observed. The added structural bonds fix the SWCNT framework in a defined position, preventing collapse and improving the SSA, which reinforces the observations carried out with SEM on the altered microstructure. The pore size distribution of the crosslinked aerogels again shows that the network contains mainly mesopores.
[0229] N of crosslinked aerogel monoliths 2 The sorption isotherm gives 956±2 m for the phenyl-bridged network. 2 g -1(Figure 12(c)). This shows an increase over the non-crosslinked control due to the presence of structural crosslinks that anchor the SWCNT framework in a defined position. The observed difference between the two crosslinked samples is due to a higher number of crosslinks grafted to the SWCNT sidewalls. At higher magnification, scanning electron microscopy (SEM) of the aerogel thin film reveals a highly interconnected random network of small diameter bundles (Figure 13(c-e)). In both crosslinked cases, a fine and uniform pore structure is observed, while in the absence of crosslinker, a coarser network is seen and a greater degree of rebundling is evident, which is also reflected in the SSA. When the average pore size of the crosslinked network is around 5 nm, a high surface area is achieved while maintaining sufficient spacing for efficient gas diffusion throughout the structure. A summary of the characterization data for each crosslinked network, as well as the non-crosslinked control and the degassed starting material, is shown in Table 1.
[0230] [Table 1]
[0231] Example 2 - Layer-by-layer deposition method Materials and Methods Purified HiPco was purchased from Nanointegris and purified under high vacuum for 10 min before being introduced into the glove box. -6 The mixture was degassed at 500 °C for 10 h at 1000 mbar. Sodium (99.95% ingot), DMAc (anhydrous 99.8%), naphthalene (99%) and p-diiodobenzene (99%) were purchased from Sigma Aldrich Ltd. (UK). Isopropanol and deionized water were purchased from VWR Ltd. (USA). Dry air (O 2 / N 2 20 / 80 v / v) was purchased from BOC. Reductive dissolution and molecular nanolayer deposition were carried out under inert conditions in a glove box (Braun, O 2 <0.1ppm, H 2All reactions were carried out at room temperature, and the multilayer films used for Raman spectroscopy were deposited on silicon wafers.
[0232] Reductive dissolution A bulk "nanotubide" solution was prepared by adding equimolar amounts of sodium ingot (30 mg, 1.30 mmol) and naphthalene (167 mg) to DMAc (15.0 mL), and 2 mg Na mL DMAc -1 The dark green solution was stirred for 18 hours. Then, sodium naphthalide solution (2.24 mL, 2.24 mmol) was added. Na ) was added to degassed SWCNT powder (40 mg) to give a sodium:carbon stoichiometry of 1:10. The solution was then diluted with additional DMAc to give 1.8 mg SWCNT mL DMAc -1 and an optimal [Na] of 15 mM. The solution was stirred overnight with a glass stir bar to obtain a homogenous solution before use.
[0233] Molecular Nanolayer Deposition The reduced SWCNTs were further diluted with DMAc to 0.2 mg mL -1 A mass loading of 100 μL was obtained. The first layer was deposited by spin-coating 200 μL of the diluted SWCNTs onto a glass substrate silanized with 3-iodopropyltrimethoxysilane. The substrate was then coated with 15 mg / mL of the crosslinker p-DIB. -1 The substrate was immersed in the solution for 10 minutes, followed by an additional 5 minutes in pure DMAc. Immersion of the substrate in the bath of nanotubes for 10 minutes, followed again by immersion in pure DMAc for 5 minutes, completed a single crosslinking cycle. Four individual immersions were repeated for each subsequent layer of SWCNTs and crosslinker. The multilayer film was then removed from the glove box and the remaining fill was filled with dry oxygen gas (20:80 O 2 :N 2 v:v) Finally, the film was washed with deionized water and isopropyl alcohol and then dried under a stream of nitrogen.
[0234] Microstructure Helium ion microscopy of the multilayer film reveals a porous network of highly individualized SWCNT species and small bundles. The large degree of individualization reflects the reductive exfoliation pathway, which is very effective in isolating larger bundles. Figure 14A shows the first layer of SWCNTs, and in most areas the film appears to consist of either single nanotubes or very few stacked SWCNTs. After adding the second layer, in the absence of crosslinker (Figure 14b), additional SWCNTs appear to be present on top of the first layer, but the absolute coverage by nanotubes remains almost unchanged. Conversely, the crosslinked film (Figure 14c) shows more addition of SWCNTs to the second layer and a much greater density of carbon material. The amount of material deposited increases when using a crosslinked layer, indicating that covalent grafting is controlling the deposition and is required to anchor a significant amount of SWCNTs to the film.
