Positive electrode active material for non-aqueous electrolyte secondary battery, positive electrode for non-aqueous electrolyte secondary battery, non-aqueous electrolyte secondary battery, method for manufacturing non-aqueous electrolyte secondary battery, and method for using non-aqueous electrolyte secondary battery

The use of a lithium transition metal composite oxide with controlled molar ratios and crystallinity in the positive electrode active material addresses the low discharge capacity and voltage surge issues in conventional lithium-excess batteries, ensuring high capacity and safety in non-aqueous electrolyte secondary batteries.

JP7574885B2Active Publication Date: 2024-10-29GS YUASA CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023109667
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-14
Filing Date
2023-07-03
Publication Date
2024-10-29
Estimated Expiration
2039-06-19

AI Technical Summary

Technical Problem

Conventional lithium-excess active materials for non-aqueous electrolyte secondary batteries face issues with low discharge capacity and a sudden increase in battery voltage when accidentally overcharged, as they are charged until the end of the flat potential change region, leading to poor charge-discharge cycle performance.

Method used

A positive electrode active material with a lithium transition metal composite oxide having a specific molar ratio of Li/Me (1.05≦Li/Me<1.4), including Ni and Mn, and controlled crystallinity to avoid charging until the end of the flat potential change region, maintaining a high discharge capacity without a sudden voltage increase.

Benefits of technology

The solution ensures a non-aqueous electrolyte secondary battery with a large discharge capacity and prevents a sudden voltage increase even at higher states of charge, enhancing safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574885000005
    Figure 0007574885000005
  • Figure 0007574885000006
    Figure 0007574885000006
  • Figure 0007574885000007
    Figure 0007574885000007
Patent Text Reader

Abstract

To provide a nonaqueous electrolyte secondary battery showing a large discharge capacity even in the case of being charged with a relatively low voltage, and not allowing rapid rise in battery voltage to be observed until reaching a higher SOC, and methods of manufacturing and using such a nonaqueous electrolyte secondary battery.SOLUTION: Provided is a nonaqueous electrolyte secondary battery comprising a positive electrode for a nonaqueous electrolyte secondary battery, in which the positive electrode containing a positive electrode active material for a nonaqueous electrolyte secondary battery, described below. The positive electrode active material for a nonaqueous electrolyte secondary battery contains a lithium transition metal composite oxide. The lithium transition metal composite oxide has an α-NaFeO2 structure in which a mole ratio Li / Me of Li to a transition metal (Me) is given by 1.05≤Li / Me<1.4, and contains, as the transition metal (Me), Ni and Mn, or Ni, Co and Mn, in which a mole ratio Mn / Me of Mn to Me is given by 0.4≤Mn / Me<0.6, and a mole ratio Ni / Me of Ni to Me is given by 0.2≤Ni / Me≤0.6.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a positive electrode active material for a nonaqueous electrolyte secondary battery, a positive electrode for a nonaqueous electrolyte secondary battery containing the positive electrode active material, a nonaqueous electrolyte secondary battery, a method for producing a nonaqueous electrolyte secondary battery using the positive electrode, and a method for using the nonaqueous electrolyte secondary battery. Regarding. [Background technology]

[0002] Conventionally, as a positive electrode active material for non-aqueous electrolyte secondary batteries such as lithium secondary batteries, a "LiMeO2 type" active material (Me is a transition metal) having an α-NaFeO2 type crystal structure has been studied, and lithium secondary batteries using LiCoO2 have been widely used. However, the discharge capacity of LiCoO2 was about 120 to 130 mAh / g. It has been desired to use Mn, which is an abundant earth resource, as the Me. However, when the "LiMeO2 type" active material contains Mn as Me, if the molar ratio Mn / Me of Mn in Me exceeds 0.5, a structural change occurs to a spinel type upon charging, and the crystal structure cannot be maintained, resulting in a problem of significantly poor charge-discharge cycle performance.

[0003] Therefore, various "LiMeO2 type" active materials, which have a molar ratio of Mn in Me of 0.5 or less and are excellent in terms of charge-discharge cycle performance, have been proposed and some have been put to practical use. For example, the lithium transition metal composite oxide LiNi 1 / 2 Mn 1 / 2 O2 and LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 The positive electrode active material containing O2 has a discharge capacity of 150 to 180 mAh / g.

[0004] On the other hand, for the so-called "LiMeO2 type" active material described above, the composition ratio Li / Me of lithium (Li) to the transition metal (Me) ratio is greater than 1, and the composition formula Li 1+α Me 1-αSo-called "lithium-rich" active materials containing lithium transition metal composite oxides represented by O2 (α>0) are also known. It is also known to produce the above-mentioned lithium transition metal composite oxides from hydroxide precursors (see, for example, Patent Documents 1 to 3).

[0005] Patent Document 1 states that "a-NaFeO2 type crystal structure, with the composition formula Li 1+α Me 1-α Regarding the lithium transition metal composite oxide represented by the formula O2 (Me is a transition metal including Co, Ni and Mn, and α>0) (Claim 1), the document states, "A method for producing a positive electrode active material for a lithium secondary battery according to Claim 1 or 2, characterized in that the precursor used in the synthesis of the lithium transition metal composite oxide is a hydroxide of a transition metal including Co, Ni and Mn." (Claim 3). In addition, "a precursor is produced by co-precipitating a compound containing Co, Ni, and Mn in a solution. The pH in the process is not limited, but can be 10.514 when the coprecipitated precursor is to be prepared as a coprecipitated hydroxide precursor. In order to increase the tap density, it is preferable to control the pH. By setting the pH to 11.5 or less, the tap density can be set to 1.00 g / cm 3 or more, thereby improving the high rate discharge performance. Furthermore, by setting the pH to 11.0 or less, the particle growth rate can be accelerated, and the stirring time after the dropwise addition of the raw material aqueous solution can be shortened." (Paragraph

[0032] ) Furthermore, with regard to the initial charge / discharge process of a lithium secondary battery using the positive electrode active material according to the embodiment, it is described that "charging was performed at a constant current and constant voltage of a current of 0.1 CA and a voltage of 4.6 V" (paragraph

[0098] ).

[0006] Patent Document 2 describes a positive electrode active material for a non-aqueous electrolyte battery, which contains a lithium transition metal composite oxide, the lithium transition metal composite oxide having a molar ratio (Li / Me) of Li to a transition metal (Me) greater than 1, the transition metal (Me) containing Mn, Ni, and Co, the lithium transition metal composite oxide having an α-NaFeO2 type crystal structure, and an X-ray diffraction pattern that can be assigned to the space group R3-m, and a CuKα ray diffraction pattern that can be assigned to the space group R3-m, The half-width of the diffraction peak of the (104) plane (FWHM(104)) in the Miller indices hkl according to the present invention is 0.21° or more and 0.55° or less, the ratio of the half-width of the diffraction peak of the (003) plane to the half-width of the diffraction peak of the (104) plane (FWHM(003) / FWHM(104)) is 0.72 or less, and the peak differential pore volume of the lithium transition metal composite oxide particles determined by the BJH method from an adsorption isotherm using a nitrogen gas adsorption method is 0.33 mm 3 / (g·nm) or less." (Claim 1), and "A method for producing a positive electrode active material for a non-aqueous electrolyte secondary battery according to any one of claims 1 to 7, comprising firing the hydroxide precursor of the transition metal and a lithium compound at a temperature of 800° C. or more and 940° C. or less." (Claim 8). Similarly to paragraph

[0032] of Patent Document 1, it is described that the pH in the process for producing the hydroxide precursor can be from 10.5 to 14, and that in order to increase the tap density, it is preferable to control the pH (paragraph

[0031] ). It is also described that the initial charge / discharge process of the lithium secondary battery produced using the positive electrode active material according to the embodiment was performed as "constant-current, constant-voltage charging at a current of 0.1 CmA and a voltage of 4.6 V" (paragraph

[0093] ).

[0007] Patent Document 3 describes an active material for lithium secondary batteries that contains a solid solution of a lithium transition metal composite oxide having an α-NaFeO2 crystal structure, the composition ratio of Li, Co, Ni, and Mn contained in the solid solution being: 1+(1 / 3)x Co 1-x-y Ni (1 / 2)y Mn (2 / 3)x+(1 / 2)y(x+y≦1, 0≦y, 1-xy=z) and Li[Li 1 / 3 Mn 2 / 3 ]O2(x)-LiNi 1 / 2 Mn 1 / 2 In the O2(y)-LiCoO2(z) triangular phase diagram, (x,y,z) are A (0.45,0.55,0), B (0.63,0.37,0), C (0.7,0.25,0.05), D (0.67,0.18,0.15), E (0.75,0,0.25), F (0.55,0,0.45), and G (0.45,0.2,0.35). " (Claim 1), "The active material for lithium secondary batteries is characterized in that the intensity ratio of the diffraction peaks of the (003) and (104) planes in X-ray diffraction measurement is I(003) / I(104)≧1.56 before charge / discharge and I(003) / I(104)>1 at the end of discharge. + ) and 4.8V or less (vs. Li / Li + ) in the positive electrode potential range, the initial charging step at least reaches a relatively flat region in which the potential change with respect to the amount of charge electricity is relatively flat, and the positive electrode potential range is 4.3V (vs. Li / Li + ) or less. The examples also state that the crystal phase of the coprecipitated hydroxide precursor obtained by adjusting the pH to 11.5 is a "single phase of β-Ni(OH)2 type" (paragraphs

[0099] to

[0100] ). In addition, regarding the initial charge / discharge process of the lithium secondary battery produced using the positive electrode active material according to the embodiment, it is described that "charging was performed at a constant current and constant voltage of a current of 0.1 ItA and a voltage of 4.5 V" (paragraph

[0114] ).

[0008] In addition, Patent Document 4 describes a non-aqueous electrolyte secondary battery including a positive electrode containing a positive electrode active material, a negative electrode containing a negative electrode active material, and a non-aqueous electrolyte containing a non-aqueous solvent, the positive electrode active material being represented by the general formula (1) Li 1+x Mn y Mz A non-aqueous electrolyte secondary battery comprising a lithium-containing transition metal oxide represented by O2 (where x, y, and z satisfy 0 < x < 0.4, 0 < y < 1, 0 < z < 1, and x + y + z = 1, and M is one or more metal elements including at least Ni or Co), wherein the non-aqueous solvent contains a fluorinated cyclic carbonate in which two or more fluorine atoms are directly bonded to a carbonate ring. (Claim 1) is described.

[0009] And, as Example 1 of the secondary battery, the positive electrode active material is "Li 1.2 Mn 0.54 Ni 0.13 Co 0.13 O2", the negative electrode contains silicon and carbon, and the non-aqueous electrolyte is "LiPF6 dissolved in a non-aqueous solvent obtained by mixing 4,5-difluoroethylene carbonate and ethyl methyl carbonate in a volume ratio of 2:8 so as to be 1 mol / liter", and the initial charge and discharge were performed by "charging at a constant current of 0.5It until the battery voltage reached 4.45V, and then performing constant voltage charging at 4.45V until the current value reached 0.05It. At this time, the potential of the positive electrode was 4.60V based on metallic lithium. Then, discharging was performed at a constant current of 0.5It until the battery voltage reached 1.50V." (described from paragraphs

[0041] to

[0049] ).

[0010] Also, Patent Document 5 discloses, "The following general formula (1): Li x Ni y Mn z Co 1-y-z O 1+x (1) (In the formula, x represents 1.02 ≤ x ≤ 1.25, y represents 0.30 ≤ y ≤ 0.40, and z represents 0.30 ≤ z ≤ 0.40.) A lithium composite oxide in which a lithium nickel manganese cobalt-based composite oxide is contained with 0.1 mol% or more and less than 5 mol% of one or more metal atoms (Me) selected from Mg, Al, Ti, Cu, and Zr, and the amount of Li2CO3 present on the particle surface is 0.05 to 0.20% by weight, which is a positive electrode active material for a lithium secondary battery. (Claim 1) is described. The document also states that "the lithium composite oxide has a tap density of 1.5 g / ml or more. The reason for this is that if the tap density of the lithium composite oxide is less than 1.5 g / ml, the electrode density decreases and the discharge capacity of the lithium secondary battery tends to decrease. In particular, it is preferable for the tap density of the lithium composite oxide to be in the range of 1.7 to 2.8 g / ml, from the viewpoint of increasing the discharge capacity of the lithium secondary battery." (paragraph

[0021] ) The Examples also state that composite hydroxide samples A and B, in which "the molar ratio of Ni:Co:Mn in the composite hydroxide is 0.334:0.333:0.333", were mixed with lithium carbonate and a compound of Me, and calcined at 900°C to obtain a lithium composite oxide sample in which Li / (Ni+Co+Mn+Me) was 1.17 to 1.19 (paragraphs

[0067] to

[0073] , Table 3 at

[0084] ).

[0011] Patent Document 6 states that "press density is 3.3 to 4.5 g / cm 3 "A lithium-nickel-manganese-cobalt composite oxide having a particle size distribution based on volume in which the ratio of particles having a size of 10 μm or less is 10 to 70 volume %." (Claim 1), "A composition represented by the following chemical formula, Li 1+a Ni b Mn c Co d M e O 2( (where M is a metal other than Ni, Mn, Co, and Li) a+b+c+d+e=1 0 <a≦0.2 0.2≦b / (b+c+d)≦0.4 0.2≦c / (b+c+d)≦0.4 0 <d / (b+c+d)≦0.4 0≦e≦0.1 Furthermore, the BET specific surface area is 0.05 to 1.0 m 2 / g of the lithium-nickel-manganese-cobalt composite oxide according to claims 1 and 2." (Claim 3) In the embodiment, the composition is Li 1.04 [Ni 0.32 Mn 0.32 Co0.32 ]O2, 2t / cm 2 The press density when pressed with a pressure of 3.56 g / cm 3 , 3.43g / cm 3 , 3.52g / cm 3 , 3.47g / cm 3 , 3.31g / cm 3 The document describes a complex oxide which is (paragraphs

[0075] ,

[0082] ,

[0086] ,

[0090] , and

[0094] ). [Prior art documents] [Patent documents]

[0012] [Patent Document 1] JP 2014-029828 A [Patent Document 2] International Publication 2016 / 190419 [Patent Document 3] Patent No. 4877660 [Patent Document 4] JP 2012-104335 A [Patent Document 5] JP 2011-113792 A [Patent Document 6] JP 2008-013405 A Summary of the Invention [Problem to be solved by the invention]

[0013] Standards (for example, GB / T (China Recommended National Standard) for automotive batteries) stipulate that non-aqueous electrolyte secondary batteries must remain safe even if accidentally overcharged. One method for evaluating whether safety has been improved is to record the SOC at which a sudden rise in battery voltage is observed when a current is forcibly applied beyond the fully charged state (SOC 100%), assuming that the charging control circuit has been broken. If no sudden rise in battery voltage is observed until a higher SOC is reached, safety is evaluated as having been improved. Here, SOC stands for State Of Charge, and is the battery's state of charge expressed as the ratio of the remaining capacity at that time to the capacity when fully charged, with the fully charged state being expressed as "SOC 100%."

