Method for reducing selenium(VI) compounds and method for recovering selenium
A solid catalyst with a platinum group element on a carrier facilitates a mutual redox reaction between selenium (VI) and arsenic (III) compounds, addressing inefficiencies and environmental concerns in existing methods by enabling simultaneous reduction and recovery of both elements.
Patent Information
- Application Number
- JP2020136749
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-13
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-08-13
AI Technical Summary
Existing methods for reducing selenium (VI) compounds are inefficient, costly, and environmentally harmful due to the use of rare and expensive catalysts, and require separate processes for arsenic and selenium recovery, which often coexist in smelting processes.
A method utilizing a solid catalyst with a platinum group element supported on a carrier, such as titanium (IV) oxide, to facilitate a mutual redox reaction between selenium (VI) and arsenic (III) compounds in an aqueous solution, allowing simultaneous reduction and recovery without external oxidizing or reducing agents.
This method effectively reduces selenium (VI) to elemental selenium and oxidizes arsenic (III) to arsenate, enabling efficient and cost-effective separation and recovery without additional chemicals, suitable for industrial applications.
Smart Images

Figure 0007572671000001 
Figure 0007572671000002 
Figure 0007572671000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for reducing selenium (VI) compounds and a method for recovering selenium using said reduction method. [Background technology]
[0002] Ores containing non-ferrous metals are broadly divided into oxide ores and sulfide ores. However, sulfide ores contain toxic elements such as arsenic and selenium as impurities, so it is necessary to efficiently separate these elements during the ore smelting process.
[0003] In the case of arsenic, in the form of arsenate, a typical arsenic(V) compound, it forms arsenates with many metal ions that have low solubility in water, and can be separated as precipitates. In the case of selenium, in the form of elemental selenium it does not dissolve in water and can be completely separated and recovered from the aqueous solution. Therefore, methods of separating, recovering, and removing selenium by converting it into these forms are widely used industrially.
[0004] However, the arsenic compounds produced by the dry smelting of sulfide ores are almost entirely arsenic (III) compounds, such as diarsenic trioxide and its hydrate, arsenous acid, which are difficult to react with cations to form precipitates with low solubility. The compounds produced by dry smelting of selenium are selenium dioxide, which is easily reduced to simple selenium, and selenious acid, which is its hydrate, but in the wet smelting that has been widely adopted in recent years, strong oxidizing agents such as chlorine are used to dissolve selenium, so most of the selenium exists in the form of compounds containing selenium (VI), which is difficult to reduce, such as selenic acid.
[0005] Since it is difficult to oxidize arsenic(III) compounds to arsenic(V) and reduce selenium(VI) compounds to selenium(0) (elementary selenium), a method of oxidation using oxygen at high temperature for a long time has long been used to oxidize arsenic(III) compounds to arsenic(V). However, this method is disadvantageous in terms of both energy and reaction time because of the high temperature required. In addition, the reduction of selenium(VI) compounds is generally performed using sulfur dioxide at high temperature for a long time in the presence of high concentration of sulfuric acid, but this method is not suitable from the viewpoint of energy required for high temperature, as well as the use of large amount of sulfuric acid and the cost of neutralizing agent.
[0006] Here, the standard electrode potential (@pH0) between HAsO2 / H3AsO4 is 0.560 V, and the standard electrode potential (@pH0) between H2SeO3 / HSeO4 is 0.560 V. - The standard electrode potential (@pH0) between the two is 1.09V, so in equilibrium theory, the reduction of arsenic acid to arsenous acid and the reduction of selenic acid to selenite should proceed easily. However, in reality, the reaction does not proceed easily, which is thought to be due to the low reaction rate (high activation energy). Therefore, the use of catalysts is being considered to improve the reaction rate.
[0007] For example, Patent Document 1 discloses a method for reducing selenite ions to elemental selenium with sulfur dioxide using iodide ions as a catalyst, while Patent Document 2 discloses a method for promoting the reaction of oxidizing arsenite ions in an aqueous solution to arsenate ions with oxygen using a catalyst supported with platinum particles on titanium oxide (IV) or zirconium oxide (IV) as a carrier.
[0008] Patent Document 3 discloses a method for reducing selenium (VI) in an aqueous solution with hydrazine monohydrate to elemental selenium using a catalyst carrying rhodium, platinum, palladium, iridium, or ruthenium particles on a support made of titanium (IV) oxide, zirconium (IV) oxide, aluminum oxide, silicon dioxide, or a mixture thereof (composite oxide). [Prior art documents] [Patent documents]
[0009] [Patent Document 1] JP 2019-73767 A [Patent Document 2] JP 2015-151289 A [Patent Document 1] JP 2016-190221 A Summary of the Invention [Problem to be solved by the invention]
[0010] However, in the method disclosed in Patent Document 1, the iodine used as the catalyst is a rare element and is expensive. In addition, although the iodine functions as a catalyst, the entire amount of the catalyst is discharged into wastewater in the process, and therefore the catalyst cannot be reused.
