Binder resin composition for toner

The binder resin composition for toner, with controlled modulus values and hydrocarbon wax, addresses the challenge of achieving both low-temperature fixability and hot offset resistance by improving wax dispersibility and viscoelasticity, resulting in improved toner performance.

JP7572852B2Active Publication Date: 2024-10-24KAO CORP
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020211317
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-21
Publication Date
2024-10-24
Estimated Expiration
2040-12-21

AI Technical Summary

Technical Problem

Existing toners face challenges in achieving both low-temperature fixability and hot offset resistance due to issues with wax dispersibility and viscosity differences during production, leading to poor kneading properties and inadequate performance.

Method used

A binder resin composition for toner is developed, characterized by specific modulus values and ratios, incorporating hydrocarbon wax to improve wax dispersibility and control viscosity, with a polyester resin containing a hydrocarbon wax, loss modulus at 130°C of 10,000 Pa or less, storage modulus at 190°C of 1,200 Pa or more, and a ratio of storage moduli at 150°C to 190°C of 4.0 or less.

Benefits of technology

The composition achieves excellent low-temperature fixability and hot offset resistance by enhancing wax dispersibility and maintaining appropriate viscoelastic properties, balancing viscosity differences during toner production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572852000001
    Figure 0007572852000001
  • Figure 0007572852000002
    Figure 0007572852000002
  • Figure 0007572852000003
    Figure 0007572852000003
Patent Text Reader

Abstract

To provide a binding resin composition for toner, which excels in low temperature fixability and hot offset resistance, and toner for electrostatic charge image development which contains the binding resin composition.SOLUTION: A binding resin composition for toner is provided in which a polyester resin contains a hydrocarbon wax, the binding resin composition satisfies condition 1: loss elastic modulus [G''(130)] at 130°C is 10,000 Pa or less; condition 2: storage elastic modulus [G'(190)] at 190°C is 1,200 Pa or more; and condition 3: the ratio (G'(150) / G'(190)) of storage elastic modulus [G'(150)] at 150°C to storage elastic modulus [G'(190)]at 190°C is 4.0 or less. Toner for electrostatic charge image development is also provided which contains a binding resin and a coloring agent, wherein the binding resin contains the binding resin composition for toner.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a binder resin composition for toners used for developing latent images formed in electrophotography, electrostatic recording, electrostatic printing, etc., and to a toner for developing electrostatic images containing the binder resin composition. [Background technology]

[0002] In recent years, with the trend toward higher speeds and energy savings in electrophotographic printing, there has been an increasing need for toners with excellent low-temperature fixability and separability. To meet this demand, toners with excellent viscoelasticity and toners containing a large amount of crystalline material that combine sharp melting properties and separability have been developed.

[0003] Patent Document 1 describes a toner binder containing a carboxylic acid component (x) and a polyol component (y) as structural units, where (x) contains 80 mol % or more of a dicarboxylic acid (x1) selected from aromatic dicarboxylic acids and their ester-forming derivatives, and also contains a trivalent or higher polycarboxylic acid (x2), and (y) contains 70 mol % or more of 1,2-propylene glycol (y1), the toner binder having a storage modulus at 150°C [G'(150)] of 1500 Pa or more, and where [G'(150)] and the storage modulus at 180°C [G'(180)] satisfy a specific formula, a specific crystalline resin (B), and, if necessary, an amorphous linear polyester resin (C), and the toner binder is described as having excellent low-temperature fixability and hot offset resistance (fixing temperature range) and also excellent storage stability.

[0004] Patent Document 2 describes a method for producing a toner for developing electrostatic images, which includes the steps of: aggregating resin particles (X) containing a composite resin, in an aqueous medium, comprising a segment of polyester resin (a) obtained by polycondensation of an alcohol component containing 80 mol % or more of an ethylene oxide adduct of bisphenol A with a polycarboxylic acid component, and a vinyl resin segment containing a structural unit derived from a styrene compound, to obtain aggregated particles (1); aggregating resin particles (Y) containing polyester resin (b) obtained by polycondensation of an alcohol component containing 80 mol % or more of a propylene oxide adduct of bisphenol A with a polycarboxylic acid component to obtain aggregated particles (2); and fusing the aggregated particles (2). Patent Document 2 describes a method for producing a toner with excellent low-temperature fixability and heat-resistant storage stability. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Laid-Open No. 2013-228724 [Patent Document 2] Japanese Patent Application Laid-Open No. 2016-14872 Summary of the Invention [Problem to be solved by the invention]

[0006] Conventionally, in order to improve the hot offset resistance of a toner, viscoelasticity has been controlled by increasing the storage modulus of the toner at high temperatures or by reducing the rate of change in storage modulus upon heating. Although increasing the elasticity in this way improves the hot offset resistance, there is a problem that during toner production, the viscosity difference with a low-viscosity wax increases, which deteriorates kneading properties and reduces dispersibility of the wax, thereby deteriorating low-temperature fixability. For example, the toner disclosed in Patent Document 1 uses a highly elastic binder resin to improve hot offset resistance, which poses problems in terms of wax dispersibility, and the low-temperature fixability is still insufficient. Furthermore, in Patent Document 2, a large amount of wax is blended. Although a toner containing a large amount of wax is advantageous in terms of low-temperature fixability, it has the problem that it cannot maintain elasticity at high temperatures and therefore has poor hot offset resistance.

[0007] The present invention relates to a binder resin composition for toners, which has excellent low-temperature fixing properties and hot offset resistance, and toners for developing electrostatic images, which contain the binder resin composition. [Means for solving the problem]

[0008] The present invention provides [1] A binder resin composition for toner, wherein the polyester resin contains a hydrocarbon wax, Condition 1: Loss modulus at 130°C [G''(130)] is 10,000 Pa or less, Condition 2: Storage modulus at 190°C [G'(190)] is 1,200 Pa or more, and Condition 3: The ratio of the storage modulus at 150°C [G'(150)] to the storage modulus at 190°C [G'(190)] (G'(150) / G'(190)) is 4.0 or less. A binder resin composition for toner, which satisfies the above requirements, and [2] A toner for developing electrostatic images, comprising a binder resin and a colorant, wherein the binder resin comprises the binder resin composition for toners according to [1] above. Regarding. [Effects of the Invention]

[0009] The toner for developing electrostatic images containing the binder resin composition of the present invention exhibits excellent effects such as good low-temperature fixability and good hot offset resistance. DETAILED DESCRIPTION OF THE INVENTION

[0010] The binder resin composition for toner of the present invention is a polyester resin containing a hydrocarbon wax, and is characterized in that it satisfies the conditions 1 to 3 described below, i.e., the loss modulus G'' at 130°C, the storage modulus G' at 190°C, and the rate of change in the storage modulus from 150°C to 190°C are controlled within predetermined ranges. The reason why the effects of the present invention are achieved is not clear, but is presumed to be as follows.

