Polysilazane-containing composition, cured film, and article
A polysilazane-containing composition with perhydropolysilazane and modified polysilazane, along with a photobase generator, addresses the challenge of forming precise patterns on electronic components without acid generation, enhancing durability and adhesion in microfabrication.
Patent Information
- Application Number
- JP2022004341
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-01-14
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2042-01-14
AI Technical Summary
Existing technologies face challenges in forming cured films on electronic components with desired patterns and shapes without generating acid, ensuring adhesion to circuit boards, and maintaining durability against corrosive gases and moisture, particularly in microfabrication of small-scale semiconductor circuits.
A polysilazane-containing composition comprising perhydropolysilazane and modified polysilazane, optionally with a photobase generator, is used to form a glassy cured film through light irradiation, allowing precise patterning and adhesion without acid generation.
The composition enables the formation of dense glass films in desired shapes and locations, improving durability and adhesion while preventing corrosion and film loss, suitable for small-scale electronic components.
Smart Images

Figure 0007572978000001 
Figure 0007572978000002 
Figure 0007572978000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a polysilazane-containing composition, a cured film formed from the composition, and an article including the cured film. [Background technology]
[0002] As electronic devices become smaller and electronic components become more highly integrated, the electronic components are becoming smaller. In order to improve the performance of electronic devices, high durability is required so that performance does not deteriorate even when used for a long time. Factors that deteriorate the characteristics of electronic components include the effects of corrosive gases and moisture. One method for reducing the effects of corrosive gases and moisture is to apply a protective material to the electronic components. Patent Document 1 reports a polyimide silicone impregnating material for electronic components that suppresses corrosion of electrodes by impregnating between electronic components or between electronic components and sealing resin.
[0003] Polysilazane compounds form a high-quality glass-like cured film by curing, and therefore exhibit excellent gas barrier properties, heat resistance, and insulation properties. High reliability is required for electronic components when used in high-temperature environments. Thus, the cured film is useful as a coating that prevents moisture and corrosive gases from penetrating into electronic components. Patent Document 2 reports that the water vapor permeation amount of a resin sheet intended for sealing an organic EL element can be reduced by applying a polysilazane compound to the surface of the resin sheet to form a glass-like cured film.
[0004] In light of the above background, functional coatings, such as gas barrier coatings using polysilazane compounds, improve the performance of electronic components. However, problems arise when coating surface-mount electronic components. The problem is that if solder mounting is attempted in a state in which not only the element body but also the electrodes are covered with a coating, a significant decrease in adhesion strength to the circuit board and poor conduction may occur. Therefore, Patent Document 3 reports a method of patterning a polysilazane cured coating at desired locations on a substrate by using a water-soluble polymer or an aliphatic salt as a masking agent. Using this method, it is possible to cover the surfaces of surface-mount electronic components other than the electrodes with a coating.
[0005] However, with the recent technological development in the field of electrical and electronic engineering, electronic components are being processed into products with a side length of less than millimeter order, and semiconductor circuits are being patterned on the nanometer order. In such microfabrication, there are limitations to handling by physical contact, so it may be difficult to apply the technology of Patent Document 3.
[0006] In the pattern formation of semiconductor circuits, a technique for forming fine patterns by exposing a photosensitive resin using a photomask has been developed and is now widely used. Patent Document 4 reports a method for forming a pattern on a substrate using a photosensitive composition containing polysilazane and a photoacid generator. However, there is a concern that the electronic components to be protected and the surrounding members after mounting may be corroded due to the influence of the acid generated from this photosensitive composition.
[0007] As described in Patent Document 2, it is preferable to use perhydropolysilazane for applications as a gas barrier coating. Patent Document 5 reports a structure of a modified polysilsesquiazane suitable for pattern formation, but it is difficult to say that the optimal composition containing perhydropolysilazane has been investigated. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] JP 2004-335124 A [Patent Document 2] International Publication No. 2018 / 174116 [Patent Document 3] JP 2020-175345 A [Patent Document 4] JP 2006-85029 A [Patent Document 5] JP 2001-288270 A Summary of the Invention [Problem to be solved by the invention]
[0009] For these reasons, there is a need for the development of a technology that does not generate acid during curing, has excellent patterning properties when cured through light irradiation, and can produce a cured film in a desired shape at a desired location on a substrate.
[0010] The present invention has been made to solve the above problems, and an object of the present invention is to provide a polysilazane-containing composition which does not generate acid during curing, has excellent patterning properties of a cured film that is irradiated with light, and can form a cured film at a desired position and in a desired shape on a substrate. [Means for solving the problem]
[0011] In order to solve the above problems, the present invention provides (A-1) Perhydropolysilazane represented by the following formula (a-1): [ka] (A-2) Modified polysilazane represented by the following formula (a-2): [ka] (In the formula, R 1 , R 2are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; R 3 is a hydrogen atom or a methyl group. 1 and R 2 is not a hydrogen atom at the same time.) (B) an organic solvent, A polysilazane-containing composition comprising: the blending amount of the (A-1) component is 30 to 95 parts by mass per 100 parts by mass of the total of the (A-1) component and the (A-2) component, A polysilazane-containing composition in which, when the weight average molecular weight of the component (A-1) is w1 and the weight average molecular weight of the component (A-2) is w2, the relationship w1>2w2 is satisfied, as determined by gel permeation chromatography. to provide.
