Composite particles, composite particle powders and light-adjusting materials

Composite particles with a specified size and pigment coating address the limitations of conventional spacers by enhancing light control performance and preventing color unevenness in light control materials.

JP7573012B2Active Publication Date: 2024-10-24SEKISUI CHEMICAL CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2022201357
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-09-01
Filing Date
2022-12-16
Publication Date
2024-10-24
Estimated Expiration
2038-08-30

AI Technical Summary

Technical Problem

Conventional spacers in light control materials have limitations in widening the gap between base materials, leading to inadequate light control performance and potential color unevenness due to small particle size and dye usage.

Method used

Composite particles with a particle size of 10 μm to 100 μm, containing a pigment and coated with a polymer, are used as spacers to enhance light control performance and prevent color unevenness.

Benefits of technology

The composite particles effectively widen the gap, improving light control performance and preventing light leakage and color unevenness in light control materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573012000002
    Figure 0007573012000002
  • Figure 0007573012000003
    Figure 0007573012000003
  • Figure 0007573012000001
    Figure 0007573012000001
Patent Text Reader

Abstract

Provided are composite particles that can effectively suppress the occurrence of color unevenness in a light-adjusting material and can effectively improve light-adjusting performance. The composite particles according to the present invention contain a pigment and have a particle diameter of 10 μm or more and 100 μm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composite particle containing a pigment. The present invention also relates to a composite particle powder and a light-adjusting material using the composite particle. [Background technology]

[0002] Light-control materials such as light-control glass and light-control films have the property of being able to change between a transparent state and an opaque state depending on whether or not a voltage is applied, and are objects that can adjust the amount of incident light, haze, etc. Depending on the mechanism of action for changing between the transparent state and the opaque state, light-control materials are broadly classified into SPD (Suspended Particle Device) type and PDLC (Polymer Dispersed Liquid Crystal) type.

[0003] A light-adjusting material is formed by disposing a light-adjusting layer containing liquid crystal or the like between two substrates such as glass or film. In the light-adjusting material, a spacer may be used as a gap control material to control the distance between the two substrates and maintain an appropriate thickness of the light-adjusting layer. Resin particles are generally used as the spacer.

[0004] Moreover, the spacer is required to be colored in a deep color in order to prevent light leakage from the spacer portion and to suppress the occurrence of color unevenness in the light-adjusting material.

[0005] As an example of particles used in the spacer, colored particles obtained by dyeing polymer particles with a dye are disclosed in the following Patent Document 1. The polymer particles are obtained by copolymerizing a monomer having an ethylenically unsaturated group with a monomer having an ethylenically unsaturated group and an epoxy group.

[0006] Furthermore, the following Patent Document 2 discloses a spacer for a liquid crystal display element in which a hot melt adhesive layer is formed on the surface of a resin sphere. The adhesive constituting the hot melt adhesive layer is a (meth)acrylic acid ester polymer or copolymer. The weight average molecular weight (Mw) of the adhesive is 100,000 or more and 500,000 or less. The ratio (Mw / Mn) of the weight average molecular weight (Mw) to the number average molecular weight (Mn) of the adhesive is 2.0 or more and 2.5 or less. The glass transition temperature of the adhesive is 60°C or more and 90°C or less. Patent Document 2 describes that the resin spheres are colored polymer particles in which a pigment is uniformly dispersed inside the polymer particles. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Japanese Patent Application Publication No. 4-103633 [Patent Document 2] Japanese Patent Application Publication No. 8-101394 Summary of the Invention [Problem to be solved by the invention]

[0008] In a light-adjusting material used in a vehicle or the like, the distance between the two substrates may be widened to increase the thickness of the light-adjusting layer in order to improve the light-adjusting performance of adjusting the amount of incident light, haze, etc. In a conventional spacer as described in Patent Document 2, the particle diameter of the spacer is small, so the distance between the two substrates in the light-adjusting material cannot be made sufficiently wide, and it is difficult to increase the thickness of the light-adjusting layer. As a result, the light-adjusting performance of the light-adjusting material of adjusting the amount of incident light, haze, etc. may be reduced.

[0009] In addition, in the conventional spacer as described in Patent Document 1, the spacer is colored with a dye, so the light-shielding property of the spacer cannot be sufficiently improved, and light leakage may occur. In addition, in the conventional spacer as described in Patent Document 1, the dye may seep into the photochromic layer. As a result, color unevenness may occur in the photochromic material.

[0010] An object of the present invention is to provide a composite particle capable of effectively suppressing the occurrence of color unevenness in a light-adjusting material and effectively improving light-adjusting performance. Another object of the present invention is to provide a composite particle powder and a light-adjusting material using the above composite particle. [Means for solving the problem]

[0011] As a result of studies to solve the above problems, the inventors have discovered a configuration in which, when particles have a relatively large particle diameter, the occurrence of color unevenness in the dimming material can be effectively suppressed and the dimming performance can be effectively improved.

[0012] According to a broad aspect of the present invention, there is provided a composite particle comprising a pigment and having a particle size of 10 μm or more and 100 μm or less.

[0013] In a specific aspect of the composite particles according to the present invention, the 20% K value is 5000 N / mm 2 That's all.

[0014] In a specific aspect of the composite particle according to the present invention, the breaking strain is 30% or more and 70% or less.

[0015] In a specific aspect of the composite particle according to the present invention, the breaking load value is 20 mN or more and 100 mN or less.

[0016] In a specific aspect of the composite particle according to the present invention, the total light transmittance is less than 5%.

[0017] In a specific aspect of the composite particle according to the present invention, the content of the pigment is 2% by weight or more and 7% by weight or less, based on 100% by weight of the composite particle.

[0018] In a specific aspect of the composite particle according to the present invention, the average particle size of the pigment is 50 nm or more and 350 nm or less.

[0019] In a specific aspect of the composite particles according to the present invention, the pigment is carbon black.

[0020] In a specific aspect of the composite particles according to the present invention, a surface of the carbon black is coated with a polymer.

[0021] In a specific aspect of the composite particle according to the present invention, the composite particle is used as a spacer in a light-adjusting material that can change between a transparent state and an opaque state depending on the applied voltage.

[0022] In a specific aspect of the composite particle according to the present invention, the light-controlling material is a window glass or a partition of a vehicle.

[0023] According to a broad aspect of the present invention, there is provided a composite particle powder containing a plurality of the above-mentioned composite particles, the composite particle powder having an average particle size of 10 μm or more and 100 μm or less.

[0024] According to a broad aspect of the present invention, there is provided a photochromic material comprising a first photochromic material component, a second photochromic material component, and a photochromic layer disposed between the first photochromic material component and the second photochromic material component, the photochromic layer including a plurality of spacers, the spacers being the composite particles described above. Effect of the Invention

[0025] The composite particles according to the present invention contain a pigment and have a particle diameter of 10 μm or more and 100 μm or less, so that the occurrence of color unevenness in the light-adjusting material can be effectively suppressed and the light-adjusting performance can be effectively improved. [Brief description of the drawings]

[0026] [Figure 1] FIG. 1 is a cross-sectional view that illustrates a PDLC type light-adjusting material that uses composite particles according to one embodiment of the present invention as a spacer for the light-adjusting material. [Diagram 2]FIG. 2 is a cross-sectional view that illustrates a light-adjusting material of the SPD type that uses a composite particle according to one embodiment of the present invention as a spacer for the light-adjusting material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will be described in detail below.

