CATALYST FOR PRODUCING CARBOXYLIC ACID ESTER AND METHOD FOR PRODUCING CARBOXYLIC ACID ESTER

Catalysts with controlled pore size distribution and silica-alumina support enhance durability and stability, addressing pH and temperature issues in carboxylic ester production.

JP7573627B2Active Publication Date: 2024-10-25ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2022546830
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-04
Publication Date
2024-10-25
Estimated Expiration
2040-09-04

AI Technical Summary

Technical Problem

Existing catalysts for producing carboxylic esters suffer from decreased activity and selectivity due to pH swings and temperature fluctuations during long-term use, leading to reduced durability.

Method used

The catalysts are designed with a narrow pore size distribution and specific pore structure, using nickel, cobalt, or their oxidized forms supported on a carrier with a silica-alumina composition, to enhance pH swing resistance and temperature stability.

Benefits of technology

The catalysts exhibit improved durability and maintain high activity and selectivity over extended periods by suppressing pore diameter variations and stabilizing the carrier structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573627000004
    Figure 0007573627000004
  • Figure 0007573627000005
    Figure 0007573627000005
  • Figure 0007573627000006
    Figure 0007573627000006
Patent Text Reader

Abstract

A carboxylate ester production catalyst comprising: catalyst particles including at least one element selected from the group consisting of nickel, cobalt, palladium, lead, platinum, ruthenium, gold, silver, and copper; and a carrier that holds the catalyst particles, wherein the half width Wa of a fine-pore distribution of the carboxylate ester production catalyst calculated using a BJH method from an adsorption isotherm obtained from a nitrogen adsorption method is 10 nm or less.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst for producing a carboxylic acid ester and a method for producing a carboxylic acid ester. [Background technology]

[0002] Nickel or nickel compounds are widely used as catalysts for chemical synthesis such as oxidation reactions, reduction reactions, and hydrogenation reactions, and in recent years, various modifications and improvements of nickel-based catalysts have been made to realize catalytic oxygen oxidation reactions of alcohols. However, in the chemical industry, nickel and nickel compounds are known to be effective not only in alcohol oxidation reactions, but also in a wide range of reactions such as various oxidation reactions, reduction reactions, and hydrogenation reactions, as well as in catalysts for purifying automobile exhaust gases and photocatalysts.

[0003] For example, Patent Document 1 proposes a method for producing a carboxylate ester, which uses a composite particle support comprising a composite particle composed of oxidized nickel and X (X represents at least one element selected from the group consisting of nickel, palladium, platinum, ruthenium, gold, silver, and copper) and a support supporting the composite particle, the composite particle support having a support layer in which the composite particle is localized, as a catalyst. It is said that such a catalyst can maintain high reactivity for a long period of time. In addition, Patent Document 1 discloses that the pore structure of a support applicable to such a catalyst can be adjusted by performing a predetermined aging. Similarly, Patent Document 2 discloses that a support having a uniform pore structure in which the pore diameter of most of the pores is in a narrow range of 3 to 5 nm can be obtained by performing a predetermined hydrothermal treatment. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 4803767 [Patent Document 2] Patent No. 5794993 Summary of the Invention [Problem to be solved by the invention]

[0005] In the production of carboxylic acid esters using the catalysts described in Patent Documents 1 and 2, methacrylic acid is generated as a by-product, so that the pH decreases during the reaction, and as a result, the activity of the catalyst tends to decrease. In consideration of such a tendency, it is conceivable to control the pH of the reaction system to a predetermined range, for example, by adding a basic substance, but it is also assumed that the addition of the basic substance will locally increase the pH in the reaction system. In consideration of long-term use in the reaction system as described above, on the scale of several years, the catalyst is required to have improved acid resistance and base resistance (hereinafter also referred to as "pH swing resistance") due to the up-and-down behavior of the pH (hereinafter also referred to as "pH swing"). In addition, although the production of carboxylic acid esters can be carried out at relatively low temperatures, when long-term use over several years is taken into consideration, the activity and selectivity of the catalyst may decrease when exposed to relatively high temperature conditions, and therefore temperature resistance is also required. As described above, assuming long-term use of a catalyst over several years, it is desirable to improve durability (hereinafter simply referred to as "durability") while also taking into consideration pH swing resistance and / or temperature resistance. However, the techniques described in Patent Documents 1 and 2 still have room for improvement in terms of durability.

[0006] The present invention has been made in consideration of the problems associated with the conventional techniques described above, and an object of the present invention is to provide a catalyst for producing a carboxylic acid ester, which has excellent durability in anticipation of long-term use. [Means for solving the problem]

[0007] As a result of investigations, the present inventors have found that durability in anticipation of long-term use can be improved by setting the half-width of the pore size distribution of a catalyst for producing a carboxylic acid ester, measured by a predetermined method, within a predetermined range and suppressing the variation in pore size inside the pores of the support, and have thus completed the present invention.

[0008] That is, the present invention includes the following aspects. [1] Catalyst particles containing at least one element selected from the group consisting of nickel, cobalt, palladium, lead, platinum, ruthenium, gold, silver, and copper; A carrier that supports the catalyst particles; A catalyst for producing a carboxylic acid ester, comprising: The catalyst for producing a carboxylic acid ester has a half-width (Wa) of a pore distribution of 10 nm or less, the half-width (Wa) of the pore distribution being calculated by the BJH method from an adsorption isotherm obtained by a nitrogen adsorption method. [2] The catalyst for producing a carboxylic acid ester according to [1], wherein a half-width Wd of a pore distribution calculated by the BJH method from a desorption isotherm obtained by a nitrogen adsorption method for the catalyst for producing a carboxylic acid ester is 5 nm or less. [3] The catalyst for producing a carboxylic acid ester according to [1] or [2], wherein a mode diameter Da of pores of the catalyst for producing a carboxylic acid ester, calculated by using the BJH method from an adsorption isotherm obtained by a nitrogen adsorption method, is 2 nm or more and 20 nm or less. [4] The catalyst for producing a carboxylic acid ester according to any one of [1] to [3], wherein a mode diameter Da of pores and the half width Wa of pores calculated by the BJH method from an adsorption isotherm obtained by a nitrogen adsorption method for the catalyst for producing a carboxylic acid ester satisfy the relationship of the following formula (1): 1 / 2Wa < Da (1) [5] The catalyst for producing a carboxylic acid ester according to any one of [1] to [4], wherein a mode diameter Dd of pores of the catalyst for producing a carboxylic acid ester, calculated by using the BJH method from a desorption isotherm obtained by a nitrogen adsorption method, is 2 nm or more and 15 nm or less. [6] The catalyst for producing a carboxylic acid ester according to any one of [1] to [5], wherein a pore mode diameter Dd calculated by the BJH method from a desorption isotherm of the catalyst for producing a carboxylic acid ester obtained by a nitrogen adsorption method, and a half-width Wd of a pore distribution calculated by the BJH method from a desorption isotherm of the catalyst for producing a carboxylic acid ester obtained by a nitrogen adsorption method, satisfy the relationship of the following formula (2): 1 / 2Wd < Dd (2) [7] The catalyst for producing a carboxylic acid ester according to any one of [1] to [6], wherein the half width Wa is 0.1 nm or more. [8] The catalyst for producing a carboxylic acid ester according to any one of [1] to [7], wherein the catalyst particles contain at least one element selected from the group consisting of nickel, cobalt, palladium, lead and gold. [9] The catalyst for producing a carboxylic acid ester according to any one of [1] to [8], wherein the catalyst particles are composite particles containing oxidized nickel and / or cobalt, and X (X represents at least one element selected from the group consisting of nickel, palladium, platinum, ruthenium, gold, silver, and copper).

[10] The catalyst for use in producing a carboxylic acid ester according to [9], wherein a composition ratio of nickel or cobalt to X in the composite particle is 0.1 or more and 10 or less, expressed as a Ni / X atomic ratio or a Co / X atomic ratio.

[11] The catalyst for producing a carboxylic acid ester according to [9], wherein the composite particle contains oxidized nickel and gold.

[12] The catalyst for use in producing a carboxylic acid ester according to

[10] , wherein a composition ratio of nickel to gold in the composite particle is 1.1 or more and 10 or less in terms of an Ni / Au atomic ratio.

[13] The catalyst for producing a carboxylic acid ester according to any one of [1] to

[12] , wherein the catalyst particles have an average particle size of 2 nm or more and 10 nm or less.

[14] The catalyst for use in the production of a carboxylic acid ester according to any one of [1] to

[13] , wherein the support is made of an aluminum-containing silica-based composition that contains silica and alumina.

[15] The carrier is Silicon, Aluminum and At least one Period 4 element selected from the group consisting of iron, cobalt, nickel, and zinc; at least one basic element selected from the group consisting of alkali metal elements, alkaline earth metal elements, and rare earth elements; in the ranges of 42 mol % or more and 90 mol % or less, 3 mol % or more and 38 mol % or less, 0.5 mol % or more and 2 mol % or more and 38 mol % or less, respectively, relative to the total molar amount of the silicon, the aluminum, the fourth periodic element, and the basic element.

[16] The catalyst for producing a carboxylic acid ester according to any one of [1] to

[15] , wherein the support layer in which the catalyst particles are localized is present in an area ranging from a surface of the catalyst for producing a carboxylic acid ester to 40% of an equivalent diameter of the catalyst for producing a carboxylic acid ester.

[17] The catalyst for producing a carboxylic acid ester according to any one of [1] to

[16] , wherein the equivalent diameter of the catalyst for producing a carboxylic acid ester is 200 μm or less, and the support layer in which the catalyst particles are localized is present in an area ranging from a surface of the catalyst for producing a carboxylic acid ester to 30% of the equivalent diameter of the catalyst for producing a carboxylic acid ester.

[18] The catalyst for producing a carboxylic acid ester according to any one of [1] to

[17] , further comprising an outer layer substantially free of catalyst particles outside the support layer in which the catalyst particles are localized, the outer layer having a thickness of 0.01 μm or more and 15 μm or less.

[19] The catalyst for producing a carboxylic acid ester according to any one of [9] to

[18] , wherein the catalyst particle has a core made of X, and the core is coated with oxidized nickel and / or cobalt.

[20] A method for producing a carboxylic acid ester, comprising a reaction step of reacting (a) an aldehyde with an alcohol, or (b) one or more alcohols, in the presence of the catalyst for producing a carboxylic acid ester according to any one of [1] to

[19] and oxygen. [twenty one] The method for producing a carboxylic acid ester according to

[20] , wherein the aldehyde is acrolein and / or methacrolein. [twenty two] The method for producing a carboxylic acid ester according to

[20] or

[21] , wherein the aldehyde is acrolein and / or methacrolein, and the alcohol is methanol. [twenty three] The method for producing a carboxylic acid ester according to any one of

[20] to

[22] , wherein the reaction step is carried out in a liquid phase. [twenty four] The method for producing a carboxylic acid ester according to any one of

[20] to

[23] , wherein the reaction step is carried out while adding a basic substance so that the pH of the reaction system is 6 or more and 8 or less. Effect of the Invention

[0009] According to the present invention, it is possible to provide a catalyst for producing a carboxylic acid ester, which has excellent durability intended for long-term use. [Brief description of the drawings]

[0010] [Figure 1] FIG. 1 is a schematic cross-sectional view showing a typical example of a pore structure of a catalyst for producing a carboxylic acid ester according to one embodiment of the present invention. [Diagram 2] FIG. 1 is a schematic cross-sectional view showing a typical example of a pore structure of a conventional catalyst. [Diagram 3] FIG. 1 is a conceptual diagram showing how to determine a half-value width. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, an embodiment of the present invention (hereinafter, also referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be practiced with various modifications within the scope of the gist of the present invention.

[0012] [Catalyst for producing carboxylic acid esters] The catalyst for producing a carboxylate ester of this embodiment is a catalyst for producing a carboxylate ester, comprising catalyst particles containing at least one element selected from the group consisting of nickel, cobalt, palladium, lead, platinum, ruthenium, gold, silver and copper, and a carrier supporting the catalyst particles, and the half-width Wa of the pore distribution of the catalyst for producing a carboxylate ester, calculated using the BJH method from an adsorption isotherm obtained by a nitrogen adsorption method, is 10 nm or less. Because of this configuration, the catalyst for producing a carboxylate ester of this embodiment is excellent in durability assuming long-term use. More specifically, the catalyst for producing a carboxylate ester of this embodiment is excellent in, for example, pH swing resistance and / or temperature resistance.

[0013] The pore structure of the catalyst for producing a carboxylate ester of this embodiment can be said to be derived from the pores of the carrier. In this embodiment, the pore structure is specified by the half-width of the pore distribution (hereinafter, simply referred to as "half-width Wa") calculated from the adsorption isotherm obtained by the nitrogen adsorption method using the BJH (Barrett, Joyner and Halenda) method. There are two possible methods for calculating the pore distribution by the BJH method: a method of calculating the pore distribution (pore distribution on the adsorption side) by obtaining an adsorption isotherm, and a method of calculating the pore distribution (pore distribution on the desorption side) by obtaining a desorption isotherm. The latter method obtains an evaluation result that appropriately reflects the pore diameter near the entrance of the pore, but the variation in pore diameter inside the pore is not accurately reflected in the evaluation result. In contrast, the former method obtains an evaluation result (true distribution) that reflects the variation from the entrance of the pore to the inside, and therefore can be said to be an appropriate evaluation index for obtaining a carrier that is uniform from the entrance of the pore to the inside. In the present embodiment, the former method is adopted to specify the pore structure, and the half-width Wa of the pore distribution is adjusted to 10 nm or less, resulting in a catalyst for producing a carboxylic acid ester having a uniform structure from the entrance of the pore to the inside (for example, in the cross-sectional schematic diagram shown in FIG. 1, the diameters L1, L2, and L3 inside the pores are each uniform values). On the other hand, when the half-width Wa exceeds 10 nm, even if the pore diameter near the pore entrance is uniform, the pore diameter inside the pore varies (for example, in the cross-sectional schematic diagram shown in FIG. 2, the diameters L4, L5, and L6 inside the pore each have varying values), and changes in the pore structure due to long-term use become apparent, making it difficult to maintain catalytic performance for a sufficiently long period of time. From the above viewpoints, the half width Wa is 10 nm or less, preferably 8 nm or less, more preferably 7 nm or less, and further preferably 5 nm or less. The lower limit of the half-width Wa is not particularly limited, but may be, for example, 0.1 nm or more, 1 nm or more, or 3 nm or more. The value of the half width Wa is measured by the method described in the examples described later. The method for adjusting the half-width Wa is not particularly limited, but for example, the half-width Wa of the catalyst for producing a carboxylate ester can be sufficiently small by adopting a preferred production method described later. More specifically, it is considered that the size of the silica chain is easily uniformed by preparing the slurry by adopting preferred conditions in the production method described later. That is, the uniformity of the pore size of silica depends on the size of the silica chain of the carrier slurry, and if the size of the silica chain is uniform, the size of the pore size is easily uniform. As a result, the uniform size of the silica chain makes it easy for the inner wall constituting the pore to become dense, and even when subjected to a pH swing, the expansion of the pore size of silica is suppressed, and the pH swing resistance is improved. However, the above is merely one possible factor for obtaining the above structure in the catalyst for producing a carboxylate ester of this embodiment, and the action mechanism of this embodiment is not limited thereto.