[0012] Such a polysilazane-containing composition does not generate acid upon curing, has excellent patterning properties of a cured film upon irradiation with light, and is capable of producing a cured film in a desired shape at a desired location on a substrate.
[0013] In the present invention, the component (A-2) is R 1 and R 2 Either one of is a hydrogen atom, and R 3 is preferably a modified polysilazane in which
[0014] Such a polysilazane-containing composition can improve the effects of the present invention.
[0015] In the present invention, the component (B) is preferably di-n-butyl ether.
[0016] Such a polysilazane-containing composition can improve the stability and handling properties of the composition.
[0017] In the present invention, it is preferable that the polysilazane-containing composition further contains (C) a photobase generator having a solubility of 1 mg or more in 1 g of the component (B) at 25°C.
[0018] Such a polysilazane-containing composition does not generate acid during curing, gives a transparent composition solution, accelerates the curing reaction of the components (A-1) and (A-2), and reduces contamination of the inside of a furnace or surrounding substrates and film loss of the cured product due to volatilization of the components during curing.
[0019] In the present invention, the blending amount of the component (C) is preferably 2 to 15 parts by mass per 100 parts by mass of the total of the components (A-1) and (A-2).
[0020] Such a polysilazane-containing composition can improve the effects of the present invention.
[0021] In the present invention, the component (C) is preferably at least one photobase generator selected from the following formulae (c-1) to (c-4). [ka] [ka] [ka] [ka] (In the formula, R 4 are each independently an amino group having 1 to 20 carbon atoms.
[0022] Such a polysilazane-containing composition can more reliably improve the effects of the present invention.
[0023] The present invention also provides a cured film which is a cured product of the polysilazane-containing composition.
[0024] Such a cured film can provide a dense glass film in a desired shape at a desired location on a substrate.
[0025] The present invention also provides an article comprising a substrate and a cured film formed on the surface of the substrate.
[0026] With such an article, it is possible to provide an article in which a dense glass film is formed in a desired shape at a desired location on a substrate.
[0027] In the present invention, the cured film contained in the article is preferably formed only on a part of the article.
[0028] With such an article, it is possible to provide an article in which a dense glass film is formed in a desired shape at a desired location on a substrate. Effect of the Invention
[0029] As described above, according to the present invention, the polysilazane-containing composition, which is a suitable combination of perhydropolysilazane and modified polysilazane having a preferred structure, and optionally contains a photobase generator, has excellent patterning properties for the cured film produced through a process including light irradiation, and can produce a cured film in a desired shape at a desired location on a substrate.Furthermore, according to the present invention, since it is not necessary to contain a photoacid generator, no acid is generated during curing, and corrosion of surrounding members can be suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0030] As described above, there has been a demand for the development of a polysilazane-containing composition capable of providing a cured film with excellent patterning properties. In particular, in order to maximize the characteristics of the glassy film as described above, it is necessary that the film does not generate acid during curing, has excellent patterning properties when cured by irradiation with light, and can be formed into a cured film at a desired location and in a desired shape on a substrate. Therefore, the present inventors have come up with the idea of searching for a compounding composition in which a modified polysilazane and, in some cases, a photobase generator are added to perhydropolysilazane.
[0031] Means for Solving the Problems The present inventors have conducted intensive research into the above-mentioned problems and have found that a polysilazane-containing composition comprising a combination of polysilazanes having appropriate structures is activated by light irradiation, thereby exhibiting a higher thermal curing rate than a non-irradiated area and excellent patterning properties, thereby completing the present invention.
[0032] That is, the present invention provides: (A-1) Perhydropolysilazane represented by the following formula (a-1): [ka] (A-2) Modified polysilazane represented by the following formula (a-2): [ka] (In the formula, R 1 , R 2 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; R 3 is a hydrogen atom or a methyl group. 1 and R 2 is not a hydrogen atom at the same time.) (B) an organic solvent, A polysilazane-containing composition comprising: the blending amount of the (A-1) component is 30 to 95 parts by mass per 100 parts by mass of the total of the (A-1) component and the (A-2) component, A polysilazane-containing composition in which, when the weight average molecular weight of the component (A-1) is w1 and the weight average molecular weight of the component (A-2) is w2, the relationship w1>2w2 is satisfied, as determined by gel permeation chromatography. It is.
[0033] The following describes in detail the embodiments of the present invention, but these are presented as examples, and it goes without saying that the present invention is not limited to these and various modifications are possible.
[0034] <Polysilazane-containing composition> <(A) Polysilazane> The polysilazane (A) constituting the polysilazane-containing composition of the present invention forms a glassy cured film by curing. In this specification, the definition of glassy is that it has Si-O bonds and is in a solid state without flowing when cured.
[0035] The polysilazanes (A) constituting the present invention include (A-1) perhydropolysilazane and (A-2) modified polysilazane.
[0036] The polysilazane-containing composition of the present invention contains polysilazanes having two or more structures in which component (A-2) is added to component (A-1) in order to realize excellent patterning properties by adjusting the extremely high curing reactivity of perhydropolysilazane (A-1).
[0037] From the viewpoints of solubility in the organic solvent of component (B) and workability during application, the weight-average molecular weight of polysilazane (A) (component (A-1) and component (A-2)) is preferably 100 to 1,000,000, more preferably 300 to 100,000, and even more preferably within the range of 500 to 50,000. A weight-average molecular weight of 100 or more is preferable because it has low volatility and there is no risk of deterioration of the film quality of the coating film due to volatilization of the organic solvent and volatilization of the polysilazane itself during the curing process, while a weight-average molecular weight of 1,000,000 or less is preferable because it has high solubility in organic solvents.
