Polymer composite
Fibrillated cellulose fibers with inorganic particles enhance light resistance and mechanical properties in polymer composites, addressing production complexities and aggregation issues, resulting in improved environmental sustainability and performance.
Patent Information
- Application Number
- JP2022568639
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-03-04
- Filing Date
- 2022-03-07
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2042-03-07
AI Technical Summary
The production of nanocellulose from cellulose fibers is complicated and expensive, and cellulose fibers face issues such as aggregation and deterioration during polymer compounding, hindering their effective dispersion and reinforcing capabilities.
Incorporating fibrillated cellulose fibers with grown inorganic particles to form a polymer composite, which includes a polymeric matrix, microcellulose fibers, and a compatibilizer, with specific properties to enhance light resistance and mechanical strength.
The resulting polymer composite exhibits improved light resistance and mechanical properties, including a color difference value of 2≦ΔE* ab ≦15, tensile strength of 35 MPa or more, and flexural modulus of 1.0 GPa or more, while being environmentally friendly.
Smart Images

Figure 0007575014000003 
Figure 0007575014000004 
Figure 0007575014000005
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0029734 dated March 5, 2021 and Korean Patent Application No. 10-2022-0028337 dated March 4, 2022, and all contents disclosed in the documents of said Korean Patent Applications are incorporated herein by reference.
[0002] The present invention relates to polymer composites comprising fibrillated microcellulose fibers. [Background technology]
[0003] Pulp is a lignocellulosic fibrous material obtained by chemically or mechanically separating cellulose fibers from wood, fiber crops, waste paper, or rags. Cellulosic fibers are primarily used in the papermaking industry and are utilized as a raw material for nanocellulose.
[0004] Nanocellulose is being applied in research to improve the physical properties of polymers by combining them with polymers. Unlike glass fiber, which is used as a reinforcing material, polymer composites using environmentally friendly nanocellulose have the advantage of being easily reusable.
[0005] However, the process of producing nanocellulose from cellulose fibers is complicated and expensive. Also, cellulose fibers have the problem of deteriorating due to the high process temperature during the composite process with polymers. In addition, cellulose fibers and nanocellulose are prone to aggregation within the polymer composite, making it very difficult to disperse them at the nanoscale, which limits the ability to achieve sufficient reinforcing effects. Summary of the Invention [Problem to be solved by the invention]
[0006] The present invention provides a polymer composite that contains cellulose fibers as a reinforcing material, which is environmentally friendly and can exhibit improved light resistance. [Means for solving the problem]
[0007] A polymer composite according to an embodiment of the present invention will now be described.
[0008] In this specification, unless expressly stated otherwise, the terminology used is for the purpose of referring to particular embodiments only and is not intended to be limiting of the invention.
[0009] As used herein, the singular forms "a," "an," and "the" include the plural forms unless the context clearly dictates to the contrary.
[0010] As used herein, the meaning of "comprising" is to embody certain properties, regions, integers, steps, operations, elements, components and / or components, and does not exclude the presence or addition of other certain properties, regions, integers, steps, operations, elements, components and / or groups.
[0011] As used herein, "nanofiber" or "nanofibril" refers to a fiber having a short axis diameter on the nanometer scale, and "microfiber" refers to a fiber having a short axis diameter on the micrometer scale. For example, the microfiber may be composed of a bundle of the nanofibers.
[0012] As used herein, "fiber" refers to lignocellulosic fibrous material obtained by chemically or mechanically separating cellulose fibers from wood, fiber crops, waste paper, or rags.
[0013] As used herein, "pulp fibers," "cellulose fibers," or "microcellulose fibers" refer to microfibers made of cellulose. As used herein, "cellulose nanofibers" or "nanocellulose fibers" refer to nanofibers made of cellulose.
[0014] In this specification, "fibrillation" refers to the phenomenon in which the nanofibrils that form the internal structure of the microcellulose fibers are unraveled and the nanofibrils appear on the microcellulose fibers like fluff.
[0015] In this specification, "fibrillated cellulose fibers" refers to microcellulose fibers in which nanofibrils having nanometer-scale short axis diameters stand up like fluff on the microcellulose fibers as a result of the fibrillation.
[0016] As a result of the ongoing research of the inventors, it has been confirmed that fibrillated cellulose fibers obtained by growing inorganic particles on cellulose fibers can exhibit a polymer reinforcing effect equivalent to that of nanocellulose obtained by nano-sizing cellulose fibers.
[0017] In particular, the inorganic particles contained on the fibrillated cellulose fibers can delay fiber deterioration caused by high process temperatures during the composite process with polymers, thereby enabling the development of excellent reinforcing effects.
[0018] And, the inorganic particles contained on the fibrillated cellulose fibers make it possible to provide a polymer composite with improved light resistance.