[0235] By thresholding the microscope image to black and white pixels (FIG. 15), a value for the total coverage of SWCNTs compared to the substrate background can be determined, providing an indication of the amount of SWCNTs present in the second layer. SWCNT ) was determined to be 1.35, but when a second layer was added without a crosslinker, only a slightly higher coverage of 1.44 was calculated. The crosslinked film had a C of 1.81. SWCNT , indicating that much more material is deposited when there are iodine groups available for grafting to the incoming layer.
[0236] Atomic force microscopy (AFM) was utilized to determine the thickness of the first SWCNT layer, then subsequent layers (Figure 16). Similar to HIM, AFM reveals a highly interconnected network of individual SWCNTs and small diameter bundles. The first layer, deposited by spin coating, had a thickness of 4 nm to 6 nm with a roughness of 1.6 nm. Upon addition of a second layer, the thickness increased to 6 to 9 nm for both crosslinked and non-crosslinked films, but a greater roughness of 2.9 nm was observed in the absence of the crosslinked layer compared to 2.1 nm for the crosslinked film. This is hypothesized to be the result of a grafting reaction with the crosslinker, which pulls the SWCNTs into the plane of the film, reducing roughness. The non-crosslinked film, on the other hand, has more material lying out of plane, increasing roughness. The 2 to 3 nm increase in thickness with the addition of the second layer suggests that the reaction terminates with the depletion of carbon-halide bonds after a single layer of SWCNTs is added.
[0237] UV-visible spectroscopy To reinforce the contention that the crosslinking reaction controls the deposition, UV-Vis spectroscopy was performed (Figure 17). A prominent Van Hove single band was observed in the film, again reflecting the high degree of individualization observed through microscopy. The presence of these discrete energy levels is typically observed in solution, but their presence in the solid state indicates that molecular layer deposition precludes significant rebundling. The transmittance of the SWCNT film at 550 nm gives a good indication for the amount of material present in the film. A larger reduction in transmittance is observed for the crosslinked bilayer than for the non-crosslinked film, reaffirming the role of crosslinking in controlling the deposition. A linear decrease in transmittance is observed for each subsequent layer up to a total of 10 layers, demonstrating the degree of control that can be achieved over film thickness and transparency (Figure 17b,c).
[0238] Raman spectroscopy The properties of MNDs were further probed by Raman spectroscopy, a technique that measures vibrational modes, allowing the determination of the types of bonds present in the structure. -1 The defect induced modes that appear in2 It is an indicator of damage to the carbon lattice and is expressed as 1600 cm -1 The ratio of this peak to the graphite peak (I D / I G + ) is used to determine the degree of sidewall functionalization. Statistical Raman spectroscopy shows that the average I D / I G + This confirms the functionalization of the first SWCNT layer with the cross-linking reagent, as the I shifts from 0.11 ± 0.015 to 0.17 ± 0.016 (Figure 18b). The cross-linked bilayer exhibits a smaller D band than the mono-functionalized SWCNT layer, indicating that additional SWCNT material has been deposited. The I of 0.13 ± 0.010 D / I G + is larger than that observed for the single layer, indicating reaction with residual halide groups in the first layer.
[0239] A method for layer-by-layer molecular nanolayer deposition (MND) of highly interconnected cross-linked SWCNT films utilizing reductive cross-linking chemistry is reported herein. Assembling films layer-on-layer provides a route to hierarchical structures with highly tunable cross-functionality, such as electrical conductivity, optical transmittance and thickness. Reductive dissolution yields a solution of highly individualized species, which can be assembled into multilayer films via cross-linking with dielectrophiles. A combination of AFM, HIM, UV-Visible and Raman spectroscopy was used to characterize the deposition process, revealing that covalent reactions with cross-linkers drive the deposition of SWCNTs. The layer-by-layer approach offers very tight control over the film properties, with thickness and transparency varying depending on the number of layers. Furthermore, the room temperature reaction conditions and simple bath dip coating process facilitate the potential scale-up of the deposition. The methods presented may be applied to thin films for a range of different potential applications, from photovoltaic devices, sensors and catalysts to conductive inks and coatings.
[0240] Example 3 - Gas Sensing Gas Sensing Measurement The SWCNT samples were placed in a custom-made flow cell and the resistance was recorded using 4-wire measurements while exposed to various gas analytes (Keysight 4410A DMM). The gas mixtures were measured using a reconditioned KinTek H 2 The permeation and diffusion tubes were generated using nitrogen carrier gas in an O Span Pac.