[0014] In this embodiment, when the pore diameter near the inlet of the pores of the support is also uniform, the durability of the catalyst for long-term use is improved more than when only the inside is made uniform, and as a result, the conversion rate tends to be improved. From the above viewpoints, the half-width (hereinafter also simply referred to as "half-width Wd") of the pore distribution of the catalyst for producing a carboxylic acid ester, calculated by the BJH method from the desorption isotherm obtained by the nitrogen adsorption method, is preferably 5 nm or less, more preferably 4 nm or less, and even more preferably 3 nm or less. The lower limit of the half-width Wd is not particularly limited, but may be, for example, 0.1 nm or more, 1 nm or more, or 2 nm or more. The value of the half width Wd is measured by the method described in the examples described later. The method for adjusting the half-value width Wd is not particularly limited. For example, the half-value width Wd of the catalyst for producing a carboxylic acid ester can be adjusted to the above range by employing a preferable production method described later.

[0015] In this embodiment, the mode diameter Da of the pores calculated by the BJH method from the adsorption isotherm obtained by the nitrogen adsorption method of the catalyst for producing a carboxylic acid ester is derived from the pore structure of the support, and is preferably 2 nm or more from the viewpoint of promoting the growth of composite particles in the pores. On the other hand, the mode diameter Da of the pores is preferably 20 nm or less from the viewpoint of preventing the catalyst from cracking. Therefore, the inner pore diameter Da of the catalyst for producing a carboxylic acid ester is preferably 2 nm or more and 20 nm or less, more preferably 2 nm or more and 15 nm or less, and even more preferably 3 nm or more and 10 nm or less. The value of the mode diameter Da of the pores is measured by the method described in the examples below. The method for adjusting the mode diameter Da of the pores is not particularly limited, but for example, the mode diameter Da of the pores can be adjusted to the above range by employing a preferable manufacturing method described later. It is preferable that the half width Wa and the mode diameter Da of the pores satisfy the relationship of the following formula (1). 1 / 2Wa < Da (1)

[0016] In this embodiment, the mode diameter Dd of the pores calculated by the BJH method from the desorption isotherm obtained by the nitrogen adsorption method of the catalyst for producing a carboxylic acid ester is preferably 2 nm or more from the viewpoint of maintaining high reaction activity without increasing the diffusion resistance in the pores too much so as not to limit the diffusion process of the reaction substrate. On the other hand, the mode diameter Dd of the pores is preferably 15 nm or less from the viewpoint of preventing the catalyst from cracking. Therefore, the pore inlet diameter Dd of the catalyst for producing a carboxylic acid ester is preferably 2 nm or more and 15 nm or less, more preferably 2 nm or more and 7 nm or less, and even more preferably 3 nm or more and 7 nm or less. The value of the mode diameter Dd of the pores is measured by the method described in the Examples below. The method for adjusting the mode diameter Dd of the pores is not particularly limited, but for example, the mode diameter Dd of the pores can be adjusted to the above range by employing a preferable manufacturing method described later. It is preferable that the half width Wd and the mode diameter Dd of the pores satisfy the relationship of the following formula (2). 1 / 2Wd < Dd (2)

[0017] In this embodiment, the catalyst particles contain at least one element selected from the group consisting of nickel, cobalt, palladium, lead, platinum, ruthenium, gold, silver, and copper. Such catalyst particles have the function of catalyzing a reaction for producing a carboxylate ester. The catalyst particles in this embodiment preferably contain at least one element selected from the group consisting of nickel, cobalt, palladium, lead, and gold, and more preferably are composite particles containing oxidized nickel and / or cobalt and X (X represents at least one element selected from the group consisting of nickel, palladium, platinum, ruthenium, gold, silver, and copper).

[0018] In this embodiment, the catalyst for producing a carboxylic acid ester preferably has a support layer in which the composite particles are localized. The term "support layer in which the composite particles are localized" refers to a region in which the composite particles are concentrated and supported in the support. In the catalyst for producing a carboxylic acid ester of this embodiment, the composite particles are preferably not randomly supported in the support but are selectively supported in a certain region, and this region is called a "support layer in which the composite particles are localized". In the catalyst for producing a carboxylic acid ester, if the composite particles are concentrated in a certain region compared to other parts, that region is a "support layer in which the composite particles are localized", and which region is the "support layer in which the composite particles are localized" can be grasped by the X-ray microprobe analysis method described later or a secondary electron reflection image of a high-resolution scanning electron microscope. The support layer in which the composite particles are localized is preferably present in a region from the surface of the catalyst for producing a carboxylic acid ester to 40% of the equivalent diameter of the catalyst for producing a carboxylic acid ester. When the support layer in which the composite particles are localized is present in the above-mentioned region, the influence of the diffusion rate of the reactants inside the support is reduced, and the reaction activity tends to be improved.

[0019] The catalyst for producing a carboxylate ester of this embodiment can have various sizes, with the effective thickness or particle diameter being on the order of μm to cm, and various shapes. Specific examples of the shape of the catalyst for producing a carboxylate ester include, but are not limited to, various shapes such as a sphere, an ellipse, a cylinder, a tablet, a hollow cylinder, a plate, a rod, a sheet, and a honeycomb. The shape can be appropriately changed depending on the reaction type, and, for example, but not limited to, a hollow cylinder or a honeycomb shape that has a small pressure loss is selected in a fixed bed reaction, and a spherical shape is generally selected under liquid phase slurry suspension conditions.

[0020] The term "equivalent diameter" as used herein refers to the diameter of a spherical particle, or in the case of an irregularly shaped particle, the diameter of a sphere having the same volume as the particle or the same surface area as the particle. The equivalent diameter can be measured by measuring the average particle diameter (volume basis) using a laser diffraction / scattering particle size distribution measuring device, and expressing this as the equivalent diameter, or by measuring the number average particle diameter using a scanning electron microscope (SEM).

[0021] The thickness of the support layer in which the composite particles are localized is selected within an optimal range depending on the thickness of the support, the particle size, the type of reaction, and the reaction format. In general, the "equivalent diameter of the catalyst for producing a carboxylic acid ester" is the same as the "equivalent diameter of the support," so the "equivalent diameter of the catalyst for producing a carboxylic acid ester" can be determined by the equivalent diameter of the support.

[0022] For example, when a large carrier having an equivalent diameter of more than 200 μm (e.g., several mm or more) is used, the catalyst for producing carboxylic acid esters is generally used for a liquid phase reaction or a gas phase reaction with a relatively slow reaction rate. Therefore, by supporting the composite particles, which are the active ingredient, in a region from the surface of the catalyst for producing carboxylic acid esters to 40% of the equivalent diameter of the catalyst for producing carboxylic acid esters and in a region from the outer surface of the catalyst for producing carboxylic acid esters to 80 μm, and providing a layer that does not support the composite particles inside the catalyst for producing carboxylic acid esters, a catalyst for producing carboxylic acid esters that is less susceptible to the diffusion rate of reactants tends to be obtained. As a result, the composite particles can be effectively used.

[0023] On the other hand, when the equivalent diameter of the catalyst for producing carboxylic acid ester is 200 μm or less, it is preferable to support the composite particles in an area from the surface of the catalyst for producing carboxylic acid ester to 30% of the equivalent diameter of the catalyst for producing carboxylic acid ester. In particular, when used in a liquid phase reaction, the reaction rate and the diffusion rate of the reactants in the pores inside the carrier are affected, so that the particle diameter of the carrier has been designed to be small according to the reaction. In this embodiment, by making the support layer in which the composite particles are localized thin, a catalyst for producing carboxylic acid ester with high activity can be obtained without making the particle diameter of the carrier small. In this case, there is also an advantage that separation of the catalyst by sedimentation is easy, and separation can be made using a small-capacity separator. On the other hand, if the volume of the part in the catalyst for producing carboxylic acid ester where the composite particles are not supported becomes too large, the volume unnecessary for the reaction per reactor may become large, resulting in waste. Therefore, it is preferable to set the carrier particle diameter according to the form of the reaction, and set the thickness of the support layer in which the necessary composite particles are localized and the thickness of the layer in which the composite particles are not supported.

[0024] The catalyst for producing a carboxylate ester may have an outer layer that does not substantially contain composite particles outside the support layer where the composite particles are localized. The outer layer is preferably formed to a thickness of 0.01 to 15 μm from the outer surface of the support. By providing an outer layer in this range, the catalyst can be used as a catalyst that is resistant to catalyst poisons and suppresses the detachment of composite particles due to wear in reactions using reactors such as fluidized beds, bubble columns, and stirred reactors where friction of catalyst particles is a concern, or in reactions where accumulation of poisoning substances occurs. In addition, since the outer layer can be controlled to be extremely thin, a significant decrease in activity can be suppressed.

[0025] The thickness of the outer layer that does not substantially contain composite particles is selected in an optimal range depending on the reaction characteristics, carrier properties, the amount of composite particles supported, etc., and is preferably 0.01 to 15 μm, more preferably 0.1 to 10 μm, and even more preferably 0.2 to 5 μm. If the thickness of the outer layer (layer not supporting composite particles) exceeds 15 μm, the effect of improving the catalyst life when using the composite particles as a catalyst remains the same, but the catalytic activity may decrease. If the thickness of the outer layer is less than 0.01 μm, the composite particles tend to easily fall off due to wear.

[0026] In this embodiment, the term "substantially free of composite particles" means that there is substantially no peak showing a distribution of nickel and / or cobalt in an oxidation state and X (X represents at least one element selected from the group consisting of nickel, palladium, platinum, ruthenium, gold, silver, and copper) with a relative intensity of 10% or more in an X-ray microprobe analysis method described below or a secondary electron reflection image of a high-resolution scanning electron microscope.

[0027] As described above, the composite particles of this embodiment preferably contain nickel and / or cobalt in an oxidized state. The oxidized nickel is preferably a nickel oxide (e.g., Ni2O, NiO, NiO2, Ni3O4, Ni2O3) formed by the combination of nickel with oxygen, or a nickel-containing composite oxide such as a nickel oxide compound or solid solution formed by the combination of nickel with X and / or one or more other metal elements and oxygen, or a mixture thereof. The oxidized cobalt is preferably a cobalt oxide (e.g., CoO, Co2O3, Co3O4) formed by combining cobalt with oxygen, or a composite oxide containing cobalt, such as a cobalt oxide compound or solid solution formed by combining cobalt with X and / or one or more other metal elements and oxygen, or a mixture thereof.

[0028] The term "nickel oxide" as used herein refers to a compound containing nickel and oxygen. Nickel oxide includes the above-mentioned Ni2O, NiO, NiO2, Ni3O4, Ni2O3, or hydrates thereof, nickel hydroperoxides containing OOH groups, nickel peroxides containing O2 groups, or mixtures thereof.

[0029] The term "composite oxide" as used herein refers to an oxide containing two or more metals. The term "composite oxide" refers to an oxide in which two or more metal oxides form a compound, and includes composite oxides in which oxoacid ions do not exist as structural units (e.g., nickel perovskite-type oxides and spinel-type oxides), but is a broader concept than composite oxides and includes all oxides in which two or more metals are composited. Oxides in which two or more metal oxides form a solid solution also fall within the category of composite oxides.

[0030] In the catalyst for producing a carboxylate ester of this embodiment, when nickel oxide and / or cobalt oxide are composited with X as described above, the inherent catalytic ability of nickel oxide and / or cobalt oxide having oxidative esterification activity is brought out, and a remarkably high catalytic performance that could not be achieved by a catalyst consisting of each single component tends to appear. This is a unique effect that appears by composite of nickel oxide and / or cobalt oxide with X, and is considered to be due to the dual function effect between the two metal components or the generation of new active species, etc., which creates a new catalytic action that is completely different from that of each single component. Furthermore, when oxidized nickel and / or oxidized cobalt and X are supported on a support in a highly dispersed state, it tends to realize revolutionary catalytic performance that cannot be obtained by conventional catalysts.

[0031] For example, when gold is selected as X and nickel oxide and gold are highly dispersed on the support, a remarkably high catalytic performance tends to be exhibited. Such a catalyst for producing carboxylic acid esters has a higher selectivity for carboxylic acid esters than a catalyst in which nickel oxide or gold is supported on a support alone, and the activity tends to be significantly improved when the Ni / Au composition ratio is within a specific range. The catalytic activity per metal atom is higher than that of a particle support consisting of each single component, and the expression of the catalytic function due to the composite strongly depends on the supported composition of nickel and gold. This is presumed to be because there is an optimal ratio for the formation of the optimal oxidation state of nickel for the reaction. In this way, by dispersing and supporting the two components of nickel oxide and gold on the support, a remarkable composite effect that cannot be predicted from the simple phase addition of each single component tends to be exhibited.

[0032] The catalyst for producing a carboxylate ester in which gold is selected as X as described above has oxidized nickel and gold highly dispersed on the support, and both components tend to be composited at nano-size. When such a catalyst for producing a carboxylate ester is observed with a transmission electron microscope / scanning transmission electron microscope (TEM / STEM), a structure in which nearly spherical nanoparticles of 2 to 3 nm are uniformly dispersed and supported on the support is typically observed. Furthermore, when the nanoparticles are subjected to elemental analysis by energy dispersive X-ray spectroscopy (EDS), nickel and gold are typically observed to coexist in each particle, with the gold nanoparticles being observed to have nickel coated on their surfaces. In addition to nanoparticles containing nickel and gold, nickel components are also observed to be supported alone on the support. Furthermore, the state of the metals can be confirmed by subjecting the material to X-ray photoelectron spectroscopy (XPS) and powder X-ray diffraction (powder XRD). Typically, it is observed that gold exists as a crystalline metal, while nickel exists as an amorphous oxide having a valence of two. Furthermore, when ultraviolet-visible spectroscopy (UV-Vis), which can observe changes in the excited state of electrons, is used, it is typically observed that the surface plasmon absorption peak (approximately 530 nm) derived from gold nanoparticles, which is observed in single-metal gold nanoparticles, disappears due to the composite of nickel oxide and gold. This phenomenon of disappearance of the surface plasmon absorption peak has not been observed in catalysts consisting of combinations of gold and other metal oxide species (e.g., metal oxides such as chromium oxide, manganese oxide, iron oxide, cobalt oxide, copper oxide, and zinc oxide) other than nickel oxide, which had no effect on the reaction. This disappearance of the surface plasmon absorption peak is thought to be the result of hybridization of the electronic state via the contact interface between oxidized nickel and gold, that is, due to hybridization of the two types of metal chemical species. The conversion to highly oxidized nickel oxide can be confirmed by the color change of the catalyst and ultraviolet-visible spectroscopy (UV-Vis). By adding gold to nickel oxide, the nickel oxide changes color from gray-green to brownish red, and the UV spectrum shows absorption across almost the entire visible light range. The shape of the UV spectrum and the color of the catalyst are similar to those of highly oxidized nickel peroxide (NiO2) measured as a reference sample. It can thus be inferred that the addition of gold converts nickel oxide into highly oxidized nickel oxide. From the above results, it is considered that the structure of the composite particle when gold is selected as X is a gold particle having a core whose surface is coated with highly oxidized nickel oxide, and that no gold atoms are present on the surface of the composite particle.

