Au sputtering target
By controlling the surface roughness (Ra and Rz) of Au sputtering targets within specific ranges, the initial film thickness distribution and deposition rate are stabilized, addressing the instability issues in conventional targets and improving sputtering efficiency.
Patent Information
- Application Number
- JP2024533934
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-10-17
- Filing Date
- 2023-09-19
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2043-09-19
AI Technical Summary
The condition of the sputtering surface of Au sputtering targets is not thoroughly investigated, leading to unstable film thickness distribution and deposition rate during initial sputtering, which affects subsequent sputtering processes.
The surface roughness (Ra and Rz) of the Au sputtering target is controlled within specific numerical ranges, with Ra between 0.1 μm and 50.0 μm and Rz between 80.0 μm or less, and the variation in these values is limited to 10.0 μm or less, to stabilize the film thickness distribution and deposition rate at the initial stage of sputtering.
This approach results in an Au sputtering target that achieves stable film thickness distribution and consistent deposition rate at the early stage of sputtering, enhancing productivity and film formation efficiency.
Smart Images

Figure 0007573792000004 
Figure 0007573792000005 
Figure 0007573792000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an Au sputtering target. [Background technology]
[0002] The sputtering method is used in the field of semiconductors for fine wiring, MEMS, optical devices, LEDs, organic electroluminescence, etc. Sputtering is a technique in which Ar gas or the like is introduced in a vacuum, a negative voltage is applied to a film-forming material called a target, and the ionized Ar gas is collided with the target surface (sputtering surface) at high speed, violently ejecting particles (atoms and / or molecules) of the film-forming material, which are then deposited on the opposing substrate surface to form a thin film. The sputtering method can form films even with materials that are difficult to form using vacuum deposition, such as high-melting-point metals and alloys, and can be used with a wide range of film-forming materials.
[0003] The development of sputtering target materials is being carried out widely, including the development of materials using precious metals. Precious metal films formed using precious metal sputtering targets are used in various fields due to the excellent chemical stability and electrical properties of the precious metals themselves. For example, in quartz crystal oscillator devices, precious metal films are used as excitation electrodes formed on both sides of quartz crystal chips. In quartz crystal oscillator devices, the vibration frequency is adjusted by the thickness of the precious metal film, so there is a demand for precious metal sputtering targets that can form precious metal films with uniform film thickness distribution during sputtering.
[0004] Sputtering targets are manufactured by a variety of methods, but the final step in their manufacture typically involves grinding and / or polishing the surface of the target. For example, Patent Document 1 discloses a technique in which a raw material containing Ag is melted in a melting furnace, cooled and solidified to obtain an Ag alloy ingot, which is then cold-rolled, heat-treated, and polished with waterproof paper and buffed to obtain a sputtering target. Furthermore, Patent Document 2 discloses a technique in which a metal ingot is repeatedly rolled, machined with a milling machine, and then buffed to obtain a sputtering target. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2017-031503 A [Patent Document 2] JP 2002-146521 A Summary of the Invention [Problem to be solved by the invention]
[0006] As described above, in the final stage of conventional methods for producing sputtering targets, various operations such as polishing are performed. However, the state of the sputtering surface of the final target, particularly that of an Au sputtering target, has not been sufficiently examined, and there is still room for improvement.
[0007] In view of these problems, an object of the present invention is to provide an Au sputtering target that has excellent stability in the film thickness distribution of a sputtering film formed in the early stage of sputtering and that can stabilize the deposition rate in the early stage of sputtering. [Means for solving the problem]
[0008] As a result of extensive research, the inventors have found that the above-mentioned problems can be solved by setting the surface roughnesses Ra and Rz of a sputtering target to specific numerical ranges and reducing the in-plane variation in surface roughness, and have arrived at the present invention.
[0009] [1] Au sputtering target comprising: The average surface roughness Ra on the sputtered surface is 0.1 μm or more and 50.0 μm or less, and the difference between the maximum and minimum values is 10.0 μm or less, and The average surface roughness Rz on the sputtered surface is 80.0 μm or less, and the difference between the maximum and minimum values is 10.0 μm or less. Au sputtering target. [2] The Au sputtering target according to [1], wherein the average surface roughness Ra exceeds 1.0 μm. [3] The Au sputtering target according to [2], wherein the average surface roughness Ra exceeds 10.0 μm. [4] The Au sputtering target according to any one of [1] to [3], wherein the difference between the maximum value and the minimum value of the surface roughness Rz is 5.0 μm or less. [5] The Au sputtering target according to [4], wherein the difference between the maximum and minimum values of the surface roughness Rz is 3.0 μm or less. [6] The Au sputtering target according to any one of [1] to [5], wherein the average half-width value of the (220) crystal plane on the sputtering surface is 1.0 or less as measured by X-ray diffraction. [7] The Au sputtering target according to any one of [1] to [6], wherein the variation of the half-width of the (220) crystal plane on the sputtering surface as measured by X-ray diffraction is ±0.1 or less. Effect of the Invention
[0010] According to the present invention, it is possible to provide an Au sputtering target which has excellent stability in the film thickness distribution of a sputtered film formed in the initial stage of sputtering and which can stabilize the deposition rate in the initial stage of sputtering. [Brief description of the drawings]
[0011] [Figure 1] FIG. 2 is a diagram for explaining measurement points A to E on the sputtering surface of the Au sputtering target. [Diagram 2] FIG. 2 is a diagram for explaining region I on the sputtering surface of the Au sputtering target. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The following describes in detail the embodiments of the present invention, but these descriptions are merely examples (representative examples) of the embodiments of the present invention, and the present invention is not limited to these contents as long as they do not depart from the gist of the present invention. In this specification, a numerical range expressed using "to" means a range that includes the numerical values before and after "to" as the lower and upper limits, and "A to B" means A or more and B or less. In addition, the dimensions, shapes, relative arrangements, and the like of the components shown in the drawings are merely examples. In addition, although a number of embodiments will be described in this specification, these can be combined to the extent possible. In addition, in this specification, the expression "A or B" can be read as "at least one selected from the group consisting of A and B."