[0011] In the present invention, attention is focused on the storage modulus G', which is an index of hot offset resistance, and the storage modulus G'(190) at 190°C of a binder resin composition containing a polyester-based resin is controlled to 1200 Pa or more, and further the rate of change in storage modulus from 150°C to 190°C (G'(150) / G'(190)) is controlled to 4.0 or less, thereby improving the hot offset resistance of the binder resin composition. Generally, when the storage modulus of a polyester-based resin is high, the viscosity difference with a low-viscosity wax increases during toner production, resulting in poor kneading properties and poor wax dispersion, which deteriorates low-temperature fixability. However, in the present invention, by incorporating a hydrocarbon-based wax into the polyester-based resin, the hydrocarbon-based wax can be more highly dispersed than when the wax is mixed with the polyester resin, and it is presumed that this makes it possible to achieve both low-temperature fixability and hot offset resistance. Furthermore, in the present invention, the loss modulus G'' of the polyester resin at 130°C is controlled to 10,000 Pa or less, thereby further improving low-temperature fixability. The loss modulus is an effective indicator of viscosity, and it is believed that the G'' value at 130°C, which is close to the fixing temperature of the toner, correlates with low-temperature fixability. Furthermore, since 130°C is also close to the temperature at which the toner raw materials are melted and kneaded, the G'' value at 130°C corresponds to the physical properties in the melting process. Controlling G'' at 130°C to 10,000 Pa or less reduces the difference in viscosity with the wax during toner production, further improving wax dispersibility, which is also believed to contribute to the improvement in low-temperature fixability of the present invention.

[0012] <Condition 1: Loss modulus at 130°C [G''(130)] is 10,000 Pa or less> The loss modulus at 130°C [G''(130)] is preferably 9,000 Pa or less, more preferably 8,000 Pa or less, and preferably 1,000 Pa or more, more preferably 2,000 Pa or more, and even more preferably 3,000 Pa or more. The loss modulus of the resin composition can be adjusted by the proportion of the hydrocarbon component, etc. For example, the loss modulus of the resin composition can be reduced by increasing the hydrocarbon component in the resin composition, for example, by adding a hydrocarbon additive such as a hydrocarbon wax to the resin composition or by using an aliphatic diol or the like in a raw material monomer of the resin to introduce a hydrocarbon chain.

[0013] <Condition 2: Storage modulus at 190°C [G'(190)] is 1200 Pa or more> The storage modulus at 190°C [G'(190)] is preferably 1,500 Pa or more, more preferably 1,800 Pa or more, even more preferably 2,000 Pa or more, and is preferably 10,000 Pa or less, more preferably 8,000 Pa or less, even more preferably 7,500 Pa or less, even more preferably 5,000 Pa or less. The storage modulus at 190°C [G'(190)] can be adjusted by controlling the progress of the crosslinking reaction when producing the resin composition. For example, using trimellitic anhydride, which acts as a crosslinking agent, as a raw monomer for the resin, and adding styrene acrylic moieties increases the number of crosslinking agent moieties, thereby increasing the storage modulus of the resin composition. In addition to the resin composition, the crosslinking reaction can also be accelerated by adjusting conditions such as the reaction temperature and time during the crosslinking reaction, thereby increasing the storage modulus.

[0014] <Condition 3: The ratio of the storage modulus at 150°C [G'(150)] to the storage modulus at 190°C [G'(190)] (G'(150) / G'(190)) is 4.0 or less.> G'(150) / G'(190) is preferably 3.0 or less, more preferably 2.5 or less, even more preferably 2.0 or less, and is preferably 0.2 or more, more preferably 0.5 or more, even more preferably 1.0 or more, even more preferably 1.5 or more. The ratio G'(150) / G'(190) can be adjusted by the crosslink density in the resin. For example, by compounding polyester resin with a styrene-based resin, the molecular weight distribution before crosslinking can be broadened, and by crosslinking this composite resin with a wide molecular weight distribution, the crosslink density of the gel portion can be reduced. Lowering the crosslink density allows the resin to soften somewhat at low temperatures (150°C) and maintain hardness even at high temperatures (190°C), thereby reducing the ratio G'(150) / G'(190). In addition to the resin composition, the crosslink density can be reduced by the copolymerization conditions of the styrene-based resin (e.g., the amount of radicals generated, the rate at which the raw monomers of the styrene-based resin are added), the temperature during compounding, and the order of the polycondensation and addition polymerization reactions.

[0015] In the binder resin composition of the present invention, the gel fraction, which is an ultrahigh molecular weight component, has high elasticity even at high temperatures. Therefore, as the gel fraction increases, condition 2 (G'(190)) increases and condition 3 (G'(150) / G'(190)) decreases. On the other hand, condition 1 (G''(130)) increases, so it is preferable to balance the amount of gel fraction. From these viewpoints, in the binder resin composition of the present invention, the value obtained by subtracting the content (mass%) of the hydrocarbon wax from the methyl ethyl ketone-insoluble matter (mass%) when the composition is dissolved in methyl ethyl ketone is preferably 15% by mass or more, more preferably 20% by mass or more, from the viewpoint of hot offset resistance, and is 40% by mass or less, more preferably 35% by mass or less, and even more preferably 30% by mass or less, from the viewpoint of low-temperature fixability.

[0016] The polyester resin preferably includes a polyester resin obtained by polycondensation of raw material monomers composed of an alcohol component and a carboxylic acid component.

[0017] Examples of the alcohol component include alkylene oxide adducts of bisphenol A, such as an ethylene oxide adduct of bisphenol A and a propylene oxide adduct of bisphenol A; aliphatic diols, such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-butenediol, 1,3-butanediol, and neopentyl glycol; and trihydric or higher alcohols, such as glycerin. Of these, from the viewpoints of low-temperature fixability and hot offset resistance, alkylene oxide adducts of bisphenol A are preferred, and ethylene oxide adducts of bisphenol A are more preferred.

[0018] The ethylene oxide adduct of bisphenol A has the formula (I):

[0019] [ka]

[0020] (In the formula, x and y represent the average number of moles of ethylene oxide added, and are each a positive number, and the sum of x and y is 1 or more, preferably 1.5 or more, and 5 or less, preferably 4 or less.) A compound represented by the following formula is preferred.

[0021] The content of the ethylene oxide adduct of bisphenol A in the alcohol component is preferably 60 mol % or more, and preferably 95 mol % or less, more preferably 90 mol % or less, from the viewpoint of low-temperature fixability. Furthermore, from the viewpoint of hot offset resistance, the content of the ethylene oxide adduct of bisphenol A in the alcohol component is preferably 60 mol% or more, more preferably 70 mol% or more, even more preferably 80 mol% or more, even more preferably 90 mol% or more, and even more preferably 100 mol%.

[0022] From the viewpoint of improving low-temperature fixability, the alcohol component preferably further contains 1,4-butanediol.

[0023] From the viewpoint of achieving both fixability and storage stability, the content of 1,4-butanediol in the alcohol component is preferably 5 mol% or more, more preferably 10 mol% or more, even more preferably 15 mol% or more, and is preferably 40 mol% or less, more preferably 35 mol% or less, even more preferably 30 mol% or less.

[0024] The carboxylic acid component is preferably at least one selected from the group consisting of aromatic dicarboxylic acid compounds, aliphatic dicarboxylic acid compounds, and trivalent or higher carboxylic acid compounds, and from the viewpoint of storage stability, it is more preferable that the composition contains an aromatic dicarboxylic acid compound.