[0019] According to one embodiment of the invention, a polymer matrix; microcellulose fibers; and a compatibilizer, A polymeric composite is provided that satisfies Formula 1:
[0020] [Formula 1] 2≦ΔE* ab <= 15
[0021] In the above formula 1, ΔE* ab is a color difference value exhibited by the polymer composite, and the color difference value is calculated by subtracting [(L* t -L*0) 2 +(a* t -a*0) 2 +(b* t -b*0) 2 ] 1 / 2 It is calculated by the formula: The L*0, a*0 and b*0 values are initial values of chromaticity exhibited by the polymer composite, Said L* t , a* t and b* t The value of the polymer composite is 0.75 W / (m 2 This is the chromaticity value of the polymer composite after being exposed to a light source (fluorescent UV lamp) for 480 hours under the conditions of (nm)@340 and 45±1°C.
[0022] The polymer composite comprises the microcellulose fibers and a compatibilizer dispersed within the polymer matrix.
[0023] The polymer matrix may be a thermoplastic resin.
[0024] As an example, the polymer matrix may be one or more polymers selected from the group consisting of polyolefins, polyamides, styrene-based polymers, and polycarbonates.
[0025] Specifically, the polymer matrix may be a polyolefin such as polyethylene, polyethylene-based copolymers, polypropylene, and polypropylene-based copolymers; an aliphatic polyamide such as nylon-6 and nylon-66; an aromatic polyamide such as aramid; a styrene-based polymer such as polystyrene, acrylonitrile-butadiene-styrene copolymer, styrene-maleic anhydride copolymer, styrene-acrylonitrile copolymer, and styrene-butadiene-styrene copolymer; a polycarbonate obtained by polymerizing a polyol including bisphenol A, polyether polyol, polyester polyol, or a mixture thereof with phosgene, and the like.
[0026] Preferably, the polymer matrix can comprise one or more polymeric resins selected from the group consisting of polyethylene, polyethylene-based copolymers, polypropylene (especially homopolypropylene), polypropylene-based copolymers, nylon-6, nylon-66, aramid, polystyrene, acrylonitrile-butadiene-styrene copolymers, styrene-maleic anhydride copolymers, styrene-acrylonitrile copolymers, and styrene-butadiene-styrene copolymers, and polycarbonates.
[0027] The polymer matrix may have a melt flow rate (MFR) of 40g / 10min to 70g / 10min, or 45g / 10min to 70g / 10min, or 45g / 10min to 65g / 10min, or 50g / 10min to 65g / 10min, or 50g / 10min to 60g / 10min, which is advantageous for the development of the effects of the present invention. The MFR of the polymer matrix is measured by the standard test method of ASTM D1238.
[0028] According to an embodiment of the invention, the polymer composite comprises the microcellulose fibers dispersed on the polymer matrix.
[0029] The microcellulose fibers refer to fibers having a minor axis diameter on the micrometer scale.
[0030] Preferably, the microcellulose fibers are cellulose fibers that have been fibrillated by the growth of inorganic particles.
[0031] The cellulose fibers may be natural cellulose fibers obtained from wood such as softwoods and hardwoods.
[0032] In general, fibrillation of microcellulose fibers refers to the phenomenon in which relatively large fibrils that form the membrane and internal structure of cellulose fibers are loosened by processes such as beating, and fine microfibrils stand on the surface like fluff.
[0033] In the present invention, the microcellulose fibers are cellulose fibers fibrillated by growing inorganic particles on the microcellulose fibers, i.e., the microcellulose fibers may be fibers in a state where some of the fibrils forming the microcellulose fibers have been loosened or defibrated by the growth of the inorganic particles on the microcellulose fibers.
[0034] FIG. 1 shows a schematic representation of (a) non-fibrillated microcellulose fibers and (b) microcellulose fibers containing nanofibrils and inorganic particles at magnification.
[0035] In Fig. 1(a), the non-fibrillated microcellulose fiber 100 is a fiber having a minor axis diameter on the micrometer scale. Referring to Fig. 1(b), when inorganic particles are grown on the cellulose fiber, some of the fibrils forming the microcellulose fiber 100' are dissolved by the growth of the inorganic particles 20, and fibers in a state in which the nanofibrils 11 stand up like fluff are formed on the microcellulose fiber 100'. In addition, the nanofibrils 11 can also be present inside the microcellulose fiber 100' due to fibrillation caused by the growth of the inorganic particles 20.
[0036] In one example, the microcellulose fibers include nanofibrils and inorganic particles, where the nanofibrils can be attached to the surface of the microcellulose fibers or present within the microcellulose fibers, and the inorganic particles can be attached to the nanofibrils or attached to the surface or within the microcellulose fibers.