[0011] The method disclosed in Patent Document 2 uses a water-insoluble solid catalyst, which is different from the technology in Patent Document 1, and therefore allows for reuse. However, oxygen is required as an oxidizing agent, and when a large amount of aqueous solution is rapidly and continuously treated, particularly in the non-ferrous smelting industry, there may be cases where oxygen cannot be sufficiently supplied and dissolved, resulting in insufficient oxidation.
[0012] The method disclosed in Patent Document 3 also uses a water-insoluble solid catalyst, which allows for reuse. However, since a separate reducing agent is used, the cost of the reducing agent is required, and if the amount of the reducing agent used exceeds the required amount, the COD and BOD of the wastewater increase, which may have an environmental impact, and to prevent this, another oxidation treatment is required.
[0013] Furthermore, the methods disclosed in Patent Documents 1 to 3 have a common problem in that they are processes specialized for reduction or oxidation, and therefore require separate processes for separating and recovering arsenic and selenium, which often coexist in the smelting process.
[0014] The present invention has been made in consideration of the above circumstances, and provides a method that enables effective and efficient reduction, separation, and recovery of selenium (VI) compounds, which are difficult to treat, without the addition of an external oxidizing or reducing agent. [Means for solving the problem]
[0015] The present inventors have conducted extensive research to solve the above-mentioned problems, and as a result, have found that the selenium (VI) compound to be treated and the arsenic (III) compound, which is also a difficult-to-treat compound, can be treated simultaneously in the presence of a solid catalyst by utilizing a mutual oxidation-reduction reaction between the two compounds, and that the selenium (VI) compound can be effectively reduced and the elemental selenium obtained by reduction can be efficiently recovered, thereby completing the present invention.
[0016] (1) The first aspect of the present invention is a method for reducing a selenium (VI) compound contained in an aqueous solution, comprising reducing selenium (VI) in the aqueous solution with an arsenic (III) compound coexisting in the aqueous solution in the presence of a catalyst comprising a platinum group element supported on a carrier.
[0017] (2) A second aspect of the present invention is a method for reducing a selenium compound according to the first aspect of the present invention, comprising mixing an aqueous solution containing the selenium (VI) compound with a liquid containing the arsenic (III) compound, thereby causing the arsenic (III) compound to coexist in the aqueous solution.
[0018] (3) A third aspect of the present invention is a method for reducing a selenium compound according to the first or second aspect of the present invention, wherein the pH of the aqueous solution is adjusted to a range of 1.0 or more and 10 or less.
[0019] (4) A fourth aspect of the present invention is a method for reducing a selenium compound according to any one of the first to third aspects of the present invention, wherein the platinum group element includes at least one selected from platinum, palladium, and rhodium.
[0020] (5) A fifth aspect of the present invention is a method for reducing a selenium compound according to any one of the first to fourth aspects of the present invention, wherein the support contains titanium(IV) oxide.
[0021] (6) A sixth aspect of the present invention is the method for reducing a selenium compound according to any one of the first to fifth aspects, wherein the aqueous solution is acidic with sulfuric acid.
[0022] (7) A seventh aspect of the present invention is a method for reducing a selenium compound according to any one of the first to sixth aspects of the present invention, wherein the reduction is carried out under conditions that do not include atmospheric oxygen and an oxidizing agent other than the arsenic (III) compound.
[0023] (8) An eighth aspect of the present invention is a method for reducing a selenium compound according to any one of the first to seventh aspects, wherein the catalyst is reduced with a reducing agent prior to use of the catalyst.
[0024] (9) A ninth aspect of the present invention is a method for recovering selenium from an aqueous solution containing a selenium (VI) compound, the method comprising: a reduction step of reducing selenium (VI) in the aqueous solution with an arsenic (III) compound coexisting in the aqueous solution in the presence of a catalyst comprising a platinum group element supported on a carrier; and a recovery step of recovering the produced elemental selenium by solid-liquid separation.
[0025] (10) A tenth aspect of the present invention is the method for recovering selenium according to the ninth aspect of the present invention, wherein in the reduction step, an aqueous solution containing the selenium (VI) compound is mixed with a liquid containing the arsenic (III) compound, thereby causing the arsenic (III) compound to coexist in the aqueous solution.
[0026] (11) An eleventh aspect of the present invention is the method for recovering selenium according to the ninth or tenth aspect of the present invention, further comprising, after the recovery step, an arsenate recovery step of converting arsenate ions remaining in the aqueous solution after the solid-liquid separation into arsenate by adding a cation to the aqueous solution and recovering the arsenate by solid-liquid separation.