[0028] (composite particles) The composite particle according to the present invention contains a pigment. The composite particle according to the present invention has, for example, a resin portion. The composite particle according to the present invention has, for example, a pigment contained in the resin portion. The composite particle according to the present invention is, for example, a resin particle. The composite particle according to the present invention has a particle diameter of 10 μm or more and 100 μm or less.

[0029] Since the composite particle according to the present invention has the above-mentioned configuration, the occurrence of color unevenness in the light-adjusting material can be effectively suppressed, and the light-adjusting performance can be effectively improved.

[0030] In addition, the composite particles according to the present invention are colored using a pigment instead of a dye, so that the light blocking properties of the composite particles can be sufficiently improved and light leakage can be effectively prevented. In addition, the composite particles according to the present invention are colored using a pigment instead of a dye, so that the dye does not seep into the photochromic layer. As a result, the occurrence of color unevenness in the photochromic material can be effectively suppressed.

[0031] Furthermore, since the composite particles according to the present invention have the above-mentioned configuration, when the composite particles are used as a spacer for a light-adjusting material, the light-adjusting performance of adjusting the amount of incident light, haze, etc. can be effectively improved in the light-adjusting material. For example, in the present invention, the particle diameter of the composite particles is relatively large. Therefore, the distance between the two substrates in the light-adjusting material can be sufficiently widened, and the thickness of the light-adjusting layer can be increased. As a result, the light-adjusting performance of adjusting the amount of incident light, haze, etc. can be effectively improved in the light-adjusting material used in vehicles, etc.

[0032] In the composite particle according to the present invention, the particle diameter of the composite particle is 10 μm or more and 100 μm or less. The particle diameter of the composite particle is preferably 12 μm or more, more preferably 15 μm or more, and preferably 35 μm or less, more preferably 30 μm or less, even more preferably 25 μm or less, and particularly preferably 20 μm or less. When the particle diameter of the composite particle is equal to or more than the lower limit and equal to or less than the upper limit, the distance between the two substrates in the light-adjusting material can be made wider, and the thickness of the light-adjusting layer can be made thicker. As a result, the light-adjusting performance of adjusting the amount of incident light, haze, etc., can be more effectively improved in the light-adjusting material used in vehicles, etc. In addition, when the particle diameter of the composite particle is equal to or more than the lower limit and equal to or less than the upper limit, the occurrence of color unevenness in the light-adjusting material can be more effectively suppressed. In the application of the light-adjusting material, it is significant that the particle diameter of the composite particle is not less than 10 μm, but is equal to or more than 10 μm. The particle diameter of the composite particle can be appropriately set according to the application. When the particle diameter of the composite particles is 10 μm or more and 100 μm or less, the composite particles can be suitably used for applications as light-adjusting materials.

[0033] The particle size of the composite particle means the diameter when the composite particle is a perfect sphere, and when the composite particle has a shape other than a perfect sphere, means the diameter when the composite particle is assumed to be a perfect sphere with a volume equivalent to that of the composite particle.

[0034] The particle size of the composite particles can be calculated, for example, by observing any composite particle with an electron microscope or an optical microscope.

[0035] The aspect ratio of the composite particles is preferably 1.05 or less, more preferably 1.02 or less. The lower limit of the aspect ratio of the composite particles is not particularly limited. The aspect ratio of the composite particles may be 1 or more. The aspect ratio of the composite particles indicates the major axis / minor axis. When the aspect ratio of the composite particles is the upper limit or less, the composite particles can be suitably used for light-adjusting materials.

[0036] In the case of multiple composite particles, the aspect ratio can be determined by observing 10 random composite particles under an electron microscope or optical microscope, taking the maximum and minimum diameters as the major axis and minor axis, respectively, and calculating the average major axis / minor axis value of each composite particle.

[0037] The particle size coefficient of variation (CV value) of the composite particles is preferably 10% or less, more preferably 7% or less. The lower limit of the particle size coefficient of variation (CV value) of the composite particles is not particularly limited. When the particle size coefficient of variation (CV value) of the composite particles is the upper limit or less, the composite particles can be suitably used for light-adjusting materials.

[0038] The coefficient of variation (CV value) can be measured as follows.

[0039] CV value (%) = (ρ / Dn) × 100 ρ: Standard deviation of particle size of composite particles Dn: average particle size of composite particles

[0040] The shape of the composite particles is not particularly limited, and may be spherical or may be a shape other than spherical, such as flat.

[0041] The 20% K value of the composite particles is preferably 5000 N / mm 2 More preferably, 5500N / mm 2 or more, preferably 7000N / mm 2 Less than or equal to 6500N / mm 2 When the 20% K value of the composite particles is equal to or greater than the lower limit, the thickness of the light-controlling layer in the light-controlling material can be further increased, and the light-controlling performance of adjusting the amount of incident light, haze, etc., in the light-controlling material used in vehicles, etc. can be further improved. When the 20% K value of the composite particles is equal to or less than the upper limit, scratches on the substrate in the light-controlling material can be further prevented.

[0042] The 20% K value (compressive elastic modulus when the composite particle is compressed by 20%) of the composite particle can be measured as follows.

[0043] Using a microcompression tester, one composite particle is compressed with a smooth cylindrical indenter end face (diameter 100 μm, made of diamond) under the conditions of 25° C., compression speed 0.3 mN / sec, and maximum test load 20 mN. The load value (N) and compression displacement (mm) at this time are measured. From the obtained measured values, the 20% K value (20% compression elastic modulus) of the composite particle can be calculated by the following formula. As the microcompression tester, for example, Shimadzu Corporation's "Microcompression Tester MCT-W200" and Fischer's "Fischerscope H-100" are used. The 20% K value of the composite particle is preferably calculated by arithmetic averaging of the 20% K values ​​of 50 arbitrarily selected composite particles.

[0044] 20% K value (N / mm 2 )=(3 / 2 1 / 2 )·F·S -3 / 2 ·R -1 / 2 F: Load value (N) when the composite particle is compressed by 20% S: Compressive displacement (mm) when the composite particle is compressed and deformed by 20% R: Radius of the composite particle (mm)

[0045] The K value universally and quantitatively represents the hardness of the composite particle. By using the K value, the hardness of the composite particle can be quantitatively and unambiguously represented.

[0046] The compression recovery rate of the composite particles is preferably 70% or more, more preferably 80% or more, and preferably 95% or less, more preferably 90% or less. When the compression recovery rate of the composite particles is equal to or more than the lower limit and equal to or less than the upper limit, the thickness of the light-controlling layer in the light-controlling material can be further increased, and the light-controlling performance of adjusting the amount of incident light, haze, etc., in the light-controlling material used in vehicles, etc. can be further effectively improved.

[0047] The compression recovery rate of the composite particles can be measured as follows.

[0048] Particles are scattered on a sample table. For each of the scattered composite particles, a load (reversed load value) is applied to the center of the composite particle at 25° C. with a smooth indenter end face of a cylinder (diameter 100 μm, made of diamond) using a micro-compression tester until the composite particle is subjected to a load of 1 gf. Then, the load is removed until the load value for the origin (0.40 mN) is reached. The load-compression displacement during this period is measured, and the compression recovery rate can be calculated from the following formula. The loading speed is 0.33 mN / sec. As the micro-compression tester, for example, Shimadzu Corporation's "Micro-Compression Tester MCT-W200" and Fischer's "Fischer Scope H-100" are used.

