Modified lignin, method for producing modified lignin, and resin composition material using modified lignin

By modifying lignin to increase H-type and G-type skeletal ratios and reduce aliphatic hydroxyl groups, the method enhances lignin's reactivity and bending strength, addressing its compatibility issues with plastics and improving molded product quality.

JP7573366B2Active Publication Date: 2024-10-25IDEMITSU KOSAN CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2019535728
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-08-10
Filing Date
2018-08-10
Publication Date
2024-10-25
Estimated Expiration
2038-08-10

AI Technical Summary

Technical Problem

Conventional methods for modifying lignin to enhance its reactivity and suitability as a plastic material are insufficient, particularly in terms of bending strength and compatibility with existing plastics, due to high aliphatic hydroxyl group content and molecular weight.

Method used

A method to modify lignin by increasing the abundance of H-type and G-type skeletal ratios and reducing aliphatic hydroxyl groups, while maintaining a low molecular weight and softening point, through a substitution reaction with phenol compounds, resulting in a modified lignin with improved reactivity and physical properties.

Benefits of technology

The modified lignin exhibits enhanced reactivity with plastics, improved mixability, and increased bending strength, making it suitable for high-quality molded products without significant loss in softening point.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573366000001
    Figure 0007573366000001
  • Figure 0007573366000002
    Figure 0007573366000002
  • Figure 0007573366000003
    Figure 0007573366000003
Patent Text Reader

Abstract

31 The modified lignin and modified polyphenols are produced in such a manner that the ratio [(2H+G) / S] of the sum of the relative abundance rate H (%) of H-type skeletons and the relative abundance rate G (%) of G-type skeletons to the relative abundance rate S (%) of S-type skeletons, as determined from the integral value measured by P-NMR, is 2.5 or more, and the abundance rate of aliphatic hydroxyl groups measured by the same method is less than 20%, as well as the modified lignin-containing resin composition material.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing modified lignin and modified polyphenol, and a resin composition material using the modified lignin. [Background technology]

[0002] From the viewpoint of reducing greenhouse gas emissions, carbon-neutral plant-derived substances are expected to be used as plastic materials. Plant-derived substances mainly include cellulose and hemicellulose derived from sugar, as well as lignin. Of these, lignin has aromatic rings, aliphatic hydroxyl groups, and aromatic hydroxyl groups, and is therefore expected to be usefully used as a plastic material. However, lignin is not easily biodegradable, is hardly soluble in solvents, and has a high softening point, making it difficult to handle. In addition, it has little reactivity with existing plastic materials, so that it has hardly been used as a plastic material. Therefore, technology is being studied to appropriately modify lignin to make it suitable as a plastic material, and to utilize the modified lignin.

[0003] For example, Patent Document 1 discloses a technology relating to modified lignin in which a benzoxazine skeleton is introduced into lignin to impart reactivity without lowering the molecular weight of the lignin, and a molding material containing the modified lignin to improve the mechanical strength, etc., of the molded product. Furthermore, Patent Document 2 discloses a technique in which lignin is reacted with phenols in the presence of a catalyst to form phenols, which are then heated together with an alkali to form alkalized lignin, and aldehydes are added to the alkalized lignin to form hydroxymethylated lignin, thereby increasing the reactivity of the lignin, and a technique in which the lignin with increased reactivity is used in a binder composition. Furthermore, Patent Document 3 discloses a phenol-modified lignin resin having improved curability and resin strength, which is produced by reacting lignin, phenols, and aldehydes in the presence of an acid. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 5671430 [Patent Document 2] Special Publication No. 2016-540058 [Patent Document 3] International Publication No. 2015 / 147165 Summary of the Invention [Problem to be solved by the invention]

[0005] According to the conventional technology, it is possible to improve the curing reactivity of materials containing lignin to some extent. However, when considering high-quality materials such as substitutes for metal parts, the performance of the formed material, such as bending strength, is insufficient when using the conventional technology. Therefore, it is necessary to further improve the reactivity of lignin.

[0006] Therefore, an object of the present invention is to provide a method for producing modified lignin and modified polyphenols that have improved reactivity with existing plastic materials, and a modified lignin-containing resin composition material that can give molded products with improved physical properties such as bending strength. [Means for solving the problem]

[0007] As a result of intensive research to solve the above problems, the inventors have found that the above problems can be solved by achieving, in a single reaction, a skeleton ratio conversion of the basic skeleton of lignin, a reduction in aliphatic hydroxyl groups, and further a reduction in molecular weight. That is, the present invention is as follows.

[0008] [1] 31 the ratio [(2H+G) / S] of the sum of twice the relative abundance H (%) of the H-type skeleton to the relative abundance S (%) of the S-type skeleton determined from the integral value measured by P-NMR and the relative abundance G (%) of the G-type skeleton is 2.5 or more; 31A modified lignin in which the proportion of aliphatic hydroxyl groups relative to the total proportion of aliphatic hydroxyl groups and aromatic hydroxyl groups, as determined from the integrated value measured by P-NMR, is less than 20%. [2] A method for producing a modified polyphenol, comprising the step of reacting a polyphenol-containing composition with a phenol compound in which at least one of the 2nd, 4th and 6th positions, which are the positions of the substituents relative to a hydroxyl group, is a hydrogen atom. [3] A modified lignin-containing resin composition material containing the modified lignin. Effect of the Invention

[0009] According to the present invention, it is possible to provide a method for producing modified lignin and modified polyphenols that have improved reactivity with existing plastic materials, as well as a modified lignin-containing resin composition material that can give molded products with improved physical properties such as bending strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] [Modified lignin] (Basic structure of lignin) Lignin is a polymer compound formed by polymerization of three types of lignin monomers, which are p-hydroxycinnamic alcohols, and has a basic skeleton represented by the following formula (2).

[0011] [ka]

[0012] In the above formula (2), the substituent R 3 and R 4 R represents a hydrogen atom or a methoxy group. 3 and R 4 When both are hydrogen atoms, it is a p-hydroxyphenyl nucleus (H-type skeleton), and R 3 and R 4 When either one of the above is a hydrogen atom, the guaiacyl nucleus (G-type skeleton) is formed, and R 3 and R 4 When neither of these is a hydrogen atom, it is called a syringyl nucleus (S-type skeleton). In the above formula (2), X represents a carbon atom, and Y represents a bond to a hydrogen atom or a carbon atom.

[0013] In the basic structure of lignin, R 3 and R 4 The carbon atom bonded to R is a highly reactive site (hereinafter, simply referred to as the "reactive site"). 3 and R 4 If R is a methoxy group, the reactivity of that carbon atom is poor. Therefore, in order to react with lignin, R 3 and R 4 must be a hydrogen atom. Furthermore, lignin contains not only the aromatic moieties mentioned above but also aliphatic moieties, and the hydroxyl groups present in the aliphatic moieties have poor oxidation stability (they are easily converted to aldehydes or carboxylic acids by oxidation). Therefore, the fewer the aliphatic hydroxyl groups, the better the reactivity with existing plastic materials. Furthermore, by reducing the molecular weight of lignin without significantly lowering its softening point, its mixability is improved, and its reactivity with existing plastic materials is improved. In other words, lignin that has few aliphatic hydroxyl groups and contains a large amount of the two highly reactive H-type and G-type skeletons, and that has been reduced in molecular weight without significantly lowering its softening point, is highly reactive and suitable as a plastic material.