[0014] As shown in Figure 1, the positive electrode containing the lithium-excess active material has a potential of 5.0 V (vs. Li / Li + ) is initially charged to 4.5V (vs. Li / Li + ) or more 5.0V (vs.Li / Li + ), a region in which the potential change with respect to the amount of charge is relatively flat is observed. In the positive electrode potential range below 5.0 V (vs. Li / Li), if the positive electrode has been charged even once until the end of this flat region of potential change, the potential change becomes flat at 5.0 V (vs. Li / Li + ), the flat region of the potential change is not observed again. Conventional nonaqueous electrolyte batteries having a positive electrode containing a lithium-excess active material (see, for example, Patent Documents 1 to 3) are manufactured on the premise that they are charged at the time of initial charging until the flat region of the potential change ends. + ) A high discharge capacity can be obtained in a potential region below 1000V.

[0015] In contrast, the present invention is premised on the fact that the battery is manufactured without undergoing any charging process until the end of the flat region of the potential change, and is used without being charged until the end of the flat region of the potential change. By manufacturing and using the lithium battery in this way, the above capacity range appears only when it is accidentally overcharged. Therefore, when a current is forcibly applied further beyond the fully charged state (SOC 100%), a battery can be provided in which no sharp rise in battery voltage is observed until a higher SOC is reached.

[0016] However, if a positive electrode containing a lithium-excess type active material is manufactured without going through the charging process until the end of the region where the potential change is flat, and is used without charging until the end of the region where the potential change is flat, the conventional lithium-excess type active material has a problem that the discharge capacity is small, as shown in Comparative Example 1-1 and Comparative Example 1-2.

[0017] In Patent Documents 1 to 4, the charging during the initial charge and discharge of the positive electrode containing the lithium-excess type active material is performed until the end of the region where the potential change is flat. Patent Documents 5 and 6 describe active materials containing lithium transition metal composite oxides with 1 < Li / Me (transition metal), but the specifically described lithium transition metal composite oxides have a Ni:Co:Mn ratio of 1:1:1 and a low Mn content, so they are not positive electrode active materials in which a region where the potential change is flat is observed.

[0018] An object of the present invention is to provide a positive electrode active material for a non-aqueous electrolyte secondary battery, a non-aqueous electrolyte secondary battery, a method for manufacturing the battery, and a method for using the battery, which have a large discharge capacity even when charged at a relatively low voltage and in which no sharp rise in battery voltage is observed until a higher SOC is reached.

Means for Solving the Problems

[0019] One aspect of the present invention for solving the above-mentioned problems is a positive electrode active material for a non-aqueous electrolyte secondary battery containing a lithium transition metal composite oxide, the lithium transition metal composite oxide having an α-NaFeO2 structure, a molar ratio of Li to a transition metal (Me) Li / Me being 1.05≦Li / Me<1.4, and containing Ni and Mn, or Ni, Co and Mn, as the transition metal (Me), a molar ratio of Mn to Me Mn / Me being 0.4≦Mn / Me<0.6, and a molar ratio of Ni to Me Ni / Me being 0.2≦Ni / Me≦0.6.

[0020] Another aspect of the present invention is a positive electrode for a non-aqueous electrolyte secondary battery, comprising the positive electrode active material according to the above aspect.

[0021] Yet another aspect of the present invention is a nonaqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a nonaqueous electrolyte, wherein the positive electrode contains the positive electrode active material according to the above aspect, and the positive electrode active material exhibits a diffraction peak in a range of 20° or more and 22° or less in an X-ray diffraction diagram using CuKα radiation.

[0022] Yet another aspect of the present invention is a non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, the positive electrode containing the positive electrode active material according to the above aspect, and a positive electrode potential of 5.0 V (vs. Li / Li + ) when charging to 4.5V (vs. Li / Li + ) or more 5.0V (vs.Li / Li + ) or less, a region in which the potential change with respect to the amount of charged electricity is relatively flat is observed.

[0023] Yet another aspect of the present invention is a non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, the positive electrode containing the positive electrode active material according to the above aspect, and a positive electrode potential of 4.6 V (vs. Li / Li + ) dZ / dV curve when charging up to 4.35V (vs. Li / Li +) is the capacity ratio (%) at each potential based on the capacity reached at the time of the charge transfer. V is the potential of the positive electrode. + ) or more than 4.6V (vs. Li / Li + ) in the potential range below dZ / The maximum dV value of the nonaqueous electrolyte secondary battery is 150 or more.

[0024] Yet another aspect of the present invention includes assembling a nonaqueous electrolyte secondary battery using the positive electrode for the nonaqueous electrolyte secondary battery, and performing initial charging and discharging, + ) and exceeds 4.5V (vs. Li / Li + ) or less.

[0025] In other words, in yet another aspect of the present invention, the "nonaqueous electrolyte secondary battery" refers to a battery that has been subjected to the above-mentioned initial charge / discharge process and has been completed in a factory to a state that it can be shipped. In the factory, the battery may be charged and discharged multiple times as necessary.

[0026] Yet another aspect of the present invention is a method for using the nonaqueous electrolyte secondary battery, comprising: + ) and exceeds 4.5V (vs. Li / Li + ) is used as a battery voltage. Effect of the Invention

[0027] The present invention can provide a positive electrode active material for a nonaqueous electrolyte secondary battery that has a large discharge capacity even when charged at a relatively low voltage and in which a rapid increase in battery voltage is not observed even up to a higher SOC, a nonaqueous electrolyte secondary battery, a method for producing the battery, and a method for using the battery. [Brief description of the drawings]

[0028] [Figure 1]A typical charging curve of a positive electrode using a lithium-excess active material, and a conceptual diagram showing the state of charge (SOC%) during manufacture and use, which are the premise of the present invention, and a region where the potential change is flat. [Diagram 2] X-ray diffraction diagrams of the positive electrode active material of the battery according to the embodiment of the present invention and the battery according to the conventional example [Diagram 3] A diagram showing the change in potential versus the amount of charge observed when the "LiMeO2 type" and "lithium-excess type" active materials are initially charged to 4.6 V (vs. Li / Li+). [Figure 4] FIG. 2 is a diagram for explaining a "region in which the potential change is relatively flat relative to the amount of charged electricity" in a nonaqueous electrolyte secondary battery according to an embodiment of the present invention. [Diagram 5] Conceptual diagram of press density measuring device [Figure 6] X-ray diffraction pattern of hydroxide precursor [Figure 7] FIG. 1 is an external perspective view showing one embodiment of a nonaqueous electrolyte secondary battery according to the present invention; [Figure 8] 1 is a schematic diagram showing an electricity storage device including a plurality of nonaqueous electrolyte secondary batteries according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present inventors have conducted various studies on the crystal structure of the transition metal hydroxide precursor used in the production of the lithium transition metal composite oxide, and the composition and crystallinity of the lithium transition metal composite oxide, and as a result have found that there are conditions under which an active material having a large charge quantity in the region where the potential change is flat, and a large discharge capacity can be obtained even when the active material is produced without undergoing any charging process until the region where the potential change is flat, and when the active material is used without charging until the region where the potential change is flat. The details are described below.

[0030] <Cathode active material for nonaqueous electrolyte secondary batteries> One embodiment of the present invention based on the above findings is a positive electrode active material for a non-aqueous electrolyte secondary battery, which contains a lithium transition metal composite oxide, the lithium transition metal composite oxide having an α-NaFeO2 structure, a molar ratio of Li to a transition metal (Me) Li / Me being 1.05≦Li / Me<1.4, containing Ni and Mn, or Ni, Co and Mn, and a molar ratio of Mn to Me Mn / Me being 0.4≦Mn / Me<0.6, The molar ratio of Ni to Me, Ni / Me, is 0.2≦Ni / Me≦0.6. The molar ratio Li / Me may be 1.15 or less. The molar ratio Mn / Me may be Mn / Me<0.55. The molar ratio Ni / Me may be 0.25≦Ni / Me. The molar ratio Ni / Me may be Ni / Me<0.6. The molar ratio of Co to Me, Co / Me, may be Co / Me≦0.35.

[0031] <Composition of lithium transition metal composite oxide> In one embodiment of the present invention, the composition formula Li 1+α Me 1-α The lithium transition metal composite oxide represented by O2(α>0) is a so-called "lithium-excess type" in which the molar ratio Li / Me of Li to the transition metal element Me represented by (1+α) / (1-α) is greater than 1. The Li / Me is preferably 1.05 or more, more preferably 1.10 or more. Also, it is preferably less than 1.40, more preferably 1.30 or less. Within this range, the discharge capacity of the positive electrode active material is improved. Also, the molar ratio Li / Me is more preferably 1.15 or more, and even more preferably 1.20 or more, in that the amount of charge electricity in the region where the potential change is flat can be increased.

[0032] The molar ratio Mn / Me of Mn to the transition metal element Me is 0.4 or more and less than 0.6. By being 0.4 or more, the amount of charge electricity in the region where the potential change is flat can be increased, and by being less than 0.6, a positive electrode active material can be produced without going through a charging process until the region where the potential change is flat, and when used without charging until the region where the potential change is flat, the discharge capacity is large. The above Mn / Me is preferably 0.55 or less, more preferably less than 0.55, even more preferably 0.53 or less, and most preferably 0.50 or less.

[0033] Co contained in the lithium transition metal composite oxide has the effect of improving the initial efficiency, but is expensive because it is a scarce resource. Therefore, the molar ratio Co / Me of Co to the transition metal element Me is preferably 0.35 or less, more preferably 0.20 or less, even more preferably 0.13 or less, and may be 0.

[0034] The molar ratio Ni / Me of Ni to the transition metal element Me is more than 0.20 and not more than 0.60. The Ni / Me is preferably 0.25 or more. Also, it is preferably less than 0.60, and more preferably not more than 0.55. When it is in this range, the polarization during charging and discharging is small, and the discharge capacity is large when used without charging until the end of the flat region of the potential change.

[0035] By using a lithium transition metal composite oxide having the above-described composition as the positive electrode active material, it is possible to obtain a nonaqueous electrolyte secondary battery that has a large charged electric quantity in the region where the potential change is flat, is manufactured without undergoing any charging process until the region where the potential change is flat, and has a large discharge capacity when used without charging until the region where the potential change is flat.

[0036] <Crystal structure and crystallinity of lithium transition metal composite oxides> The lithium transition metal composite oxide according to one embodiment of the present invention has an α-NaFeO2 structure. The lithium transition metal composite oxide after synthesis (before charging and discharging) belongs to the space group P3112 or R3-m. Among them, the one belonging to the space group P3112 has a superlattice peak (Li[Li 1 / 3 Mn 2 / 3 However, even once the voltage exceeds 4.5V (vs. Li / Li + ), the symmetry of the crystal changes with the desorption of Li from the crystal, and the superlattice peak disappears, and the lithium transition metal composite oxide belongs to the space group R3-m. You will be able to do so. Here, P3112 is a crystal structure model in which the atomic positions of the 3a, 3b, and 6c sites in R3-m are subdivided, and the P3112 model is adopted when order is observed in the atomic arrangement in R3-m. Note that "R3-m" is originally written with a bar "-" over the "3" in "R3m".

[0037] When the space group R3-m is used as a crystal structure model based on the X-ray diffraction pattern, the lithium transition metal composite oxide preferably has a half-width of the diffraction peak assigned to the (104) plane, i.e., a value of FWHM(104) of 0.2° to 0.6°. The FWHM(104) is an index of the degree of crystallinity from all directions. If it is too small, the crystallinity progresses too much, the crystallites become large, and the diffusion of Li ions is not performed sufficiently, so the discharge capacity decreases. If it is too large, the crystallinity is low, so the transport efficiency of Li ions decreases, and the discharge capacity also decreases. If the value of FWHM(104) is in the above range, it is possible to increase the discharge capacity, so it is preferable. The diffraction peak at 2θ=44.1°±1° is indexed to the (114) plane in the space group P3112 and to the (104) plane in the space group R3-m. Therefore, in the case of those belonging to the space group P3112, the portion described as (104) in this specification should be read as (114).

[0038] <X-ray diffraction measurement> In this specification, the measurement of the diffraction peak and half-width of the lithium transition metal composite oxide is performed using an X-ray diffractometer (manufactured by Rigaku Corporation, model name: MiniFlex II) under the following conditions and procedures. The X-ray source is CuKα, and the acceleration voltage and current are 30 kV and 15 mA, respectively. The sampling width is 0.01 deg, the scanning time is 15 min (scan speed is 5.0), the divergence slit width is 0.625 deg, the receiving slit is open, and the scattering slit width is 8.0 mm. For the obtained X-ray diffraction data, the peaks derived from CuKα2 are not removed, and the half-width FWHM (104) of the diffraction peak present at 2θ=44±1° on the X-ray diffraction diagram, which is indexed to the (104) plane in the space group R3-m, is calculated using "PDXL", which is the attached software of the X-ray diffraction device.

[0039] <Positive electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery> Another embodiment of the present invention is a positive electrode for a non-aqueous electrolyte secondary battery, containing the positive electrode active material according to the above embodiment. Yet another embodiment of the present invention is a nonaqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a nonaqueous electrolyte, in which the positive electrode contains the positive electrode active material according to the embodiment, and the positive electrode active material exhibits a diffraction peak in the range of 20° or more and 22° or less in an X-ray diffraction diagram using CuKα radiation.

[0040] <Confirmation of diffraction peaks> X-ray diffraction measurement of the positive electrode active material used in the nonaqueous electrolyte secondary battery according to this embodiment and the positive electrode active material included in the positive electrode of the nonaqueous electrolyte secondary battery according to this embodiment, and confirmation that a diffraction peak is observed in the range of 20° to 22° in an X-ray diffraction diagram using CuKα radiation are performed according to the procedures and conditions described below. Here, "observed" refers to the difference (I 18) for the diffraction angle range of 20° to 22°, the difference between the maximum and minimum intensity (I 21 ), i.e., "I 21 / I 18 " is in the range of 0.001 to 0.1.