[0049] Compression recovery rate (%) = [L2 / L1] x 100 L1: Compressive displacement from the load value for the origin to the load value for the reverse load when applying a load L2: Unloading displacement from the reverse load value when releasing the load to the load value for the origin

[0050] The breaking strain of the composite particles is preferably 30% or more, more preferably 35% or more, and is preferably 80% or less, more preferably 70% or less. When the breaking strain of the composite particles is equal to or more than the lower limit and equal to or less than the upper limit, the breakage of the composite particles can be further suppressed, the thickness of the light-controlling layer in the light-controlling material can be further increased, and the light-controlling performance of adjusting the amount of incident light, haze, etc. in the light-controlling material used in vehicles, etc. can be further effectively improved.

[0051] The composite particles have a breaking load value of preferably 20 mN or more, more preferably 30 mN or more, even more preferably 40 mN or more, and preferably 100 mN or less, more preferably 80 mN or less. When the composite particles have a breaking load value of not less than the lower limit and not more than the upper limit, the composite particles can be further prevented from breaking, the thickness of the light-controlling layer in the light-controlling material can be further increased, and the light-controlling performance of adjusting the amount of incident light, haze, etc., in the light-controlling material used in vehicles, etc. can be further effectively improved.

[0052] The breaking strain and breaking load value of the composite particle can be measured as follows.

[0053] The composite particles are scattered on a sample stage. A load (breaking load value) is applied to each scattered composite particle in the direction of the center of the composite particle using a micro-compression tester until the composite particle breaks. The displacement at which the composite particle breaks is then measured. The ratio of the displacement at which the composite particle breaks to its particle diameter is taken as the breaking strain. The loading speed is 0.33 mN / sec. Examples of the micro-compression tester that can be used include Shimadzu Corporation's "Micro-Compression Tester MCT-W200" and Fischer's "Fischerscope H-100."

[0054] The total light transmittance of the composite particles is preferably less than 5%, more preferably 4% or less, and even more preferably 3% or less. The lower limit of the total light transmittance of the composite particles is not particularly limited. When the total light transmittance of the composite particles is equal to or less than the upper limit, the occurrence of light leakage can be more effectively prevented, and the occurrence of color unevenness in the light-adjusting material can be more effectively suppressed.

[0055] The total light transmittance of the composite particles can be measured as follows.

[0056] A transparent double-sided tape is attached to the surface of a transparent plate (such as a transparent acrylic plate), and composite particles are uniformly spread and attached onto the adhesive surface of the double-sided tape to prepare an evaluation sample in which the composite particles are arranged in a single layer on the double-sided tape. The total light transmittance is measured using the obtained evaluation sample. The total light transmittance can be measured, for example, using a spectrophotometer ("V-670" manufactured by JASCO Corporation). An integrating sphere can be used as the detector.

[0057] The L*a*b* color system is sometimes used to represent the color of an object. In the L*a*b* color system, lightness is represented by L*, and chromaticity indicating hue and saturation is represented by a* and b*. The L* value of the composite particles is preferably 1 or more, more preferably 5 or more, and preferably 20 or less, more preferably 15 or less. The a* value of the composite particles is preferably 0.01 or more, more preferably 0.05 or more, and preferably 1 or less, more preferably 0.5 or less. The b* value of the composite particles is preferably 0.1 or more, more preferably 0.3 or more, and preferably 3 or less, more preferably 2 or less. When the L* value of the composite particles, the a* value of the composite particles, and the b* value of the composite particles are in the above preferred ranges, the occurrence of light leakage can be more effectively prevented, and the occurrence of color unevenness in the light-adjusting material can be more effectively suppressed.

[0058] The L* value of the composite particles, the a* value of the composite particles, and the b* value of the composite particles can be measured as follows.

[0059] The L* value, a* value, and b* value of the composite particles are measured in accordance with JIS Z8781-4:2013 using the L*a*b* color system. Specifically, 2.5 g of the composite particles are filled into a measurement container (Konica Minolta's "CR-A50"). The L* value, a* value, and b* value of the filled composite particles are measured using a colorimeter (Konica Minolta's "CR-300").

[0060] From the viewpoint of further preventing the elution and diffusion of impurities, it is preferable that the surface of the composite particle is coated with a coating agent such as a silane coupling agent. The coating film of the coating agent is preferably a monomolecular film or a polymer film. The composite particle does not have to have the coating film.

[0061] The silane coupling agent is not particularly limited. Examples of the silane coupling agent include amino-based silane coupling agents such as γ-aminopropyltrimethoxysilane, N-β-(aminoethyl)-γ-aminopropyltrimethoxysilane, 3-[N-allyl-N-(2-aminoethyl)]aminopropyltrimethoxysilane, 3-(N-allyl-N-glycidyl)aminopropyltrimethoxysilane, 3-(N-allyl-N-methacryl)aminopropyltrimethoxysilane, and 3-(N,N-diglycidyl)aminopropyltrimethoxysilane; N,N-bis[3-(methyldimethoxysilyl)propyl]amine, N,N-bis[3-(trimethoxysilyl)propyl]amine, and N,N-bis[3-(methyldimethoxysilyl)propyl]ethyl. Examples of the silane coupling agents include amide-based silane coupling agents such as diamine, N,N-bis[3-(trimethoxysilyl)propyl]ethylenediamine, N-glycidyl-N,N-bis[3-(methyldimethoxysilyl)propyl]amine, and N-glycidyl-N,N-bis[3-(trimethoxysilyl)propyl]amine; vinyl-based silane coupling agents such as vinyltriethoxysilane and vinyl-tris(2-methoxyethoxy)silane; methacryl-based silane coupling agents such as γ-methacryloxypropyltrimethoxysilane; glycidyl-based silane coupling agents such as γ-glycidoxypropyltrimethoxysilane; and mercapto-based silane coupling agents such as γ-mercaptopropyltrimethoxysilane.

[0062] The method of coating the surface of the composite particles with a coating agent is not particularly limited. Examples of the method of coating the surface of the composite particles with a coating agent include a method of mixing the composite particles and the coating agent in an inorganic solvent such as water or an organic solvent such as alcohol, heating under stirring, separating the composite particles after heating by decantation or the like, and removing the solvent by drying under reduced pressure or the like, and a method of directly mixing the composite particles and the coating agent and heating them.

[0063] The composite particles are preferably used as spacers in a light-adjusting material that can change between a transparent state and an opaque state depending on the applied state of a voltage. For example, when a voltage is applied between the electrodes, the light-adjusting material becomes transparent, and when no voltage is applied between the electrodes, the light-adjusting material becomes opaque or the transparency of the light-adjusting material decreases. The composite particles are preferably used as spacers for light-adjusting materials. The composite particles are preferably used for spacers for light-adjusting materials. Since the composite particles have good compression deformation characteristics, when the composite particles are used as spacers to be disposed between two substrates in a light-adjusting material, the spacers can maintain an appropriate thickness of the light-adjusting layer, and the light-adjusting performance of adjusting the amount of incident light, haze, etc. can be more effectively improved. Furthermore, since the composite particles have the above-mentioned configuration, the occurrence of light leakage can be more effectively prevented, and the occurrence of color unevenness in the light-adjusting material can be more effectively suppressed.