[0014] However, the abundance of each of the above basic skeletons and the aliphatic hydroxyl groups vary depending on the type of plant from which the lignin is made. In addition, natural lignin is originally a gigantic molecule whose molecular weight cannot be measured, and existing separation methods have the disadvantage that reducing the molecular weight also significantly reduces the softening point. For example, in woody biomass, the lignin derived from broadleaf trees contains the above G-type and S-type skeletons, while the lignin derived from coniferous trees contains the above G-type and S-type skeletons, but the G-type skeleton is more prevalent. Furthermore, the lignin derived from broadleaf trees and coniferous trees contains almost no H-type skeletons. In addition, in lignin derived from herbaceous biomass, the above-mentioned H-type skeleton, G-type skeleton and S-type skeleton are present, but the occurrence rate of the H-type skeleton is low. In addition, coniferous lignin has many aliphatic hydroxyl groups, while the presence of aliphatic hydroxyl groups decreases in broadleaf lignin and herbaceous lignin, in that order. Therefore, in order to increase the reactivity of lignin, it is necessary to increase the proportion of H-type and G-type skeletons, reduce the aliphatic hydroxyl groups, and modify lignin using a low-molecular-weight method that does not significantly lower the softening point.

[0015] (Modified lignin) The modified lignin of the present invention is 31 The ratio of the sum of the relative abundance rate H (%) of the H-type skeleton to the relative abundance rate S (%) of the S-type skeleton determined from the integral value measured by P-NMR and the relative abundance rate G (%) of the G-type skeleton [(2H+G) / S] is 2.5 or more, and 31 The percentage of aliphatic hydroxyl groups relative to the total percentage of aliphatic hydroxyl groups and aromatic hydroxyl groups, as determined from the integrated value measured by P-NMR, is less than 20%. Furthermore, the modified lignin of the present invention is preferably reduced in molecular weight to a number average molecular weight of less than 1,000 and has a softening point of 90° C. or higher.

[0016] <Ratio of the abundance of reactive sites (H-type skeleton × 2 + G-type skeleton) to non-reactive sites (S-type skeleton) [(2H+G) / S], and the abundance of aliphatic hydroxyl groups> The raw lignin is converted into the above R by the substitution reaction in the production method described later. 3 and R 4 becomes a hydrogen atom, the reaction points of the modified lignin increase, the aliphatic hydroxyl groups decrease, and the molecular weight is reduced without significantly lowering the softening point. As mentioned above, H type has two reactive sites and G type has one, and as the above ratio [(2H+G) / S] shows, the modified lignin of the present invention has many reactive sites and has good reactivity. However, in the case of lignin derived from coniferous trees such as cedar, it has been analytically proven that the above ratio [(2H+G) / S] is 3 or more before modification, but aliphatic hydroxyl groups account for 20% or more of the total hydroxyl groups (the sum of the abundance of aliphatic hydroxyl groups and aromatic hydroxyl groups), which is undesirable as a plastic material. Therefore, if the above ratio is less than 2.5 or the proportion of aliphatic hydroxyl groups is 20% or more, the reactivity of the modified lignin is insufficient, making it unsuitable as a plastic material, and it cannot be expected to give molded products with improved physical properties such as bending strength.

[0017] In contrast, the modified lignin of the present invention has a ratio of the abundance ratios [(2H+G) / S] of 2.5 or more, and the abundance ratio of aliphatic hydroxyl groups relative to the total abundance ratios of aliphatic hydroxyl groups and aromatic hydroxyl groups is less than 20%. In addition, from the viewpoint of further improving the reactivity of the modified lignin and expecting to give a molded product with improved physical properties such as bending strength, the ratio [(2H+G) / S] is preferably 2.8 or more, more preferably 3.0 or more, even more preferably 3.5 or more, even more preferably 4.5 or more, even more preferably 5.5 or more, even more preferably 7.0 or more, even more preferably 9.0 or more, even more preferably 12.0 or more, and even more preferably 14.0 or more. In addition, from the same viewpoint, the abundance ratio of aliphatic hydroxyl groups is preferably less than 15%, more preferably less than 12%, even more preferably less than 10%, even more preferably less than 6%, and even more preferably less than 3%.

[0018] The relative abundance rates of the S-type skeleton, the H-type skeleton, and the G-type skeleton and the abundance rate of the aliphatic hydroxyl group are as follows: 31 This is a value calculated from the integral value measured by P-NMR. 31 More details about the P-NMR measurement are as described in MAGNETIC RESONANCE IN CHEMISTRY, VOL. 33, 375-382 (1995). In the present invention, more specifically, the measurement can be performed by the method described in the examples below.

[0019] <Lower molecular weight and softening point> The modified lignin of the present invention is produced by a substitution reaction in the production method described below. 3 and R 4The molecular weight of lignin is reduced because the molecular chain of the lignin is modified. In this way, the lowering of the molecular weight of lignin is expected to improve its mixability (kneadability or stirrability) with other plastic materials and to provide molded products with improved physical properties such as bending strength.

[0020] As described above, the raw lignin is reduced in molecular weight by the cleavage of the carbon chain caused by the substitution reaction. However, in the modified lignin of the present invention, since a phenol compound is always inserted at the substitution site in the production method described below, the softening point does not decrease significantly even if the molecular weight is reduced. Therefore, the modified lignin of the present invention can have a softening point of preferably 90°C or higher, more preferably 130°C or higher, and even more preferably 160°C or higher. If the softening point is 90°C or higher, defects such as swelling are unlikely to occur during molding and post-curing of the resin composition material containing the modified lignin. In addition, the softening point of the modified lignin is preferably 200°C or lower, more preferably 190°C or lower, even more preferably 180°C or lower, and even more preferably 170°C or lower. If the softening point is 200°C or lower, the resin composition material containing the modified lignin becomes easier to handle. Furthermore, the modified lignin of the present invention preferably has a number average molecular weight of 900 or more and 1,200 or less and a weight average molecular weight of 1,900 or more and 2,700 or less; preferably has a number average molecular weight of 600 or more and less than 900 and a weight average molecular weight of 1,100 or more and less than 1,900; and preferably has a number average molecular weight of 500 or more and less than 600 and a weight average molecular weight of 900 or more and less than 1,100.

[0021] The modified lignin of the present invention, for example, has a molecular weight distribution (Mw / Mn) of usually about 1.2 to 3.0, preferably 1.3 to 2.8, more preferably 1.4 to 2.5, even more preferably 1.5 to 2.0, even more preferably 1.5 to 1.9, and even more preferably 1.5 to 1.8.