[0041] The lower part of FIG. 2 shows the upper limit charge potential of the nonaqueous electrolyte secondary battery according to Example 1 described later. .25V (vs. Li / Li + ), and the lower limit of discharge potential is 2.0V (vs. Li / Li + ) indicates the range including 20° to 22° in the X-ray diffraction pattern measured by the procedure described below for the positive electrode in a fully discharged state after charging and discharging. Here, a diffraction peak is observed in the range of 20° to 22°. In contrast, the upper part of FIG. 2 shows the positive electrode of the nonaqueous electrolyte secondary battery according to the same Example 1 when the upper limit charging potential was set to 4.6 V (vs. Li / Li + ), and the lower limit of discharge potential is 2.0V (vs. Li / Li + ) shows the range including 20° to 22° in the X-ray diffraction pattern measured by the above procedure for the positive electrode in a fully discharged state after charging and discharging. Here, the diffraction peaks in the range of 20° to 22° have disappeared. In addition, the upper limit charging potential of the positive electrode of the nonaqueous electrolyte secondary battery according to Example 1 was set to 4.6 V (vs. Li / Li + ), and the lower limit of discharge potential is 2.0V (vs. Li / Li + ), and then the first charge and discharge was performed, and the upper limit of the charge potential was 4.25V (vs. Li / Li + ), and the lower limit of discharge potential is 2.0V (vs. Li / Li + ), and the positive electrode in a completely unused state after the second charge / discharge was measured using the above procedure. The X-ray diffraction pattern obtained was the same as that shown in the upper part of Figure 2. In other words, the diffraction peak in the range of 20° to 22° never appeared again, and as mentioned above, even once at 4.5 V (vs. Li / Li + ), the peak in the range of 20° to 22° disappears. In the battery according to this embodiment, even in the X-ray diffraction measurement after charging and discharging according to the above procedure, a diffraction peak in the range of 20° to 22° is observed in the X-ray diffraction diagram of the positive electrode active material. Therefore, the battery according to this embodiment has a high resistance to shock waves at 4.5 V (vs. Li / Li), including the initial charge and discharge. + ) battery was used at a potential of less than 100V.

[0042] Yet another embodiment of the present invention is a non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode contains the positive electrode active material according to the embodiment, and the positive electrode potential is 5.0 V (vs. Li / Li + ) when charging to 4.5V (vs. Li / Li + ) or more 5.0V (vs.Li / Li + In this nonaqueous electrolyte secondary battery, a region in which the potential change is relatively flat relative to the amount of charged electricity (hereinafter, also referred to as a "region in which the potential change is flat") is observed within a positive electrode potential range of 0.1 V or less.

[0043] Yet another embodiment of the present invention is a non-aqueous electrolyte secondary battery including a positive electrode, a negative electrode, and a non-aqueous electrolyte, wherein the positive electrode contains the positive electrode active material according to the embodiment, and a positive electrode potential with respect to the positive electrode is 4.6 V (vs. Li / Li + ) dZ / dV curve when charging up to 4.35V (vs. Li / Li + ) is the capacity ratio (%) at each potential based on the capacity reached at the time of the charge transfer. V is the potential of the positive electrode. + ) or more than 4.6V (vs. Li / Li + ) or less, the maximum value of dZ / dV is 150 or more. In the nonaqueous electrolyte secondary battery according to the further embodiment of the present invention, the maximum potential of the positive electrode in a fully charged state (SOC 100%) is 4.3 V (vs. Li / Li + ) and exceeds 4.5V (vs. Li / Li + It is preferable to use the battery at a voltage lower than 100 V.

[0044] The principle of the mechanism of action of the present invention will be described with reference to Fig. 3. The solid line in Fig. 3 indicates the maximum charge potential of a non-aqueous electrolyte secondary battery assembled with a positive electrode using the lithium transition metal composite oxide according to this embodiment (referred to as lithium-excess type) as the positive electrode active material and a negative electrode using Li metal, and the maximum charge potential is set to 4.6 V (vs. Li / Li + The dashed line shows the change in the positive electrode potential when the battery is first charged. 1 / 3 Co 1 / 3 Mn 1 / 3 The potential change when the battery was initially charged in the same manner as the solid line, except that it had a positive electrode using O2 (denoted as LiMeO2 type) as the positive electrode active material, was 4.45 V (vs. Li / Li + ) or more than 4.6V (vs. Li / Li + ) or less, a flat region of potential change is observed. On the other hand, in the LiMeO2-type active material, .Li / Li + ) or more than 4.6V (vs. Li / Li + ) No flat region of potential change is observed. Note that the potential at which the flat region is observed and the capacity during charging and discharging vary slightly depending on the physical properties such as the composition even in a lithium-excess positive electrode, and therefore this figure is merely an example.

[0045] The nonaqueous electrolyte secondary battery according to this embodiment has a maximum capacitance of 5.0 V (vs. Li / Li + When charging is performed up to 4.5V (vs. Li / Li), a "lithium-excess" active material is used for the positive electrode, in which a flat region of potential change is observed. However, in the initial charge / discharge process, the battery is completed without charging until the end of the charging process where the above flat region is observed. +) or less. Furthermore, the nonaqueous electrolyte secondary battery according to this embodiment is used under charging conditions in which charging is not performed until the end of the charging process in which the above-mentioned flat region is observed. Therefore, since the nonaqueous electrolyte secondary battery according to this embodiment has never been charged until the end of the charging process in which the above-mentioned flat region is observed, from the manufacturing stage to the time of use, when it is overcharged, it is preferable that the charging voltage is less than 4.5 V (vs. Li / Li + ) or more 5.0V (vs.Li / Li + Within the positive electrode potential range below 100 V, a region in which the potential change is flat with respect to the amount of charging electricity is observed. By utilizing the behavior described above, the nonaqueous electrolyte secondary battery according to this embodiment can suppress a sudden rise in electrode potential up to a higher SOC, even if the battery is overcharged beyond SOC 100%, which is the fully charged state during normal use.

[0046] <How to confirm the area where the potential change is flat> Here, the observation of the "region where the potential change is flat" is confirmed by the following procedure. A test battery is prepared by disassembling and removing the positive electrode and using Li metal as the working electrode and the counter electrode, and the test battery is subjected to a current value of 10 mA per 1 g of positive electrode mixture to obtain a voltage of 2.0 V (vs. Li / Li + ), then rest for 30 minutes. Then discharge to 5.0 V (vs. Li / Li) at a current of 10 mA per 1 g of positive electrode mixture. + ) is charged at a constant current until the voltage drops to 4.45V (vs. Li / Li) from the start of charging. + The ratio of capacity Y (mAh) at each potential to capacity X (mAh) when the potential reaches 100V is defined as Z (=Y / X*100(%)). The horizontal axis represents potential, the vertical axis represents dZ / dV, with the denominator being the difference in potential change and the numerator being the difference in capacity ratio change, to obtain a dZ / dV curve. The solid line in FIG. 4 shows the results of assembling a nonaqueous electrolyte secondary battery equipped with a positive electrode using a lithium-excess active material as the positive electrode active material and a negative electrode using Li metal, and performing an initial charge to 4.5 V (vs. Li / Li + ) for batteries with a voltage of less than 4.6V (vs. Li / Li +) is an example of a dZ / dV curve when charging to 4.5V (vs. Li / Li) for a lithium-excess active material. As can be seen from the formula, the dZ / dV value is large when the potential change is small relative to the capacity ratio change, and the dZ / dV value is small when the potential change is large relative to the capacity ratio change. + ), the value of dZ / dV becomes large when the potential change begins to plateau. After that, when the potential change ends and the potential starts to rise again, the value of dZ / dV becomes small. In other words, a peak is observed in the dZ / dV curve. Here, 4.5V (vs. Li / Li + ) to 5.0V (vs. Li / Li + ) is 150 or more, it is determined that a flat region of potential change is observed with respect to the amount of charged electricity. On the other hand, the dashed line is a dZ / dV curve of a battery having a similar configuration except that it has a positive electrode using commercially available LiMeO2 as a positive electrode active material. Corresponding to the fact that a flat region of potential change is not observed, a peak such as that observed in the lithium-excess type is not observed. In this specification, normal use refers to the case where the nonaqueous electrolyte secondary battery is used by adopting the charge and discharge conditions recommended or specified for the nonaqueous electrolyte secondary battery, and if a charger for the nonaqueous electrolyte secondary battery is prepared, the charger is used to use the nonaqueous electrolyte secondary battery.

[0047] <Press density of lithium transition metal composite oxide> The lithium transition metal composite oxide according to the first embodiment further has a density when pressed at a pressure of 40 MPa (hereinafter referred to as "press density") of 2.7 g / cm 3 More preferably, it is equal to or greater than this. Press density is 2.7g / cm 3 As described above, by satisfying the above composition, the battery can be manufactured without undergoing a charging process until the end of the flat region of the potential change, and the discharge capacity can be increased when the battery is used without charging until the end of the flat region of the potential change. As shown in Comparative Example 2-5 described later, when Li / Me is 1.1 but Mn / Me is smaller than 0.4, and as shown in Comparative Example 2-4 when Li / Me is 1.0, the discharge capacity is large in a relatively low potential range, but no flat region of potential change is observed.

[0048] In this specification, the conditions for measuring the press density are as follows. The measurement is carried out in air at room temperature between 20°C and 25°C. A schematic diagram of the device used to measure the press density is shown in Figure 5. A pair of measurement probes 1A and 1B are prepared. The measurement probes 1A and 1B have measurement surfaces 2A and 2B, which are flattened ends of stainless steel (SUS304) cylinders with a diameter of 8.0 mm (±0.05 mm), and the other ends are attached to stainless steel pedestals 3A and 3B (with an area of ​​10 cm 2 The cylinder is fixed vertically to a support (above). A side body 6 is prepared, which has a through hole 7 at the center of the acrylic cylinder, the inner diameter of which is adjusted and polished so that the stainless steel cylinder can slowly and naturally descend in the air by gravity. The upper and lower surfaces of the side body 6 are polished smoothly. One of the measurement probes, 1A, is placed on a horizontal desk with its measurement surface 2A facing upward, and the cylindrical portion of the measurement probe 1A is inserted into the through hole 7 of the side body 6 so as to cover it from above. The other measurement probe, 1B, is inserted from above into the through hole 7 with its measurement surface 2B facing down, and the distance between the measurement surfaces 2A, 2B is set to zero. At this time, the distance between the base 3B of measurement probe 1B and the base 3A of measurement probe 1A is measured using a vernier caliper.

[0049] Next, the measurement probe 1B is pulled out, 0.3 g of the powder sample to be measured is poured into the through hole 7 from above with a medicine spoon, and the measurement probe 1B is reinserted from above the through hole 7 with the measurement surface 2B facing down. The area of ​​the contact part with the jig (the contact area with surface 3A in this figure) is 10 cm 2Then, a manual hydraulic press equipped with a pressure gauge is used to apply pressure from above the measurement probe 1B until the pressure scale of the press reaches a value that indicates that the pressure applied to the active material is calculated to be 40 MPa. After the scale reaches the value, no additional pressure is applied even if the value indicated by the scale decreases. Then, in this state, the distance between the base 3B of the measurement probe 1B and the base 3A of the measurement probe 1A is measured again using the caliper. The difference (cm) from the distance before the sample to be measured was added, and the area of ​​the through hole (0.50 cm2) are recorded. 2 ) and the amount of the test sample (0.3 g) used to calculate the density of the test sample under pressure, which is called the press density (g / cm 3 The pressure applied to the active material is calculated from the relationship between the area of ​​the contact part with the jig and the area of ​​the measurement surface (contact area with the powder).

[0050] Although the tap density of the lithium transition metal composite oxide does not necessarily correlate with the effect of the present embodiment, in order to obtain a large press density, it is preferable that the tap density is relatively large. From this viewpoint, the tap density is set to 1.5 g / cm 3 More than 1.6 g / cm is preferable. 3 More preferably, 1.7 g / cm 3 The above is even more preferable.

[0051] In this specification, the tap density is measured according to the following procedure. 10 -2 dm 3 2g±0.2g of the powder sample to be measured is placed in a measuring cylinder, and the volume of the sample to be measured after counting 300 times using a tapping device manufactured by REI ELECTRIC CO.LTD. is divided by the mass of the sample placed in to obtain the value.

[0052] The samples to be subjected to the above-mentioned various measurements are prepared according to the following procedure. If the powder is lithium transition metal composite oxide powder before the positive electrode is made (powder before charging / discharging), it is used for measurement as is. When taking samples from the electrodes taken out by dismantling a battery, before dismantling the battery, discharge the battery at a constant current at a current value (A) that is one-tenth of the nominal capacity (Ah) of the battery until the battery voltage reaches the lower limit of the voltage specified for normal use, to bring the battery into a fully discharged state. If the battery used after dismantling is one that uses a metallic lithium electrode as the negative electrode, the additional work described below is not carried out, and the positive electrode mixture taken from the positive electrode plate is used as the measurement object. If the battery does not use a metallic lithium electrode as the negative electrode, in order to accurately control the positive electrode potential, after dismantling the battery and taking out the positive electrode plate, assemble a battery with a metallic lithium electrode as the counter electrode, and measure the voltage at a current value of 10 mA per 1 g of positive electrode mixture until the voltage reaches 2.0 V (positive electrode potential is 2.0 V (vs. Li / Li + )), and after adjusting to a fully discharged state, dismantle again. The removed positive plate is thoroughly washed with dimethyl carbonate to remove the non-aqueous electrolyte adhering to the electrode, and dried at room temperature for a day and night, after which the mixture on the current collector is collected. The above operations from dismantling to dismantling the battery, as well as the washing and drying of the positive plate, are carried out in an argon atmosphere with a dew point of -60°C or less. The sample to be used for the X-ray diffraction measurement is prepared by lightly crushing the collected mixture in an agate mortar and placing it in a sample holder for X-ray diffraction measurement. To prepare samples for press density and tap density measurements, the mixture is fired in a small electric furnace at 600°C for 4 hours to remove the conductive agent and binder, and the lithium transition metal composite oxide particles are extracted and used as the active material powder (powder after charging and discharging) for the above measurements.