[0064] When the composite particles are used as a spacer for a light-adjusting material, the light-adjusting material is preferably a light-adjusting glass, a light-adjusting film, or the like. The light-adjusting materials such as the light-adjusting glass and the light-adjusting film are preferably used for window glass or partitions of vehicles. Examples of the vehicles include vehicles, ships, and aircraft. The light-adjusting materials such as the light-adjusting glass and the light-adjusting film are preferably used for window glass or partitions of vehicles such as vehicles, ships, and aircraft. The light-adjusting material is preferably a window glass or partition, and more preferably a window glass or partition of vehicles such as vehicles, ships, and aircraft. The light-adjusting material may be a window glass or partition of vehicles such as vehicles, ships, and aircraft. The vehicle is preferably a transportation facility.

[0065] The composite particle preferably includes a base particle body and a pigment within the base particle body. The base particle body is preferably a resin particle body. In this specification, for example, "(meth)acrylate" means one or both of "acrylate" and "methacrylate", and "(meth)acrylic" means one or both of "acrylic" and "methacrylic".

[0066] As the material of the composite particle and the material of the base particle body, various organic substances are suitably used. As the material of the composite particle and the material of the base particle body, for example, polyolefin resins such as polyethylene, polypropylene, polystyrene, polyvinyl chloride, polyvinylidene chloride, polyisobutylene, polybutadiene, etc.; acrylic resins such as polymethyl methacrylate and polymethyl acrylate, etc.; polycarbonate, polyamide, phenol formaldehyde resin, melamine formaldehyde resin, benzoguanamine formaldehyde resin, urea formaldehyde resin, phenol resin, melamine resin, benzoguanamine resin, urea resin, epoxy resin, unsaturated polyester resin, saturated polyester resin, polyethylene terephthalate, polysulfone, polyphenylene oxide, polyacetal, polyimide, polyamideimide, polyether ether ketone, polyether sulfone, divinylbenzene polymer, and divinylbenzene copolymer, etc. As the divinylbenzene copolymer, etc., divinylbenzene-styrene copolymer and divinylbenzene-(meth)acrylic acid ester copolymer, etc. can be mentioned. Since the compression deformation characteristics of the composite particles can be easily controlled within a suitable range, it is preferable that the material of the composite particles and the material of the base particle body are polymers obtained by polymerizing one or more polymerizable monomers having an ethylenically unsaturated group.

[0067] When the composite particle and the base particle body are obtained by polymerizing a polymerizable monomer having an ethylenically unsaturated group, the polymerizable monomer having an ethylenically unsaturated group includes a non-crosslinkable monomer and a crosslinkable monomer.

[0068] Examples of the non-crosslinkable monomer include vinyl compounds such as styrene monomers, α-methylstyrene, and chlorostyrene; vinyl ether compounds such as methyl vinyl ether, ethyl vinyl ether, and propyl vinyl ether; acid vinyl ester compounds such as vinyl acetate, vinyl butyrate, vinyl laurate, and vinyl stearate; halogen-containing monomers such as vinyl chloride and vinyl fluoride; and (meth)acrylic compounds such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, cyclohexyl Examples of suitable (meth)acrylate compounds include alkyl (meth)acrylate compounds such as (meth)acrylate and isobornyl (meth)acrylate; oxygen-containing (meth)acrylate compounds such as 2-hydroxyethyl (meth)acrylate, glycerol (meth)acrylate, polyoxyethylene (meth)acrylate, and glycidyl (meth)acrylate; nitrile-containing monomers such as (meth)acrylonitrile; halogen-containing (meth)acrylate compounds such as trifluoromethyl (meth)acrylate and pentafluoroethyl (meth)acrylate; α-olefin compounds such as diisobutylene, isobutylene, linearne, ethylene, and propylene; and conjugated diene compounds such as isoprene and butadiene.

[0069] Examples of the crosslinkable monomer include vinyl compounds such as vinyl monomers, e.g., divinylbenzene, 1,4-divinyloxybutane, and divinylsulfone; (meth)acrylic compounds such as polyfunctional (meth)acrylate compounds, e.g., tetramethylolmethane tetra(meth)acrylate, polytetramethylene glycol diacrylate, tetramethylolmethane tri(meth)acrylate, tetramethylolmethane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate, glycerol tri(meth)acrylate, glycerol di(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, and 1,4-butanediol di(meth)acrylate; and allyl compounds. Examples of the silane compounds include silane alkoxide compounds such as tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, methyltriethoxysilane, ethyltrimethoxysilane, ethyltriethoxysilane, isopropyltrimethoxysilane, isobutyltrimethoxysilane, cyclohexyltrimethoxysilane, n-hexyltrimethoxysilane, n-octyltriethoxysilane, n-decyltrimethoxysilane, phenyltrimethoxysilane, dimethyldimethoxysilane, dimethyldiethoxysilane, diisopropyldimethoxysilane, trimethoxysilylstyrene, γ-(meth)acryloxypropyltrimethoxysilane, 1,3-divinyltetramethyldisiloxane, methylphenyldimethoxysilane, and diphenyldimethoxysilane;Examples of the silane alkoxides include silanes containing polymerizable double bonds, such as vinyltrimethoxysilane, vinyltriethoxysilane, dimethoxymethylvinylsilane, dimethoxyethylvinylsilane, diethoxymethylvinylsilane, diethoxyethylvinylsilane, ethylmethyldivinylsilane, methylvinyldimethoxysilane, ethylvinyldimethoxysilane, methylvinyldiethoxysilane, ethylvinyldiethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane; cyclic siloxanes such as decamethylcyclopentasiloxane; modified (reactive) silicone oils such as one-end modified silicone oil, both-end silicone oil, and side-chain silicone oil; and carboxyl group-containing monomers such as (meth)acrylic acid, maleic acid, and maleic anhydride.

[0070] The composite particles and the base particle body can be obtained by uniformly mixing and dispersing the pigment in the polymerizable monomer having the ethylenically unsaturated group, and polymerizing the pigment. The polymerization method is not particularly limited, and the polymerization can be performed by known methods such as radical polymerization, ionic polymerization, polycondensation (condensation polymerization, condensation polymerization), addition condensation, living polymerization, and living radical polymerization. Examples of this method include a suspension polymerization method in the presence of a radical polymerization initiator, and a seed polymerization method and a dispersion polymerization method in which a monomer is swelled and polymerized together with a radical polymerization initiator using non-crosslinked seed particles.

[0071] In order to uniformly mix and disperse the pigment in the polymerizable monomer having an ethylenically unsaturated group, a ball mill, a bead mill, a sand mill, an attritor, a sand grinder, a nanomizer, etc. may be used. In this case, a dispersant, etc. may be added to improve the dispersibility of the pigment.

[0072] The dispersant is not particularly limited. Examples of the dispersant include water-soluble polymers such as polyvinyl alcohol, starch, methyl cellulose, carboxymethyl cellulose, hydroxyethyl cellulose, and sodium poly(meth)acrylate. Examples of the dispersant include barium sulfate, calcium sulfate, aluminum sulfate, calcium carbonate, calcium phosphate, talc, clay, and metal oxide powder.