[0033] The composite particles are preferably supported on the carrier in a highly dispersed state, more preferably in the form of fine particles or thin films, and the average particle size is preferably 2 to 10 nm, more preferably 2 to 8 nm, and even more preferably 2 to 6 nm. When the average particle diameter of the composite particles is within the above range, a specific active species structure consisting of nickel and / or cobalt and X is formed, and the reaction activity tends to be improved. Here, the average particle diameter in this embodiment means the number average particle diameter measured by a transmission electron microscope (TEM). Specifically, in an image observed by a transmission electron microscope, the part with black contrast is the composite particle, and the diameter of each particle can be measured and the number average can be calculated.

[0034] The composition of nickel or cobalt and X in the composite particles is preferably in the range of 0.1 to 10, more preferably 0.2 to 8.0, and further preferably 0.3 to 6.0, as the Ni / X atomic ratio or Co / X atomic ratio. When the Ni / X atomic ratio or Co / X atomic ratio is within the above range, a specific active species structure consisting of nickel and / or cobalt and X and an oxidation state of nickel and / or cobalt optimal for the reaction are formed, and as a result, the activity and selectivity tend to be higher than when it is outside the above range.

[0035] The form of the composite particles is not particularly limited, but is preferably a form in which both components nickel and / or cobalt and X coexist in the particles and have a phase structure, for example, a solid solution structure in which chemical species randomly occupy crystal sites, a core-shell structure in which each chemical species is separated concentrically, an anisotropic phase separation structure in which phases are separated anisotropically, or a heterobondophilic structure in which both chemical species exist adjacent to each other on the particle surface. More preferably, it has a core made of X, and the surface of the core is preferably coated with nickel and / or cobalt in an oxidized state. The form of the composite particles is not particularly limited as long as it contains both components, and may be any shape such as spherical or hemispherical.

[0036] As an analytical method for observing the morphology of the composite particles, for example, a transmission electron microscope / scanning transmission electron microscope (TEM / STEM) is effective as described above, and by irradiating an electron beam on a nanoparticle image observed by TEM / STEM, elemental analysis in the particles and depiction of an element distribution image are possible. As shown in the examples described later, the composite particles of this embodiment have been confirmed to have a morphology in which nickel and / or cobalt and X are contained in each particle, and the surface of X is coated with nickel and / or cobalt. When the composite particles have such a morphology, the atomic ratio of nickel and / or cobalt to X varies depending on the position of the composition analysis point in the particle, and more nickel and / or cobalt is detected at the particle edge than at the particle center. Therefore, even in individual particles, the atomic ratio of nickel or cobalt to X has a range depending on the position of the analysis point, and the range is included in the range of the Ni / X atomic ratio or Co / X atomic ratio described above.

[0037] When gold, silver, or copper is selected as X, ultraviolet-visible spectroscopy (UV-Vis) is a useful means for identifying the structure. In the case of a single gold-silver-copper nanoparticle, the light electric field in the visible to near-infrared region is coupled with the surface free electrons of the metal, resulting in surface plasmon absorption. For example, when visible light is irradiated onto a catalyst carrying gold particles, an absorption spectrum based on the plasmon resonance originating from the gold particles is observed at a wavelength of about 530 nm. However, in the catalyst for producing carboxylates carrying nickel oxide and gold according to this embodiment, the surface plasmon absorption disappears, so it can be considered that no gold is present on the surface of the composite particle according to this embodiment.

[0038] The solid form of nickel is not particularly limited as long as it can provide a desired activity, but is preferably an amorphous form in which no diffraction peak is observed by X-ray diffraction. By providing nickel in this form, it is presumed that the interaction with oxygen is enhanced when used as a catalyst for an oxidation reaction, and further, the bonding interface between oxidized nickel and X is increased, so that more excellent activity tends to be obtained.

[0039] In this embodiment, X is at least one element selected from the group consisting of nickel, palladium, platinum, ruthenium, gold, silver, and copper, and X is preferably at least one element selected from nickel, palladium, ruthenium, gold, and silver, more preferably at least one element selected from palladium and gold, and even more preferably gold.

[0040] The chemical state of X may be any of a metal, an oxide, a hydroxide, a composite compound containing X and nickel, cobalt or one or more other metal elements, or a mixture thereof, but the preferred chemical state is a metal or an oxide, more preferably a metal. The solid form of X is not particularly limited as long as it can provide a desired activity, and may be either a crystalline or amorphous form.

[0041] The term "other metal elements" used herein refers to a third component element or a metal component such as an alkali metal, an alkaline earth metal, or a rare earth metal contained in the catalyst for producing a carboxylate ester, in addition to the constituent elements of the support, nickel and / or cobalt in an oxidized state, and X, as described below.

[0042] In the present embodiment, from the viewpoint of further improving pH swing resistance, the composite particles preferably contain oxidized nickel and gold. The composition ratio of nickel to gold in the composite particles is preferably 1.1 to 10, more preferably 2 to 9, and even more preferably 3 to 8, as the Ni / Au atomic ratio.

[0043] As described above, the catalyst for producing a carboxylate ester of this embodiment exerts excellent effects by supporting oxidized nickel and / or cobalt and X on a carrier and forming composite particles composed of oxidized nickel and / or cobalt and X. In this embodiment, the term "composite particles" refers to particles containing different bimetallic species in one particle. Examples of bimetallic species other than these include bimetallic particles in which both components nickel and / or cobalt and X are metals, and metal particles in which nickel and / or cobalt form an alloy or intermetallic compound with X. However, when used as a catalyst for chemical synthesis, these tend to have lower selectivity to the target product and lower catalytic activity than the catalyst for producing a carboxylate ester of this embodiment.

[0044] The catalyst for producing a carboxylate ester of this embodiment preferably contains oxidized nickel and / or cobalt alone on a support, in addition to composite particles composed of oxidized nickel and / or cobalt and X. The presence of oxidized nickel and / or cobalt that is not composited with X further enhances the structural stability of the catalyst for producing a carboxylate ester, and suppresses the increase in pore size due to a long-term reaction and the accompanying particle growth of the composite particles. This effect tends to be remarkable when an aluminum-containing silica-based composition containing silica and alumina is used as the support, as described below.

[0045] The following describes the effect of increasing the structural stability of the catalyst for producing carboxylic acid esters and suppressing the increase in pore size due to a long-term reaction and the accompanying particle growth of composite particles by having oxidized nickel and / or cobalt present alone on the support.

[0046] As described later, in a synthesis reaction of a carboxylate ester, by adding an alkali metal or alkaline earth metal compound to the reaction system and maintaining the pH of the reaction system at 6 to 9, more preferably under neutral conditions (e.g., pH 6.5 to 7.5), i.e., as close to pH 7 as possible, the production of by-products inherent to the production reaction of a carboxylate ester, such as acetals due to acidic substances typified by methacrylic acid or acrylic acid, tends to be suppressed.

[0047] According to the study by the present inventors, when a gold particle support in which a single component of gold particles is supported on a carrier made of an aluminum-containing silica-based composition containing silica and alumina is used to carry out a long-term reaction by the above-mentioned reaction operation, the structure of the gold particle support tends to change gradually. This phenomenon is considered to be due to the fact that the support particles are repeatedly exposed locally to acid and base by the above-mentioned reaction operation, a part of the Al in the support is dissolved and precipitated, and the silica-alumina bridge structure is rearranged, causing the pore size of the support particles to expand. In addition, as the pore size expands, sintering of the gold particles occurs, and the surface area decreases, which tends to reduce the catalytic activity.

[0048] On the other hand, by having the composite particles and nickel and / or cobalt in a single oxidized state present on the carrier, the structural stability of the supported particles due to the above reaction operation is enhanced, and the expansion of the pore size and the growth of the composite particles tend to be suppressed. The reason for this is thought to be that, as described above, the oxidized nickel and / or cobalt react with the constituent elements of the carrier to generate a composite oxide containing nickel and / or cobalt, such as an oxide compound or solid solution of nickel and / or cobalt, and as a result of the nickel compound acting to stabilize the silica-alumina bridge structure, the structural change of the supported particles is thought to be greatly improved. The inventors presume that the manifestation of such a structural stabilization effect of the supported material is due to the oxidized nickel and / or cobalt present on the carrier. Therefore, when the oxidized nickel and / or cobalt contained in the composite particles are in contact with the carrier, this effect is of course obtained, and when the oxidized nickel and / or cobalt are present alone on the carrier, it is thought that an even greater stabilization effect can be obtained.

[0049] The support for the catalyst for producing a carboxylic acid ester of this embodiment is not particularly limited as long as it can support the catalyst particles of this embodiment, and any catalyst support used for conventional chemical synthesis can be used.

[0050] Examples of the carrier include various carriers such as activated carbon, silica, alumina, silica-alumina, titania, silica-titania, zirconia, magnesia, silica-magnesia, silica-alumina-magnesia, calcium carbonate, zinc oxide, zeolite, and crystalline metallosilicate. Preferred are activated carbon, silica, alumina, silica-alumina, silica-magnesia, silica-alumina-magnesia, titania, silica-titania, and zirconia, and more preferred are silica-alumina and silica-alumina-magnesia.

[0051] The support may contain one or more metal components selected from alkali metals (Li, Na, K, Rb, Cs), alkaline earth metals (Be, Mg, Ca, Sr, Ba), and rare earth metals (La, Ce, Pr). The metal components to be supported are preferably those that become oxides by calcination, such as nitrates or acetates.

[0052] The carrier is preferably made of an aluminum-containing silica-based composition containing silica and aluminum. That is, the carrier preferably contains silica and alumina. The carrier has higher water resistance than silica and higher acid resistance than alumina. In addition, the carrier has superior physical properties to conventional carriers that are generally used, such as being harder and having higher mechanical strength than activated carbon, and can stably support the active components, nickel and / or cobalt in an oxidized state and X. As a result, the catalyst for producing a carboxylic acid ester tends to maintain high reactivity for a longer period of time.

[0053] A catalyst for producing a carboxylic acid ester, which has a specific atomic ratio of oxidized nickel and / or cobalt to X and is supported by an aluminum-containing silica-based composition, tends to have a large surface area suitable for use as a catalyst support when used as a catalyst for chemical synthesis, while also having high mechanical strength and physical stability, and also to have satisfactory corrosion resistance against the liquid properties specific to the reaction.

[0054] The characteristics of the carrier made of the alumina-containing silica-based composition containing silica and alumina according to the present embodiment, which enables a significant improvement in catalyst life, will be described below. The reason why the mechanical strength and chemical stability of the carrier can be significantly improved is presumed to be as follows.

[0055] In the carrier made of the aluminum-containing silica-based composition, by adding aluminum (Al) to the uncrosslinked silica (Si-O) chain of the silica gel, a new Si-O-Al-O-Si bond is formed, and the Si-O bond is strengthened by the formation of an Al crosslinked structure without losing the inherent stability of the Si-O chain against acidic substances, and it is considered that the hydrolysis resistance stability (hereinafter also simply referred to as "water resistance") is significantly improved. In addition, when the Si-O-Al-O-Si crosslinked structure is formed, the number of Si-O uncrosslinked chains is reduced compared to the case of silica gel alone, and the mechanical strength is also increased. In other words, it is presumed that the amount of Si-O-Al-O-Si structure formed is correlated with the improvement of the mechanical strength and water resistance of the obtained silica gel.

[0056] One of the reasons why it has become possible to stably support oxidized nickel and / or cobalt and X on a support for a long period of time is that the support has significantly improved mechanical strength and chemical stability, as described above, and has superior physical properties compared to conventional supports that are commonly used. As a result, it is believed that the active components nickel and / or cobalt and X are less likely to peel off, making it possible to stably support them for a long period of time.

[0057] In the case of commonly used carriers, such as silica or silica-titania, nickel and / or cobalt components tend to be gradually eluted in a long-term reaction. In contrast, when the above carrier is used, the elution of nickel and / or cobalt components tends to be suppressed for a long period of time. In particular, the results of X-ray photoelectron spectroscopy (XPS), transmission electron microscopy (TEM / EDX), and double crystal high resolution X-ray fluorescence analysis (HRXRF) have confirmed that when a silica or silica-titania carrier is used, the eluted nickel and / or cobalt components are nickel oxide or cobalt oxide present alone on the carrier. Since nickel oxide or cobalt oxide is a compound soluble in acid, when it is used as a catalyst for synthesizing carboxylic acid esters, it is presumed that it is eluted by acidic substances such as methacrylic acid or acrylic acid, which are by-products specific to this reaction.

[0058] Analysis of the chemical state of nickel and / or cobalt by double crystal high resolution X-ray fluorescence spectrometry (HRXRF) suggests that the nickel and / or cobalt in the catalyst for producing a carboxylate ester of the present embodiment is not limited to nickel oxide and / or cobalt oxide, which are single compounds, but is presumed to be a composite oxide containing nickel and / or cobalt, such as nickel and / or cobalt oxide compounds or solid solutions produced by the combination of nickel oxide and / or cobalt oxide with constituent elements of the support, or mixtures thereof.

[0059] Double crystal high resolution X-ray fluorescence spectrometry (HRXRF) has extremely high energy resolution, and the chemical state can be analyzed from the energy position (chemical shift) and shape of the spectrum obtained. In particular, in the Kα spectrum of 3d transition metal elements, changes in chemical shift and shape occur due to changes in valence and electronic state, and the chemical state can be analyzed in detail. In the catalyst for producing a carboxylate ester of this embodiment, typically, as in the examples described later, changes occur in the NiKα spectrum, and a chemical state of nickel different from that of nickel oxide, which is a single compound, is confirmed.

[0060] For example, nickel aluminate, which is formed from nickel oxide and alumina, is a compound that is insoluble in acid. It is presumed that the formation of such a nickel compound on the carrier significantly improved the elution of nickel components.

[0061] In this embodiment, the support is preferably a silica-based material containing silicon, aluminum, at least one fourth period element selected from the group consisting of iron, cobalt, nickel, and zinc, and at least one basic element selected from the group consisting of alkali metal elements, alkaline earth metal elements, and rare earth elements in the ranges of 42 mol% to 90 mol%, 3 mol% to 38 mol%, 0.5 mol% to 20 mol%, and 2 mol% to 38 mol%, respectively, based on the total molar amount of the silicon, the aluminum, the fourth period element, and the basic element. When the silica-based material containing silicon, aluminum, the above-mentioned fourth period element, and the above-mentioned basic element contains 42 to 90 mol% silicon, 3 to 38 mol% aluminum, 0.5 to 20 mol% fourth period element, and 2 to 38 mol% basic element relative to the total molar amount of silicon, aluminum, the fourth period element, and the basic element, silicon, aluminum, the fourth period element, the basic element, and oxygen atoms form a specific stable bond structure with each other, and the bond structure is easily formed in a state of being uniformly dispersed in the silica-based material. From the above viewpoint, in this embodiment, it is more preferable to contain 70 to 90 mol% silicon, 5 to 30 mol% aluminum, 0.75 to 15 mol% fourth period element, and 2 to 30 mol% basic element, and it is even more preferable to contain 75 to 90 mol% silicon, 5 to 15 mol% aluminum, 1 to 10 mol% fourth period element, and 2 to 15 mol% basic element. In particular, when the composition ratio of the fourth period element is 0.75 mol % or more and each component is uniformly dispersed throughout the material, there are few parts in the structure where the fourth period element is not present, and a silica-based material that exhibits resistance (high acid resistance and basicity) even when repeatedly exposed to acid and / or base tends to be obtained. From the viewpoint of obtaining a silica-based material with high mechanical strength and large specific surface area, it is preferable that the fourth period element is 10 mol % or less and the basic element is 30 mol % or less. The composition ratio of silicon to aluminum is set in a preferred range from the viewpoint of the acid resistance, base resistance, and water resistance of the silica-based material. The composition ratio of silicon to aluminum is preferably (silicon / aluminum)=2 to 4. If (silicon / aluminum) is smaller than the above range, the acid resistance and base resistance tend to be low. If (silicon / aluminum) is larger than the above range, the water resistance tends to be low. Examples of the alkali metals of the basic metal component include Li, Na, K, Rb, and Cs, examples of the alkaline earth metals include Be, Mg, Ca, Sr, and Ba, and examples of the rare earth metals include La, Ce, and Pr.