[0013] <Auスパッタリングターゲット> The sputtering target according to an embodiment of the present invention (hereinafter also simply referred to as "target") is A gold sputtering target comprising: The surface roughness Ra measured on the surface of the target has an average value of 0.1 μm or more and 50.0 μm or less, and the difference between the maximum value and the minimum value is 10.0 μm or less. The surface roughness Rz measured on the surface of the target has an average value of 80.0 μm or less, and the difference between the maximum value and the minimum value is 10.0 μm or less. This is a Au sputtering target.
[0014] The average value of surface roughness Ra in the present disclosure is the average value of the surface roughness Ra of the target measured at each of the five measurement points A to E shown below, and the difference between the maximum and minimum values of surface roughness Ra in the present disclosure is the difference between the maximum and minimum values of the surface roughness Ra of the target measured at each of the five measurement points shown below. The same applies to Rz. (measurement point) Measurement point A: the center point of the sputtering surface of the target. Measurement point B: When a first imaginary line segment is drawn connecting the measurement point A and an arbitrary point b on the edge of the sputtering surface of the target, the point on the first imaginary line segment is located 5 mm from the point b. Measurement point C: the midpoint of a second imaginary line segment connecting the measurement point A and the measurement point B. Measurement point D: When an imaginary straight line D is drawn on the sputtering surface of the target that passes through the measurement point A and is perpendicular to the first imaginary line segment, and at least one of the two points on the edge of the sputtering surface of the target that intersect with the straight line D is designated as point d, and a third imaginary line segment is drawn connecting the measurement point A and point d, the point on the third imaginary line segment that is located 5 mm away from point d toward the measurement point A. Measurement point E: the midpoint of a fourth imaginary line segment connecting the measurement point A and the measurement point D.
[0015] FIG. 1 illustrates the measurement points A to E. FIG. 1(a) is a plan view of a target, and shows the measurement points A to E when the shape of the target's sputtered surface (sputtering surface) is round, and FIG. 1(b) shows the measurement points A to E when the shape of the target's sputtering surface is square. Note that the positions of the measurement points A to E in FIG. 1 are just an example, and if the position of an arbitrary point B on the edge of the target's sputtering surface for setting point B changes, the positions of points C to E also change. Note that the above points b and d are omitted from FIG. 1.
[0016] The measurement points for evaluating the surface roughness Ra, Rz described below, and the difference between the maximum and minimum values of each of these surface roughnesses may be any of the five measurement points A to E described above, but it is preferable to measure any of five points arbitrarily selected from a region (measurement region I) of the sputtering surface of the target other than the region included in the position 5 mm long from the edge of the sputtering surface of the target. A diagram for explaining this measurement region I is shown in Figure 2. The shaded region in Figure 2 is the measurement region I. In addition, when performing a measurement at a specific measurement point, if the measurement point is a point, the measurement can be performed at the target measurement point. If the measurement point occupies a certain area, the measurement can be performed so that the target measurement point is included in that area.
[0017] Conventionally, in the final stage of the manufacturing process for Au sputtering targets, a process was provided for polishing the surface of the target on the side where sputtering is performed (the sputtering surface). In the polishing process in conventional target manufacturing, polishing and other treatments were carried out in a manner that minimized the surface roughness of the sputtering surface of the final target. However, the condition of the sputtering surface of the sputtering target is a factor that affects the film thickness distribution of the film formed by the initial sputtering and the deposition rate in the initial sputtering, but the relationship between these factors has not been fully investigated. If the characteristics of the sputtered film in the initial sputtering stage or the characteristics of the initial sputtering stage tend to be unstable, this tendency will affect subsequent sputtering. In addition, if these characteristics are unstable, the pre-sputtering time tends to be longer. Therefore, the inventors have conducted extensive research and have found that, with regard to Ra, which evaluates the average surface roughness, measured at various points on the target, while maintaining a relatively rough state of 0.1 μm or more, the difference between the maximum and minimum values of surface roughness Ra is reduced, in other words, the in-plane distribution (variation) is reduced, thereby making it possible to obtain an Au sputtering target that has excellent stability in the film thickness distribution of the sputtering film formed in the early stage of sputtering and that can stabilize the deposition rate (deposition rate) in the early stage of sputtering.
[0018] On the other hand, the surface roughness Ra is an arithmetic mean roughness, and is the average of the unevenness, so it is not easily affected by one protruding scratch. A small Ra indicates that the unevenness from the average surface roughness is small. Further intensive studies by the present inventors have revealed that these conditions alone are insufficient, and that sufficient deposition rate and film thickness distribution characteristics can be ensured by reducing the number of localized protrusions at the μm level and further reducing the variation in the number of localized protrusions at various points on the target. Therefore, the present inventors have studied Rz, which evaluates the presence or absence of localized convexities on the target surface, and by making the Rz measured at various points on the Au sputtering target below a specific value and reducing the difference between the average values of these Rz, a target with excellent characteristics of deposition rate and film thickness distribution at the initial stage of sputtering can be obtained. The present inventors speculate that when a target with localized convexities at the μm level is used, the voltage distribution on the target surface becomes more uneven during sputtering, causing discharge unevenness and reducing the characteristics of deposition rate and film thickness distribution at the initial stage of sputtering. In particular, when there are protruding convexities on the target surface, sputtering at the convexities proceeds first, and the characteristics of deposition rate and film thickness distribution at the initial stage of sputtering deteriorate. Furthermore, the inventors speculate that when sputtering is performed using the sputtering target according to the present embodiment, the film formation speed will be increased, leading to improved productivity.