[0073] (Pigments) The composite particle according to the present invention includes a pigment. The pigment is not particularly limited. The pigment is preferably a pigment that can make the total light transmittance of the composite particle less than 5%. The pigment may be a black pigment, a dark navy blue pigment, or a dark brown pigment. From the viewpoint of more effectively preventing the occurrence of light leakage and more effectively suppressing the occurrence of color unevenness in the light-adjusting material, the pigment is preferably a black pigment.

[0074] Examples of the black pigment include carbon black, lamp black, graphite, iron oxide, copper-chromium composite oxide, copper-chromium-zinc composite oxide, etc. The black pigment may be used alone or in combination of two or more kinds.

[0075] Examples of the navy blue pigment include copper phthalocyanine, cobalt phthalocyanine, cobalt aluminate, etc. The navy blue pigment may be used alone or in combination of two or more kinds.

[0076] Examples of the dark brown pigment include zinc ferrite, iron oxide, etc. The dark brown pigment may be used alone or in combination of two or more kinds.

[0077] The pigment preferably contains carbon black, titanium black, aniline black, or iron oxide. The pigment may be used alone or in combination of two or more. From the viewpoint of more effectively preventing light leakage and more effectively suppressing color unevenness in the light-adjusting material, the pigment is preferably carbon black.

[0078] The carbon black is not particularly limited. Examples of the carbon black include channel black, roll black, furnace black, thermal black, ketjen black, and acetylene black. The carbon black may be used alone or in combination of two or more.

[0079] From the viewpoint of further preventing the elution and diffusion of impurities, the surface of the pigment is preferably coated with a polymer. The surface of the pigment is preferably coated with a polymer. From the viewpoint of further preventing the elution and diffusion of impurities, the surface of the carbon black is preferably coated with a polymer. The surface of the carbon black is preferably coated with a polymer. By using a pigment whose surface is coated with a polymer, it is possible to effectively prevent a decrease in the properties of the composite particles, such as the electrical resistance, even if the amount of the pigment is increased. Furthermore, the dispersibility of the pigment is improved by coating the surface with a polymer, and the composite particles can be colored with a smaller amount. Examples of the polymer that coats the surface of the pigment include thermoplastic resins.

[0080] The thermoplastic resin is not particularly limited. Examples of the thermoplastic resin include alkyd resin, modified alkyd resin, phenol resin, natural resin modified phenol resin, maleic acid resin, natural resin modified maleic acid resin, fumaric acid resin, ester gum, rosin, petroleum resin, coumarone resin, indene resin, polyester resin, polyimide resin, polyamide resin, polycarbonate resin, polyethylene resin, epoxy resin, phenoxy resin, styrene resin, vinyl resin, acrylic resin, chlorinated rubber, benzoguanamine resin, urea resin, polyolefin resin, ethylene-vinyl acetate copolymer, and urethane resin. The thermoplastic resin may be used alone or in combination of two or more.

[0081] The method for coating the surface of the pigment with the thermoplastic resin is not particularly limited, and examples of the method for coating the surface of the pigment with the thermoplastic resin include a method of pulverizing the pigment in a hydrophobic solvent containing the thermoplastic resin using a grinding device such as a ball mill, and a method of emulsifying the pigment by adding and mixing an aqueous dispersion of the pigment in a hydrophobic solvent containing the thermoplastic resin, and then distilling off the water by heating.

[0082] The average particle size of the pigment is preferably 50 nm or more, more preferably 100 nm or more, and is preferably 350 nm or less, more preferably 300 nm or less. When the average particle size of the pigment is equal to or more than the lower limit and equal to or less than the upper limit, the dispersibility of the pigment is further improved, and the pigment can be mixed more uniformly in the composite particles.

[0083] The average particle size of the pigment means the average particle size measured by any particle size measuring device. For example, a particle size distribution measuring device using the principles of laser light scattering, electrical resistance change, image analysis after imaging, etc. can be used. Specifically, the average particle size of the pigment can be measured by, for example, measuring the particle sizes of about 100,000 pigment particles using a particle size distribution measuring device (Beckman Coulter's "Multisizer4") to measure the average particle size. The average particle size refers to the number average particle size.

[0084] In 100% by weight of the composite particles, the content of the pigment is preferably 1% by weight or more, more preferably 2% by weight or more, and even more preferably 5% by weight or more, and is preferably 15% by weight or less, more preferably 10% by weight or less, and even more preferably 7% by weight or less. When the content of the pigment is equal to or more than the lower limit and equal to or less than the upper limit, the occurrence of light leakage can be more effectively prevented, and the occurrence of color unevenness in the light-adjusting material can be more effectively suppressed.

[0085] (composite particle powder) The composite particle powder according to the present invention contains a plurality of the composite particles. The average particle diameter of the composite particle powder is preferably 10 μm or more, more preferably 12 μm or more, and preferably 100 μm or less, more preferably 35 μm or less. When the average particle diameter of the composite particle powder is equal to or more than the lower limit and equal to or less than the upper limit, the distance between the two substrates in the light-adjusting material can be made wider, and the thickness of the light-adjusting layer can be made thicker. As a result, the light-adjusting performance of adjusting the amount of incident light, haze, etc., in the light-adjusting material used in vehicles, etc. can be more effectively improved. The average particle diameter of the composite particle powder can be appropriately set according to the application. When the average particle diameter of the composite particle powder is equal to or more than 10 μm and equal to or less than 100 μm, the composite particles can be suitably used for the application of the light-adjusting material.

[0086] The average particle size of a composite particle powder containing a plurality of composite particles means the average particle size of an arbitrary number of composite particles measured by an arbitrary particle size measuring device. For example, a particle size distribution measuring device using the principles of laser light scattering, electrical resistance change, image analysis after imaging, etc. can be used. Specifically, the average particle size of a composite particle powder can be measured by measuring the particle sizes of about 100,000 composite particles using a particle size distribution measuring device (Beckman Coulter's "Multisizer4") to measure the average particle size. The above average particle size indicates the number average particle size.

[0087] (Light-adjusting materials) The light-adjusting material according to the present invention includes a first light-adjusting material component, a second light-adjusting material component, and a light-adjusting layer disposed between the first light-adjusting material component and the second light-adjusting material component. In the light-adjusting material according to the present invention, the light-adjusting layer includes a plurality of spacers. In the light-adjusting material according to the present invention, the spacers are the composite particles described above.

[0088] Photochromic Layer: The light-controlling layer preferably has a light-controlling property, which is a property that allows the light transmittance and the like to change depending on the presence or absence of applied voltage, thereby making it possible to adjust the amount of incident light, haze, and the like.

[0089] The light-adjusting materials are roughly classified into a PDLC (Polymer Dispersed Liquid Crystal) type and an SPD (Suspended Particle Device) type, depending on the action mechanism of the light-adjusting layer.

[0090] When the light-adjusting material is of the PDLC type, the light-adjusting layer preferably contains a binder and a liquid crystal material dispersed in the binder.

[0091] The liquid crystal material is not particularly limited. The liquid crystal material may be any liquid crystal material as long as it has the property of changing its orientation depending on the applied voltage state. The liquid crystal material may be dispersed in the binder as a continuous phase, or may be dispersed in the binder in the form of liquid crystal drops or liquid crystal capsules. Examples of the liquid crystal material include nematic liquid crystal and cholesteric liquid crystal.