[0053] <Transition metal hydroxide precursor and its manufacturing method> The transition metal hydroxide precursor used in the production of the lithium transition metal composite oxide contained in the positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention preferably contains Ni and Mn, or Ni, Co and Mn, as the transition metal (Me), and is a mixture of a compound having an αNi(OH)2 type crystal structure (hereinafter referred to as αMe(OH)2) and a compound having a βNi(OH)2 type crystal structure (hereinafter referred to as βMe(OH)2).

[0054] The reasons for limiting the molar ratios Mn / Me and Ni / Mn of the transition metal hydroxide precursor (hereinafter also simply referred to as "precursor") and the reasons for limiting the molar ratio Li / Me of the lithium transition metal composite oxide produced using the same are the same as in one embodiment of the present invention.

[0055] The precursor having a crystal structure containing αMe(OH)2 and βMe(OH)2 can have a larger tap density than a precursor having a crystal structure of αMe(OH)2 single phase or βMe(OH)2 single phase. This precursor can be used to produce a lithium transition metal composite oxide with a high press density. The reason why the crystal structure of the transition metal hydroxide precursor is related to the tap density of the transition metal hydroxide precursor and the press density of the lithium transition metal composite oxide is not necessarily clear, but the present inventor speculates as follows. In the transition metal hydroxide of αMe(OH)2 single phase, the primary particle diameter of αMe(OH)2 having a plate-like form is large, so the volume of the gap between the primary particles constituting the secondary particles is large, and therefore the density of the transition metal hydroxide precursor is considered to be low. In addition, the production conditions of the transition metal hydroxide that produces the βMe(OH)2 single phase are high pH, ​​so nucleation takes precedence over particle growth of the transition metal hydroxide, resulting in the production of many fine particles, and therefore, it is considered that the density of the transition metal hydroxide precursor is also low. Therefore, it is believed that a transition metal hydroxide precursor with a high tap density can be obtained by adopting production conditions for a transition metal hydroxide that produces a mixed phase of αMe(OH)2 and βMe(OH)2. Since a lithium transition metal composite oxide is synthesized using a precursor with a high tap density, a lithium transition metal composite oxide with a high press density can be obtained.

[0056] The precursor can be produced by reacting a compound containing Ni and Mn, or Ni, Co and Mn, in an aqueous solution having a pH of 10.2 or less.

[0057] The pH when producing a transition metal hydroxide precursor by a coprecipitation method is usually 10.5 to 14, as described in Patent Documents 1 and 2. As described in Patent Document 3, a hydroxide precursor produced at pH 11.5 is a single phase of βMe(OH)2. In contrast, a precursor containing αMe(OH)2 and βMe(OH)2 can be produced by reacting a transition metal compound in an aqueous solution of pH 10.2 or less. When a lithium transition metal composite oxide produced from such a precursor is used as a positive electrode active material, the resistance of the electrode is reduced, and therefore the potential at which the potential change does not reach a flat region, for example, 4.35 V (vs. Li / Li + ) the amount of Li that can be extracted by charging up to the upper limit, and the reversible capacity can be increased.

[0058] When producing the precursor, it is preferable to add an alkaline solution containing an alkali metal hydroxide, a complexing agent, and a reducing agent together with a solution containing a transition metal (Me) to a reaction tank kept alkaline, thereby coprecipitating the transition metal hydroxide. The complexing agent may be ammonia, ammonium sulfate, ammonium nitrate, etc., and is preferably ammonia. A precursor having a higher tap density can be produced by a crystallization reaction using a complexing agent. It is preferable to use a reducing agent together with the complexing agent. As the reducing agent, hydrazine, sodium borohydride, etc. can be used, and hydrazine is preferable in order to obtain a lithium transition metal composite oxide having a high press density of the active material. The alkali metal hydroxide (neutralizing agent) may be sodium hydroxide, lithium hydroxide or potassium hydroxide.

[0059] In preparing a hydroxide precursor, Mn among Ni, Co, and Mn is easily oxidized, and it is not easy to prepare a coprecipitated precursor in which Ni, Mn, or Ni, Co, and Mn are uniformly distributed in a divalent state, so that uniform mixing of Ni, Mn, or Ni, Co, and Mn at the atomic level is likely to be insufficient. In the composition range of the second embodiment of the present invention, the molar ratio Mn / Me of Mn to Me is 0.4 or more, so it is important to remove dissolved oxygen in the aqueous solution. As a method for removing dissolved oxygen, a method of bubbling a gas that does not contain oxygen (O2) can be mentioned. As the gas that does not contain oxygen, it is not limited, but nitrogen gas, argon gas, etc. can be used.

[0060] As described above, the pH (reaction pH in the reaction tank) in the step of producing a hydroxide precursor by coprecipitating Ni, Mn, or a compound containing Ni, Co, and Mn in a solution is preferably 10.2 or less in order to obtain a precursor containing αMe(OH)2 and βMe(OH)2 with a high tap density. In addition, by setting the pH at the above level, the particle growth rate can be promoted, so that the stirring time after the end of the dropwise addition of the raw material aqueous solution can be shortened. If the pH is too low, a precursor of αMe(OH)2 single phase will be obtained (see Example 1-12 described later), so the reaction pH is preferably more than 9.

[0061] The fact that the precursor is a mixed phase of αMe(OH)2 and βMe(OH)2 is determined by the above-mentioned X-ray diffraction measurement. As shown in FIG. 6, the αNi(OH)2 type crystal structure (αMe(OH)2) has the largest peak at 2θ=10° to 12°, and the βNi(OH)2 type crystal structure (βMe(OH)2) has the largest peak at 2θ=18° to 20°. Therefore, after background processing using the attached software, the maximum value of the peak intensity at 2θ=10° to 12° is used as the numerator, and the maximum value of the peak intensity at 2θ=18° to 20° is used as the denominator. 11 / I 19 By calculating this, it is possible to determine the degree to which αMe(OH)2 and βMe(OH)2 are mixed.

[0062] I11 / I 19 The lower limit is preferably 0.04, more preferably 0.05, and most preferably 0.08. 11 / I 19 The upper limit of is preferably 3.0, more preferably 2.0, and more preferably 1. .0 is most preferred.

[0063] In addition, a method of using a transition metal carbonate precursor as a precursor of a positive electrode active material for a non-aqueous electrolyte secondary battery is also known. However, when a transition metal carbonate precursor is used, gas (mainly carbon dioxide) is generally generated from the precursor during the firing process. This gas generation generates many voids in the positive electrode active material, so that the press density of the positive electrode active material becomes small.

[0064] Examples of raw materials for the hydroxide precursor include manganese oxide, manganese carbonate, manganese sulfate, manganese nitrate, manganese acetate, etc. as Mn compounds, nickel hydroxide, nickel carbonate, nickel sulfate, nickel nitrate, nickel acetate, etc. as Ni compounds, and cobalt sulfate, cobalt nitrate, cobalt acetate, etc. as Co compounds.

[0065] A preferred method is to drop a mixed alkali solution containing an alkali metal hydroxide (neutralizing agent) such as sodium hydroxide, a complexing agent such as ammonia, and a reducing agent such as hydrazine while the raw material aqueous solution of the hydroxide precursor (aqueous solution containing a transition metal) is being dropped. The concentration of the alkali metal hydroxide to be dropped is preferably 1.0M or more and 8.0M or less. The concentration of the complexing agent is preferably 0.4M or more, more preferably 0.6M or more. Also, it is preferably 2.0M or less, more preferably 1.6M or less, and even more preferably 1.5M or less. The concentration of the reducing agent is preferably 0.05M or more and 1.0M or less, more preferably 0.1M or more and 0.5M or less. By lowering the pH of the reaction tank and setting the concentration of ammonia (complexing agent) to 0.6M or more, the tap density of the hydroxide precursor can be increased.

[0066] The dripping speed of the raw material aqueous solution has a large effect on the uniformity of element distribution within one particle of the hydroxide precursor to be produced. In particular, care must be taken with Mn, as it is difficult to form a uniform element distribution with Ni and Co. A preferred dripping speed is 30 mL / min or less, although it is influenced by the size of the reaction vessel, stirring conditions, pH, reaction temperature, etc. In order to improve the discharge capacity, the dripping speed is more preferably 10 mL / min or less, and most preferably 5 mL / min or less.

[0067] In addition, when a complexing agent such as ammonia is present in the reaction vessel and certain convection conditions are applied, the rotation of the particles and the revolution in the stirring vessel are promoted by continuing the stirring after the end of the dripping of the raw aqueous solution, and in this process, the particles collide with each other and grow stepwise into concentric spheres. That is, the hydroxide precursor is formed through a two-stage reaction: a metal complex formation reaction when the raw aqueous solution is dripped into the reaction vessel, and a precipitation formation reaction that occurs while the metal complex is retained in the reaction vessel. Therefore, by appropriately selecting the time for continuing the stirring after the end of the dripping of the raw aqueous solution, a hydroxide precursor with a desired particle size can be obtained.

[0068] The preferred duration of stirring after the end of the dropwise addition of the raw material aqueous solution is preferably 0.5 hours or more, more preferably 1 hour or more, in order to grow the particles into uniform spherical particles, although it depends on the size of the reaction vessel, the stirring conditions, the pH, the reaction temperature, etc. Also, in order to reduce the risk of the particle size becoming too large and the output performance in the low SOC region of the battery becoming insufficient, the duration is preferably 15 hours or less, more preferably 10 hours or less, and most preferably 5 hours or less.

[0069] In addition, it is preferable that the cumulative volume in the particle size distribution of the hydroxide precursor and the secondary particles of the lithium transition metal composite oxide, that is, the particle size at 50%, D50 is 13 μm or less. To achieve this, for example, when the pH is controlled to 9.1 to 10.2, the stirring duration is preferably 1 hour to 3 hours.

[0070] When the hydroxide precursor particles are produced using a sodium compound such as sodium hydroxide as a neutralizing agent, it is preferable to wash and remove sodium ions attached to the particles in a subsequent washing step. For example, when the produced hydroxide precursor is extracted by suction filtration, washing conditions can be adopted in which the number of washings with 500 mL of ion-exchanged water is 6 or more times.

[0071] <Method of manufacturing lithium transition metal composite oxide> The lithium transition metal composite oxide contained in the positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention can be produced by mixing a lithium compound with the transition metal hydroxide precursor prepared as described above, and firing the mixture at 750° C. or more and 1000° C. or less. By setting the firing temperature within the above range, the crystallinity of the lithium transition metal composite oxide, as shown by FWHM(104), can be set within a range that satisfies the object of the present invention.

[0072] The lithium compound may be lithium hydroxide, lithium carbonate, lithium nitrate, lithium acetate, etc. However, the amount of the lithium compound is preferably about 1 mol % to 5 mol % in excess, in anticipation of the loss of a portion of the lithium compound during firing.

[0073] The firing temperature affects the reversible capacity of the active material. If the sintering temperature is too high, the obtained active material will collapse due to an oxygen releasing reaction, and the monoclinic Li[Li 1 / 3 Mn 2 / 3]O2 type phase tends to be observed as a separated phase, not as a solid solution phase. If too many such separated phases are included, it is not preferable because it leads to a decrease in the reversible capacity of the active material. In such materials, impurity peaks are observed around 35° and 45° on the X-ray diffraction diagram. Therefore, it is preferable that the firing temperature is lower than the temperature at which the oxygen release reaction of the active material is affected. The oxygen release temperature of the active material varies slightly depending on the composition of the active material, and when a lithium-excess active material is produced using the precursor according to the second embodiment, it is generally 1000°C or higher, but it is preferable to check the oxygen release temperature of the active material in advance. In particular, it has been confirmed that the oxygen release temperature of the hydroxide precursor shifts to the lower temperature side as the amount of Co contained in the sample increases, so caution is required. As a method for confirming the oxygen release temperature of an active material, a mixture of a hydroxide precursor and a lithium compound may be subjected to thermogravimetric analysis (TG-DTA measurement) in order to simulate the firing reaction process. However, this method has the risk of causing damage to the instrument by corroding the platinum used in the sample chamber of the measuring instrument due to the volatilized Li component. Therefore, it is better to first use a firing temperature of about 500°C to allow a certain degree of crystallization of the composition before subjecting it to thermogravimetric analysis.

[0074] On the other hand, if the sintering temperature is too low, crystallization does not proceed sufficiently, and the electrode properties tend to deteriorate. Sufficient crystallization reduces the resistance of the crystal grain boundaries and promotes smooth lithium ion transport. The inventors analyzed the half-width of the diffraction peak of the lithium-excess active material in detail, and found that in the sample synthesized at a temperature below 750°C, distortion remains in the lattice, and that the distortion can be almost completely removed by synthesizing at a temperature of 750°C or higher. It was also found that the size of the crystallite increases in proportion to the increase in the synthesis temperature. Therefore, in the case of using the precursor according to the second embodiment, it is preferable to manufacture the active material by adopting a baking temperature at which there is almost no distortion of the lattice in the system and the crystallite size can be sufficiently grown, specifically, a baking temperature at which the amount of distortion affecting the lattice constant is 2% or less and the crystallite size grows to 50 nm or more. When the electrode using this active material is charged and discharged, it was found that the crystallite size remains 30 nm or more even during the charge and discharge process, although it changes due to expansion and contraction. That is, by selecting the baking temperature as close as possible to the oxygen release temperature of the above-mentioned active material, it is possible to obtain an active material with a significantly large reversible capacity. It is possible.

[0075] As described above, the preferred firing temperature varies depending on the oxygen release temperature due to the composition of the active material. However, in order to obtain an active material having sufficient discharge capacity under the usage conditions assumed in the present invention, the firing temperature is preferably 750°C or higher and 1000°C or lower, and more preferably 750°C or higher and 950°C or lower.

[0076] <Positive electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery> As described above, another embodiment of the present invention is a positive electrode for a non-aqueous electrolyte secondary battery containing the positive electrode active material according to the embodiment, and yet another embodiment of the present invention is a non-aqueous electrolyte secondary battery including the positive electrode, a negative electrode, and a non-aqueous electrolyte. This will be described in detail.

[0077] ≪Positive electrode≫ The positive electrode includes a powder containing the positive electrode active material according to the embodiment as a main component, and may contain other components such as a conductive agent, a binder, a thickener, and a filler.

[0078] The powder of the positive electrode active material preferably has an average particle size of 100 μm or less. In particular, the powder of the positive electrode active material preferably has an average particle size of 15 μm or less in order to improve the high-output characteristics of the nonaqueous electrolyte battery. In order to obtain the powder in a predetermined shape, there are a method of preparing a precursor of a predetermined size, and a method using a grinder, a classifier, etc. For example, a mortar, a ball mill, a sand mill, a vibration ball mill, a planetary ball mill, a jet mill, a counter jet mill, a swirling airflow type jet mill, a sieve, etc. are used. When grinding, wet grinding in which water or an organic solvent such as hexane is coexistent can also be used. The classification method is not particularly limited, and a sieve, a wind classifier, etc. are used as necessary for both dry and wet methods.

