Infrared cut filter, camera structure, and method for manufacturing infrared cut filter
The infrared cut filter with laminated resin layers addresses image quality issues in compact camera modules by minimizing reflections, enhancing resolution, and facilitating efficient production.
Patent Information
- Application Number
- JP2024508591
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-02-09
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Current compact camera modules suffer from image quality deterioration due to ghost flare and shading caused by close proximity of components, particularly with the increasing use of high-resolution CMOS image sensors with pixel pitches of 2 μm or less, leading to prolonged development times.
An infrared cut filter composed of alternately laminated high and low refractive index resin layers, integrated with an infrared absorption and reflection filter, and an anti-reflection film, optimized for reduced thickness and improved optical characteristics to minimize reflections and enhance image quality.
The infrared cut filter effectively suppresses ghost flare and shading, enabling high-resolution imaging while facilitating mass production and reducing module thickness.
Smart Images

Figure 0007573332000001 
Figure 0007573332000002 
Figure 0007573332000003
Abstract
Description
[Technical field]
[0001] The present invention relates to an infrared cut filter provided in a digital imaging device or the like. [Background technology]
[0002] It has been a quarter century since CMOS image sensors were put to practical use and digital cameras replaced film cameras as the mainstream. Digital cameras are now indispensable for mobile information terminals such as smartphones, as well as in-vehicle cameras, web cameras, security devices, and so on. Digital cameras vary greatly in size, from high-end single-lens reflex digital cameras that are the same size as conventional interchangeable lens cameras, to small camera modules built into smartphones that are about 1 / 400 the volume of conventional interchangeable lens cameras. In terms of production volume, the number of small camera modules built into smartphones and other devices is overwhelmingly greater, and in the last 10 years, the production volume of small camera modules has expanded by about 700 times compared to dedicated digital cameras, and is currently estimated to be around 6 billion units per year. Moreover, while smartphones used to be equipped with a single small camera module, they are now equipped with multiple cameras, and one smartphone is now equipped with 3 to 5 small camera modules. The reason for the multi-lens system is that as smartphones become thinner, the space available for mounting small camera modules in the optical axis direction is limited, making it difficult for one small camera module to provide lens functions ranging from ultra-wide angle to telephoto, and so they are distributed. Incidentally, in high-end single-lens reflex digital cameras, etc., sufficient spatial volume is maintained in the optical axis direction, making it possible to provide functions ranging from ultra-wide angle to telephoto with a single lens module.
[0003] On the other hand, the sensitivity curve of the CMOS sensor in a compact camera module extends beyond the visible light wavelength range (380nm to 780nm) and into the near-infrared range (wavelength of approximately 1.1μm), so images captured without any modification will have a different color tone from images seen by the human eye. For this reason, an infrared cut filter (IRCF) that cuts out near-infrared light (NIR) is essential for CMOS image sensors. In the early days of digital cameras, infrared cut filters made only of near-infrared reflective multilayer film were used, but this was prone to image degradation due to ghosting, flare, shading, etc. Therefore, current infrared cut filters (IRCFs) are shifting to combinations that also include near-infrared absorbing filters.
[0004] The infrared cut filter is usually installed between the CMOS image sensor and the lens module. The infrared cut filter is composed of a near-infrared absorption filter that absorbs near-infrared light and converts it into thermal energy, a near-infrared reflection filter made of an inorganic dielectric multilayer film, and an anti-reflection film formed on the interface between the filter and air (see, for example, JP 2006-182586 A).
[0005] The characteristics of an infrared cut filter are a composite value of the individual characteristics of three components: the characteristics of the near-infrared absorption filter, the characteristics of the near-infrared reflection filter, and the characteristics of the anti-reflection film. Infrared cut filters come in two types: an integrated structure in which the near-infrared absorption filter, near-infrared reflection filter, and anti-reflection film are combined into one piece, and a structure in which the near-infrared absorption filter and near-infrared reflection filter are separated and positioned within the optical path, but the composite characteristic value of each does not change. Summary of the Invention [Problem to be solved by the invention]
[0006] Current compact camera modules are about 8 mm thick in the optical axis direction, and incorporate components such as six to seven lenses, various filters, a CMOS image sensor, and a lens actuator with a movable width of 1.5 mm. Therefore, the distance between the components is extremely close, which makes it easy for image quality degradation to occur due to ghosts and flares caused by repeated reflections between the elements.
[0007] At the same time, there is a high need to increase the resolution even for compact camera modules, so an increasing number of models are being equipped with CMOS image sensors with pixel pitches narrowed to 2μm or less (especially sub-μCMOS image sensors with pixel pitches of 1μm or less). As a result, the trade-off for higher resolution is the occurrence of the phenomenon of petal-shaped ghost images being reflected. As a result, compact camera modules often suffer from image quality degradation, which is a factor in lengthening the development lead time for compact camera modules.
[0008] In view of the above circumstances, the present invention aims to provide an infrared cut filter that suppresses image quality degradation such as ghosts, flares, and shading, and also has improved mass productivity. [Means for solving the problem]
[0009] The present invention, which achieves the above-mentioned object, is an infrared cut filter for use in a digital camera, characterized in that it comprises a near-infrared reflective filter constructed by alternately laminating high refractive index layers made of a high refractive index resin and low refractive index layers made of a low refractive index resin, and an infrared absorbing film filter constructed of a light-transmitting resin containing a pigment or a light-transmitting resin coated with a pigment.
[0010] The infrared cut filter may further include an anti-reflection portion formed on a surface of the near-infrared reflection filter and / or the infrared absorbing film filter that comes into contact with air.
[0011] In relation to the above infrared cut filter, the high refractive index resin, the low refractive index resin, and the light transmitting resin constituting the infrared absorbing film filter may be made of an organic resin.
[0012] In relation to the above infrared cut filter, the high refractive index resin, the low refractive index resin, the light transmitting resin constituting the infrared absorbing film filter, and the antireflection portion may be made of an organic resin.
[0013] In relation to the infrared cut filter, the near-infrared reflection filter may be characterized in that the high refractive index layer and the low refractive index layer are co-extruded.
[0014] The infrared cut filter may be characterized in that the thickness of each of the high refractive index layer and / or the low refractive index layer is within a range of 10 nm to 300 nm.
[0015] In relation to the above infrared cut filter, the total number of the high refractive index layers and the low refractive index layers may be 30 or more.
[0016] In relation to the above infrared cut filter, the near-infrared reflecting filter may be characterized in that the total thickness thereof is 100 μm or less.
[0017] In relation to the infrared cut filter, the near-infrared reflective filter and the infrared absorbing film filter may be integrated together.
[0018] The infrared cut filter may be characterized in that at least one of the high refractive index resin and the low refractive index resin contains the dye, so that the infrared cut filter also functions as the infrared absorbing film filter.
[0019] In relation to the above-mentioned infrared cut filter, the antireflection portion may have a structure in which irregularities are formed on a surface of the light-transmitting resin.
[0020] In relation to the above infrared cut filter, the antireflection portion may have a multi-layer structure in which low refractive index resin films and high refractive index resin films are alternately laminated.
[0021] In relation to the above-mentioned infrared cut filter, a portion of the plurality of high refractive index layers and the plurality of low refractive index layers in the near-infrared reflection filter may serve as the low refractive index resin film and the high refractive index resin film of the anti-reflection section.
[0022] In relation to the above-mentioned infrared cut filter, the near-infrared reflection filter and the infrared absorbing film filter may be bonded to each other to be integrated, a first anti-reflection film is formed on a surface of the near-infrared reflection filter opposite the infrared absorbing film filter, and a second anti-reflection film is formed on a surface of the infrared absorbing film filter opposite the near-infrared reflection filter.
[0023] In relation to the above-mentioned infrared cut filter, the antireflection portion may have a moth-eye structure in which irregularities are formed on a surface of a light-transmitting resin.
[0024] In relation to the infrared cut filter, the total thickness of the near-infrared reflection filter, the infrared absorption film filter, and the antireflection portion may be 300 μm or less.
[0025] In relation to the above-mentioned infrared cut filter, the near-infrared reflective filter may have a film thickness occupancy rate of 20% or more based on the total thickness of the near-infrared reflective filter, the infrared absorbing film filter, and the antireflection portion.
[0026] In relation to the above-mentioned infrared cut filter, the infrared absorbing film filter may have a thickness occupancy rate of 20% or more based on the total thickness of the near-infrared reflection filter, the infrared absorbing film filter, and the antireflection portion.
[0027] In relation to the above infrared cut filter, when the wavelength at which the light transmittance decreases to 50% as the wavelength of the incident light increases in the near-infrared reflection filter alone is defined as the reflective film cutoff wavelength, the reflective film cutoff wavelength when the incident angle of the incident light is 0° may be within a range of 750 nm to 900 nm.