[0092] Examples of the cholesteric liquid crystal material include nematic liquid crystals and smectic liquid crystals such as steroid cholesterol derivatives, Schiff bases, azos, azoxys, benzoates, biphenyls, terphenyls, cyclohexyl carboxylates, phenylcyclohexanes, biphenylcyclohexanes, pyrimidines, dioxanes, cyclohexylcyclohexane esters, cyclohexylethanes, cyclohexanes, tolanes, alkenyls, stilbenes, and condensed polycyclics. Examples of the cholesteric liquid crystal material include materials obtained by adding chiral components of optically active materials such as Schiff bases, azos, esters, and biphenyls to the above mixed liquid crystals. Only one type of cholesteric liquid crystal material may be used, or two or more types may be used in combination.

[0093] The binder holds the liquid crystal material and suppresses the flow of the liquid crystal material. The binder is not particularly limited as long as it is not dissolved in the liquid crystal material, has a strength capable of withstanding an external force, and has high transmittance to reflected light and incident light. Examples of the binder material include water-soluble polymer materials such as gelatin, polyvinyl alcohol, cellulose derivatives, polyacrylic acid polymers, ethyleneimine, polyethylene oxide, polyacrylamide, polystyrene sulfonate, polyamidine, and isoprene-based sulfonic acid polymers. Examples of the binder material include materials that can be made into an aqueous emulsion such as fluorine resin, silicone resin, acrylic resin, urethane resin, and epoxy resin. Only one type of the binder material may be used, or two or more types may be used in combination.

[0094] The binder is preferably crosslinked by a crosslinking agent. The crosslinking agent is not particularly limited as long as it is a compound that forms a crosslink between the binders and hardens, makes the binder difficult to dissolve, or makes it insoluble. Examples of the crosslinking agent include acetaldehyde, glutaraldehyde, glyoxal, potassium alum hydrate, a polyvalent metal salt compound, adipic acid dihydrazide, melamine formalin oligomer, ethylene glycol diglycidyl ether, polyamide epichlorohydrin, and polycarbodiimide. The crosslinking agent may be used alone or in combination of two or more.

[0095] When the light-adjusting material is of the SPD type, the light-adjusting layer preferably includes a resin matrix and a light-adjusting suspension dispersed in the resin matrix.

[0096] The light control suspension includes a dispersion medium and light control particles dispersed in the dispersion medium.

[0097] The light control particles include carbon-based materials such as polyiodides and carbon black, metal materials such as copper, nickel, iron, cobalt, chromium, titanium, and aluminum, and inorganic compound materials such as silicon nitride, titanium nitride, and aluminum oxide. These materials may also be particles coated with a polymer. The light control particles may be used alone or in combination of two or more kinds.

[0098] The dispersion medium disperses the light control particles in a flowable state. The dispersion medium is preferably a material that selectively adheres to the light control particles, covers the light control particles, and acts to move the light control particles to the phase-separated droplet phase during phase separation with the resin matrix, and has no electrical conductivity and no affinity with the resin matrix. Furthermore, the dispersion medium is preferably a liquid copolymer that has a refractive index similar to that of the resin matrix when made into a light control laminate. As the liquid copolymer, a (meth)acrylic acid ester oligomer having a fluoro group or a hydroxyl group is preferable, and a (meth)acrylic acid ester oligomer having a fluoro group and a hydroxyl group is more preferable. When such a copolymer is used, the monomer unit of the fluoro group or the hydroxyl group faces the light control particles, and the remaining monomer unit stabilizes the droplets of the light control suspension in the resin matrix. For this reason, the light control particles are easily dispersed in the light control suspension, and the light control particles are easily guided into the droplets that are phase-separated during phase separation with the resin matrix.

[0099] Examples of the (meth)acrylic acid ester oligomer having a fluoro group or a hydroxyl group include 2,2,2-trifluoroethyl methacrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer, 3,5,5-trimethylhexyl acrylate / 2-hydroxypropyl acrylate / fumaric acid copolymer, butyl acrylate / 2-hydroxyethyl acrylate copolymer, 2,2,3,3-tetrafluoropropyl acrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer, 1H,1H,5H-octafluoropentyl acrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer, 1H,1H,5H-octafluoropentyl acrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer, and 1H,1H,5H-octafluoropentyl acrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer. , 1H,2H,2H-heptadecafluorodecyl / butyl acrylate / 2-hydroxyethyl acrylate copolymer, 2,2,2-trifluoroethyl methacrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer, 2,2,3,3-tetrafluoropropyl methacrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer, 1H,1H,5H-octafluoropentyl methacrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer, and 1H,1H,2H,2H-heptadecafluorodecyl methacrylate / butyl acrylate / 2-hydroxyethyl acrylate copolymer. It is more preferable that these (meth)acrylic acid ester oligomers have both a fluoro group and a hydroxyl group.

[0100] The weight average molecular weight of the (meth)acrylic acid ester oligomer is preferably 1,000 or more, more preferably 2,000 or more, and is preferably 20,000 or less, more preferably 10,000 or less.

[0101] The weight average molecular weight is a weight average molecular weight calculated as polystyrene, measured by gel permeation chromatography.

[0102] When the light-adjusting material is of the SPD type, the light-adjusting layer can be produced using a resin material for forming the resin matrix and the light adjusting suspension.

[0103] The resin material is preferably a resin material that is cured by irradiation with energy rays. Examples of the resin material that is cured by irradiation with energy rays include a polymer composition containing a photopolymerization initiator and a polymer compound that is cured by energy rays such as ultraviolet rays, visible rays, and electron beams. Examples of the polymer composition include a polymer composition containing a polymerizable monomer having an ethylenically unsaturated group and a photopolymerization initiator. Examples of the polymerizable monomer having an ethylenically unsaturated group include a non-crosslinkable monomer and a crosslinkable monomer.

[0104] The non-crosslinkable monomer may be the non-crosslinkable monomer described above.The crosslinkable monomer may be the crosslinkable monomer described above.

[0105] Examples of the photopolymerization initiator include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-(4-(2-hydroxyethoxy)phenyl)-2-hydroxy-2-methyl-1-propan-1-one, bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2-hydroxy-2-methyl-1-phenylpropan-1-one, and (1-hydroxycyclohexyl)phenyl ketone.

[0106] The resin material may contain an organic solvent-soluble resin, a thermoplastic resin, poly(meth)acrylic acid, etc. The resin material may also contain various additives such as a coloring inhibitor, an antioxidant, and an adhesion imparting agent, and may also contain a solvent.

[0107] A first photochromic component and a second photochromic component (each of which is also referred to as a photochromic component): The material of the light-adjusting member is not particularly limited. The light-adjusting member is preferably a transparent substrate. The material of the first light-adjusting member and the material of the second light-adjusting member may be the same or different. Examples of the material of the light-adjusting member include glass plates and resin films. Examples of the glass plates include soda-lime glass for general construction, lead glass, borosilicate glass, and glass of various compositions for other uses, as well as functional glass such as heat-reflecting glass, heat-absorbing glass, and reinforced glass. Examples of the resin films include polyester films such as polyethylene terephthalate, polyolefin films such as polypropylene, and acrylic resin films. The transparent substrate is preferably a glass plate or a resin film, more preferably a resin film, because of its excellent transparency, formability, adhesion, and processability.