[0027] (12) A twelfth aspect of the present invention is a method for recovering selenium according to the ninth or tenth aspect of the present invention, further comprising an arsenate generation step of converting arsenate ions generated in the aqueous solution into arsenate by adding a cation to the aqueous solution after the reduction step, and recovering a mixture of elemental selenium generated in the aqueous solution and the arsenate by solid-liquid separation in the recovery step. Effect of the Invention
[0028] According to the present invention, it is possible to provide a method that enables effective and efficient reduction, separation, and recovery of selenium (VI) compounds, which are difficult to treat, without adding an external oxidizing agent or reducing agent. [Brief description of the drawings]
[0029] [Figure 1] 1 is a graph showing the test results of Example 1, illustrating the relationship between the type of carrier constituting the catalyst and the reduction rate of selenium (VI). [Diagram 2] 1 is a graph showing the test results of Example 1, illustrating the relationship between the type of carrier constituting the catalyst and the oxidation rate of arsenic (III). [Diagram 3] 1 is a graph showing the test results of Example 2, illustrating the relationship between pH conditions and the reduction rate of selenium (VI). [Figure 4] 1 is a graph showing the test results of Example 2, illustrating the relationship between pH conditions and the oxidation rate of arsenic (III). [Diagram 5] 1 is a graph showing the test results of Example 3, illustrating the relationship between the presence or absence of pretreatment for prior reduction of the catalyst and the reduction rate of selenium (VI). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] Hereinafter, specific embodiments of the present invention will be described in detail. Note that the present invention is not limited to the following embodiments, and various modifications are possible without departing from the spirit and scope of the present invention.
[0031] ≪1. Method for reducing selenium compounds≫ The method for reducing a selenium compound according to the present embodiment is a method for reducing a selenium (VI) compound contained in an aqueous solution to selenium (0) (elemental selenium).
[0032] Specifically, this reduction method is characterized in that a selenium (VI) compound (selenic acid) in an aqueous solution is reduced by an arsenic (III) (arsenous acid) compound coexisting in the same aqueous solution in the presence of a catalyst made of a platinum group element supported on a carrier. That is, in this method, a selenium (VI) compound and an arsenic (III) compound coexisting in the aqueous solution are treated simultaneously by utilizing a mutual oxidation-reduction reaction between the selenium (VI) compound and the arsenic (III) compound, which coexist in the aqueous solution, to reduce the selenium (VI) compound.
[0033] According to this method, since a water-insoluble solid catalyst is used, it is possible to reuse the catalyst, and since an arsenic (III) compound contained in the same aqueous solution is used as a reducing agent, the selenium (VI) compound can be effectively reduced to elemental selenium without adding a separate reducing agent. In addition, the arsenic (III) compound used as a reducing agent is also a difficult-to-treat compound, but since the arsenic (III) compound is effectively oxidized by using the arsenic (III) compound as a reducing agent, the arsenic (III) compound can be effectively treated (treated to arsenate ions) without adding a separate oxidizing agent.
[0034] For example, in the process of smelting sulfide ores of nonferrous metals such as copper, lead, zinc, nickel, and cobalt, the process liquid and waste liquid discharged from the process, and the aqueous solution (waste liquid) obtained through wet processing in the exhaust gas treatment process contain arsenic (III) compounds as well as selenium (VI) compounds. Therefore, by reducing selenium (VI) compounds in the aqueous solution of such process liquid with arsenic (III) compounds, selenium (VI) can be effectively reduced to elemental selenium and recovered. At the same time, arsenic (III) compounds can also be effectively oxidized (treated to arsenate ions) and recovered.
[0035] In addition, in a waste liquid treatment process, for example, a waste liquid containing a selenium (VI) compound discharged from a precious metal treatment process and a waste liquid containing an arsenic (III) compound discharged from an arsenic concentration process may be mixed and supplied. Therefore, even in such a mixed aqueous solution of waste liquids, selenium (VI) can be effectively reduced to elemental selenium and recovered by reducing the selenium (VI) compound with an arsenic (III) compound, and at the same time, the arsenic (III) compound can also be effectively oxidized and recovered.
[0036] [About the catalyst] In the method for reducing a selenium compound according to the present embodiment, a solid catalyst is used. More specifically, a catalyst in which particles of a platinum group element are supported on a carrier is used. In this reduction method, the solid catalyst serves as a reduction catalyst (hereinafter also referred to as a "selenic acid reduction catalyst") for reducing selenic acid (selenium (VI) compound) and also serves as an oxidation catalyst for oxidizing arsenous acid (arsenic (III) compound).