[0079] The conductive agent is not limited as long as it is an electronically conductive material that does not adversely affect battery performance, but typically includes one or a mixture of conductive materials such as natural graphite (scale graphite, flake graphite, earthy graphite, etc.), artificial graphite, carbon black, acetylene black, ketjen black, carbon whiskers, carbon fibers, metal (copper, nickel, aluminum, silver, gold, etc.) powder, metal fibers, conductive ceramic materials, etc.

[0080] Among these, acetylene black is preferred as the conductive agent from the viewpoint of electronic conductivity and coating property. The amount of conductive agent added is preferably 0.1% by mass or more and 50% by mass or less, and particularly preferably 0.5% by mass or more and 30% by mass or less, based on the total mass of the positive electrode or the negative electrode. In particular, it is preferable to use acetylene black after pulverizing it into ultrafine particles of 0.1 μm to 0.5 μm, since the required amount of carbon can be reduced. These mixing methods are physical mixing, and the ideal is uniform mixing. Therefore, it is possible to mix in a dry or wet manner using a powder mixer such as a V-type mixer, an S-type mixer, a mortar, a ball mill, or a planetary ball mill.

[0081] The binder may be one or a mixture of two or more of thermoplastic resins such as polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), polyethylene, polypropylene, etc., or polymers having rubber elasticity such as ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber, etc. The amount of binder added is preferably 1% by mass or more and 50% by mass or less, particularly preferably 2% by mass or more and 30% by mass or less, based on the total mass of the positive electrode or negative electrode.

[0082] There are no limitations on the filler, so long as it does not adversely affect the battery performance. Usually, olefin polymers such as polypropylene and polyethylene, amorphous silica, alumina, zeolite, glass, carbon, etc. are used. The amount of filler added is determined based on the total mass of the positive electrode or negative electrode. On the other hand, the amount added is preferably 30 mass % or less.

[0083] ≪Negative electrode≫ There is no limitation on the negative electrode active material used in the negative electrode of the nonaqueous electrolyte secondary battery. Any material that can absorb and release lithium ions may be selected. For example, Li[Li 1 / 3 Ti 5 / 3 Examples of such materials include titanium-based materials such as lithium titanate having a spinel-type crystal structure, represented by

[04] O4; alloy-based materials such as Si, Sb, and Sn-based materials; lithium metal; lithium alloys (lithium-silicon, lithium-aluminum, lithium-lead, lithium-tin, lithium-aluminum-tin, lithium-gallium, and lithium metal-containing alloys such as Wood's alloy); lithium composite oxides (lithium-titanium); and silicon oxide; as well as alloys capable of absorbing and releasing lithium; and carbon materials (for example, graphite, hard carbon, low-temperature fired carbon, amorphous carbon, etc.). The negative electrode active material is used in the form of a powder, similar to the positive electrode active material, and the negative electrode may contain other components, similar to the positive electrode.

[0084] <Preparation of positive and negative electrodes> The positive and negative electrodes are preferably produced by kneading the main components (active materials) and other materials to prepare a mixture, mixing the mixture with an organic solvent such as N-methylpyrrolidone or toluene or water, and then applying or pressing the resulting mixture onto a current collector described in detail below and heat-treating it for about 2 hours at a temperature of about 50° C. to 250° C. The coating method is preferably, for example, coating to any thickness and shape using a means such as roller coating, such as an applicator roll, screen coating, a doctor blade method, spin coating, or a bar coater, but is not limited thereto.

[0085] As the current collector, a current collector foil such as aluminum foil or copper foil can be used. Aluminum foil is preferable as the current collector foil for the positive electrode, and copper foil is preferable as the current collector foil for the negative electrode. The thickness of the current collector foil is preferably 10 μm or more and 30 μm or less. In addition, the thickness of the mixture layer after pressing is preferably 40 μm or more and 150 μm or less (excluding the thickness of the current collector foil).

[0086] <Non-aqueous electrolyte> The nonaqueous electrolyte used in the nonaqueous electrolyte secondary battery according to still another embodiment of the present invention is not limited, and any nonaqueous electrolyte proposed for use in lithium batteries or the like can be used. Examples of non-aqueous solvents used in the non-aqueous electrolyte include cyclic carbonates such as propylene carbonate, ethylene carbonate, butylene carbonate, and chloroethylene carbonate, or fluorides thereof; cyclic esters such as γ-butyrolactone and γ-valerolactone; chain carbonates such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; chain esters such as methyl formate, methyl acetate, and methyl butyrate; tetrahydrofuran or a derivative thereof; ethers such as 1,3-dioxane, 1,4-dioxane, 1,2-dimethoxyethane, 1,4-dibutoxyethane, and methyl diglyme; nitriles such as acetonitrile and benzonitrile; dioxolane or a derivative thereof; ethylene sulfide or a derivative thereof, and the like, used alone or in mixtures of two or more of these.

[0087] Among these, it is particularly preferable to use a non-aqueous electrolyte in which the non-aqueous solvent contains a fluorinated cyclic carbonate. Examples of the fluorinated cyclic carbonate include 4-fluoroethylene carbonate, 4,4-difluoroethylene carbonate, 4,5-difluoroethylene carbonate, 4,4,5-trifluoroethylene carbonate, and 4,4,5,5-tetrafluoroethylene carbonate. Among these, it is preferable to use 4-fluoroethylene carbonate (FEC) in that it can suppress battery swelling caused by gas generation in the battery. The content of the fluorinated cyclic carbonate in the non-aqueous solvent is preferably 3% or more and 30% or less, and more preferably 5% or more and 25% or less, in terms of volume ratio.

[0088] <Method for measuring internal resistance after storage> By using a non-aqueous electrolyte containing a fluorinated cyclic carbonate as the non-aqueous solvent, an increase in internal resistance after storage can be suppressed. In this specification, the internal resistance after storage is measured under the following conditions. The completed battery is fully charged under normal use conditions. It is then left at 45°C for 15 days, and then discharged at a constant current of 0.2C until the closed circuit voltage between the terminals reaches the voltage that is expected to be reached during normal use. The battery is then opened and left for 2 hours or more. This completes the fully discharged state of the non-aqueous electrolyte battery. Using an impedance meter that applies 1 kHz alternating current (AC), measure the resistance between the positive and negative terminals at 25°C. Overcharged or overdischarged non-aqueous electrolyte batteries should not be measured.

[0089] The non-aqueous solvent according to the present embodiment may contain additives generally used in non-aqueous electrolyte secondary batteries, provided that the effects of the present invention are not impaired. Examples of additives include aromatic compounds such as biphenyl, alkylbiphenyl, terphenyl, partially hydrogenated terphenyl, cyclohexylbenzene, t-butylbenzene, t-amylbenzene, diphenyl ether, and dibenzofuran; partially fluorinated compounds of the aromatic compounds such as 2-fluorobiphenyl, o-cyclohexylfluorobenzene, and p-cyclohexylfluorobenzene; overcharge inhibitors such as fluorine-containing anisole compounds such as 2,4-difluoroanisole, 2,5-difluoroanisole, 2,6-difluoroanisole, and 3,5-difluoroanisole; negative electrode film-forming agents such as vinylene carbonate, methylvinylene carbonate, ethylvinylene carbonate, succinic anhydride, glutaric anhydride, maleic anhydride, citraconic anhydride, glutaconic anhydride, itaconic anhydride, and cyclohexanedicarboxylic anhydride; and ethylene sulfite and sulfite. Propylene, dimethyl sulfite, propane sultone, propene sultone, butane sultone, methyl methanesulfonate, busulfan, methyl toluenesulfonate, dimethyl sulfate, ethylene sulfate, sulfolane, dimethyl sulfone, diethyl sulfone, dimethyl sulfoxide, diethyl sulfoxide, tetramethylene sulfoxide, diphenyl sulfide, 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane, 4-methylsulfonyloxymethyl-2,2-dioxo-1,3,2-dioxathiolane, thioanisole, diphenyl disulfide, dipyridinium disulfide, perfluorooctane, tristrimethylsilyl borate, tristrimethylsilyl phosphate, tetrakistrimethylsilyl titanate, lithium monofluorophosphate, lithium difluorophosphate, etc. can be added to the non-aqueous electrolyte alone or in combination of two or more kinds. The content ratio of these compounds in the non-aqueous solvent is not particularly limited, but is preferably 0.01 mass% or more, more preferably 0.1 mass% or more, and even more preferably 0.2 mass% or more, with respect to the entire non-aqueous solvent, and the upper limit is preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 2 mass% or less. The purpose of adding these compounds includes improving charge / discharge efficiency, suppressing an increase in internal resistance, suppressing battery swelling, improving cycle performance, etc.

[0090] Examples of electrolyte salts used in the non-aqueous electrolyte include LiClO4, LiBF4, LiAsF6, LiPF6, LiSCN, LiBr, LiI, Li2SO4, and Li2B 10 Cl 10 , NaClO4, NaI, NaSCN, NaBr, KClO4, KSCN and other inorganic ion salts containing one of lithium (Li), sodium (Na) or potassium (K), LiCF3SO3, LiN(CF3SO2)2, LiN(C2F5SO2)2, LiN(CF3SO2)(C4F9SO2), LiC(CF3SO2)3, LiC(C2F5SO2)3, (CH3)4NBF4, (CH3)4NBr, (C2H5)4NClO4, (C2H5 )4NI, (C3H7)4NBr, (n-C4H9)4NClO4, (n-C4H9)4NI, (C2H5)4N-maleate, (C2H5)4N-benzoate, (C2H5)4N-phthalate, lithium stearylsulfonate, lithium octylsulfonate, lithium dodecylbenzenesulfonate, and other organic ion salts. These ionic compounds can be used alone or in combination of two or more.

[0091] Furthermore, by mixing LiPF6 or LiBF4 with a lithium salt having a perfluoroalkyl group such as LiN(C2F5SO2)2, the viscosity of the electrolyte can be further reduced, so that the low-temperature characteristics can be further improved and self-discharge can be suppressed, which is more preferable. Furthermore, a room temperature molten salt or an ionic liquid may be used as the non-aqueous electrolyte.

[0092] In order to reliably obtain a nonaqueous electrolyte battery having high battery characteristics, the concentration of the electrolyte salt in the nonaqueous electrolyte is preferably 0.1 mol / L to 5 mol / L, and more preferably 0.5 mol / L to 2.5 mol / L.

[0093] <Separator> As the separator for the non-aqueous electrolyte secondary battery, it is preferable to use a porous film or a nonwoven fabric, which exhibits excellent high-rate discharge performance, either alone or in combination. Examples of materials constituting the separator for nonaqueous electrolyte batteries include polyolefin resins such as polyethylene and polypropylene, polyester resins such as polyethylene terephthalate and polybutylene terephthalate, polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, vinylidene fluoride-perfluorovinyl ether copolymer, vinylidene fluoride-tetrafluoroethylene copolymer, vinylidene fluoride-trifluoroethylene copolymer, vinylidene fluoride-fluoroethylene copolymer, vinylidene fluoride-hexafluoroacetone copolymer, vinylidene fluoride-ethylene copolymer, vinylidene fluoride-propylene copolymer, vinylidene fluoride-trifluoropropylene copolymer, vinylidene fluoride-tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-ethylene-tetrafluoroethylene copolymer, and the like.

[0094] The porosity of the separator is preferably 98% by volume or less from the viewpoint of strength, and is preferably 20% by volume or more from the viewpoint of charge / discharge characteristics.

[0095] The separator may be a polymer gel composed of an electrolyte and a polymer such as acrylonitrile, ethylene oxide, propylene oxide, methyl methacrylate, vinyl acetate, vinylpyrrolidone, polyvinylidene fluoride, etc. Using the non-aqueous electrolyte in a gel state as described above is preferable in that it has an effect of preventing leakage.

[0096] Furthermore, it is preferable to use a polymer gel in combination with the above-mentioned porous membrane or nonwoven fabric as the separator, since this improves the electrolyte retention. That is, a film is formed on the surface and the wall surface of the micropores of a polyethylene microporous membrane, in which a solvent-philic polymer having a thickness of several μm or less is coated, and the electrolyte is retained in the micropores of the film, whereby the solvent-philic polymer gels.

[0097] Examples of the solvent-philic polymer include polyvinylidene fluoride, and polymers obtained by crosslinking acrylate monomers having ethylene oxide groups or ester groups, epoxy monomers, monomers having isocyanate groups, etc. The monomers can be crosslinked by irradiation with electron beams (EB), or by adding a radical initiator and then heating or irradiating with ultraviolet rays (UV).

[0098] <Configuration of non-aqueous electrolyte secondary battery> The configuration of the nonaqueous electrolyte secondary battery according to still another embodiment of the present invention is not particularly limited, and may be a cylindrical battery having a positive electrode, a negative electrode, and a roll-shaped separator, or a square battery ( Examples include rectangular batteries and flat batteries. FIG. 7 shows an external perspective view of a rectangular nonaqueous electrolyte secondary battery 1 according to one embodiment of the present invention. The figure is a see-through view of the inside of the container. In the nonaqueous electrolyte secondary battery 1 shown in FIG. 7, an electrode group 2 is housed in a battery container 3. The electrode group 2 is formed by winding a positive electrode having a positive electrode active material and a negative electrode having a negative electrode active material with a separator interposed therebetween. The positive electrode is electrically connected to a positive electrode terminal 4 via a positive electrode lead 4', and the negative electrode is electrically connected to a negative electrode terminal 5 via a negative electrode lead 5'.

[0099] <Configuration of the power storage device> An embodiment of the present invention also includes an electricity storage device in which a plurality of the above nonaqueous electrolyte secondary batteries are assembled. An electricity storage device 30 shown in Fig. 8 includes a plurality of electricity storage units 20. Each electricity storage unit 20 includes a plurality of nonaqueous electrolyte secondary batteries 1. The electricity storage device 30 can be mounted as a power source for automobiles such as electric vehicles (EVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs).

[0100] <Method of manufacturing and method of using non-aqueous electrolyte secondary battery> Yet another embodiment of the present invention includes assembling a nonaqueous electrolyte secondary battery using the positive electrode for a nonaqueous electrolyte secondary battery, and performing initial charging and discharging, + ) and exceeds 4.5V (vs. Li / Li + ) or less.