[0108] In order to be able to apply a voltage for dimming, the light-adjusting member preferably includes a substrate body and a transparent conductive film formed on the surface of the substrate body. Examples of the transparent conductive film include indium tin oxide (ITO), SnO2, and In2O3.

[0109] From the viewpoint of further increasing the visibility of the light-adjusting material, the visible light transmittance of the member for the light-adjusting material is preferably 75% or more, and more preferably 80% or more.

[0110] The visible light transmittance of the light-adjusting material member can be measured by spectroscopic measurement or the like in accordance with ISO13837:2008.

[0111] Fig. 1 is a cross-sectional view showing a PDLC type light control material using a composite particle according to one embodiment of the present invention as a spacer for the light control material. Note that in Fig. 1, the size, thickness, shape, and amount of the light control layer and the composite material are appropriately changed from the actual size and shape for convenience of illustration.

[0112] The PDLC type light control material 1 shown in FIG. 1 includes a first light control material component 2, a second light control material component 3, and a light control layer 4. The light control layer 4 is sandwiched between the first light control material component 2 and the second light control material component 3. The light control layer 4 is disposed between the first light control material component 2 and the second light control material component 3. A sealant may be disposed around the light control layer 4 between the first light control material component 2 and the second light control material component 3.

[0113] The light-controlling layer 4 includes liquid crystal capsules 4A, a binder 4B, and composite particles 6. The liquid crystal capsules 4A are a liquid crystal material. The liquid crystal capsules 4A are dispersed in the binder 4B. The liquid crystal capsules 4A are held in the binder 4B in a capsule-like form. The liquid crystal material may be dispersed in the binder in a capsule-like form, or may be dispersed in the binder as a continuous phase.

[0114] The composite particle 6 is used as a spacer for the light-adjusting material. The composite particle 6 is in contact with the first component 2 for the light-adjusting material and the second component 3 for the light-adjusting material. The composite particle 6 controls the gap between the first component 2 for the light-adjusting material and the second component 3 for the light-adjusting material.

[0115] A transparent electrode (not shown) is formed on each of the surfaces of the first light-adjusting member 2 and the second light-adjusting member 3. Examples of materials for the transparent electrodes include indium tin oxide (ITO).

[0116] When no voltage is applied to the PDLC-type light control material 1, the orientation of the liquid crystal molecules in the liquid crystal capsules 4A is not uniform, and therefore, due to the difference in refractive index between the binder 4B and the liquid crystal material, the incident light is refracted on the surface and inside of the liquid crystal capsules 4A and scattered within the binder, resulting in an opaque state.

[0117] When a voltage is applied to the PDLC type light control material 1, the liquid crystal molecules in the liquid crystal capsules 4A are aligned parallel to the voltage. In this state, if the refractive index of the binder 4B and the liquid crystal material are equivalent, light can pass through and the material becomes transparent.

[0118] Fig. 2 is a cross-sectional view showing a schematic diagram of an SPD type light-adjusting material using a composite particle according to one embodiment of the present invention as a spacer for the light-adjusting material. Note that in Fig. 2, the size, thickness, shape, and amount of the light-adjusting layer and the composite material are appropriately changed from the actual size and shape for convenience of illustration.

[0119] The SPD type light-adjusting material 11 shown in FIG. 2 includes a first light-adjusting material component 2, a second light-adjusting material component 3, and a light-adjusting layer 5. The light-adjusting layer 5 is sandwiched between the first light-adjusting material component 2 and the second light-adjusting material component 3. The light-adjusting layer 5 is disposed between the first light-adjusting material component 2 and the second light-adjusting material component 3.

[0120] The light control layer 5 includes droplets 5A of a light controlling suspension, a resin matrix 5B, and composite particles 6. The droplets 5A of the light controlling suspension are dispersed in the resin matrix 5B. The droplets 5A of the light controlling suspension are held in a droplet state in the resin matrix 5B.

[0121] The droplets 5A of the light control suspension contain a dispersion medium 5Aa and light control particles 5Ab. The light control particles 5Ab are dispersed in the dispersion medium 5Aa.

[0122] The composite particle 6 is used as a spacer for the light-adjusting material. The composite particle 6 is in contact with the first component 2 for the light-adjusting material and the second component 3 for the light-adjusting material. The composite particle 6 controls the gap between the first component 2 for the light-adjusting material and the second component 3 for the light-adjusting material.

[0123] A transparent electrode (not shown) is formed on each of the surfaces of the first light-adjusting member 2 and the second light-adjusting member 3. Examples of materials for the transparent electrodes include indium tin oxide (ITO).

[0124] When no voltage is applied to the SPD type dimming material 11, the incident light is absorbed, scattered, or reflected by the light control particles 5Ab due to Brownian motion of the light control particles 5Ab dispersed in the dispersion medium 5Aa that constitutes the droplets 5A of the light control suspension, and the incident light cannot pass through the dimming layer 5, resulting in an opaque state.

[0125] When a voltage is applied to the SPD type light control material 11, the light control particles 5Ab are aligned in a direction parallel to the voltage. Therefore, the incident light passes between the aligned light control particles 5Ab and can be transmitted through the light control layer 5, resulting in a transparent state.

[0126] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0127] Example 1 (1) Preparation of Composite Particle 1 Carbon black with a surface coated with a polymer was prepared. 5 parts by weight of this carbon black, 47.5 parts by weight of divinylbenzene, and 47.5 parts by weight of tetramethylolmethane triacrylate were mixed to obtain a dispersion. 20 parts by weight of benzoyl peroxide was added to this dispersion and mixed uniformly to obtain a mixed liquid. The obtained mixed liquid was added to 8500 parts by weight of a 3% by weight aqueous polyvinyl alcohol solution, thoroughly stirred, and then adjusted to a predetermined emulsion diameter with a homogenizer to obtain an emulsion.

[0128] This emulsion was transferred to a 20-liter reaction vessel equipped with a thermometer, a stirrer, and a reflux condenser, and heated to 85°C with stirring in a nitrogen atmosphere to carry out a polymerization reaction for 7 hours, and then further heated at 90°C for 3 hours to carry out a polymerization reaction, thereby obtaining a polymerization reaction liquid.

[0129] Thereafter, the polymerization reaction liquid was cooled, and the resulting particles were washed successively with water, methanol, and acetone, and then classified and dried overnight at 55°C to obtain composite particles 1 with a particle diameter of 10 μm.

[0130] (2) Preparation of photochromic material Preparation of PDLC type light control material: A light-control film was fabricated in which the obtained composite particles were dispersed at 5% by weight between two sheets of PET film onto which transparent and conductive ITO had been vapor-deposited, but with a known PDLC layer disposed between them. The light-control film was then sandwiched between two sheets of transparent glass to produce a PDLC-type light-control material.

[0131] Preparation of SPD photochromic material: A light-control film was produced in which the obtained composite particles were dispersed at 5% by weight between two PET films on which transparent and conductive ITO had been vapor-deposited, but with a known SPD layer disposed between them. The light-control film was then sandwiched between two pieces of transparent glass to produce an SPD-type light-control material.