[0022] Furthermore, the modified lignin of the present invention preferably has a softening point of 160°C or higher and 200°C or lower if the number average molecular weight is 900 or higher and 1,200 or lower; preferably has a softening point of 130°C or higher and 190°C or lower if the number average molecular weight is 600 or higher and less than 900; preferably has a softening point of 110°C or higher and 170°C or lower if the number average molecular weight is 500 or higher and less than 600; and preferably has a softening point of 90°C or higher and 170°C or lower if the number average molecular weight is 300 or higher and less than 500. In addition, the modified lignin of the present invention preferably has a softening point of 160 ° C. or more and 200 ° C. or less if the number average molecular weight is 900 or more and 1,200 or less and the weight average molecular weight is 2,400 or more and 3,000 or less, and preferably has a softening point of 130 ° C. or more and 190 ° C. or less if the number average molecular weight is 600 or more and less than 900 and the weight average molecular weight is 1,100 or more and less than 2,400, and preferably has a softening point of 110 ° C. or more and 170 ° C. or less if the number average molecular weight is 500 or more and less than 600 and the weight average molecular weight is 900 or more and less than 1,100, and preferably has a softening point of 90 ° C. or more and 170 ° C. or less if the number average molecular weight is 300 or more and less than 500 and the weight average molecular weight is 600 or more and less than 900. These can be used depending on the properties of the existing plastic material to be reacted, and it is expected that the reactivity of the modified lignin can be improved by improving the mixability, and a molded product with improved physical properties such as bending strength can be obtained. The number average molecular weight and weight average molecular weight can be measured by the method described in the Examples section below.

[0023] [Method of producing modified polyphenols] The method for producing a modified polyphenol of the present invention includes a step of reacting a polyphenol-containing composition with a phenol compound (hereinafter sometimes simply referred to as a "phenol compound") in which at least one of the 2nd, 4th, and 6th positions, which are the positions of the substituents relative to the hydroxyl group, is a hydrogen atom.

[0024] The method for producing modified polyphenol of the present invention is a method for producing modified polyphenol that is applied to the modification of polyphenol-containing compositions such as tannin and lignin. In particular, in the method for producing modified polyphenol of the present invention, the raw material polyphenol contained in the polyphenol-containing composition is preferably lignin from the viewpoint of usefulness as a plastic material. Therefore, the polyphenol-containing composition is preferably a lignin-containing composition or lignin, more preferably lignin, and the modified polyphenol is preferably modified lignin. In the following, a specific example will be given in which the raw polyphenol contained in the polyphenol-containing composition is lignin (hereinafter sometimes referred to as "raw lignin") and the modified polyphenol is modified lignin, but the method for producing modified polyphenol of the present invention is not limited to these raw lignins and modified lignins.

[0025] (Reaction process) <Lignin> The raw material lignin used as the raw material in the method for producing modified polyphenols of the present invention is derived from plant biomass, such as woody biomass and herbaceous biomass. In addition, in the method for producing modified lignin of the present invention, biomass residues derived from plant biomass such as woody biomass and herbaceous biomass can also be used as the lignin-containing composition. Examples of biomass residues include black liquor (sulfite lignin, kraft lignin, soda lignin, etc.) and tannin, and these may be used alone or in combination of two or more kinds.

[0026] Examples of plant biomass include woody biomass and herbaceous biomass. Examples of woody biomass include coniferous and broad-leaved trees such as cedar, cypress, Japanese cypress, cherry blossom, eucalyptus, beech, and bamboo. Examples of herbaceous biomass include palm trunks and empty bunches, palm fruit fiber and seeds, bagasse (sugar cane and high-biomass sugar cane residue), cane tops (sugar cane tops and leaves), energy cane, rice straw, wheat straw, corn cobs, stems and leaves, and residues (corn stover, corn cobs, corn hulls), sorghum residues (including sweet sorghum), jatropha seed husks and shells, cashew husks, switchgrass, erianthus, high-biomass yield crops, and energy crops. Among these, from the viewpoints of availability and compatibility with the production method applied in the present invention, herbaceous biomass is preferred, with empty palm bunches, wheat straw, corn cobs, stems and leaves, residues (corn stover, corn cob, corn hull), bagasse, cane tops, energy cane, and residues thereof after useful component extraction being more preferred, with corn cobs, stems and leaves, residues (corn stover, corn cob, corn hull), bagasse, cane tops, and energy cane being even more preferred. The above useful components include, for example, hemicellulose, carbohydrates, minerals, moisture, etc. Bagasse contains about 5 to 30 mass % of lignin, and the lignin in bagasse contains all of the H, G and S nuclei as basic skeletons. The plant biomass may be in the form of a pulverized material, or may be in the form of a block, chip, powder, or a water-containing material.

[0027] Methods for separating raw lignin from plant biomass include the organosolv method, the hot compressed water method, the steam explosion method, the ammonia treatment method, the ammonia explosion method, the acid treatment method, the alkali treatment method, the oxidative decomposition method, the thermal decomposition method, and the microwave heating method. Among these, the organosolv method is preferred from the viewpoint of easy removal of the solvent. Specifically, for example, lignin contained in plant biomass is dissolved into the solvent by treating it at high temperature using an organic solvent or a solvent containing an organic solvent and water, and the lignin-containing solution is filtered to remove cellulose and the like, and the solution is then concentrated and dried to separate the raw lignin.

[0028] The number average molecular weight (Mn) of the raw material lignin is usually about 500 to 10,000, preferably 1,000 to 5,000, more preferably 1,250 to 3,000, and even more preferably 1,250 to 2,500. Within the above range, dissolution of the raw material lignin in the phenol compound can proceed smoothly at the reaction temperature. For the same reasons as above, the weight average molecular weight (Mw) of the raw lignin is usually about 1,000 to 100,000, preferably about 2,000 to 10,000, more preferably about 2,500 to 4,000, and even more preferably 2,500 to 3,500. For the same reasons as above, the molecular weight distribution (Mw / Mn) of the raw material lignin is usually about 1.5 to 10.0, preferably 2.0 to 5.0, more preferably 2.0 to 3.0, and even more preferably 2.0 to 2.5. The number average molecular weight, weight average molecular weight and molecular weight distribution can be measured by the methods described in the Examples section below.

[0029] When the biomass residue is used as a lignin-containing composition (raw material), the pH of the biomass residue in a water-containing state is adjusted to acidic. A phenolic compound is added thereto in an amount equal to or greater than the amount of lignin contained in the raw material by weight. Heating is performed to remove water while hot (phenolic compounds have a high boiling point, and water can be removed by providing an appropriate oil-water separator such as a Dean-Stark). Heating is continued for 1 to 2 hours after water removal. The heated liquid contains insoluble matter, and is filtered while hot using 5C filter paper. The filtered solid is unreacted matter and inorganic impurities. The filtrate is distilled under reduced pressure to remove unreacted phenolic compounds. Phenol compounds that cannot be completely removed by distillation are dissolved in acetone as necessary and removed by repeated reprecipitation with water, which is a poor solvent. The separated solid is modified lignin that has already been modified. If the phenolic compounds remaining during distillation do not cause problems in subsequent reactions, they can be used as is.

[0030] <Phenol compounds> The phenolic compound used in the method for producing modified polyphenols of the present invention must have a hydrogen atom at at least one of the 2-, 4- and 6-positions, which are the positions of the substituents relative to the hydroxyl group. This is because a phenolic compound having hydrogen atoms at the 2-, 4- and 6-positions (i.e., the ortho and para positions) is particularly suitable as a receptacle for the substituents in the substitution reaction due to its orientation, and by mixing the raw lignin with the phenolic compound, the R 3 and R 4 This is because the substituent of R of the raw lignin is transferred to the 2-position, 4-position, or 6-position of the phenol compound. 3 or R 4 Alternatively, both may be hydrogen atoms, resulting in a modified lignin with an increased number of the aforementioned reaction sites. Therefore, the substitution reaction reduces the S-type skeleton in the raw lignin and increases the G-type and H-type skeletons, improving the reactivity. As described above, the substitution reaction also modifies the molecular chain of the raw lignin, resulting in a decrease in molecular weight and improving the mixability of the modified lignin. The phenol compounds may be used alone or in combination of two or more.