[0019] In this specification, the term "sputtered film" refers to a film formed by sputtering. In addition, in this specification, "the thickness distribution of the sputtered film is stabilized" means that when the thickness is measured at multiple points on the surface of the sputtered film, the standard deviation calculated from the multiple thicknesses obtained is small. For example, it is preferable that the standard deviation of the thickness obtained at nine measurement points of the sputtered film described below is 100 Å or less. In addition, in this specification, "the deposition rate in sputtering is stabilized" means that when sputtering is performed multiple times, the variation in the deposition rate of the sputtered film in each sputtering is small. For example, when 30 sputtering films are formed, the variation in the deposition rate in the 30 sputterings is preferably within 5 Å / sec, more preferably within 2 Å / sec. Hereinafter, the stabilization of the film thickness distribution of the sputtered film formed in the initial stage of sputtering and the stabilization of the deposition rate in the initial stage of sputtering will be collectively expressed as "stabilization of the initial sputtering characteristics."
[0020] The material of the sputtering target is gold (Au), and may contain unavoidable impurities as other components. The content of unavoidable impurities in the sputtering target is preferably 1000 wtppm or less, more preferably 100 wtppm or less, and even more preferably 20 wtppm or less.
[0021] The shape of the sputtering target is not particularly limited, and may be a plate shape or a cylindrical shape. In this specification, the sputtering surface of the target means the surface on which sputtering is performed. Furthermore, the shape of the sputtering surface of the sputtering target is not particularly limited and may be circular or a polygonal shape such as a square, pentagon, or hexagon, but is preferably circular or rectangular. There is no particular limit to the area of the sputtering surface of the sputtering target. However, based on the size of the targets currently in use, the maximum area is 10 cm, depending on the size of the equipment. 2 More than 5000cm 2 It may be less than 50cm 2 More than 2000cm 2or less. If the target is disk-shaped, the diameter may be 100 mm or more, if the target is plate-shaped, the shorter side may be 5 cm or more, and if the target is cylindrical, the outer diameter is 10 cm or more. Whatever the shape of the target, it is preferable that the sputtering surface has a shape that allows a line segment with a length of more than 1 cm from the viewpoint of efficiency of use.
[0022] (Surface roughness Ra) Regarding the surface roughness Ra, by roughening the surface to a value of 0.1 μm or more measured at various points on the sputtering target while making the in-plane distribution of Ra uniform (reducing the difference between the maximum and minimum values), it is possible to obtain an Au sputtering target with excellent deposition rate and film thickness distribution characteristics at the initial stage of sputtering. The average value of the surface roughness Ra measured at each of the five measurement points indicated by the measurement points A to E may be 0.1 μm or more and 50.0 μm or less, more than 0.1 μm and 50.0 μm or less, more than 1 μm and 50.0 μm or less, more than 1 μm and 50.0 μm or less, more than 5 μm and 50.0 μm or less, more than 5 μm and 50.0 μm or less, more than 10 μm and 50.0 μm or less, more than 15 μm and 50.0 μm or less, or more than 15 μm and 50.0 μm or less, from the viewpoint of stabilizing the initial sputtering characteristics. If the surface roughness is large, the surface area becomes large and the sputtering area becomes large, so the film formation speed tends to be fast.
[0023] Any method may be used to set the surface roughness Ra within the above range, for example, when using abrasive paper, the method of adjusting the roughness of the abrasive paper can be used, and when using an automatic lathe using a machine such as a lathe, the method of adjusting the polishing speed or the feed speed of the object to be polished can be used. When using a machine such as a lathe, for example, Ra can be increased by increasing the feed speed, and Ra can be decreased by decreasing the feed speed. In addition, when polishing the target, if the desired average value of Ra cannot be obtained in one polishing, it is necessary to polish the target multiple times while checking the surface roughness Ra after polishing until it reaches the desired range.
[0024] It is preferable that the polishing operation is performed not only to adjust the surface roughness Ra to a desired range, but also to reduce the variation in Ra, adjust the Rz (maximum height) to a desired range, and reduce the variation in Rz, as described below, so that the final target satisfies the desired surface conditions.
[0025] There are no particular limitations on the method for measuring the surface roughness Ra and Rz described below, and the measurements can be performed using a general surface roughness measuring device (for example, a contact type surface roughness measuring device manufactured by Mitutoyo, a small surface roughness measuring device SJ-210).
[0026] From the viewpoint of stabilizing the initial sputtering characteristics, the difference (variation) between the maximum and minimum values of surface roughness Ra measured at each of the five measurement points indicated by measurement points A to E may be 10.0 μm or less, preferably 10.0 μm or less, may be 5 μm or less, may be 3 μm or less, may be 1 μm or less, may be 0.5 μm or less, or may be 0.1 μm or less, and the lower limit may be 0.0 μm or more, may be 0.01 μm or more, may be 0.5 μm, may be 1.0 μm, or may be 3 μm.
[0027] The method of making the variation of the surface roughness Ra within the above range is not particularly limited as long as the polishing can reduce the variation, and for example, it can be achieved by repeatedly polishing to reduce the variation to a desired range, but from the viewpoint of manufacturing efficiency, it is preferable to use an automatically rotating machine such as a lathe to polish the surface so that the polishing marks form concentric circles while considering the desired range and method of the average value of Ra. In addition, when using a machine such as a lathe, the variation of Ra can be reduced by, for example, keeping the feed rate constant and reducing the feed rate. It is also preferable to use a machine capable of automatic polishing to minimize the variation in surface roughness caused by manual work. However, if the desired condition for the variation in Ra is not met due to insufficient polishing in a part of the sputtering surface of the target after automatic polishing, it is acceptable to polish only that part manually or mechanically so that the condition is met. In addition, in the case of polishing the target, if the desired variation in Ra cannot be obtained by one polishing, the surface roughness Ra after polishing can be confirmed and polished multiple times to achieve the desired range. In this case, the area with the largest maximum value of Ra may be polished partially to reduce the overall variation.
