MASK BLANK, METHOD FOR MANUFACTURING TRANSFER MASK, AND METHOD FOR MANUFACTURING SEMICONDUCTOR DEVICE

The use of a silicon-oxygen-based hard mask film in mask blanks addresses the issue of excessive side etching in chromium-based films, enabling precise and miniaturized pattern formation in phase shift masks and semiconductor devices.

JP7573344B2Active Publication Date: 2024-10-25HOYA CORPORATION
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023111188
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2023-07-06
Publication Date
2024-10-25
Estimated Expiration
2039-03-18

AI Technical Summary

Technical Problem

Existing mask blanks for halftone phase shift masks face challenges in forming fine patterns with high dimensional accuracy due to excessive side etching during dry etching processes, particularly when using chromium-based light-shielding films and oxygen-containing chlorine gas, which limits the miniaturization and quality of patterns.

Method used

A mask blank structure with a hard mask film made of silicon and oxygen, characterized by specific X-ray photoelectron spectroscopy analysis conditions, is used to minimize side etching and enhance etching controllability, allowing for further miniaturization and improved pattern quality.

Benefits of technology

The proposed mask blank enables the formation of fine patterns with high precision and reduced side etching, enhancing the accuracy and quality of phase shift masks and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573344000001
    Figure 0007573344000001
  • Figure 0007573344000002
    Figure 0007573344000002
  • Figure 0007573344000003
    Figure 0007573344000003
Patent Text Reader

Abstract

To provide a mask blank comprising a hard mask film being suitable for a high bias etching condition and having excellent performance, and capable of achieving further fine patterns which should be formed on a thin film for pattern formation and improving pattern quality.SOLUTION: A mask blank 100 comprises a structure in which, on a substrate 1, a thin film 3 for pattern formation and a hard mask film 4 are stacked in this order. The hard mask film 4 is configured so that a narrow spectrum of Si2p obtained by analyzing by X-ray photoelectron spectroscopy has a maximum peak at binding energy of 103 eV or greater, the hard mask film 4 is configured so that the maximum peak of the narrow spectrum of N1s obtained by analyzing using the X-ray photoelectron spectroscopy is equal to or less than a detection lower limit value, and the hard mask film 4 is configured so that an inclusion ratio (atom%) of silicon and oxygen shows Si:O=1:less than 2.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a mask blank, a method for manufacturing a transfer mask using the mask blank, and and a method for manufacturing a semiconductor device using a transfer mask manufactured from this mask blank. Regarding. [Background technology]

[0002] As a mask blank for a halftone phase shift mask, a metal silicon film was formed on a transparent substrate. Halftone phase shift film made of side-based materials, light-shielding film made of chromium-based materials, inorganic A mask block having a structure in which an etching mask film (hard mask film) made of a material is laminated. The rank has been known for some time (see, for example, Patent Document 1). When manufacturing a phase shift mask by this method, first, a resist pattern formed on the surface of a mask blank is Using the turn as a mask, the etching mask film is patterned by dry etching with fluorine gas. Then, the etching mask film is used as a mask to perform drying with a mixture of chlorine and oxygen gas. The light-shielding film is patterned by etching, and then the light-shielding film pattern is used as a mask to apply a fluorine-based The phase shift film is patterned by dry etching using gas. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2004 / 090635 [Patent Document 2] Patent No. 6158460 Summary of the Invention [Problem to be solved by the invention]

[0004] In a mask blank as described in Patent Document 1, a chromium-based compound is used. The light-shielding film has a light-shielding performance for reducing the amount of exposure light transmitted through the phase shift film to a predetermined level or less. When a phase shift mask is made from this mask blank, the light-shielding film is required to have a thickness of 100 nm. A pattern including a light-shielding band is formed. Then, a predetermined thickness is obtained by stacking the phase shift film and the light-shielding film. At the same time, the light-shielding film is required to have a phase shift film made of fluorine-based When forming a phase shift pattern by patterning using gas dry etching, It is required to function as an etching mask. At the completion stage of the phase shift mask, Generally, a relatively sparse pattern such as a light-shielding pattern is formed on the light-shielding film. In the process of manufacturing a phase shift mask from a mask blank, the light-shielding film is When forming a phase shift pattern, which is a fine transfer pattern, it is used as an etching mask. For this reason, fine patterns must be formed with high dimensional accuracy even in the light-shielding film. It is hoped that this is possible.

[0005] In dry etching of light-shielding films made of chromium-based materials, a mixture of chlorine-based gas and oxygen gas is used. Gas (oxygen-containing chlorine-based gas) is used as the etching gas. Dry etching using chlorine-based gas as the etching gas has a small tendency to be anisotropic. There is a strong tendency for isotropic etching.

[0006] In general, when forming a pattern on a thin film by dry etching, the etching is performed on the film. Etching not only in the thickness direction but also in the sidewall direction of the pattern formed on the thin film, so-called In order to suppress the progression of this side etching, dry etching is performed. During etching, a bias voltage is applied from the opposite side of the main surface of the substrate on which the thin film is formed. Previous studies have attempted to control the amount of gas that comes into contact with the film in the thickness direction. Using an etching gas that has a tendency to become ionic plasma, such as a fluorine-based gas In the case of ion-based dry etching, the etching method is performed by applying a bias voltage. The etching direction is highly controllable and the anisotropy of the etching is enhanced, so the size of the thin film being etched is The amount of etching can be made very small.

[0007] On the other hand, in the case of dry etching using oxygen-containing chlorine gas, oxygen gas acts as a radical proton. Since the etching direction is highly likely to become plasma, the etching direction can be controlled by applying a bias voltage. The etching effect is small, and it is difficult to increase the anisotropy of etching. A pattern is formed in a light-shielding film made of a chromium-based material by dry etching using a gas. In this case, the amount of side etching tends to be large.

[0008] Using an organic resist pattern as an etching mask, an oxygen-containing chlorine-based gas When patterning a light-shielding film made of a chromium-based material by dry etching using The turn is etched from above and is reduced. At this time, the sidewall direction of the pattern is also etched. Therefore, the width of the pattern formed in the resist film is determined by the side width in advance. The amount of attenuation caused by etching is estimated. The width of the pattern is designed taking into account the amount of side etching of the light-shielding film made of chromium-based material.

[0009] In recent years, dry etching with oxygen-containing chlorine-based gas on a light-shielding film made of chromium-based material has been An etching mask made of a material having sufficient etching selectivity with respect to chromium-based materials. Mask blanks with a hard mask film are beginning to be used. In this case, the hard mask film is patterned by dry etching using a resist pattern as a mask. Then, the patterned hard mask film is used as a mask to form a pattern on the oxygen-containing The light-shielding film is subjected to dry etching using a chlorine-containing gas to form a pattern in the light-shielding film. This hard mask film is made of a material that can be patterned by dry etching with fluorine-based gas. Dry etching with fluorine-based gas is generally performed by ion-based etching. Because the etching is done by a metal, it tends to be anisotropic. This is why phase shift patterns are formed. The amount of side etching of the pattern sidewalls of the hard mask film is small. In the case of dry etching using silicon-based gas, a resist for forming a pattern on the hard mask film is used. The amount of side etching also tends to be small in the chrome pattern. The side edge of the light-shielding film made of chlorine-based material was also improved by dry etching with oxygen-containing chlorine-based gas. It is desirable that the amount of chipping be small.

[0010] As a means for reducing the amount of side etching in the light-shielding film made of this chromium-based material, In dry etching of oxygen-containing chlorine-based gas, the mixture of chlorine-based gas in oxygen-containing chlorine-based gas A significant increase in the ratio is being considered. Chlorine gas tends to become ionic plasma. This is because the tendency is large. In etching, it is inevitable that the etching rate of the light-shielding film made of chromium-based material will decrease. In order to compensate for the decrease in the etching rate of the chromium-based light-shielding film, dry etching is used. The bias voltage applied at the time of the laser irradiation is significantly increased (hereafter, oxygen-containing laser with a higher ratio of chlorine gas). Dry etching using chlorine-containing gases and under high bias voltage conditions This is called "high bias etching with oxygen-containing chlorine gas." There are.

[0011] The high bias etching of the oxygen-containing chlorine-based gas for the light-shielding film of the chromium-based material The etching rate is comparable to that of dry etching under conventional etching conditions. The amount of side etching of the light-shielding film that occurs during etching is also smaller than in the past. It is possible.

[0012] Furthermore, by examining and adjusting the bonds and compositions of chromium-based materials in the light-shielding film, Using the hard mask film on which the transfer pattern is formed as a mask, etching is performed using an oxygen-containing chlorine-based gas. When the light-shielding film is patterned under high bias etching conditions, This allows a significant reduction in the amount of side etching of the light-shielding film pattern, resulting in a phase It is possible to form a fine pattern with high precision in the shift film (Patent Document 2).

[0013] However, there is a demand for further miniaturization of the patterns to be formed in the phase shift film. In order to achieve this, only the technology described above, such as drastically reducing the amount of side etching of the light-shielding film pattern, is required. In addition, the pattern or hardness to be formed on the thin film for pattern formation such as the light-shielding film is not sufficient. There is a demand for further miniaturization of the patterns to be formed on the mask film and improvement of the pattern quality. These are the characteristics of binary masks that have a light-shielding film, which is a thin film for forming patterns, and The same is true for a reflective mask having an absorber film that is a turn-forming thin film.

[0014] In order to solve the above-mentioned problems, the present invention provides a method for forming a thin film for patterning, such as a light-shielding film, on a substrate. Regarding the mask blank having a structure in which hard mask films are laminated in this order, Further development of the pattern to be formed in the thin film for forming the slit and the pattern to be formed in the hard mask film To provide a mask blank that enables miniaturization and improvement of pattern quality. The hard mask film has excellent performance suitable for high bias etching conditions, and the pattern This enables further finer patterns to be formed on the thin film and improved pattern quality. The present invention also provides a mask blank. Manufacture of a transfer mask capable of forming fine patterns with high accuracy on a thin film for forming turns Further, a method for manufacturing a semiconductor device using the transfer mask is provided. do. [Means for solving the problem]

[0015] The present invention has the following configuration as a means for solving the above problems.

[0016] (Configuration 1) A mask having a structure in which a thin film for pattern formation and a hard mask film are laminated in this order on a substrate. It is a kublanc, the hard mask film is made of a material containing silicon and oxygen; The hard mask film has a narrow spectrum of Si2p obtained by X-ray photoelectron spectroscopy. Torr has a maximum peak at a binding energy of 103 eV or more, The hard mask film has a narrow spectrum of N1s obtained by X-ray photoelectron spectroscopy. The maximum peak of the sample is below the detection limit. The hard mask film has a silicon to oxygen content (atomic %) of Si:O=less than 1:2. is A mask blank comprising:

[0017] (Configuration 2) The hard mask film has a narrow spectrum of O1s obtained by X-ray photoelectron spectroscopy. 2. The method according to claim 1, wherein the molecule has a maximum peak at a binding energy of 532 eV or more. Mask blanks listed. (Configuration 3) The hard mask film has a narrow spectrum of O1s obtained by X-ray photoelectron spectroscopy. 1. The method according to claim 1, wherein the molecule has a maximum peak at a binding energy of less than 533 eV. 3. The mask blank according to claim 2.

[0018] (Configuration 4) The surface of the hard mask film was analyzed by X-ray photoelectron spectroscopy to obtain a narrow band of Si2p. The binding energy at which the maximum peak occurs in the spectrum and the inside of the hard mask film are measured using X-ray photoelectron The binding energy of the maximum peak in the narrow spectrum of Si2p obtained by spectroscopic analysis 4. The marker according to claim 1, wherein the difference between the marker and the target is 0.2 eV or less. Scribblank. (Configuration 5) The surface of the hard mask film was analyzed by X-ray photoelectron spectroscopy to obtain a narrow spectrum of O1s. The binding energy at which the maximum peak occurs in the spectrum and the inside of the hard mask film are analyzed by X-ray photoelectron spectroscopy. The bond energy of the maximum peak in the narrow spectrum of O1s obtained by the spectroscopic analysis and 5. The mask according to claim 1, wherein the difference between the blank.

[0019] (Configuration 6) The hard mask film has a narrow spectrum of Si2p obtained by X-ray photoelectron spectroscopy. It is characterized in that the torr does not have a peak in the binding energy range of 97 eV to 100 eV. 6. The mask blank according to claim 1 , (Configuration 7) 2. The hard mask film has an oxygen content of 60 atomic % or more. 7. A mask blank according to any one of 1 to 6.