[0031] The phenol compound is preferably a compound represented by the following formula (1): By using the phenol compound, the substitution reaction can proceed smoothly since there are at least three positions for accepting the above-mentioned substituents.

[0032] [ka]

[0033] In the above formula (1), R 1 and R 2 each independently represents a hydrogen atom, a hydroxyl group, or an alkyl group having 1 to 15 carbon atoms; R 1 and R 2 may be the same or different. The alkyl group having 1 to 15 carbon atoms may be linear or branched. It is preferably a linear or branched alkyl group having 1 to 15 carbon atoms, more preferably a linear or branched alkyl group having 1 to 10 carbon atoms, even more preferably a linear or branched alkyl group having 1 to 5 carbon atoms, and still more preferably a linear alkyl group having 1 to 5 carbon atoms.

[0034] Examples of the phenol compound represented by the above formula (1) include phenol, resorcinol, phloroglucinol; 3-alkylphenols such as meta-cresol, 3-ethylphenol, and 3-propylphenol; 5-alkylresorcinols such as 5-methylresorcinol, 5-ethylresorcinol, and 5-propylresorcinol; and 3,5-dialkylphenols such as 3,5-dimethylphenol, 3-methyl-5-ethyl-phenol, and 3,5-diethylphenol.

[0035] In addition, since the phenolic compound has multiple hydroxyl groups, the acidity of the compound increases, and it is expected that the reaction will proceed without the need for a catalyst. 1 and R 2 It is more preferable that at least one of the above groups is a hydroxyl group. Specific examples of such phenolic compounds include resorcinol, phloroglucinol, and 5-alkylresorcinols (5-methylresorcinol, 5-ethylresorcinol, etc.).

[0036] <Mass ratio [phenolic compounds / raw polyphenols]> In the production method of the present invention, the mass ratio of the phenol compound to the raw lignin (raw polyphenol, or in the case of a biomass residue, the lignin in the biomass residue) [phenol compound / raw lignin] is usually about 0.1 to 15, preferably 0.3 to 15, more preferably 0.5 to 15, even more preferably 1 to 15, even more preferably 1 to 13, even more preferably 1 to 12, even more preferably 1 to 10, and even more preferably 1 to 5. When the mass ratio of the phenol compound to the raw lignin is within the above range, the substitution reaction described above can be smoothly carried out. The lignin content in the biomass residue is calculated by crushing the sample raw material using a Willey mill, pretreating it by drying at 105°C, and then measuring it by analyzing the constituent sugars.

[0037] <Acid catalyst> In the production method of the present invention, the reaction between lignin and a phenolic compound is preferably carried out without a catalyst or in the presence of an acid catalyst, preferably in an amount of more than 0 to 3.0 mass%, and more preferably 0.2 to 3.0 mass%, based on the total amount of the raw lignin and the phenolic compound. As described above, the reaction can proceed without a catalyst depending on the phenol compound used in the reaction. By proceeding without a catalyst, for example, it is possible to omit post-treatment (purification process) after the reaction process, and it is expected that the physical properties such as bending strength of molded products using the obtained modified lignin as a plastic material will be improved.

[0038] Examples of the acid catalyst include inorganic acids such as phosphoric acid, phosphoric acid esters, hydrochloric acid, sulfuric acid, and sulfuric acid esters, and organic acids such as acetic acid, formic acid, oxalic acid, and p-toluenesulfonic acid. One or more types of acid catalysts may be used in combination. When an acid catalyst is used in the above reaction, the amount of the acid catalyst used is not particularly limited as long as it is usually more than 0 relative to the total amount of the raw lignin and the phenolic compound, but the effect of adding the acid catalyst can be exhibited well, and the reaction is usually carried out in the presence of 0.01 to 3.0 mass% of the acid catalyst from the viewpoint of impurities remaining in the modified lignin, preferably 0.1 to 3.0 mass%, more preferably 0.2 to 3.0 mass%, and even more preferably 0.4 to 2.6 mass%. If the amount of the acid catalyst used is within the above range, the above-mentioned substitution reaction can be smoothly progressed.

[0039] <Reaction temperature and time> The reaction temperature is not particularly limited as long as it is usually 100° C. or higher, but is usually about 140° C. or higher and 350° C. or lower, preferably 140° C. or higher and 300° C. or lower, more preferably 140° C. or higher and 270° C. or lower, even more preferably 140° C. or higher and 250° C. or lower, even more preferably 150 to 230° C., and even more preferably 150 to 200° C. If it is above 140° C., most of the phenol compounds can be dissolved to allow the reaction to proceed, and if it is 300° C. or lower, the proceeding of the reverse reaction can be prevented. The reaction time is usually about 0.1 to 15 hours, but from the viewpoint of allowing the reaction to proceed sufficiently and modifying the raw lignin, it is preferably 0.5 hours or more, and more preferably 1 hour or more. Also, from the viewpoint that the reaction cannot be expected to proceed if the reaction time is too long, the upper limit is preferably 10 hours or less, and more preferably 2 to 8 hours.

[0040] <solvent> The reaction between the raw lignin and the phenolic compound can be carried out without a solvent. In addition, any one or more of organic solvents such as alcohols such as methanol, ethanol, isopropyl alcohol, ketones such as acetone, methyl ethyl ketone, ethers such as tetrahydrofuran, and aromatics, and water may be used, and it is preferable to use any one or more of ethanol, acetone, and water. From the viewpoint of preventing the solvent from being mixed into the modified lignin and of making the reaction efficient without requiring a process of removing the solvent after the reaction, it is preferable to carry out the reaction without a solvent.