[0037] In this way, by using a solid catalyst in which particles of a platinum group element are supported on a carrier, it becomes possible to reuse the catalyst since it is insoluble in water, and efficient processing can be performed.
[0038] (Support material) The platinum group element particles (supporting material) constituting the catalyst include particles of one or more metal elements selected from the group consisting of platinum, palladium, and rhodium. Although particles of these metal elements can fully exert the effect as a catalyst, it is particularly preferable to use rhodium from the viewpoint of exerting a more excellent catalytic activity.
[0039] The amount of platinum group element particles (support material) supported (amount supported on the carrier described below) is not particularly limited, but is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, and even more preferably 0.8 mass% or more, based on the dry mass of the carrier. If the amount supported is too small, the efficiency of reducing selenic acid (reduction efficiency) may be insufficient.
[0040] In addition, the upper limit of the loading amount is not particularly limited. However, if the loading amount is too large, the dispersion degree of the particles of the platinum group element, which is the loading material, is insufficient, which may affect the reduction efficiency per unit mass of the loading material. Furthermore, considering that the loading material is a particle of a platinum group element and is a high-cost material, it is preferable to consider not only the apparent reduction efficiency but also the reduction efficiency per unit mass of the loading material. From this viewpoint, the upper limit of the loading amount is preferably 20 mass% or less, more preferably 15 mass% or less, and even more preferably 10 mass% or less, based on the dry mass of the carrier.
[0041] The particle size of the platinum group element particles is not particularly limited, but is preferably as small as possible, and specifically, is preferably 20 nm or less, more preferably 10 nm or less, and even more preferably 3 nm or less.
[0042] (Carrier) The carrier constituting the catalyst is preferably one or more carriers selected from the group consisting of aluminum oxide, titanium (IV) oxide, and silicon dioxide. In general, solutions and waste liquids containing selenium (VI) compounds are often acidic. Therefore, the carrier needs to be a material that can suppress dissolution in the acidic range and can enhance the catalytic effect of the above-mentioned support material. In addition, from the viewpoint of economy, it is more preferable that the carrier is a material that is inexpensive and can be easily supplied in large quantities.
[0043] From these viewpoints, as described above, the carrier constituting the catalyst is preferably aluminum oxide, titanium(IV) oxide (TiO2), or silicon dioxide (silica, SiO2), and it is particularly preferable that the carrier contains titanium(IV) oxide, since this can further enhance the reduction catalytic activity for reducing selenium(VI) compounds.
[0044] (Catalyst manufacturing method) The method for producing the catalyst described above is not particularly limited, and can be produced by a known method. For example, a method of impregnating a support such as titanium oxide (IV) with a solution containing one or more platinum group elements, drying, and calcining can be mentioned. In addition, a method of repeatedly impregnating with a dilute solution containing a platinum group element, an incipinent wetness method in which a solution containing a platinum group element at a high concentration close to the limit, a spray drying method, etc. can be mentioned.
[0045] The amount of platinum group element particles (support material) supported on the support can be adjusted by the amount of platinum group element solution on the support, the platinum group element concentration in the solution, the impregnation time of the support in the solution containing the platinum group element, etc. From this viewpoint, the platinum group element concentration in the solution is preferably 0.5 g / L or more and 200 g / L or less, more preferably 1 g / L or more and 100 g / L or less, and even more preferably 3 g / L or more and 100 g / L or less.
[0046] In addition, the degree of dispersion of the platinum group element particles (support material) can be further adjusted by measuring the degree of dispersion of a catalyst (selenate reduction catalyst) supported in a suitable range of amounts, or by controlling the strength of stirring when supporting the support material on the carrier.
[0047] In the method for producing a catalyst, drying and calcination are performed to remove components other than metal from the metal raw material and form fine particles on the carrier. The drying process is not particularly limited as long as the liquid components contained in the solution containing the platinum group element can be evaporated. The calcination process is not particularly limited as long as fine particles of an appropriate metal particle size are formed. However, when calcination is performed in a reducing atmosphere such as in the presence of hydrogen, the subsequent pre-reduction process can be omitted. On the other hand, when calcination is performed in an inert gas atmosphere or an oxidizing atmosphere, a process for reducing the platinum group element is required. In addition, when a catalyst preparation method is used in which a precursor of the platinum group element, which is a support material, is reduced in a liquid phase to precipitate and fix particles of the platinum group element on the carrier, drying and calcination processes are not required.
[0048] (Pretreatment for catalyst) As described above, the catalyst obtained by calcination in the presence of hydrogen can be used immediately after the calcination treatment, whereas the catalyst obtained by calcination in an inert gas atmosphere or an oxidizing atmosphere can be subjected to a reduction treatment (pre-reduction treatment) with a reducing agent before use to enhance the catalytic activity.