[0241] The sensor was zeroed by heating to 100° C. under nitrogen flow. Measurements were taken with a continuous 6 min exposure of analyte followed by 6 min exposure of pure carrier gas. Analyte concentration was adjusted by controlling the temperature of the permeation device and the dilution gas flow rate.
[0242] Analytical response to amines The aerogel films were fashioned into the active components of chemiresistor gas sensors by contacting the SWCNT surface with source and drain contact probes. Gas analytes at various concentrations ranging from low parts per billion (ppb) to parts per million (ppm) were delivered to the sensor in a dry nitrogen carrier gas. The phenyl-bridged network showed high sensitivity to odorous amines, ammonia, n,n-dimethylethylamine (DMEA) and triethylamine (TEA) (Figure 19). Ammonia was detected at concentrations as low as 0.1 ppm for both the uncrosslinked and phenyl-bridged networks. Both DMEA and TMEA elicit strong responses from 55 ppm to 4.5 ppm and from 32 ppm to 2 ppm, respectively. Since the phenyl bridges do not contain functional groups that contribute significantly to analyte binding, signal transduction is caused by the adsorption of amines to the SWCNT surface. The tendency for resistance to increase is explained by the electronic structure of the SWCNTs, where the surface adsorption of amines causes a partial charge transfer of electrons to the SWCNT network. This reduces the availability of holes, the main charge carriers in the p-type network, limiting the electrical conductance. Extremely high sensitivity was observed, which can be attributed to the reductively exfoliated and subsequently crosslinked SWCNTs, which offer a large surface for amine adsorption.
[0243] The non-crosslinked networks still show good performance, but considering that they still undergo the same individualization process, the device sensitivity is still measurably lower than when crosslinkers were used to prevent rebundling. Another reason for the enhanced sensitivity of the more individualized sensor networks could be the greater number of CNT junctions. In highly conductive networks, the conductivity is limited at the tube-tube junctions, so perturbing the electronic structure at these locations gives a more pronounced response. A greater degree of rebundling makes the intratube sensing response the dominant effect, whereas in more exfoliated crosslinked networks, the intratube effect is more dominant.
[0244] Volatile acid sensing Further investigations were carried out into the gas sensing behavior of the aerogel films with the VOCs acetic acid and isovaleric acid. Networks crosslinked with aniline bridges were utilized in an attempt to both increase the binding affinity for acid molecules using free amine sites and to localize the binding event to the tube junctions and increase the dominance of the intertube sensing mechanism. Boc-protected aniline was used in the synthesis to facilitate grafting between C-Br and the charged SWCNT surface and eliminate unwanted side reactions at the nitrogen-containing groups. Free amines were detected by XPS (Table 1), indicating the presence of selective binding sites in the samples. Upon exposure to acetic acid, a strong signal was observed and significant linear resistance changes were seen both from 1 ppm up to 16 ppm (Figure 20(a)) and at lower concentrations ranging from 0.15 ppm to 2.4 ppm. The increase in conductivity contrasts with the effect seen upon exposure to amine molecules and favors the explanation of charge transfer from the SWCNTs to the adsorbed electron-withdrawing acid. The reduction in electron density increases the hole conductivity in the network, inducing a response in the form of lower resistance. A significant increase in sensitivity is observed compared to aerogel films without aniline crosslinks. This increase indicates that there is additional adsorption of acid onto the network due to complementary interactions between the free amine binding sites and the adsorbed acid. In addition, if an acetic acid molecule is interacting at the amine sites, there is a charge transfer from the conjugated network, giving a larger sensing response in addition to the doping effect. By positioning the analyte binding site at the intertube junction, a single binding event can modulate the transport along the entire permeation path. It is hypothesized that this type of binding induces a larger response than adsorption at sidewall locations where electrical transport is not limited. Although the network without the selector moiety is still highly sensitive to acetic acid in the low ppm range, the sensitivity is reduced by a factor of 2-3, highlighting the important role that the amine functional group plays in the response.
[0245] Similar behavior was observed with isovaleric acid, another low molecular weight carboxylic acid, where a measurable decrease in resistance was found as low as 7 ppb, with a linear response covering a dynamic range up to 110 ppb. Control networks lacking the aniline linker showed no significant resistance change up to exposure to 28 ppb, with a smaller % resistance change than the aniline-crosslinked samples.