[0037] In the microcellulose fibres comprising the nanofibrils and inorganic particles, the microcellulose fibres may have a minor axis diameter of 1 μm or more and 30 μm or less, alternatively 25 μm or less, alternatively 20 μm or less, alternatively 15 μm or less, alternatively 10 μm or less. Preferably, the microcellulose fibres may have an average minor axis diameter of 5 μm to 30 μm, alternatively 5 μm to 25 μm, alternatively 10 μm to 20 μm, alternatively 15 μm to 20 μm.
[0038] In the microcellulose fiber containing the nanofibrils and inorganic particles, the nanofibrils may have a minor axis diameter of 10 nm or more, alternatively 20 nm or more, alternatively 30 nm or more, alternatively 40 nm or more, alternatively 50 nm or more; and 400 nm or less, alternatively 350 nm or less, alternatively 300 nm or less, alternatively 250 nm or less, alternatively 200 nm or less, alternatively 150 nm or less, or alternatively 100 nm or less. Specifically, the nanofibrils may have a minor axis diameter of 10 nm to 400 nm, alternatively 10 nm to 350 nm, alternatively 10 nm to 300 nm, alternatively 20 nm to 300 nm, alternatively 20 nm to 250 nm, alternatively 30 nm to 250 nm, alternatively 30 nm to 200 nm, alternatively 40 nm to 200 nm, alternatively 40 nm to 150 nm, alternatively 50 nm to 150 nm, or alternatively 50 nm to 100 nm.
[0039] The length of the microcellulose fibers and the nanofibrils is not particularly limited.
[0040] The microcellulose fibers containing the nanofibrils and inorganic particles are produced by adding a reducing agent, catalyst, ligand, or mixtures thereof to a mixture containing microcellulose fibers, inorganic particle precursors, and a solvent to grow inorganic particles from the inorganic particle precursors distributed on the cellulose fibers.
[0041] As an example, the process includes providing a mixture including microcellulose fibers, inorganic particle precursors, and a solvent.
[0042] The solvent may be a compound capable of dissolving the inorganic particle precursor and swelling the microcellulose fiber. As an example, the solvent may be water, alcohol (e.g., lower alcohol such as methanol, ethanol, propanol, butanol, etc.), dimethyl sulfoxide, sodium hydroxide aqueous solution, ammonia aqueous solution, urea aqueous solution, or a mixture thereof.
[0043] The solvent can be used in an amount of 1,000 to 10,000 parts by weight per 100 parts by weight of the microcellulose fibers. Within the solvent content range, the microcellulose fibers are sufficiently swollen, the flowability of the inorganic particle precursor is ensured, and the inorganic particle precursor can be uniformly dispersed on the microcellulose fibers.
[0044] Depending on the type of inorganic particles grown on the microcellulose fibers, a polymer composite having various physical properties can be provided. That is, the inorganic particle precursor can be appropriately selected depending on the physical properties to be imparted to the polymer composite. As a non-limiting example, if the purpose is to impart antibacterial properties and heat resistance to the polymer composite, an inorganic particle precursor capable of growing zinc oxide can be selected.
[0045] For example, the inorganic particles may include one or more elements selected from the group consisting of copper, zinc, calcium, aluminum, iron, silver, platinum, palladium, ruthenium, iridium, rhodium, osmium, chromium, cobalt, nickel, manganese, vanadium, molybdenum, magnesium, strontium, titanium, zirconium, hafnium, and gallium. The components of the inorganic particles may be one or more.
[0046] The inorganic particle precursor may be a salt of one or more elements selected from the group consisting of copper, zinc, calcium, aluminum, iron, silver, platinum, palladium, ruthenium, iridium, rhodium, osmium, chromium, cobalt, nickel, manganese, vanadium, molybdenum, magnesium, strontium, titanium, zirconium, hafnium, and gallium. The salt may be an acetate, chloride, or nitrate. The inorganic particle precursor may be a silicon oxide precursor such as tetraethyl orthosilicate (TEOS).
[0047] The content of the inorganic particles may be 1 to 40 parts by weight relative to 100 parts by weight of the microcellulose fibers. Specifically, the content of the inorganic particles may be 1 part by weight or more, alternatively 5 parts by weight or more, alternatively 8 parts by weight or more; and 40 parts by weight or less, alternatively 35 parts by weight or less, alternatively 30 parts by weight or less, alternatively 25 parts by weight or less relative to 100 parts by weight of the microcellulose fibers. Preferably, the content of the inorganic particles may be 1 to 40 parts by weight, alternatively 5 to 40 parts by weight, alternatively 5 to 35 parts by weight, alternatively 8 to 35 parts by weight, alternatively 8 to 30 parts by weight, alternatively 8 to 25 parts by weight relative to 100 parts by weight of the microcellulose fibers.
[0048] The content of the inorganic particle precursor in the mixture can be controlled so that the content of the inorganic particles finally generated on the microcellulose fibers satisfies the above range. Within this range, the inorganic particle precursor is uniformly distributed on the microcellulose fibers, and sufficient fibrillation can be induced, enabling the development of improved light resistance.