[0049] Specifically, the reduction treatment as a pretreatment prior to the use of the catalyst is preferably carried out using a reducing agent capable of reducing the oxide of a platinum group element, which is the support material constituting the catalyst, to an elemental metal (particles). Examples of the reducing agent include hydrogen, oxalic acid, citric acid, methanol, ethanol, formaldehyde, hydrazine, and sodium borohydride.
[0050] [Method for reducing selenium compounds] In the method for reducing a selenium compound according to the present embodiment, a selenium (VI) compound (selenic acid) in an aqueous solution is reduced by an arsenic (III) (arsenous acid) compound coexisting in the aqueous solution in the presence of the above-mentioned solid catalyst, i.e., a catalyst in which a platinum group element is supported on a carrier. In other words, the selenium (VI) compound and the arsenic (III) compound coexisting in the aqueous solution are treated simultaneously by utilizing a mutual oxidation-reduction reaction between the selenium (VI) compound and the arsenic (III) compound, which coexist in the aqueous solution, to reduce the selenium (VI) compound. This makes it possible to effectively reduce the selenium (VI) compound to elemental selenium and recover it.
[0051] Here, in this reduction method, the subject of treatment is not limited to an aqueous solution in which a selenium (VI) compound and an arsenic (III) compound already coexist, for example, a waste liquid containing a selenium (VI) compound and an arsenic (III) compound discharged from an exhaust gas treatment process in the process of dry smelting of sulfide ore. For example, the present invention also includes an embodiment in which an arsenic (III) compound is made to coexist in an aqueous solution by mixing a waste liquid (aqueous solution) containing a selenium (VI) compound with a waste liquid containing an arsenic (III) compound. In this way, the respective aqueous solutions (waste liquids) can be mixed to allow the reduction reaction and the oxidation reaction to proceed, and the mixing ratio of each aqueous solution at that time can be appropriately adjusted to realize the progress of a more effective oxidation-reduction reaction.
[0052] The selenate ion, a compound of hexavalent selenium, is H2SeO3 / HSeO4 - The standard electrode potential (when pH is changed) between HAsO2 and H3AsO4 is 1.090-0.0886 pH (V), and as the pH decreases, reduction becomes easier in equilibrium. Therefore, lower pH conditions are more advantageous for the reduction of selenium (VI) compounds. On the other hand, the standard electrode potential (when pH is changed) between HAsO2 and H3AsO4 is 0.560-0.0594 pH (V), and as the pH increases, arsenite ions, which are trivalent arsenic compounds, become easier to oxidize in equilibrium.
[0053] Generally, in the redox reaction of oxoacids, both the redox potential and pH are involved in equilibrium theory. In fact, when reduction is performed using a reducing agent alone, the lower the pH, the more the reduction reaction of selenic acid proceeds. However, in this reaction system, as the pH decreases, the dissociation of selenic acid into selenate ions is suppressed and molecular selenic acid is formed, making it easier for the solid catalyst to act, and as a result, the reduction rate increases.
[0054] Therefore, in a method for reducing selenium (VI) compounds (selenic acid) in an aqueous solution with arsenic (III) (arsenous acid) compounds contained in the aqueous solution, that is, a method for reducing selenium (VI) compounds while simultaneously treating both selenium (VI) compounds and arsenic (III) compounds by utilizing their mutual oxidation-reduction reaction, there exists an optimal pH range.
[0055] Specifically, the pH of the aqueous solution is preferably adjusted to a range from acidic to weakly alkaline, 1 to 10, more preferably adjusted to a range from 1.5 to 4.0, and even more preferably adjusted to a range from 1.0 to 3.0. If the pH of the aqueous solution is less than 1.0, the rate of the oxidation reaction of arsenite ions may decrease, resulting in a decrease in the reduction efficiency of the selenium (VI) compound. If the pH of the aqueous solution is more than 10, the rate of the reduction reaction of selenate ions may decrease, resulting in a decrease in the reduction efficiency of the selenium (VI) compound.
[0056] The pH of the aqueous solution can be adjusted by adding an acid. Specifically, sulfuric acid is particularly preferred as the acid to be added to the aqueous solution containing the selenium (VI) compound. When adding an acid, the pH can also be adjusted by using an acid such as hydrochloric acid or nitric acid. However, when hydrochloric acid is used, it may form a complex with the platinum group element and dissolve, and when an oxidizing acid such as nitric acid is used, the reduction reaction of the selenate ion may be hindered and the supported material may be eluted. When the pH of the aqueous solution is adjusted to a weak alkaline region, it may be adjusted by adding a water-soluble alkali such as sodium hydroxide.