[0246] The aniline cross-linked aerogel film sensor was reproducible and stable for periods longer than 6 months. Similar behavior was observed for both acid analytes, indicating the same linkage between the molecule and the SWCNT network, pointing to charge transfer from the carboxyl groups. By extrapolating the dynamic range of the acetic acid response, the detection limit appears to be in the same region as isovaleric acid. The detection limit reaches 7 ppb, the detection limit of the human olfactory system, which has evolved over millennia to be extremely sensitive to such harmful malodorous compounds. By enhancing the sensitivity to acid molecules, a degree of selectivity was imparted to the sensing material.
[0247] The full dynamic range of both types of aerogel thin film sensors shows sensitivity to both electron-rich and electron-deficient analytes over a wide concentration range from low ppb to ppm (Figure 19). It shows a linear relationship between analyte concentration and measured resistance response for each measured analyte, allowing for quantification of gases in real samples. The opposite trends seen for acid and amine analytes indicate a charge transfer mechanism.
[0248] The work function of the aerogel films is determined by ambient pressure photoelectron spectroscopy (APS), in which surface electrons are liberated by the photoelectric effect. The onset energy of the photoemission provides the work function energy.
[0249] In summary, a unique aerogel thin film deposition has been demonstrated in which a solution of reduced carbon nanotubes (SWCNTs) is crosslinked into a three-dimensional network. The SWCNT aerogel films show a high degree of individualization with a uniform mesoporous structure. These properties observed in the active material resulted in a chemical sensor that is highly sensitive to a variety of acid and amine gases in the ppb range. Functionalization with free amine binding sites enhances the sensitivity to acid compounds and confers some selectivity for this class of molecules. The shift in Raman G peak position and the opposite change in resistance for the two classes of compounds indicate that the signal transduction differs depending on the chemical doping from the adsorbed analyte molecules. By modifying the crosslinking motif, this network structure may be applied to the selective sensing of any class of analyte. The high sensitivity coupled with the ease of selector attachment means that this technology can be used to develop effective solid-state gas sensors.
[0250] Example 4 MND Gas Sensing A molecular nanolayer deposition (MND) process was applied with BocDBA to form aniline-crosslinked multilayer films, which were exposed to low concentrations of acetic acid vapor to evaluate the utility of the new structure in solid-state gas sensors.
[0251] The 6-layer MND film showed high sensitivity, inducing a resistance change of 1.3% when exposed to 2.5 ppm of AcOH (Figure 22). The device showed a significant resistance response of 0.18% at a low AcOH concentration of 0.16 ppm, with minimal signal noise. The resistance response was highly linear over the measured concentration range. The sensing response of this device was used to plot the linear range, allowing the determination of the LoD. The high sensitivity and low noise resulted in a theoretical detection limit of 10 ppb, well above the odor threshold. Also, the response was highly reversible, with the initial resistance almost completely recovered after a 6-minute cycle of pure nitrogen.
[0252] Values disclosed herein as range endpoints should not be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each numerical range is intended to mean both the recited value, any integer within the stated range, and any range having a stated range. For example, a range disclosed as "1 to 10" is intended to mean "1, 2, 3, 4, 5, 6, 7, 8, 9, and 10." Every maximum numerical limitation given throughout this specification should be understood to include every lower numerical limitation, as if such lower numerical limitations were expressly written herein. Every minimum numerical limitation given throughout this specification should be understood to include every higher numerical limitation, as if such higher numerical limitations were expressly written herein. Every numerical range given throughout this specification includes every narrower numerical range that falls within such broader numerical range, as if such narrower numerical ranges were all expressly written herein.
[0253] Values disclosed herein as range endpoints should not be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise specified, each numerical range is intended to mean both the recited value, any integer within the stated range, and any range having a stated range. For example, a range disclosed as "1 to 10" is intended to mean "1, 2, 3, 4, 5, 6, 7, 8, 9, and 10."
[0254] Dimensions and values disclosed herein should not be understood as being strictly limited to the exact numerical values recited. Instead, unless otherwise indicated, each such dimension is intended to mean both the recited value and a functionally equivalent range surrounding that value. For example, a dimension disclosed as "40 mm" is intended to mean "about 40 mm."
[0255] All documents cited herein, including any cross-referenced or related patents or patent applications, and any patent applications or patents to which this application claims priority or benefit, are incorporated herein by reference in their entirety, unless expressly stated to the contrary. The citation of any document shall not be deemed to be prior art to any invention disclosed or claimed herein, or to teach, suggest or disclose such invention, either alone or in combination with any other reference(s). Furthermore, to the extent that any meaning or definition of a term in this document conflicts with any meaning or definition of the same term in a document incorporated by reference, the meaning or definition assigned to that term in this document shall govern.