[0028] (Surface roughness Rz) By reducing the local convexities at the μm level, i.e., by reducing the average value of Rz measured at each of the above five measurement points, and further reducing the variation in the degree of local unevenness at each location on the target, i.e., by reducing the difference between the maximum and minimum values of surface roughness Rz measured at each of the above five measurement points, it is possible to obtain an Au sputtering target that can ensure sufficient deposition rate and film thickness distribution characteristics at the initial stage of sputtering. From the viewpoint of stabilizing the initial sputtering characteristics, the average value of surface roughness Rz measured at each of the five measurement points indicated by measurement points A to E should be 80 μm or less, and a smaller average value is preferable, and it may be 70 μm or less, 50 μm or less, or 30 or less, and there is no particular need to set a lower limit, but it should be 0.1 μm or more, may be more than 0.1 μm, may be 1 μm or more, may be more than 1 μm, 5 μm or more, may be more than 5 μm, 10 μm or more, may be more than 10 μm, 15 μm or more, or may be more than 15 μm.
[0029] Surface roughness Rz (maximum height) is the arithmetic average roughness, which is calculated by extracting a portion of the roughness curve measured by a roughness meter etc. over a reference length, and finding the sum of the highest and deepest parts, and is used when checking for protruding scratches, etc. A large Rz indicates that there are partially defective areas, specifically that the local variation in the target surface is large. Any method may be used to set the average value of the surface roughness Rz within the above range, and for example, when using abrasive paper, the coarseness of the abrasive paper may be adjusted, and when using an automatic lathe such as a lathe, the polishing speed or the feed speed of the object to be polished may be adjusted. When using a machine such as a lathe, for example, Rz can be increased by making the cutting depth of the lathe blade deeper, and Rz can be decreased by making the cutting depth of the lathe blade smaller. In addition, in polishing the target, if the desired average value of Rz cannot be obtained by one polishing, the surface roughness Rz after polishing can be checked and polished multiple times to bring it within the desired range. In this case, it is preferable to first adjust the above-mentioned Ra conditions so that they are within the desired range, and then polish to reduce Rz, that is, to reduce local convexities.
[0030] The difference (variation) between the maximum and minimum values of the surface roughness Rz measured at each of the five measurement points A to E may be 10.0 μm or less, more preferably 5.0 μm or less, more preferably 3.0 μm or less, even more preferably 1.0 μm or less, may be 0.5 μm or less, or may be 0.1 μm or less, from the viewpoint of stabilizing the initial sputtering characteristics. Also, from the viewpoint of the film thickness distribution of the sputtered film, the smaller the difference between the maximum and minimum values of the surface roughness Rz is, the more preferable it is, and there is no need to set a lower limit, but it may be 0.0 μm or more, or may be 0.01 μm or more.
[0031] The method for making the variation of the surface roughness Rz within the above range is not particularly limited as long as the polishing can reduce the variation, and for example, it can be achieved by repeatedly polishing to reduce the variation to a desired range, but from the viewpoint of manufacturing efficiency, it is preferable to use an automatically rotating machine such as a lathe to polish the surface so that the polishing marks form concentric circles while considering the desired range and method of the average value of Rz. Also, when using a machine such as a lathe, the variation of Rz can be reduced by, for example, keeping the cutting depth of the blade constant, keeping the feed rate constant, and reducing the feed rate. It is also preferable to use a machine capable of automatic polishing to minimize the variation in surface roughness caused by manual work. However, if the desired condition for the variation in Ra is not met due to insufficient polishing in a part of the sputtering surface of the target after automatic polishing, it is acceptable to polish only that part manually or mechanically so that the condition is met. In addition, in the case of polishing the target, if the desired Rz variation cannot be obtained by one polishing, the surface roughness Rz after polishing is checked and polished multiple times to bring it into the desired range. In this case, it is preferable to first adjust the above-mentioned Ra conditions so that they are in the desired range, and then polish partially to reduce the areas with the largest Rz values, that is, local convex parts, and polish to reduce the overall variation.
[0032] (Half width) The target has a surface distortion (process distortion) caused by processing such as polishing. A large degree of this processing distortion means a large residual stress, and there is a disadvantage that the deposition rate at the beginning of sputtering and the uniformity of the film thickness distribution are also deteriorated. Therefore, it is preferable that the processing distortion of the target surface is small. The processing distortion is affected by the degree of the load applied to the target during polishing, and the smaller the degree of the load, the smaller the processing distortion. Therefore, if the target is polished by pressing it, the processing distortion will be large, so it is preferable to polish it so as to reduce this pressing. In this embodiment, it is necessary to set the above-mentioned surface roughness within the desired range, but in order to reduce the difference between the maximum and minimum values of the surface roughness, the number of polishings is increased, and the processing distortion tends to be large. In order to set the processing distortion within the desired range while maintaining the surface roughness condition within the desired range, for example, the surface roughness can be adjusted with as little load as possible, or the grit size of the abrasive paper used for polishing can be adjusted. If the processing distortion is not within the desired range, polishing may be repeated until it is within the desired range.