[0062] For example, when nickel is selected as the fourth periodic element and magnesium as the basic element, and the chemical state of nickel is analyzed by double crystal high resolution X-ray fluorescence spectrometry (HRXRF) for a silica-based material made of a composite oxide containing silicon-aluminum-nickel-magnesium, the nickel in the silica-based material of this embodiment does not exist as nickel oxide, which is a single compound, but exists as a composite oxide containing nickel, such as a nickel oxide compound or solid solution produced by combining nickel oxide with alumina and / or magnesia, or a mixture thereof.

[0063] In the silica-based materials mentioned above, nickel is presumed to exist, for example, as nickel aluminate (NiAl2O4), which is a spinel compound of nickel oxide and alumina, or as a solid solution of nickel oxide and magnesia (NiO·MgO). Similarly, for the above-mentioned 4th period elements other than nickel, it is considered that their oxides form spinel compounds with alumina or solid solutions with basic metal oxides, thereby stabilizing the silica-alumina bridge structure and increasing chemical stability.

[0064] When the fourth period element is nickel and the basic element is magnesium, the silica-based material made of a composite oxide containing silicon, aluminum, nickel, and magnesium preferably contains silicon in the range of 42 to 90 mol%, aluminum in the range of 3 to 38 mol%, nickel in the range of 0.5 to 20 mol%, and magnesium in the range of 2 to 38 mol% relative to the total molar amount of silicon, aluminum, nickel, and magnesium from the viewpoint of acid resistance, basicity, mechanical strength, and water resistance. More preferably, it contains silicon in the range of 70 to 90 mol%, aluminum in the range of 5 to 30 mol%, nickel in the range of 0.75 to 15 mol%, and magnesium in the range of 2 to 30 mol%, and even more preferably, it contains silicon in the range of 75 to 90 mol%, aluminum in the range of 5 to 15 mol%, nickel in the range of 1 to 10 mol%, and magnesium in the range of 2 to 15 mol%. When the elemental composition of silicon, aluminum, nickel, and magnesium is within the above range, silicon, aluminum, nickel, and magnesium are likely to form a specific stable bond structure. In particular, in the case of a more preferable composition ratio, the above-mentioned stable bond structure is expected to be formed at a sufficient density to contribute to the stabilization of the entire silica-based material, even if it is assumed that it is uniformly dispersed in the silica-based material, and as a result, the silica-based material tends to exhibit good acid resistance, base resistance, and mechanical strength that can withstand repeated use.

[0065] [Determination of the content of constituent elements in silica-based materials and precious metal-supported materials] The concentrations of Si, Al, period 4 elements, and basic elements in the silica-based material are quantified using an ICP atomic emission spectrometer (ICP-AES, MS) "IRIS Intrepid II XDL" (product name) manufactured by Thermo Fisher Scientific Co., Ltd. The sample is prepared as follows. First, the silica-based material is weighed into a Teflon (registered trademark) decomposition vessel, and nitric acid and hydrogen fluoride are added thereto. The resulting solution is thermally decomposed using a Milestone General microwave decomposition device, "ETHOS·TC Model" (product name), and then evaporated to dryness on a heater. Next, nitric acid and hydrochloric acid are added to the precipitated residue, which is then pressure-decomposed using the microwave decomposition device. The resulting decomposition liquid is adjusted to a certain volume with pure water to prepare the sample. The sample is quantified using the internal standard method with the ICP-AES, and the blank value obtained at the same time is subtracted to determine the contents of Si, Al, period 4 elements, and basic elements in the silica-based material, and the contents of metal elements in the precious metal-supported material, and the composition ratio (molar basis) and supported amount are calculated.

[0066] Next, a preferred method for preparing a carrier having the above-mentioned structure or composition will be described. The method for preparing a carrier made of an aluminum-containing silica-based composition containing silica and alumina is not particularly limited, and for example, the carrier can be prepared by reacting a silica sol with an aluminum compound solution to form an aluminum-containing silica composition, subjecting the composition to hydrothermal synthesis under the conditions described below, followed by drying and calcination.

[0067] The method for preparing the carrier will be described in detail below. As the silica source, for example, silica sol or silica gel is used. As the silica gel, it is sufficient that it has an uncrosslinked Si site that reacts with Al, and there is no particular restriction on the length of the Si-O chain. As the aluminum compound, water-soluble compounds such as sodium aluminate, aluminum chloride hexahydrate, aluminum perchlorate hexahydrate, aluminum sulfate, aluminum nitrate nonahydrate, and aluminum diacetate are preferable, but water-insoluble compounds such as aluminum hydroxide and aluminum oxide can also be used as long as they react with the uncrosslinked Si in the silica sol or silica gel.

[0068] A silica sol and an aluminum compound are mixed to obtain a mixed sol containing the silica sol and the aluminum compound, which is subjected to a multi-stage hydrothermal reaction at 20 to 100°C for 1 to 48 hours, then dried to obtain a gel, which is then fired under the temperature, time and atmosphere conditions described below, or an alkaline aqueous solution is added to the mixed sol to co-precipitate silica and the aluminum compound, which is subjected to hydrothermal synthesis under the conditions described below, dried and then fired. It is also possible to obtain a carrier made of an aluminum-containing silica-based composition having a desired particle size by a process such as pulverizing the mixed sol as it is using a spray dryer, or drying the mixed sol to granulate the gel.

[0069] A method for preparing a carrier containing silica, alumina, and an oxide of at least one basic metal selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals can be performed according to the above-mentioned method for preparing a carrier consisting of an aluminum-containing silica-based composition containing silica and alumina, by drying a slurry in which an alkali metal compound, an alkaline earth metal compound, and / or a rare earth metal compound is mixed with silica and aluminum components, and then calcining the slurry under conditions described below.

[0070] As the raw materials of the alkali metals, alkaline earth metals, and rare earth metals, generally commercially available compounds can be used, similar to the aluminum raw material. Water-soluble compounds are preferred, and hydroxides, carbonates, nitrates, and acetates are more preferred.

[0071] As another preparation method, a method of adsorbing a basic metal component selected from alkali metals, alkaline earth metals and rare earth metals to a carrier made of an aluminum-containing silica-based composition can be used.For example, a method using a dipping method, such as adding a carrier to a liquid in which a basic metal compound is dissolved and then drying, or a method using an impregnation method, such as impregnating a carrier with a basic compound in an amount equivalent to the pore volume and then drying, can be applied.However, when the method of adsorbing a basic metal component later, it is necessary to pay attention to carrying out the liquid drying process under mild conditions in order to highly disperse the basic metal component on the carrier.

[0072] In addition, inorganic or organic substances can be added to the mixed slurry of the above-mentioned various raw materials in order to control the properties of the slurry and to finely adjust the characteristics of the product, such as the pore structure, and the physical properties of the carrier to be obtained.

[0073] Specific examples of inorganic substances that can be used include mineral acids such as nitric acid, hydrochloric acid, and sulfuric acid, metal salts of alkali metals such as Li, Na, K, Rb, and Cs, and alkaline earth metals such as Mg, Ca, Sr, and Ba, water-soluble compounds such as ammonia and ammonium nitrate, and clay minerals that disperse in water to form a suspension.Specific examples of organic substances include polymers such as polyethylene glycol, methyl cellulose, polyvinyl alcohol, polyacrylic acid, and polyacrylamide.

[0074] The effects of adding inorganic and organic substances are various, but mainly include forming a spherical carrier, controlling the pore size and pore volume, etc. Specifically, the liquid quality of the mixed slurry is an important factor for obtaining a spherical carrier. By adjusting the viscosity and solid content concentration with inorganic or organic substances, the liquid quality can be changed to one that makes it easier to obtain a spherical carrier. In addition, the pore size and pore volume can be controlled by a multi-stage hydrothermal synthesis process of the mixed slurry described below. It is also preferable to appropriately select and use an optimal organic compound that remains inside the carrier during the forming stage and can be removed by firing and washing operations after forming.

[0075] In the hydrothermal synthesis step in this embodiment, the mixed slurry is stirred while adjusting the heating conditions and stirring conditions. As for the heating conditions, it is preferable to raise the temperature to a predetermined temperature in the first stage and hold it for a predetermined time, to lower the temperature to a predetermined temperature in the second stage and hold it for a predetermined time, and to raise the temperature to a predetermined temperature in the third stage and hold it for a predetermined time. Specifically, it is preferable to adjust the temperature T1 in the first stage to 70 to 90°C and hold it for 1 to 10 hours, it is preferable to adjust the temperature T2 in the second stage to 20 to 40°C and hold it for 0.5 to 10 hours, and it is preferable to adjust the temperature T3 in the third stage to 40 to 60°C and hold it for 1 to 20 hours. By adopting such conditions, the formation of secondary particles in the mixed slurry is easily controlled, and a uniform pore structure tends to be obtained from the vicinity of the pore inlet to the inside of the pore. From the same viewpoint, the value of T1-T2 is preferably 30 to 70°C, more preferably 40 to 60°C, and the value of T3-T2 is preferably 5 to 40°C, more preferably 15 to 30°C. Next, as the stirring conditions, it is preferable to adjust the tip speed of the stirring blade (hereinafter also referred to as "stirring tip speed"), etc. The stirring tip speed V can be defined by the following formula. V=N / 60×πD (N: rotation speed rpm, D: stirring blade diameter) The stirring tip speed V is not particularly limited, but is preferably 5.0 to 20 m / s. The diameter of the stirring blade is not particularly limited, but can be 0.3 to 5 m, preferably 0.5 to 3 m, and more preferably 0.5 to 2 m. The shape of the impeller is not particularly limited, but examples thereof include anchor-type impellers, paddle-type impellers, and turbine-type impellers. From the viewpoint of shear performance, paddle-type impellers and turbine-type impellers are preferred, and turbine-type impellers are more preferred. Examples of turbine-type impellers include radial flow turbine impellers, axial flow turbine impellers, and edged turbine impellers. In the hydrothermal synthesis step in this embodiment, it is preferable to adopt one of the heating conditions and the stirring conditions described above, and more preferably to adopt both of them.

[0076] The carrier can be produced by spray-drying a mixed slurry of the above-mentioned various raw materials and additives. The mixed slurry can be turned into droplets using a known spraying device such as a rotating disk type, a two-fluid nozzle type, or a pressure nozzle type.

[0077] The liquid to be sprayed must be well mixed before use. If the mixture is poor, the performance of the carrier will be affected, such as a decrease in durability due to uneven distribution of the composition. In particular, when mixing the raw materials, the viscosity of the slurry may increase and partial gelation (condensation of colloids) may occur, raising concerns about the formation of non-uniform particles. For this reason, it is sometimes preferable to take measures such as gradually mixing the raw materials under stirring, and to control the silica sol's metastable region, for example, around pH 2, by adding an acid or alkali.

[0078] The liquid to be sprayed must have a certain degree of viscosity and solid content concentration. If the viscosity or solid content concentration is too low, the porous body obtained by spray drying will not be a perfect sphere, and many sunken spheres will be generated. If the viscosity or solid content concentration is too high, it may have an adverse effect on the dispersibility of the porous bodies, and depending on the properties, it may not be possible to stably form droplets. Therefore, if the viscosity is sprayable, it is preferable that it is in the range of 5 to 10,000 cp, and from the perspective of shape, a high viscosity that is sprayable tends to be preferable, and from the perspective of balance with operability, it is more preferable to select from the range of 10 to 1,000 cp. In addition, from the perspective of shape and particle size, it is preferable that the solid content concentration is in the range of 10 to 50 mass%. As a guideline for spray drying conditions, the hot air temperature at the inlet of the drying tower of the spray dryer is preferably 200 to 280 ° C, and the temperature at the outlet of the drying tower is preferably in the range of 110 to 140 ° C.

[0079] The calcination temperature of the carrier is generally selected from the range of 200 to 800°C. Calcination at a temperature exceeding 800°C is undesirable because the specific surface area tends to decrease significantly. The calcination atmosphere is not particularly limited, but calcination is generally performed in air or nitrogen. The calcination time can be determined according to the specific surface area after calcination, but is generally 1 to 48 hours. The calcination conditions change the carrier properties such as porosity, so it is necessary to select appropriate temperature conditions and heating conditions. If the calcination temperature is too low, it tends to be difficult to maintain durability as a composite oxide, and if it is too high, there is a risk of a decrease in the pore volume. The temperature rise conditions are preferably gradually increased using a program temperature rise or the like. If calcination is performed under suddenly high temperature conditions, gasification and combustion of inorganic and organic substances become intense, and the material is exposed to a high temperature condition above the set temperature, which is undesirable because it causes pulverization.

[0080] The specific surface area of ​​the support is set to 10 m as measured by the BET nitrogen adsorption method from the viewpoints of ease of supporting the composite particles, reaction activity when used as a catalyst, difficulty of detachment, and reaction activity. 2 / g or more is preferable, and 20m 2 / g or more is more preferable, and 50m 2 From the viewpoint of activity, there is no particular limitation, but from the viewpoint of mechanical strength and water resistance, it is more preferable that the content of the polymer is 700m 2 / g or less is preferable, and 350m 2 / g or less is more preferable, and 300m 2 / g or less is more preferable.

[0081] When the pore diameter of the carrier is smaller than 3 nm, the peeling property of the supported metal tends to be good, but when used as a catalyst in a liquid phase reaction or the like, the pore diameter is preferably 3 nm or more from the viewpoint of maintaining high reaction activity without increasing the diffusion resistance in the pores too much so as not to limit the diffusion process of the reaction substrate. On the other hand, from the viewpoint of the difficulty of cracking the supported material and the difficulty of peeling off the supported metal, it is preferable that it is 50 nm or less. Therefore, the pore diameter of the carrier is preferably 3 nm to 50 nm, more preferably 3 nm to 30 nm. The pore volume is necessary for the existence of pores that support composite nanoparticles. However, there is a tendency for the strength to decrease rapidly as the pore volume increases. Therefore, from the viewpoint of strength and support characteristics, the pore volume is preferably in the range of 0.1 to 1.0 mL / g, more preferably in the range of 0.1 to 0.5 mL / g. It is preferable that the carrier of this embodiment has both the pore diameter and the pore volume that satisfy the above range.