[0256] While particular embodiments of the present disclosure have been illustrated and described, it would be obvious to those skilled in the art that various other changes and modifications can be made without departing from the spirit and scope of the invention. It is therefore intended to cover in the appended claims all such changes and modifications that are within the scope of this invention.
Claims
1. 1. A system for utilizing a consumer product, comprising: a central communication unit capable of receiving incoming signals and transmitting outgoing instructions, communicatively connected to a memory configured to store an algorithm; a sensor communicatively connectable to the central communication unit and configured to transmit an incoming signal to the central communication unit alerting the central communication unit of an identity and concentration of a target gas of interest, the sensor comprising a bridged carbon nanotube network comprising a plurality of carbon nanotubes and at least one linker covalently linking adjacent carbon nanotubes, the bridged carbon nanotube network being an aerogel; A consumer product capable of enhancing or mitigating the target gas of said subject. A system comprising:
2. 2. The system of claim 1, wherein the consumer product is communicatively connectable to the central communication unit via a wireless communication link, and the algorithm controls the consumer product using incoming signals transmitted from the sensor to the central communication unit.
3. 3. The system of claim 1 or 2, wherein the consumer product is selected from the group consisting of an air freshener device, an air purification device, a toothbrush, a razor, a diaper, a feminine care product, a cleaning implement, and combinations thereof.
4. The system of any one of claims 1 to 3, wherein the plurality of carbon nanotubes are single-walled carbon nanotubes.
5. 5. The system of claim 1, wherein the plurality of carbon nanotubes are bonded into a series of parallel layers, and optionally the bridged carbon nanotube has an in-plane electrical conductivity greater than its through-thickness electrical conductivity.
6. The linker has the structure * -A- * wherein A is a divalent conjugated system comprising one or more aryl or heteroaryl rings; * The system of any one of claims 1 to 5, wherein is a point of attachment to the carbon nanotube.
7. A, 【Chemistry 1】 and During the ceremony, each ring B is independently an optionally substituted aryl or heteroaryl; Ring C is an optionally substituted porphyrin ring; n is an integer from 1 to 5; * indicates a point of attachment to the carbon nanotube; Optionally, each ring B is independently 【Chemistry 2】 and / or 【Chemistry 3】 may be 7. The system of claim 6, wherein M is Zn, Cu, Ni or Co, each of which may be optionally substituted.
8. The one or more aryl or heteroaryl rings are 1 ~C 20 Alkyl, amino (including alkylamino and dialkylamino), carboxylic acid, amino-C 1 ~C 6 Alkyl, C 1 ~C 6 Alkyl-COOH and -NHC(S)(NH 2 8. The system of claim 7, wherein the compound is substituted with one or more of the following substituents: a noble metal nanoparticle, a porphyrin, a calix[4]arene, or a crown ether.
9. The linker has the structure: 【Chemistry 4】 The system according to any one of claims 1 to 8, wherein M is Zn, Cu, Ni or Co.
10. The linker has the structure * -Y- * wherein Y is a multivalent rigid linker; * The system of any one of claims 1 to 9, wherein is a point of attachment to the carbon nanotube.
11. The system of claim 10 , wherein Y comprises a cycloalkyl group or a polyoctahedral silsesquioxane.
12. The system of any one of claims 1 to 11, wherein the plurality of carbon nanotubes form a film, the film being provided on a substrate.
13. The system of claim 12, wherein the film has a thickness of about 1 nm to about 500 nm.
14. The system of claim 2 , wherein the wireless communication link is selected from the group consisting of Wi-Fi, Bluetooth, ZigBee, 6 LoWPAN, Thread, a mesh network, or a combination thereof.
15. 15. The system of any one of claims 1 to 14, further comprising additional sensors for measuring temperature, relative humidity, indoor air quality, outdoor air quality, noise, human presence, movement, indoor air velocity, particle concentration in the air, allergens, and / or other airborne substances.
Citation Information
Patent Citations
Conductive carbon nanotube with interspersed metal, and manufacturing method of biosensor using it
JP2005003687A
Carbon nanotube composite
JP2005162790A
System and method for combining the operation of an air treatment device and a volatile composition dispenser
JP2019501354A
Electrical response using nanotubes on a fibrous substrate
US10031097B1
Analyte sensors having nanostructured electrodes and methods for making and using them
US20090198117A1