[0028] In relation to the above infrared cut filter, when the wavelength at which the light transmittance decreases to 50% as the wavelength of the incident light increases in the near-infrared reflection filter alone is defined as the reflective film cutoff wavelength, the wavelength fluctuation range of the reflective film cutoff wavelength when the incident angle of the incident light is changed in the range of 0° to 60° may be 150 nm or less.
[0029] In relation to the above-mentioned infrared cut filter, when a wavelength of 440 nm of incident light is defined as a reference blue wavelength, the near-infrared reflective filter alone may be characterized in that the transmittance of the reference blue wavelength is 70% or more when the incident angle of the incident light is 60°.
[0030] In relation to the above infrared cut filter, when the wavelength of incident light of 450 nm to 500 nm is defined as the low wavelength transmission band, and the average transmittance of incident light in the low wavelength transmission band in the near infrared reflection filter alone is defined as the low wavelength transmittance of the reflection film, the low wavelength transmittance of the reflection film may be 75% or more when the angle of incidence of the incident light is changed in the range of 0° to 60°.
[0031] In order to achieve the above object, the present invention may be characterized in that the resin constituting the near-infrared reflective filter and / or the infrared absorbing film filter contains an ultraviolet absorbing agent.
[0032] The present invention, which achieves the above-mentioned object, is a digital camera structure comprising an optical lens group arranged on the light incident side, and an image sensor that receives light incident through the optical lens group, characterized in that the above-mentioned infrared cut filter is arranged between the optical lens group and the image sensor.
[0033] The present invention, which achieves the above-mentioned object, is a digital camera structure comprising, in order from the light incident side, a cover glass, an optical lens group, and an image sensor, and is characterized in that the camera structure is equipped with the above-mentioned infrared cut filter, the near-infrared reflective filter is disposed between the cover glass and the optical lens group, and the infrared absorbing film filter is disposed between the optical lens group and the image sensor.
[0034] In relation to the above camera structure, the near-infrared reflective filter may be attached to the cover glass.
[0035] The present invention, which achieves the above-mentioned object, is a method for manufacturing an infrared cut filter for a digital camera, characterized in that it comprises a reflective film manufacturing process in which high refractive index layers made of a high refractive index resin and low refractive index layers made of a low refractive index resin are alternately laminated by co-extrusion molding to form a near-infrared reflective filter, and a chip processing process in which at least the near-infrared reflective filter is cut or punched to form a desired shape.
[0036] In relation to the above-mentioned method for manufacturing an infrared cut filter, the method may be characterized by including an integration step of laminating or bonding an infrared absorbing film filter composed of a light-transmitting resin containing a dye or a light-transmitting resin for an absorbing film to which a dye is applied, to the near-infrared reflecting filter.
[0037] In relation to the above-mentioned method for manufacturing the infrared cut filter, the reflective film manufacturing process may be characterized in that, in addition to the high refractive index resin and the low refractive index resin, a light-transmitting resin containing a dye that absorbs infrared rays is co-extruded to integrally mold a near-infrared reflective filter in which high refractive index layers made of the high refractive index resin and low refractive index layers made of the low refractive index resin are alternately laminated, and an infrared absorbing film filter made of the light-transmitting resin.
[0038] In relation to the above-mentioned method for manufacturing the infrared cut filter, the reflective film manufacturing process may be characterized in that a dye that absorbs infrared rays is incorporated into either the high refractive index resin or the low refractive index resin, and then the high refractive index resin and the low refractive index resin are co-extruded to integrally mold a near-infrared reflective filter in which high refractive index layers made of the high refractive index resin and low refractive index layers made of the low refractive index resin are alternately laminated, and an infrared absorbing film filter made of the high refractive index layer and the low refractive index layer that contain the dye.
[0039] The method for producing the infrared cut filter may further include an anti-reflection film application step, which is carried out before the chip processing step, and which forms an anti-reflection film on the surface in contact with air.
[0040] The method for producing the infrared cut filter may further include a mask adding step of printing a light-shielding mask, which is carried out before the chip processing step.
[0041] In relation to the above-mentioned method for manufacturing the infrared cut filter, the integration step may be characterized in that the near-infrared reflection filter and the infrared absorption film filter in roll form are supplied to a laminating device, integrated, and wound up into a roll. Effect of the Invention
[0042] According to the present invention, it is possible to obtain an infrared cut filter in which image quality degradation such as ghost flare and shading is suppressed and mass production efficiency is dramatically improved. [Brief description of the drawings]
[0043] [Figure 1] 1 is a cross-sectional view of an infrared ray cut filter according to a first embodiment of the present invention. [Diagram 2] 3 is an enlarged cross-sectional view showing a near-infrared reflective filter of the infrared cut filter. FIG. [Diagram 3] 4 is a spectral graph showing the transmission characteristics of the near-infrared reflection filter. [Figure 4] 1 is a spectral graph showing the transmission characteristics of a conventional near-infrared reflection filter for comparative explanation. [Diagram 5] 13 is a graph showing the wavelength-specific incident angle dependency characteristics of a near-infrared reflection filter according to an additional example of the first embodiment. [Figure 6] 1 is a graph showing the wavelength-specific incident angle dependency characteristics of the near-infrared reflection filter of Comparative Example 1. [Figure 7] 13 is a graph showing the wavelength-specific incident angle dependency characteristics of the near-infrared reflection filter of Comparative Example 2. [Figure 8] 4 is a spectroscopic graph showing the absorption characteristics of an infrared absorbing film filter of the infrared cut filter of the first embodiment. [Figure 9] 3A and 3B are enlarged views showing the cross-sectional shape and refractive index of an antireflection film of the infrared cut filter according to the first embodiment. [Figure 10] 4 is a spectral graph showing the transmission and reflection characteristics of the antireflection film. [Figure 11] FIG. 2 is a side view showing the structure of a laminating device used in the bonding process. [Figure 12] FIG. 2 is a side view showing the structure of a film forming apparatus used in an anti-reflection film adding process. [Figure 13] 4 is a spectroscopic graph showing the overall optical characteristics of the infrared cut filter of the first embodiment. [Figure 14] 11 is a spectroscopic graph showing the overall optical characteristics of the infrared cut filter of Comparative Example 3. [Figure 15] 1 is a cross-sectional view of a camera module incorporating an infrared cut filter according to a first embodiment. [Figure 16] 1A is a cross-sectional view of an infrared cut filter according to a second embodiment of the present invention, and FIG. 1B is a cross-sectional view of a camera module incorporating the infrared cut filter. [Figure 17] 1A is a cross-sectional view of an infrared cut filter according to a third embodiment of the present invention, FIG. 1B is a cross-sectional view of an infrared cut filter according to a fourth embodiment of the present invention, and FIG. 1C is a cross-sectional view of an infrared cut filter according to a fifth embodiment of the present invention. [Figure 18]1A is a cross-sectional view of an infrared ray cut filter according to a sixth embodiment of the present invention, FIG. 1B is a cross-sectional view of an infrared ray cut filter according to a seventh embodiment of the present invention, and FIG. 1C is a cross-sectional view of an infrared ray cut filter according to an eighth embodiment of the present invention. [Figure 19] 15. (A) is an image captured by the camera module of this embodiment shown in FIG. 15, and (B) is an image captured by a conventional camera module serving as a comparative example. [Figure 20] 15. (A) is an image captured by the camera module of this embodiment shown in FIG. 15, and (B) is an image captured by a conventional camera module serving as a comparative example. [Figure 21] This is an image taken with a conventional camera module. [Figure 22] 13A is a cross-sectional view of an infrared cut filter according to a ninth embodiment of the present invention, and FIG. 13B is a cross-sectional view of a camera structure incorporating the infrared cut filter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0044] Hereinafter, an embodiment of the present invention will be described with reference to the accompanying drawings.
[0045] FIG. 1 shows a cross-sectional structure of an infrared cut filter 1 according to a first embodiment of the present invention. The infrared cut filter 1 is an infrared cut filter for digital cameras, and includes a near-infrared reflection filter Fref1, an infrared absorbing film filter Fab1, an anti-reflection film (anti-reflection portion) Far1, and a light-shielding mask M. The near-infrared reflection filter Fref1 is configured by alternately laminating a high refractive index layer made of a high refractive index resin for the reflection film and a low refractive index layer made of a low refractive index resin for the reflection film. The infrared absorbing film filter Fab1 is configured of a light-transmitting resin for the absorption film containing a dye or a light-transmitting resin for the absorption film to which a dye is applied. The anti-reflection film Far1 is formed on the surface of the near-infrared reflection filter Fref1 and / or the infrared absorbing film filter Fab1 that is in contact with the air, and is configured of a light-transmitting resin for anti-reflection. Each member will be described in detail below.