[0038] The weight average molecular weight referred to in this specification refers to a value obtained by gel permeation chromatography (GPC) measured under the following conditions using polystyrene as a standard substance. [Measurement conditions] Developing solvent: Tetrahydrofuran (THF) Flow rate: 0.35mL / min Detector: Differential refractive index detector Column: TSKguardcolumn SuperMP(HZ)-M TSKgel SuperMultipore HZ-M (4.6mmI.D.×15cm,4μm×4) (All manufactured by Tosoh Corporation) Column temperature: 40℃ Sample injection volume: 20 μL (THF solution with a concentration of 0.5% by mass)
[0039] Of the polysilazanes (A), the polysilazane of the component (A-1) is a perhydropolysilazane represented by the following formula (a-1). [ka] Among the polysilazanes (A), the polysilazane of the component (A-2) is a modified polysilazane represented by the following formula (a-2). [ka] (In the formula, R 1 , R 2 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; R 3 is a hydrogen atom or a methyl group. 1 and R 2 is not a hydrogen atom at the same time.)
[0040] Ingredient (A-1) The component (A-1) is a perhydropolysilazane and therefore forms a denser glass film with a higher crosslinking density than the component (A-2), and therefore forms the main skeleton that governs the physical properties of the cured film in the present invention.
[0041] The component (A-1) may be used alone or in the form of a mixture of perhydropolysilazanes selected from two or more perhydropolysilazanes having the same polysilazane skeleton but different weight average molecular weights.
[0042] Ingredient (A-2) The component (A-2) is a polysilazane represented by the above formula (a-2), R 1 and R 2In this specification, the definition of modified polysilazane is that all of the substituents in the above formula (a-2) are not hydrogen atoms at the same time, and at least one of them is an organic substituent.
[0043] In the above formula (a-2), R 1 , R 2 The aliphatic hydrocarbon group has 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and examples thereof include alkyl groups such as methyl group, ethyl group, n-propyl group, isopropyl group, n-butyl group, isobutyl group, t-butyl group, n-pentyl group, neopentyl group, hexyl group, octyl group, nonyl group, and decyl group; cycloalkyl groups such as cyclopentyl group, cyclohexyl group, norbornyl group, and adamantyl group; and alkenyl groups such as vinyl group, allyl group, and 7-octenyl group. Among these, methyl group and vinyl group are preferable, and methyl group is more preferable.
[0044] In the above formula (a-2), R 1 , R 2 The aromatic hydrocarbon group has 6 to 12 carbon atoms, preferably 6 to 7 carbon atoms, and examples thereof include aryl groups such as a phenyl group, a tolyl group, a xylyl group, and a naphthyl group, and aralkyl groups such as a benzyl group, a phenylethyl group, a phenylpropyl group, and a p-vinylbenzyl group, and among these, a phenyl group is preferable.
[0045] In the above formula (a-2), R 1 , R 2 The alkoxy group has 1 to 10 carbon atoms, preferably 1 to 4 carbon atoms, and examples thereof include a methoxy group, an ethoxy group, a propoxy group, a butoxy group, a pentoxy group, a hexoxy group, a heptoxy group, an octoxy group, a nonoxy group, and a decoxy group. Of these, a methoxy group and an ethoxy group are preferable, and a methoxy group is more preferable.
[0046] In the above formula (a-2), R 3 is a hydrogen atom or a methyl group, and is preferably a hydrogen atom.
[0047] Among them, the component (A-2) is R in the above formula (a-2).1 and R 2 Either one of is a hydrogen atom, and R 3 is preferably a modified polysilazane in which
[0048] The curing reaction rate of the component (A-2) is slower than that of the component (A-1) due to greater steric hindrance and other reasons. Therefore, the curing reaction rate can be suitably adjusted by adding the component (A-2) to the component (A-1).
[0049] For the above reasons, the blending amount of the (A-1) component is 30 to 95 parts by mass, and more preferably 50 to 90 parts by mass, relative to 100 parts by mass of the total of the (A-1) component and the (A-2) component. If the blending amount is more than 95 parts by mass, the curing reaction rate is too fast, and not only the exposed part is cured sufficiently in the temporary curing step during patterning, but also the curing of the unexposed part proceeds too much, making it difficult to wash away the unexposed part and develop the pattern. If the blending amount is less than 30 parts by mass, the curing rate is too slow, and the temporary curing of the exposed part does not proceed satisfactorily in a short temporary curing step. Therefore, not only the unexposed part but also the exposed part is washed away by the development step, and the pattern of the cured film collapses.
[0050] In the present invention, since the highly reactive component (A-1) is used, a sufficient curing rate can be obtained by combining the components (A-1) and (A-2) in the above composition, and therefore it is not necessary to include a photoacid generator to accelerate the curing reaction.
[0051] The polysilazane of the component (A-2) can be arbitrarily selected from one type alone, a mixture of two or more types of polysilazanes, and a polysilazane copolymer having two or more types of polysilazane structures.
[0052] The (A-1) component forms a dense glassy cured film, and the (A-2) component penetrates into the gaps to form a highly accurate pattern after the development step. For this reason, when the weight average molecular weight of the (A-1) component is w1 and the weight average molecular weight of the (A-2) component is w2, as determined by gel permeation chromatography, w1>2w2, and when compatibility with the composition is taken into consideration, 200w2>w1>3w2 is more preferable, and 100w2>w1>4w2 is even more preferable.