[0041] (purification process) The modified lignin of the present invention is produced by carrying out the above-mentioned reaction process. Therefore, the modified lignin-containing material obtained by the reaction process can be used as it is as a plastic material, but a purification process may be carried out after the reaction process. <Solid-liquid separation> After the above reaction, the modified lignin is dissolved in the phenol compound, but unreacted substances and inorganic residues remain in the liquid as solids. These are preferably removed by filtration (hot). For example, the reaction liquid is placed in a pressurized hot filter equipped with filter paper such as No. 5C or No. 2, and pressure-filtered at about 20 to 150°C, usually about 40 to 90°C, and at about 0.1 to 0.99 MPa, usually about 0.1 to 0.4 MPa. The filtered solid may be appropriately diluted and / or washed with a phenol compound and filtered. In this filtration, the modified lignin is contained in the filtrate. In addition, for example, the reaction product liquid may be diluted and / or washed with any one or more of low-boiling point general-purpose hydrophilic solvents such as water, ketones such as acetone and methyl ethyl ketone, alcohols such as methanol, ethanol, and isopropyl alcohol, and ethers such as tetrahydrofuran, and separated into solid and liquid. In this solid-liquid separation, the modified lignin is contained in the solution. The method for performing solid-liquid separation is not particularly limited, but examples thereof include filtration, a filter press, centrifugation, and a dehydrator. <distillation> Distillation can be carried out, for example, by distilling the modified lignin-containing material obtained by the reaction step at a temperature of about 40 to 200°C, usually about 80 to 150°C, under a reduced pressure of about 3 to 20 kPa, usually about 5 to 10 kPa, to remove the phenolic compounds after the reaction, thereby purifying the product. In this distillation, the modified lignin is obtained as a solid. In addition, for example, when a dilution solvent other than the phenolic compounds is used, the solvent other than the phenolic compounds can be distilled under reduced pressure at an appropriate temperature taking into account the boiling point of the solvent to remove the low-boiling point general-purpose hydrophilic solvent, and then the phenolic compounds can be removed by the same method as above. In this distillation, the modified lignin is obtained as a solid. <Drying under reduced pressure> The modified lignin obtained by distillation may be purified by removing the phenolic compounds after the reaction by heating it to typically 50 to 200° C. and vacuum drying it in a solid or molten state. Alternatively, the modified lignin in a heated and fluid state after distillation may be similarly vacuum dried as it is to remove the phenolic compounds after the reaction. <Reprecipitation> In addition, the modified lignin-containing material obtained by the reaction process can be purified by dissolving it in a solvent such as acetone and reprecipitating it by adding ion-exchanged water, which is a poor solvent for the modified lignin, to remove the phenolic compounds after the reaction. In the purification, the above-mentioned filtration, distillation under reduced pressure, solidification to dryness under reduced pressure, and reprecipitation may be combined, or the same steps may be repeated. The amount of phenol compounds remaining in the modified lignin is not particularly limited, but is usually less than 30%, preferably less than 10%, more preferably less than 5%, and even more preferably less than 1%.

[0042] (Degree of modification) The method for producing modified polyphenols of the present invention allows for the production of modified lignin in which the H-type and G-type skeletons are abundant compared to the basic skeleton of the raw lignin, while at the same time reducing the aliphatic hydroxyl groups of the raw lignin, thereby increasing the reaction sites and reducing the aliphatic hydroxyl groups. In addition, the modified polyphenol produced by the method of the present invention has a smaller number average molecular weight and weight average molecular weight than the raw polyphenol in the polyphenol-containing composition. Therefore, the modified lignin obtained by the above-mentioned production method has a lower molecular weight and improved mixability. Furthermore, it is preferable that the modified polyphenol produced by the method of the present invention has a smaller molecular weight distribution (Mw / Mn) than the raw polyphenol in the polyphenol-containing composition. Specifically, by the production method of the present invention, 31The total reaction site [2H+G] based on the relative abundance H(%) of H-type skeletons and the relative abundance H(%) of G-type skeletons determined from the integral value measured by P-NMR is usually increased by 3% or more, preferably by 4% or more, before and after modification, and it is also possible to obtain a modified lignin having the abundance of the above-mentioned aliphatic hydroxyl groups of less than 20%. Furthermore, the number average molecular weight and weight average molecular weight of the modified lignin are lowered compared to the raw lignin, but the softening point is preferably not lowered below 90°C.

[0043] [Modified lignin-containing resin composition materials and molded products] The present invention also provides a modified lignin-containing material, particularly a modified lignin-containing resin composition material, containing the modified lignin or the modified lignin produced by the above-mentioned production method, as well as a molded product using the same. In addition to the modified lignin obtained by the above-mentioned production method, resin components such as thermosetting resins and thermoplastic resins may be included. The components other than the modified lignin are described below. (thermosetting resin) The modified lignin-containing resin composition may further contain a thermosetting resin. Examples of the thermosetting resin include other general thermosetting resins such as phenolic resins, epoxy resins, polyurethane resins, melamine resins, urea resins, unsaturated polyester resins, silicone resins, and alkyd resins. Among these, phenolic resins are preferred because, like modified lignin, they have phenolic hydroxyl groups, can react with modified lignin, and can be used as a diluent for modified lignin. Among phenolic resins, novolac-based phenolic resins and resol-based phenolic resins are more preferred. These thermosetting resins may be used alone or in combination of two or more.

[0044] The content of the thermosetting resin in the modified lignin-containing resin composition material may be determined according to the purpose, but from the viewpoint of obtaining good physical properties and moldability, it is preferably 100 to 300 parts by mass, more preferably 150 to 250 parts by mass, per 100 parts by mass of the modified lignin.

[0045] (Aldehydes) The modified lignin-containing resin composition may further contain aldehydes. A self-curing molding material can be produced by using a modified lignin-containing resin composition material that contains modified lignin and aldehydes. Examples of aldehydes include formaldehyde, paraformaldehyde, acetaldehyde, propionaldehyde, furfural, benzaldehyde, phenylacetaldehyde, salicylaldehyde, and the like, and among these, formaldehyde is preferred.

[0046] The molar ratio of the phenol group to formaldehyde contained in the modified lignin [formaldehyde / phenol group] is preferably 1.0 to 2.5, more preferably 1.2 to 2.0. If the molar ratio is within the above range, there is no risk of a decrease in the curing rate during the reaction. In order to accelerate the hardening reaction between the modified lignin and aldehydes, it is preferable to use an alkali, such as sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ammonia, tetramethylammonium hydroxide, or an alkylamine. There are no limitations on the temperature and reaction time during the curing reaction of the modified lignin and the aldehydes, but it is usually about 60 to 130° C., and the reaction time is usually about 0.5 to 5 hours. The modified lignin-containing resin composition may further contain one or more selected from the group consisting of thermosetting resins and aldehydes.

[0047] (Filler) The modified lignin-containing resin composition may further contain a filler, which may be an inorganic filler or an organic filler. Examples of inorganic fillers include spherical or crushed fused silica, silica powder such as crystalline silica, alumina powder, glass powder, glass fiber, glass flake, mica, talc, calcium carbonate, alumina, hydrated alumina, boron nitride, aluminum nitride, silicon nitride, silicon carbide, titanium nitride, zinc oxide, tungsten carbide, magnesium oxide, and the like. Examples of organic fillers include carbon fiber, aramid fiber, paper powder, wood powder, cellulose fiber, cellulose powder, rice husk powder, fruit shell / nut powder, chitin powder, and starch.

[0048] The inorganic filler and the organic filler may be used alone or in combination of two or more, and the content is determined according to the purpose. When the inorganic filler and / or the organic filler are contained, it is desirable that the content of the inorganic filler and / or the organic filler is appropriate in order to obtain good physical properties and moldability. From this viewpoint, the content of the inorganic filler and / or the organic filler is preferably 50 to 200 parts by mass, more preferably 80 to 150 parts by mass, based on 100 parts by mass of the modified lignin.

[0049] (hardening agent) The modified lignin-containing resin composition may further contain a curing agent. Examples of the curing agent include hexamethylenetetramine, hexaformaldehyde, paraformaldehyde, etc. These may be used alone or in combination of two or more kinds. In addition to the curing agent, in order to further increase the curing speed and degree of curing, inorganic bases such as calcium hydroxide, sodium hydroxide, potassium hydroxide, calcium oxide, and magnesium oxide, Lewis acids such as zinc chloride and zinc acetate, and catalysts such as triethylamine may be used. These may be used alone or in combination of two or more.