[0046] <Near infrared reflective filter>
[0047] (Membrane structure of this embodiment) As shown enlarged in FIG. 2, the near-infrared reflection filter Fref1 of this embodiment is configured by alternately laminating a high refractive index layer Hind made of a high refractive index resin for the reflection film and a low refractive index layer Lind made of a low refractive index resin for the reflection film. The multi-layer formation of the high refractive index layer Hind and the low refractive index layer Lind can be performed by co-extrusion or spin coating. In this embodiment, the co-extrusion method using a T-die is used. In the co-extrusion method, the high refractive index resin for the reflection film and the low refractive index resin for the reflection film are extruded together in the number of layers corresponding to the laminated configuration, and these are merged and flowed out of the T-die in a film form, thereby simultaneously performing film formation and lamination (mutual bonding). In this case, there are a multi-manifold method in which each single layer of the high refractive index layer Hind and the low refractive index layer Lind are made into a film form inside the T-die and then merged, and a feed block method in which the high refractive index resin for the reflection film and the low refractive index resin for the reflection film are merged before each single layer is made into a film form, and then combined inside the T-die to form a film form, and either method may be used. According to the co-extrusion method, it is possible to alternately laminate a high refractive index layer Hind and a low refractive index layer Lind each having a thickness of 1 μm or less, which are difficult to form into a film by themselves, in a state of 100 layers or more (for example, several hundred layers) or 1,000 layers or more, and further, it is possible to temporarily wind them up on a roll as a long near-infrared reflection filter Fref1. Note that, although the co-extrusion method using a T-die is introduced here, a co-extrusion method using an inflation method may also be adopted.
[0048] The high refractive index resin for the reflective film and the low refractive index resin for the reflective film can be selected from a variety of transparent resins with different refractive indices between adjacent films, such as acrylic resins, polyester resins (e.g., polyethylene terephthalate), polycarbonate resins, polystyrene resins, polyethylene resins, polypropylene resins, cellulose resins, olefin resins, fluorine resins, and vinyl resins.
[0049] The high refractive index resin for the reflective film is preferably selected from resins having a refractive index of 1.53 or more, specifically polyester resins, polystyrene resins, polyethylene resins, polycarbonate resins, acrylic resins, and vinyl resins, and more preferably from resins having a refractive index of 1.56 or more, specifically polystyrene resins, polyester resins, and polycarbonate resins.
[0050] The low refractive index resin for the reflective film is preferably selected from resins with a refractive index of less than 1.53, specifically vinyl resins, polypropylene resins, acrylic resins, cellulose resins, and fluorine resins, and more preferably resins with a refractive index of less than 1.50, specifically vinyl resins (polyvinyl alcohol), polypropylene resins, acrylic resins (e.g., polymethyl methacrylate resins), cellulose resins, and fluorine resins. The refractive index may be adjusted by using multiple resins selected from these resins, or copolymers obtained by (co)polymerizing these resins with other resins. Furthermore, with regard to the high refractive index layers Hind and low refractive index layers Lind that are alternately laminated, it is not necessary for all the multiple high refractive index layers Hind to be made of the same resin material, and similarly, it is not necessary for all the multiple low refractive index layers Lind to be made of the same resin material.
[0051] Furthermore, in order to finely adjust the refractive index, an additive for adjusting the refractive index may be added to the high refractive index resin for the reflective film and / or the low refractive index resin for the reflective film, and further, the refractive index can be adjusted by mixing a plurality of types of resins. Furthermore, in order to improve the ultraviolet resistance, a quencher (quenching dye) such as a sulfur compound may be added to the high refractive index resin for the reflective film and / or the low refractive index resin for the reflective film.
[0052] The thickness of each of the high refractive index layer Hind and the low refractive index layer Lind is preferably formed to be equal to or less than λ / 4, where λ is the wavelength (or wavelength band) to be reflected. For example, in this embodiment, since it is required to reflect light having a wavelength λ in the range of 600 nm to 1200 nm, the thickness of each of the high refractive index layer Hind and the low refractive index layer Lind is set to be within a range of, for example, 400 nm or less.
[0053] When a high refractive index resin for a reflective film and a low refractive index resin for a reflective film are used, the difference in refractive index must be set small compared to conventional dielectric films, and the reflectance of near-infrared light at each boundary unit is therefore reduced. In order to achieve high reflectance of near-infrared light, in this embodiment, the thickness of each film is reduced and the number of layers is increased at the same time. More specifically, in this embodiment, the thickness of each of the high refractive index layer Hind and the low refractive index layer Lind is preferably, for example, 200 nm or less, more preferably 100 nm or less, even more preferably 80 nm or less, and even more preferably 50 nm or less. In this embodiment, the thickness is set to 15 nm, which is 20 nm or less. In addition, the total number of layers of the high refractive index layer Hind and the low refractive index layer Lind alternately stacked is preferably 30 layers or more, more preferably 100 layers or more, and even more preferably 200 layers or more. More preferably, the total number of layers is 300 layers or more, and for example, 400 layers are used.
[0054] By reducing each film thickness, the total film thickness of the near-infrared reflective filter Fref1 is preferably 100 μm or less, more preferably 50 μm or less. From the viewpoint of handling during mass production, the total film thickness of the near-infrared reflective filter Fref1 is preferably 10 μm or more, more preferably 30 μm or more.
[0055] As described above, the infrared absorbing film filter Fab1 of this embodiment is made of organic resin as the base material, so that it is easy to adjust the refractive index by selecting the material and mixing additives and resins. In other words, the refractive index difference between the high refractive index layer Hind and the low refractive index layer Lind can be freely set. Furthermore, by adopting the co-extrusion processing method, it is possible to control the thickness of each film to 1 μm or less. In addition, there is an advantage that the film characteristics do not deteriorate during the die-cutting processing described later.
[0056] (Reflection properties) FIG. 3 shows the reflection characteristics of the near-infrared reflection filter Fref1 alone. Here, the wavelength at which the light transmittance of the near-infrared reflection filter Fref1 decreases to 50% as the wavelength of the incident light increases is defined as the "reflection film cutoff wavelength." When the incident angle of the incident light is 0° (i.e., light perpendicular to the film), the reflection film cutoff wavelength is set within the range of 750 nm to 900 nm. More specifically, the reflection film cutoff wavelength is set within the range of 750 nm to 880 nm, still more specifically, the reflection film cutoff wavelength is set within the range of 770 nm to 880 nm, and even more specifically, the reflection film cutoff wavelength is set within the range of 780 nm to 880 nm.
[0057] In this embodiment, the fluctuation width (wavelength shift amount) Sref1 of the reflection film cutoff wavelength when the incident angle of the incident light is changed in the range of 0° to 60° is 170 nm or less, preferably 150 nm or less, more preferably 120 nm or less, and even more preferably 100 nm or less. In other words, the wavelength difference between the reflection film cutoff wavelength at an incident angle of 0° and the reflection film cutoff wavelength at an incident angle of 60° is 150 nm or less. The thinner the camera module is, the easier it is for light with a large incident angle to reach the near-infrared reflection filter Fref1. However, in the near-infrared reflection filter Fref1 of this embodiment, the wavelength shift amount Sref1 of the reflection film cutoff wavelength to the short wavelength side is suppressed, so that high-quality imaging can be realized. Note that the reflection film cutoff wavelength at an incident angle of 60° is desirably set to 650 nm or more, and does not need to be smaller than the absorption film cutoff wavelength at an incident angle of 60° of the infrared absorption film filter Fab1, so that the imaging result is less likely to be disturbed.
[0058] Furthermore, the wavelength range where the light transmittance of the near-infrared reflective filter Fref1 decreases to 10% or less is defined as the "reflective film total reflection wavelength range." The reflective film total reflection wavelength range Wref1 at an incident angle of 0° is approximately 790 nm to 1100 nm. Note that the reflective film total reflection wavelength range Wref1 varies (shifts) toward shorter wavelengths depending on the incident angle, but the amount of variation is close to the wavelength shift amount Sref1 of the reflective film cutoff wavelength.
[0059] Next, when the wavelength of incident light of 440 nm is defined as the reference blue wavelength, the near-infrared reflective filter Fref1 alone has a transmittance of 70% or more for the reference blue wavelength when the angle of incidence of the incident light is 60°. As a result, the conventional problem of the blue component decreasing due to the variation in the angle of incidence can be reduced. Furthermore, the wavelength of incident light of 450 nm to 500 nm is defined as the low wavelength band, and the average transmittance of incident light in the low wavelength band is defined as the low wavelength transmittance of the reflective film. The near-infrared reflective filter Fref1 always has a low wavelength transmittance of 75% or more when the angle of incidence of the incident light is changed in the range of 0° to 60°. In other words, in the case of the near-infrared reflection filter Fref1 alone, if the range from the reflection film cut-on wavelength with a transmittance of 50% to the reflection film cut-off is defined as the reflection film transmission band Tref1, the shape of the low-wavelength side angular region TR1 in the rectangular waveform of the reflection film transmission band Tref1 is always stable even if the incident angle varies from 0° to 60° (the angular shape on the long-wavelength side shifts toward the short-wavelength side). As a result, the near-infrared reflection filter Fref1 can reduce the phenomenon in which the low-wavelength band components are disturbed (the so-called ripple phenomenon) even if the incident angle increases.