[0132] Example 2 During the preparation of Composite Particle 1, classification conditions were changed to obtain Composite Particle 2 having a particle diameter of 15 μm, which is different from that of Composite Particle 1. A light-controlling material was prepared in the same manner as in Example 1, except that Composite Particle 2 was used instead of Composite Particle 1.

[0133] Example 3 During the preparation of the composite particles 1, the classification conditions were changed to obtain composite particles 3 having a particle diameter of 20 μm, which is different from that of the composite particles 1. A light-adjusting material was prepared in the same manner as in Example 1, except that the composite particles 3 were used instead of the composite particles 1.

[0134] Example 4 During the preparation of the composite particles 1, the classification conditions were changed to obtain composite particles 4 having a particle diameter of 25 μm, which is different from that of the composite particles 1. A light-adjusting material was prepared in the same manner as in Example 1, except that the composite particles 4 were used instead of the composite particles 1.

[0135] Example 5 During the preparation of Composite Particle 1, classification conditions were changed to obtain Composite Particle 5 having a particle diameter of 35 μm, which is different from that of Composite Particle 1. A light-adjusting material was prepared in the same manner as in Example 1, except that Composite Particle 5 was used instead of Composite Particle 1.

[0136] Example 6 During the preparation of the composite particles 1, the classification conditions were changed to obtain composite particles 6 having a particle diameter of 97 μm, which is different from that of the composite particles 1. A light-adjusting material was prepared in the same manner as in Example 1, except that the composite particles 6 were used instead of the composite particles 1.

[0137] Comparative Example 1 Composite particles having a particle diameter of 10 μm were obtained in the same manner as in Example 1, except that 5 parts by weight of carbon black whose surface was coated with a polymer was not added when preparing composite particles 1. The obtained particles were dyed with a dye ("KAYALON POLYESTER BLACK TN200" manufactured by Nippon Kayaku Co., Ltd.), washed with water and then with methanol, and dried overnight at 55° C. to obtain dyed composite particles 7 having a particle diameter of 10 μm. A light-adjusting material was prepared in the same manner as in Example 1, except that composite particles 7 were used instead of composite particles 1.

[0138] Comparative Example 2 During the preparation of the composite particles 1, the classification conditions were changed to obtain composite particles 8 having a particle diameter of 5 μm, which is different from that of the composite particles 1. A light-controlling material was prepared in the same manner as in Example 1, except that the composite particles 8 were used instead of the composite particles 1.

[0139] Comparative Example 3 In the preparation of the composite particles, the classification conditions were changed to obtain composite particles 9 having a particle diameter of 105 μm. A light-adjusting material was prepared in the same manner as in Example 1, except that composite particles 9 were used instead of composite particles 1.

[0140] (evaluation) (1) Particle size of composite particles The composite particles thus obtained were observed under an electron microscope to calculate the particle size.

[0141] (2) Average particle size of composite particle powder For the composite particle powder containing a plurality of the obtained composite particles, the particle sizes of approximately 100,000 composite particles were measured using a particle size distribution measuring device (Multisizer 4 manufactured by Beckman Coulter Inc.), and the average particle size was calculated.

[0142] (3) 20% K value of composite particles The 20% K value of the obtained composite particles was measured using Fischerscope H-100 manufactured by Fischer Co., Ltd., by the method described above.

[0143] (4) Fracture strain and fracture load of composite particles The fracture strain and fracture load value of the obtained composite particles were measured using a Fisherscope H-100 manufactured by Fisher Instruments by the above-mentioned method.

[0144] (5) Total light transmittance of composite particles The total light transmittance of the obtained composite particles was measured using "V-670" manufactured by JASCO Corporation by the method described above.

[0145] (6) L* value of composite particles, a* value of composite particles, and b* value of composite particles The L* value, a* value, and b* value of the obtained composite particles were measured using Konica Minolta's "CR-A50" and "CR-300" by the above-mentioned method.

[0146] (7) Color unevenness The obtained light-adjusting material was visually evaluated for the presence or absence of color unevenness. The color unevenness was judged according to the following criteria.

[0147] [Color unevenness criteria] ○: No uneven coloring △: There is very little color unevenness (no problem in actual use) ×: Color unevenness occurs

[0148] (8) Photochromic performance (haze) The haze of the obtained light-adjusting material was calculated when a voltage was applied and when no voltage was applied. The haze was measured using a Tokyo Denshoku Haze Meter TC-H3PDK. The obtained haze was evaluated as the light-adjusting performance of the light-adjusting material. The light-adjusting performance was evaluated according to the following criteria.

[0149] [Dimming performance (haze) evaluation criteria (when no voltage is applied)] ○: Haze is 98% or more △: Haze is 95% or more but less than 98% ×: Haze is less than 95%

[0150] [Dimming performance (haze) evaluation criteria (when voltage is applied)] ○: Haze is less than 4% △: Haze is between 4% and 6% ×: Haze is 6% or more

[0151] The results are shown in Table 1 below.

[0152] [Table 1] [Explanation of symbols]

[0153] 1. PDLC type light control material 2...First photochromic material component 3...Second photochromic material 4,5…Photochromic layer 4A…Liquid crystal capsule 4B…Binder 5A…droplet of light-adjusting suspension 5Aa...Dispersion medium 5Ab…Light adjustment particle 5B…Resin matrix 6…Composite particles 11…SPD type photochromic material

Claims

1. A spherical composite particle, The composite particles include a divinylbenzene copolymer and a pigment, the composite particle has a resin portion, and the pigment is contained in the resin portion, The particle diameter of the composite particles is 10 μm or more and 100 μm or less, The average particle size of the pigment is 50 nm or more and 350 nm or less, The composite particles have a breaking strain of 30% or more and 70% or less.

2. The 20% K value of the composite particle is 5000N / mm 2 The composite particle according to claim 1 .

3. A composite particle described in claim 1 or 2, wherein the breaking load value of the composite particle is 20 mN or more and 100 mN or less.

4. A composite particle described in any one of claims 1 to 3, wherein the total light transmittance of the composite particle is less than 5%.

5. 5. The composite particle according to claim 1, wherein the content of the pigment is 2% by weight or more and 7% by weight or less, based on 100% by weight of the composite particle.

6. The composite particle according to any one of claims 1 to 5, wherein the pigment is carbon black.

7. The composite particle according to claim 6 , wherein the surface of the carbon black is coated with a polymer.

8. A composite particle described in any one of claims 1 to 7, which is used as a spacer in a light-adjusting material that can change its state between a transparent state and an opaque state depending on the applied voltage.

9. The composite particle according to claim 8 , wherein the light control material is a window glass or a partition of a vehicle.

10. A composite particle powder containing a plurality of composite particles according to any one of claims 1 to 9, The composite particle powder has an average particle size of 10 μm or more and 100 μm or less.

11. A first light control member; A second light control member; A light-adjusting layer is disposed between the first light-adjusting member and the second light-adjusting member, The light-controlling layer includes a plurality of spacers; A light-adjusting material, wherein the spacer is the composite particle according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Dimming body for vehicle and production of this body

    JP1990091622A

  • Matte coating composition

    JP1991064374A

  • Colored fine particle and its production

    JP1992103633A

  • Spacer for liquid crystal display element, its production and liquid crystal display element using that

    JP1996101394A

  • Liquid crystal display element and light shieldable spacer

    JP1997325343A