[0082] The shape of the carrier is selected depending on the reaction format, and in the case of a fixed bed, a hollow cylindrical or honeycomb shape with a structure with little pressure loss is selected, while in the case of a liquid phase slurry suspension condition, a spherical shape is generally selected with an optimal particle size selected from the reactivity and separation method. For example, when adopting a catalyst separation process by sedimentation separation, which is generally simple, a particle size of 10 to 200 μm is preferably selected from the balance with the reaction characteristics, more preferably 20 to 150 μm, and even more preferably 30 to 150 μm. In the cross filter method, small particles of 0.1 to 20 μm or less are preferred because they have higher reactivity. The type and shape can be changed according to the purpose of use and used as a catalyst for chemical synthesis.

[0083] The amount of oxidized nickel or cobalt supported on the carrier is not particularly limited, but is usually 0.01 to 20 mass%, preferably 0.1 to 10 mass%, more preferably 0.2 to 5 mass%, and even more preferably 0.5 to 2 mass% as nickel or cobalt relative to the carrier mass. The amount of X supported on the carrier is usually 0.01 to 10 mass%, preferably 0.1 to 5 mass%, more preferably 0.2 to 2 mass%, even more preferably 0.3 to 1.5 mass%, and particularly preferably 0.5 to 1.0 mass% as metal relative to the carrier mass.

[0084] Furthermore, in this embodiment, there is a suitable range for the atomic ratio of nickel and / or cobalt to the constituent elements of the support. When using a support made of an aluminum-containing silica-based composition containing silica and alumina in this embodiment, the composition ratio of nickel or cobalt to alumina in the catalyst is preferably 0.01 to 1.0, more preferably 0.02 to 0.8, and even more preferably 0.04 to 0.6, in terms of Ni / Al atomic ratio or Co / Al atomic ratio. Furthermore, when a carrier containing silica, alumina, and an oxide of at least one basic metal selected from alkali metals, alkaline earth metals, and rare earth metals is used, the composition ratio of nickel or cobalt to alumina in the support is preferably 0.01 to 1.0, more preferably 0.02 to 0.8, and even more preferably 0.04 to 0.6, in terms of Ni / Al atomic ratio or Co / Al atomic ratio, and the composition ratio of nickel or cobalt to basic metal components is preferably 0.01 to 1.2, more preferably 0.02 to 1.0, and even more preferably 0.04 to 0.6, in terms of Ni / (alkali metal+alkaline earth metal+rare earth metal) atomic ratio or Co / (alkali metal+alkaline earth metal+rare earth metal) atomic ratio.

[0085] When the atomic ratio of nickel and / or cobalt to the aluminum and basic metal oxide, which are the carrier constituent elements, is within the above range, the effect of improving the dissolution of nickel and / or cobalt and the structural change of the supported particles tends to be large. This is thought to be because nickel and / or cobalt, aluminum, and basic metal oxide form a specific composite oxide within the above range, forming a stable bond structure.

[0086] The catalyst for producing a carboxylate ester of this embodiment may contain a third component element in addition to oxidized nickel and / or cobalt and X as active components. Examples of the third component element include titanium, vanadium, chromium, manganese, iron, zinc, gallium, zirconium, niobium, molybdenum, rhodium, cadmium, indium, tin, antimony, tellurium, hafnium, tantalum, tungsten, rhenium, osmium, iridium, mercury, thallium, lead, bismuth, aluminum, boron, silicon, and phosphorus. The content of these third component elements in the support is preferably 0.01 to 20 mass%, more preferably 0.05 to 10 mass%. The catalyst for producing a carboxylate ester may also contain at least one metal component selected from alkali metals, alkaline earth metals, and rare earth metals. The content of the alkali metals, alkaline earth metals, and rare earth metals in the support is preferably selected from the range of 15 mass% or less.

[0087] The third component element or the alkali metal, alkaline earth metal, and rare earth metal may be incorporated into the support during the production or reaction of the catalyst for producing a carboxylate ester, or a method may be used in which the third component element or the alkali metal, alkaline earth metal, and rare earth metal are incorporated into the support in advance.

[0088] The specific surface area of ​​the catalyst for producing a carboxylic acid ester of the present embodiment is preferably 20 to 350 m as measured by the BET nitrogen adsorption method from the viewpoint of reaction activity and difficulty in releasing the active component. 2 / g, more preferably 50 to 300m 2 / g, more preferably 100 to 250 m 2 / g range.

[0089] The pore size of the catalyst for producing carboxylic acid ester is derived from the pore structure of the carrier. If the pore size is smaller than 3 nm, the peeling property of the supported metal component tends to be good. However, when the catalyst is used in a liquid phase reaction or the like, the pore size is preferably 3 nm or more from the viewpoint of maintaining high reaction activity without increasing the diffusion resistance in the pores too much so as not to limit the diffusion process of the reaction substrate. On the other hand, from the viewpoint of the difficulty of cracking the supported material and the difficulty of peeling off the supported composite particles, the pore size is preferably 50 nm or less. Therefore, the pore size of the catalyst for producing carboxylic acid ester is preferably 3 nm to 50 nm, more preferably 3 nm to 30 nm, and even more preferably 3 nm to 10 nm. From the viewpoint of the supporting characteristics and the reaction characteristics, the pore volume is preferably in the range of 0.1 to 1.0 mL / g, more preferably 0.1 to 0.5 mL / g, and even more preferably 0.1 to 0.3 mL / g. The catalyst for producing carboxylic acid ester of this embodiment is preferably one in which both the pore size and the pore volume satisfy the above ranges.

[0090] [Method of producing a catalyst for producing carboxylic acid esters] The method for producing the catalyst for producing a carboxylic acid ester according to the present embodiment is not particularly limited, but may include the following preferred steps. Each step will be described below.

[0091] In the first step, a water slurry containing a carrier is mixed with an acidic aqueous solution of a soluble metal salt containing at least one element selected from the group consisting of nickel, cobalt, palladium, lead, platinum, ruthenium, gold, silver, and copper. The temperature of the mixture of the two liquids is adjusted to 60° C. or higher. In the mixture, a precursor of a catalyst for producing a carboxylic acid ester is generated in which catalyst particles are precipitated on the carrier.

[0092] Next, in the second step, the precursor obtained in the first step is washed with water, dried, and then heat-treated to obtain a catalyst for producing a carboxylic acid ester.

[0093] According to this method, it is possible to obtain a catalyst for producing a carboxylic acid ester, which has a support layer in which the composite particles are localized, and which does not contain the composite particles in the region including the center of the support.

[0094] In this embodiment, it is preferable to carry out a water dispersion step in which the carrier is dispersed in water and aged prior to the first step. By dispersing the carrier in water in advance, a sharper composite particle distribution layer can be obtained. It is presumed that the effect of dispersing the carrier in water is due to the rearrangement of the pore structure of the carrier, which results in a more uniform and sharp pore structure, based on the results of pore distribution measurement by nitrogen adsorption method. The temperature of dispersing the carrier in water can be room temperature, but since the change in the pore structure is slow, it is preferable to select from a range of 60 to 150 ° C, which is higher than room temperature. When performing at normal pressure, the range of 60 to 100 ° C is preferable. In addition, the time for putting the carrier into water is not particularly limited, but can be 0.5 to 10 minutes, and from the viewpoint of making the value of the half-width Wd smaller, it is preferably 0.5 to 8 minutes, more preferably 0.5 to 6 minutes. Furthermore, the time of the water dispersion treatment varies depending on the temperature conditions, but for example, in the case of 90 ° C, it is preferably 1 minute to 5 hours, more preferably 1 to 60 minutes, and even more preferably 1 to 30 minutes. As for the operation of the first step, after dispersing the carrier in water, the carrier can be used after drying and calcining once, but it is preferable to contact a slurry in which the carrier is dispersed in water with an acidic aqueous solution of a soluble metal salt containing at least one element selected from the group consisting of nickel, cobalt, palladium, lead, platinum, ruthenium, gold, silver, and copper, thereby insoluble and immobilizing the catalyst particles on the carrier.

[0095] Examples of soluble metal salts containing nickel include nickel nitrate, nickel acetate, nickel chloride, etc. Examples of soluble metal salts containing X include, for example, palladium chloride, palladium acetate, etc. when palladium is selected as X, ruthenium chloride, ruthenium nitrate, etc. when ruthenium is selected, chloroauric acid, sodium gold chloride, potassium dicyanoaurate, diethylamine gold trichloride, gold cyanide, etc. when gold is selected, and silver chloride, silver nitrate, etc. when silver is selected.

[0096] The concentration of each of the aqueous solutions containing nickel and / or cobalt and X is usually in the range of 0.0001 to 1.0 mol / L, preferably 0.001 to 0.5 mol / L, and more preferably 0.005 to 0.2 mol / L. The ratio of nickel or cobalt and X in the aqueous solution, expressed as the Ni / X atomic ratio or the Co / X atomic ratio, is preferably in the range of 0.1 to 10, more preferably 0.2 to 5.0, and further preferably 0.5 to 3.0.

[0097] The temperature when the carrier is contacted with the acidic aqueous solution is one of the important factors for controlling the distribution of catalyst particles, and although it varies depending on the amount of catalyst particles pre-loaded on the carrier, if the temperature is too low, the reaction slows down and the distribution of catalyst particles tends to spread. In the manufacturing method of this embodiment, from the viewpoint of obtaining a loading layer with sharper catalyst particles localized, the temperature when the carrier is contacted with the acidic aqueous solution is a temperature at which a high reaction rate can be obtained, and is preferably 60°C or higher, more preferably 70°C or higher, even more preferably 80°C or higher, and particularly preferably 90°C or higher. Since it is sufficient to mix the acidic aqueous solution and the water slurry so that the temperature of the mixed liquid is 60°C or higher, the water slurry may be heated to such an extent that the mixed liquid exceeds 60°C even when the acidic aqueous solution is added, or conversely, only the acidic aqueous solution may be heated. Both the acidic aqueous solution and the water slurry may be heated to 60°C or higher.

[0098] The reaction can be carried out under pressure at a temperature equal to or higher than the boiling point of the solution, but is usually preferably carried out at a temperature equal to or lower than the boiling point for ease of operation. The time required for immobilizing nickel and / or cobalt and the X component is not particularly limited, and varies depending on conditions such as the type of carrier, the amount and ratio of nickel and / or cobalt and X supported, but is usually within the range of 1 minute to 5 hours, preferably 5 minutes to 3 hours, and more preferably 5 minutes to 1 hour.

[0099] The method for producing a catalyst for producing a carboxylate ester according to the present embodiment may be carried out based on the principle of insoluble immobilization of nickel and / or cobalt and the X component by chemical reaction between an oxide of at least one basic metal selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals, which is preliminarily supported on a support, and a soluble metal salt containing nickel and / or cobalt and X. To obtain a more sufficient composite of nickel and / or cobalt and the X component, it is preferable to immobilize them simultaneously from a mixed aqueous solution of both components.

[0100] In addition, in the production method of this embodiment, the aqueous slurry containing a support carrying an oxide of at least one basic metal selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals preferably contains at least one basic metal salt selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals.

[0101] This makes it possible to suppress the generation of black metal of X, promote the composite of nickel and / or cobalt with X, and furthermore, to more precisely control the distribution of the composite particles. It is presumed that such effects are due to the fact that the addition of at least one metal salt selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals to the aqueous solution controls the rate of chemical reaction between the basic metal oxide pre-supported on the carrier, nickel and / or cobalt, and the soluble metal salt containing X.

[0102] As the at least one basic metal salt selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals, one or more selected from water-soluble salts such as inorganic salts, such as organic acid salts, nitrates, and chlorides of these metals can be used.

[0103] The amount of at least one basic metal salt selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals varies depending on the amount and ratio of nickel and / or cobalt and the X component, and is determined by the amount of basic metal oxide preliminarily supported on the support. It is usually 0.001 to 2 times by mol, preferably 0.005 to 1 times by mol, based on the amount of nickel and / or cobalt and the X component in the aqueous solution.

[0104] In addition, the aqueous slurry containing a support carrying an oxide of at least one basic metal selected from the group consisting of alkali metals, alkaline earth metals, and rare earth metals preferably contains a soluble aluminum salt, such as aluminum chloride or aluminum nitrate.

[0105] By adding a soluble aluminum salt to the water slurry, an outer layer that is substantially free of composite particles can be formed outside the support layer in which the composite particles are localized. This is also based on the above-mentioned principle of insoluble immobilization. As the soluble aluminum salt, soluble salts such as aluminum chloride and aluminum nitrate are used, and aluminum reacts with the basic metal oxide pre-supported on the support by chemical reaction, consuming the reaction field of nickel and / or cobalt with X, and further immobilizing the basic metal oxide, nickel and / or cobalt, and X component inside by reaction.

[0106] The amount of the aluminum component varies depending on the thickness of the layer not carrying nickel and / or cobalt and the X component, and is determined by the amount of the basic metal oxide previously carried on the support. It is usually 0.001 to 2 times by mol, preferably 0.005 to 1 times by mol, the amount of the basic metal oxide carried on the support.

[0107] Although many details remain unclear as to the mechanism by which the distribution of nickel and / or cobalt and the X component is achieved, it is presumed that the balance between the diffusion rate of nickel and / or cobalt and the X-containing soluble component in the carrier and the rate at which the component becomes insoluble through chemical reaction is well-balanced under the conditions of this embodiment, making it possible to fix the composite particles in a very narrow region near the surface of the carrier.

[0108] In addition, when an outer layer substantially not containing composite particles is formed on the outer surface of the carrier, aluminum is reacted with the basic metal component in the vicinity of the outer surface of the carrier to consume the basic metal component capable of reacting with nickel and / or cobalt and the X component in the vicinity of the outer surface of the carrier, and then nickel and / or cobalt and X are supported. Since the reactive basic metal component in the vicinity of the outer surface of the carrier has already been consumed, it is presumed that nickel and / or cobalt and X are immobilized by reacting with the basic metal oxide inside the carrier.

[0109] Next, the second step will be described. Prior to the heat treatment in the second step, the first precursor is washed with water and dried as necessary. The heating temperature of the first precursor is usually 40 to 900°C, preferably 80 to 800°C, more preferably 200 to 700°C, and further preferably 300 to 600°C.

[0110] The heat treatment is carried out in air (or atmospheric air), an oxidizing atmosphere (oxygen, ozone, nitrogen oxides, carbon dioxide, hydrogen peroxide, hypochlorous acid, inorganic / organic peroxides, etc.), or an inert gas atmosphere (helium, argon, nitrogen, etc.). The heating time may be appropriately selected depending on the heating temperature and the amount of the first precursor. The heat treatment may be carried out under normal pressure, elevated pressure, or reduced pressure.

[0111] After the second step described above, reduction treatment can be performed in a reducing atmosphere (hydrogen, hydrazine, formalin, formic acid, etc.) as necessary. In this case, a treatment method is selected that does not completely reduce the oxidized nickel and / or cobalt to the metallic state. The temperature and time of the reduction treatment can be appropriately selected depending on the type of reducing agent, the type of X, and the amount of catalyst.

[0112] Furthermore, after the above heat treatment or reduction treatment, an oxidation treatment can be carried out in air (or atmosphere) or in an oxidizing atmosphere (oxygen, ozone, nitrogen oxides, carbon dioxide, hydrogen peroxide, hypochlorous acid, inorganic or organic peroxides, etc.) as necessary. In this case, the temperature and time are appropriately selected depending on the type of oxidizing agent, the type of X, and the amount of catalyst.