[0060] (Comparison with the conventional method) Conventional near-infrared reflection filters achieve infrared reflection function by forming an inorganic dielectric multilayer film by a PVD process on the other side of blue glass coated with an infrared absorbing film filter material on one side. Figure 4 shows the optical characteristics of a conventional near-infrared reflection filter. Conventional near-infrared reflection filters have a fluctuation range (wavelength shift amount) Sreft of the reflection film cutoff wavelength when the incident angle of incident light is changed in the range of 0° to 60°, and the fluctuation range (wavelength shift amount) Sreft is 150 nm or more. In particular, when the incident angle is 60°, the waveform of the spectral characteristics is prone to disturbance and ripples. This is because, when the incident light is divided into a P component whose vibration plane coincides with the propagation plane and an S component whose vibration plane coincides with a plane perpendicular to the propagation plane, a deviation occurs in the transmission characteristics of the P component and the S component as the incident angle to the dielectric multilayer film increases. As a result, the reflection film cutoff wavelength of conventional near-infrared reflection filters is less than 650 nm, which is smaller than the absorption film cutoff wavelength of an infrared absorbing film filter at an incident angle of 60°, causing disturbance in the imaging results. In addition, when the wavelength of incident light of 440 nm is defined as the reference indigo wavelength, the transmittance of the reference indigo wavelength of the conventional near-infrared reflection filter fluctuates when the angle of incidence of the incident light is 60°, and may even be less than 60%. As a result, the indigo component decreases due to the fluctuation in the angle of incidence. Furthermore, in the low wavelength band of the incident light wavelength of 450 nm to 500 nm, the average transmittance of the conventional near-infrared reflection filter becomes less than 75% when the angle of incidence of the incident light is 60°, and the ripple increases.
[0061] For reference, if an inorganic dielectric multilayer film is formed on the front and back sides of the infrared absorbing film filter Fab1 made of the resin film of this embodiment by the PVD process, a high level of technology and experience is required, including the subsequent dicing process, and the yield is likely to decrease. Specifically, in the PVD process, micro-defects are inevitably generated in the inorganic dielectric multilayer film, and they must be removed afterwards by inspection of all products. Furthermore, in the dicing process, the inorganic dielectric multilayer is prone to peeling, so the peeling state must also be visually confirmed by inspection of all products. In other words, from the viewpoint of mass production, the compatibility between the resin film and the PVD process is extremely poor.
[0062] Additional Examples As the near-infrared reflection filter Fref1 of this embodiment, 200 layers of high refractive index layers Hind and low refractive index layers Lind were formed using polyethylene terephthalate resin and polymethyl methacrylate resin, and the total thickness of the near-infrared reflection filter Fref1 was set to 50 μm. As a result, the cutoff wavelength of the reflection film when the incident angle of the incident light was 0° was 850 nm. As shown in FIG. 5, for all visible light (R: red 630 nm, G: green 546 nm, B: blue 436 nm), even if the incident angle increased, the overall transparency (transmittance) was maintained at a high level, and no interference color due to reflection was observed visually. Moreover, even when the incident angle was in the range of 50° to 60°, the transmittance was maintained at 75% or more, and there was no extreme decrease, and the decrease tendency was relatively smooth. Of the RGB colors, the short-wavelength B band deviates by several points compared to the remaining R and G bands, but the amount of deviation is within a range that does not affect image quality, and the deviation width is stable across the entire incidence angle, so image quality is unlikely to change due to fluctuations in the incidence angle.
[0063] Comparative Example 1 FIG. 6 shows the optical characteristics of the near-infrared reflection filter of Comparative Example 1. In Comparative Example 1, an inorganic dielectric multilayer film was formed on a completely transparent optical glass plate by a PVD process, and the cutoff wavelength of the reflection film at an incident angle of 0° of the inorganic dielectric multilayer film was adjusted to 780 nm. In this near-infrared reflection filter, when the incident angle exceeds 50°, the transmittance of the R band drops sharply, and is completely lost at an incident angle of 70°. This is because the reflection film cutoff wavelength shifts to the low wavelength side as the incident angle increases, and the light of the R band is reflected. In the case of this near-infrared reflection filter, the red interference color was easily observed even with the naked eye. When an infrared cut filter combining a conventional near-infrared reflection filter and an absorption film was incorporated into a camera module and the image quality was checked by actual shooting, the green became relatively stronger in the peripheral part of the image (i.e., the area where the incident angle is large), and typical color shading with a lack of red was observed.
[0064] Comparative Example 2 FIG. 7 shows the optical characteristics of the near-infrared reflection filter of Comparative Example 2. In Comparative Example 2, an inorganic dielectric multilayer film is formed on an optical glass plate by a PVD process, and the cutoff wavelength of the reflection film at an incident angle of 0° of the inorganic dielectric multilayer film is adjusted to 850 nm. In this case, interference colors are no longer visible to the naked eye. Looking at the incidence angle dependency of the RGB transmittance, although there is little deviation between the RGB, when the incidence angle is 40° or more, a decrease in the transmittance of the entire RGB occurs, and when the incidence angle is 60°, the transmittance of all RGB decreases to 65%. In other words, it can be seen that although the decrease in the transmittance of the R band alone does not occur, an overall insufficient amount of transmission occurs.
[0065] <Infrared absorbing film filter>
[0066] (membrane structure) The infrared absorbing film filter Fab1 of this embodiment adopts a so-called blue film structure (near-infrared absorbing dye added to light-transmitting resin for absorbing film). The film thickness of the infrared absorbing film filter Fab1 is preferably 100 μm or less, and more preferably 50 μm or less. From the viewpoint of handling during mass production, the film thickness of the infrared absorbing film filter Fab1 is preferably 10 μm or more, and more preferably 30 μm or more.
[0067] As the organic dye having a near-infrared light absorbing function, azo compounds, phthalocyanine compounds, cyanine compounds, diimonium compounds, etc. can be used. The light-transmitting resin for the absorbing film (which can also be called a binder or base material for the organic dye) constituting the infrared absorbing film filter Fab1 is an organic polymer such as an acrylic resin, a polyester resin (e.g., polyethylene terephthalate), a polycarbonate resin, a polystyrene resin, a polyethylene resin, a polypropylene resin, a cellulose resin (e.g., cellulose triacetate), an olefin resin (e.g., cycloolefin, polyolefin), a fluorine resin, or a vinyl resin. The light-transmitting resin for the absorbing film may be a mixture of a plurality of resins, or may be a copolymer using monomers of the above resins. In addition, the light-transmitting resin for the absorbing film may be any resin having a high transmittance for light in the visible light region, and is selected in consideration of compatibility with the organic dye, the film formation process, costs, etc. In addition, in order to improve the ultraviolet resistance of the infrared absorbing film filter Fab1, a quencher (quenching dye) such as a sulfur compound may be added to the light-transmitting resin for the absorbing film.
[0068] (Absorption characteristics) FIG. 8 shows the absorption characteristics of the infrared absorbing film filter Fab1 alone. The characteristics of the infrared absorbing film filter Fab1 are set in correlation with the near-infrared reflecting filter Fref1. The infrared absorbing film filter Fab1 has a transmission characteristic close to the human visible light sensitivity curve in the visible light wavelength region of 400 nm to 700 nm, and the transmittance is 2% or less, preferably 1% or less, in the wavelength region of 685 nm to 800 nm. In this way, if the region in which the transmittance is 2% or less in the infrared absorbing film filter Fab1 alone is defined as the light absorption region Wab1, the reflection film cutoff wavelength variation region on the near-infrared reflecting filter Fref1 side, which varies in the range of the incident angle from 0° to 30°, is set to be within this light absorption region. Note that, as a more preferable infrared absorbing film filter Fab1, the transmittance is set to be 2% or less in the wavelength region of 685 nm to 850 nm, and more preferably, the transmittance is set to be 2% or less in the wavelength region of 685 nm to 900 nm.
[0069] Furthermore, in the wavelength region from 800 nm to 1150 nm, which overlaps with the total reflection wavelength region Wref1 (e.g., 790 nm to 1100 nm) on the near-infrared reflection filter Fref1 side, the maximum transmittance of the infrared absorbing film filter Fab1 alone is set to 60% or less, preferably 40% or less. Similarly, the average transmittance of the infrared absorbing film filter Fab1 in the wavelength region from 800 nm to 1150 nm is set to 40% or less, preferably 25% or less.