[0020] (Configuration 8) The hard mask film is made of a material consisting of silicon and oxygen, or a nonmetallic element other than nitrogen and and semi-metallic elements, silicon, and oxygen. 8. The mask blank according to claim 1, (Configuration 9) The pattern-forming thin film is made of one or more elements selected from chromium, tantalum, and nickel. 8. The mask blank according to claim 1, characterized in that it is made of a material containing nitrogen. Rank.

[0021] (Configuration 10) 10. The thin film for pattern formation according to claim 1, wherein the thin film for pattern formation is a light-shielding film. The mask blank according to claim 1. (Configuration 11) 11. The method according to claim 10, further comprising providing a phase shift film between the substrate and the light-shielding film. Mask blank. (Configuration 12) 10. The method according to claim 1, wherein the pattern-forming thin film is an absorber film. The mask blank according to any one of claims 1 to 5,

[0022] (Configuration 13) A method for manufacturing a transfer mask using the mask blank according to any one of claims 1 to 12. And, A resist film having a transfer pattern formed on the hard mask film is used as a mask, and A transfer pattern is formed on the hard mask film by dry etching using fluorine-based gas. And a process of The hard mask film on which the transfer pattern is formed is used as a mask, and a gas containing chlorine is used to forming a transfer pattern on the pattern-forming thin film by dry etching using the above-mentioned method; 2. A method for producing a transfer mask comprising the steps of:

[0023] (Configuration 14) The dry etching using the chlorine-containing gas is carried out by using an oxygen-containing gas having a high ratio of chlorine-based gas. Dry etching using chlorine-containing gases and under high bias voltage conditions 14. The method for producing a transfer mask according to claim 13, wherein the method is a process for producing a transfer mask. (Configuration 15) The dry etching using a gas containing chlorine uses a chlorine-based gas that does not contain oxygen. The dry etching is characterized by being performed under a high bias voltage. 14. The method for producing a transfer mask according to claim 13,

[0024] (Configuration 16) A transfer mask manufactured by the method for manufacturing a transfer mask according to any one of claims 13 to 15. Using a photomask, a transfer pattern is exposed and transferred to the resist film on the substrate on which the semiconductor device is to be formed. 13. A method for manufacturing a semiconductor device, comprising: Effect of the Invention

[0025] According to the mask blank of the present invention having the above-mentioned configuration, a pattern such as a light-shielding film is formed on a substrate. A mask blank having a structure in which a forming thin film and a hard mask film are laminated in this order, A pattern to be formed on a thin film for pattern formation such as a photoresist film or a hard mask film. It is possible to provide a mask blank that enables further miniaturization of patterns and improvement of pattern quality. In addition, the present invention provides a hard mask film having excellent performance suitable for high bias etching conditions. This allows for further finer patterns to be formed on the pattern-forming thin film and improved pattern quality. The present invention also provides a mask blank that can improve the optical properties of the mask. By this, it is possible to form a fine pattern with high accuracy on the thin film for pattern formation. A method for manufacturing a transfer mask can be provided. A method for producing the above-mentioned can be provided. [Brief description of the drawings]

[0026] [Figure 1] 1 is a cross-sectional schematic diagram of an embodiment of a mask blank. [Diagram 2] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a phase shift mask. [Diagram 3] FIG. 13 is a diagram showing the results (Si2p narrow spectrum) of an XPS analysis (depth direction chemical bond state analysis) performed on the mask blank according to Example 1. [Figure 4] 1 is a diagram showing the results (N1s narrow spectrum) of an XPS analysis (depth direction chemical bond state analysis) performed on the mask blank of Example 1. FIG. [Diagram 5] 1 is a diagram showing the results (O1s narrow spectrum) of an XPS analysis (depth direction chemical bond state analysis) performed on the mask blank of Example 1. FIG. [Figure 6] FIG. 2 is a cross-sectional schematic diagram of an embodiment of a reflective mask blank. [Figure 7] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a reflective mask. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Each embodiment of the present invention will be described below, but first, the background to the invention will be described. Reveal. The present inventors have been developing a method for further miniaturizing a pattern formed in a hard mask film and improving a pattern quality. We conducted a study on quality improvement, and the following findings were obtained: First, the hard mask film made of a material containing silicon and oxygen is a compound of silicon (Si) and oxygen. The content ratio (atomic %) of oxygen (O) is less than Si:O=1:2 (oxygen-deficient Si Condition 1: Si:O=1:2 (SiO2 film without oxygen deficiency) The etching rate for fluorine-based gas is higher than that for the hard mask film. It was found that etching can be performed quickly and cleanly.

[0028] Second, the hard mask film made of a material containing silicon and oxygen has a low degree of oxidation, Si- When the ratio of O bonds is high, or when silicon bonds that are not bonded to oxygen (Si-Si When the ratio of SiO2 bonds is high, the resistance to dry etching using oxygen-containing chlorine gas is high. When the resistance to dry etching decreases, the fine patterns become Using the formed hard mask film as a mask, dry etching is performed using oxygen-containing chlorine-based gas. During the patterning of a thin film for pattern formation (such as a light-shielding film), The edge shape of the pattern deteriorates and side etching of the sidewalls of fine patterns progresses. In this case, a fine pattern is formed on the hard mask film with high accuracy. Even if the hard mask film is used as a mask for dry etching, the pattern is The phenomenon in which the pattern shape of a hard mask film deteriorates when a thin film is being processed. Due to this, it is difficult to form a fine pattern on the pattern forming thin film with high accuracy. This would result in a problem in which it would be impossible to do this.

[0029] The resistance of this hard mask film to dry etching using an oxygen-containing chlorine-based gas is reduced. This was particularly noticeable under high bias etching conditions. When etching, both chemical and physical etching occurs. Chemical etching occurs when an etching gas in plasma state comes into contact with the surface of a thin film. It combines with silicon or metal elements in the thin film to form compounds with low boiling points (e.g. SiF4, CrO2C This is done by a process in which a metal oxide (such as 12) is produced and sublimated. In chemical etching, other Breaks the bond between silicon or metal elements and elements (e.g., O, N, etc.) In contrast, physical etching is performed by applying a bias voltage The ionic plasma in the etching gas accelerated by the (This phenomenon is also called "ion bombardment.") Each of the silicon or metal elements on the thin film surface is The elements are physically repelled (the bonds between the elements are broken) and the silicon This is done by producing a compound with a low boiling point and a metal element, which is then sublimated.

[0030] High bias etching is a dry etching process that uses a physical action to reduce the amount of etching gas. Etching by physical action is an etching in the thickness direction. It contributes greatly to etching in the direction of the sidewall of the pattern, but does not contribute much to etching in the direction of the sidewall of the pattern. In contrast, etching by chemical reaction etches the film thickness direction and the pattern. This also contributes to etching in the sidewall direction (side etching).

[0031] The hard mask film has low resistance to dry etching using the above-mentioned oxygen-containing chlorine-based gas. To solve the problem of the oxidation of the hard mask film, the ratio of Si-O bonds with low oxidation degree is low. It is necessary to form the material with a low Si-Si bond ratio. As a result of the research, X-ray photoelectron spectroscopy was used as an index to measure the ratio of bonds in the materials that make up the hard mask film. Si2p nanoparticles obtained by spectroscopy (XPS: X-ray Photoelectron Spectroscopy) Specifically, the hard mask film is The Si2p narrow spectrum obtained when analyzing the hard mask film by X-ray photoelectron spectroscopy. The spectrum should be adjusted so that it has a maximum peak at a binding energy of 103 eV or more. Condition 2> It was found that the hardware that can obtain such a Si2p narrow spectrum is The mask film has a silicon (Si) and oxygen (O) content ratio (atomic percent) of Si:O=1:2 or less. Even if the degree of oxidation is less than 100%, the ratio of Si-O bonds with low oxidation degree is low, or the Si-O bonds with low oxidation degree are not bonded to oxygen. This means that the proportion of silicon bonds (Si-Si bonds) that are not present is low.

[0032] Silicon (Si) and oxygen (O) can form various bonds. For example, A form in which one oxygen atom is bonded to one silicon atom (Si), and two oxygen atoms are bonded to one silicon atom (Si). Form, one silicon (Si) bonded to three oxygen atoms, one silicon (Si) bonded to four oxygen atoms In addition, silicon (Si), oxygen (O) and hydrogen (H ) can take various bond forms. For example, one silicon (Si) and three oxygen (O ) and one hydrogen (H), one silicon (Si) and one oxygen (O) A hydrogen (H) is bonded to one silicon (Si), and two oxygens (O) and one hydrogen ( H) bond. Therefore, it is important to specify the composition of the hard mask film. Therefore, it is difficult to identify the bonding form of each component element inside the film.

[0033] On the other hand, the Si2p narrow band obtained by analyzing the silicon nitride film using X-ray photoelectron spectroscopy The position where the binding energy at which the spectrum reaches its maximum peak is the position where the X-ray The binding energy of the maximum peak in the Si2p narrow spectrum obtained by photoelectron spectroscopy analysis This is relatively close to the location where the energy is generated. Therefore, hard If the mask film contains nitrogen, the hard mask film will have a low degree of oxidation due to the presence of Si-O bonds. Even if the ratio of Si-Si bonds is high, the ratio of Si-N bonds is high. Due to the presence of This can result in a coupling of the maximum peak of the Si2p narrow spectrum. The position of energy cannot be used as an indicator.

[0034] Considering this issue, we performed X-ray photoelectron spectroscopy analysis on the hard mask film. If the maximum peak of the N1s narrow spectrum is below the detection limit, <Condition 3> is met. The bond energy at the maximum peak of the Si2p narrow spectrum is determined by the presence or absence of nitrogen in the mask film. The conclusion was that this would not affect Lugi's position.

[0035] As a result of the above intensive investigation, it was found that a hard mask film containing silicon and oxygen satisfies the above three conditions: That is, <Condition 1> The content ratio (atomic %) of silicon (Si) and oxygen (O) is Si:O= <Condition 2> The ratio of Si2p obtained by X-ray photoelectron spectroscopy analysis is less than 1:2. The narrow spectrum has a maximum peak at a binding energy of 103 eV or more. 3> The maximum peak of the N1s narrow spectrum is below the detection limit. If so, the pattern to be formed in the thin film for pattern formation and the pattern to be formed in the hard mask film can be It was concluded that it is possible to further refine the turns and improve the pattern quality.

[0036] Such a hard mask film requires a shorter etching time, allowing the resist to be made thinner. In addition, the thinner the resist, the more precise the resist pattern can be prevented from collapsing. It is possible to form a finer resist pattern. This allows the film to be etched quickly, which reduces the sidewall roughness of the hard mask film pattern. and a hard mask film having small line edge roughness and clean (smooth) sidewalls. As a result, the pattern quality of the hard mask film can be improved.

[0037] In addition, when the etching rate of a certain film increases, the etching time when the film is patterned increases. The etching time for patterning the film is shortened. This reduces the time that the sidewall of the film is exposed to the etching gas, and the amount of side etching is reduced. This leads to less In addition, when the etching rate of a certain film becomes faster, the etching time in the film thickness direction is shortened. This reduces the time that the sidewalls of a film are exposed to the etching gas. It is possible to form patterns with small defects and clean (smooth) side walls.

[0038] In order to obtain the above effects and conditions, a hard mask made of a material containing silicon and oxygen is used. The oxygen content of the screen film is preferably 66.5 atomic % or less, and more preferably 66.0 atomic % or less. It is more preferable that the oxygen content is 65.5 atomic % or less, and further more preferable that the oxygen content is 65.5 atomic % or less. If it is too long, it will be difficult to obtain the above-mentioned effects and conditions.

[0039] In order to obtain the above three effects and conditions, silicon and oxygen are required. The oxygen content of the hard mask film made of the material having the above structure is preferably 60 atomic % or more. %, more preferably 62 atomic % or more, and even more preferably 64 atomic % or more. If the content is too low, it is difficult to obtain the above-mentioned effects and conditions.

[0040] In order to obtain the above effects and conditions, a hard mask made of a material containing silicon and oxygen is used. The silicon content of the screen film is preferably 30 atomic % or more, and more preferably 31 atomic % or more. It is more preferable that the silicon content is 32 atomic % or more, and even more preferable that the silicon content is 32 atomic % or more. , it is difficult to obtain the above-mentioned effects and conditions. In order to obtain the above effects and conditions, a hybrid material containing silicon and oxygen is used. The silicon content of the hard mask film is preferably 40 atomic % or less, and more preferably 39 atomic % or less. It is more preferable that the silicon content is 38 atomic % or less, and further more preferable that the silicon content is 38 atomic % or less. If the amount is too large, it will be difficult to obtain the above-mentioned effects and conditions.