[0033] The processing distortion can be evaluated by, for example, the half-width of the crystal plane measured by X-ray diffraction, and the smaller the half-width, the smaller the processing distortion, and the smaller the half-width is, the better. Specifically, the average half-width of the (220) crystal plane measured by X-ray diffraction in the target at each of the five measurement points indicated by measurement points A to E is preferably 1.0 or less, more preferably 0.6 or less. In addition, it is not necessary to set a lower limit for the half-width, but it may be 0.01 or more, or 0.05 or more.
[0034] Furthermore, the variation in the half-width of the (220) crystal plane measured by X-ray diffraction on the target at each of the five measurement points indicated by measurement points A to E is preferably ±0.1 or less, more preferably ±0.06 or less, and while there is no need to set a lower limit for the variation in the half-width, it may be ±0.005 or more, or may be ±0.01 or more. In this specification, the variation in half-width refers to the range of deviation from the average value of the half-width. Specifically, the variation in half-width being ±0.1 or less means that all of the five measured values of the half-width are within the range of (average value -0.1) to (average value +0.1).
[0035] The above half-width can be measured by an X-ray diffraction device (Cu-Kα tube, such as RINTULTIMA IV manufactured by Rigaku Corporation).
[0036] Of the above two half-width evaluation parameters, it is preferable that at least one of the evaluation parameters falls within the preferred range, and it is more preferable that both evaluation parameters fall within the preferred range.
[0037] Moreover, the evaluation parameters of the above two processing distortions are measured at each of the above five measurement points in the same manner as the above surface roughness, and calculated as the average value.
[0038] By using the above target, it is possible to obtain a sputtering film having excellent stability in thickness of the sputtering film formed in the initial stage of sputtering. The method for evaluating this sputtering film is not particularly limited, but for example, the sputtering surface of the target is subjected to the following evaluation: DC power: 1 kW, sputtering pressure: 9.5×10 -5 The sputtering temperature can be evaluated by sputtering Au at least 30 times under the conditions of 50 Pa, 50 Pa, and a sputtering time of 42 seconds to obtain a sputtered film, and measuring the thickness of each sputtered film obtained. The deposition rate in the initial stage of sputtering can be evaluated by dividing the thickness of the sputtered film formed in the above sputtering by the sputtering time (42 seconds).
[0039] Although there is no particular restriction on the variation in thickness (thickness distribution) of the sputtered film, the standard deviation (standard deviation σ) of the film thickness obtained by measuring the film thickness at the nine measurement points shown below (measurement points) is preferably 100 Å or less, and more preferably 50 Å or less. This is preferably satisfied in each of at least 30 sputtered films obtained by at least 30 sputtering operations. When a stylus-type device is used to measure the film thickness, the resistance value at each point is measured by applying a probe for measuring resistance to the target point. (measurement point) An imaginary line segment is formed by connecting any imaginary straight line passing through the center of the surface of the sputtered film with two intersections with the edge of the surface of the sputtered film, and nine points on the line segment are positioned so as to divide the line segment into 10 equal parts.
[0040] The average crystal grain size on the sputtering surface of the target is not particularly limited, and may be, for example, 1 μm or more and 500 μm or less, 10 μm or more and 200 μm or less, or 10 μm or more and 100 μm or less. The average crystal grain size can be evaluated by observing the sputtering surface of the target using a scanning electron microscope (SEM).
[0041] The crystal orientation of the crystals on the sputtering surface of the target is not particularly limited and may be, for example, (111), (100)((200)), or (110)(220), etc. The crystal orientation can be evaluated by an X-ray diffractometer using Cu as an X-ray source.
[0042] The target may be used with a backing plate for supporting the Au member. The form of the backing plate is not particularly limited, and the shape and material can be selected according to the application. In this specification, when a backing plate is used, the backing plate is treated as constituting the target, and the Au member is also referred to as the target member. In this case, the wording "target" in the description of the target member is replaced with "target member". The shape of the backing plate may be, for example, a plate shape having a polygonal surface such as a square, pentagon, or hexagon, or a circular surface. The area of the backing plate is not particularly limited, and may be in the same range as the area of the target described above, and more specifically, the shape of the surface of the backing plate on the side where the target member and the backing plate are bonded may be the same as the shape of the surface of the backing plate on the bonding side.
[0043] <Manufacturing method of sputtering target> The method for producing the sputtering target is not particularly limited, and the target can be produced by a known method or a combination of known methods. For example, the target can be produced by a production method including a casting step of casting a raw material containing noble metal to obtain an ingot, a processing step of processing the ingot to obtain a workpiece having a desired shape, a heating step of heat-treating the workpiece to obtain a sintered body, and a polishing step of polishing the sintered body. Each step will be described below.
[0044] [Casting process] The casting process is not particularly limited, but for example, a raw material containing Au is prepared, melted in a container such as a graphite crucible or a ceramic crucible in the air, a vacuum atmosphere, or an inert atmosphere, and the molten raw material is poured into a mold having a desired shape, and then cooled and solidified for casting to obtain an ingot. The melting conditions are not particularly limited, and may be any conditions that allow the raw material to melt. The raw material used is one having a high purity, preferably with a gold purity of 99.9% by weight or more, more preferably 99.95% by weight or more, and even more preferably 99.99% by weight or more.
[0045] [Processing process] The processing step is not particularly limited, but for example, the ingot obtained in the above casting step is cut into a desired shape (plate shape, cylindrical shape, etc.) to form a billet, which is then forged and processed. When preparing a plate-shaped target, for example, surface defects on the outer peripheral surface of an ingot formed into a plate are ground away to prepare a billet of the desired shape, whereas when preparing a cylindrical target, surface defects on the outer peripheral surface of an ingot formed into a cylindrical shape are ground away and the inside is hollowed out to prepare a cylindrical billet. Next, the billet is forged into a desired shape. The forging conditions are not particularly limited, and for example, it is preferable to perform the forging in a hot state in the range of 100 to 800°C. Also, instead of or in addition to forging, the billet may be worked into a desired shape by rolling. Forging or rolling may be performed multiple times.