[0057] In the method for reducing a selenium (VI) compound according to the present embodiment, the reaction shown in the following reaction formula [1] occurs. As shown in reaction formula [1], selenium (VI) is reduced by 3 times the moles of arsenic (III), so in an anaerobic atmosphere, the reaction proceeds without excess or deficiency by mixing them in a stoichiometric ratio. However, in an industrial context, the inclusion of oxygen from the atmosphere is unavoidable, so the reaction proceeds without excess or deficiency under conditions where an excess of arsenic (III) compounds is present. Se 6+ +3As 3+ → Se(0)+3As 5+ [1]
[0058] In addition, in this reduction method, it is preferable to carry out the reaction under conditions that do not include atmospheric oxygen and oxidizing agents other than arsenic (III) compounds. When atmospheric oxygen and oxidizing agents other than arsenic (III) compounds are present, the supported material made of a platinum group element supported on a support used as a reduction catalyst may be eluted into an aqueous solution, which may result in a decrease in catalytic activity.
[0059] As the redox reaction progresses, the selenium (VI) in the aqueous solution is reduced to elemental selenium (zero valence) and precipitates, and the arsenic becomes arsenate ions. Therefore, after the redox reaction shown in the above reaction formula [1] is completed, selenium can be effectively removed from the aqueous solution by separating the solid precipitate (elemental selenium).
[0060] 2. How to recover selenium As described above, selenium can be effectively reduced and removed from aqueous solutions by reducing selenium (VI) compounds to elemental selenium through the redox reaction shown in reaction formula [1].
[0061] Therefore, the method for recovering selenium using the above-mentioned method for reducing a selenium compound can be defined as follows: That is, the method for recovering selenium according to the present embodiment is a method for recovering selenium from an aqueous solution containing a selenium (VI) compound, and includes a reduction step of reducing selenium (VI) in the aqueous solution with an arsenic (III) compound coexisting in the aqueous solution in the presence of a catalyst in which a platinum group element is supported on a carrier, and a recovery step of recovering elemental selenium produced by the reduction by solid-liquid separation.
[0062] [Reduction process] The reduction step is a step in which a selenium (VI) compound in an aqueous solution is reduced with an arsenic (III) compound in the same aqueous solution in the presence of a catalyst comprising a platinum group element supported on a carrier.
[0063] The specific treatment in the reduction step is the same as that in the method for reducing a selenium (VI) compound, and therefore a detailed explanation will be omitted here. However, in this reduction step, the selenium (VI) compound and the arsenic (III) compound contained in the aqueous solution are simultaneously treated by utilizing a mutual oxidation-reduction reaction between the two compounds to reduce the selenium (VI) compound.
[0064] As described above, the present invention is not limited to treating an aqueous solution in which a selenium (VI) compound and an arsenic (III) compound already coexist, but also includes an embodiment in which, for example, a waste liquid (aqueous solution) containing a selenium (VI) compound is mixed with a waste liquid containing an arsenic (III) compound, thereby causing the arsenic (III) compound to coexist in the aqueous solution.
[0065] According to this method, since a water-insoluble solid catalyst is used, it can be reused and an efficient treatment can be performed, and since an arsenic (III) compound coexisting in the aqueous solution is used as a reducing agent, a selenium (VI) compound can be effectively reduced to an elemental selenium without adding a separate reducing agent. In addition, although the arsenic (III) compound used as a reducing agent is also a difficult-to-treat compound, by using the arsenic (III) compound as a reducing agent, the arsenic (III) compound itself is effectively oxidized, so that the arsenic (III) compound can be effectively treated (treated to arsenate ions) without adding a separate oxidizing agent.
[0066] [Recovery process] The recovery step is a step of recovering the elemental selenium produced by the reduction by solid-liquid separation. As described above, in the reduction step, the selenium (VI) compound is reduced to solid elemental selenium by the reduction action of the arsenic (III) compound in the aqueous solution. Therefore, by separating the elemental selenium produced in the aqueous solution by a solid-liquid separation operation such as filtration, the selenium can be effectively recovered from the aqueous solution.
[0067] The method of solid-liquid separation for recovering elemental selenium is not particularly limited, and any known method can be used. In addition, the method is not limited to the filtration method given above.
[0068] In addition, when the aqueous solution to be treated in the reduction step contains metal ions that form poorly soluble selenides in water, such as copper ions or silver ions, the metal ions may form selenide precipitates. In this case, the solid precipitates of the selenides are also recovered by solid-liquid separation in the recovery step.
[0069] [Arsenate recovery process] In addition, the selenium recovery method according to this embodiment may further include, after the recovery step of recovering elemental selenium described above, an arsenate recovery step of converting arsenate ions remaining in the aqueous solution after solid-liquid separation into arsenate salts and recovering the arsenate salts.