[0050] (Other additives) Various additives can be added to the resin composition material according to the present embodiment within the range that does not impair the properties of the molded product obtained from the resin composition material. In addition, a compatibilizer, a surfactant, etc. can be further added depending on the purpose. As the compatibilizer, a resin obtained by adding maleic anhydride or epoxy to a thermoplastic resin to introduce a polar group, such as a maleic anhydride-modified polyethylene resin or a maleic anhydride-modified polypropylene resin, or various commercially available compatibilizers may be used in combination. Examples of surfactants include, but are not limited to, straight-chain fatty acids such as stearic acid, palmitic acid, and oleic acid, and branched or cyclic fatty acids with rosins. In addition to the above, other additives that can be added include flexibilizers, heat stabilizers, ultraviolet absorbers, flame retardants, antistatic agents, antifoaming agents, thixotropic agents, release agents, antioxidants, plasticizers, stress reducing agents, coupling agents, dyes, light scattering agents, small amounts of thermoplastic resins, etc. These may be used alone or in combination of two or more.

[0051] (thermoplastic resin) The thermoplastic resin that can be blended in the modified lignin-containing resin composition is preferably an amorphous thermoplastic resin having a glass transition temperature of 200°C or less, or a crystalline thermoplastic resin having a melting point of 200°C or less. Examples of thermoplastic resins include polycarbonate resins, styrene resins, polystyrene elastomers, polyethylene resins, polypropylene resins, polyacrylic resins (polymethyl methacrylate resin, etc.), polyvinyl chloride resins, cellulose acetate resins, polyamide resins, low-melting-point polyester resins (PET, PBT, etc.) typified by polyesters formed from combinations of terephthalic acid and ethylene glycol, and terephthalic acid and 1,4-butanediol, polylactic acid and / or copolymers containing polylactic acid, acrylonitrile-butadiene-styrene resins (ABS resins), polyphenylene oxide resins (PPO), polyketone resins, polysulfone resins, polyphenylene sulfide resins (PPS), fluororesins, silicone resins, polyimide resins, polybenzimidazole resins, polyamide elastomers, and copolymers of these with other monomers.

[0052] When using modified lignin as an additive for a thermoplastic resin, for example, a conventionally known method such as those described in JP 2014-15579 A, ​​WO 2016 / 104634 A, etc. can be used. From the viewpoint of obtaining remarkable fluidity and strength, the content of the thermoplastic resin in the modified lignin resin composition material is preferably 30% by mass or more and 99.9% by mass or less, more preferably 40% by mass or more and 99.9% by mass or less, even more preferably 45% by mass or more and 99.9% by mass or less, and particularly preferably 50% by mass or more and 99.9% by mass or less, based on the total amount of the resin composition material. The modified lignin-containing resin composition material may contain, in addition to the above-mentioned cellulose-containing solid matter and thermoplastic resin, a resin compatible with the thermoplastic resin composition material, an additive, and a filler.

[0053] (Mixing and molding) The blending and kneading of each component used in the modified lignin-containing resin composition material can be carried out by premixing using commonly used equipment such as a ribbon blender, drum tumbler, etc., and then using a Henschel mixer, Banbury mixer, single screw extruder, twin screw extruder, multi-screw extruder, roll kneader, co-kneader, etc. The heating temperature during kneading is usually appropriately selected in the range of 100 to 300 ° C. The method for molding the modified lignin-containing resin composition is not particularly limited. For example, press molding, injection molding, transfer molding, medium-sized molding, FRP molding, etc. can be mentioned. In addition, when the resin composition is a thermoplastic resin composition, the method for molding into a predetermined shape can be extrusion molding, injection molding, etc.

[0054] Examples of molded products using modified lignin-containing resin compositions include those obtained by curing resin compositions containing modified lignin and a curing agent, those further containing various fillers or industrially obtained general phenolic resins as necessary, and molding them into a predetermined shape and then curing them, or those molded after curing, and those molded resin compositions obtained by mixing modified lignin with a thermoplastic resin, etc. Examples of molded products using such modified lignin-containing resin compositions include, for example, insulation materials for housing, electronic parts, resins for frac sand, resins for coated sand, resins for impregnation, resins for lamination, resins for FRP molding, automobile parts, reinforcing materials for automobile tires, office automation equipment, machinery, information and communication equipment, industrial materials, etc.

[0055] Modified lignin can be used for modified lignin-containing materials other than resin composition materials. Examples of modified lignin-containing materials other than modified lignin-containing resin composition materials include carbon materials such as carbon black and carbon fiber, lubricants such as grease base materials, foods and cosmetics with antioxidant and antibacterial properties, cement additives, concrete additives, binders, rubber compositions, packaging materials such as gas barrier films, agricultural materials such as plant activators and soil conditioners, inks and toners, adhesives, surfactants, ultraviolet absorbers, storage battery electrode materials, growth promoters for marine organisms, and food discoloration inhibitors. EXAMPLES

[0056] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to these.

[0057] The modified lignins and raw lignins obtained in the examples were subjected to various measurements by the following methods. <Molecular weight measurement> The number average molecular weight (Mn), weight average molecular weight (Mw), and molecular weight distribution (Mw / Mn) of the modified lignins obtained in each example and the raw lignins 1 and 2 were determined in terms of standard polystyrene molecular weight by GPC (gel permeation chromatography). Note that since raw lignin 2 does not dissolve completely in tetrahydrofuran, only the soluble portion was measured. The measurement apparatus and conditions are as follows. Separation column: 2 columns of TSKgel SuperMultiporeHZ-M manufactured by Tosoh Corporation Eluent: Tetrahydrofuran ·Eluent flow rate: 1.0mL / min Detector: Index of Refraction (RI) ·Measurement temperature: 40℃

[0058] <Relative abundance rate (%) of basic skeleton and hydroxyl group ratio (%)> (1) A solvent mixture of deuterated chloroform, pyridine, and cyclohexanol (internal standard) was added to the modified lignin obtained in each Example or raw lignin 1 or 2, and 2-chloro-4,4,5,5-tetramethyl-1,3,2-dioxaphospholane was further added as a derivatization reagent, followed by heating at 50°C for 1 hour. Note that raw lignin 2 was not completely soluble in tetrahydrofuran, so only the soluble portion was measured. Then, the following measurement conditions were used: 31 P-NMR measurements were carried out. Pulse width: 30° Repeat time: 2 seconds Measurement range: -60~200ppm -Number of times: 200 The signal derived from cyclohexanol, the internal standard, was set at 145.2 ppm, 144.0 to 142.0 ppm was identified as the S-type skeleton, and 141.0 to 136.6 ppm was identified as the G-type skeleton, and the relative abundance percentage of each basic skeleton was calculated from the integral value. The relative abundance percentage of the H-type skeleton was calculated by subtracting the relative abundance percentages of the S-type skeleton and the G-type skeleton from the total amount of aromatic hydroxyl groups. Furthermore, 150.0 to 145.5 ppm was identified as aliphatic hydroxyl groups, and 144.7 to 136.6 ppm as aromatic hydroxyl groups. The amount of aliphatic hydroxyl groups (mol / g) and the amount of aromatic hydroxyl groups (mol / g) were calculated from the integral curve to determine the percentage of each hydroxyl group. (2) Abundance ratio and reaction point Based on the relative abundance percentage of each basic skeleton above, The ratio of the sum of twice the relative abundance of the H-type skeleton H (%) and the relative abundance of the G-type skeleton G (%) to the relative abundance of the S-type skeleton S (%) [(2H+G) / S], The sum of reaction sites based on the relative abundance of H-type skeletons (H) (%) and the relative abundance of G-type skeletons (G) (2H+G), · Increase rate (%) of [2H+G] before and after modification was calculated.