[0041] The hard mask film made of a material containing silicon and oxygen is composed of silicon (Si) and oxygen (O). The content ratio (atomic %) of Si:O is less than 1:2 (SiO2 film with oxygen deficiency). In the case where oxygen vacancies are present, for example, in the deposition chamber under high vacuum conditions, e.g. For example, it is thought that small amounts of atoms such as N and C may be included.

[0042] In addition, the characteristics of the thin film (etching speed, pattern quality (etching processing quality, processing accuracy, The properties of the thin film (including sidewall roughness, line edge roughness, etc.) are determined solely by the film composition. The film density and crystal state of the thin film also determine the properties of the thin film. For this reason, the conditions for forming a thin film by sputtering must be adjusted to ensure that the thin film has a desired thickness. For example, the pressure in the deposition chamber during deposition, the spark plug, The power applied to the target, the distance between the target and the substrate, and other positional relationships A wide range of conditions are adjusted to form the thin film with the desired characteristics. These deposition conditions are specific to the deposition apparatus and must be adjusted appropriately so that the thin film has the desired characteristics. It is something that is adjusted. When forming a thin film by reactive sputtering, a mixture of noble gas and reactive gas (oxygen gas) is used. Adjusting the gas ratio is effective, but is not limited to this.

[0043] As a method for forming an oxygen-deficient SiO2 film, for example, a SiO2 target is used. For example, a sputtering method may be used to form the film. As a method for forming a SiO2 film without oxygen deficiency, for example, a Si target is used, One method is to form the film by sputtering using O2 gas.

[0044] In order to obtain the above effects and conditions, at least X-ray photoelectron spectroscopy (XPS: X-ray photoelectron spectroscopy) The Si2p narrow spectrum obtained by analyzing with y Photoelectron Spectroscopy (PSI) is 103 Preferably, the bond energy of the cation pair is between 0.5 eV and 1.0 eV. The hard mask film contains not only high-oxidation Si-O bonds, but also low-oxidation Si-O bonds and Si- This means that Si bonds are also present.

[0045] In addition to the above conditions, the O1s nanometers obtained by analyzing the hard mask film using X-ray photoelectron spectroscopy were It is preferred that the spectrum has a maximum peak at a binding energy of 532 eV or more. This is because the hard mask film contains a large amount of highly oxidized Si-O bonds. In addition to the above conditions, the hard mask film was analyzed by X-ray photoelectron spectroscopy. The O1s narrow spectrum obtained has a maximum peak at a binding energy below 533 eV. This means that the hard mask film preferably has low oxidation properties such as low oxidation Si-O bonds. It means that something exists.

[0046] The hard mask film, made of a material containing silicon and oxygen, was analyzed by X-ray photoelectron spectroscopy. The Si2p narrow spectrum obtained is in the binding energy range of 97 eV to 100 eV. It is preferable that the hard mask film has no peak in the above range (below the detection limit). The Si2p narrow spectrum of the peaks is in the binding energy range of 97 eV to 100 eV. When the hard mask film has a Si-Si bond, the Si-Si bond is present at a certain ratio or more. This is undesirable.

[0047] In addition, the hard mask film made of a material containing silicon and oxygen actively promotes the formation of Si-Si bonds. (For example, the area intensity of the Si-Si bond is more than half that of the Si-O bond.) There are about the same amount of Si-O bonds and Si-Si bonds in the top and bottom, respectively. In this case, the hard mask film has a narrow spectrum of Si2p obtained by X-ray photoelectron spectroscopy. The spectrum has a maximum peak at a binding energy of less than 103 eV and a maximum peak at a binding energy of 97 eV or more and 10 The Si-Si bond has a maximum peak at a bond energy of 0 eV or less.

[0048] The hard mask film, which is made of a material containing silicon and oxygen, is exposed to X-rays to The bond energy with the maximum peak in the narrow spectrum of Si2p obtained by photoelectron spectroscopy The Si2p energy obtained by analyzing the inside of the hard mask film by X-ray photoelectron spectroscopy The difference between the binding energy of the maximum peak in the narrow spectrum of the In addition, the hard mask film made of a material containing silicon and oxygen is preferably The maximum peak in the narrow spectrum of O1s obtained by analyzing the surface of the screen film by X-ray photoelectron spectroscopy The bond energy of the peak and the inside of the hard mask film were analyzed by X-ray photoelectron spectroscopy. The difference between the binding energy of the maximum peak in the narrow spectrum of O1s obtained is 0.1e V or less. The narrow spectrum of Si2p and O1 In both narrow spectra, the binding energy is smaller (preferably substantially the same) during etching of the hard mask film. This is preferable in order to obtain a high degree of controllability.

[0049] The detailed configuration of the present invention will be described below with reference to the drawings. In the following description, similar components are given the same reference numerals.

[0050] <First embodiment> [Mask blanks and their manufacturing] <Mask Blank> FIG. 1 shows a schematic configuration of a first embodiment of a mask blank. The substrate 100 has a phase shift film 2 and a light-shielding film 3 (pattern) on one main surface of a light-transmitting substrate 1. The mask layer is a thin film for forming a mask pattern, and a hard mask film 4 are laminated in this order. The screen blank 100 has a structure in which a resist film is laminated on a hard mask film 4 as required. The main components of the mask blank 100 will be described in detail below.

[0051] [Transparent substrate] The light-transmitting substrate 1 is transparent to the exposure light used in the exposure step of lithography. Such materials include synthetic quartz glass, aluminosilicate Glass, soda lime glass, low thermal expansion glass (SiO2-TiO2 glass, etc.), others Various types of glass substrates can be used. In particular, substrates made of synthetic quartz glass are suitable for ArF High transparency to excimer laser light (wavelength: approx. 193 nm) for mask blanks It can be suitably used as the light-transmitting substrate 1 of 100.

[0052] The exposure process in lithography mentioned here is a process using this mask blank 100. In the exposure process of lithography, a phase shift mask manufactured by In the following, the exposure light refers to the exposure light used in this exposure process. The exposure light was ArF excimer laser light (wavelength: 193 nm), KrF excimer laser light (wavelength: 193 nm), Both laser light (wavelength: 248 nm) and i-line light (wavelength: 365 nm) can be used. From the viewpoint of miniaturizing the phase shift pattern in the exposure process, the ArF excimer laser It is desirable to use an ArF excimer laser as the exposure light. An embodiment in which the light is applied to the exposure light will be described.

[0053] [Phase shift film] The phase shift film 2 has a predetermined transmittance with respect to the exposure light used in the exposure transfer process, The exposure light that passes through the phase shift film 2 and the exposure light that passes through the atmosphere for a distance equal to the thickness of the phase shift film 2 are The film has optical properties that provide a predetermined phase difference between the exposed light and the film that has passed through it.

[0054] Such a phase shift film 2 is formed here from a material containing silicon (Si). The phase shift film 2 is made of a material containing nitrogen (N) in addition to silicon. Such a phase shift film 2 is preferably formed by dry etching using a fluorine-based gas. Patterning is possible by etching, and the CrOCN film constituting the light-shielding film 3 described later is A material having sufficient etching selectivity to the above is used.

[0055] The phase shift film 2 is patterned by dry etching using a fluorine-based gas. If possible, one or more elements selected from metalloid elements, nonmetallic elements, and metallic elements It may also contain. Among these, the metalloid element may be any metalloid element in addition to silicon. The element may be any non-metallic element, in addition to nitrogen, such as oxygen (O), carbon (C), or the like. It is preferable that the alloy contains one or more elements selected from the group consisting of gold (A), fluorine (F) and hydrogen (H). The group elements are molybdenum (Mo), tungsten (W), titanium (Ti), and tantalum (Ta ), zirconium (Zr), hafnium (Hf), niobium (Nb), vanadium (V), Cobalt (Co), Chromium (Cr), Nickel (Ni), Ruthenium (Ru), Tin (S n), boron (B), and germanium (Ge).

[0056] Such a phase shift film 2 is made of, for example, MoSiN, and is irradiated with exposure light (for example, ArF ion). A given phase difference (e.g., 140[deg]~190[deg]) ], preferably 150[deg] to 180[deg]) and a predetermined transmittance (for example, 1% to The refractive index n, the extinction coefficient k, and the film thickness of the phase shift film 2 are selected so as to satisfy the following condition: The composition of the film material and the film formation conditions are adjusted to obtain the refractive index n and extinction coefficient k. It is being done.

[0057] [Light-shielding film] The light-shielding film 3 is made of a material containing at least one element selected from the group consisting of chromium and tantalum. The light-shielding film 3 may have a single-layer structure or a laminated structure of two or more layers. In the case of a laminated structure, the exposure light or the inspection light used for defect inspection is In addition, the light shielding film having a single layer structure and the light shielding film having a single layer structure can have a reflection reducing effect. Each layer of the light-shielding film having a laminated structure of two or more layers has a structure in which the composition is almost the same in the thickness direction of the film or layer. The composition may be a single layer or a layer having a graded composition in the thickness direction. The film containing at least one element selected from the group consisting of a mixture of chlorine gas and oxygen gas is (Oxygen-containing chlorine-based gas), dry etching using chlorine-based gas that does not contain oxygen gas This is a film that can be patterned by etching.

[0058] The light-shielding film 3 is preferably made of a material containing chromium. Materials that contain chromium include chromium metal, chromium (Cr) with oxygen (O) and nitrogen (N ), carbon (C), boron (B) and fluorine (F) In general, chromium-based materials are etched with oxygen-containing chlorine-based gases. However, the etching rate of chromium metal with this etching gas is not very high. In order to increase the etching rate of the chlorine-containing gas, The material for forming the light-emitting film 3 is selected from the group consisting of chromium, oxygen, nitrogen, carbon, boron, and fluorine. It is preferable that the material contains one or more elements that are useful for forming the light-shielding film 3. The material contains one or more of molybdenum (Mo), indium (In) and tin (Sn). The above elements may be contained. One or more of the elements molybdenum, indium and tin By including the compound, the etching rate with respect to oxygen-containing chlorine-based gas can be made faster. In addition, when the light-shielding film 3 is formed of a material containing chromium, the silicon content is It is preferably 5 atomic % or less, more preferably 3 atomic % or less, and is substantially contained. It is more preferable that the film does not contain silicon. This is because the etching rate decreases, which is not preferable in terms of dry etching of the light-shielding film 3.

[0059] In addition, when the light-shielding film 3 is made of a material containing tantalum, it may contain tantalum nitride in addition to tantalum metal. Examples of such materials include materials containing one or more elements selected from the group consisting of nitrogen, oxygen, boron, and carbon. For example, Ta, TaN, TaO, TaON, TaBN, TaBO, TaBON, T aCN, TaCO, TaCON, TaBCN, TaBOCN, etc. When Ta or TaN is used as the light shielding layer of the film 3, Ta or TaN has a low reflectance with respect to the exposure light. Therefore, a laminated structure is formed by providing an anti-reflection layer made of TaO or the like on the light-shielding layer. In addition, when the light-shielding film 3 is formed of a material containing tantalum, The silicon content in the organic material is preferably 5 atomic % or less, and more preferably 3 atomic % or less. It is more preferable that the light-shielding film 3 does not substantially contain the above-mentioned tantalum oxide. The light-shielding film 3 is formed of a material containing palladium, and the light-shielding film 3 is dried using the hard mask film 4 as a mask. When patterning is performed by etching, the etching gas is a chlorine-based gas that does not contain oxygen. is used.

[0060] The light-shielding film 3 has an amorphous structure or a microcrystalline structure, and the surface roughness and shape are controlled accordingly. Reduces the line edge roughness (LER) of the light-shielding pattern formed This is preferable.

[0061] The light-shielding film 3 is preferably formed by sputtering, and is preferably formed by DC sputtering, R Both sputtering methods, such as F sputtering and ion beam sputtering, It is also possible to apply the magnetron sputtering method. It can be magnetron type or conventional type. By forming the light-shielding film 3, the light-shielding film 3 can be made into a film having an amorphous or microcrystalline structure. The deposition apparatus may be of either an in-line type or a single wafer type.

[0062] The light-shielding film 3 has a laminated structure with the phase shift film 2 and has an optical transmittance of more than 2.0 against the exposure light. It is necessary to ensure the optical density (OD). The optical density is preferably 2.8 or more, and 3 It is more preferable that it is .0 or greater.

[0063] [Hard mask film] The hard mask film 4 is made of a material consisting of silicon and oxygen, or a material consisting of nonmetallic elements other than nitrogen and and semi-metallic elements, silicon, and oxygen. In this case, the hard mask film 4 may contain any metalloid element. Among the elements, one or more elements selected from boron, germanium, antimony and tellurium When the element is contained, the hard mask film 4 is formed by a sputtering method. It is preferable because it is expected to increase the electrical conductivity of silicon used as a nonmetallic element. can include carbon (C), fluorine (F) and hydrogen (H).