[0113] The third component element other than nickel and / or cobalt and X can be added during preparation of the support or under reaction conditions. The alkali metal, alkaline earth metal, and rare earth metal can also be added during preparation of the catalyst or to the reaction system. The raw materials for the third component element, alkali metal, alkaline earth metal, and rare earth metal are selected from organic acid salts, inorganic acid salts, hydroxides, etc.

[0114] [Method of producing carboxylic acid ester] The catalyst for producing a carboxylate ester of the present embodiment can be widely used as a catalyst for chemical synthesis. For example, it can be used for a reaction for producing a carboxylate ester between an aldehyde and an alcohol, or for a reaction for producing a carboxylate ester from an alcohol. That is, the method for producing a carboxylate ester of the present embodiment can include a reaction step of reacting (a) an aldehyde and an alcohol, or (b) one or more alcohols, in the presence of the catalyst for producing a carboxylate ester of the present embodiment and oxygen.

[0115] The catalyst for producing carboxylate esters of this embodiment exerts excellent effects, particularly when used as a catalyst for oxidation reactions. In addition to the aldehydes and alcohols used in the reactions for producing carboxylate esters shown in the examples, various reaction substrates, such as alkanes, olefins, alcohols, ketones, aldehydes, ethers, aromatic compounds, phenols, sulfur compounds, phosphorus compounds, oxygen-containing nitrogen compounds, amines, carbon monoxide, and water, can be used as reaction substrates. These reaction substrates can be used alone or as a mixture of two or more kinds. From these reaction substrates, various industrially useful oxygen-containing compounds and oxidation products such as oxidized adducts and oxidized dehydrogenates can be obtained.

[0116] Specific examples of reaction substrates include alkanes, such as aliphatic alkanes such as methane, ethane, propane, n-butane, isobutane, n-pentane, n-hexane, 2-methylpentane, and 3-methylpentane; and alicyclic alkanes such as cyclopentane, cyclohexane, cycloheptane, and cyclooctane.

[0117] Examples of olefins include aliphatic olefins such as ethylene, propylene, butene, pentene, hexene, heptene, octene, decene, 3-methyl-1-butene, 2,3-dimethyl-1-butene, and allyl chloride; alicyclic olefins such as cyclopentene, cyclohexene, cycloheptene, cyclooctene, and cyclodecene; and aromatic substituted olefins such as styrene and α-methylstyrene.

[0118] Examples of the alcohol include saturated and unsaturated aliphatic alcohols such as methanol, ethanol, n-propanol, isopropanol, n-butanol, s-butanol, t-butanol, n-pentanol, n-hexanol, n-heptanol, allyl alcohol, and crotyl alcohol; saturated and unsaturated alicyclic alcohols such as cyclopentanol, cyclohexanol, cycloheptanol, methylcyclohexanol, and cyclohexen-1-ol; aliphatic and alicyclic polyhydric alcohols such as ethylene glycol, propylene glycol, trimethylene glycol, 1,3-butanediol, 1,2-cyclohexanediol, and 1,4-cyclohexanediol; and aromatic alcohols such as benzyl alcohol, salicylic alcohol, and benzhydrol.

[0119] Examples of aldehydes include aliphatic saturated aldehydes such as formaldehyde, acetaldehyde, propionaldehyde, isobutyraldehyde, and glyoxal; aliphatic α,β-unsaturated aldehydes such as acrolein, methacrolein, and crotonaldehyde; aromatic aldehydes such as benzaldehyde, tolylaldehyde, benzylaldehyde, and phthalaldehyde, and derivatives of these aldehydes.

[0120] Examples of ketones include aliphatic ketones such as acetone, methyl ethyl ketone, diethyl ketone, dipropyl ketone, and methyl propyl ketone; alicyclic ketones such as cyclopentanone, cyclohexanone, cyclooctanone, 2-methylcyclohexanone, and 2-ethylcyclohexanone; and aromatic ketones such as acetophenone, propiophenone, and benzophenone.

[0121] Examples of aromatic compounds include benzene, toluene, xylene, naphthalene, anthracene, and derivatives thereof substituted with alkyl groups, aryl groups, halogens, sulfone groups, and the like.

[0122] Examples of phenols include phenol, cresol, xylenol, naphthol, anthol (hydroxyanthracene), and derivatives thereof (wherein the hydrogen atom of the aromatic ring is substituted with an alkyl group, an aryl group, a halogen atom, a sulfonic acid group, or the like).

[0123] Examples of the sulfur compounds include mercaptans such as methyl mercaptan, ethyl mercaptan, propyl mercaptan, benzyl mercaptan, and thiophenol.

[0124] Examples of the amines include aliphatic amines such as methylamine, ethylamine, propylamine, isopropylamine, butylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, dibutylamine, trimethylamine, triethylamine, tripropylamine, tributylamine, allylamine, and diallylamine; alicyclic amines such as cyclopentylamine, cyclohexylamine, cycloheptylamine, and cyclooctylamine; and aromatic amines such as aniline, benzylamine, and toluidine.

[0125] These reaction substrates can be used alone or in the form of a mixture of two or more kinds. In addition, they do not necessarily need to be purified, and may be used in the form of a mixture with other organic compounds.

[0126] Hereinafter, a method for producing a carboxylic acid ester by oxidative esterification reaction from an aldehyde and an alcohol in the presence of oxygen using the catalyst for producing a carboxylic acid ester of the present embodiment will be described as an example.

[0127] The aldehydes used as raw materials include, for example, C1-C aldehydes such as formaldehyde, acetaldehyde, propionaldehyde, isobutyraldehyde, and glyoxal. 10 Aliphatic saturated aldehydes; C3-C such as acrolein, methacrolein, and crotonaldehyde 10 Aliphatic α-β-unsaturated aldehydes; C6-C such as benzaldehyde, tolylaldehyde, benzylaldehyde, and phthalaldehyde 20Examples of the aldehyde include aromatic aldehydes and derivatives of these aldehydes. These aldehydes can be used alone or in a mixture of any two or more kinds. In this embodiment, the aldehyde is preferably selected from acrolein, methacrolein, or a mixture thereof.

[0128] Examples of alcohols include C1-C ethanol, isopropanol, butanol, 2-ethylhexanol, and octanol. 10 Aliphatic saturated alcohols; C5-C such as cyclopentanol and cyclohexanol 10 Alicyclic alcohols; C2-C such as ethylene glycol, propylene glycol, butanediol 10 Diols; C3-C such as allyl alcohol and methallyl alcohol 10 Aliphatic unsaturated alcohols; C6-C such as benzyl alcohol 20 Aromatic alcohols; hydroxyoxetanes such as 3-alkyl-3-hydroxymethyloxetane. These alcohols can be used alone or in any mixture of two or more. In this embodiment, the aldehyde is preferably acrolein and / or methacrolein, and the alcohol is preferably methanol.

[0129] In this embodiment, from the viewpoint of further improving the reaction performance, the water content in the alcohol is preferably 10% by mass or less, more preferably 0.01% by mass or more and 10% by mass or less, still more preferably 7% by mass or less, even more preferably 5% by mass or less, and even more preferably 1% by mass or less. In addition, since it is preferable that the water content in the alcohol is small, the lower limit is not particularly limited. For example, the water content may be 0.01% by mass or a value smaller than this.

[0130] The ratio of the amounts of aldehyde and alcohol is not particularly limited and can be in a wide range, for example, an aldehyde / alcohol molar ratio of 10 to 1 / 1,000, but is generally in the range of 1 / 2 to 1 / 50.

[0131] The amount of the catalyst used can vary significantly depending on the type of reaction raw materials, the composition and preparation method of the catalyst, the reaction conditions, the reaction format, etc., and is not particularly limited. However, when the catalyst is reacted in a slurry state, the catalyst is used so that the solid concentration in the slurry is preferably within the range of 1 to 50 mass / volume%, more preferably 3 to 30 mass / volume%, and even more preferably 10 to 25 mass / volume%.

[0132] The production of the carboxylic acid ester can be carried out by any method such as a gas phase reaction, a liquid phase reaction, or a flood reaction, either batchwise or continuously, but the reaction step is preferably carried out in the liquid phase.

[0133] The reaction can be carried out without a solvent, but can also be carried out using a solvent inert to the reactants, such as hexane, decane, benzene, dioxane, and the like.

[0134] The reaction may be carried out in a conventional manner such as a fixed bed, a fluidized bed, a stirred tank, etc. For example, when the reaction is carried out in a liquid phase, any reactor type such as a bubble column reactor, a draft tube reactor, a stirred tank reactor, etc. may be used.

[0135] The oxygen used in the production of a carboxylate ester can be in the form of molecular oxygen, i.e., oxygen gas itself or a mixed gas obtained by diluting oxygen gas with a diluent inert to the reaction, such as nitrogen or carbon dioxide gas. From the viewpoints of operability, economy, etc., air is preferably used as the oxygen source.

[0136] The oxygen partial pressure varies depending on the reaction raw materials such as aldehyde species and alcohol species, the reaction conditions, the reactor type, etc., but in practice, the oxygen partial pressure at the reactor outlet is in a range where the concentration is below the lower limit of the explosion range, and is preferably controlled to, for example, 20 to 80 kPa. The reaction pressure can be carried out at any wide pressure range from reduced pressure to pressurized pressure, but is usually carried out at a pressure in the range of 0.05 to 2 MPa. In addition, from the viewpoint of safety, it is preferable to set the total pressure so that the oxygen concentration of the reactor outflow gas does not exceed the explosion limit (for example, oxygen concentration 8%).

[0137] In this embodiment, the reaction step is preferably carried out while adding a basic substance so that the pH of the reaction system is 6 or more and 8 or less. Examples of the basic substance include compounds of alkali metals or alkaline earth metals (e.g., oxides, hydroxides, carbonates, and carboxylates). These compounds of alkali metals or alkaline earth metals can be used alone or in combination of two or more kinds.

[0138] The reaction temperature for producing a carboxylate ester can be as high as 200° C. or higher, but is preferably 30 to 200° C., more preferably 40 to 150° C., and further preferably 60 to 120° C. The reaction time is not particularly limited and cannot be uniquely determined since it varies depending on the conditions set, but is usually 1 to 20 hours. EXAMPLES

[0139] The present embodiment will be described in more detail below with reference to examples, but the present embodiment is not limited to these examples.

[0140] In the following examples and comparative examples, measurement of the distribution of nickel and X in the composite particle support, observation of the shapes of the support and the composite particle support, measurement of the average particle size, determination of the amounts of Ni and X supported and the Ni / (Ni+X) atomic ratio, determination of the contents of the support component elements (Si, Al, basic metals), analysis of the crystal structure of the composite particles, analysis of the chemical state of the metal components of the composite particles, analysis of the chemical state of nickel, observation of the morphology and elemental analysis of the composite particles, measurement of the ultraviolet-visible spectrum of the composite particles, and measurement of the physical properties of the support and the composite particle support (specific surface area, pore diameter, pore volume) were performed by the following methods.

[0141] [Measurement of nickel and X distribution in composite particle supports] The composite particle support was embedded in resin and polished to obtain a sample, which was then measured using a Shimadzu 1600-type X-ray microprobe (EPMA) at an accelerating voltage of 15 kV. Analysis of the depth direction from the outer surface of Ni and X(Au) was performed using backscattered electron images and line analysis (Ni: wavelength 14.5829, RAP analyzing crystal; X(Au): wavelength 5.8419, PET analyzing crystal).

[0142] [Observation of the shape of carriers and composite particle supports] The carrier and the composite particle-loaded material were observed using a Hitachi X-650 scanning electron microscope (SEM).

[0143] [Measurement of the average particle size of carriers and composite particle supports] The average particle size (volume basis) was measured using a Beckman Coulter LS230 laser diffraction / scattering particle size distribution analyzer.

[0144] [Determination of Ni and X loading amount and Ni / X atomic ratio] The concentrations of nickel and X in the composite particle support were quantified using an IRIS Intrepid II XDL type ICP atomic emission spectrometer (ICP-AES, MS) manufactured by Thermo Fisher Scientific. The sample was prepared by weighing the support into a Teflon decomposition vessel, adding nitric acid and hydrogen fluoride, and decomposing by heating using a Milestone General ETHOS TC microwave decomposition apparatus. The mixture was then evaporated to dryness on a heater, and nitric acid and hydrochloric acid were added to the precipitated residue, which was then decomposed under pressure using the microwave decomposition apparatus. The decomposition liquid thus obtained was pure and of a constant volume, and used as the test liquid. The quantitative determination was performed by the internal standard method using ICP-AES, and the nickel and X contents in the catalyst were obtained by subtracting the blank value obtained at the same time, and the supported amount and atomic ratio were calculated.

[0145] [Determination of the content of carrier component elements (Si, Al, basic metals)] A sample was prepared by dissolving the support in aqua regia and a sample was prepared by dissolving the support in an alkaline molten salt. Using a JY-38P2 ICP atomic emission spectrometer (ICP-AES) manufactured by Seiko Electronic Industries Co., Ltd., the basic metal and / or Mg content was measured in the sample dissolved in aqua regia, and the Al and Si contents were measured in the sample dissolved in an alkaline molten salt, and the atomic ratio was calculated from the obtained metal contents.

[0146] [Analysis of the crystal structure of composite particles] The measurements were performed using a Rigaku Rint2500 powder X-ray diffractometer (XRD) with a Cu X-ray source (40 kV, 200 mA), a measurement range of 5 to 65 deg (0.02 deg / step), a measurement speed of 0.2 deg / min, and slit widths (scattering, diverging, receiving) of 1 deg, 1 deg, and 0.15 mm. The sample was uniformly spread on a non-reflective sample plate and fixed with neoprene rubber.

[0147] [Analysis of the chemical state of metal components in composite particles] The measurements were performed using a Thermo Electron ESCALAB250 X-ray photoelectron spectrometer (XPS) under the following conditions: excitation source AlKα 15 kV × 10 mA, analysis area approximately 1 mm (shape: ellipse), capture region: survey scan 0 to 1,100 eV, narrow scan Ni2p. The measurement sample was prepared by grinding the composite particle-supported material in an agate mortar, collecting it on a powder sample stage, and subjecting it to XPS measurement.

[0148] [Chemical state analysis of nickel] The NiKα spectrum was measured using a Technos XFRA190 double crystal high resolution X-ray fluorescence analyzer (HRXRF), and the various parameters obtained were compared with those of standard substances (nickel metal, nickel oxide) to infer the chemical state of nickel in the support, such as its valence. The measurement samples were used as they were. The Ni Kα spectrum was measured in partial spectrum mode. A Ge(220) crystal was used, and the slit had a vertical divergence angle of 1°. The excitation voltage and current were set to 35 kV and 80 mA, respectively. Filter paper was used as an absorber for the standard sample, and the counting time for the support sample was selected for each sample so that the peak intensity of the Kα spectrum was 3,000 cps or less and 10,000 counts or more. Each sample was measured five times, and the metal sample was measured before and after the repeated measurements. After smoothing the measured spectrum (SG method 7 points - 5 times), the peak position, full width at half maximum (FWHM), and asymmetry coefficient (AI) were calculated, and the peak position was treated as the deviation from the measured value of the metal sample measured before and after the sample measurement, i.e., the chemical shift (ΔE).