[0025] Examples of aromatic dicarboxylic acid compounds include phthalic acid, isophthalic acid, terephthalic acid, anhydrides of these acids, and alkyl esters in which the alkyl group has 1 to 3 carbon atoms. Among these, terephthalic acid or isophthalic acid is preferred, and terephthalic acid is more preferred.

[0026] The content of the aromatic dicarboxylic acid compound in the carboxylic acid component is preferably 50 mol% or more, more preferably 70 mol% or more, and 100 mol% or less, preferably 95 mol% or less, more preferably 90 mol% or less, and even more preferably 85 mol% or less.

[0027] Examples of the aliphatic dicarboxylic acid compound include aliphatic dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, succinic acid which may be substituted with a hydrocarbon group having 1 to 20 carbon atoms, adipic acid, and the like; anhydrides of these acids; and alkyl esters in which the alkyl group has 1 to 3 carbon atoms.

[0028] Examples of trivalent or higher carboxylic acid compounds include 1,2,4-benzenetricarboxylic acid (trimellitic acid), 2,5,7-naphthalenetricarboxylic acid, pyromellitic acid, anhydrides of these acids, and alkyl esters in which the alkyl group has 1 to 3 carbon atoms, and among these, trimellitic acid compounds are preferred.

[0029] From the viewpoint of durability, the content of the trivalent or higher carboxylic acid compound in the carboxylic acid component is preferably 5 mol % or more, more preferably 10 mol % or more, and from the viewpoint of low-temperature fixability, the content is preferably 60 mol % or less, more preferably 40 mol % or less, in the carboxylic acid component.

[0030] The alcohol component may contain a monohydric alcohol, and the carboxylic acid component may contain a monocarboxylic acid compound, as appropriate.

[0031] The equivalent ratio of the carboxylic acid component to the alcohol component (COOH group / OH group) in the polyester resin is preferably 0.6 or more, more preferably 0.7 or more, even more preferably 0.75 or more, from the viewpoint of adjusting the softening point of the polyester resin, and is preferably 1.2 or less, more preferably 1.15 or less.

[0032] The polyester resin can be obtained, for example, by polycondensing an alcohol component and a carboxylic acid component in an inert gas atmosphere, preferably in the presence of an esterification catalyst, and optionally in the presence of an esterification promoter, a polymerization inhibitor, etc., at a temperature of preferably 130°C or higher, more preferably 170°C or higher, and preferably 250°C or lower, more preferably 240°C or lower.

[0033] Examples of esterification catalysts include tin compounds such as dibutyltin oxide and tin(II) 2-ethylhexanoate, and titanium compounds such as titanium diisopropylate bistriethanolamine, with tin compounds being preferred. The amount of the esterification catalyst used is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and preferably 1.5 parts by mass or less, more preferably 1 part by mass or less, per 100 parts by mass of the alcohol component and the carboxylic acid component combined. Examples of esterification promoters include gallic acid. The amount of the esterification promoter used is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and preferably 0.5 parts by mass or less, more preferably 0.1 parts by mass or less, per 100 parts by mass of the alcohol component and the carboxylic acid component combined. Examples of polymerization inhibitors include tert-butylcatechol. The amount of the polymerization inhibitor used is preferably 0.001 part by mass or more, more preferably 0.01 part by mass or more, and preferably 0.5 part by mass or less, more preferably 0.1 part by mass or less, relative to 100 parts by mass of the total amount of the alcohol component and the carboxylic acid component.

[0034] The polyester resin in the present invention is preferably a composite resin in which the polyester resin and a styrene resin are bonded together.

[0035] The styrene-based resin is obtained by addition polymerization of raw material monomers containing a styrene compound.

[0036] Styrene-based resins are addition polymers of raw material monomers containing at least styrene or styrene derivatives such as α-methylstyrene and vinyltoluene (hereinafter, styrene and styrene derivatives are collectively referred to as "styrene compounds").

[0037] The content of the styrene compound, preferably styrene, in the raw material monomers of the styrene-based resin is preferably 50% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more, from the viewpoint of low-temperature fixability and storage stability, and is preferably 95% by mass or less, more preferably 93% by mass or less, and even more preferably 90% by mass or less, from the viewpoint of improving the low-temperature fixability of the toner.

[0038] The styrene-based resin may also contain, as a raw material monomer, a (meth)acrylic acid alkyl ester having an alkyl group with 7 or more carbon atoms. Examples of (meth)acrylic acid alkyl esters include 2-ethylhexyl (meth)acrylate, (iso)octyl (meth)acrylate, (iso)decyl (meth)acrylate, and (iso)stearyl (meth)acrylate. It is preferable to use one or more of these. In this specification, "(iso)" means both the presence and absence of this group, and indicates normal when this group is not present. Furthermore, "(meth)acrylic acid" refers to acrylic acid, methacrylic acid, or both.

[0039] From the viewpoint of improving the low-temperature fixability of the toner, the number of carbon atoms in the alkyl group in the (meth)acrylic acid alkyl ester as a raw material monomer for the styrene-based resin is preferably 7 or more, more preferably 8 or more, and preferably 12 or less, more preferably 10 or less. The number of carbon atoms in the alkyl ester refers to the number of carbon atoms derived from the alcohol component constituting the ester.

[0040] The raw material monomers for styrene-based resins may include raw material monomers other than styrene compounds and (meth)acrylic acid alkyl esters, for example, ethylenically unsaturated monoolefins such as ethylene and propylene; diolefins such as butadiene; halovinyls such as vinyl chloride; vinyl esters such as vinyl acetate and vinyl propionate; ethylenic monocarboxylic acid esters such as dimethylaminoethyl (meth)acrylate; vinyl ethers such as methyl vinyl ether; vinylidene halides such as vinylidene chloride; and N-vinyl compounds such as N-vinylpyrrolidone.

[0041] The addition polymerization reaction of raw material monomers for the styrene-based resin can be carried out by a conventional method, for example, in the presence of a polymerization initiator such as dicumyl peroxide, a polymerization inhibitor, a crosslinking agent, etc., in the presence of an organic solvent or without a solvent. The temperature conditions are preferably 110°C or higher, more preferably 140°C or higher, and preferably 200°C or lower, more preferably 170°C or lower.

[0042] When an organic solvent is used in the addition polymerization reaction, xylene, toluene, methyl ethyl ketone, acetone, etc. can be used. The amount of the organic solvent used is preferably 10 parts by mass or more and 50 parts by mass or less per 100 parts by mass of the raw material monomer of the styrene-based resin.

[0043] The mass ratio of the polyester resin to the styrene-based resin in the composite resin (polyester resin / styrene-based resin) is preferably 60 / 40 or more, more preferably 70 / 30 or more, and even more preferably 80 / 20 or more, from the viewpoint of low-temperature fixability, and is preferably 98 / 2 or less, more preferably 95 / 5 or less, and even more preferably 90 / 10 or less, from the viewpoint of grindability. In the above calculation, the mass of the polyester resin is the mass of the raw material monomers of the polyester resin used, minus the amount of reaction water (calculated value) dehydrated by the polycondensation reaction, and the amount of the bireactive monomer is included in the amount of raw material monomers of the polyester resin. In addition, the amount of the styrene-based resin is the total amount of the raw material monomers of the styrene-based resin and the polymerization initiator.