[0064] The hard mask film 4 is provided in contact with the surface of the light-shielding film 3. The hard mask film 4 is The etching gas used in etching the light-shielding film 3 has etching selectivity. The hard mask film 4 is a film formed of a material that forms a pattern in the light-shielding film 3. This can act as an etching mask until the dry etching for the It is sufficient to have a film thickness that can accommodate the optical characteristics, and there are no limitations to the optical properties. Therefore, the thickness of the hard mask film 4 can be made significantly thinner than the thickness of the light-shielding film 3 .

[0065] The thickness of the hard mask film 4 is required to be 20 nm or less, and is 15 nm or less. It is preferable that the thickness of the hard mask film 4 is 10 nm or less, and more preferable that the thickness of the hard mask film 4 is 10 nm or less. In the dry etching for forming the light-shielding pattern in the hard mask film 4, This is because the thickness of the resist film that serves as the hard mask is required. The thickness of the hard mask film 4 is required to be 2 nm or more, and preferably 3 nm or more. If the thickness is too thin, depending on the conditions of high bias etching with oxygen-containing chlorine-based gas, Before the dry etching for forming the light-shielding pattern in the light-shielding film 3 is completed, the hard mask film 4 is This is because there is a risk that the pattern will disappear.

[0066] Then, a pattern is formed on the hard mask film 4 by dry etching using a fluorine-based gas. The organic resist film used as an etching mask in the etching process is a hard mask film. The thickness of the film is sufficient to function as an etching mask until the dry etching in step 4 is completed. Therefore, the hard mask film 4 is more effective than the hard mask film 4 not provided. By providing the mask film 4, the thickness of the resist film can be significantly reduced.

[0067] When the hard mask film 4 is made of a material containing silicon and oxygen, the hard mask film 4 is formed of an organic material. Since the adhesion of the hard mask film 4 to the resist film tends to be low, the surface of the hard mask film 4 is coated with HMDS (Hexamethasone). thyldisilazane) treatment (or equivalent treatment, either alone or in combination with HMDS treatment). It is preferable to improve the adhesion of the surface.

[0068] The hard mask film 4 has an amorphous structure or a microcrystalline structure, which reduces surface roughness and The line edge roughness (LER) of the formed light-shielding pattern was also measured. ) is preferable in terms of reducing

[0069] The hard mask film 4 is preferably formed by sputtering, and is preferably formed by DC sputtering. sputtering, RF sputtering and ion beam sputtering. The magnetron sputtering method can also be applied. Dual) magnetron type or conventional type is acceptable. By forming the hard mask film 4 by etching, the hard mask film 4 is made amorphous or The deposition equipment can be either an in-line type or a single-wafer type. I don't. The target material may be silicon as the main component. , a target containing silicon and oxygen, a SiO2 target, etc. can be used.

[0070] [Resist film] In the mask blank 100, a resist of an organic material is formed on the surface of the hard mask film 4. It is preferable that the thickness of the resist film is 100 nm or less. In the case of a fine pattern corresponding to the mth generation, the light-shielding pattern to be formed in the light-shielding film 3 has a line width of 4 0nm SRAF (Sub-Resolution Assist Feature) may be provided. In this case, the thickness of the resist film is reduced by providing the hard mask film 4 as described above. This allows the cross-sectional area of ​​the resist pattern formed from this resist film to be reduced. The aspect ratio can be as low as 1:2.5. Therefore, when the resist film is developed, the This can prevent the resist pattern from collapsing or coming off during the application of the resist. The resist film preferably has a thickness of 80 nm or less. It is preferable that the resist is a photoresist, and more preferable that the resist is a chemically amplified type. stomach.

[0071] [Mask blank manufacturing procedure] The mask blank 100 having the above configuration is manufactured in the following manner. The light-transmitting substrate 1 has end faces and a main surface with a predetermined surface roughness (for example, Polished to a root mean square roughness (Rq) of 0.2 nm or less within the inner area of ​​a 1 μm square After that, the substrate is subjected to a predetermined cleaning process and drying process.

[0072] Next, a phase shift film 2 is formed on the light-transmitting substrate 1 by sputtering. After the phase shift film 2 is formed, an annealing process is performed at a predetermined heating temperature. The light-shielding film 3 is formed on the shift film 2 by a sputtering method. The hard mask film 4 is formed on the substrate 3 by sputtering. In the deposition of each layer by the sputtering method, the materials constituting each layer are deposited in a predetermined composition ratio. A ring target and sputtering gas are used. If necessary, it is also reactive with rare gas. A film is formed using a mixture of the gas and the mask gas as a sputtering gas. If the rank 100 has a resist film, a hard mask film 4 may be added as necessary. The surface of the glass is treated with HMDS (Hexamethyldisilazane). A resist film is formed on the surface of the hard mask film 4 by a coating method such as spin coating. This completes the mask blank 100.

[0073] <Method of manufacturing a phase shift mask> Next, a method for manufacturing a phase shift mask according to the present embodiment will be described with reference to a mask having the structure shown in FIG. A method for manufacturing a half-tone phase shift mask using the blank 100 will be described as an example.

[0074] First, a resist film is formed on the hard mask film 4 of the mask blank 100 by spin coating. Next, a first pattern to be formed in the phase shift film 2 is applied to the resist film. The phase shift pattern is then exposed to the electron beam. The resist film is then subjected to predetermined processes such as a photoresist treatment, a developing treatment, and a post-baking treatment to form a first pattern. (Resist pattern 5a) is formed (see FIG. 2(a)).

[0075] Next, the hard mask film 4 is formed by using the resist pattern 5a as a mask and a fluorine-based gas. Then, the hard mask film 4 is dry-etched to form a first pattern (hard mask pattern 4a) is formed (see FIG. 2(b)). After that, the resist pattern 5a is removed. Here, the resist pattern 5a is not removed but left as it is, and the light-shielding film 3 is dry-etched. In this case, a resist pattern may be formed during dry etching of the light-shielding film 3. 5a disappears.

[0076] Next, using the hard mask pattern 4a as a mask, a high-bypass etch process is performed using an oxygen-containing chlorine-based gas. As a result, a first pattern (light-shielding pattern 3a) is formed in the light-shielding film 3 by assembling. 2(c)). Dry etching of the light-shielding film 3 using an oxygen-containing chlorine-based gas has been conventionally performed. The etching gas used is one having a higher mixture ratio of chlorine gas than that of the other. The mixture ratio of oxygen-containing chlorine gas in the etching equipment (chamber) is The flow rate ratio of the chlorine gas to the oxygen gas is preferably 10:1 or more, more preferably 15:1 or more. It is more preferable that the mixture ratio of the chlorine gas is 20:1 or more. By using a low-temperature etching gas, the anisotropy of dry etching can be increased. In addition, in the dry etching of the light-shielding film 3, a mixture of a chlorine-based gas and an oxygen gas is used. The combined ratio is the gas flow ratio in the etching chamber, chlorine gas:oxygen gas = 40 or less. :1 is preferred.

[0077] In addition, in the dry etching of the light-shielding film 3 using an oxygen-containing chlorine-based gas, The bias voltage applied from the back side of the substrate 1 is also higher than in the past. There are differences in the effect of increasing the bias voltage, but for example, the power [W] is preferably 15 [W] or more, more preferably 20 [W] or more, It is more preferable that the bias voltage is 0 [W] or more. By increasing the bias voltage, the oxygen-containing chlorine This can enhance the anisotropy of dry etching using the base gas.

[0078] Next, using the light-shielding pattern 3a as a mask, dry etching is performed using a fluorine-based gas. A first pattern (phase shift pattern 2a) is formed in the phase shift film 2, and The mask pattern 4a is then removed (see FIG. 2(d)). Next, a resist film is formed on the light-shielding pattern 3a by spin coating. A second pattern (light-shielding pattern) to be formed in the light-shielding film 3 is exposed to the light-shielding film by electron beam. Then, a predetermined process such as development is performed to form a second pattern (light-shielding pattern). Then, a resist film (resist pattern 6b) is formed (see FIG. 2(e)).

[0079] Next, using the resist pattern 6b as a mask, dry etching is performed using an oxygen-containing chlorine-based gas. Then, a second pattern (light-shielding pattern 3b) is formed in the light-shielding film 3 (FIG. 2(f)). In this case, the dry etching of the light-shielding film 3 is performed using a mixture of oxygen-containing chlorine-based gas at a ratio of 1:1. Conventional conditions of rate and bias voltage may be used. Furthermore, the resist pattern 6b is removed, and after a predetermined process such as cleaning, the phase shift mass 200 is obtained (see FIG. 2(g)).

[0080] The chlorine-based gas used in the dry etching in the above manufacturing process is Cl. There are no particular restrictions as long as it is included. For example, chlorine gases include Cl2, SiCl2, and C HCl3, CH2Cl2, CCl4, BCl3, etc. Also, during the above manufacturing process There are no particular restrictions on the fluorine-based gases used in dry etching as long as they contain F. For example, fluorine gases include CHF3, CF4, C2F6, C4F8, and SF6 In particular, fluorine-based gases that do not contain C have a high etching rate for glass substrates. Since the radiation rate is relatively low, damage to the glass substrate can be reduced.

[0081] The phase shift mask 200 manufactured by the above steps has a transparent substrate 1 on which a transparent substrate 2 is formed. The phase shift pattern 2a and the light shielding pattern 3b are laminated in this order from the plate 1 side. do.

[0082] In the above-described method for producing a phase shift mask, the mask blank described with reference to FIG. A phase shift mask 200 is manufactured using the mask 100. In the manufacturing process, a phase shift pattern (a fine pattern to be formed in the phase shift film 2) is formed on the light-shielding film 3. In the step of FIG. 2(c), which is a dry etching step for forming a thin film, Dry etching using an oxygen-containing chlorine-based gas that has a tendency to cause etching is applied. The dry etching using oxygen-containing chlorine-based gas in the step of FIG. 2(c) is The etching conditions are high in chlorine gas and high bias voltage. This prevents a decrease in the etching rate in the dry etching process of the light-shielding film 3. This makes it possible to suppress the etching anisotropy while enhancing the tendency of the light-shielding film 3 This reduces side etching when forming a phase shift pattern on the semiconductor substrate. In addition, the present invention provides a hard mask having excellent performance suitable for high bias etching conditions. By applying the hard mask film 4, further definition of the pattern to be formed in the hard mask film 4 is achieved. As a result, the pattern to be formed on the light-shielding film 3 can be finely formed and the pattern quality can be improved. This enables further miniaturization of the pattern and improvement of pattern quality.

[0083] In addition, side etching of the light-shielding film 3 is reduced, and the pattern to be formed in the light-shielding film 3 is Phase shift patterns formed with high precision due to further miniaturization and improved pattern quality. The light-shielding pattern 3a having turns is used as an etching mask, and the phase shift film 2 is etched with fluorine-based gas. By dry etching using a gas, the phase shift pattern 2a can be formed with high precision. By the above-mentioned operations, a phase shift mask 200 having a good pattern accuracy can be manufactured. It is possible.

[0084] (Method of Manufacturing Semiconductor Device) Next, a method for manufacturing a semiconductor device using a phase shift mask manufactured by the above-mentioned manufacturing method is described. The manufacturing method of the semiconductor device will be described. Using a half-tone phase shift mask 200, a resist film on a substrate is positioned The transfer pattern (phase shift pattern 2a) of the phase shift mask 200 is transferred by exposure. The method for manufacturing such a semiconductor device is carried out as follows.

[0085] First, a substrate on which a semiconductor device is to be formed is prepared. It may be a substrate having a semiconductor thin film, or a substrate having a fine processing layer on top of these. A resist film may be formed on the prepared substrate. A half-tone phase shift mask manufactured by the above-mentioned manufacturing method for a photoresist film 200 is used to perform pattern exposure. The transfer pattern is transferred to the resist film by exposure. The exposure light used is the ArF excimer laser, which corresponds to the phase shift film 2 formed by the laser. Uses laser light.

[0086] Furthermore, the resist film onto which the transfer pattern has been transferred is subjected to a development process to form a resist pattern. This resist pattern is then used as a mask to etch the surface of the substrate. After the processing is completed, the resist pattern is removed. The above-mentioned process is repeated on the substrate while replacing the transfer mask. Further necessary processing is carried out to complete a semiconductor device.