[0149] [Morphological observation and elemental analysis of composite particles] A JEOL 3100FEF transmission electron microscope / scanning transmission electron microscope (TEM / STEM) [accelerating voltage 300 kV, energy dispersive X-ray detector (EDX) attached] was used to measure TEM bright-field images, STEM dark-field images, and STEM-EDS compositional analysis (point analysis, mapping, line analysis). Data analysis software: TEM image, STEM image analysis (length measurement, Fourier transform analysis): DigitalMicrograph TM Ver.1.70.16, Gatan; EDS data analysis (mapping image processing, quantitative composition calculation): NORAN System SIX ver.2.0, Thermo Fisher Scientific was used. The measurement sample was prepared by crushing the composite particle support in a mortar, dispersing it in ethanol, and ultrasonically cleaning it for about 1 minute. The resultant was then dropped and blown onto a Mo microgrid to prepare a sample for TEM / STEM observation.

[0150] [UV-Visible Spectroscopic Measurement of Composite Particles] The measurements were performed using a JASCO V-550 ultraviolet-visible spectrophotometer (UV-Vis) [integrating sphere unit, powder sample holder included] with a measurement range of 800-200 nm and a scanning speed of 400 nm / min. The measurement sample was prepared by grinding the composite particle-supported material in an agate mortar, placing it in a powder sample holder, and subjecting it to UV-Vis measurement.

[0151] [Half-width Wa and mode diameter Da of the catalyst pore distribution, and half-width Wd and mode diameter Dd] The pore size was measured using Quantachrome's Quadrasorb evo with nitrogen as the adsorption gas (nitrogen adsorption method). In the "He measure" mode, the reference cell and 9mm Large bulb included with the Quadrasorb evo were used as sample cells, and free space measurements were performed using pure helium. The samples were dried at 200°C for 18 hours under reduced pressure to remove moisture. The sample weight was 0.1 g. The measurement points were relative pressures (P / P0) of 0.025 to 0.9875 for adsorption and 0.975 to 0.025 for desorption. The pore distribution was calculated for both adsorption and desorption using the BJH method. For both adsorption and desorption, the pore diameter (D) and the cumulative pore volume (V) differentiated by the common logarithm of the pore diameter (D) (dV / d(logD)) were plotted. For example, in Figure 3, the pore diameters at peak top A were the mode diameters Da and Dd, and a horizontal line was drawn at point B, where a perpendicular line was drawn from the peak top and the line segment AC intersecting the baseline was bisected, and the lengths of the intersection points D and E with the pore distribution were the half-widths Wa and Wd.

[0152] Example 1 An aqueous solution of 18.75 parts by mass of aluminum nitrate 9 hydrate, 12.8 parts by mass of magnesium nitrate, and 2.7 parts by mass of 60% by mass nitric acid dissolved in 25 parts by mass of pure water was gradually dropped into 100 parts by mass of silica sol solution (SiO2 content 30% by mass) with colloidal particle diameter of 10 to 20 nm in a stirred state maintained at 15 ° C., and a mixed slurry of silica sol, aluminum nitrate, and magnesium nitrate was obtained. After that, the mixed slurry was maintained at 80 ° C. for 5 hours, cooled to 30 ° C., stirred for 5 hours, and then further heated to 50 ° C. and maintained for 10 hours, during which stirring was continued with a paddle-type stirring blade with a stirring blade diameter of 0.5 m at a stirring tip speed of 6.5 m / s. After cooling to room temperature, it was spray-dried with a spray dryer device set at an outlet temperature of 130 ° C. to obtain a solid. The solid obtained was then packed in an open-top stainless steel container to a depth of about 1 cm, and heated in an electric furnace from room temperature to 300°C over 2 hours, after which it was held for 3 hours. The temperature was then raised to 600°C over 2 hours, after which it was held for 3 hours and slowly cooled to obtain a carrier. The obtained carrier contained 83.3 mol %, 8.3 mol %, and 8.3 mol % of silicon, aluminum, and magnesium, respectively, based on the total molar amounts of silicon, aluminum, and magnesium. The specific surface area measured by the nitrogen adsorption method was 149 m 2 The molecular weight of the carrier was 1.01g / g, the pore volume was 0.27mL / g, and the average pore diameter was 7nm. The average particle diameter of the carrier was 60μm based on the results of particle size distribution measurement using a laser scattering method. Furthermore, observation with a scanning electron microscope (SEM) showed that the shape of the carrier was almost spherical.

[0153] 300 g of the carrier obtained as described above was poured into 1.0 L of water heated to 90° C. over a period of 1 minute, dispersed, and stirred at 90° C. for 15 minutes. Next, an aqueous solution containing 16.35 g of nickel nitrate hexahydrate and 12 mL of a 1.3 mol / L aqueous solution of chloroauric acid was prepared and heated to 90° C. This was added to the carrier slurry, and stirring was continued for an additional 30 minutes at 90° C. to insoluble and immobilize the nickel and gold components on the carrier. The mixture was then left to stand to remove the supernatant, washed several times with distilled water, and filtered. The mixture was dried in a dryer at 105°C for 10 hours, and then calcined in a muffle furnace in air at 450°C for 5 hours to obtain a catalyst for producing carboxylic acid esters (NiOAu / SiO2-Al2O3-MgO composite particle support) carrying 1.05% by mass of nickel and 0.91% by mass of gold. The Ni / Au atomic ratio in the composite particles contained in the obtained catalyst for producing carboxylic acid esters was 4.0.

[0154] (Evaluation of the physical properties of catalysts for the production of carboxylic acid esters) The specific surface area of ​​the resulting catalyst for producing carboxylic acid esters was found to be 141 m 2 The pore size distribution was also obtained, and the half width of the pore size distribution for adsorption was 5 nm, and the half width of the pore size distribution for desorption was 2 nm. Next, the obtained catalyst for producing a carboxylic acid ester was embedded in a resin and polished to obtain a sample, which was subjected to line analysis of the particle cross section using an X-ray microprobe (EPMA). It was confirmed that the support had an outer layer that was substantially free of nickel and gold in a region 0.5 μm deep from the outermost surface, nickel and gold were supported in a region up to a depth of 10 μm from the surface, and no composite particles were present inside the support. Next, the morphology of the catalyst for producing carboxylic acid esters was observed by a transmission electron microscope (TEM / STEM), and it was confirmed that spherical nanoparticles with a maximum distribution of 2-3 nm particles (number average particle size: 3.0 nm) were supported on the carrier. Further magnification of the nanoparticles revealed that the nanoparticles had lattice fringes corresponding to the interplanar spacing of Au(111). When composition point analysis was performed on each nanoparticle by STEM-EDS, nickel and gold were detected in each particle. The average nickel / gold atomic ratio of the nanoparticles (calculated number: 50) was 1.05. Further nano-area analysis of the observed particles revealed that the Ni / Au atomic ratio in the center of the particle was 0.90 and that in the particle edge was 2.56. Only a small amount of nickel was detected in the area other than the particle. Similar measurements were performed at 50 points, and a large amount of nickel was detected around the edge of each particle. From EDS element mapping, it was observed that the distribution of nickel and gold was almost the same. Furthermore, the composition line profile showed that nickel was distributed in a larger area than gold in both scanning directions. Powder X-ray diffraction (XRD) results showed that no diffraction pattern originating from nickel was observed, confirming that it exists in an amorphous state. However, although the peak was not clearly defined, a broad peak corresponding to gold crystals was present. Although this was close to the detection limit of powder X-ray diffraction (2 nm), the average crystallite diameter calculated using Scherrer's formula was approximately 3 nm. Regarding the chemical state of nickel, the results of X-ray photoelectron spectroscopy (XPS) confirmed that nickel was divalent. From the results of double crystal high resolution X-ray fluorescence spectrometry (HRXRF), the chemical state of nickel was estimated to be high spin divalent nickel, and the difference in the NiKα spectrum revealed that this was a different chemical state from nickel oxide, which is a single compound. The full width at half maximum (FWHM) of the NiKα spectrum of the catalyst obtained from the measured spectrum was 3.470, and the chemical shift (ΔE) was 0.335. The full width at half maximum (FWHM) of the NiKα spectrum of nickel oxide measured as a standard substance was 3.249, and the chemical shift (ΔE) was 0.344. In addition, when the changes in the electronic excitation state of this catalyst for producing carboxylic acid esters were examined using ultraviolet-visible spectroscopy (UV-Vis), it was found that no surface plasmon absorption peak originating from gold nanoparticles appeared near 530 nm, but a broad absorption due to NiO2 was observed in the wavelength range of 200 to 800 nm. From the above results, it is inferred that the microstructure of the composite particles has a morphology in which gold nanoparticles serve as cores, the surfaces of which are covered with oxidized nickel.

[0155] (Production of Carboxylic Acid Esters) 240 g of the obtained catalyst for producing carboxylate ester was charged into a stirred stainless steel reactor equipped with a catalyst separator and a liquid phase of 1.2 liters, and an oxidative reaction of producing carboxylate ester from aldehyde and alcohol was carried out while stirring the contents at a tip speed of 4 m / s of the stirring blade. A 36.7 mass% methacrolein / methanol solution (a methanol solution with a water content of 0.50 mass% was used) was continuously supplied to the reactor at 0.6 liters / hr, and a 1-4 mass% NaOH / methanol solution was continuously supplied to the reactor at 0.06 liters / hr. Air was blown in so that the outlet oxygen concentration was 4.0 volume% (corresponding to an oxygen partial pressure of 0.02 MPa) at a reaction temperature of 80°C and a reaction pressure of 0.5 MPa, and the NaOH concentration supplied to the reactor was controlled so that the pH of the reaction system was 7. The reaction product was continuously extracted from the reactor outlet by overflow and analyzed by gas chromatography to examine the reactivity. The methacrolein conversion rate after 500 hours from the start of the reaction was 75.2%, and the selectivity for methyl methacrylate was 98.1%.

[0156] (Durability test) Next, in order to evaluate the acid resistance, base resistance, and temperature resistance of the catalyst for producing carboxylic acid ester, a durability test was performed by the following method. 10 g of the unused catalyst for producing carboxylic acid ester obtained as described above was added to 100 mL of a buffer solution of pH 4 in a glass container, and the mixture was stirred at 90 ° C for 10 minutes, then left to stand to remove the supernatant, washed with water, and decanted. The solid thus obtained was added to 100 mL of a buffer solution of pH 10 in a glass container, and the mixture was stirred at 90 ° C for 10 minutes, then left to stand to remove the supernatant, washed with water, and decanted. The above operations constitute one cycle, and a total of 100 cycles of treatment were performed. The half-width of the pore distribution of the catalyst for producing carboxylic acid ester after this durability test was determined in the same manner as described above. Furthermore, the entire amount of the catalyst for producing carboxylic acid ester after the durability test was used to produce carboxylic acid ester for 500 hours in the same manner as described above, and the methacrolein conversion rate and methyl methacrylate selectivity were determined. These results are also shown in Table 1.

[0157] Comparative Example 1 A catalyst for producing a carboxylate ester was obtained in the same manner as in Example 1, except that the stirring conditions of the mixed slurry before spray drying with a spray dryer were changed to stirring with an anchor-type stirring blade having a stirring blade diameter of 0.2 m at a stirring tip speed of 1.3 m / s (100 rpm), and the hydrothermal synthesis conditions during carrier preparation were changed to the conditions shown in the table. The above-mentioned durability test was carried out on the catalyst for producing a carboxylate ester, and the pore distribution half width, methacrolein conversion rate, and methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0158] Example 2 (Production of catalyst for producing carboxylic acid ester) 300 g of the carrier obtained in Example 1 was poured into 1.0 L of water heated to 90° C. over a period of 1 minute, dispersed, and stirred at 90° C. for 15 minutes. Next, an aqueous solution containing 16.36 g of cobalt nitrate hexahydrate and 12 mL of a 1.3 mol / L aqueous solution of chloroauric acid was prepared and heated to 90° C. This was added to the carrier slurry, and stirring was continued for an additional 30 minutes at 90° C. to insoluble and immobilize the cobalt and gold components on the carrier. The mixture was then left to stand to remove the supernatant, washed several times with distilled water, and filtered. The mixture was dried in a dryer at 105°C for 10 hours, and then calcined in a muffle furnace in air at 450°C for 5 hours to obtain a catalyst for producing carboxylic acid esters (CoOAu / SiO2-Al2O3-MgO composite particle support) carrying 1.05% cobalt and 0.91% gold by mass. The Co / Au atomic ratio of the obtained catalyst for producing carboxylic acid esters was 4.0.

[0159] (Evaluation of the physical properties of catalysts for the production of carboxylic acid esters) The specific surface area of ​​the resulting catalyst for producing carboxylic acid esters was found to be 139 m 2 The pore size distribution was also obtained, and the half-width of the pore size distribution for adsorption (Wa) was 5 nm, and the half-width of the pore size distribution for desorption (Wd) was 3 nm.

[0160] (Production of Carboxylic Acid Esters) 240 g of the obtained catalyst for producing carboxylate ester was charged into a stirred stainless steel reactor equipped with a catalyst separator and a liquid phase of 1.2 liters, and an oxidative reaction of producing carboxylate ester from aldehyde and alcohol was carried out while stirring the contents at a tip speed of 4 m / s of the stirring blade. A 36.7 mass% methacrolein / methanol solution (a methanol solution with a water content of 0.50 mass% was used) was continuously supplied to the reactor at 0.6 liters / hr, and a 1-4 mass% NaOH / methanol solution was continuously supplied to the reactor at 0.06 liters / hr. Air was blown in so that the outlet oxygen concentration was 4.0 volume% (corresponding to an oxygen partial pressure of 0.02 MPa) at a reaction temperature of 80°C and a reaction pressure of 0.5 MPa, and the NaOH concentration supplied to the reactor was controlled so that the pH of the reaction system was 7. The reaction product was continuously extracted from the reactor outlet by overflow and analyzed by gas chromatography to examine the reactivity. 500 hours after the start of the reaction, the methacrolein conversion was 74.5%, and the selectivity for methyl methacrylate was 97.8%.

[0161] Next, a durability test was carried out by the method described in Example 1. The results are shown in Table 1.