[0070] In this embodiment, by combining the near-infrared reflection filter Fref1 and the infrared absorption film filter Fab1, light with a wavelength of 800 nm or more, which cannot be absorbed by the infrared absorption film filter Fab1 alone, is cut (reflected) by the near-infrared reflection filter Fref1, making it possible to obtain an image with natural coloring. On the other hand, if one tries to cut (reflect) all light in the near-infrared region only by the near-infrared reflection filter Fref1, as described above, the incidence angle of the incident light increases, causing the reflection film cutoff wavelength to shift (move) to the short wavelength side. Therefore, by combining the infrared absorption film filter Fab1, which does not depend on the incidence angle, it becomes possible to configure an infrared cut filter 1 whose infrared cut characteristics in a wide range from 700 nm to 1150 nm do not depend on the incidence angle of light.
[0071] Here, the wavelength at which the light transmittance of the infrared absorbing film filter Fab1 alone decreases to 50% as the wavelength of the incident light increases is defined as the "absorbing film cutoff wavelength." The absorbing film cutoff wavelength is almost independent of the incident angle of the incident light. The absorbing film cutoff wavelength is set within the range of 600 nm to 680 nm. In addition, the absorbing film cutoff wavelength is set so as to always be smaller than the minimum value of the reflective film cutoff wavelength on the near-infrared reflective filter Fref1 side when the incident angle is changed within the range of 0° to 60°.
[0072] (Comparison with the conventional method) Conventional infrared absorbing film filters use so-called blue glass, which is phosphate glass with an appropriate amount of Cu added, as the base material. This blue glass can obtain favorable near-infrared light absorption characteristics. However, when the blue glass is thinned, the amount of copper ions dissolved in the blue glass is limited, resulting in insufficient near-infrared light absorption. For this reason, an auxiliary infrared absorbing film filter is formed by separately applying infrared absorbing ink to one surface of the blue glass by spin coating or the like, and the insufficient infrared absorption of the blue glass is compensated for as a whole. As a result, the production process is significantly increased.
[0073] <Anti-reflection film (anti-reflection part)>
[0074] (membrane structure) The anti-reflection film Far1 is composed of an anti-reflection light-transmitting resin. This anti-reflection film Far1 is essential for maintaining the image quality and brightness of the camera module. In particular, in the case of a small camera module, the distance between the optical elements is extremely narrow, so various image noises such as ghosts and flares are likely to occur, but this anti-reflection film Far1 can reduce the image noise.
[0075] The anti-reflection film Far1 can adopt, as its basic structure, a "single-layer film structure" made of low refractive index resin, a "multi-layer film structure" in which resin films with different refractive indexes (low refractive index film and high refractive index film) are alternately laminated to convert light into heat and provide an absorbing function, a "porous low refractive index film structure" in which a low refractive index is formed by making the resin surface porous, a "porous gradient refractive index structure" in which the resin surface is made porous and the air occupancy rate is gradient in the optical axis direction (film thickness direction) to generate a refractive index gradient, and a "moth-eye gradient refractive index structure" in which fine protrusions (moth eyes) with narrow tips are formed on the resin surface to generate a refractive index gradient in the optical axis direction (film thickness direction), etc. In addition, the "moth-eye gradient refractive index structure" can be either a regular moth-eye structure in which fine protrusions (moth eyes) are regularly arranged, or a "random moth-eye structure" in which irregular protrusions with different heights and pitches are formed, and either can be adopted.
[0076] From the viewpoint of adopting the roll-to-roll manufacturing process described later, it is preferable that the anti-reflection film Far1 adopts a "multilayer film structure" and a "moth-eye gradient refractive index structure". Here, a regular moth-eye structure as shown in FIG. 9 is adopted. The refractive index gradient is the refractive index of the anti-reflection light-transmitting resin at the base end of the protrusion, and the refractive index of air at the tip of the protrusion. For example, an ultraviolet-curing resin is adopted as the anti-reflection light-transmitting resin, and the liquid ultraviolet-curing resin before curing is applied to a substrate (here, a near-infrared reflection filter Fref1 or an infrared absorption film filter Fab1), and the moth-eye shape is transferred and formed on the surface by irradiating ultraviolet rays while pressing a transfer film or transfer roll having a moth-eye shape. The "moth-eye gradient refractive index structure" has the advantage that it is not easily affected by the wavelength range of the incident light or the fluctuation of the incident angle. It is preferable that the size of the fine protrusions is 2 μm or less in the protrusion height and 2 μm or less in the pitch (lattice interval) between the protrusions. More preferably, the protrusion height is 1 μm or less and the pitch between the protrusions (lattice interval) is 1 μm or less, and even more preferably, the protrusion height is 0.5 μm or less and the pitch between the protrusions (lattice interval) is 0.5 μm or less.
[0077] When the antireflection film Far1 has a "multilayer film structure", a part of the surface side of the high refractive index layer Hind of the near-infrared reflection filter Fref1 and a part of the surface side of the low refractive index layer Lind can serve as both the low refractive index film and the high refractive index film of the antireflection film Far1. In other words, the function of the antireflection film Far1 is simultaneously exerted in the vicinity of the surface of the near-infrared reflection filter Fref1.
[0078] In addition, since the near-infrared reflection filter Fref1 of this embodiment is made of a resin, its surface reflection is significantly suppressed compared to conventional inorganic dielectric multilayer films. As a result, the combination of the surface reflection state of this near-infrared reflection filter Fref1 and the "moth-eye gradient refractive index structure" can provide an even better anti-reflection function, dramatically improving image quality.
[0079] (Transmission and reflection characteristics) The spectral characteristics of the anti-reflection film Far1 are shown in Fig. 10. In this figure, the spectral characteristics of the transmittance Tm at an incidence angle of 6° (Tm6), an incidence angle of 15° (Tm15), an incidence angle of 30° (Tm30), an incidence angle of 45° (Tm45), and an incidence angle of 60° (Tm60) are shown, and the spectral characteristics of the reflectance Rm at an incidence angle of 6° (Rm6), an incidence angle of 15° (Rm15), an incidence angle of 30° (Rm30), an incidence angle of 45° (Rm45), and an incidence angle of 60° (Rm60) are shown.
[0080] The transmittance Tm in the visible light region (400nm to 700nm) is 95% or more over the incidence angle range of 0° to 45°, and the reflectance Rm is 3% or less, preferably 1% or less. Furthermore, even if the incidence angle is 60°, the transmittance T in the visible light region is 90% or more, and the reflectance R is 5% or less. Incidentally, the average transmittance in the visible light region is 99.2%, and the average reflectance is 0.8%.
[0081] <Infrared cut filter manufacturing method> Next, a method for manufacturing the infrared cut filter 1 will be described.
[0082] (Anti-reflective film manufacturing process) First, the near-infrared reflection filter Fref1 is manufactured by a co-extrusion method. The sheet extruded from the co-extruder is uniaxially (longitudinal) stretched or biaxially (longitudinal and transverse) stretched by a stretching device to become the near-infrared reflection filter Fref1. The completed near-infrared reflection filter Fref1 is preferably temporarily wound into a roll.
[0083] (Infrared absorbing film filter manufacturing process) An infrared absorbing film filter Fab1 is manufactured by an extrusion method using a light-transmitting resin for an absorbing film containing an organic dye. The sheet extruded from the extruder is uniaxially (longitudinal) stretched or biaxially (longitudinal and transverse) stretched by a stretching device to become the infrared absorbing film filter Fab1. The completed infrared absorbing film filter Fab1 is preferably temporarily wound into a roll.
[0084] (Laminating process) As shown in Fig. 11, a laminating device RS with a roll-to-roll structure is used to bond the near-infrared reflection filter Fref1 and the infrared absorption film filter Fab1 together. Specifically, the near-infrared reflection filter Fref1 and the infrared absorption film filter Fab1 in roll form are unwound, and an adhesive is applied to one of the surfaces by an adhesive applicator CT, and both films are sandwiched and pressed between a pair of heated laminating rolls RR to bond the two films together. The bonded near-infrared reflection filter Fref1 and the infrared absorption film filter Fab1 are preferably wound up again in a roll. A thermosetting optical adhesive can be used as the adhesive applied by the adhesive applicator CT.
[0085] (Anti-reflection film addition process) As shown in FIG. 12, a film forming apparatus MS having a roll-to-roll structure is used to form an anti-reflection film Far1 on the outer surface of the near-infrared reflection filter Fref1 and the outer surface of the infrared absorption film filter Fab1. Specifically, a first coater device CT1 applies an anti-reflection light-transmitting resin (ultraviolet-curable resin) to the outer surface of the near-infrared reflection filter Fref1, and the resin is hardened by irradiating ultraviolet rays UV1 while pressing the first transfer roll PR1, thereby forming a first anti-reflection film Far1 having a moth-eye gradient refractive index structure. Next, a second coater device CT2 applies an anti-reflection light-transmitting resin to the outer surface of the infrared absorption film filter Fab1, and the resin is hardened by irradiating ultraviolet rays UV2 while pressing the second transfer roll PR2, thereby forming a second anti-reflection film Far1 having a moth-eye gradient refractive index structure. As a result, a sheet material for an infrared cut filter having an all-polymer structure in which the near-infrared reflection filter Fref1, the infrared absorption film filter Fab1, and a pair of anti-reflection films Far1 are integrated is completed. It is preferable to temporarily wind up the completed sheet material into a roll.