[0101] Further, still another embodiment of the present invention is a method for using a nonaqueous electrolyte secondary battery, the method comprising the steps of: + ) and exceeds 4.5V (vs. Li / Li + ) is used as a battery voltage.

[0102] That is, a nonaqueous electrolyte secondary battery according to yet another embodiment of the present invention is presumed to be manufactured without undergoing any charging process until the end of the flat region of the potential change, and to be used without charging until the end of the flat region of the potential change. The charging voltage employed in the charging process during manufacture and during use is preferably set so that the potential reached by the positive electrode through the charging, i.e., the upper limit charging potential, is equal to or lower than the potential at which the flat region of the potential change begins. The upper limit charging potential is, for example, 4.40 V (vs. Li / Li + The upper limit of the charging potential is 4.38V (vs. Li / Li + ) and 4.36V (vs. Li / Li +) and 4.34V (vs. Li / Li + ) and 4.32V (vs. Li / Li + ) may also be used. EXAMPLES

[0103] (Experimental Example 1) Experimental Example 1 is an example and a comparative example corresponding to a positive electrode active material for a non-aqueous electrolyte secondary battery according to one embodiment of the present invention. First, examples will be shown in which the production conditions for lithium transition metal composite oxides having the same composition were changed.

[0104] <Preparation of positive electrode active material (lithium transition metal composite oxide)> (Example 1-1) In preparing the example active material, a transition metal hydroxide precursor was prepared using a reactive crystallization method. First, 315.4 g of nickel sulfate hexahydrate, 168.6 g of cobalt sulfate heptahydrate, and 530.4 g of manganese sulfate pentahydrate were weighed out, and all of these were dissolved in 4 L of ion-exchanged water to prepare a 1.0 M sulfate aqueous solution with a Ni:Co:Mn molar ratio of 30:15:55. Next, 2 L of ion-exchanged water was poured into a 5 L reaction tank, and N2 gas was bubbled in for 30 minutes to remove oxygen contained in the ion-exchanged water. The temperature of the reaction tank was 50°C ( The temperature was set to ±2°C, and the inside of the reaction vessel was stirred at a rotation speed of 1500 rpm using a paddle blade equipped with a stirring motor, while sufficient convection was generated in the reaction vessel. The sulfate stock solution was dripped into the reaction vessel at a rate of 1.3 mL / min for 50 h. Here, from the start to the end of the dripping, a mixed alkaline solution consisting of 4.0 M sodium hydroxide, 1.25 M ammonia, and 0.1 M hydrazine was appropriately dripped to control the pH in the reaction vessel to always be kept at 9.8 (±0.1), and a part of the reaction liquid was discharged by overflow to control the total amount of the reaction liquid not to exceed 2 L at all times. After the dripping was completed, stirring in the reaction vessel was continued for another 1 h. After the stirring was stopped, the reaction vessel was left to stand at room temperature for 12 h or more. Next, the hydroxide precursor particles produced in the reaction tank were separated using a suction filter, and sodium ions attached to the particles were washed off using ion-exchanged water. The particles were then dried in an air atmosphere at normal pressure and 80°C for 20 hours using an electric furnace. After that, the particles were ground in an automatic agate mortar for several minutes to make the particle size uniform. In this way, a transition metal hydroxide precursor was produced.

[0105] 1.294 g of lithium hydroxide monohydrate was added to 2.262 g of the transition metal hydroxide precursor, and mixed thoroughly using an automatic agate mortar to prepare a mixed powder with a Li: (Ni, Co, Mn) molar ratio of 120:100. Using a pellet molding machine, the mixture was molded at a pressure of 13.5 MPa to obtain a pellet with a diameter of 25 mm. The amount of the mixed powder used for pellet molding was determined by converting it so that the mass of the expected final product was 2.5 g. One pellet was placed on an alumina boat with a total length of about 100 mm, placed in a box-type electric furnace (model number: AMF20), and heated from room temperature to 800 ° C. over 10 hours under normal pressure in an air atmosphere, and fired at 800 ° C. for 4 hours. The internal dimensions of the box-type electric furnace were 10 cm long, 20 cm wide, and 30 cm deep, with heating wires spaced 20 cm apart in the width direction. After firing, the heater was turned off and the alumina boat was left in the furnace to cool naturally. As a result, the temperature of the furnace dropped to about 200°C after 5 hours, but the temperature drop rate thereafter was somewhat slow. After a day and night, it was confirmed that the temperature of the furnace was below 100°C, and the pellets were taken out and crushed in an automatic agate mortar for several minutes to make the particle size uniform. In this way, the lithium transition metal composite oxide Li according to Example 1-1 was obtained. 1.09 Ni 0.27 Co 0.14 Mn 0.50 O2 was produced.

[0106] (Examples 1-2 to 1-5) The lithium transition metal composite oxides of Examples 1-2 to 1-5 were prepared in the same manner as in Example 1-1, except that the mixed powders of the transition metal hydroxide precursor and lithium hydroxide monohydrate were calcined at 850°C, 900°C, 1000°C, and 750°C, respectively.

[0107] (Examples 1-6 and 1-7) Lithium transition metal composite oxides according to Examples 1-6 and 1-7 were prepared in the same manner as in Example 1-1, except that in the preparation of the transition metal hydroxide precursor, the pH of the reaction vessel was set to 10.0 and 10.2.

[0108] (Examples 1-8 and 1-9) The lithium transition metal composite oxides of Examples 1-8 and 1-9 were prepared in the same manner as in Example 1-1, except that the mixed powders of the transition metal hydroxide precursor and lithium hydroxide monohydrate were calcined at 700° C. and 650° C., respectively.

[0109] (Examples 1-10 to 1-13) Lithium transition metal composite oxides according to Examples 1-10 to 1-12 were prepared in the same manner as in Example 1-1, except that in preparing the transition metal hydroxide precursor, the pH of the reaction vessel was set to 10.5, 10.7, and 9.0. Further, the same procedure as in Example 1-9 was carried out except that the pH of the reaction tank was set to 11.0. The lithium transition metal composite oxide according to 1-13 was prepared.

[0110] Next, examples and comparative examples in which the composition and / or production conditions of the lithium transition metal composite oxide were changed will be shown below.

[0111] (Examples 1 to 14) The lithium transition metal composite oxide of Example 1-14 was produced in the same manner as in Example 1-1, except that the composition of the transition metal hydroxide precursor was adjusted to have a Ni:Co:Mn molar ratio of 40:5:55, and the mixed powder of the transition metal hydroxide precursor and the lithium compound was adjusted to have a Li:(Ni, Co, Mn) molar ratio of 110:100.

[0112] (Examples 1 to 15) The lithium transition metal composite oxide of Example 1-15 was produced in the same manner as in Example 1-1, except that the composition of the transition metal hydroxide precursor was adjusted to a Ni:Co:Mn molar ratio of 45:5:50, the pH of the reaction tank in producing the transition metal hydroxide precursor was adjusted to 10.0, and the Li:(Ni, Co, Mn) molar ratio of the mixed powder of the transition metal hydroxide precursor and the lithium compound was adjusted to 110:100 and calcined at 850°C.

[0113] (Examples 1-16 to 1-29) The lithium transition metal composite oxides of Examples 1-16 to 1-29 were prepared in the same manner as in Example 1-1, except that the molar ratio of Ni:Co:Mn in the transition metal hydroxide precursor, the molar ratio Li / Me of the transition metal and lithium compound in the precursor, the pH of the reaction vessel, and the firing temperature of the precursor and the lithium compound were set to the conditions shown in Table 1 below.

[0114] (Comparative Examples 1-1 and 1-2) The composition of the transition metal hydroxide precursor was adjusted to a molar ratio of Ni:Co:Mn of 30:10:60, the ammonia concentration dropped into the reaction tank was 0.6 M, the hydrazine concentration was 0.3 M, and the pH of the reaction tank was 9.6 to produce the precursor, the molar ratio Li / Me of the transition metal to the lithium compound in the precursor was adjusted to 1.3, and the precursor was fired at the firing temperature shown in Table 1 below. Except for this, the lithium transition metal composite oxides of Comparative Examples 1-1 and 1-2 were produced in the same manner as in Example 1-1.

[0115] (Comparative Example 1-3) A lithium transition metal composite oxide of Comparative Example 1-3 was produced in the same manner as in Example 1-1, except that the mixed powder of the transition metal hydroxide precursor and the lithium compound was prepared so that the Li:Me molar ratio Li / Me was 1.0.

[0116] (Comparative Examples 1-4 and 1-5) The lithium transition metal composite oxides of Comparative Examples 1-4 and 1-5 were prepared in the same manner as in Example 1-1, except that the composition of the transition metal hydroxide precursor was adjusted to a molar ratio of Ni:Co:Mn of 33:33:33 (1:1:1), the pH of the reaction vessel was adjusted to 10.0, and the molar ratio Li / Me of the transition metal hydroxide precursor to the lithium compound was adjusted to 1.0 or 1.1, and the mixture was fired at 900°C.

[0117] <Confirmation of the crystal phase of the precursor> In order to confirm the crystal phase of the transition metal hydroxide precursors prepared in the above examples and comparative examples, measurements were performed using an X-ray diffractometer (manufactured by Rigaku, model name: MiniFlex II) according to the above-mentioned X-ray diffraction measurement method.

[0118] For reference, the results of X-ray diffraction measurement of the precursor are shown in FIG. 6. In Example 1-13, which was synthesized with the pH of the reaction tank set to 11.0, diffraction lines derived from the βNi(OH)2 crystal structure were observed. In Example 1-12, which was synthesized with the pH of the reaction tank set to 9.0, diffraction lines derived from the αNi(OH)2 crystal structure were observed. On the other hand, in Example 1-1, which was synthesized with the pH of the reaction tank set to 9.8, a mixed phase of the αNi(OH)2 crystal structure and the βNi(OH)2 crystal structure was observed. The αNi(OH)2 crystal structure had the largest peak at 2θ=10° to 12°, and the βNi(OH)2 crystal structure had the largest peak at 2θ=18° to 20°.

[0119] <Calculation of peak intensity ratio> The maximum peak intensity at 2θ = 10° to 12° is used as the numerator, and the maximum peak intensity at 2θ = 18° to 20° is used as the denominator. 11 / I 19 That is, I 11 / I 19 This can be said to be an index showing the extent to which α and β types are present. Here, background processing is performed by the attached software.

[0120] <Confirmation of the crystal structure and half-width of lithium transition metal composite oxide> The half-width of the lithium transition metal composite oxides according to the above-mentioned Examples and Comparative Examples was measured according to the above-mentioned conditions and procedures. It was confirmed that each of them had an α-NaFeO2 type crystal structure because the diffraction pattern matched the structural model in the X-ray diffraction measurement. In addition, the half-width FWHM(104) of the diffraction peak present at 2θ=44±1° on the X-ray diffraction diagram, which is indexed to the (104) plane in the space group R3-m, was determined using "PDXL", which is an accessory software of the X-ray diffraction device. In Examples 1-1 to 1-29 and Comparative Examples 1-1 and 1-2, a superlattice peak specific to the lithium-excess type positive electrode active material was observed in the range of 2θ=20° or more and 22° or less.

[0121] <Measurement of tap density and press density> The tap density and press density of the lithium transition metal composite oxides according to the above examples and comparative examples were measured according to the above-mentioned conditions and procedures.

[0122] <Preparation of Positive Electrode for Non-Aqueous Electrolyte Secondary Battery> The lithium transition metal composite oxides according to the above examples and comparative examples were used as the positive electrode active material to fabricate positive electrodes for non-aqueous electrolyte secondary batteries according to the examples and comparative examples in the following procedure.

[0123] A paste for coating was prepared by kneading and dispersing a positive electrode active material, acetylene black (AB) and polyvinylidene fluoride (PVdF) in a mass ratio of 90:5:5 using N-methylpyrrolidone as a dispersion medium. The paste for coating was applied to one side of an aluminum foil current collector having a thickness of 20 μm, dried, and pressed to prepare a positive electrode plate. The mass of the active material applied per fixed area and the porosity after pressing were adjusted to be the same in all examples and comparative examples.

[0124] <Preparation of non-aqueous electrolyte secondary battery> A portion of the positive electrode for a non-aqueous electrolyte secondary battery prepared as described above was cut out, and a test battery, which was a non-aqueous electrolyte secondary battery, was prepared by the following procedure. In order to accurately observe the independent behavior of the positive electrode, metallic lithium was attached to a nickel foil current collector as the counter electrode, i.e., the negative electrode, and a sufficient amount of metallic lithium was placed in the negative electrode so that the capacity of the nonaqueous electrolyte secondary battery would not be limited by the negative electrode.

[0125] The non-aqueous electrolyte was a solution in which LiPF6 was dissolved in a mixed solvent of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 6:7:7 to a concentration of 1 mol / L. A microporous polypropylene film with a surface modified with acrylate was used. A metal resin composite film consisting of polyethylene terephthalate (15 μm) / aluminum foil (50 μm) / metal adhesive polypropylene film (50 μm) was used for the exterior. The electrodes were stored so that the open ends of the positive and negative electrode terminals were exposed to the outside, and the fusion margins where the inner faces of the metal resin composite films faced each other were hermetically sealed except for the part that would become the liquid injection hole. After the nonaqueous electrolyte was injected, the liquid injection hole was sealed. Since the counter electrode is metallic lithium, the battery voltage (V) is the same as the positive electrode potential (V vs Li / Li + ) may be read as follows.

[0126] <Initial charge / discharge process> The nonaqueous electrolyte secondary batteries assembled by the above procedure were completed through an initial charge / discharge step, in which the batteries were divided into a first group to which initial charge / discharge condition 1 was applied and a second group to which initial charge / discharge condition 2 was applied.

[0127] (Initial charge / discharge condition 1) The first group of batteries was subjected to an initial charge / discharge process under the following conditions. In an environment of 25°C, charging was performed at a constant current and constant voltage of 0.1C and 4.35V, and the charge termination condition was the point when the current value decayed to 0.02C. Discharging was performed at a constant current of 0.1C and a termination voltage of 2.5V. This charging / discharging was performed for one cycle. A 10-minute rest period was provided after charging. The charge quantity and discharge capacity at this time were recorded as "charge quantity at 4.35 V charge" and "discharge capacity at 4.35 V charge", respectively. That is, "discharge capacity at 4.35 V charge" is an index representing the discharge capacity when a battery is manufactured without undergoing any charging process until the end of the flat region of the potential change and is used in a lower potential range without charging until the end of the flat region of the potential change.