[0046] [Heating process] The heating step is not particularly limited, but for example, an electric furnace or the like is used to heat the processed material at a heating temperature of preferably 100 to 800°C, more preferably 300 to 700°C, and for a heating time of preferably 10 to 500 minutes, more preferably 50 to 250 minutes, to obtain a target material having a certain crystal structure. By carrying out the heat treatment, the internal strain generated during processing can be sufficiently removed. Furthermore, the number of times of the heat treatment may be one or more.
[0047] [Polishing process] The polishing process is not particularly limited, but by performing the polishing operation described in the above description of the surface roughness Ra and Rz and their variations, polishing is performed so that the above-mentioned surface roughness Ra is within a desired range, preferably so that the variation of Ra, Rz, and Rz are within a desired range. For example, the target material obtained by the heating process is surface-polished by an automatic polishing machine or an automatic rotating body such as a rotating potter's wheel. When polishing is performed by a lathe as an automatic polishing machine, the polishing mode is not particularly limited, but from the viewpoint of further stabilizing the initial sputtering characteristics, it is preferable to perform the polishing without changing the center position when polishing in a circular shape, that is, to perform the polishing so that the polishing marks form a concentric circle. In order to stabilize the initial sputtering characteristics, it is preferable to avoid manual polishing as much as possible. Furthermore, in order to prevent foreign matter from being mixed into the surface of the target, it is preferable to avoid polishing using an abrasive such as buff polishing. In the polishing step, if chemical mechanical polishing (CMP) is performed after surface polishing using the above-mentioned polishing with an automatic rotor or the like, the average surface roughness Ra may become smaller than the desired range, so it is not preferable to perform CMP polishing after polishing using an automatic rotor or the like.
[0048] Furthermore, when a backing plate and / or a bonding layer is provided, the method for providing them is not particularly limited, and the backing plate and / or the bonding layer can be provided on the target (target member) manufactured by the above-mentioned method.
[0049] As described above, from the viewpoint of reducing the depth and amount of processing distortion on the surface of the target caused by polishing, it is preferable to perform polishing so as to reduce the load on the target.
[0050] In the measurement of each characteristic in this specification, unless otherwise specified, the measurement sample is kept in an environment similar to the measurement environment for 48 hours or more before the measurement. In addition, the measurement temperature, measurement humidity, and measurement pressure are normal temperature (20±10°C), normal humidity (40±20% RH), and normal pressure (atmospheric pressure) unless otherwise specified. EXAMPLES
[0051] The present invention will be described in more detail below with reference to examples, but the present invention should not be construed as being limited to the following examples.
[0052] [Evaluate target characteristics] (Surface roughness Ra and Rz) Using a target, the following measurement points A to E were determined on the sputtering surface of the target as shown in Figure 1, and the surface roughness Ra and Rz were measured using a surface roughness measuring device (Mitutoyo's contact type surface roughness measuring device, small surface roughness measuring device SJ-210). The average values, maximum values, minimum values, and differences between the maximum and minimum values of surface roughness Ra and Rz at measurement points A to E are shown in Table 1. In Table 1, "large" means the maximum value, "small" means the minimum value, and "difference" means the difference between the maximum and minimum values. (measurement point) Measurement point A: the center point of the sputtering surface of the target. Measurement point B: When a first imaginary line segment is drawn connecting the measurement point A and an arbitrary point b on the edge of the sputtering surface of the target, the point on the first imaginary line segment is located 5 mm from the point b. Measurement point C: the midpoint of a second imaginary line segment connecting the measurement point A and the measurement point B. Measurement point D: When an imaginary straight line D is drawn on the sputtering surface of the target that passes through the measurement point A and is perpendicular to the first imaginary line segment, and at least one of the two points on the edge of the sputtering surface of the target that intersect with the straight line D is designated as point d, and a third imaginary line segment is drawn connecting the measurement point A and point d, the point on the third imaginary line segment that is located 5 mm away from point d toward the measurement point A. Measurement point E: the midpoint of a fourth imaginary line segment connecting the measurement point A and the measurement point D.
[0053] (Half width) An X-ray diffractometer was used to measure the half-value width of the (220) plane on the target surface at the above five measurement points A to E. The average value and the variation are shown in Table 1.
[0054] [Evaluation of sputtered film characteristics] The target was attached to a sputtering device (SRV-4320 manufactured by Shinko Seiki) and the inside of the device was heated to 9.5 × 10 -5After evacuation to 10 Pa or less, sputtering was performed under the conditions of input power: DC 1 kW, target-substrate distance: 50 mm, and sputtering time: 42 seconds to form an Au film on a 6-inch Si substrate (wafer), producing a sputtered film (thickness: about 1100 Å). This sputtering was repeated 30 times using the same target to obtain 30 sputtered films. Among these 30 films, the first, 15th, and 30th sputtered films were used to evaluate the film thickness distribution using the method described below. In addition, the deposition rate was evaluated in the first, 15th, and 30th sputtering of the 30 sputterings using the method described below.
[0055] (Deposit) The deposition rate in the sputtering was evaluated by dividing the thickness of the sputtered film formed in the above sputtering by the sputtering time (42 seconds). The evaluation results are shown in Table 2.