[0086] (Light-shielding mask printing process) The sheet material for the infrared cut filter that has been subjected to the process of FIG. 12 is cut into a desired rectangular sheet and put into a sheet state, and then a frame-shaped light-shielding mask is printed on the sheet using a printing device. The light-shielding mask plays a role in blocking unnecessary peripheral light for the CMOS pixel sensor. For example, a total of 100 or more, preferably 300 or more, light-shielding masks are printed on the rectangular sheet in a lattice or staggered pattern. The light-shielding mask can be printed on either the near-infrared reflection filter Fref1 side or the infrared absorption film filter Fab1 side, but here it is printed on the infrared absorption film filter Fab1 side. The size of the rectangular sheet is not particularly limited, but from the viewpoint of mass production efficiency, it is preferable that it is at least 150 mm long and 150 mm wide, and more preferably 200 mm long and 200 mm wide, and even more preferably 300 mm long and 300 mm wide. In the case of infrared cut filters with a conventional blue glass structure, the size of the glass plate was limited to 100 mm or less in length and width due to problems with handling the glass substrate.
[0087] (Chip processing process) The rectangular sheet on which the light-shielding mask is printed is entirely made of organic resin. Therefore, the rectangular sheet is punched into a desired shape (for example, a rectangular shape of several millimeters in length and several millimeters in width) using a punching device on the press side, and is chipped into a plurality of individual infrared cut filters 1. As a result, the infrared cut filter 1 shown in FIG. 1 is completed. It is preferable that the punching blade has a double-edged structure in which blades are provided on both dies that sandwich the rectangular sheet, thereby suppressing the generation of burrs on the periphery. Since the rectangular sheet is made of organic resin, there is very little contamination of foreign matter (fragments) during chip processing, compared to glass, inorganic dielectric films, etc. It is not limited to a die with a double-edged structure, and a die with a single-edged structure may be used. Furthermore, dicing using a cutter or the like may be adopted, not limited to press punching.
[0088] (Appearance inspection process) In the case of the infrared cut filter 1 of this embodiment, there is almost no variation between components in the mass production process described above, so quality can be guaranteed by inspecting only some elements rather than inspecting every item.
[0089] <Overall structure and characteristics of infrared cut filter> The infrared cut filter 1 shown in FIG. 1 is entirely made of organic resin and does not include a glass substrate or a dielectric multilayer film. As a result, the manufacturing process can be significantly simplified and the optical characteristics during mass production can be stabilized. For example, by setting the film thickness of each of the near-infrared reflection filter Fref1, the infrared absorption film filter Fab1, and the anti-reflection film Far1 to 100 μm or less, the total thickness of the infrared cut filter 1 can be 300 μm or less. As a result, a low profile of the camera module can be achieved. In this embodiment, the film thickness of each of the near-infrared reflection filter Fref1, the infrared absorption film filter Fab1, and the anti-reflection film Far1 is set to 50 μm or less, so that the total thickness is 150 μm or less, specifically, the total thickness is 100 μm or less. It is preferable that the total film thickness of the infrared cut filter 1 is 30 μm or more from the viewpoint of handling during assembly of the camera module. In this case, the total thickness of the infrared cut filter 1 can be distributed between the thickness of the near-infrared reflection filter Fref1 and the thickness of the infrared absorption film filter Fab1, and as a result, during mass production by roll-to-roll, both the handling characteristics of the near-infrared reflection filter Fref1 and the handling characteristics of the infrared absorption film filter Fab1 can be improved. From this viewpoint, when the total thickness of the infrared cut filter 1 is 100%, the film thickness occupancy rate of the near-infrared reflection filter Fref1 is set to 20% or more, preferably 30% or more. Similarly, the film thickness occupancy rate of the infrared absorption film filter Fab1 is set to 20% or more, preferably 30% or more. In addition, the film thickness difference between the near-infrared reflection filter Fref1 and the infrared absorption film filter Fab1 is preferably set to 100 μm or less, preferably 80 μm or less, and more preferably 50 μm or less.
[0090] FIG. 13 shows the optical characteristics of the infrared cut filter 1 of this embodiment. The transmittance of the transmission band Q from 50% cut-on to 50% cut-off in the visible light region (400 nm to 700 nm) reflects the spectral characteristics of the infrared absorbing film filter Fab1 almost as they are. In particular, even if the incident angle changes from 0° to 60°, the spectral characteristics of the transmittance of this transmission band Q hardly change, and there is little ripple. In particular, for the reference blue wavelength of 440 nm and the low wavelength band of 450 nm to 500 nm, the drop in the transmittance is small even if the incident angle becomes 60°. As a result, the occurrence of shading and ghosting in the captured image is significantly suppressed. Furthermore, it can be seen that the infrared region maintains a low transmittance over the entire 700 nm to 1150 nm range by combining the light absorption region Wab1 (see FIG. 8) of the infrared absorbing film filter Fab1 and the reflection film total reflection wavelength region Wref1 (see FIG. 3) of the near-infrared reflection filter Fref1. That is, it is possible to prevent infrared images from being captured in the captured image.
[0091] Comparative Example 3 FIG. 14 shows the optical characteristics of an infrared cut filter obtained by combining the same infrared absorption film filter Fab1 (FIG. 8) as in this embodiment with the conventional near-infrared reflection filter (FIG. 4) shown in Comparative Example 1. In this infrared cut filter, the spectral characteristics of the infrared absorption film filter Fab1 are reflected in the transmittance in the visible light region (400 nm to 700 nm), but ripples caused by the conventional near-infrared reflection filter are generated in the reference deep blue wavelength of 440 nm and the low wavelength band of 450 nm to 500 nm. Furthermore, when the incident angle becomes 60°, the overall transmittance in the visible light region (400 nm to 700 nm) decreases, and in particular, the transmittance in the reference deep blue wavelength of 440 nm in the visible light region and the low wavelength band of 450 nm to 500 nm drops significantly and the ripples become large. As a result, shading and ghosts are likely to occur on the periphery of the captured image.
[0092] <Integration into camera module> 15 shows a camera module 20 incorporating the infrared cut filter 1 of the first embodiment. The camera module 20 includes, as a camera structure, a lens unit 50 which is an optical lens group, a lens carrier 40 which holds the lens unit 50, a magnet holder 30 which moves the lens unit 50 in the axial direction to realize an autofocus function, an image sensor 70 which receives light incident via the lens unit 50, a substrate 80 on which the image sensor 70 is mounted, and an infrared cut filter 1 which is disposed between the lens unit 50 and the image sensor 70.
[0093] In this camera module 20, the infrared cut filter 1 has a thin structure, and furthermore, the lens unit 50 and the image sensor 70 can be brought closer to each other, so that a low height can be achieved. Furthermore, even if the pixel pitch of the CMOS image sensor that constitutes the image sensor 70 is set to 2 μm or less, preferably 1 μm or less, degradation of image quality is unlikely to occur. The clearance between the infrared cut filter 1 and the image sensor 70 can be set to 0.5 mm or less, preferably 0.3 mm or less. Similarly, the clearance between the infrared cut filter 1 and the lens unit 50 can be set to 0.5 mm or less, preferably 0.3 mm or less.
[0094] Although not shown, a cover glass may be disposed on the light incident side of the camera module 20. It is preferable to form a dielectric multilayer film on this cover glass, which is formed by alternately laminating a plurality of dielectrics having different refractive indices. The dielectric multilayer film is laminated on the inside of the cover glass by vacuum deposition. This dielectric multilayer film can supplement the reflection function of the near-infrared reflection filter Fref1.
[0095] <Filming experiment> 19(A) and 20(A) show images of a subject captured using the camera module 20. Virtual images caused by repeated reflections of the components of the module 20 are hardly generated. On the other hand, images captured by a camera module incorporating a conventional infrared cut filter are shown in FIG. 19(B), FIG. 20(B), and FIG. 21. In the images of FIG. 19(B) and FIG. 20(B), ghost images GST-A spreading in a petal shape (radial shape) and ghost images GST-B formed in a balloon shape are formed. In the image of FIG. 21, a color shading region SHD is formed in which the peripheral part of the image is greener than the central part. This color shading region SHD coincides with the area where the angle of incidence of external light to the infrared cut filter becomes larger, which means that the transmittance of R (red) and B (indigo blue) decreases, the dimming of red and indigo becomes noticeable, and as a reaction to this, G (green) is emphasized.