[0162] Example 3 A carrier was obtained in the same manner as in Example 1, except that the mixed slurry before spray drying with a spray dryer was stirred at a stirring tip speed of 6.5 m / s using a turbine-type stirring blade with a stirring blade diameter of 0.5 m. Then, 300 g of the carrier was poured into 1.0 L of water heated to 90° C. over 1 minute, dispersed, and stirred at 90° C. for 30 minutes, and a catalyst for producing a carboxylic acid ester was obtained in the same manner as in Example 1. The above-mentioned durability test was carried out on the catalyst for producing a carboxylic acid ester, and the pore distribution half-width, methacrolein conversion rate, and methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0163] Example 4 A catalyst for producing a carboxylate ester was obtained in the same manner as in Example 1, except that 300 g of the carrier obtained in Example 1 was added over 1 minute to 1.0 L of water heated to 90° C., dispersed, and stirred at 90° C. for 10 minutes. The above-mentioned durability test was carried out on the catalyst for producing a carboxylate ester, and the half-width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0164] Comparative Example 2 A carrier was obtained in the same manner as in Comparative Example 1, and then a catalyst for producing a carboxylic acid ester was obtained in the same manner as in Example 2. The above-mentioned durability test was carried out on the catalyst for producing a carboxylic acid ester, and the half-width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0165] Comparative Example 3 A catalyst for producing a carboxylic acid ester was obtained in the same manner as in Example 3, except that 300 g of the carrier obtained in Comparative Example 1 was added over 1 minute to 1.0 L of water heated to 90° C., dispersed, and stirred at 90° C. for 30 minutes, and the catalyst for producing a carboxylic acid ester was obtained. The above-mentioned durability test was carried out on the catalyst for producing a carboxylic acid ester, and the half-width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0166] Example 5 An aqueous solution of aluminum nitrate, magnesium nitrate, and 2.7 parts by mass of 60% nitric acid dissolved in 25 parts by mass of pure water was gradually dropped into 100 parts by mass of silica sol solution (SiO2 content 30% by mass) with a colloidal particle diameter of 10 to 20 nm in a stirred state maintained at 15 ° C., so that aluminum and magnesium contained in the carrier were 36.6 mol % and 17.2 mol %, respectively, relative to the total molar amount of silicon, aluminum, and magnesium, to obtain a mixed slurry of silica sol, aluminum nitrate, and magnesium nitrate. After that, the mixed slurry was held at 80 ° C. for 5 hours, cooled to 30 ° C., stirred for 5 hours, and then further heated to 50 ° C. and held for 10 hours, during which stirring was continued with a paddle-type stirring blade with a stirring blade diameter of 0.5 m at a stirring tip speed of 6.5 m / s. After cooling to room temperature, it was spray-dried with a spray dryer device set at an outlet temperature of 130 ° C. to obtain a solid. The solid obtained was then packed to a thickness of about 1 cm into an open-topped stainless steel container, and heated in an electric furnace from room temperature to 300°C over two hours, after which it was held for three hours. The temperature was then raised to 800°C over two hours, after which it was held for three hours and then slowly cooled to obtain a carrier. The average particle size of the carrier was 64 μm, as determined by particle size distribution measurement using a laser scattering method. Furthermore, observation with a scanning electron microscope (SEM) showed that the shape of the carrier was nearly spherical. 300 g of the carrier obtained as described above was poured into 1.0 L of water heated to 85° C. over a period of 3 minutes, dispersed, and stirred at 85° C. for 10 minutes. Next, an aqueous solution containing 16.35 g of nickel nitrate hexahydrate and 13 mL of a 1.3 mol / L aqueous solution of chloroauric acid was prepared, heated to 85°C, and added to the above slurry. Stirring was continued at 85°C for an additional 30 minutes to precipitate nickel and gold components onto the support. The mixture was then left to stand to remove the supernatant, washed several times with distilled water, and filtered. This was dried at 105°C for 16 hours, and then calcined in air at 500°C for 3 hours to obtain a catalyst (NiOAu / SiO2-Al2O3-MgO) for producing carboxylic acid esters that supported 1.0% by mass of nickel and 0.90% by mass of gold. The Ni / Au atomic ratio in the composite particles contained in the obtained catalyst for producing carboxylic acid esters was 3.7. The average particle size of the catalyst was 65 μm based on the results of particle size distribution measurement using a laser scattering method. Observation with a scanning electron microscope (SEM) showed that the shape of the catalyst was almost spherical. Wa was 6 nm and Wd was 7 nm. When the morphology of the active species of this catalyst was observed with a transmission electron microscope (TEM / STEM), it was confirmed that nanoparticles with a maximum particle size distribution of 2 to 3 nm (number average particle size: 3.3 nm) were supported on the carrier. The above-mentioned durability test was carried out on the catalyst for producing a carboxylate ester, and the half width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0167] Example 6 300 g of the carrier obtained in Example 1 was poured into 1.0 L of water heated to 90 ° C. over 1 minute, dispersed, and stirred at 90 ° C. for 15 minutes. The temperature was then lowered to 60 ° C., and while stirring, a dilute hydrochloric acid solution of palladium chloride and an aqueous lead nitrate solution in amounts equivalent to 2.5 mass % as Pd and Pb, respectively, were quickly dropped. Then, the mixture was held at 60 ° C. for 1 hour, and 1.2 times the stoichiometric amount of hydrazine was added thereto for reduction. Next, the mixture was left to stand, the supernatant was removed, and the mixture was washed several times with distilled water, and then filtered. The mixture was further vacuum dried at 60 ° C. to obtain a catalyst for producing carboxylic acid esters (PdPb / SiO2-Al2O3-MgO composite particle support) carrying 2.5 mass % of Pd and Pb, respectively. According to the results of powder X-ray diffraction (XRD) of the above-mentioned precious metal-supported material, diffraction peaks (2θ=38.6°, 44.8°, 65.4°, 78.6°) attributed to the intermetallic compound Pd3Pb1 were observed. The above-mentioned durability test was carried out on the catalyst for producing a carboxylate ester, and the half width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0168] Comparative Example 4 A catalyst for producing a carboxylate ester was obtained in the same manner as in Example 6, except that the stirring conditions of the mixed slurry before spray drying with a spray dryer were changed to stirring with an anchor-type stirring blade having a stirring blade diameter of 0.2 m at a stirring tip speed of 1.3 m / s, and the hydrothermal synthesis conditions during carrier preparation were changed to the conditions shown in the table. The above-mentioned durability test was carried out on the catalyst for producing a carboxylate ester, and the pore distribution half width, methacrolein conversion rate, and methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0169] Example 7 A catalyst for producing a carboxylic acid ester was obtained in the same manner as in Example 6, except that 300 g of the carrier obtained in Example 1 was added over 3 minutes to 1.0 L of water heated to 90° C., dispersed, and stirred at 85° C. for 10 minutes, and then the temperature was lowered to 60° C. The above-mentioned durability test was carried out on the catalyst for producing a carboxylic acid ester, and the half-width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0170] Example 8 A catalyst for producing a carboxylate ester was obtained in the same manner as in Example 1, except that the hydrothermal synthesis conditions in the preparation of the carrier were changed to those shown in the table. The above-mentioned durability test was carried out on the catalyst for producing a carboxylate ester, and the half-width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0171] Example 9 A catalyst for producing a carboxylic acid ester was obtained in the same manner as in Example 8, except that the stirring conditions of the mixed slurry before spray drying with a spray dryer apparatus were changed to a stirring tip speed of 10.2 m / s. The above-mentioned durability test was carried out on the catalyst for producing a carboxylic acid ester, and the half-width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0172] Example 10 A catalyst for producing a carboxylate ester was obtained in the same manner as in Example 8, except that the stirring conditions of the mixed slurry before spray drying with a spray dryer were such that the stirring was performed with a turbine-type stirring blade having a stirring blade diameter of 0.5 m at a stirring tip speed of 6.5 m / s. The above-mentioned durability test was performed on the catalyst for producing a carboxylate ester, and the pore distribution half width, methacrolein conversion rate, and methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0173] Example 11 An aqueous solution was prepared by dissolving 1.5 parts by mass of aluminum nitrate nonahydrate, 0.24 parts by mass of nickel nitrate hexahydrate, 0.98 parts by mass of magnesium nitrate hexahydrate, and 0.27 parts by mass of 60% by mass nitric acid in 3.0 parts by mass of pure water. The aqueous solution was gradually added dropwise to 100 parts by mass of a silica sol solution (SiO2 content: 30% by mass) having a colloidal particle diameter of 10 to 20 nm and kept at 15°C under stirring to obtain a mixed slurry of silica sol, aluminum nitrate, nickel nitrate, and magnesium nitrate. A silica-containing carrier was obtained in the same manner as in Example 1, except that the aqueous solution was gradually added dropwise to 100 parts by mass of a silica sol solution (SiO2 content: 30% by mass) having a colloidal particle diameter of 10 to 20 nm and kept at 15°C under stirring to obtain a mixed slurry of silica sol, aluminum nitrate, nickel nitrate, and magnesium nitrate. The obtained silica-containing carrier contained 85.3 mol % of silicon, 6.8 mol % of aluminum, 1.4 mol % of nickel, and 6.5 mol % of magnesium based on the total molar amounts of silicon, aluminum, nickel, and magnesium. Using the silica-containing carrier, a catalyst for producing a carboxylic acid ester (NiOAu / SiO2-Al2O3-NiO-MgO composite particle support) was obtained in the same manner as in Example 1. The Ni / Au atomic ratio in the composite particles contained in the obtained catalyst for producing a carboxylic acid ester was 4.0. The above-mentioned durability test was carried out on the catalyst for producing a carboxylate ester, and the half width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0174] Example 12 A catalyst for producing a carboxylate ester was obtained in the same manner as in Example 1, except that 300 g of the carrier obtained in Example 1 was added to 1.0 L of water heated to 95° C. over a period of 3 minutes, dispersed, and stirred at 95° C. for 15 minutes, and the catalyst for producing a carboxylate ester was subjected to the above-mentioned durability test, and the half-width of the pore distribution, the methacrolein conversion rate, and the methyl methacrylate selectivity before and after the test were determined in the same manner as in Example 1. These results are shown in Table 1.

[0175] [Table 1-1]

[0176] [Table 1-2]

[0177] [Table 1-3]

Claims

1. Catalyst particles containing at least one element selected from the group consisting of nickel, cobalt, palladium, lead, platinum, ruthenium, gold, silver, and copper; A carrier that supports the catalyst particles; A catalyst for producing a carboxylic acid ester, comprising: The catalyst for producing a carboxylic acid ester has a half-width Wa of a pore distribution of 10 nm or less, as calculated by the BJH method from an adsorption isotherm obtained by a nitrogen adsorption method.

2. 2. The catalyst for producing a carboxylic acid ester according to claim 1, wherein the half-width Wd of the pore distribution calculated by the BJH method from a desorption isotherm obtained by a nitrogen adsorption method for the catalyst for producing a carboxylic acid ester is 5 nm or less.

3. 3. The catalyst for producing a carboxylic acid ester according to claim 1 or 2, wherein a mode diameter Da of pores calculated by the BJH method from an adsorption isotherm obtained by a nitrogen adsorption method of the catalyst for producing a carboxylic acid ester is 2 nm or more and 20 nm or less.

4. The catalyst for producing a carboxylate ester according to any one of claims 1 to 3, wherein a mode diameter Da of pores and the half width Wa of pores calculated by the BJH method from an adsorption isotherm obtained by a nitrogen adsorption method for the catalyst for producing a carboxylate ester satisfy the relationship of the following formula (1): 1 / 2 Wa < Da (1)

5. The catalyst for producing a carboxylate ester according to any one of claims 1 to 4, wherein a mode diameter Dd of pores, calculated by using the BJH method from a desorption isotherm obtained by a nitrogen adsorption method, is 2 nm or more and 15 nm or less.

6. The catalyst for producing a carboxylate ester according to any one of claims 1 to 5, wherein a pore mode diameter Dd calculated by the BJH method from a desorption isotherm of the catalyst for producing a carboxylate ester obtained by a nitrogen adsorption method, and a half-width Wd of a pore distribution calculated by the BJH method from a desorption isotherm of the catalyst for producing a carboxylate ester obtained by a nitrogen adsorption method satisfy the relationship of the following formula (2): 1 / 2Wd < Dd (2)

7. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 6, wherein the half width Wa is 0.1 nm or more.

8. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 7, wherein the catalyst particles contain at least one element selected from the group consisting of nickel, cobalt, palladium, lead, and gold.

9. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 8, wherein the catalyst particles are composite particles containing oxidized nickel and / or cobalt and X (X represents at least one element selected from the group consisting of nickel, palladium, platinum, ruthenium, gold, silver, and copper).

10. 10. The catalyst for producing a carboxylic acid ester according to claim 9, wherein a composition ratio of nickel or cobalt to X in the composite particle is from 0.1 to 10 in terms of an Ni / X atomic ratio or a Co / X atomic ratio.

11. The catalyst for producing a carboxylic acid ester according to claim 9 , wherein the composite particles contain nickel in an oxidized state and gold.

12. The catalyst for producing a carboxylic acid ester according to claim 10, wherein a composition ratio of nickel to gold in the composite particle is 1.1 or more and 10 or less in terms of an Ni / Au atomic ratio.

13. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 12, wherein the catalyst particles have an average particle size of 2 nm or more and 10 nm or less.

14. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 13, wherein the support is made of an aluminum-containing silica-based composition containing silica and alumina.

15. The carrier is Silicon, Aluminum and At least one Period 4 element selected from the group consisting of iron, cobalt, nickel, and zinc; at least one basic element selected from the group consisting of alkali metal elements, alkaline earth metal elements, and rare earth elements; in the ranges of 42 mol % or more and 90 mol % or less, 3 mol % or more and 38 mol % or less, 0.5 mol % or more and 2 mol % or less, and 2 mol % or more and 38 mol % or less, respectively, relative to the total molar amount of the silicon, the aluminum, the fourth periodic element, and the basic element.

16. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 15, wherein the support layer in which the catalyst particles are localized is present in a region from a surface of the catalyst for producing a carboxylic acid ester to 40% of an equivalent diameter of the catalyst for producing a carboxylic acid ester.

17. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 16, wherein the equivalent diameter of the catalyst for producing a carboxylic acid ester is 200 µm or less, and the support layer in which the catalyst particles are localized is present in an area ranging from a surface of the catalyst for producing a carboxylic acid ester to 30% of the equivalent diameter of the catalyst for producing a carboxylic acid ester.

18. The catalyst for producing a carboxylic acid ester according to any one of claims 1 to 17, further comprising an outer layer substantially free of catalyst particles outside the support layer in which the catalyst particles are localized, the outer layer being formed to a thickness of 0.01 µm or more and 15 µm or less.

19. The catalyst for producing a carboxylic acid ester according to any one of claims 9 to 18, wherein the catalyst particles have a core made of X (X represents at least one element selected from the group consisting of nickel, palladium, platinum, ruthenium, gold, silver, and copper), and the core is coated with oxidized nickel and / or cobalt.

20. A method for producing a carboxylic acid ester, comprising a reaction step of reacting (a) an aldehyde with an alcohol, or (b) one or more alcohols, in the presence of the catalyst for producing a carboxylic acid ester according to any one of claims 1 to 19 and oxygen.

21. The method for producing a carboxylic acid ester according to claim 20, wherein the aldehyde is acrolein and / or methacrolein.

22. The method for producing a carboxylic acid ester according to claim 20 or 21, wherein the aldehyde is acrolein and / or methacrolein, and the alcohol is methanol.

23. The method for producing a carboxylic acid ester according to any one of claims 20 to 22, wherein the reaction step is carried out in a liquid phase.

24. The method for producing a carboxylic acid ester according to any one of claims 20 to 23, wherein the reaction step is carried out while adding a basic substance so that the pH of the reaction system is 6 or more and 8 or less.

Citation Information

Patent Citations

  • Modified mesoporous silica material, as well as preparation method and application thereof

    CN109046259A

  • Microprogram controller

    JP1982094993A

  • Catalyst for carboxylic acid ester production, method for producing the catalyst, and method for producing carboxylic acid ester using the same

    JP2003305366A

  • Composite particle support, method for producing the composite particle support, and method for producing a compound using the composite particle support as a catalyst for chemical synthesis.

    JP4803767B2