[0053] <(B) Organic solvent> The polysilazane (A) used in the present invention is diluted with an organic solvent (B) for the purpose of improving workability during application and storage stability. The organic solvent is not particularly limited as long as it dissolves the components (A-1) and (A-2). For example, saturated aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, n-octane, isooctane, n-nonane, isononane, n-decane, and isodecane; unsaturated aliphatic hydrocarbons such as 1-octene, 1-nonene, 1-decene, 1-dodecene, and β-myrcene; saturated alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, and decahydronaphthalene; unsaturated alicyclic hydrocarbons such as cyclohexene; terpene compounds such as p-menthane, d-limonene, l-limonene, and dipentene; aromatic hydrocarbons such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene; acetone, methylbenzene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene; ketone compounds such as n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, isoamyl acetate, ethyl acetoacetate, and ethyl caproate; alkyl ether compounds such as diethyl ether, di-n-propyl ether, di-n-butyl ether, di-n-pentyl ether, di-n-hexyl ether, and tert-butyl methyl ether; aryl ether compounds such as anisole and diphenyl ether; and glycol ether compounds such as bis(2-methoxyethyl)ether, bis(2-ethoxyethyl)ether, and bis(2-butoxyethyl)ether.
[0054] From the viewpoints of workability during application and storage stability of the polysilazane, the dilution ratio is preferably within the range of 100 to 100,000 parts by mass, and more preferably 400 to 10,000 parts by mass, of component (B) per 100 parts by mass of the total of the polysilazanes (A-1) and (A-2).
[0055] As described above, from the viewpoints of workability during application, and of the ability to improve storage stability due to its comparatively low moisture absorption, di-n-butyl ether is preferred as component (B).
[0056] The water content in the polysilazane-containing composition of the present invention is preferably 500 ppm or less, more preferably 300 ppm or less. If the water content is 500 ppm or less, polysilazane and the contained water do not react with each other, so there is no risk of heat generation, hydrogen gas or ammonia gas generation, and there is also no risk of thickening or gelation. Therefore, it is preferable that the water content in the (B) component is controlled so that the water content in the polysilazane-containing composition of the present invention is within the above range.
[0057] In addition, since the polysilazane-containing composition of the present invention does not use a photoacid generator, it does not generate acid during curing, and when used as a protective agent for electronic components, it can prevent corrosion of the electronic components to be protected and the surrounding members after mounting.
[0058] <(C) Photobase Generator> The photobase generator (C) is a compound that releases an organic base by absorbing light of a specific wavelength. The organic base generated by light absorption accelerates the curing reaction of the components (A-1) and (A-2), and can reduce contamination of the inside of the curing reactor and surrounding substrates and film loss of the cured product caused by partial volatilization of the components (A-1) and (A-2) during curing. In addition, if the photobase generator (C) is used in the polysilazane-containing composition of the present invention, acid is not generated during curing of the polysilazane-containing composition of the present invention, so that when used as a protective agent for electronic components, corrosion of the electronic components to be protected and surrounding members after mounting can be avoided.
[0059] In addition, since the (C) component releases an organic base triggered by electronic excitation accompanying the absorption of light of a specific wavelength, the wavelength of the irradiated light is preferably within the range of 200 to 1,000 nm. Furthermore, when the (C) component is electronically excited using light of a wavelength of 400 to 700 nm, the (C) component has absorption of the wavelength of the irradiated light at that time, and considering that 400 to 700 nm is a wavelength range in the visible region, there is a risk of coloring of the cured film. For this reason, the wavelength of the irradiated light is more preferably 200 to 400 nm or 700 to 1000 nm, and even more preferably 200 to 400 nm.
[0060] If the component (C) is not dissolved in a solution containing the components (A) and (B), there is a concern that the component (C) may be present in a biased manner during application to a substrate, resulting in an uneven film quality of the final cured film. From the viewpoint of solubility in the composition of the present invention, the component (C) preferably has a solubility of 1 mg or more in 1 g of the organic solvent of the component (B) at 25°C.
[0061] There are no particular restrictions on the structure of component (C) so long as it is a compound that releases a base upon light absorption. From the viewpoint of solubility in component (B) as described above, however, it is preferable for the compound to be a nonionic compound.
[0062] From the viewpoint of excellent efficiency in base generation by light absorption, the component (C) more preferably has a structure selected from the group consisting of (c-1) anthryl group-containing carbamate compounds, (c-2) anthraquinyl group-containing carbamate compounds, (c-3) nitrophenyl group-containing carbamate compounds, and (c-4) hydroxyphenyl group-containing amide compounds represented by the following formulas.
[0063] [ka] [ka] [ka] [ka] (In the formula, R 4 are each independently an amino group having 1 to 20 carbon atoms.
[0064] Among these, (c-1) anthryl group-containing carbamate compounds are more preferred because of their high light absorption intensity at 365 nm.