[0096] Next, FIG. 16(A) shows an infrared cut filter 101 according to a second embodiment of the present invention. In this infrared cut filter 101, a near-infrared reflection filter Fref1 and an infrared absorption film filter Fab1 are separated, and an anti-reflection film Far1 is formed on both surfaces of each. That is, the infrared cut filter 101 includes a reflection member REF which becomes the near-infrared reflection filter Fref1 having the anti-reflection film Far1 on both surfaces, and an absorption member AB which becomes the infrared absorption film filter Fab1 having the anti-reflection film Far1 on both surfaces, which are independent of each other. In addition, here, a light-shielding mask M is printed on the absorption member AB side. Note that the configurations of the near-infrared reflection filter Fref1, the infrared absorption film filter Fab1, and the anti-reflection film Far1 are the same as those of the infrared cut filter 1 of the first embodiment, so the description here is omitted. In addition, the optical characteristics of the infrared cut filter 101 as a whole are almost the same as those of the infrared cut filter 1 of the first embodiment.
[0097] Since the absorbing member AB and the reflecting member REF are independent, in view of the ease of handling during assembly, the film thickness of the absorbing member AB is preferably within a range of 50 μm to 100 μm, and the film thickness of the reflecting member REF is preferably within a range of 50 μm to 100 μm.
[0098] FIG. 16B shows a camera module 120 incorporating the infrared cut filter 101. The camera module 120 includes a lens unit 50 that is an optical lens group, a lens carrier 40 that holds the lens unit 50, a magnet holder 30 that moves the lens unit 50 in the axial direction to realize an autofocus function, an image pickup element 70 that receives light incident through the lens unit 50, a substrate 80 on which the image pickup element 70 is mounted, an absorbing member AB that is disposed between the lens unit 50 and the image pickup element 70, and a reflecting member REF that is disposed on the light incident side of the lens unit 50. That is, in the camera module 120, the absorbing member AB and the reflecting member REF of the infrared cut filter 1 are separately disposed. The reflecting member REF may be attached to the inside of a so-called cover glass. The reflecting member REF may also be inserted in the middle of the optical lens group in the lens unit 50. Although not particularly illustrated here, the reflecting member REF may be disposed between the lens unit 50 and the image pickup element 70, and the absorbing member AB may be disposed on the light incident side of the lens unit 50.
[0099] Although not shown, a cover glass may be disposed on the light incident side of the camera module 120. It is preferable to form a dielectric multilayer film on this cover glass, which is formed by alternately laminating a plurality of dielectrics having different refractive indices. The dielectric multilayer film is laminated on the inside of the cover glass by vacuum deposition. This dielectric multilayer film can supplement the reflection function of the near-infrared reflection filter Fref1.
[0100] FIG. 17(A) shows an infrared cut filter 201 according to a third embodiment of the present invention. In this infrared cut filter 201, an infrared absorbing film filter Fab1 is inserted inside a multilayer film of a near-infrared reflection filter Fref1. Therefore, both surfaces are near-infrared reflection filters Fref1, and an anti-reflection film Far1 is formed on each surface. In other words, the multilayer film of the near-infrared reflection filter Fref1 is divided into two or more groups, and an infrared absorbing film filter Fab1 is interposed between the groups. In this case, the multilayer film of the near-infrared reflection filter Fref1 may be manufactured by a co-extrusion method in groups, and the infrared absorbing film filter Fab1 may be sandwiched and bonded together. In addition, the entire near-infrared reflection filter Fref1 and the anti-reflection film Far1 may be manufactured integrally by a co-extrusion method. Here, a case where a single-layer infrared absorbing film filter Fab1 is inserted is exemplified, but the infrared absorbing film filter Fab1 may have a multilayer structure. Furthermore, a plurality of infrared absorbing film filters Fab1 may be distributed among a plurality of groups of near infrared reflective filters Fref1.
[0101] FIG. 17B shows an infrared cut filter 301 according to a fourth embodiment of the present invention. In this infrared cut filter 301, a multi-layered near-infrared reflection filter Fref1 is inserted inside an infrared absorption film filter Fab1 formed in a plurality of layers. Therefore, both surfaces are infrared absorption film filters Fab1, and an anti-reflection film Far1 is formed on each surface. In this case, the multi-layer film of the near-infrared reflection filter Fref1 may be manufactured in groups by a co-extrusion method, and the multi-layer film may be sandwiched between a plurality of infrared absorption film filters Fab1 and bonded together. In addition, the entire near-infrared reflection filter Fref1 and the anti-reflection film Far1 may be manufactured integrally by a co-extrusion method. Here, a case where a group of infrared absorption film filters Fab1 is inserted is exemplified, but the infrared absorption film filter Fab1 may have a multi-group structure.
[0102] 17C shows an infrared cut filter 401 according to a fifth embodiment of the present invention. In this infrared cut filter 401, infrared absorbing film filters Fab1 formed in a plurality of layers and near-infrared reflective filters Fref1 formed in a plurality of groups to form a multilayer structure are alternately laminated. In this case, the multilayer film of the near-infrared reflective filter Fref1 may be manufactured in groups by co-extrusion, and the plurality of infrared absorbing film filters Fab1 may be bonded alternately. Alternatively, the plurality of groups of near-infrared reflective filters Fref1 and the plurality of anti-reflection films Far1 may be integrally manufactured by co-extrusion.
[0103] FIG. 18(A) shows an infrared cut filter 501 according to a sixth embodiment of the present invention. In this infrared cut filter 501, an organic dye having a near-infrared light absorbing function is contained in the low refractive index resin for the reflection film of the near-infrared reflection filter Fref1, so that the low refractive index layer Lind also serves as the infrared absorbing film filter Fab1. As a result, the infrared absorbing film filter Fab1 is dispersed and disposed in the multilayer of the near-infrared reflection filter Fref1. In this case, if the multilayer film of the near-infrared reflection filter Fref1 is manufactured by a co-extrusion method, the infrared absorbing film filter Fab1 is simultaneously formed in a superimposed manner. In the co-extrusion method, only two types of resins are required, so that the production efficiency is improved. Here, the case where an organic dye having a near-infrared light absorbing function is contained on the low refractive index layer Lind side is exemplified, but the organic dye may be contained on the high refractive index layer Hind side.
[0104] 18B shows an infrared cut filter 601 according to a seventh embodiment of the present invention. In this infrared cut filter 601, both the low refractive index resin for the reflection film and the high refractive index resin for the reflection film of the near-infrared reflection filter Fref1 contain an organic dye having a near-infrared light absorbing function, so that both the low refractive index layer Lind and the high refractive index layer Hind also serve as the infrared absorbing film filter Fab1. As a result, the entire near-infrared reflection filter Fref1 also serves as the infrared absorbing film filter Fab1. In this case, if the multilayer film of the near-infrared reflection filter Fref1 is manufactured by a co-extrusion method, the infrared absorbing film filter Fab1 is simultaneously formed in a superimposed manner.
[0105] FIG. 18C shows an infrared cut filter 701 according to an eighth embodiment of the present invention. In this infrared cut filter 701, both the low refractive index resin for the reflection film and the high refractive index resin for the reflection film of the near-infrared reflection filter Fref1 contain an organic dye having a near-infrared light absorption function, so that both the low refractive index layer Lind and the high refractive index layer Hind also serve as the infrared absorption film filter Fab1. Here, the low refractive index layer Lind and the high refractive index layer Hind close to the CMOS pixel sensor side (not shown) contain the organic dye. As a result, a part of the multilayer group of the near-infrared reflection filter Fref1 also serves as the infrared absorption film filter Fab1. In this case, if the multilayer film of the near-infrared reflection filter Fref1 is manufactured by a co-extrusion method, the infrared absorption film filter Fab1 is simultaneously formed in a superimposed manner.
[0106] FIG. 22(A) shows an infrared cut filter 901 according to a ninth embodiment of the present invention. In this infrared cut filter 901, a near-infrared reflection filter Fref1 and an infrared absorption film filter Fab1 are separated, and an anti-reflection film Far1 is formed on both surfaces of the infrared absorption film filter Fab1. Meanwhile, the near-infrared reflection filter Fref1 is attached to the inside of a cover glass 215 that protects the internal mechanism of the imaging device from the outside world. The cover glass 215 uses crystallized glass 130 as a transparent substrate that transmits light. Note that a dielectric multilayer film formed by alternately laminating multiple dielectrics with different refractive indices may be interposed between the cover glass 215 and the infrared absorption film filter Fab1. The dielectric multilayer film may be laminated on the inside of the cover glass 215 by vacuum deposition. This dielectric multilayer film can supplement the reflection function of the near-infrared reflection filter Fref1.
[0107] 22B shows a camera structure incorporating an infrared cut filter 901. The camera structure includes a cover glass 215 and a camera module 920. The camera module 920 includes a lens unit 50 that is an optical lens group, a lens carrier 40 that holds the lens unit 50, a magnet holder 30 that moves the lens unit 50 in the axial direction to realize an autofocus function, an image sensor 70 that receives light incident through the lens unit 50, a substrate 80 on which the image sensor 70 is mounted, an absorbing member AB that is disposed between the lens unit 50 and the image sensor 70, and a reflecting member REF that is attached to the inside of the cover glass 215. The cover glass 215 is fixed to a housing 20 of an image sensor such as a smartphone.