[0087] In the manufacturing of the above-mentioned semiconductor device, By using a light-tone phase shift mask, the initial design specifications can be fully recorded on the substrate. Therefore, the pattern of the resist film can be formed with a precision that satisfies the requirements. Using the pattern as a mask, the underlayer film beneath the resist film is dry etched to form a circuit pattern. When this is done, a highly accurate circuit pattern is formed that is free of wiring short circuits or breaks caused by insufficient precision. It is possible.

[0088] <Second embodiment> [Mask blanks and their manufacturing] In the mask blank according to the second embodiment of the present invention, the thin film for pattern formation is a light-shielding film. A mask blank used to manufacture binary masks (transfer masks). The mask blank according to the second embodiment is a recessed Levenson type phase shift mask. Masks for manufacturing masks or Chromeless Phase Lithography (CPL) masks It can also be used as a blank. The mask blank according to the second embodiment of the present invention is a mask blank according to the first embodiment. However, in the second embodiment, the phase shift film 2 is omitted. The film 3 is the light-shielding film 3 alone, and has a laminated structure of the phase shift film 2 and the light-shielding film 3 of the first embodiment. It is required to meet the required optical density (OD). The method for producing the mask blank includes the steps of: This embodiment does not include the manufacturing process and processing process (etching process) of the film 2. In the mask blank according to the second embodiment of the present invention, a substrate 1, a light-shielding film 3, and All the configurations of the mask blank, such as the hard mask film 4, are the same as those described in the mask blank according to the first embodiment. This is similar to all other configurations.

[0089] <Third embodiment> [Mask blanks and their manufacturing] In the mask blank according to the third embodiment of the present invention, the pattern-forming thin film is an absorber film (position To manufacture reflective masks (transfer masks) that have a phase shift function. It is a mask blank used in.

[0090] FIG. 6 is a diagram illustrating the configuration of a reflective mask blank according to a third embodiment of the present invention. As shown in FIG. 6, the reflective mask blank 300 includes a substrate 11 and multiple A layered reflective film 12, a protective film 13, and an absorber film that absorbs EUV (Extreme Ultra Violet) light. 14 and a hard mask film (hard mask for etching, i.e., etching mask) 15. The multilayer reflective film 12 is formed on the first main surface (front surface) side. The protective film 13 is provided to protect the multilayer reflective film 12. The protective film 13 is an etchant used for patterning the absorber film 14, which will be described later. The hard mask film 15 is made of a material that is resistant to the solvent and the cleaning solution. This serves as a mask when etching the absorber film 14. In addition, the second main surface (rear surface) side of the substrate 11 A back surface conductive film 16 for an electrostatic chuck is usually formed on the back surface of the support 11.

[0091] Each layer will be explained below.

[0092] [substrate] The substrate 11 is made of a material that prevents distortion of the absorber pattern due to heat during exposure to EUV light. Therefore, it is preferable to use a material having a low thermal expansion coefficient within the range of 0±5 ppb / °C. Examples of materials with a low thermal expansion coefficient in this range include SiO2-TiO2 glass, polycrystalline silicon, and Separation glass ceramics and the like can be used.

[0093] [Multilayer reflective film] The multilayer reflective film 12 has a function of reflecting EUV light in a reflective mask 400 described later. The multilayer reflective film 12 is made up of layers each having a periodic structure, the layers being mainly composed of elements with different refractive indices. The film has a multi-layer structure in which the films are laminated in an orderly manner.

[0094] Generally, the multilayer reflective film 12 is a thin film of a light element or a compound thereof that is a high refractive index material ( The high refractive index layer is intersected with a thin film of a heavy element or its compound, which is a low refractive index material. A multilayer film is used in which the layers are stacked in about 40 to 60 periods. A high refractive index layer / low refractive index layer laminate structure in which a refractive index layer and a low refractive index layer are laminated in this order is called one period. Alternatively, a low refractive index layer and a high refractive index layer may be laminated in this order from the substrate 11 side. The laminated structure of the low refractive index layer / high refractive index layer may be counted as one period, and multiple periods may be laminated. The outermost layer of the multilayer reflective film 12 (i.e., the surface layer of the multilayer reflective film 12 on the side opposite to the substrate 11) is In the above multi-layer film, the substrate 11 is preferably provided with a high refractive index layer and a low refractive index layer. A laminated structure in which the refractive index layers are laminated in this order (high refractive index layer / low refractive index layer) is counted as one period, and multiple periods are In the case of lamination, the uppermost layer is a low refractive index layer. The multilayer reflective film 12 is easily oxidized, and the reflectance of the multilayer reflective film 12 decreases. Therefore, a high refractive index layer can be further formed on the uppermost low refractive index layer to form a multilayer reflective film 12. On the other hand, in the above multilayer film, a low refractive index layer and a high refractive index layer are formed in this order on the substrate 11. When stacking multiple periods, one period is defined as a laminated structure (low refractive index layer / high refractive index layer) in which In this case, there is no need to further form a high refractive index layer.

[0095] In this embodiment, a layer containing silicon (Si) is used as the high refractive index layer. In addition to silicon itself, materials containing i include boron (B), carbon (C), and nitrogen (N A Si compound containing oxygen (O) and / or a Si compound containing oxygen (O) can be used. By using it as a refractive index layer, it has excellent reflectivity for EUV lithography. A reflective mask 400 is obtained. In this embodiment, the substrate 11 is a glass substrate. A plate is preferably used. Silicon has excellent adhesion to a glass substrate. The refractive index layers are made of molybdenum (Mo), ruthenium (Ru), rhodium (Rh), and A metal selected from platinum (Pt) or an alloy thereof is used. For example, a wavelength of 13n The multilayer reflective film 12 for EUV light of 1000 nm to 14 nm is preferably a Mo film and a Si film. A Mo / Si periodic laminated film is used, in which the layers are alternately laminated for about 40 to 60 periods. The high refractive index layer, which is the top layer of the reflective film 12, is formed of silicon (Si), and the top layer (Si) and A silicon oxide layer containing silicon and oxygen can be formed between the Ru-based protective film 13. By forming a silicon oxide layer, the cleaning resistance of the reflective mask 400 is improved. It is possible.

[0096] The method of forming the multilayer reflective film 12 is known in the art. Each layer of the multilayer reflective film 12 can be formed by sputtering. In the case of a Si periodic multilayer film, for example, a Si target is first deposited by ion beam sputtering. A Si film with a thickness of about 4 nm was formed on the substrate 11 using a target, and then a Mo target was used. This Si film / Mo film is one cycle, and the cycle is repeated from 40 to 6 0 period, the multilayer reflective film 12 is formed. This layer is preferably a Si layer.

[0097] [Protective film] The protective film 13 is formed by dry etching and etching in the manufacturing process of the reflective mask 400 described later. In order to protect the multilayer reflective film 12 from cleaning, the multilayer reflective film 12 is formed on the multilayer reflective film 12. When repairing a black defect in a phase shift pattern using a sagittal beam (EB), the protective film 13 prevents the multilayer The protective film 13 can protect the reflective film 12. For example, the bottom and top layers of the protective film 13 may be made of a material containing Ru. A metal other than Ru or an alloy is interposed between the bottom layer and the top layer. The protective film 13 may be made of a material containing ruthenium as a main component. Materials, such as Ru metal, Ru with titanium (Ti), niobium (Nb), molybdenum (Mo) , Zirconium (Zr), Yttrium (Y), Boron (B), Lanthanum (La), Ru alloys containing metals such as cobalt (Co) and rhenium (Re) can be used. Moreover, the material of the protective film 13 may further contain nitrogen. In particular, it is preferable to use a Ru-based protective film containing Ti. In the case of using a Ru-based protective film, the multilayer reflective film is formed by the elements constituting the multilayer reflective film from the surface of the multilayer reflective film 12 to the Ru-based protective film. The diffusion of silicon is reduced. This reduces the surface roughness during mask cleaning, and the film is The reduction in surface roughness is also a feature that reduces the reaction to EUV exposure light. Therefore, reducing surface roughness is important for improving the exposure efficiency of EUV exposure and preventing the decrease in the reflectance. This is important for improving throughput.

[0098] The thickness of the protective film 13 is not particularly limited as long as it can function as the protective film 13. From the viewpoint of the reflectance of EUV light, the thickness of the protective film 13 is preferably 1.0 nm or less. to 8.0 nm, more preferably 1.5 nm to 6.0 nm.

[0099] The protective film 13 can be formed by any known film forming method without any particular limitations. Specific examples of the method for forming the protective film 13 include a sputtering method and an ion beam sputtering method. Examples include the 'pairing' method.

[0100] [Absorber film] An absorber film 14 for absorbing EUV light is formed on the protective film 13. The material in item 4 is a gas that absorbs EUV light and is made of oxygen-containing chlorine gas or oxygen. A material that can be processed by dry etching using a chlorine-based gas that does not contain gas is used. When the absorber film 14 is patterned by dry etching using an oxygen-containing chlorine-based gas, As a suitable material, for example, the crystalline silicon used for forming the light-shielding film 3 in the first embodiment is used. On the other hand, oxygen-free chlorine-based gas is used for the Examples of suitable materials for patterning the absorber film 14 by dry etching include: Materials containing tantalum (Ta), materials containing nickel (Ni), and cobalt (Co) Examples of the material include those containing:

[0101] The tantalum (Ta)-containing material forming the absorber film 14 includes tantalum metal and tantalum containing one or more elements selected from nitrogen, oxygen, boron and carbon Examples of a-based materials include Ta, TaN, TaO, TaON, TaBN, and TaBO , TaBON, TaCN, TaCO, TaCON, TaBCN, TaBOCN, etc. In addition, tantalum (Ta) and titanium (T TaTi-based materials including i) are also applicable. A Ti alloy and a TaTi alloy containing at least one of oxygen, nitrogen, carbon, and boron. Examples of the TaTi compound include TaTiN , TaTiO, TaTiON, TaTiCON, TaTiB, TaTiBN, TaTiB O, TaTiBON, and TaTiBCON.

[0102] As a material containing nickel (Ni) for forming the absorber film 14, nickel (Ni) alone is used. Ni is more resistant to EUV light than Ta. This material has a large extinction coefficient and can be dry etched with chlorine (Cl) gas. The refractive index n of Ni at 13.5 nm is approximately 0.948, and the extinction coefficient k is approximately 0.073. In contrast, the refractive index n of TaBN, an example of a conventional absorber film material, is approximately 0. 949, and the extinction coefficient k is approximately 0.030.

[0103] Nickel compounds include nickel with boron (B), carbon (C), nitrogen (N), and oxygen. (O), phosphorus (P), titanium (Ti), niobium (Nb), molybdenum (Mo), ruthenium Ru (Ru), Rhodium (Rh), Tellurium (Te), Palladium (Pd), Tantalum (Ta ) and tungsten (W). By adding it, the etching rate can be increased to improve processability and / or cleaning. The Ni content of these nickel compounds is 50 atomic % or more. It is preferable that the content is less than 100 atomic %, and more preferably, the content is 80 atomic % or more and less than 100 atomic %. is more preferred.

[0104] On the other hand, the absorber film 14 is configured to contain cobalt (Co) and / or nickel (Ni). This makes it possible to increase the extinction coefficient k to 0.035 or more, making it possible to reduce the thickness of the absorber film. In addition, by making the absorber film 14 from an amorphous metal, the etching speed can be increased. This makes it possible to improve the pattern shape and processing characteristics. The fast metal is at least one of cobalt (Co) and nickel (Ni). The elements include tungsten (W), niobium (Nb), tantalum (Ta), titanium (Ti), Zr, hafnium (Hf), yttrium (Y) and phosphorus (P) At least one element (X) is added.

[0105] The absorber film 14 is formed by a known method, for example, a DC sputtering method or an RF sputtering method. It can be formed by a magnetron sputtering method such as a ring method.

[0106] The absorber film 14 is an absorber for EUV light for the binary type reflective mask blank 300. The absorber film 14 may be a phase shift type absorber film 14 for the purpose of absorption. For the reflective mask blank 300, we developed a phase shift function that takes into account the phase difference of EUV light. The absorber film 14 may have a thickness of 100 nm.

[0107] In the case of the absorber film 14 intended to absorb EUV light, the reflection of the EUV light on the absorber film 14 The film thickness is set so that the reflectance is 2% or less.