[0059] <Softening point (℃)> The modified lignin or raw lignin 1 or 2 (solid sample) obtained in each example was crushed in a mortar, sieved (40 mesh) to remove large particles, and the crushed sample was placed in an aluminum cup (circular upper φ60, lower φ53 × depth 15 mm) of 10 to 20 mg. The aluminum cup containing the sample was placed on a hot plate (ASONEND-2A) and covered with a glass plate (thickness 0.5 mm). After heating to 80 ° C, the temperature was increased in 10 ° C increments, and visual observation was made through the glass, and the temperature at which it melted visually was adopted as the softening point.

[0060] <Raw material lignin 1> 500 g of bagasse (dried sugarcane residue) was heat treated at 200°C for 4 hours in the presence of 2.1 L of 1-butanol and 3.3 L of water, and the 1-butanol layer was extracted. The extracted 1-butanol layer was filtered (Whatman No. 2 filter paper) to remove cellulose-containing solids. The filtrate was concentrated and dried to obtain 90 g of raw lignin 1.

[0061] <Modified lignin> [Example 1] (1) Reaction process 100 parts by mass (100.0 g) of raw material lignin 1, 100 parts by mass of phenol, and 1 part by mass of phosphoric acid were placed in a 1.0 L pressure-resistant container capable of stirring and heated. When the phenol was dissolved, stirring was started. Heating was continued at 200°C for 4 hours. (2) Purification process Distillative removal of phenol: The reaction liquid was removed from the pressure vessel and the reaction liquid was distilled under reduced pressure (5-10 kPa) and heated (100-130°C) using a Kugelrohr to remove phenol. The phenol after the reaction could not be completely removed using the Kugelrohr, and about 10% by mass of the modified lignin remained. Modified lignin reprecipitation: Two parts by mass of acetone were added to 1 part by mass (5.0 g) of the modified lignin from which the phenol had been distilled off, and the lignin was completely dissolved. 40 parts by mass of ion-exchanged water was added to the mixture to precipitate the modified lignin. The precipitated modified lignin was collected by centrifugation. This procedure was repeated 3 to 4 times to completely remove the phenol after the reaction, and modified lignin 1 (4.5 g) was obtained.

[0062] [Example 2] The same procedure as in Example 1 was carried out except that no acid catalyst was used, to obtain modified lignin 2 (4.5 g). [Example 3] The same procedure as in Example 1 was carried out except that the amount of raw lignin 1 was 19 parts by mass and the amount of phenol was 181 parts by mass, to obtain modified lignin 3 (4.4 g). [Example 4] The same procedure as in Example 3 was repeated except that the reaction time was changed to 8 hours, to obtain modified lignin 4 (4.5 g). [Example 5] The same procedure as in Example 3 was carried out except that the reaction temperature was changed to 220° C., and modified lignin 5 (4.5 g) was obtained. [Example 6] The same procedure as in Example 3 was carried out except that the amount of catalyst was changed to 5 parts by mass, and modified lignin 6 (4.4 g) was obtained. [Example 7] The same procedure as in Example 3 was repeated except that m-cresol was used instead of phenol, to obtain modified lignin 7 (4.5 g). [Example 8] The same procedure as in Example 1 was carried out except that the amount of raw lignin 1 was 61 parts by mass and the amount of phenol was 139 parts by mass, to obtain modified lignin 8 (4.6 g). [Example 9] The same procedure as in Example 8 was carried out except that no acid catalyst was used, to obtain modified lignin 9 (4.5 g). [Example 10] The same procedure as in Example 1 was carried out except that the reaction temperature was 150° C. and the reaction time was 1 hour, to obtain modified lignin 10 (4.4 g). [Example 11] The same procedure as in Example 10 was carried out except that the acid catalyst was changed to sulfuric acid, to obtain modified lignin 11 (4.6 g). [Example 12] The same procedure as in Example 3 was carried out except that the acid catalyst was changed to 0.2 parts by mass of sulfuric acid, and modified lignin 12 (4.5 g) was obtained.

[0063] The properties of the modified lignins 1 to 12 obtained in the above Examples 1 to 12 and the raw lignin 1 are shown in Table 1.

[0064] [Table 1]

[0065] <Cured product> Next, the modified lignins obtained in Examples 1 to 12 or the raw lignin 1 were used to produce resin composition materials and molded articles using the same in the following Examples and Comparative Examples. The resin composition and the molded article were evaluated by the following methods. (Easy to mix) In Examples 13 to 24 and Comparative Example 1, the ease of kneading was evaluated based on the following index. ○: Easy to knead △: Difficult but possible to knead ×: Unable to knead

[0066] (stirrability) In Examples 25 to 36 and Comparative Example 2, the ease of stirring during the reaction was evaluated based on the following index. ○: Easy to stir △: Difficult but possible to mix ×: Stirring not possible

[0067] (Bending strength) Samples of 5 mm x 50 mm x 1 mm were cut out from the molded bodies obtained in each of the Examples and Comparative Examples, and the bending strength was measured using an Instron 5566 manufactured by Instron Japan under conditions of a three-point bending mode, a span of 30 mm, and a speed of 2 mm / min, and evaluated based on the index. ○: The sample was not easily broken. △: The sample was broken. ×: The sample broke immediately. -:Poor molding

[0068] [Examples 13 to 24] 100 parts by mass of novolac-type phenolic resin (PR-53195, manufactured by Sumitomo Bakelite Co., Ltd.), 50 parts by mass of wood flour, 50 parts by mass (50.0 g) of each of the modified lignins 1 to 12 obtained in Examples 1 to 12 above, 20 parts by mass of hexamethylenetetramine as a curing agent, and 1 part by mass of zinc stearate as an internal release agent were mixed and kneaded in a two-roll kneader at 100 to 110°C for 3 minutes to obtain a modified lignin-containing resin composition material. The modified lignin-containing resin composition material obtained above was pressed into a heated mold cavity and molded by transfer molding at 170°C for 5 minutes, and then cured in an oven at 180°C for 8 hours to obtain a molded product. The results of the evaluation of the resin composition and the molded article are shown in Table 2.

[0069] [Comparative Example 1] A resin composition material and a molded body were obtained in the same manner as in Example 13, except that raw lignin 1 was used instead of the modified lignin. The evaluation results of the resin composition material and the molded product are shown in Table 2 (Table 2-1 or Table 2-2).

[0070] [Table 2]

[0071] [Examples 25 to 36] In a 0.5 L separable flask equipped with a reflux device and a stirring blade, 50 parts by mass (50.0 g) of each of the modified lignins 1 to 12 obtained in Examples 1 to 12 above and 30 parts by mass of a 40% by mass aqueous formaldehyde solution were added and stirred. The molar ratio of formaldehyde to phenol in the modified lignin was 1.5. While gradually dropping 35 parts by mass of a 50% by mass aqueous sodium carbonate solution, the mixture was heated at 100°C for 2 hours to obtain a liquid composition. Furthermore, 54 parts by mass of wood flour was added and stirred until homogenous, to obtain a modified lignin-containing resin composition material. The modified lignin-containing resin composition material obtained above was decompressed to remove moisture, and press-molded at a surface pressure of 0.2 MPa, 180° C., and 10 minutes, and then cured in an oven at 200° C. for 4 hours to obtain a molded product. The results of the evaluation of the resin composition and the molded article are shown in Table 3.