[0044] The composite resin is more preferably a resin chemically bonded by a covalent bond via a bireactive monomer capable of reacting with both the raw material monomer of the polyester resin and the raw material monomer of the styrene-based resin.

[0045] The bireactive monomer is preferably a compound having at least one functional group selected from the group consisting of hydroxyl, carboxyl, epoxy, primary amino, and secondary amino groups, preferably a hydroxyl and / or carboxyl group, more preferably a carboxyl group, and an ethylenically unsaturated bond in the molecule, more preferably at least one selected from the group consisting of acrylic acid, methacrylic acid, fumaric acid, maleic acid, and maleic anhydride, and from the viewpoint of the reactivity of polycondensation reactions and addition polymerization reactions, even more preferably at least one selected from the group consisting of acrylic acid, methacrylic acid, and fumaric acid. However, when used together with a polymerization inhibitor, a polycarboxylic acid compound having an ethylenically unsaturated bond, such as fumaric acid, functions as a raw material monomer for polyester resin. In this case, fumaric acid, etc., is not a bireactive monomer but a raw material monomer for polyester resin.

[0046] The amount of the bireactive monomer used is preferably 1 mol or more, more preferably 2 mol or more, relative to a total of 100 mols of the alcohol components of the polyester resin, from the viewpoint of low-temperature fixability, and is preferably 30 mol or less, more preferably 20 mol or less, and even more preferably 10 mol or less, from the viewpoint of improving the dispersibility of the styrene-based resin and the polyester resin and improving the durability of the toner. The amount of the bireactive monomer used is preferably 1 part by mass or more, more preferably 2 parts by mass or more, per 100 parts by mass of the total raw material monomers of the styrene resin, from the viewpoint of low-temperature fixability, and is preferably 30 parts by mass or less, more preferably 20 parts by mass or less, and even more preferably 10 parts by mass or less, from the viewpoint of improving the dispersibility of the styrene resin and the polyester resin and improving the durability of the toner. Here, the polymerization initiator is included in the total raw material monomers of the styrene resin.

[0047] The binder resin composition of the present invention is preferably a resin in which a hydrocarbon wax is internally added to a polyester resin. Therefore, the binder resin composition is preferably a polyester resin obtained by carrying out a polycondensation reaction of raw material monomers for a polyester resin in the presence of a hydrocarbon wax, or a composite resin obtained by carrying out a polycondensation reaction of raw material monomers for a polyester resin and / or an addition polymerization reaction of raw material monomers for a styrene resin in the presence of a hydrocarbon wax.

[0048] Examples of hydrocarbon waxes include polypropylene wax, polyethylene wax, polypropylene-polyethylene copolymer wax, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax. Of these, polypropylene wax, paraffin wax, and Fischer-Tropsch wax are preferred, with Fischer-Tropsch wax being more preferred.

[0049] The hydrocarbon wax preferably does not have a functional group that reacts with the raw material monomer of the polyester resin.

[0050] The melting point of the hydrocarbon wax is preferably 80°C or higher, more preferably 85°C or higher, even more preferably 90°C or higher, and even more preferably 95°C or higher, and from the viewpoint of low-temperature fixability, is preferably 160°C or lower, more preferably 140°C or lower, even more preferably 130°C or lower, even more preferably 120°C or lower, and even more preferably 115°C or lower.

[0051] The content of the hydrocarbon wax in the binder resin composition is preferably 5% by mass or more, more preferably 7.5% by mass or more, and even more preferably 10% by mass or more, from the viewpoint of hot offset resistance, and is preferably 30% by mass or less, more preferably 25% by mass or less, even more preferably 20% by mass or less, and even more preferably 14% by mass or less, from the viewpoint of low-temperature fixability and durability.

[0052] When the polyester resin is a composite resin, it is preferably produced by the following method, and it is preferable to carry out a polycondensation reaction of raw material monomers of the polyester resin in the presence of a hydrocarbon wax. When a bireactive monomer is used, it is preferable to use the bireactive monomer in an addition polymerization reaction together with raw material monomers of a styrene resin, from the viewpoint of improving the durability of the toner and improving the low-temperature fixability and heat-resistant storage stability of the toner.

[0053] (i) A method in which a step (A) of polycondensation reaction of raw material monomers of a polyester resin in the presence of a hydrocarbon wax is followed by a step (B) of addition polymerization reaction of raw material monomers of a styrene resin and a bireactive monomer. In this method, a hydrocarbon wax is added together with raw material monomers for the polyester resin, and step (A) is carried out under reaction temperature conditions suitable for a polycondensation reaction. The reaction temperature is then lowered, and step (B) is carried out under temperature conditions suitable for an addition polymerization reaction. The raw material monomers for the styrene resin and the bireactive monomer are preferably added to the reaction system at a temperature suitable for the addition polymerization reaction. The bireactive monomer undergoes the addition polymerization reaction and also reacts with the polyester resin. After step (B), the reaction temperature is raised again, and if necessary, a raw material monomer of a trivalent or higher polyester resin that serves as a crosslinking agent is added to the polymerization system, thereby further promoting the polycondensation reaction of step (A) and the reaction with the bireactive monomer.

[0054] (ii) A method in which step (B) of an addition polymerization reaction of raw material monomers of a styrene-based resin and a bireactive monomer is followed by step (A) of a polycondensation reaction of raw material monomers of a polyester resin in the presence of a hydrocarbon wax. In this method, step (B) is carried out under reaction temperature conditions suitable for an addition polymerization reaction, and then the reaction temperature is increased, and a hydrocarbon wax is added under temperature conditions suitable for a polycondensation reaction, followed by the polycondensation reaction of step (A). The bireactive monomer is involved in both the addition polymerization reaction and the polycondensation reaction. The raw material monomers and hydrocarbon wax for the polyester resin may be present in the reaction system during the addition polymerization reaction, or may be added to the reaction system under temperature conditions suitable for the polycondensation reaction. In the former case, the progress of the polycondensation reaction can be controlled by adding an esterification catalyst at a temperature suitable for the polycondensation reaction.

[0055] (iii) A method in which the reaction is carried out under conditions in which step (A) of polycondensation reaction of raw material monomers of polyester resin and step (B) of addition polymerization reaction of raw material monomers of styrene resin and bireactive monomer proceed in parallel in the presence of hydrocarbon wax. In this method, hydrocarbon wax is added along with the raw material monomers for the polyester resin and the raw material monomers for the styrene resin, and steps (A) and (B) are carried out in parallel under reaction temperature conditions suitable for the addition polymerization reaction. The reaction temperature is then raised, and, if necessary, a raw material monomer for the trivalent or higher polyester resin that serves as a crosslinking agent is added to the polymerization system under temperature conditions suitable for the polycondensation reaction, and the polycondensation reaction of step (A) is preferably further carried out. In this case, a polymerization inhibitor can be added under temperature conditions suitable for the polycondensation reaction to allow only the polycondensation reaction to proceed. Bireactive monomers are involved in both the addition polymerization reaction and the polycondensation reaction.