[0065] R in the above formula (c-1), (c-2), (c-3) or (c-4) 4 Examples of the amino group represented by the formula (I) include a methylamino group, a dimethylamino group, an ethylamino group, a diethylamino group, an n-propylamino group, an isopropylamino group, a di-n-propylamino group, a diisopropylamino group, an n-butylamino group, a sec-butylamino group, an isobutylamino group, a tert-butylamino group, a di-n-butylamino group, a di-sec-butylamino group, a diisobutylamino group, a di-tert-butylamino group, an n-pentylamino group, a 2-pentylamino group, a 3-pentylamino group, an isopentylamino group, a neopentylamino group, a di-n-pentylamino group, a diisopentylamino group, a dineopentylamino group, an n-hexylamino group, a di-n- Examples of the amino groups include alkylamino groups such as a hexylamino group, an n-heptylamino group, a di-n-heptylamino group, an n-octylamino group, a di-n-octylamino group, an n-nonylamino group, a di-n-nonylamino group, an n-decylamino group, a di-n-decylamino group, a cyclohexylamino group, a dicyclohexylamino group, a bicyclo[2.2.1]heptylamino group, and a bicyclo[2.2.2]hexylamino group; and cyclic amino groups such as a piperidinyl group, a hydroxypiperidinyl group, a methacryloyloxypiperidinyl group, an imidazole group, a methylimidazole group, an ethylimidazole group, and a benzimidazole group. Of these, a diethylamino group or a dicyclohexyl group is preferred.
[0066] The blend amount of the component (C) is preferably 2 to 15 parts by mass, and more preferably 5 to 10 parts by mass, per 100 parts by mass of the combined total of the components (A-1) and (A-2).
[0067] The component (C) may be used alone or in combination of two or more kinds.
[0068] <Method of producing polysilazane-containing composition> The polysilazane-containing composition of the present invention is not limited in its production method, and can be obtained, for example, by mixing the components (A-1), (A-2), and (B) in a solution, optionally adding the component (C), and stirring the mixture under ultrasonic irradiation.
[0069] In addition, additives other than those mentioned above can be added to the composition of the present invention depending on the purpose.
[0070] <Cured film> The cured film of the present invention is a cured film that is a cured product of a polysilazane-containing composition. Such a cured film can provide a dense glass film in a desired shape at a desired location on a substrate.
[0071] <Article Containing Cured Film> The article of the present invention is an article comprising a substrate and a cured film which is a cured product of a polysilazane-containing composition formed on the surface of the substrate.
[0072] The article of the present invention is an article comprising a substrate and a cured film formed on only a portion of the substrate, the cured film being a cured product of the polysilazane-containing composition formed on the surface of the substrate. With such an article, it is possible to provide an article in which a dense glass film is formed in a desired shape at a desired location on a substrate.
[0073] <Method for forming a patterned cured film> The method for forming a patterned cured film using the polysilazane-containing composition of the present invention is not particularly limited, and may include, for example, the following steps: (i) a coating step of coating the polysilazane-containing composition on a substrate to form a polysilazane-containing coating film; (ii) an exposure step of imagewise exposing the polysilazane-containing coating film; (iii) a temporary curing step of gelling the exposed area of the polysilazane-containing coating film; (iv) a development step of removing the unexposed parts of the polysilazane-containing coating film; (v) A main curing step for curing the developed exposed areas.
[0074] (i) Coating process Examples of methods for applying the polysilazane-containing composition of the present invention to a substrate include roll coating methods using a direct gravure coater, a chamber doctor coater, an offset gravure coater, a reverse kiss coater, a reverse roll coater, a slot die, a lip coater, an air doctor coater, a single roll kiss coater, a positive rotation roll coater, a blade coater, an impregnation coater, an MB coater, an MB reverse coater, a knife coater, a bar coater, etc., spin coating methods, dispensing methods, dipping methods, spraying methods, transfer methods, slit coating methods, etc.
[0075] The thickness of the coating film varies depending on the purpose of use of the cured film, but the cured film thickness is preferably 10 to 100,000 nm, and more preferably 50 to 10,000 nm.
[0076] Before applying the polysilazane-containing composition, the substrate may be subjected to a surface modification treatment. The surface modification treatment is mainly performed for the purpose of improving the adhesion between the substrate and polysilazane, and is realized by decomposing and removing organic matter attached to the substrate surface, or by forming chemical reaction points on the substrate surface. Examples of the surface modification treatment method include argon plasma treatment, oxygen plasma treatment, ozone treatment, UV irradiation treatment, and xenon excimer light irradiation treatment, and are used depending on the type of substrate.
[0077] (ii) Exposure process Examples of light sources for forming an image by irradiating a polysilazane-containing coating film with light include metal halide lamps, LEDs, high-pressure mercury lamps, low-pressure mercury lamps, excimer lasers, and electron beams. The irradiation energy is 5 to 5000 mJ / cm. 2 is preferable, and 10 to 2000 mJ / cm2 More preferably, 50 to 1000 mJ / cm 2 More preferably, the irradiation energy is 5 mJ / cm 2 If the irradiation energy is less than 5000 mJ / cm, the polysilazane-containing coating film is not sufficiently activated, and there is no difference in the curing speed between the exposed and unexposed areas, so there is a risk that a pattern will not be formed after development. 2 If it is larger, overexposure may occur, which may cause halation.
[0078] Since the polysilazane-containing coating film reacts with moisture in the air to cause a curing reaction, curing proceeds over time not only in the exposed portion where the curing reaction is activated, but also in the unexposed portion of the polysilazane-containing coating film. For this reason, in order to obtain a highly accurate pattern, the exposure step needs to be performed in a short time, preferably within 5 minutes, more preferably within 1 minute.