[0072] [Comparative Example 2] A molded body was obtained in the same manner as in Example 25, except that raw lignin 1 was used instead of the modified lignin. The results of the evaluation of the resin composition material and the molded article are shown in Table 3 (Table 3-1 or Table 3-2).

[0073] [Table 3]

[0074] From Tables 2 and 3, it can be seen that the modified lignins 1 to 12 have improved mixability because they are easier to knead and have better stirrability during reaction than the raw lignin 1. It can also be seen that the bending properties of the molded bodies made using the modified lignins are better than those of the raw lignin 1.

[0075] <Raw material lignin 2> As the raw material lignin 2, kraft lignin (Lignin, alkali (product number 370959) manufactured by SIGMA-ALDRICH) was used. <Modified lignin> [Example 37] The same procedure as in Example 5 was carried out except that the raw material lignin 2 was 40 parts by mass, the phenol was 160 parts by mass, the acid catalyst was 0.4 parts by mass of sulfuric acid, and the reaction time was 2 hours, to obtain modified lignin 13 (4.3 g).

[0076] [Example 38] The same procedure as in Example 37 was carried out except that no acid catalyst was used and the reaction temperature was 300° C., to obtain modified lignin 14 (4.5 g).

[0077] The properties of modified lignins 13 and 14 obtained in Examples 37 and 38 above, and raw lignin 2 are shown in Table 4.

[0078] [Table 4]

[0079] <Cured product> Next, using the modified lignin 13 obtained in Example 37 or the raw lignin 2, the resin composition materials and molded bodies in the following Examples and Comparative Examples were evaluated for ease of kneading, stirrability, and bending strength by the methods described above.

[0080] [Example 39] The procedure of Example 13 was repeated except that Modified Lignin 13 was used to obtain a resin composition material and a molded product. The results of the evaluation of the resin composition and the molded article are shown in Table 5. [Comparative Example 3] A resin composition material and a molded body were obtained in the same manner as in Example 13, except that raw lignin 2 was used instead of the modified lignin. The results of the evaluation of the resin composition and the molded article are shown in Table 5.

[0081] [Table 5]

[0082] [Example 40] The same procedure as in Example 25 was carried out except that Modified Lignin 13 was used, to obtain a resin composition material and a molded body. The results of the evaluation of the resin composition and the molded article are shown in Table 6. [Comparative Example 4] A resin composition material and a molded body were obtained in the same manner as in Example 25, except that raw lignin 2 was used instead of the modified lignin. The results of the evaluation of the resin composition and the molded article are shown in Table 6.

[0083] [Table 6]

[0084] From Tables 5 and 6, it can be seen that the mixability of Modified Lignin 13 is improved because it is easier to knead and has better stirrability during reaction than Raw Lignin 2. It can also be seen that the bending properties of the molded body using the modified lignin are better than those of the raw lignin 2. [Industrial Applicability]

[0085] The modified lignin of the present invention has a lower molecular weight, which improves its mixability with other plastic materials and increases the number of reaction sites. The improved mixability and increased reaction sites are expected to improve the physical properties of molded products, and the ease of mixing makes it possible to eliminate the need for large-scale equipment that is costly when producing hardened parts. In addition, since lignin, which has been almost entirely discarded until now, can be effectively utilized, it is also effective in protecting the environment.

Claims

1. A method for producing modified lignin, comprising the step of reacting a raw lignin separated from plant biomass by at least one method selected from an organosolv method, a hot compressed water method, a steam explosion method, an ammonia treatment method, an ammonia explosion method, an acid treatment method, an alkali treatment method, an oxidative decomposition method, a thermal decomposition method, and a microwave heating method with a phenol compound having a hydrogen atom at at least one of the 2-position, 4-position, and 6-position, which are the positions of the substituents relative to the hydroxyl group, at a temperature higher than 140° C. and not higher than 350° C. The modified lignin produced is 31 the ratio [(2H+G) / S] of the sum of twice the relative abundance H(%) of the H-type skeleton to the relative abundance S(%) of the S-type skeleton determined from the integral value measured by P-NMR and the relative abundance G(%) of the G-type skeleton is 2.5 or more; The modified lignin produced is 31 A method for producing modified lignin, in which the proportion of aliphatic hydroxyl groups relative to the total proportion of aliphatic hydroxyl groups and aromatic hydroxyl groups, as determined from an integrated value measured by P-NMR, is less than 20%.

2. The method for producing modified lignin according to claim 1, wherein the phenol compound is represented by the following formula (1): [Formula 1] (In formula (1), R 1 and R 2 each independently represents a hydrogen atom, a hydroxyl group, or an alkyl group having 1 to 15 carbon atoms; R 1 and R 2 may be the same or different.)

3. The method for producing modified lignin according to claim 1 or 2, wherein the reaction is carried out without a catalyst or in the presence of more than 0 to 3.0 mass% of an acid catalyst relative to the total amount of the raw lignin and the phenol compound.

4. The method for producing modified lignin according to claim 1 or 2, wherein the reaction is carried out without a catalyst or in the presence of 0.2 to 3.0 mass% of an acid catalyst based on the total amount of the raw lignin and the phenol compound.

5. The method for producing modified lignin according to claim 1 or 2, wherein the reaction is carried out without a catalyst.

6. The method for producing modified lignin according to any one of claims 1 to 5, wherein the mass ratio of the phenol compound to the raw lignin [phenol compound / raw lignin] is 1 to 15.

7. The method for producing modified lignin according to any one of claims 1 to 6, wherein the reaction is carried out at a reaction temperature of more than 140 ° C. and not more than 250 ° C.

8. The method for producing modified lignin according to any one of claims 1 to 7, wherein the modified lignin has a smaller number average molecular weight and weight average molecular weight than the raw lignin.

9. 31 The method for producing modified lignin according to any one of claims 1 to 8, wherein the sum of reaction sites [2H + G] based on the relative abundance H (%) of H-type skeletons and the relative abundance H (%) of G-type skeletons determined from the integral value measured by P-NMR increases by 4% or more before and after modification.

10. The method for producing modified lignin according to any one of claims 1 to 9, wherein the softening point of the modified lignin produced is 90 ° C. or higher.

11. The method for producing modified lignin according to any one of claims 1 to 10, wherein the softening point of the modified lignin produced is 130 ° C. or higher.

12. The method for producing modified lignin according to any one of claims 1 to 11, wherein the ratio of relative abundance rates [(2H + G) / S] is 2.8 or more.

13. 31 The method for producing modified lignin according to any one of claims 1 to 12, wherein the abundance rate of aliphatic hydroxyl groups relative to the total abundance rate of aliphatic hydroxyl groups and aromatic hydroxyl groups determined from an integral value measured by P-NMR is less than 15%.

Citation Information

Patent Citations

  • Excitation control system

    JP1981071430A

  • Lignin-modified novolac type phenolic resin, method of producing the same, and phenolic resin molding material

    JP2008156601A

  • Lignin derivative and secondary derivative thereof

    JP2009084320A

  • Friction material

    JP2013199561A

  • Method for increasing the reactivity of lignin

    JP2016540058A