[0056] In the above method (iii), when the reaction is carried out under conditions in which step (A) and step (B) proceed in parallel, the reaction can also be carried out by adding dropwise a mixture containing raw material monomers for the styrene-based resin to a mixture containing raw material monomers for the polyester resin.

[0057] The above methods (i) to (iii) are preferably carried out in the same container.

[0058] Of the above methods (i) to (iii), method (ii) is preferred from the viewpoint of reducing the crosslink density in the composite resin.

[0059] The softening point of the binder resin composition of the present invention is preferably 90° C. or higher, more preferably 100° C. or higher, even more preferably 110° C. or higher, and still more preferably 115° C. or higher, from the viewpoints of durability and hot offset resistance, and is preferably 150° C. or lower, more preferably 140° C. or lower, even more preferably 130° C. or lower, and still more preferably 120° C. or lower, from the viewpoints of pulverization productivity and low-temperature fixability.

[0060] The glass transition temperature of the binder resin composition of the present invention is preferably 45° C. or higher, more preferably 50° C. or higher, and even more preferably 55° C. or higher, from the viewpoint of storage stability, and is preferably 70° C. or lower, and more preferably 65° C. or lower, from the viewpoint of low-temperature fixability.

[0061] Furthermore, the present invention provides a toner for developing electrostatic images (hereinafter also simply referred to as toner) which contains a binder resin and a colorant, and the binder resin contains the binder resin composition of the present invention.

[0062] The content of the binder resin composition of the present invention in the binder resin is preferably 20% by mass or more, more preferably 30% by mass or more, even more preferably 40% by mass or more, and is preferably 90% by mass or less, more preferably 80% by mass or less, even more preferably 70% by mass or less.

[0063] The binder resin may contain a resin other than the binder resin composition of the present invention. Examples of the other resin include a polyester resin (polyester resin P) having a softening point lower than that of the binder resin composition of the present invention, from the viewpoint of low-temperature fixability.

[0064] The difference in softening point between the binder resin composition of the present invention and the polyester resin P is preferably 5°C or more, more preferably 10°C or more, even more preferably 15°C or more, and is preferably 50°C or less, more preferably 40°C or less, even more preferably 35°C or less, even more preferably 30°C or less.

[0065] Furthermore, the softening point of the polyester resin P is preferably 80°C or higher, more preferably 85°C or higher, even more preferably 90°C or higher, even more preferably 95°C or higher, and preferably 120°C or lower, more preferably 115°C or lower, even more preferably 110°C or lower.

[0066] Examples of the alcohol component of the polyester resin P include aromatic diols such as alkylene oxide adducts of bisphenol A, aliphatic diols such as ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-butenediol, 1,3-butanediol, and neopentyl glycol, and trihydric or higher alcohols such as glycerin.

[0067] Examples of the carboxylic acid component of the polyester resin P include aromatic dicarboxylic acids such as phthalic acid, isophthalic acid, and terephthalic acid; aliphatic dicarboxylic acids such as oxalic acid, malonic acid, maleic acid, fumaric acid, citraconic acid, itaconic acid, and glutaconic acid; succinic acid which may be substituted with a hydrocarbon group having 1 to 20 carbon atoms; adipic acid; trivalent or higher carboxylic acids such as trimellitic acid and pyromellitic acid; anhydrides of these acids; and alkyl esters having 1 to 3 carbon atoms.

[0068] The polyester resin P can be obtained by polycondensing an alcohol component and a carboxylic acid component in the presence of an ester catalyst or the like using a conventional method.

[0069] The glass transition temperature of the polyester resin P is preferably 40°C or higher, more preferably 45°C or higher, even more preferably 50°C or higher, and preferably 70°C or lower, more preferably 65°C or lower, even more preferably 60°C or lower.

[0070] When the binder resin contains polyester resin P, the mass ratio of polyester resin P to the binder resin composition of the present invention (polyester resin P / binder resin composition) is preferably 20 / 80 or more, more preferably 30 / 70 or more, and preferably 80 / 20 or less, more preferably 70 / 30 or less, and even more preferably 60 / 40 or less.

[0071] The content of the binder resin in the toner is preferably 60% by mass or more, more preferably 70% by mass or more, even more preferably 80% by mass or more, and is preferably less than 100% by mass, more preferably 98% by mass or less, even more preferably 95% by mass or less.

[0072] When the binder resin contains two or more resins, a mixture of these resins may be used as the binder resin, or these resins may be directly used to mix the raw materials when producing the toner.

[0073] As the colorant, any of the dyes, pigments, etc. used as colorants for toners can be used, such as carbon black, phthalocyanine blue, permanent brown FG, brilliant fast scarlet, pigment green B, rhodamine-B base, solvent red 49, solvent red 146, solvent blue 35, quinacridone, carmine 6B, disazo yellow, etc., and the toner of the present invention may be either a black toner or a color toner.

[0074] From the viewpoint of improving the image density and low-temperature fixability of the toner, the content of the colorant is preferably 1 part by mass or more, more preferably 2 parts by mass or more, and is preferably 40 parts by mass or less, more preferably 10 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0075] The toner for developing electrostatic images of the present invention may contain additives such as a release agent, a charge control agent, a magnetic powder, a flowability improver, a conductivity adjuster, a reinforcing filler such as a fibrous substance, an antioxidant, and a cleaning property improver, in addition to the binder resin and the colorant.

[0076] Examples of the release agent include aliphatic hydrocarbon waxes such as polypropylene wax, polyethylene wax, polypropylene-polyethylene copolymer wax, microcrystalline wax, paraffin wax, and Fischer-Tropsch wax, or oxides thereof; ester waxes such as carnauba wax, montan wax, or deacidified waxes thereof, and fatty acid ester wax; fatty acid amides, fatty acids, higher alcohols, and fatty acid metal salts, and these may be used alone or in combination.

[0077] Since the binder resin composition already contains wax, it is preferable that the binder resin composition does not contain a release agent, or if it does contain a release agent, it contains a small amount of the release agent so as not to impair the effects of the present invention. When the binder resin composition contains a release agent, the content thereof is preferably 6 parts by mass or less, more preferably 4 parts by mass or less, and even more preferably 2 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0078] The charge control agent is not particularly limited, and may contain either a positively chargeable charge control agent or a negatively chargeable charge control agent.

[0079] Examples of positively chargeable charge control agents include nigrosine dyes such as "Nigrosine Base EX," "Oil Black BS," "Oil Black SO," "Bontron N-01," "Bontron N-04," "Bontron N-07," "Bontron N-09," "Bontron N-11," and "Bontron N-79" (all manufactured by Orient Chemical Industries Co., Ltd.); triphenylmethane dyes containing a tertiary amine as a side chain; quaternary ammonium salt compounds such as "Bontron P-51" (manufactured by Orient Chemical Industries Co., Ltd.); cetyltrimethylammonium bromide; and "COPY CHARGE PX Examples of suitable resins include polyamine resins such as "AFP-B" (manufactured by Orient Chemical Industries Co., Ltd.); imidazole derivatives such as "PLZ-2001" and "PLZ-8001" (both manufactured by Shikoku Chemical Industry Co., Ltd.); and styrene-acrylic resins such as "FCA-701PT" (manufactured by Fujikura Chemical Industries Co., Ltd.).