[0056] (Film thickness) For any imaginary line segment (a line segment that connects a straight line that passes through the center of the surface of the sputtered film at two intersections with the edge of the sputtered film) that passes through the center of the surface of the sputtered film, nine points were drawn on the line segment so as to divide the line segment into 10 equal parts. At each of these nine points, the thickness of the sputtered film was measured using a stylus-type surface shape measuring instrument, a small surface roughness measuring instrument SJ-210 manufactured by Mitutoyo Corporation, and the average thickness and the average standard deviation of the thickness (standard deviation σ) were calculated from these thicknesses. The results of these calculations are shown in Table 3. The thickness of the film at each point was measured by applying a probe for measuring resistance to the target point.
[0057] [Manufacturing of sputtering targets] Example 1 First, an Au lump (purity 99.99 wt%) was placed in a high-frequency melting furnace and melted at 1200°C to obtain molten Au, which was then poured into a mold to obtain an Au ingot. The Au ingot was then cut to obtain a billet, which was then hot forged at 500°C to obtain a disk-shaped workpiece with a diameter of 300 mm and a height of 7 mm. The surface was then cut with a milling machine to remove oxides on the surface, and the surface was then uniformly hairline polished with 2000 grit abrasive paper while rotating on a rotary table. Regarding polishing, specifically, first, the surface was polished with abrasive paper #2000 so that the surface roughness Ra of the polished surface approached the values shown in Table 1 by repeatedly checking the surface roughness Rz of the polished surface, and then the surface roughness Rz of the polished surface was repeatedly checked to polish the parts with large surface roughness Rz, and finally, a sputtering target was manufactured so that the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points reached the values shown in Table 1. When polishing using a rotary table (turntable), polishing was performed without changing the center position when polishing in a circular shape.
[0058] The obtained target had a disk shape with a diameter of 290 mm and a height of 6 mm. In addition, elemental analysis using an ICP-MS analyzer (Shimadzu Corporation's inductively coupled plasma atomic emission spectrometry ICPS-8100) showed that the composition ratio of the target was 99.99% by weight of Au. The average value of Ra was about 0.3 μm, the average value of Rz was about 3.6 μm, the variation of Ra and Rz was small, the deposition rate was about 23 Å / sec, and the film thickness distribution was about 1000 Å with a small standard deviation.
[0059] Example 2 After obtaining the workpiece, the milling machine was changed to an NC automatic lathe, and the cutting depth per cut by the tool was set to about 0.05 mm, the rotation speed was 100 rpm, and the feed rate was 0.01 mm / rev, and polishing was performed. Specifically, as with Example 1, first, polishing was performed with an NC automatic lathe so that the surface roughness Ra of the surface after polishing approached the values shown in Table 1 by repeatedly checking the surface roughness Rz of the surface after polishing, and then the parts with large surface roughness Rz were polished by repeatedly checking the surface roughness Rz of the surface after polishing, and finally, the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were set to the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also the same as in Example 1. The average value of Ra was about 3.0 μm, the average value of Rz was about 15 μm, the variation of Ra and Rz was very small, the deposition rate was about 29 Å / sec, and the film thickness distribution was about 1200 Å with a small standard deviation.
[0060] Example 3 After obtaining the workpiece, the milling machine was changed to an NC automatic lathe, and the cutting depth per cut by the tool was set to about 0.1 mm, the rotation speed was 200 rpm, and the feed rate was 0.1 mm / rev, and polishing was performed. Specifically, as with Example 1, first, polishing was performed with an NC automatic lathe so that the surface roughness Ra of the surface after polishing approached the values shown in Table 1 by repeatedly checking the surface roughness Rz of the surface after polishing, and then the parts with large surface roughness Rz were polished by repeatedly checking the surface roughness Rz of the surface after polishing, and finally, the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were set to the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also similar to those of Example 1. The average value of Ra was about 10 μm, the average value of Rz was about 45 μm, the variation of Ra and Rz was small, the deposition rate was about 30 Å / sec, and the film thickness distribution was about 1250 Å with a small standard deviation.
[0061] Example 4 After obtaining the workpiece, the milling machine was changed to an NC automatic lathe, and the cutting depth per cut by the tool was set to about 0.5 mm, the rotation speed was 500 rpm / min, and the feed rate was 0.2 mm / rev, and polishing was performed. Specifically, as with Example 1, first, polishing was performed with an NC automatic lathe so that the surface roughness Ra of the surface after polishing approached the values shown in Table 1 by repeatedly checking the surface roughness Rz of the surface after polishing, and then the parts with large surface roughness Rz were polished by repeatedly checking the surface roughness Rz of the surface after polishing, and finally, the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were set to the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also similar to those of Example 1. The average value of Ra was about 35 μm, the average value of Rz was about 75 μm, the variation of Ra and Rz was small, the deposition rate was about 32 Å / sec, and the film thickness distribution was about 1350 Å with a small standard deviation.
[0062] Example 5 In the polishing in Example 1 described above, the degree of pressing of the abrasive paper against the target was reduced so that the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points finally became the values shown in Table 1, and furthermore, polishing was performed so as to become the half-value width shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also the same as in Example 1. The average value of Ra was about 0.71 μm, the average value of Rz was about 3.3 μm, the variation of Ra and Rz was small, the deposition rate was about 25 Å / sec, and the film thickness distribution was about 1200 Å with a small standard deviation, which was better than the target in Example 1.
[0063] Comparative Example 1 After obtaining the workpiece, the method of cutting was changed to a face milling process of an automatic vertical milling machine by rotating a cylindrical cutting tool with multiple blades, and polishing was performed at a rotation speed of 300 rpm and a feed rate of 45 mm / min so that the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also the same as in Example 1. As a result, the average value of Ra was about 5 μm and the average value of Rz was about 22.5 μm, but there was a large variation, the deposition rate was about 20 to 23 Å / sec, and the film thickness distribution was 850 to 970 Å with a very large standard deviation.