[0108] In the case of the absorber film 14 having a phase shift function, in the portion where the absorber film 14 is formed, The device absorbs EUV light and reduces the intensity while reflecting some of the light at a level that does not adversely affect pattern transfer. On the other hand, the reflected light from the field portion where the absorber film 14 is not formed is reflected by the protective film 13. The light is reflected from the multilayer reflective film 12 via the phase shift function of the absorber film 14. A desired phase difference is obtained between the portion where the absorber film 14 is formed and the reflected light from the field portion. The absorber film 14 can form a difference between the reflected light from the absorber film 14 and the multilayer reflective film 1 The phase difference between the reflected light from the field section and the reflected light from the field section is 160° to 200°. The light with inverted phase difference of about 180° interferes with each other at the pattern edge. This improves the image contrast of the projected optical image. The image quality is improved, and various exposure tolerances such as exposure dose tolerance and focus tolerance are expanded. Although it depends on the exposure conditions, the general guideline for the reflectance required to obtain this phase shift effect is Absolute reflectance of 1% or more, and reflectance ratio to the multilayer reflective film 12 (with protective film 13) of 2% or more It is.

[0109] The absorber film 14 can be a single layer film. Alternatively, the absorber film 14 can be a multi-layer film having two or more layers. When the absorber film 14 is a single layer film, the mask blank The number of manufacturing steps can be reduced, improving production efficiency. In this case, the upper layer is made to function as an anti-reflection film during mask pattern inspection using light. The optical constants and film thickness of the mask are appropriately set. This allows the mask pattern to be inspected using light. In this way, the use of the multi-layer absorber film 14 improves the inspection sensitivity. It is possible to add various functions to the absorber film 14. In the case of the absorber film 14 having a multi-layer structure, the absorber film 14 is used to improve the optical performance. This widens the range of adjustment of the reflectance, making it easier to obtain a desired reflectance. As a part (uppermost layer), a hard mask film 15 of the present invention described later may be used. can.

[0110] It is preferable to form an oxide layer on the surface of the nickel compound absorber film 14. By forming an oxide layer of the fluorine compound, the absorber pattern of the resulting reflective mask 400 The cleaning resistance of 14a can be improved. The thickness of the oxide layer is preferably 1.0 nm or more. The thickness of the oxide layer is preferably 5 nm or less, and more preferably 1.5 nm or more. If the thickness of the Ni oxide layer is less than 1.0 nm, it is too thin and the effect is not sufficient. If the thickness exceeds 5 nm, the effect on the surface reflectance for the mask inspection light becomes large. This makes it difficult to control the surface reflectance to a desired value.

[0111] The method for forming the oxide layer is to perform hot water treatment on the mask blank after the absorber film is formed, Ozone water treatment, heat treatment in an oxygen-containing gas, ultraviolet irradiation in an oxygen-containing gas Examples of such treatments include irradiation and O2 plasma treatment.

[0112] [Hard mask film] A hard mask film 15 is formed on the absorber film 14. The material and film of the hard mask film 15 All the details of the material, thickness, etc. of the hard mask film 4 described in the first embodiment are the same as those of the hard mask film 4 described in the first embodiment. All are the same in content.

[0113] In addition, the dry etching rate of Ni with chlorine gas is slower than that of Ta. If a resist film 11 is formed directly on an absorber film 14 made of a material containing The photoresist film 11 must be thick, making it difficult to form a fine pattern. A hard mask film 15 made of a material containing Si is formed on the resist film 14. It is possible to etch the absorber film 14 without increasing the thickness of the absorber film 11. Therefore, by using the hard mask film 15, a fine absorber pattern 4a can be formed. It can be achieved. In addition, the hard mask film 15 made of a material containing silicon and oxygen according to the present invention is different from the conventional hard mask film 15 made of a material containing silicon and oxygen according to the present invention. The present invention provides excellent performance suitable for high bias etching conditions. By applying the hard mask 15 film having the above structure, the pattern to be formed in the hard mask film 15 can be formed. This allows for further finer turns and improved pattern quality, resulting in a thinner absorber film. It is possible to further miniaturize the patterns to be formed and improve the pattern quality.

[0114] The thickness of the hard mask film 15 is determined based on an etching process for forming a transfer pattern on the absorber film 14 with high accuracy. From the viewpoint of obtaining the function as a mask, it is preferable that the thickness is 2 nm or more. The thickness of the mask film 15 is preferably 20 nm or less in order to reduce the thickness of the resist film 17. It is preferable that the thickness is 15 nm or less.

[0115] [Conductive film on the back] The second main surface (rear surface) of the substrate 11 (opposite the surface on which the multilayer reflective film 12 is formed) is generally A back surface conductive film 16 for an electrostatic chuck is formed. The electrical characteristics of the back conductive film 16 are typically 100 Ω / square or less. Chromium, tungsten, etc. are deposited by magnetron sputtering or ion beam sputtering. The substrate can be formed using targets of metals and alloys such as tin. The material of the film 16 is C 1000 nm, which is often used in the manufacture of mask blanks such as light-transmitting mask blanks. The thickness of the back conductive film 16 is set to a value sufficient for the function of the electrostatic chuck. The thickness of the back conductive film 1 is not particularly limited, but is usually 10 nm to 200 nm. The back surface conductive film 16 also functions to adjust the stress on the second main surface side of the mask blank 300. The flat reflective mass is formed by balancing the stress from the various films formed on the first main surface. It is adjusted to obtain 300 cubrans.

[0116] <Reflection mask and manufacturing method thereof> A reflective mask 400 is manufactured using the reflective mask blank 300 of this embodiment. It is possible.

[0117] A reflective mask blank 300 is prepared, and a hard mask film 15 is formed on the first main surface of the reflective mask blank 300. Then, a resist film 17 is formed (a reflective mask blank 300 is provided with the resist film 17). (Not required if the Next, a desired pattern is drawn (exposed) on the resist film 17, and then developed and rinsed. As a result, a predetermined resist pattern 17a is formed (FIG. 7(b)).

[0118] The hard mask film 15 is etched using the resist pattern 17a as a mask. A etching mask pattern 15a is then formed (FIG. 7(c)). Next, the resist pattern 17a is removed by ashing and using a resist remover. Then, dry etching is performed using the etching mask pattern 15a as a mask. The absorber film 14 is then etched to form an absorber pattern 14a (FIG. 7(d)). Thereafter, the etching mask pattern 15a is removed by dry etching (FIG. 7). (e)) Finally, wet cleaning is performed using an acidic and / or alkaline aqueous solution.

[0119] When the hard mask film 15 is made of a material containing silicon (Si), the hard mask film 15 and etching gas for removing the etching mask pattern 15a. Examples include CF4, CHF3, C2F6, C3F6, C4F6, C4F8, CH2F2, Fluorine gases such as CH3F, C3F8, SF6 and F2, as well as fluorine gases and He, H2, N2, Ar, C2H4 and mixed gases with O2, etc. (collectively referred to as "fluorine-containing gases") Examples include the "sus" system.

[0120] The etching gas for the absorber film 14 is Cl2, SiCl4, CHCl3, and CCl Chlorine gases such as chlorine gas, mixed gas containing chlorine gas and He in a specified ratio, and chlorine gas A gas mixture containing Ar and Ar at a predetermined ratio can be used as the etching gas for the absorber film 14. In this etching process, the etching gas contains virtually no oxygen, so the In this specification, the term "etching gas substantially does not contain oxygen" means that the surface is not roughened. "Not containing oxygen" means that the oxygen content in the etching gas is 5 atomic % or less. do.

[0121] The resist pattern 17a is removed immediately after the etching mask pattern 15a is formed. First, the absorber is etched using the etching mask pattern 15a with the resist pattern 17a as a mask. There is also a method of etching the film 14. In this case, the absorber film 14 is etched with a laser. The resist pattern 17a is automatically removed, simplifying the process. Then, the etching mask pattern 15a from which the resist pattern 17a has been removed is used as a mask. In the method of etching the absorber film 14, the active material from the resist disappears during the etching. The advantage of this method is that it allows stable etching without any changes in outgassing. There are signs.

[0122] The above process results in a highly accurate microfabrication with little shadowing effect and little sidewall roughness. A reflective mask 400 having a fine pattern is obtained.

[0123] <Method of Manufacturing Semiconductor Device> By performing EUV exposure using the reflective mask 400 of this embodiment, On the substrate on which the chair is to be formed, a desired pattern based on the absorber pattern 14a on the reflective mask 400 is formed. A transfer pattern can be formed. EXAMPLES

[0124] The following examples further illustrate the embodiments of the present invention.

[0125] Example 1 [Mask blank manufacturing] Referring to FIG. 1, the dimensions of the main surface are approximately 152 mm by approximately 152 mm, and the thickness is approximately 6.35 mm. The transparent substrate 1 was made of synthetic quartz glass. The surface is polished to a specified surface roughness (Rq 0.2 nm or less), and then the specified cleaning and Drying treatment is carried out.

[0126] Next, the light-transmitting substrate 1 is placed in a single-wafer DC sputtering apparatus, and molybdenum (Mo) A mixed sintered target of Mo and silicon (Si) (Mo:Si=11 atomic %:89 atomic %) was used. A mixture of argon (Ar), nitrogen (N2) and helium (He) was used for sputtering. A molybdenum film is formed on a transparent substrate 1 by reactive sputtering (DC sputtering) using a gas. A phase shift film 2 made of lysine, silicon and nitrogen was formed to a thickness of 69 nm.

[0127] Next, the phase shift film 2 is subjected to a film reaction with the transparent substrate 1 on which the phase shift film 2 is formed. In order to reduce the stress and to form an oxide layer on the surface, a heat treatment was performed. Using a heating furnace (electric furnace), heat the sample in air at 450°C for 1 hour. Heat treatment was performed. A phase shift measurement device (Lasertec MPM193) was used. The transmittance and phase difference of the phase shift film 2 after the heat treatment for light with a wavelength of 193 nm were measured. The transmittance was 6.0% and the phase difference was 177.0 degrees (deg).

[0128] Next, the light-transmitting substrate 1 on which the phase shift film 2 is formed is placed in a single-wafer DC sputtering apparatus. A chromium (Cr) target was used, and argon (Ar), carbon dioxide (CO2) , reactive sputtering (DC) in a mixed gas atmosphere of nitrogen (N2) and helium (He) As a result, chromium, oxygen, and carbon were deposited on the phase shift film 2. A light-shielding film (CrOCN film) 3 made of nitrogen was formed to a thickness of 43 nm.

[0129] Next, the light-transmitting substrate 1 on which the light-shielding film (CrOCN film) 3 is formed is subjected to a heat treatment. Specifically, a hot plate was used to heat the sample in air at a temperature of 280°C for a heating time of 20 min. After the heat treatment, the phase shift film 2 and the light-shielding film 3 were laminated. The transparent substrate 1 was measured using a spectrophotometer (Cary 4000, manufactured by Agilent Technologies). The wavelength of the ArF excimer laser light (approximately 100 nm) of the laminated structure of the phase shift film 2 and the light shielding film 3 is The optical density at 193 nm was measured and found to be 3.0 or higher.

[0130] Next, in a single-wafer RF sputtering apparatus, a phase shift film 2 and a light-shielding film 3 are laminated. A light-transmitting substrate 1 is placed, and a silicon dioxide (SiO2) target is used, and argon (Ar) Gas (pressure 0.03 Pa) was used as the sputtering gas, and the power of the RF power source was set to 1.5 kW. Then, a hard mask film made of silicon and oxygen is formed on the light-shielding film 3 by RF sputtering. The mask blank 4 was formed to a thickness of 15 nm. They manufactured 100.

[0131] The hard mask film 4 made of silicon and oxygen is resistant to fluorine-based gases, as described later. The etching rate is high, and the hard mask film can be etched quickly and cleanly. I found out that... The hard mask film 4 made of silicon and oxygen has a relatively low film density (low density). The ratio of silicon (Si) and oxygen (O) (atomic %) is Si:O = less than 1:2 (the SiO2 film is oxygen deficient).

[0132] On the main surface of another light-transmitting substrate 1, a phase shift film 2, a light-shielding film 3 and a hard mask film were formed under the same conditions. A mask blank 100 having a pattern 4 formed thereon was prepared. The mask blank 100 was subjected to X-ray The hard mask film 4 was analyzed by photoelectron spectroscopy (XPS, with RBS correction). The average contents of the constituent elements are Si: 35 atomic % and O: 65 atomic %. I did.

[0133] In addition, the light-transmitting substrate 1, the phase shift film 2, the light-shielding film 3 and the hard mask film 4 in this Example 1 The deep Si2p narrow spectrum obtained as a result of X-ray photoelectron spectroscopy analysis of The results of the depth direction chemical bond state analysis are shown in Figure 3. The results of the chemical bond state analysis in the depth direction of the O1s narrow spectrum are shown in Fig. 4. 5, respectively.