[0080] Examples of negatively chargeable charge control agents include metal-containing azo dyes such as "Balifast Black 3804," "Bontron S-31," "Bontron S-32," "Bontron S-34," and "Bontron S-36" (all manufactured by Orient Chemical Industries, Ltd.), "Eisenspiron Black TRH," and "T-77" (manufactured by Hodogaya Chemical Co., Ltd.); metal compounds of benzilic acid compounds such as "LR-147" and "LR-297" (manufactured by Nippon Carlit Co., Ltd.); metal compounds of salicylic acid compounds such as "Bontron E-81," "Bontron E-84," "Bontron E-88," and "Bontron E-304" (all manufactured by Orient Chemical Industries, Ltd.), and "TN-105" (manufactured by Hodogaya Chemical Co., Ltd.); copper phthalocyanine dyes; and quaternary ammonium salts such as "COPY CHARGE NX VP434 (manufactured by Clariant), nitroimidazole derivatives, etc.; organometallic compounds, etc.

[0081] From the viewpoint of the charging stability of the toner, the content of the charge control agent is preferably 0.01 parts by mass or more, more preferably 0.2 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 3 parts by mass or less, and even more preferably 2 parts by mass or less, relative to 100 parts by mass of the binder resin.

[0082] Known methods for producing toner include melt-kneading, emulsion phase inversion, polymerization, and emulsion aggregation. However, since the viscoelasticity of the binder resin is controlled in the toner of the present invention, the effects of the present invention are significantly exhibited by producing the toner by the melt-kneading method. Therefore, the toner of the present invention is preferably a pulverized toner obtained by a method including a step of pulverizing a melt-kneaded mixture of raw materials including the binder resin and the colorant. The pulverized toner produced by the melt-kneading method can be produced, for example, by uniformly mixing raw materials such as the binder resin, colorant, and charge control agent in a mixer such as a Henschel mixer, melt-kneading the mixture in an internal kneader, a single-screw or twin-screw extruder, an open-roll kneader, or the like, followed by cooling, pulverization, and classification.

[0083] In order to improve the transferability of the toner of the present invention, it is preferable to use an external additive. Examples of the external additive include inorganic fine particles such as silica, alumina, titania, zirconia, tin oxide, and zinc oxide, and organic fine particles such as resin particles such as melamine-based resin fine particles and polytetrafluoroethylene resin fine particles, and two or more of these may be used in combination. Among these, silica is preferred, and from the viewpoint of the transferability of the toner, hydrophobic silica that has been subjected to a hydrophobic treatment is more preferred.

[0084] Examples of hydrophobic treatment agents for hydrophobizing the surfaces of silica particles include hexamethyldisilazane (HMDS), dimethyldichlorosilane (DMDS), silicone oil, octyltriethoxysilane (OTES), and methyltriethoxysilane.

[0085] From the viewpoint of the chargeability, fluidity, and transferability of the toner, the average particle diameter of the external additive is preferably 10 nm or more, more preferably 15 nm or more, and is preferably 250 nm or less, more preferably 200 nm or less, even more preferably 150 nm or less, and even more preferably 90 nm or less.

[0086] From the viewpoint of the chargeability, fluidity, and transferability of the toner, the content of the external additive is preferably 0.05 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.3 parts by mass or more, relative to 100 parts by mass of the toner before treatment with the external additive, and is preferably 5 parts by mass or less, and more preferably 3 parts by mass or less.

[0087] The volume median particle size (D 50 ) is preferably 3 μm or more, more preferably 4 μm or more, and is preferably 15 μm or less, more preferably 10 μm or less. 50 ) means the particle size at which the cumulative volume frequency calculated by volume fraction is 50% starting from the smallest particle size. In addition, when the toner is treated with an external additive, the volume median particle size of the toner particles before treatment with the external additive is taken as the volume median particle size of the toner.

[0088] The toner of the present invention can be used as a toner for one-component development, or mixed with a carrier to form a two-component developer. [Example]

[0089] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Physical properties of resins and the like can be measured by the following methods.

[0090] [Resin loss modulus (G'') and storage modulus (G')] Measurement is carried out using a viscoelasticity measuring device (rheometer) "MCR-302" (manufactured by Anton Paar) at a shear strain of 0.05% and a frequency of 1 Hz. Parallel plates with a diameter of 25 mm are heated to 100°C and left there, and 2.0 g of sample is pressed at 30 MPa to obtain a pellet with a diameter of 20 mm and a thickness of 5 mm. The pellet is placed on the parallel plates at 100°C and sandwiched from above between 8 mm parallel plates. The temperature is then lowered to 40°C and then raised to 190°C at a rate of 5°C / min. The loss modulus (G'') at 130°C and the storage modulus (G') at 150°C and 190°C are measured.

[0091] [Methyl ethyl ketone (MEK) insoluble resin] (1) Sample preparation Using a JIS Z8801 sieve, collect a powdered sample that passes through a 22 mesh sieve but does not pass through a 30 mesh sieve. If the sample is in a lump, crush it using a commercially available hammer or coffee mill, and sieve it in powder form. (2) Dissolution of the sample 2-1. 2,000 g of sample is weighed into a glass bottle (M-140, manufactured by Kakuyo Glass Co., Ltd.), and then 95 g of MEK is added, and the inner and outer lids are attached. 2-2. Mix in a ball mill for 5 hours (circumferential speed: 200 mm / sec). 2-3. Leave it to stand for 10 hours. (3) Filtration 3-1. Prepare a glass filter (mesh size 11G-3) attached to a pre-weighed (to the nearest 1 / 1000 g) recovery flask (mass A (g)). Use a rubber stopper that allows for pressure reduction to seal the glass filter. 3-2. Using a measuring pipette, take 20 mL of the supernatant from the solution left to stand for 10 hours in 2-3, and filter it under reduced pressure using the glass filter prepared in 3-1. The supernatant is defined as the area 2 cm below the liquid surface. Before filtering the solution, adjust the vacuum in the recovery flask to 40 kPa. 3-3. Suck up 20 mL of unused methyl ethyl ketone (MEK) into a measuring pipette and filter the soluble matter adhering to the glass filter under reduced pressure. (4) Drying 4-1. Remove the MEK from the recovery flask using an evaporator. Water bath temperature: 70℃ Eggplant flask rotation speed: 200 r / min Degree of vacuum inside the recovery flask during MEK removal: Adjust to 40-20kPa Time: 10 minutes 4-2. After drying for 12 hours at 50°C and 1 torr, measure the mass B (g) of the recovery flask. (5) Calculation of gel content 5-1. Calculate the MEK soluble matter X (g) dissolved in 20 mL of MEK. X=BA 5-2. Calculate the MEK solubles Y (g) dissolved in 95 g of MEK, assuming the specific gravity of MEK is 0.805. Y = X × 95 / (20 × 0.805) 5-3. Calculate the soluble matter Z (mass%) per 1 g of sample. Z=Y / 2×100 5-4. MEK insoluble content (mass%) = 100-Z The MEK insoluble matter (mass %) is the average value of three measurements.