[0070] As described above, the reduction step is characterized by reducing the selenium (VI) compound in the aqueous solution with the arsenic (III) compound in the same aqueous solution, and the arsenic (III) compound itself is oxidized by this reduction reaction. In other words, the selenium (VI) compound is reduced by simultaneously treating both the selenium (VI) compound and the arsenic (III) compound by utilizing their mutual oxidation-reduction reaction. Therefore, in the aqueous solution after the reduction step, arsenate ions are generated by oxidizing arsenic (III) together with selenium element generated by reduction.
[0071] Therefore, an arsenate recovery step can be provided in which a cation is added to the aqueous solution after solid-liquid separation in the recovery step, i.e., the aqueous solution after separation of elemental selenium, to generate poorly soluble arsenate, and the arsenate is recovered by solid-liquid separation. Arsenic (III) is a difficult-to-treat component, just like selenium (VI). By generating arsenate ions by oxidation of the selenium (VI) compound itself in association with its reduction, and converting the arsenate into a poorly soluble arsenate, not only selenium but also arsenic can be effectively recovered.
[0072] The cations added when producing the arsenate are not particularly limited, but examples thereof include iron (III) ions, calcium (II) ions, etc. The amount of the cations added can be appropriately set depending on the amount of arsenate ions produced in the aqueous solution.
[0073] In another embodiment, after the reduction step and prior to the recovery step, an arsenate generation step may be included in which arsenate ions generated in the aqueous solution after the reduction step are converted into arsenates by adding cations to the aqueous solution. That is, in this embodiment, a poorly soluble arsenate is generated in the aqueous solution prior to recovery of elemental selenium by solid-liquid separation. Therefore, in this case, in the recovery step, a mixture of elemental selenium and arsenate generated in the aqueous solution is recovered by solid-liquid separation.
[0074] In such a method, arsenate is precipitated before the solid-liquid separation of elemental selenium, so that both elements can be recovered together in the recovery process.
[0075] However, from the viewpoint of resource recovery, it is more preferable to recover selenium and arsenic separately, and therefore it is preferable to provide an arsenate recovery step after the recovery step of recovering elemental selenium by solid-liquid separation, and to recover arsenate ions remaining in the aqueous solution in the form of arsenate salts separately. EXAMPLES
[0076] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples in any way.
[0077] [Example 1: Reduction treatment of selenium (VI) compounds and testing of carrier types] (Synthesis of selenate reduction catalyst) 9 g (dry weight) of titanium oxide (IV) (product name: P25, manufactured by Nippon Degussa Co., Ltd.) was added as a carrier to 16 ml of an aqueous solution of rhodium (III) chloride containing 1.0 g of rhodium as a carrier material, and the mixture was stirred with a stirrer while maintaining the temperature at 75°C to evaporate water for 2 hours. The mixture was then vacuum dried at 80°C, and then calcined in hydrogen at 350°C for 2 hours to obtain a catalyst (rhodium-supported catalyst). Analysis of the rhodium content of the obtained catalyst revealed that the amount of rhodium supported was 10% by mass based on the dry mass of the catalyst.
[0078] In addition, a rhodium-supported catalyst was also separately produced using silicon dioxide (product name: CALiACT-50, manufactured by Fuji Silysia Chemical Ltd.) instead of titanium (IV) oxide as the support.
[0079] (Reduction of selenium compounds) 100 ml of an aqueous solution containing 0.63 mM sodium selenate and 1.89 mM sodium arsenite was adjusted to pH 3.0 with 1 M sulfuric acid and placed in a three-neck flask together with 300 mg of the synthesized rhodium-supported catalyst. After that, the mixture was stirred and mixed with a stirrer at 80°C while replacing with argon gas, and sodium selenate was reduced.
[0080] Figures 1 and 2 are graphs showing the results of the treatment. Figure 1 is a graph showing the relationship between the type of carrier constituting the catalyst and the reduction rate of selenium (VI), and Figure 2 is a graph showing the relationship between the type of carrier and the oxidation rate of arsenic (III).
[0081] As shown in Figures 1 and 2, when titanium oxide (IV) was used as the support constituting the catalyst under acidic conditions of pH 3, both the reduction of selenium and the oxidation of arsenic were effective. On the other hand, when silicon dioxide was used as the support, a tendency for the reduction of selenium to be suppressed was confirmed. From this, it can be concluded that titanium oxide is more suitable as a support.
[0082] [Example 2: Test on pH conditions] The molar ratio of selenium (VI) and arsenic (III) in the aqueous solution was set to 1:1, and the catalyst support was limited to titanium (IV) oxide, and the reduction treatment was carried out while replacing with nitrogen gas. At this time, the pH of the aqueous solution was set to four types of conditions: 1.2, 2.8, 4.0, and 7.0, and the reaction status of the reduction of selenium and the oxidation of arsenic was confirmed for each condition. The other conditions were the same as in Example 1.