[0134] In the analysis of the hard mask film 4 by X-ray photoelectron spectroscopy, The surface of the hard mask film 4) is irradiated with X-rays to generate photoelectric conversion film 4. The energy distribution of the molecules is measured, and the hard mask film 4 is sputtered with Ar gas for a specified time. The surface of the hard mask film 4 in the recessed region is irradiated with X-rays to form a hard mask. The energy distribution of the photoelectrons emitted from the screen 4 is measured. The hard mask film 4, the light-shielding film 3, the phase shift film 2 and the light-transmitting substrate 1 are arranged in this order in the thickness direction. In this analysis, monochromated Al(1486 The photoelectron detection area is 100 μmφ, and the detection depth is about 4 to 5 nm (extraction The test was performed under the condition of a tilt angle of 45 deg (the same applies to the other examples and comparative examples described below).

[0135] In the depth direction chemical bond state analysis shown in Figs. 3 to 5, Ar gas sputtering was used. The analysis result of the outermost surface of the hard mask film 4 before (sputtering time: 0 min) was " In the "0.00 min plot," Ar is applied from the top surface of the hard mask film 4 for 1.00 min. Analysis of the hard mask film 4 at different positions in the thickness direction after it is recessed by gas sputtering The results are shown in the "1.00 min plot".

[0136] In the depth direction chemical bond state analyses in FIGS. 3 to 5, The thickness direction of the light-shielding film 3 after being engraved by Ar gas sputtering for 4.00 min. The analysis results at the position are shown in the "4.00 min plot". After digging from the top surface of the film 4 by Ar gas sputtering for 9.00 min, The analysis results for the thickness direction of the light-shielding film 3 are shown in the "9.00 min plot." In addition, the hard mask film 4 was sputtered with Ar gas for 14.00 min from the top surface. The analysis result at the thickness direction of the light-shielding film 3 after the excavation was "14.00 min. The numbers are shown in the "Lot".

[0137] In the depth direction chemical bond state analyses in FIGS. 3 to 5, Phase shift film 2 after being engraved by Ar gas sputtering for 19.00 min The analysis results for the thickness direction are shown in the "19.00 min plot". After digging from the top surface of mask film 4 by Ar gas sputtering for 24.00 min The analysis result at the thickness direction of phase shift film 2 is "24.00 min plot" The hard mask film 4 was sputtered with Ar gas for 30.00 min from the top surface. The analysis result at the thickness direction position of the phase shift film 2 after the ring is dug is "30. The plot at 44.00 min from the top surface of the hard mask film 4 is shown in FIG. At a position in the thickness direction of the transparent substrate 1 after being dug by Ar gas sputtering by n The analysis results are shown in the "44.00 min plot."

[0138] The vertical scales of the graphs in each narrow spectrum of FIGS. 3 to 5 are not the same. In the Si2p narrow spectrum of 3, the plot at 9.00 min and the plot at 14.00 min Each narrow spectrum in the "n" plot corresponds to the Si2p narrow spectrum in the other plots. The vertical scale is significantly expanded compared to the Si2p narrow spectrum in Fig. 3. The narrow spectrum of the "9.00 min plot" and "14.00 min plot" The vibration waves at the tor are not showing the presence of peaks, but rather just noise. This result is the position in the thickness direction corresponding to each Si2p narrow spectrum of the light-shielding film 3. This indicates that the silicon content is below the detection limit.

[0139] In the N1s narrow spectrum of Figure 4, the plots of "0.00min", "1.00min The narrow spectra of "n plot" and "44.00 min plot" are also similar to those of other The vertical scale is greatly expanded compared to the N1s narrow spectrum plot. That is, the plots of the N1s narrow spectrum in Figure 3 at 0.00 min and 1.00 min The amplitudes in the narrow spectra of "n plot" and "44.00 min plot" The wave of the movement does not show the presence of peaks, but only noise (i.e. That is, it is below the lower detection limit.) This result is due to the hard mask film 4 and the light-transmitting substrate 1. At the thickness direction position corresponding to each N1s narrow spectrum, the nitrogen content was below the detection limit. This indicates that it is below.

[0140] The Si2p narrow spectrum of the "4.00 min plot" in Figure 3 is also The vertical axis of the plot is smaller than that of the narrow spectrum of "n plot" and "1.00 min plot". The scale is expanded. That is, the Si2p narrow spectrum of the "4.00 min plot" The results show that a slight peak was detected in the 4.0 At the position in the thickness direction of the light-shielding film 4 corresponding to the "0 min plot", It is believed that the peak was detected due to a slight influence of the hard mask film 5.

[0141] In addition, the light-shielding film 3 was recessed from the top surface thereof by Ar gas sputtering for 1.00 min. The analysis results for the thickness direction of the hard mask film 4 after the above process showed that the surface layer of the hard mask film 4 The measurement results are for the part excluding the part.

[0142] From the results of the Si2p narrow spectrum in FIG. 3, the hard mask film 4 of this Example 1 has It has a maximum peak at a binding energy between 0.3 and 103.5 eV (103.4 eV). This result indicates that Si-O bonds exist at a certain ratio or more (degree of oxidation). This means that the Si-O bonds with a low degree of oxidation and S This means that the proportion of i-Si bonds is low.

[0143] The Si2p narrow spectrum of the hard mask film 4 in Figure 3 ("0.00 min plot" From the results of each of the narrow spectra of "1.00 min plot" and "2.00 min plot", The hard mask film 4 of Example 1 has a substantially flat waveform at binding energies between 97 and 100 eV. It was found that the sample was flat and had no peaks (below the detection limit). means that no Si—Si bond was detected in the hard mask film 4.

[0144] From the results of the Si2p narrow spectrum in FIG. 3, the hard mask film 4 of this Example 1 is The maximum peak position on the surface (0.00 min) and the maximum peak position inside the film (1.00 min) It can be seen that the difference between the two positions is just under 0.2 eV. In order to obtain high controllability during etching of the hard mask film, it is preferable to Understood.

[0145] From the results of the N1s narrow spectrum in FIG. 4, the hard mask film 4 of Example 1 has a maximum It was found that the peak was below the detection limit. This result shows that the hard mask film of Example 1 This means that no atoms bonded to nitrogen, including Si-N bonds, were detected from 4. As described above, the hard mask film 4 of the first embodiment satisfies the following three conditions simultaneously: It was found that the material is made up of the following elements: silicon (Si) and oxygen (O) The ratio of Si:O is less than 1:2 (1:1.86), which satisfies condition 1. The spectrum has a maximum peak at binding energies between 103 and 103.5 eV (103.4 eV). The maximum peak of the N1s narrow spectrum is within the detection limit. value and condition 3 is satisfied.

[0146] From the result of the O1s narrow spectrum of FIG. 5, the hard mask film 4 of this Example 1 has a It can be seen that the maximum peak occurs at binding energies between 2 and 533 eV. is the presence of a certain ratio or more of highly oxidized Si-O bonds (SiO This means that 2 is the subject. In addition, from the result of the O1s narrow spectrum of FIG. 5, the hard mask film 4 of this Example 1 The maximum peak position at the outermost surface (0.00 min) and the maximum peak position inside the film (1.00 min) It can be seen that there is almost no difference (less than 0.05 eV) between the positions of the two electrons. A very small size is preferable in order to obtain high controllability during etching of the hard mask film. I found this to be interesting.

[0147] [Phase shift mask manufacturing] Next, the mask blank 100 of Example 1 is used to perform the half-transfer of Example 1 in the following procedure. A phase shift mask 200 of a ring type was manufactured. First, a HMD was applied to the surface of the hard mask film 4. S treatment was applied.

[0148] Next, a chemical for electron beam lithography is applied to the surface of the hard mask film 4 by spin coating. A resist film made of an amplified resist was formed with a thickness of 70 nm (conventionally 80 nm). A first phase shift pattern to be formed in the phase shift film 2 is applied to the resist film. The pattern is then exposed to electron beam exposure, and a predetermined development process and cleaning process are performed to obtain a first pattern. A resist pattern 5a was formed (see FIG. 2(a)). This first pattern is a light semi-transmitting The fine pattern to be formed on the permeation film 2 (line width of 35 nm or less (conventionally 40 nm or less) SRA The hard mask film 4 is formed on the substrate 1. The resist pattern 5a thus formed is a good one with no collapse of the resist pattern being observed. there were.

[0149] Next, using the resist pattern 5a as a mask, dry etching is performed using CF4 gas. Then, a first pattern (hard mask pattern 4a) was formed in the hard mask film 4 (FIG. 2). (see (b)).

[0150] At this time, the hard mask film 4 made of silicon and oxygen is etched by a fluorine-based gas. It was found that the etching rate was large and the hard mask film could be etched quickly and with high precision. Ta. The etching rate of the hard mask film 4 depends on the thickness of the hard mask film 4 and the etching time. As a result of calculation from the time, the hard mask film 4 of Comparative Example 1 described later had a higher resistance to fluorine-based gases than the hard mask film 4 of Comparative Example 1 described later. The etching rate was relatively large. In addition, when the hard mask pattern 4a was observed with a scanning electron microscope (SEM), The wall cross section was smooth.

[0151] Next, the resist pattern 5a was removed. Then, the hard mask pattern 4a was masked. A mixture of chlorine gas (Cl2) and oxygen gas (O2) (gas flow ratio Cl2:O2= Dry etching using a 13:1 ratio (power of 50 [W] when bias voltage was applied) Then, a first pattern (light-shielding pattern 3a) is formed in the light-shielding film 3. (See FIG. 2(c)). The etching time of the light-shielding film 3 (total etching time) The time from the start of etching the light-shielding film 3 to the first exposure of the surface of the phase shift film 2 is The time was set to 1.5 times the just etching time. Overetching is performed for 50% of the etching time. By carrying out this over-etching, the verticality of the pattern sidewall of the light-shielding film 3 is improved. It becomes possible to do so.

[0152] After over-etching, the hard mask pattern 4a was observed under a scanning electron microscope (S When observed by EM, the sidewall and surface of the pattern (the surface opposite the bottom of the pattern (pattern The edges between the turns were sharp (not rounded). The cross section of the sidewall of the mask pattern 4a was smooth.

[0153] Next, the light-shielding pattern 3a is used as a mask, and dry etching is performed using fluorine-based gas (SF6+He). Etching is performed to form a first pattern (phase shift pattern 2a) in phase shift film 2. At the same time, the hard mask pattern 4a was removed (see FIG. 2(d)).

[0154] Next, a chemically amplified resist for electron beam lithography is applied onto the light-shielding pattern 3a by spin coating. A resist film made of 150 nm thick fluorine was then formed on the resist film. The second pattern, which is the pattern to be formed in the next step (a pattern including a light-shielding band pattern), is then exposed and written. Then, a predetermined process such as development is carried out to obtain a resist pattern 6 having a light-shielding pattern. b was formed (see Figure 2(e)). Next, using the resist pattern 6b as a mask, chlorine gas (Cl2) and oxygen gas (O2 ) gas mixture (gas flow ratio Cl2:O2=4:1) was used for dry etching. A second pattern (light-shielding pattern 3b) was formed on the light-shielding film 3 (see FIG. 2(f)). Furthermore, the resist pattern 6b is removed, and after a predetermined process such as cleaning, the phase shift mass As a result, 200 was obtained (see FIG. 2(g)).

[0155] A mask defect was found in the manufactured transfer mask 200 (half-tone phase shift mask). When a defect inspection was performed using a defect inspection device, the CD accuracy and line It was confirmed that both edge roughnesses met the required levels.

[0156] [Evaluation of pattern transfer performance] The phase shift mask 200 produced by the above procedure was subjected to AIMS193 (Car A Zeiss (manufactured by Zeiss) was used to expose the resist on the semiconductor device with exposure light of 193 nm wavelength. A simulation was carried out on the transferred image when the film was exposed and transferred. When the exposed image of the lithography was verified, it fully met the design specifications. The phase shift mask 200 of the first embodiment is set on the mask stage of an exposure tool, and a semiconductor device is Even if the pattern is transferred to the resist film on the device, the pattern will eventually be formed on the semiconductor device. It can be said that the path pattern can be formed with high precision.

[0157] Comparative Example 1 [Mask blank manufacturing] In Comparative Example 1, the hard mask film 4 has a silicon (Si) and oxygen (O) content ratio (atomic %) of Assuming that the Si:O ratio is 1:2 (the SiO2 film is not oxygen-deficient), The ink was manufactured and the transfer mask was manufactured. Other than the film formation method, the present embodiment is the same as that of the first embodiment. The following describes the differences from the first embodiment. do.

[0158] After forming the light-shielding film 3 in the same manner as in Example 1, a silicon (Si) target was used. Argon (Ar) gas and oxygen (O2) gas were used as sputtering gas. By performing the ring process, a hard mask made of silicon and oxygen having a thickness of 15 nm is formed on the light-shielding film 3. A mask film 4 was formed. The composition of the formed hard mask film was Si:O=1:2 (atomic percentage). ) This composition was measured by XPS.