[0092] [Softening point of resin] Using a flow tester "CFT-500D" (Shimadzu Corporation), 1 g of sample is heated at a temperature increase rate of 6°C / min while applying a load of 1.96 MPa with the plunger, and extruding it from a nozzle 1 mm in diameter and 1 mm in length. The plunger depression distance of the flow tester is plotted against the temperature, and the temperature at which half of the sample flows out is taken as the softening point.

[0093] [Glass transition temperature of resin] Using a differential scanning calorimeter "Q-100" (TA Instruments Japan), 0.01-0.02 g of sample is weighed into an aluminum pan, heated to 200°C, and cooled to 0°C at a rate of 10°C / min. The sample is then heated at a rate of 10°C / min, and the endothermic peak is measured. The glass transition temperature is the temperature at the intersection of an extension of the baseline below the maximum endothermic peak temperature and a tangent line showing the maximum slope from the rising part of the peak to the peak apex.

[0094] [Melting point of wax] Using a differential scanning calorimeter "DSC Q-100" (TA Instruments Japan), 0.01-0.02 g of sample is weighed into an aluminum pan, heated to 200°C at a rate of 10°C / min, and cooled to -10°C at a rate of 5°C / min. The sample is then heated to 180°C at a rate of 10°C / min and measured. The maximum endothermic peak temperature observed in the resulting melting endothermic curve is taken as the melting point of the wax.

[0095] [Average particle size of external additives] The average particle size refers to the number-average particle size, and is calculated by measuring the particle sizes (average values ​​of major and minor axes) of 500 particles in a scanning electron microscope (SEM) photograph and averaging these values ​​by number.

[0096] [Volume Median Particle Size of Toner] Measuring instrument: Coulter Multisizer II (manufactured by Beckman Coulter, Inc.) Aperture diameter: 50 μm Analysis software: Coulter Multisizer AccuComp version 1.19 (Beckman Coulter, Inc.) Electrolyte: Isoton II (Beckman Coulter, Inc.) Dispersion liquid: Emulgen 109P (Kao Corporation, polyoxyethylene lauryl ether, HLB (Griffin): 13.6) dissolved in the electrolyte to adjust the concentration to 5% by mass Dispersion conditions: 10 mg of the measurement sample was added to 5 mL of the dispersion, and the mixture was dispersed for 1 minute using an ultrasonic disperser (machine name: US-1 manufactured by SND Co., Ltd., output: 80 W). Then, 25 mL of the electrolyte solution was added, and the mixture was further dispersed for 1 minute using the ultrasonic disperser to prepare a sample dispersion. Measurement conditions: The sample dispersion was added to 100 mL of the electrolyte solution so that the particle size of 30,000 particles could be measured in 20 seconds. 30,000 particles were measured, and the volume median particle size (D 50 ) is found.

[0097] Resin manufacturing example 1 The raw material monomers for polyester resins other than trimellitic anhydride, esterification catalyst, and hydrocarbon wax shown in Tables 1 and 2 were placed in a 10-liter four-neck flask equipped with a thermometer, stainless steel stirrer, downflow condenser, and nitrogen inlet tube. The flask was heated to 160°C in a nitrogen atmosphere in a mantle heater, and a mixed solution of the raw material monomers for styrene resins, bireactive monomers, and polymerization initiators shown in Tables 1 and 2 was added dropwise over 1 hour. The temperature was then maintained at 160°C for 30 minutes to allow addition polymerization, followed by heating to 200°C over 1 hour and reaction for 1 hour under a reduced pressure of 8 kPa. The temperature was then raised to 235°C over 30 minutes, polycondensation at 235°C for 5 hours, and reaction for 1 hour under a reduced pressure of 8 kPa. The mixture was then cooled to 220°C, and the trimellitic anhydride shown in Tables 1 and 2 was added and reaction for 1 hour. Crosslinking reaction was then carried out at 8 kPa until the desired softening point was reached, yielding hydrocarbon wax-containing composite resins (Resins A to F).

[0098] Resin manufacturing example 2 A composite resin (resin G) was obtained in the same manner as in Production Example 1 of a resin composition, except that the hydrocarbon wax in Production Example 1 was not added.

[0099] Resin manufacturing example 3 The raw material monomers for polyester resin other than trimellitic anhydride, the esterification catalyst, and the hydrocarbon wax shown in Table 2 were placed in a 10-liter four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 235°C over 2 hours in a nitrogen atmosphere in a mantle heater. After polycondensation at 235°C for 5 hours, the mixture was reacted for 1 hour under a reduced pressure of 8 kPa. The mixture was then cooled to 220°C, and trimellitic anhydride shown in Table 2 was added and reacted for 1 hour. After that, the crosslinking reaction was carried out at 8 kPa until the specified softening point was reached, to obtain a hydrocarbon wax-containing polyester resin (Resin H).

[0100] Resin manufacturing example 4 The raw material monomers for polyester resin other than trimellitic anhydride and the esterification catalyst shown in Table 2 were placed in a 10-liter four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 235°C over 2 hours in a nitrogen atmosphere in a mantle heater. After polycondensation at 235°C for 5 hours, the mixture was reacted for 1 hour under a reduced pressure of 8 kPa. The mixture was then cooled to 220°C, and trimellitic anhydride shown in Table 2 was added and reacted for 1 hour. After that, a crosslinking reaction was carried out at 8 kPa until the specified softening point was reached, yielding a polyester resin (Resin I).

[0101] Resin manufacturing example 5 The raw material monomers and esterification catalyst for the polyester resin shown in Table 3 were placed in a 10-liter four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 235°C over 2 hours in a nitrogen atmosphere in a mantle heater. After that, polycondensation was carried out at 235°C for 6 hours, and the reaction was continued under a reduced pressure of 8 kPa until the specified softening point was reached, yielding a polyester resin (Resin J).

[0102] Resin manufacturing example 6 The raw material monomers and esterification catalyst for the polyester resin other than fumaric acid shown in Table 3 were placed in a 10-liter four-neck flask equipped with a thermometer, a stainless steel stirring rod, a downflow condenser, and a nitrogen inlet tube, and the temperature was raised to 235°C over 2 hours in a nitrogen atmosphere in a mantle heater. Polycondensation was then carried out at 235°C for 3 hours, followed by reaction under a reduced pressure of 8 kPa for 1 hour. The mixture was then cooled to 190°C, and fumaric acid and a polymerization inhibitor were added. The reaction was continued at 190°C until the specified softening point was reached, yielding a polyester resin (Resin K).