[0128] (Initial charge / discharge condition 2) The second group of batteries was subjected to an initial charge / discharge process under the following conditions. In an environment of 25°C, charging was performed at a constant current and constant voltage of 0.1C and 4.6V, and the charge termination condition was the point when the current value decayed to 0.02C. Discharging was performed at a constant current of 0.1C and a termination voltage of 2.0V. This charging / discharging was performed for one cycle. A rest period of 10 minutes was provided after charging. The difference between the amount of charge at this time and the above-mentioned "amount of charge at 4.35 V" was calculated as the "amount of charge between 4.35 V and 4.6 V." In other words, the "amount of charge between 4.35 V and 4.6 V" is an index representing the amount of charge in a region where the potential change is flat.

[0129] <Overcharge test> Using the non-aqueous electrolyte secondary batteries according to the above examples and comparative examples, constant current (CC) charging was performed at a current value of 10 mA per 1 g of positive electrode mixture without setting an upper limit on the voltage. Here, the ratio of the capacity Y (mAh) at each voltage to the capacity X (mAh) at 4.45 V from the start of charging was defined as Z (= Y / X * 100 (%)), and the capacity ratio Z (%) when the positive electrode potential suddenly increased and the voltage reached 5.1 V was recorded as the "delay effect". The maximum value of dZ / dV was also determined.

[0130] The above results are shown in Tables 1 and 2.

[0131] [Table 1]

[0132] [Table 2]

[0133] The positive electrode active materials of Examples 1-1 to 1-13 shown in Tables 1 and 2 all have the same composition. The reaction pH for producing the transition metal hydroxide precursors was also the same, 9.8, and the precursors contained α-type and β-type crystal phases. In Examples 1-1 to 1-13, the composition of the lithium transition metal composite oxide satisfies the composition range of one embodiment of the present invention, so that the "discharge capacity at 4.35 V charge" is 120 mAh / g or more, the "charged electricity amount between 4.35 and 4.6 V" is large at 100 mAh / g or more, and the dZ / dV is 4.35 (vs. Li / Li + ) or more than 4.6V (vs. Li / Li + ) in the positive electrode potential range, the maximum value was 150 or more. Therefore, it can be said that this is a positive electrode active material for a non-aqueous electrolyte secondary battery that has a large discharge capacity even when charged at a relatively low voltage, and does not show a rapid increase in battery voltage even up to a higher SOC. In addition, in Examples 1-1 to 1-5 in which the precursor and the lithium compound were sintered at 750° C. or more and 1000° C. or less, the FWHM(104) of the lithium transition metal composite oxide was in the range of 0.2° or more and 0.6° or less, whereas in Examples 1-8 and 1-9 in which the sintering temperature was less than 750° C. In Example 1-9, a lithium transition metal composite oxide having a FWHM(104) exceeding 0.6° is obtained. It can also be seen that Examples 1-1 to 1-5, in which the firing temperature is 750° C. or more and 1000° C. or less, have a larger “4.35 V charge / discharge capacity” than Examples 1-8 and 1-9.

[0134] Examples 1-6, 1-7 and Examples 1-10 to 1-12 are examples in which the pH of the reaction vessel was set to 10.0, 10.2, 10.5, 10.7, and 9.0, respectively, compared to 9.8 in Example 1-1, in the preparation of the transition metal hydroxide precursor. Example 1-13 is an example in which the pH of the reaction vessel was set to 11.0 and the firing temperature was also set to 650 °C. In Examples 1-6 and 1-7 where the pH of the reaction vessel was 10.2 or less, the precursor contained α-type and β-type crystal phases, and the lithium transition metal composite oxide prepared using this precursor had a press density of 2.7 g / cm 3 exceeded. On the other hand, the precursor according to Examples 1-10, 1-11, and 1-13 where the pH of the reaction vessel exceeded 10.2 was a single β-phase, and in Example 1-12 where the pH of the reaction vessel was 9.0, it was a single α-phase. The lithium transition metal composite oxide prepared using the single-phase precursor according to Examples 1-10 to 1-13 did not exceed a press density of 2.7 g / cm 3 even when the firing temperature was 800 °C. In addition, Example 1-13 had a low firing temperature and a large FWHM(104) exceeding 0.6°, so the degree of crystallization was low. And it can be seen that Examples 1-1 to 1-7 have a larger "discharge capacity during charging at 4.35 V" than Examples 1-10 to 1-13.

[0135] According to Examples 1-14 to 1-29, the composition of the transition metal hydroxide precursor was adjusted so that the molar ratio Mn / Me was 0.4 ≦ Mn / Me < 0.6 and 0.2 < Ni / Me ≦ 0.6. In the preparation of the transition metal hydroxide precursor, the pH of the reaction vessel was set to 10.2 or less to prepare a hydroxide precursor containing α-Mn(OH)2 and β-Mn(OH)2. This precursor and a lithium compound were mixed so that the molar ratio Li / Me of Li to Me was 1.05 or more, and the lithium transition metal composite oxide obtained by firing at a temperature of 1000 °C or lower was used as a positive electrode active material. It can be seen that the battery has a large "discharge capacity during charging at 4.35 V" and a large "charge amount between 4.35 and 4.6 V". The above lithium transition metal composite oxide had a press density of 2.7 g / cm 3The FWHM(104) was within the range of 0.2° to 0.6°.

[0136] The lithium transition metal composite oxides according to Comparative Examples 1-1 and 1-2 have a molar ratio Mn / Me of 0.6 or more in the transition metal hydroxide precursor. It is clear that the batteries using these lithium transition metal composite oxides as the positive electrode active material have a large "charged electrical quantity between 4.35-4.6 V", but are unable to obtain a large "discharge capacity at 4.35 V charge". Furthermore, in the lithium transition metal composite oxide of Comparative Example 1-2, the calcination temperature of the transition metal hydroxide precursor and the lithium compound is low at 650°C, and the FWHM(104) exceeds 0.6°, indicating that the crystallization is insufficient.

[0137] The lithium transition metal composite oxide according to Comparative Example 1-3 has a molar ratio Mn / Me that satisfies the composition range of the present invention, but does not satisfy the composition range of the present invention in that the molar ratio Li / Me is 1.0 (not a lithium-excess type). It can be seen that the "discharge capacity at 4.35 V charge" is extremely small, even though the production conditions are the same as those of Example 1-1.

[0138] The lithium transition metal composite oxide according to Comparative Example 1-4 is an example of a LiMeO2 type active material having Ni:Co:Mn of 1:1:1 and Li / Me of 1.0. Unlike lithium-excess type active materials, the LiMeO2 type active material has a positive electrode potential of 5.0 V (vs. Li / Li + Even if you perform an initial charge of up to 4.5 (vs. Li / Li + ) or more 5.0V (vs.Li / Li + ) Within the potential range below this value, no region in which the potential change with respect to the amount of charged electricity is relatively flat is observed, and the amount of charged electricity between 4.35 and 4.6 V is small. The lithium transition metal composite oxide according to Comparative Example 1-5 has a Li / Me ratio of 1.1, but a Mn / Me ratio of 0.33, which is smaller than 0.4. The active material containing the lithium transition metal composite oxide according to Comparative Example 1-5 has a positive electrode potential of 5.0 V (vs. Li / Li + Even if you perform an initial charge of up to 4.5 (vs. Li / Li +) or more 5.0V (vs.Li / Li + ) Within the potential range below this value, no region in which the potential change with respect to the amount of charged electricity is relatively flat is observed, and the amount of charged electricity between 4.35 and 4.6 V is small. Therefore, it can be seen that the batteries of Comparative Examples 1-4 and 1-5 are unable to sufficiently expand the SOC until a sudden increase in battery voltage is observed when further current is forcibly applied beyond the fully charged state (SOC 100%).

[0139] Next, the effect of the molar ratio Mn / Me on the "discharge capacity upon charging at 4.35 V" will be considered. As described above, Comparative Examples 1-1 and 1-2, in which the molar ratio Mn / Me is 0.6, all have a small "4.35 V charge discharge capacity" of less than 120 mAh / g. In contrast, Examples 1 to 29, in which the molar ratio Mn / Me is less than 0.6, all have an excellent "4.35 V charge discharge capacity" of 120 mAh / g or more. Among them, Examples 1-15 to 1-1 to 1-7 and 1-19 to 1-28, in which the molar ratio Mn / Me is 0.50 or less, all have an even more excellent "4.35 V charge discharge capacity" of 140 mAh / g or more.

[0140] According to the findings of the present inventors, when the molar ratio Li / Me is 1.1 or more, a large "4.35 V charge-discharge capacity" may be obtained depending on the composition, but in order to obtain a large "charged electric quantity between 4.35-4.6 V", it is preferable to set the molar ratio Li / Me to 1.15 or more. For example, when comparing Example 1-14 and Example 1-29, which have the same conditions of the composition ratio of Ni:Co:Mn, reaction pH, and firing temperature except for the different molar ratio Li / Me, it can be seen that Example 1-29, which has a molar ratio Li / Me of 1.2, has a significantly improved "charged electric quantity between 4.35-4.6 V" compared to Example 1-14, which has a molar ratio Li / Me of 1.1. In addition, regarding the molar ratio Ni / Me, it is found that the "charged electrical quantity between 4.35 V and 4.6 V" is larger in Examples 1-18 and 1-19, in which the molar ratio Ni / Me is less than 0.6, than in Example 1-20, in which the molar ratio Ni / Me is 0.6, so that it is preferable to set the molar ratio Ni / Me to less than 0.6.

[0141] <Confirmation of the crystal structure of the electrode after charge / discharge test> Of the nonaqueous electrolyte secondary batteries after the charge-discharge test, for Examples 1-1, 1-6, 1-14, and 1-22, the batteries were disassembled and the positive electrode mixture was subjected to X-ray diffraction measurement according to the above procedure. A superlattice peak was observed for the secondary battery to which the initial charge / discharge condition 1 was applied. On the other hand, no superlattice peak was observed for the secondary battery to which the initial charge / discharge condition 2 was applied.

[0142] (Experimental Example 2) Experimental Example 2 is an example and a comparative example corresponding to a nonaqueous electrolyte secondary battery according to still another embodiment of the present invention.

[0143] (Example 2-1) <Preparation of lithium transition metal composite oxide> 284 g of nickel sulfate hexahydrate, 303 g of cobalt sulfate heptahydrate, and 443 g of manganese sulfate pentahydrate were weighed out, and all of these were dissolved in 4 L of ion-exchanged water to prepare a 1.0 M sulfate aqueous solution with a Ni:Co:Mn molar ratio of 27:27:46. Next, 2 L of ion-exchanged water was poured into a 5 L reaction vessel, and Ar gas was bubbled through it for 30 minutes to remove oxygen contained in the ion-exchanged water. The temperature of the reaction vessel was 50°C (±2 The temperature was set to 1500°C, and the inside of the reaction tank was stirred at a rotation speed of 1500 rpm using a paddle blade equipped with a stirring motor, while sufficient convection was generated in the reaction layer. The sulfate aqueous solution was dripped into the reaction tank at a rate of 3 mL / min. From the start to the end of the dripping, a mixed alkaline solution consisting of 4.0 M sodium hydroxide, 0.5 M ammonia water, and 0.2 M hydrazine was appropriately dripped to control the pH in the reaction tank to always be 9.8 (±0.1), and a part of the reaction liquid was discharged by overflow to control the total amount of the reaction liquid not to exceed 2 L. After the dripping was completed, stirring in the reaction tank was continued for another 3 hours. After stirring was stopped, the reaction tank was left to stand at room temperature for 12 hours or more. Next, the hydroxide precursor particles produced in the reaction tank were separated using a suction filter, and sodium ions attached to the particles were washed off using ion-exchanged water. The particles were then dried in an air atmosphere at normal pressure and 80°C for 20 hours using an electric furnace. After that, the particles were ground in an automatic agate mortar for several minutes to make the particle size uniform. In this way, the hydroxide precursor was produced.

[0144] 0.971 g of lithium hydroxide monohydrate was added to 1.852 g of the hydroxide precursor, and mixed thoroughly using an automatic agate mortar to prepare a mixed powder with a molar ratio of Li: (Ni, Co, Mn) of 130:100. Using a pellet molding machine, the mixture was molded at a pressure of 6 MPa to obtain a pellet with a diameter of 25 mm. The amount of the mixed powder used for pellet molding was determined by converting it so that the mass of the expected final product was 2 g. One pellet was placed on an alumina boat with a total length of about 100 mm, placed in a box-type electric furnace (model number: AMF20), and heated from room temperature to 900 ° C. in an air atmosphere under normal pressure over 10 hours, and fired at 900 ° C. for 5 hours. The internal dimensions of the box-type electric furnace were 10 cm long, 20 cm wide, and 30 cm deep, with heating wires spaced 20 cm apart in the width direction. After firing, the heater was turned off and the alumina boat was left in the furnace to cool naturally. As a result, the temperature of the furnace dropped to about 200°C after 5 hours, but the rate of temperature drop thereafter was somewhat slow. After a day and night, it was confirmed that the temperature of the furnace was below 100°C, and the pellets were then taken out and lightly crushed in an agate mortar to make the particle size uniform. In this way, the lithium transition metal composite oxide Li 1.13 Ni 0.235 Co 0.235 Mn 0.40 O2 (hereinafter referred to as "LR") was prepared.

[0145] <Confirmation of crystal structure> The lithium transition metal composite oxide was subjected to X-ray diffraction measurement according to the above-mentioned conditions and procedures, and was confirmed to have an α-NaFeO2 type crystal structure.

[0146] <Preparation of positive electrode> A coating paste was prepared in which N-methylpyrrolidone was used as a dispersion medium, the above-mentioned lithium transition metal composite oxide was used as an active material, and the active material, acetylene black (AB) and polyvinylidene fluoride (PVdF) were kneaded and dispersed in a mass ratio of 90:5:5. The coating paste was applied to one side of an aluminum foil current collector with a thickness of 20 μm to prepare a positive electrode according to Example 1. Note that the mass of the active material applied per certain area and the coating thickness were unified so that the test conditions were the same for all the examples and comparative examples described below.

[0147] <Preparation of negative electrode> A negative electrode was prepared by placing metallic lithium foil on a nickel current collector, the amount of metallic lithium being adjusted so that the capacity of the battery was not limited by the negative electrode when combined with the positive plate.