[0064] Comparative Example 2 After obtaining the workpiece, the surface was cut under the conditions of the milling machine used in Comparative Example 1, and then the surface was polished by CMP. A sputtering target was manufactured in the same manner as in Example 1 so that the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were the values shown in Table 1. The size of the target finally obtained and the purity of Au were also the same as in Example 1. As a result, the average value of Ra and the average value of Rz were both less than 0.1 μm, the variation of Ra and Rz was very small, and the film thickness distribution was good, but the deposition rate was very slow and the variation was large.
[0065] Comparative Example 3 After obtaining the workpiece, the cutting was changed to a manual lathe with a cutting speed of 0.05 to 0.5 m / min, a cutting depth of 0.1 mm, and a feed rate of 0.1 to 1.0 mm / rev, with variations, so that the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also the same as in Example 1. The average values of Ra and Rz were about 12.5 μm and 32.4 μm, respectively, and the variations of Ra and Rz were very large, the deposition rate was about 22 Å / sec, and the film thickness distribution was about 910 to 960 Å with a large standard deviation.
[0066] Comparative Example 4 After obtaining the workpiece, the machine was changed to an NC automatic lathe, the cutting depth per cut by the cutting tool was set to about 1.0 mm, the rotation speed was set to 600 rpm / min, and the feed rate was set to 0.2 mm / rev, and the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were set to the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also the same as in Example 1. The average value of Ra was about 61 μm and the average value of Rz was about 83 μm, with large variations in Ra and Rz, the deposition rate was about 19.5 Å / sec, and the film thickness distribution was about 790 to 850 Å with a large standard deviation.
[0067] Comparative Example 5 After obtaining the workpiece, the surface was manually polished uniformly using No. 800 abrasive paper so that the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size of the target finally obtained and the purity of Au were also the same as in Example 1. The average value of Ra was about 1.5 μm and the average value of Rz was about 10.6 μm, and while the variation in Ra was small, the variation in Rz was large, the deposition rate was about 19 to 22 Å / sec, and the film thickness distribution was about 760 to 820 Å with a large standard deviation.
[0068] Comparative Example 6 After obtaining the workpiece, the surface was polished uniformly by hand using abrasive paper #120 so that the surface roughness Ra and Rz of the sputtering target measured at the above five measurement points were the values shown in Table 1. A sputtering target was manufactured in the same manner as in Example 1. The size and Au purity of the target finally obtained were also the same as in Example 1. The average value of Ra was about 42 μm and the average value of Rz was about 85.1 μm, and while the variation in Ra was small, the variation in Rz was large, the deposition rate was about 10 to 16 Å / sec, and the film thickness distribution was about 370 to 680 Å with a large standard deviation.
[0069] [Table 1]
[0070] [Table 2]
[0071] [Table 3]
[0072] From Table 1, it was found that by setting the average value of the surface roughness Ra of the sputtering surface of the target obtained by the above measurement to 0.1 μm or more and 50 μm or less, the variation of Ra to 10 μm or less, the average value of Rz to 80 μm or less, and the variation of the surface roughness Rz to 10 μm or less, the sputtering film formed at the beginning of sputtering has excellent stability of the film thickness distribution, and the deposition rate at the beginning of sputtering can be stabilized. In Comparative Example 2, in which the average value of Ra is too small, it is presumed that the deposition rate at the beginning of sputtering is small because the average of the unevenness is too small. In addition, in Comparative Examples 1 and 3 to 6, in which Rz is large or the variation of Rz is large, it is presumed that the variation in the film thickness distribution of the sputtering film is large due to the presence of local convex parts, or the existence of variation in the degree of the height of the local convex parts on the target surface, etc. [Industrial Applicability]
[0073] According to the present invention, it is possible to provide an Au sputtering target in which the sputtering film formed in the initial stage of sputtering has excellent stability in thickness distribution and the deposition rate in the initial stage of sputtering can be stabilized. The sputtering target according to the embodiment of the present invention can be widely used in the formation of elements in electronic components, semiconductor devices, optical thin films, magnetic devices, LEDs, organic EL, LCDs, etc., using a sputtering method.
Claims
1. A gold sputtering target comprising: The average surface roughness Ra of the sputtered surface is 0.1 μm or more and 50.0 μm or less, and the difference between the maximum value and the minimum value is 10.0 μm or less, and The average surface roughness Rz of the sputtered surface is 80.0 μm or less, and the difference between the maximum and minimum values is 10.0 μm or less; and The average half-width value of the (220) crystal plane measured by X-ray diffraction on the sputtered surface is 1.0 or less. Au sputtering target.
2. 2. The Au sputtering target according to claim 1, wherein the average surface roughness Ra is greater than 1.0 μm.
3. 3. The Au sputtering target according to claim 2, wherein the average surface roughness Ra is greater than 10.0 μm.
4. 4. The Au sputtering target according to claim 1, wherein the difference between the maximum value and the minimum value of the surface roughness Rz is 5.0 μm or less.
5. 5. The Au sputtering target according to claim 4, wherein the difference between the maximum value and the minimum value of the surface roughness Rz is 3.0 μm or less.
6. 4. The Au sputtering target according to claim 1, wherein the variation of the half-width of the (220) crystal plane on the sputtering surface measured by X-ray diffraction is ±0.1 or less.
Citation Information
Patent Citations
Gold alloy target and preparation method thereof
CN104561639A
Method for manufacturing gold target
JP2002146521A
Sputtering target manufacturing method, sputtering target cleaning method, sputtering target, and sputtering apparatus
JP2009191323A
Ag ALLOY FILM AND METHOD FOR PRODUCING SAME, Ag ALLOY SPUTTERING TARGET AND LAMINATED FILM
JP2017031503A
Au film formation method
JP2022128463A