[0103] [Table 1]

[0104] [Table 2]

[0105] [Table 3]

[0106] Details of the hydrocarbon waxes used are as follows: FNP-0090: Fischer-Tropsch wax, manufactured by Nippon Seiro Co., Ltd., melting point (mp) 90°C H-105: Fischer-Tropsch wax manufactured by Sasol, melting point (mp) 105°C

[0107] Examples 1 to 7 and Comparative Example 2 100 parts by weight of the binder resin shown in Table 4, 2.0 parts by weight of a positively charged charge control agent "Bontron N-79" (manufactured by Orient Chemical Industries Co., Ltd.), and 6.0 parts by weight of a colorant "Regal 330R" (manufactured by Cabot Corporation, carbon black) were added and thoroughly premixed in a Henschel mixer. The mixture was then melt-kneaded using a co-rotating twin-screw extruder at a roll rotation speed of 200 r / min (circumferential speed of 0.3 m / min) and an internal roll heating temperature of 100°C. The resulting melt-kneaded mixture was cooled and coarsely pulverized, and then melt-kneaded using a co-rotating twin-screw extruder with a total length of 1560 mm, a screw diameter of 42 mm, and a barrel inner diameter of 43 mm. The screw rotation speed was 200 r / min (circumferential speed of 0.3 m / min), the internal roll heating temperature was set to 100°C, the temperature of the kneaded mixture was 140°C, the feed rate of the kneaded mixture was 10 kg / h, and the average residence time was approximately 18 seconds.

[0108] After cooling the kneaded product, it was coarsely pulverized to about 1 mm using a hammer mill (manufactured by Hosokawa Micron Corporation). The obtained coarsely pulverized product was finely pulverized in a collision plate type jet mill pulverizer IDS-2 (manufactured by Nippon Pneumatic Co., Ltd.) at a feed rate of 4.0 kg / h to obtain the desired volume median particle size (D 50 ) was set to 6.5 μm, and the grinding pressure was adjusted to obtain toner particles.

[0109] To 100 parts by mass of the obtained toner particles, 1.0 part by mass of hydrophobic silica "NAX-50" (manufactured by Nippon Aerosil Co., Ltd., hydrophobic treatment agent: HMDS, average particle diameter: 30 nm) was added, and the mixture was mixed in a Henschel mixer to obtain a toner.

[0110] Comparative Examples 1 and 3 A toner was obtained in the same manner as in Example 1, except that 7.0 parts by mass of "H-105" (manufactured by Sasol Wax Co., Ltd.) was added as a hydrocarbon wax during pre-mixing.

[0111] Test Example 1 [Low temperature fixability] Toner was loaded into a modified "HL-2040" printer (manufactured by Brother Industries, Ltd.) to print a 2 cm square solid unfused image. Using an external fixing device modified from an "OKI MICROLINE 3010" (manufactured by OKI Data Corporation), the unfused image was fixed at each temperature, increasing the temperature of the fixing roll from 100°C to 190°C in 5°C increments at a fixing roll rotation speed of 100 mm / sec, to obtain a fixed image. Mending tape (manufactured by Sumitomo 3M Limited) was then applied to the image obtained at each fixing temperature, and a 500 g cylindrical weight was placed on top to thoroughly adhere the tape to the fixed image. The mending tape was then slowly peeled off the fixed image. The image density before and after peeling was measured using an image densitometer "GRETAG SPM50" (manufactured by GRETAG). The temperature at which the image density ratio before and after rubbing ([image density after rubbing / image density before rubbing] x 100) first exceeded 90% was taken as the minimum fixing temperature and used as an index of low-temperature fixability. The smaller the value, the better the low-temperature fixability. The results are shown in Table 4.

[0112] Test Example 2 [Hot Offset Resistance] Toner was loaded into a printer "HL-2040" (manufactured by Brother Industries, Ltd.) modified to capture unfused images, and a 2 cm square unfused solid image was printed. Using an external fixing device modified from an "OKI MICROLINE 3010" (manufactured by OKI Data Corporation), the unfused image was fixed at each temperature, increasing the temperature of the fixing roll from 100°C to 190°C in 5°C increments at a fixing roll rotation speed of 100 mm / sec, to obtain a fixed image. After printing the solid image at each temperature, a blank sheet of paper was passed through the fixing roll. The temperature at which toner staining occurred on the blank sheet of paper was recorded as the hot offset temperature, and the temperature before staining occurred was recorded as the hot offset resistance. The higher the value, the better the hot offset resistance. The results are shown in Table 4.

[0113] [Table 4]

[0114] From the above results, it is clear that the toners of Examples 1 to 7 are excellent in both low-temperature fixability and hot offset resistance. In contrast, in Comparative Example 1, in which the composite resin did not contain a hydrocarbon-based wax, the composite resin had a high loss modulus at 130°C, and both the low-temperature fixability and hot offset resistance were insufficient. In Comparative Example 2, in which a polyester resin containing a hydrocarbon-based wax was used instead of a composite resin, the polyester resin had a low storage modulus at 190°C and a large rate of change in storage modulus from 150°C to 190°C, resulting in poor hot offset resistance. In Comparative Example 3, in which a polyester resin not containing a hydrocarbon-based wax was used, the composite resin had a high loss modulus at 130°C and a large rate of change in storage modulus from 150°C to 190°C, resulting in poor low-temperature fixability. [Industrial Applicability]

[0115] The binder resin composition for toner of the present invention is suitably used for electrostatic image developing toner used for developing latent images formed in electrostatic image developing methods, electrostatic recording methods, electrostatic printing methods and the like.

Claims

1. A toner binder resin composition comprising a polyester resin containing a hydrocarbon wax, Condition 1: Loss modulus at 130°C [G''(130)] is 10,000 Pa or less, Condition 2: The storage modulus at 190°C [G'(190)] is 1,200 Pa or more, and Condition 3: The ratio of the storage modulus at 150°C [G'(150)] to the storage modulus at 190°C [G'(190)] (G'(150) / G'(190)) is 4.0 or less. the polyester resin is a composite resin obtained by bonding a polyester resin and a styrene resin, the polyester resin is a polycondensate of an alcohol component containing 60 mol % or more of an ethylene oxide adduct of bisphenol A and a carboxylic acid component containing 5 mol % to 60 mol % of trimellitic anhydride, the hydrocarbon wax does not have a functional group that reacts with a raw material monomer of the polyester resin, and the content of the hydrocarbon wax is 5 mass % to 30 mass %.

2. 2. The binder resin composition for toner according to claim 1, wherein the hydrocarbon wax is a resin added internally to a polyester resin.

3. 3. The binder resin composition for toner according to claim 1, which has a softening point of 90° C. or higher and 150° C. or lower.

4. 4. The binder resin composition for toner according to claim 1, wherein a value obtained by subtracting a content (mass%) of the hydrocarbon wax from a methyl ethyl ketone insoluble matter (mass%) when the binder resin composition is dissolved in methyl ethyl ketone is 15 mass% or more and 40 mass% or less.

5. 5. A toner for developing electrostatic images, comprising a binder resin and a colorant, the binder resin comprising the binder resin composition for toners according to claim 1.

Citation Information

Patent Citations

  • Toner, two-component developer, heat fixing method, image forming method and device unit

    JP2001075305A

  • Toner

    JP2004163570A

  • Toner for image formation, developer for image formation and image forming method

    JP2006195106A

  • Electrophotographic toner

    JP2011059418A

  • Toner binder and toner composition

    JP2013228724A