[0159] As will be described later, the hard mask film 4 has an etching rate with respect to a fluorine-based gas. It is smaller than that in Example 1, and it cannot be said that the hard mask film can be etched quickly and cleanly. I found that... This hard mask film 4 has a tendency to have a relatively high film density (high density), The ratio (atomic percent) of silicon (Si) and oxygen (O) is Si:O=1:2 (oxygen deficiency). It was found that the SiO2 film was not damaged.

[0160] The Si2p narrow spectrum of the mask blank of Comparative Example 1 was measured in the same manner as in Example 1. N1s and O1s narrow spectra were obtained. From the results of the low spectrum (not shown), the hard mask film 4 of Comparative Example 1 had a refractive index of 103. It was found that the maximum peak was observed at a binding energy of more than 5 eV (103.8 eV). This result indicates that the proportion of Si-O bonds is very high. From the results of the i2p narrow spectrum (not shown), the hard mask film 4 of Comparative Example 1 has the following properties: The waveform is essentially flat and has no peaks between 97 and 100 eV of binding energy. This result shows that the hard mask film 4 is not This means that no i-Si bonds were detected.

[0161] From the results of the N1s narrow spectrum (not shown), the hard mask film 4 of Comparative Example 1 It was found that the maximum peak was below the detection limit. In the silicon-based film 4, the proportion of atoms bonded to nitrogen, including Si-N bonds, was not detected. As described above, the hard mask film 4 of Comparative Example 1 is made of silicon (Si). The ratio of oxygen (O) to Si is Si:O=1:2, which does not satisfy condition 1. -The spectrum has a maximum peak at a binding energy above 103.5 eV (103.8 eV). The hard mask film 4 of Comparative Example 1 had N1s The maximum peak of the narrow spectrum was below the detection limit, and only condition 3 was met. .

[0162] From the results of the O1s narrow spectrum (not shown), the hard mask film 4 of Comparative Example 1 It was found that the maximum peak was at a binding energy between 532 and 533 eV. This result indicates that there is at least a certain ratio of high oxides (Si-O bonds) (S This means that iO2 is the main

[0163] [Phase shift mask manufacturing] Next, the mask blank 100 of Comparative Example 1 was used to perform half-tone printing in the same manner as in Example 1. A phase shift mask 200 of the silicide type was manufactured. First, HMDS was applied to the surface of the hard mask film 4. Processing was carried out.

[0164] Next, a resist pattern 5a having a first pattern is formed in the same manner as in Example 1. (See Figure 2(a)).

[0165] Next, using the resist pattern 5a as a mask, dry etching is performed using CF4 gas. Then, a first pattern (hard mask pattern 4a) was formed in the hard mask film 4 (FIG. 2). (see (b)).

[0166] At this time, the etching rate of the hard mask film 4 with respect to the fluorine-based gas is the same as that in Example 1. It was found that the hard mask film could not be etched quickly and precisely. It was. The etching rate of the hard mask film 4 depends on the thickness of the hard mask film 4 and the etching time. As a result of calculation from the time, the hard mask film 4 of the first embodiment has a higher resistance to fluorine-based gases than the hard mask film 4 of the first embodiment. The etching rate was relatively small. In addition, when the hard mask pattern 4a was observed with a scanning electron microscope (SEM), The wall cross section was not as smooth as in Example 1.

[0167] Next, the resist pattern 5a was removed. Then, the hard mask pattern 4a was masked. A mixture of chlorine gas (Cl2) and oxygen gas (O2) (gas flow ratio Cl2:O2= Dry etching using a 13:1 ratio (power of 50 [W] when bias voltage was applied) Then, a first pattern (light-shielding pattern 3a) is formed in the light-shielding film 3. At this time, over-etching was carried out in the same manner as in Example 1 (see FIG. 2(c)).

[0168] After over-etching, the hard mask pattern 4a was observed under a scanning electron microscope (S Observation by EM showed that the edge between the sidewall of the pattern and the surface was sharp (no rounded corners). In addition, the cross section of the sidewall of the hard mask pattern 4a was not smooth. Ta.

[0169] After that, under the same conditions as in Example 1, the transfer mask 200 ( A phase-shift mask (light-tone type phase shift mask) was fabricated. For the transfer mask 200 (half-tone phase shift mask) of Comparative Example 1 manufactured When a defect inspection was performed using a mask defect inspection system, the CD accuracy and It was found that both the surface roughness and line edge roughness did not meet the required levels.

[0170] Comparative Example 2 [Mask blank manufacturing] In Comparative Example 2, the hard mask film 4 is formed of a material having a relatively high ratio of Si-Si bonds. The mask blanks and transfer masks were manufactured using the hard masks. The characteristics of the film 4 and the method of forming the film are the same as those of the first embodiment. I will explain the location.

[0171] After forming the light-shielding film 3 in the same manner as in Example 1, a silicon (Si) target was used. Sputtering was performed using oxygen (O2) and argon (Ar) gas as sputtering gas. By carrying out the above steps, a hard mask film 4 made of a SiO2 film having a thickness of 15 nm is formed on the light-shielding film 3. The composition of the hard mask film 4 of Comparative Example 2 was Si:O=38.5:61.5 ( The composition was measured by XPS.

[0172] The Si2p narrow spectrum of the mask blank of Comparative Example 2 was measured in the same manner as in Example 1. The N1s narrow spectrum and the O1s narrow spectrum were obtained. From the results of the p narrow spectrum (not shown), the hard mask film 4 of Comparative Example 2 had a Binding energies between 100 eV and 100 eV (99.2 eV) and binding energies below 103 eV It was found that the two compounds had peaks at 102.7 eV and 103.3 eV, respectively.

[0173] Furthermore, in the narrow spectrum of Si2p, the hard mask film 4 of Comparative Example 2 has the following characteristics: The area intensity of the Si-Si bond is more than half or equal to the area intensity of the Si-O bond. It was also found that both O bonds and Si-Si bonds exist in a considerable proportion. .

[0174] [Phase shift mask manufacturing] Next, the mask blank 100 of Comparative Example 1 was used to perform half-tone printing in the same manner as in Example 1. A phase shift mask 200 of the silicide type was manufactured. First, HMDS was applied to the surface of the hard mask film 4. Processing was carried out.

[0175] Next, a resist pattern 5a having a first pattern is formed in the same manner as in Example 1. (See Figure 2(a)).

[0176] Next, using the resist pattern 5a as a mask, dry etching is performed using CF4 gas. Then, a first pattern (hard mask pattern 4a) was formed in the hard mask film 4 (FIG. 2). (see (b)).

[0177] At this time, the hard mask film 4 has an etching rate with respect to the fluorine-based gas of Example 1. It was larger than the hard mask film 4. Therefore, the hard mask film 4 can be etched quickly and accurately. It was found that it is possible to process the material into

[0178] Next, the resist pattern 5a was removed. Then, the hard mask pattern 4a was masked. A mixture of chlorine gas (Cl2) and oxygen gas (O2) (gas flow ratio Cl2:O2= Dry etching using a 13:1 ratio (power of 50 [W] when bias voltage was applied) Then, a first pattern (light-shielding pattern 3a) is formed in the light-shielding film 3. At this time, over-etching was carried out in the same manner as in Example 1 (see FIG. 2(c)).

[0179] After over-etching, the hard mask pattern 4a was observed under a scanning electron microscope (S When observed by EM, the edges between the sidewalls of the pattern and the surface were rounded. However, the cross section of the side wall of the hard mask pattern 4a was not smooth. The etching resistance against chlorine gas is significantly reduced. , and especially under high bias etching conditions, the etching resistance tends to decrease significantly. For this reason, a dry etch process was performed using the hard mask pattern 4a as a mask. The light-shielding pattern 3a processed by etching has deteriorated CD accuracy and line edge roughness. Furthermore, a phase shifter processed by dry etching using the light-shielding pattern 3a as a mask was formed. Shift pattern 2a also had poor CD accuracy and line edge roughness.

[0180] After that, under the same conditions as in Example 1, the transfer mask 200 ( A phase-shift mask (light-tone type phase shift mask) was fabricated. For the transfer mask 200 (half-tone phase shift mask) of Comparative Example 2 manufactured When a mask defect inspection was performed using this method, the CD accuracy and line edge accuracy of the phase shift pattern 2a were It was discovered that neither Giraffeness nor the other met the required level. [Explanation of symbols]

[0181] 1 Translucent substrate 2 Phase shift film 2a Phase shift pattern 3. Light-shielding film 3a, 3b Light-shielding pattern 4. Hard mask film 4a Hard mask pattern 5a Resist pattern 6b Resist pattern 11 Substrate 12 Multilayer reflective coating 13 Protective film 14 Absorber film (phase shift film) 15 Hard mask film 16 Backside conductive film 100 mask blanks 200 Phase Shift Mask 300 Reflective Mask Blanks 400 Reflective Mask

Claims

1. A mask blank having a structure in which a pattern-forming thin film and a hard mask film are laminated in this order on a substrate, the hard mask film is made of a material containing silicon and oxygen; the maximum peak of a narrow spectrum of N1s obtained by analyzing the hard mask film by X-ray photoelectron spectroscopy is equal to or lower than the lower detection limit; The hard mask film has an O1s narrow spectrum obtained by analyzing the hard mask film by X-ray photoelectron spectroscopy, the O1s narrow spectrum having a maximum peak at a binding energy of 532 eV or more; The hard mask film is analyzed by X-ray photoelectron spectroscopy to obtain a narrow spectrum of Si2p having a maximum peak at a binding energy of 103 eV or more and 103.5 eV or less. A mask blank comprising:

2. a difference between a binding energy at a maximum peak in a narrow spectrum of Si2p obtained by analyzing a surface of the hard mask film by X-ray photoelectron spectroscopy and a binding energy at a maximum peak in a narrow spectrum of Si2p obtained by analyzing an inside of the hard mask film by X-ray photoelectron spectroscopy is 0.2 eV or less; The mask blank according to claim 1 .

3. a difference between a binding energy at a maximum peak in a narrow spectrum of O1s obtained by analyzing a surface of the hard mask film by X-ray photoelectron spectroscopy and a binding energy at a maximum peak in a narrow spectrum of O1s obtained by analyzing an inside of the hard mask film by X-ray photoelectron spectroscopy is 0.1 eV or less; The mask blank according to claim 1 or 2.

4. A mask blank described in any one of claims 1 to 3, characterized in that the hard mask film has a silicon to oxygen content (atomic %) of Si:O = less than 1:

2.

5. 5. The mask blank according to claim 1, wherein the hard mask film has a maximum peak at a binding energy of less than 533 eV in an O1s narrow spectrum obtained by X-ray photoelectron spectroscopy analysis.

6. 6. The mask blank according to claim 1, wherein the hard mask film has no peak in a Si2p narrow spectrum obtained by X-ray photoelectron spectroscopy analysis in a binding energy range of 97 eV or more and 100 eV or less.

7. 7. The mask blank according to claim 1, wherein the hard mask film has an oxygen content of 60 atomic % or more.

8. 8. The mask blank according to claim 1, wherein the hard mask film is formed of a material consisting of silicon and oxygen, or a material consisting of silicon, oxygen, and one or more elements selected from non-metallic elements and semi-metallic elements excluding nitrogen.

9. 9. The mask blank according to claim 1, wherein the pattern-forming thin film is made of a material containing one or more elements selected from the group consisting of chromium, tantalum, and nickel.

10. 10. The mask blank according to claim 1, wherein the pattern-forming thin film is a light-shielding film.

11. The mask blank according to claim 10, further comprising a phase shift film between the substrate and the light-shielding film.

12. 10. The mask blank according to claim 1, wherein the pattern-forming thin film is an absorber film.

13. A method for producing a transfer mask using the mask blank according to any one of claims 1 to 12, comprising the steps of: forming a transfer pattern on the hard mask film by etching using a resist film having a transfer pattern formed on the hard mask film as a mask; and forming a transfer pattern in the pattern-forming thin film by etching using the hard mask film on which the transfer pattern is formed as a mask.

14. 14. A method for manufacturing a semiconductor device, comprising the step of exposing and transferring a transfer pattern to a resist film on a substrate on which a semiconductor device is to be formed, using a transfer mask manufactured by the method for manufacturing a transfer mask according to claim 13.

Citation Information

Patent Citations

  • Torque motor

    JP1986058460A

  • Mask blank, phase shift mask, method for producing them, and method for producing semiconductor device

    JP2014232191A

  • Photomask blank and method for manufacturing the same

    JP2016035546A

  • Photomask blank, method for manufacturing photomask, method for forming mask pattern