[0148] <Assembly of non-aqueous electrolyte secondary battery> Using the positive electrode prepared as described above, a nonaqueous electrolyte secondary battery was assembled in the following manner. As the non-aqueous electrolyte, 0.5 mass% of lithium difluorophosphate (LiDFP) and 1 mass% of 4,4'-bis(2,2-dioxo-1,3,2-dioxathiolane) (compound A) were added to a mixed solvent of 4-fluoroethylene carbonate (FEC) / propylene carbonate (PC) / ethyl methyl carbonate (EMC) in a volume ratio of 1:1:8, and LiPF6 was dissolved in the solution to a concentration of 1 mol / L. As the separator, a microporous film made of polypropylene with a surface modification by polyacrylate was used. As the exterior body, a metal resin composite film consisting of polyethylene terephthalate (15 μm) / aluminum foil (50 μm) / metal adhesive polypropylene film (50 μm) was used. The positive electrode according to Example 1 and the negative electrode were housed in the exterior body with the separator interposed therebetween such that the open ends of the positive electrode terminal and the negative electrode terminal were exposed to the outside, and the fusion margin where the inner surfaces of the metal resin composite films faced each other was hermetically sealed except for a portion that would become a liquid injection hole, and after the nonaqueous electrolyte was injected, the liquid injection hole was sealed to assemble a nonaqueous electrolyte secondary battery.

[0149] <Initial charge / discharge process> The assembled non-aqueous electrolyte secondary battery was set to have an upper limit voltage of 4.25V during normal use, and was subjected to an initial charge / discharge process at 25°C. Charging was performed by constant current constant voltage (CCCV) charging at a current of 0.1C and a voltage of 4.25V, and the charge termination condition was the point when the current value attenuated to 1 / 6. Discharging was performed by constant current discharging at a current of 0.1C and a termination voltage of 2.0V. This charge / discharge was performed twice. Here, a rest period of 30 minutes was set after each charging and discharging, and the discharge capacity was confirmed. Through the above manufacturing steps, the nonaqueous electrolyte secondary battery according to Example 2-1 was completed.

[0150] (Comparative Example 2-1) Commercially available LiNi 0.5 Co 0.2 Mn 0.3 Except for using O2 (hereinafter referred to as "NCM523") as the positive electrode active material, the nonaqueous electrolyte secondary battery was assembled and initially charged and discharged in the same manner as in Example 2-1 to complete the nonaqueous electrolyte secondary battery according to Comparative Example 2-1.

[0151] (Comparative Example 2-2) The lithium transition metal composite oxide prepared in Example 2-1 was used as a positive electrode active material, and a nonaqueous electrolyte secondary battery was assembled in the same manner as in Example 2-1. The first charge in the initial charge / discharge process was performed at a voltage of 4.6 V (vs. Li / Li + ) was charged at a constant current, constant voltage (CCCV) at 100° C., and the same initial charge-discharge steps as in Example 2-1 were carried out to complete a nonaqueous electrolyte secondary battery according to Comparative Example 2-2.

[0152] (Example 2-2) The lithium transition metal composite oxide Li prepared in Example 2-1 1.13 Ni 0.235 Co 0.235 Mn 0.40358g of O2 was added to 200mL of 0.1M aluminum sulfate aqueous solution, and stirred at 25°C and 400 rpm for 30 seconds using a magnetic stirrer. Then, the mixture was separated into powder and filtrate by suction filtration. The obtained powder was dried in air at 80°C for 20 hours. Furthermore, heat treatment was performed in air at 400°C for 4 hours using the box-shaped electric furnace described above. In this way, a lithium transition metal composite oxide coated with an aluminum compound (hereinafter referred to as "LR-Al") was produced. Except for using this lithium transition metal composite oxide as a positive electrode active material, the nonaqueous electrolyte secondary battery was assembled and initially charged and discharged in the same manner as in Example 2-1, and the nonaqueous electrolyte secondary battery according to Example 2-2 was completed.

[0153] <Confirmation of X-ray diffraction peaks of positive electrode active material> X-ray diffraction measurements were performed under the conditions described above using the positive electrode mixtures collected from the nonaqueous electrolyte batteries according to Example 2-1 and Comparative Example 2-2 by the procedure and conditions described above. It was confirmed that, in the X-ray diffraction diagram using CuKα radiation, the positive electrode active material of Example 2-1 had a diffraction peak in the range of 20° to 22° (see the lower part of FIG. 2), whereas the positive electrode active material of Comparative Example 2-2 had no diffraction peak in the range of 20° to 22° (see the upper part of FIG. 2). reference).

[0154] <Overcharge test> Using the non-aqueous electrolyte secondary batteries according to the above examples and comparative examples, constant current (CC) charging was performed at a current value of 10 mA per 1 g of positive electrode mixture without setting an upper limit on the voltage. Here, the ratio of the capacity Y (mAh) at each voltage to the capacity X (mAh) at 4.45 V from the start of charging was defined as Z (= Y / X * 100 (%)), and the capacity ratio Z (%) when the positive electrode potential suddenly increased and the voltage reached 5.1 V was recorded as the "delay effect". The maximum value of dZ / dV was also determined.

[0155] Table 3 shows the delay effect (%) and the maximum value of dZ / dV in the overcharge test of the nonaqueous electrolyte secondary batteries according to Examples 2-1 and 2-2 and Comparative Examples 2-1 and 2-2.

[0156] [Table 3]

[0157] According to Table 3, in the nonaqueous electrolyte secondary battery according to Comparative Example 2-1 in which NCM523 was used as the active material in the positive electrode, the positive electrode potential rose sharply at Z of 135% in the overcharge test, and the voltage reached 5.1 V, indicating that the delay effect was insufficient. This is because, in the overcharge test, when charging was performed without setting an upper limit on the voltage, the positive electrode of the nonaqueous electrolyte secondary battery according to Comparative Example 2-1 rose to 4.5 V (vs. Li / Li + ) or more 5.0V (vs.Li / Li + This is related to the fact that within the positive electrode potential range below 100 V, no flat region of potential change with respect to the amount of charging electricity is observed. In addition, the nonaqueous electrolyte secondary battery according to Comparative Example 2-2 uses a lithium-excess active material in the positive electrode, but in the overcharge test, a sudden rise in the positive electrode potential was observed when Z was 130%, and the delay effect was also insufficient. This is because, in the initial charge / discharge process, the positive electrode potential was 4.6 V (vs. Li / Li + ), so that in the overcharge test, when charging was performed without setting an upper limit on the voltage, the positive electrode of the nonaqueous electrolyte secondary battery according to Comparative Example 2 reached 4.5 V (vs. Li / Li + ) or more 5.0V (vs.Li / Li + This is related to the fact that within the positive electrode potential range below 100 V, no flat region of potential change with respect to the amount of charging electricity is observed. In contrast, a lithium-rich positive electrode was used as the active material, and the initial charge / discharge process was performed at 4.5 V (vs. Li / Li + In the nonaqueous electrolyte secondary batteries according to Examples 2-1 and 2-2, which were operated at a potential of less than 100 V, a superior delay effect was observed compared to Comparative Examples 2-1 and 2-2.

[0158] Next, nonaqueous electrolyte batteries were fabricated in which the composition of the nonaqueous electrolyte was changed from that of Example 2-1 or 2-2.

[0159] (Example 2-3) A nonaqueous electrolyte secondary battery according to Example 2-3 was completed by assembling the nonaqueous electrolyte secondary battery and performing initial charging and discharging in the same manner as in Example 2-1, except that the lithium transition metal composite oxide prepared in Example 1 was used as the positive electrode active material and the solvent of the nonaqueous electrolyte was changed to a mixed solvent of ethylene carbonate (EC) / propylene carbonate (PC) / ethyl methyl carbonate (EMC) in a volume ratio of 25:5:70.

[0160] (Examples 2-4) The nonaqueous electrolyte solvent was changed to that of Example 2-3, and 0.2 mass % of vinylene carbonate (VC) was further added as an additive. In the same manner as in Example 1, except that, a nonaqueous electrolyte secondary battery was assembled and an initial charge / discharge was performed to complete a nonaqueous electrolyte secondary battery according to Example 2-4.

[0161] (Examples 2-5) A nonaqueous electrolyte secondary battery according to Example 2-5 was completed in the same manner as in Example 2-1, except that the solvent for the nonaqueous electrolyte was changed to a mixed solvent in which FEC / EMC had a volume ratio of 20:80.

[0162] (Examples 2-6) A nonaqueous electrolyte secondary battery according to Example 2-6 was completed in the same manner as in Example 2-1, except that the solvent for the nonaqueous electrolyte was changed to a mixed solvent in which FEC / EMC had a volume ratio of 5:95.

[0163] (Examples 2-7 and 2-8) The lithium transition metal composite oxide coated with the aluminum compound prepared in Example 2-2 was used as the positive electrode active material, and the solvent of the nonaqueous electrolyte was changed to the same as in Examples 3 and 4, respectively. Except for this, the assembly and initial charge / discharge of nonaqueous electrolyte secondary batteries were performed in the same manner as in Example 2-1, to complete the nonaqueous electrolyte secondary batteries of Examples 2-7 and 2-8.

[0164] <Preservation test> The internal resistance after storage was measured under the above-mentioned conditions for the nonaqueous electrolyte secondary batteries according to Examples 2-1 to 2-8. The results are shown in Table 4.

[0165] [Table 4]

[0166] According to Table 4, in Examples 2-1, 2-3 to 2-6 using LR as the positive electrode active material, the increase in internal resistivity after storage is more suppressed in the nonaqueous electrolyte secondary batteries according to Examples 2-1, 2-5, and 2-6 using a nonaqueous electrolyte containing FEC, compared to the nonaqueous electrolyte secondary batteries according to Examples 2-3 and 2-4 using a nonaqueous electrolyte not containing FEC. In addition, in Examples 2-2, 2-7, and 2-8 using LR-Al as the positive electrode active material, the increase in internal resistivity after storage is more suppressed in the nonaqueous electrolyte secondary battery according to Example 2-2 using a nonaqueous electrolyte containing FEC, compared to the nonaqueous electrolyte secondary batteries according to Examples 2-7 and 2-8 using a nonaqueous electrolyte not containing FEC. [Industrial Applicability]

[0167] By using a positive electrode active material containing the lithium transition metal composite oxide according to the present invention, a nonaqueous electrolyte secondary battery can be provided that has a large discharge capacity even when charged at a relatively low voltage and has improved safety. Therefore, this nonaqueous electrolyte secondary battery is useful as a nonaqueous electrolyte secondary battery for hybrid vehicles, electric vehicles, plug-in hybrid vehicles, etc. [Explanation of symbols]

[0168] 1A, 1B measurement probe 2A, 2B measurement surface 3A, 3B pedestal 6 Lateral body 7 Through hole 1 Non-aqueous electrolyte secondary battery 2 electrode groups 3 Battery container 4 Positive terminal 4' Positive lead 5 Negative terminal 5' Negative lead 20 Energy Storage Unit 30 Energy storage device

Claims

1. The maximum potential of the positive electrode in a fully charged state (SOC 100%) is 4.3 V (vs. Li / Li + ) and 4.5V (vs. Li / Li + ) a non-aqueous electrolyte secondary battery used at a battery voltage of less than The nonaqueous electrolyte secondary battery includes a positive electrode, a negative electrode, and a nonaqueous electrolyte, The positive electrode contains a positive electrode active material, The positive electrode active material contains a lithium transition metal composite oxide, The lithium transition metal composite oxide is It has an α-NaFeO 2 structure, The molar ratio Li / Me of Li to the transition metal (Me) is 1.05≦Li / Me<1.4; The transition metal (Me) includes Ni and Mn, or Ni, Co and Mn, the molar ratio of Mn to Me is 0.4≦Mn / Me<0.6; a molar ratio of Ni to Me, Ni / Me, of 0.2≦Ni / Me≦0.6; A non-aqueous electrolyte secondary battery that satisfies any one of the following (1) to (3): (1) In an X-ray diffraction diagram using CuKα radiation, the positive electrode active material exhibits a diffraction peak in the range of 20° to 22°. (2) When the positive electrode is charged until the positive electrode potential reaches 5.0 V (vs. Li / Li + ), a region in which the potential change with respect to the amount of charging electricity is relatively flat is observed within the positive electrode potential range of 4.5 V (vs. Li / Li + ) or more and 5.0 V (vs. Li / Li + ) or less. (3) In the dZ / dV curve when the positive electrode is charged until the positive electrode potential reaches 4.6 V (vs. Li / Li + ) (where Z is the capacity ratio (%) at each potential based on the capacity at which 4.35 V (vs. Li / Li + ) is reached from the start of charging, and V is the potential of the positive electrode), the maximum value of dZ / dV within the potential range of 4.35 V (vs. Li / Li + ) or more and 4.6 V (vs. Li / Li + ) or less is 150 or more.

2. 2. A method for using the nonaqueous electrolyte secondary battery according to claim 1, wherein the maximum potential of the positive electrode in a fully charged state (SOC 100%) is 4.3 V (vs. Li / Li + ) and 4.5V (vs. Li / Li + ) a method for using a non-aqueous electrolyte secondary battery.

3. A method for manufacturing a nonaqueous electrolyte secondary battery, comprising assembling a nonaqueous electrolyte secondary battery using a positive electrode for the nonaqueous electrolyte secondary battery, and performing initial charging and discharging, The positive electrode for the non-aqueous electrolyte secondary battery contains a positive electrode active material, The positive electrode active material contains a lithium transition metal composite oxide, The lithium transition metal composite oxide is It has an α-NaFeO 2 structure, The molar ratio Li / Me of Li to the transition metal (Me) is 1.05≦Li / Me<1.4; The transition metal (Me) contains Ni and Mn, or Ni, Co and Mn, and the molar ratio of Mn to Me, Mn / Me, is 0.4≦Mn / Me<0.6; a molar ratio of Ni to Me, Ni / Me, of 0.2≦Ni / Me≦0.6; The maximum potential of the positive electrode in the initial charge / discharge step is 4.3 V (vs. Li / Li + ) and 4.5V (vs. Li / Li + ) or less.

Citation Information

Patent Citations

  • JP1973077660A

  • Lithium-nickel-manganese-cobalt multiple oxide, method for producing the same, and application of the multiple oxide

    JP2008013405A

  • Non-aqueous electrolyte secondary battery

    JP2010050079A

  • Positive electrode active material for lithium secondary battery, method of manufacturing the same, and the lithium secondary battery

    JP2011113792A

  • Nonaqueous electrolyte secondary battery

    JP2012104335A