[0079] In order to perform imagewise exposure, methods for distinguishing exposed and unexposed areas on the coating film include, for example, the use of a photomask and scanning exposure with light. The use of a photomask is preferred because of its high versatility for use with various light sources.
[0080] (iii) Pre-curing process The provisional curing step is carried out for the purpose of progressing the curing reaction of the exposed areas, which have been activated by the light irradiation for the thermal curing reaction, to an extent that they will not be removed in the subsequent development step.
[0081] There are no particular limitations on the method of pre-curing as long as the method allows the curing reaction to proceed. Since the exposed area has increased activity in relation to heat curing, the exposed area may be subjected to a heat treatment within a temperature range that does not deteriorate the base material.
[0082] The temporary curing temperature is preferably 20 to 200° C., more preferably 50 to 150° C., and even more preferably 80 to 120° C. If the temporary curing temperature is 20° C. or higher, a significant difference in the thermal curing speed between the exposed portion, whose activity against thermal curing has been increased by exposure, and the unexposed portion can be obtained, making it possible to form a pattern by development. If the temperature is 200° C. or lower, the unexposed portion is not immediately thermally cured, making it possible to form a pattern by development.
[0083] For the reasons mentioned above, the boiling point of the (B) organic solvent used in the present invention under atmospheric pressure (1013 hPa) is preferably from 20 to 200° C., and more preferably from 25 to 150° C. If it is within this range, the organic solvent will not remain in the temporarily cured film and will not adversely affect the accuracy of the pattern.
[0084] Since the polysilazane-containing coating film contains (A-1) perhydropolysilazane, the curing reaction proceeds by reacting with moisture in the air, so that not only the exposed portion but also the unexposed portion of the polysilazane coating film may be partially cured in the provisional curing step. For this reason, in order to obtain a highly accurate pattern, the provisional curing must be performed in a short time, preferably within 30 minutes, more preferably within 15 minutes.
[0085] Depending on the light source used in the exposure step, the light source may generate heat, which may heat the substrate and the coating film during exposure. In this case, the temporary curing by heat proceeds simultaneously with the exposure, so that it is not necessarily necessary to carry out the temporary curing step.
[0086] (iv) Development process In the unexposed areas, curing does not proceed in the provisional curing step or the degree of curing is extremely low compared to the exposed areas. For this reason, negative patterning can be achieved by removing the coating film in the unexposed areas in the development step and leaving only the exposed areas.
[0087] The developing method is not particularly limited as long as it is a method in which the coating film is brought into contact with a cleaning agent described below and the unexposed portions of the coating film are removed. For example, the coating film is immersed in the cleaning agent and, if necessary, the cleaning agent is stirred, or the cleaning agent is poured over the coating film to rinse it.
[0088] The cleaning agent is not particularly limited as long as it easily dissolves the polysilazane in the unexposed area and does not dissolve the provisionally cured coating film in the exposed area. For example, saturated aliphatic hydrocarbons such as n-pentane, isopentane, n-hexane, isohexane, n-heptane, isoheptane, n-octane, isooctane, n-nonane, isononane, n-decane, and isodecane; unsaturated aliphatic hydrocarbons such as 1-octene, 1-nonene, 1-decene, 1-dodecene, and β-myrcene; saturated alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, and decahydronaphthalene; unsaturated alicyclic hydrocarbons such as cyclohexene; terpene compounds such as p-menthane, d-limonene, l-limonene, and dipentene; aromatic compounds such as benzene, toluene, xylene, ethylbenzene, diethylbenzene, trimethylbenzene, triethylbenzene, and tetrahydronaphthalene. Examples of the ether include aromatic hydrocarbons, ketone compounds such as acetone, methyl ethyl ketone, diethyl ketone, methyl isobutyl ketone, di-n-butyl ketone, diisobutyl ketone, cyclopentanone, cyclohexanone, and diacetone alcohol; ester compounds such as n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, isoamyl acetate, ethyl acetoacetate, and ethyl caproate; alkyl ether compounds such as diethyl ether, di-n-propyl ether, di-n-butyl ether, di-n-pentyl ether, di-n-hexyl ether, and tert-butyl methyl ether; aryl ether compounds such as anisole and diphenyl ether; and glycol ether compounds such as bis(2-methoxyethyl)ether, bis(2-ethoxyethyl)ether, and bis(2-butoxyethyl)ether. Of these, toluene, xylene, and di-n-butyl ether are preferred.
[0089] In order to prevent the polysilazane in the unexposed areas from gelling due to moisture contained in the cleaner in the development step, the moisture content in the cleaner is preferably 500 ppm or less, and more preferably 300 ppm or less.
[0090] (v) Main curing process The curing treatment for the main curing is not particularly limited as long as the curing reaction proceeds, but it is necessary to select an appropriate method that does not alter the substrate. Examples of the curing treatment method include heat treatment, steam heating treatment, atmospheric pressure plasma treatment, low temperature plasma treatment, UV treatment, and excimer light treatment. EXAMPLES
[0091] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples. The weight average molecular weight is a value measured by GPC under the above conditions.