[0108] In the infrared cut filter 1 of this embodiment, the antireflection film (antireflection portion) Far1 is made of a resin material, but the present invention is not limited to this. The antireflection film (antireflection portion) Far1 may be made of a conventional inorganic dielectric multilayer film. In this case, as shown in FIG. 11, a near-infrared reflection filter Fref1 and an infrared absorption film filter Fab1 are laminated together using a laminating device RS with a roll-to-roll structure, and then the film is cut into a sheet of a desired size, and an inorganic dielectric multilayer film is formed on the surface of the sheet by a vacuum deposition process.
[0109] Incidentally, the present invention is not limited to the above-described embodiment, and it goes without saying that various modifications can be made without departing from the spirit and scope of the present invention. [Explanation of symbols]
[0110] 1, 101, 201, 301, 401, 501, 601, 701, 901 Infrared cut filter 20 Camera Module 30 Magnet holder 40 Lens Carrier 50 Lens unit 70 Image sensor 80 Substrate 120 Camera Module AB Absorbing material CT adhesive application device CT1 First coater device CT2 Second coater device Fab1 Infrared absorbing film filter Far1 Anti-reflection coating Fref1 Near infrared reflectance filter Hind high refractive index layer Lind low refractive index layer M Light-shielding mask MS film deposition equipment PR1 First transfer roll PR2 Second transfer roll REF Reflective material RR Laminate Roll RS Laminating Machine
Claims
1. An infrared cut filter for use in a digital camera, a near-infrared reflective filter formed by alternately laminating high refractive index layers made of a high refractive index resin and low refractive index layers made of a low refractive index resin; an infrared absorbing film filter made of a light-transmitting resin containing a dye or a light-transmitting resin coated with a dye; an antireflection portion formed on a surface of the near-infrared reflection filter and / or the infrared absorbing film filter that is in contact with air; Equipped with the total number of the high refractive index layers and the low refractive index layers in the near-infrared reflective filter is 200 or more; When the wavelength at which the light transmittance of the near-infrared reflection filter alone decreases to 50% as the wavelength of the incident light increases is defined as the reflection film cutoff wavelength, the reflection film cutoff wavelength when the incident angle of the incident light is 0° is within a range of 750 nm to 880 nm, The infrared absorbing film filter has a transmittance of 2% or less in a wavelength range of 685 nm to 800 nm, The infrared cut filter is characterized in that the anti-reflection portion has a structure in which irregularities are formed on the surface of a light-transmitting resin.
2. the near-infrared reflective filter alone has a wavelength fluctuation width of the reflective film cutoff wavelength of 170 nm or less when the angle of incidence of incident light is changed in a range of 0° to 60°; The near-infrared reflective filter unit is characterized in that, when the wavelength of incident light of 440 nm is defined as a reference blue wavelength, the transmittance of the reference blue wavelength is 70% or more when the incident angle of the incident light is 60°. The infrared cut filter according to claim 1 .
3. The high refractive index resin, the low refractive index resin, and the light-transmitting resin constituting the infrared absorbing film filter are made of organic resins. The infrared cut filter according to claim 1 .
4. The anti-reflection portion is made of an organic resin. The infrared cut filter according to claim 3 .
5. The thickness of each of the high refractive index layer and / or the low refractive index layer is within a range of 10 nm to 300 nm. The infrared cut filter according to claim 1 .
6. The total thickness of the near-infrared reflective filter is 100 μm or less. The infrared cut filter according to claim 1 .
7. The near-infrared reflective filter and the infrared absorbing film filter are integrated together. The infrared cut filter according to claim 1 .
8. At least one of the high refractive index resin and the low refractive index resin contains the dye, so that the resin also functions as the infrared absorbing film filter. The infrared cut filter according to claim 1 .
9. the near-infrared reflective filter and the infrared absorbing film filter are bonded to each other and integrated, a first antireflection portion is formed on a surface of the near-infrared reflection filter opposite to the infrared absorption film filter; A second antireflection portion is formed on a surface of the infrared absorbing film filter opposite to the near infrared reflective filter. The infrared cut filter according to claim 1 .
10. The total thickness of the near-infrared reflective filter, the infrared absorbing film filter, and the anti-reflection portion is 300 μm or less. The infrared cut filter according to claim 1 .
11. a film thickness occupancy rate of the near-infrared reflection filter is 20% or more based on a total thickness of the near-infrared reflection filter, the infrared absorbing film filter, and the antireflection portion. The infrared cut filter according to claim 1 .
12. a film thickness occupancy rate of the infrared absorbing film filter being 20% or more based on a total thickness of the near-infrared reflective filter, the infrared absorbing film filter, and the antireflection portion. The infrared cut filter according to claim 11.
13. The wavelength of incident light is defined as 450 nm to 500 nm as the low wavelength transmission band, When the average transmittance of incident light in the low wavelength transmission band in the near-infrared reflection filter alone is defined as the low wavelength transmittance of the reflection film, The reflecting film has a low wavelength transmittance of 75% or more when the angle of incidence of incident light is changed in the range of 0° to 60°. The infrared cut filter according to claim 1 .
14. The resin constituting the near-infrared reflective filter and / or the infrared absorbing film filter contains an ultraviolet absorbing agent. The infrared cut filter according to claim 1 .
15. A digital camera structure including an optical lens group disposed on a light incident side, and an image sensor that receives light incident through the optical lens group, The infrared cut filter according to claim 1 is disposed between the optical lens group and the image sensor. Camera structure.
16. A digital camera structure including, in order from the light incident side, a cover glass, an optical lens group, and an image sensor, The infrared cut filter according to claim 1 is provided, The near-infrared reflective filter is disposed between the cover glass and the optical lens group; The infrared absorbing film filter is disposed between the optical lens group and the image sensor. Camera structure.
17. The near-infrared reflective filter is attached to the cover glass.
17. A camera arrangement according to claim 16.
18. A method for manufacturing an infrared cut filter for a digital camera, comprising the steps of: a reflective film manufacturing process in which high refractive index layers made of a high refractive index resin and low refractive index layers made of a low refractive index resin are alternately laminated by co-extrusion molding to form a near-infrared reflective filter, the total number of layers being 200 or more; an integration step of laminating or bonding an infrared absorbing film filter made of a light transmitting resin containing a dye or a light transmitting resin for an absorbing film to which a dye is applied, on the near-infrared reflective filter; an anti-reflection film application step of forming an anti-reflection film having projections and recesses made of a light-transmitting resin on a surface in contact with air; a chip processing step of forming at least the near-infrared reflective filter, the infrared absorbing film filter, and the anti-reflection film into a desired shape by cutting or punching after the reflection film manufacturing step, the integration step, and the anti-reflection film adding step are completed; Equipped with When the wavelength at which the light transmittance of the near-infrared reflection filter alone decreases to 50% as the wavelength of the incident light increases is defined as the reflection film cutoff wavelength, the reflection film cutoff wavelength when the incident angle of the incident light is 0° is within a range of 750 nm to 880 nm, The infrared absorbing film filter has a transmittance of 2% or less in a wavelength range of 685 nm to 800 nm.
19. In the reflection film manufacturing process and the integration process, in addition to the high refractive index resin and the low refractive index resin, a light-transmitting resin containing a dye that absorbs infrared rays is co-extruded to integrally mold a near-infrared reflection filter in which high refractive index layers made of the high refractive index resin and low refractive index layers made of the low refractive index resin are alternately laminated, and an infrared absorbing film filter made of the light-transmitting resin. A method for producing the infrared cut filter according to claim 18.
20. In the reflection film manufacturing process and the integration process, a dye that absorbs infrared rays is contained in either the high refractive index resin or the low refractive index resin, and then the high refractive index resin and the low refractive index resin are co-extruded to integrally form a near-infrared reflection filter in which high refractive index layers made of the high refractive index resin and low refractive index layers made of the low refractive index resin are alternately laminated, and an infrared absorption film filter made of the high refractive index layer and the low refractive index layer containing the dye. A method for producing the infrared cut filter according to claim 18.
21. The method further comprises the steps of: printing a light-shielding mask on the substrate; A method for producing the infrared cut filter according to claim 18.
22. In the integration step, the near-infrared reflection filter and the infrared absorption film filter are supplied to a laminating device, integrated, and wound into a roll. A method for producing the infrared cut filter according to claim 18.
Citation Information
Patent Citations
transparent multilayer device
JP1999508380A
Optical filter and imaging device
JP2005345680A
Liquid crystal display
JP2016200716A
Near-infrared cut filter and imaging device
WO2016114363A1