[0083] 3 and 4 are graphs showing the results of the treatment. FIG. 3 is a graph showing the relationship between pH conditions and the reduction rate of selenium (VI), and FIG. 4 is a graph showing the relationship between pH conditions and the oxidation rate of arsenic (III).
[0084] As shown in Figures 3 and 4, taking into consideration the reaction rates of both the reduction rate of selenium (VI) and the oxidation rate of arsenic (III), the pH condition of the aqueous solution is preferably in the range of pH 1.0 to 4.0, with a pH of around 2.8 being considered to be the optimal pH.
[0085] [Example 3: Test for pre-reduction before treatment] The reaction status of the reduction of selenium and the oxidation of arsenic was confirmed under the same conditions as in Example 1, except that the catalyst support was limited to titanium (IV) oxide and that the synthesized catalyst was reduced with 300 mg of sodium borohydride as a pre-treatment prior to use.
[0086] FIG. 5 is a graph showing the results of the treatment, and is a graph showing the relationship between the presence or absence of pretreatment for prior reduction of the catalyst and the reduction rate of selenium (VI).
[0087] As shown in FIG. 5, it was confirmed that the reduction rate of selenium (VI) was increased by performing a pre-reduction pretreatment before using the catalyst. [Industrial Applicability]
[0088] According to the method of the present invention, it is possible to simultaneously oxidize and reduce selenium (VI) compounds and arsenic (III) compounds, which are difficult to treat and cause problems in non-ferrous smelting, etc., and by combining this method with existing processes, it is possible to effectively render both compounds harmless, making it extremely valuable in industrial applications.
Claims
1. 1. A method for reducing selenium (VI) compounds contained in an aqueous solution, comprising the steps of: reducing selenium (VI) in the aqueous solution with an arsenic (III) compound coexisting in the aqueous solution in the presence of a catalyst comprising a platinum group element supported on a carrier containing titanium (IV) oxide; The pH of the aqueous solution is adjusted to a range of 1.2 to 7.
0. A method for reducing selenium compounds.
2. mixing a liquid containing the arsenic (III) compound with an aqueous solution containing the selenium (VI) compound, thereby causing the arsenic (III) compound to coexist in the aqueous solution; The method for reducing a selenium compound according to claim 1 .
3. The platinum group element includes at least one selected from platinum, palladium, and rhodium; A method for reducing a selenium compound according to claim 1 or 2.
4. The aqueous solution is acidified with sulfuric acid. A method for reducing a selenium compound according to any one of claims 1 to 3.
5. reduction under conditions that do not include atmospheric oxygen and oxidizing agents other than the arsenic (III) compound; A method for reducing a selenium compound according to any one of claims 1 to 4.
6. Prior to use of the catalyst, the catalyst is subjected to a reduction treatment using a reducing agent; A method for reducing a selenium compound according to any one of claims 1 to 5.
7. 1. A method for recovering selenium from an aqueous solution containing selenium (VI) compounds, comprising the steps of: a reduction step of reducing selenium (VI) in the aqueous solution with an arsenic (III) compound coexisting in the aqueous solution in the presence of a catalyst comprising a platinum group element supported on a support containing titanium (IV) oxide; a recovery step of recovering the produced elemental selenium by solid-liquid separation; having In the reduction step, the pH of the aqueous solution is adjusted to a range of 1.2 to 7.
0. Methods for recovering selenium.
8. In the reduction step, mixing a liquid containing the arsenic (III) compound with an aqueous solution containing the selenium (VI) compound, thereby causing the arsenic (III) compound to coexist in the aqueous solution; The method for recovering selenium according to claim 7.
9. After the recovery step, The method further includes an arsenate recovery step of converting arsenate ions remaining in the aqueous solution after the solid-liquid separation into arsenate by adding a cation to the aqueous solution, and recovering the arsenate by solid-liquid separation. The method for recovering selenium according to claim 7 or 8.
10. After the reduction step, The method further includes an arsenate generation step of converting the arsenate ions generated in the aqueous solution into arsenates by adding cations to the aqueous solution, In the recovery step, a mixture of elemental selenium produced in the aqueous solution and the arsenate is recovered by solid-liquid separation. The method for recovering selenium according to claim 7 or 8.
Citation Information
Patent Citations
Method for recovering valuable matter from scrap alloy
JP1987030826A
Arsenic oxidation method
JP2015151289A
Selenate reduction catalyst, production method of selenate reduction catalyst and reduction method of selenate solution
JP2016190221A
Method of recovering selenium
JP2019073767A