[0092] (A) Polysilazane (Synthesis example) (A-1) Synthesis of perhydropolysilazane Dehydrated pyridine (4,500 g) was cooled to -10°C under a nitrogen atmosphere, and dichlorosilane (64 L) was blown in, followed by stirring at -10°C for 1 hour. Ammonia (216 L) was blown in, and the mixture was stirred for 12 hours while returning to 25°C. The resulting solid was filtered off, and di-n-butyl ether (1,000 g) was added to the filtrate. The pyridine in the liquid was distilled off under reduced pressure while azeotroping with di-n-butyl ether, and when the distillate reached 4,500 g, di-n-butyl ether (1,000 g) was further added. Subsequently, pyridine was distilled off under reduced pressure while azeotroping with di-n-butyl ether to obtain a di-n-butyl ether solution of perhydropolysilazane. The weight-average molecular weight of this perhydropolysilazane was 6,100. Thereafter, di-n-butyl ether was added so that the amount of polysilazane was 20 parts by mass when the entire solution was 100 parts by mass. In the following Examples and Comparative Examples, this solution was used assuming that it contained 20 parts by mass of perhydropolysilazane as the component (A-1) and 80 parts by mass of di-n-butyl ether as the component (B).
[0093] (A-1)' Synthesis of perhydropolysilazane (low molecular weight) Dehydrated pyridine (4,500 g) was cooled to -10°C under a nitrogen atmosphere, and dichlorosilane (16 L) was blown in, followed by stirring at -10°C for 1 hour. Ammonia (54 L) was blown in, and the mixture was stirred for 12 hours while returning to 25°C. The resulting solid was filtered off, and di-n-butyl ether (1,000 g) was added to the filtrate. The pyridine in the liquid was distilled off under reduced pressure while azeotroping with di-n-butyl ether, and when the distillate reached 4,500 g, di-n-butyl ether (1,000 g) was further added. Subsequently, pyridine was distilled off under reduced pressure while azeotroping with di-n-butyl ether to obtain a di-n-butyl ether solution of perhydropolysilazane. The weight-average molecular weight of this perhydropolysilazane was 1,800. Thereafter, di-n-butyl ether was added so that the amount of polysilazane was 20 parts by mass when the entire solution was 100 parts by mass. In the following Examples and Comparative Examples, this solution was used assuming that it contained 20 parts by mass of perhydropolysilazane as component (A-1)' and 80 parts by mass of di-n-butyl ether as component (B).
[0094] (A-2) Synthesis of methylhydropolysilazane Dehydrated pyridine (4,000 g) was cooled to -10°C under a nitrogen atmosphere, dichloromethylsilane (873 g) was added dropwise, and the mixture was stirred at -10°C for 1 hour. Ammonia (510 L) was blown in, and the mixture was stirred for 12 hours while returning to 25°C. The mixture was filtered, and di-n-butyl ether (1,000 g) was added to the filtrate. The pyridine in the liquid was distilled off under reduced pressure while azeotroping with di-n-butyl ether, and when the distillate reached 4,000 g, di-n-butyl ether (1,000 g) was further added. The pyridine was then distilled off under reduced pressure while azeotroping with di-n-butyl ether to obtain a di-n-butyl ether solution of methylhydropolysilazane. The weight-average molecular weight of this methylhydropolysilazane was 1,200. Di-n-butyl ether was then added so that the amount of polysilazane was 20 parts by mass when the entire solution was 100 parts by mass. In the following Examples and Comparative Examples, this solution was used assuming that it contained 20 parts by mass of methylhydropolysilazane as component (A-2) and 80 parts by mass of di-n-butyl ether as component (B).
[0095] (B) Organic solvent (B-1) Di-n-butyl ether (Kanto Chemical)
[0096] (C) Photobase Generator (C-1) 9-Anthrylmethyl N,N-dicyclohexylcarbamate (Fujifilm Wako Pure Chemical Industries, Ltd.) (C-2) 9-Anthrylmethyl N,N-diethylcarbamate (Fujifilm Wako Pure Chemical Industries, Ltd.)
[0097] In addition, the solubility of both the component (C-1) and the component (C-2) in 1 g of di-n-butyl ether (B) at 25° C. was 1 mg or more.
[0098] [Examples 1 to 14, Comparative Examples 1 to 3] (1) Evaluation of solution appearance A polysilazane-containing composition was prepared by adding component (C) to a solution prepared by mixing components (A-1), (A-1)', (A-2), and (B) prepared in the above Synthesis Example in the ratios shown in Tables 1 and 2, and stirring the mixture for 5 minutes while applying ultrasonic waves (38 kHz) using an ultrasonic cleaner. The appearance of the obtained polysilazane-containing composition was visually observed, and those that were transparent were marked with ◯, and those that had precipitated were marked with ×, as shown in Tables 1 and 2.
[0099] (2) Evaluation of patterning ability (i) Coating process The polysilazane-containing composition that was evaluated as "good" in (1) was spin-coated onto a Si wafer (rotation speed: 1000 rpm, rotation time: 30 seconds).
[0100] (ii) Exposure process A photomask (exposed area has a line width of 100 μm and a line spacing of 500 μm) was placed on the coating film prepared in the above step (i), and a metal halide lamp (manufactured by Eye Graphics) was used to irradiate light with a wavelength of 365 nm at an irradiation energy of 800 mJ / cm. 2 The light was irradiated so that
[0101] (iii) Pre-curing process After removing the photomask from the coating film exposed in the above step (ii), the coating film was pre-cured by heating in a dryer at 100° C. for 10 minutes.
[0102] (iv) Development process The coating film heated in the above step (iii) was rinsed with 20 mL of toluene.
[0103] (v) Main curing process The provisionally cured film developed in the above step (iv) was heated in a dryer at 150° C. for 3 hours to produce a patterned cured film on a Si wafer.
[0104] The cured film patterns prepared through the above steps (i) to (v) were observed using a digital microscope (VHX-7000 manufactured by KEYENCE). Those that produced a pattern with a line width of 100 μm and a line spacing of 500 μm were marked with an ◯, and those in which the pattern was interrupted because the unexposed areas were not completely washed off or the exposed areas were excessively dissolved were marked with an ×, as shown in Tables 1 and 2.
[0105] (3) Evaluation of film thickness The film thickness of the patterned film prepared in the evaluation in (2) above was measured using a microspectrophotometer (OPTM-A1 manufactured by Otsuka Electronics), and the measured values are shown in Tables 1 and 2.
[0106] [Table 1] (In the table, the unit of each component is parts by mass.)
[0107] [Table 2] (In the table, the unit of each component is parts by mass.)
[0108] Although Examples 1 to 5 did not contain the component (C), the patterning properties were good and the film thickness was sufficient. Among Examples 1 to 14, the blending amounts of the components (A-1) and (A-2) were the same, but in Examples 6 to 14 (for example, compare Example 1 with Example 6) which contained the component (C), the organic base promoted the curing of the coating film in the exposed area, so that the film loss of the cured product during development was reduced and the film thickness of the obtained pattern was large. Furthermore, Examples 1 to 5 which did not contain the component (C) naturally did not generate acid, and Examples 6 to 14 which contained the component (C) used a photobase generator which did not generate acid, so that in Examples 1 to 14, no acid was generated during curing.
[0109] On the other hand, in Comparative Examples 1 and 2, the amount of the (A-1) component relative to the total of the (A-1) and (A-2) components in the present invention was outside the range of the present invention, so that the patterning of the cured film was not possible. In Comparative Example 2, the amount of the (A-1) component relative to the total of the (A-1) and (A-2) components was less than the range of the present invention, compared with Examples 1 to 14, so that the curing of the coating film was slow, and the amount of component volatilization during heating and the amount of coating film dissolution during development were large. As a result, the film thickness of the cured film was small. In Comparative Example 3, the amount of the (A-1) component eluted during the development process increased because w1>2w2 was not satisfied, compared with Examples 1 to 14. As a result, the film thickness of the cured film was small.
[0110] The present invention is not limited to the above-described embodiment. The above-described embodiment is merely an example, and anything that has substantially the same configuration as the technical idea described in the claims of the present invention and exhibits similar effects is included in the technical scope of the present invention.
[0111] [Industrial Applicability] The polysilazane-containing composition of the present invention has excellent patterning properties of the cured film produced through a process including light irradiation, and therefore can form a glassy cured film on a desired minute portion on a substrate. This can be used as a protective coating that improves the reliability of microelectronic components during long-term use without impairing their electrical and mechanical performance.
Claims
1. (A-1) Perhydropolysilazane represented by the following formula (a-1): 【Chemistry 1】 (A-2) Modified polysilazane represented by the following formula (a-2): 【Chemistry 2】 (In the formula, R 1 , R 2 are each independently a hydrogen atom, an aliphatic hydrocarbon group having 1 to 10 carbon atoms, an aromatic hydrocarbon group having 6 to 12 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms; R 3 is a hydrogen atom or a methyl group. 1 and R 2 is not a hydrogen atom at the same time.) (B) an organic solvent, A polysilazane-containing composition comprising: the blending amount of the component (A-1) is 30 to 95 parts by mass per 100 parts by mass of the total of the components (A-1) and (A-2), The weight average molecular weight of the component (A-1) determined by gel permeation chromatography is w 1 The weight average molecular weight of the component (A-2) is w 2 When we say, w 1 >2w 2 , The polysilazane-containing composition is characterized in that
2. The component (A-2) is R represented by the formula (a-2). 1 and R 2 Either one of is a hydrogen atom, and R 3 The polysilazane-containing composition according to claim 1, which is a modified polysilazane in which
3. 3. The polysilazane-containing composition according to claim 1, wherein the component (B) is di-n-butyl ether.
4. The polysilazane-containing composition according to any one of claims 1 to 3, further comprising a photobase generator (C) having a solubility of 1 mg or more in 1 g of the component (B) at 25°C.
5. The polysilazane-containing composition according to claim 4, wherein the blending amount of the component (C) is 2 to 15 parts by mass per 100 parts by mass of the total of the component (A-1) and the component (A-2).
6. The polysilazane-containing composition according to claim 4 or 5, wherein the component (C) is at least one photobase generator selected from the following formulae (c-1) to (c-4): 【Chemistry 3】 【Chemistry 4】 【Chemistry 5】 【Chemistry 6】 (In the formula, R 4 is an amino group having 1 to 20 carbon atoms.
7. A cured film, which is a cured product of the polysilazane-containing composition according to any one of claims 1 to 6.
8. An article comprising a substrate and the cured film according to claim 7 formed on the surface of the substrate.
9. The article according to claim 8 , wherein the cured film included in the article is formed only on a portion of the article.
Citation Information
Patent Citations
Modified polysil sesquiazane, photosensitive composition, and method for forming patterned modified polysil sesquiazane film
JP2001288270A
Impregnant for polyimide silicone electronic component
JP2004335124A
Method for forming pattern using photosensitive polysilazane film
JP2006085029A
Low refractive index film forming composition, manufacturing method of low refractive index film, and low refractive index film and Anti-reflection film formed by the method
JP2012181334A
Gas barrier film
JP2013233716A