[0049] The mixture is prepared by dissolving the inorganic particle precursor in the solvent and then adding microcellulose fibers, and agitating the mixture to swell the microcellulose fibers and simultaneously distribute the inorganic particle precursor evenly over the swollen microcellulose fibers.
[0050] The types and contents of the reducing agent, catalyst, and ligand added to the mixture can be appropriately selected according to the types and contents of the inorganic particle precursors added and the inorganic particles to be grown. As an example, the reducing agent can be sodium hydroxide (NaOH), a metal hydride-based, borohydride-based, borane-based, silane-based, hydrazine, or hydrazide-based reducing agent. The catalyst can be ammonia or urea. The ligand can be benzene-1,3,5-tricarboxylate.
[0051] 2 and 4 are scanning electron microscope (SEM) images of microcellulose fibers fibrillated by the growth of the inorganic particles according to Preparation Example 1 below.
[0052] Referring to FIG. 2, it can be seen that inorganic particles having a uniform particle size grew on the microcellulose fibers, causing fibrillation.
[0053] Referring to FIG. 4, it can be seen that (a) the metal element (zinc) and (b) oxygen are uniformly distributed on the fibrillated microcellulose fibers due to the growth of the inorganic particles.
[0054] Alternatively, the inorganic particles may be grown on the microcellulose fibers and then modified to provide additional physical properties. For example, after the inorganic particles are grown on the cellulose fibers, a process of modifying the inorganic particles by adding a lipophilic compound having a thiol group may be additionally performed. By modifying the inorganic particles to be lipophilic, the compatibility of the microcellulose fibers with the polymer matrix may be further improved. As the lipophilic compound having a thiol group, 1-decanethiol, 1-undecanethiol, 1-dodecanethiol, 1-tetradecanethiol, 1-pentadecanethiol, 1-hexadecanethiol, 1-octadecanethiol, etc. may be used.
[0055] The above-mentioned process results in microcellulose fibers containing the nanofibrils and inorganic particles.
[0056] According to an embodiment of the invention, the inorganic particles contained in the microcellulose fibers may have a minor axis diameter of 0.01 μm or more, alternatively 0.03 μm or more, alternatively 0.05 μm or more; and 10 μm or less, alternatively 7 μm or less, alternatively 5 μm or less. Preferably, the inorganic particles have a minor axis diameter of 0.01 μm to 10 μm, alternatively 0.03 μm to 7 μm, alternatively 0.05 μm to 5 μm.
[0057] If the particle size of the inorganic particles contained on the microcellulose fibers is too large, the inorganic particles may act as defects and the mechanical properties of the polymer composite may be reduced. Therefore, the particle size of the inorganic particles is preferably 10 μm or less, 7 μm or less, or 5 μm or less.
[0058] In order to improve light resistance while exerting the fibrillation effect of the microcellulose fibers due to the growth of the inorganic particles, it is preferable that the particle diameter of the inorganic particles is 0.01 μm or more, or 0.03 μm or more, or 0.05 μm or more.
[0059] The inorganic particles may be spherical particles having a diameter of 0.01 μm to 10 μm. The inorganic particles may also be columnar particles having one axial diameter of 0.01 μm to 10 μm and another axial diameter of 0.02 μm to 30 μm. The inorganic particles may include a mixture of the spherical particles and the columnar particles. The diameter of the inorganic particles is measured using a scanning electron microscope. As a non-limiting example, the diameter, minor axis diameter, or major axis diameter of 20 inorganic particles is measured using a scanning electron microscope, and then the average value is calculated by excluding the maximum and minimum values.
[0060] According to an embodiment of the invention, the inorganic particles are present in an amount of 1 part by weight or more, alternatively 5 parts by weight or more, alternatively 8 parts by weight or more, and 40 parts by weight or less, alternatively 35 parts by weight or less, alternatively 30 parts by weight or less, alternatively 25 parts by weight or less, based on 100 parts by weight of the microcellulose fibers. Preferably, the inorganic particles are present in an amount of 1 to 40 parts by weight, alternatively 5 to 40 parts by weight, alternatively 5 to 35 parts by weight, alternatively 5 to 30 parts by weight, alternatively 8 to 30 parts by weight, alternatively 8 to 25 parts by weight, based on 100 parts by weight of the microcellulose fibers.
[0061] In order to fully express the fibrillation effect and light resistance of the microcellulose fibers due to the growth of the inorganic particles, it is preferable that the inorganic particles are contained in an amount of 1 part by weight or more, or 5 parts by weight or more, or 8 parts by weight or more per 100 parts by weight of the microcellulose fibers.
[0062] However, if the inorganic particles are contained in the microcellulose fiber in excess, the compatibility with the polymer matrix may decrease, which may result in poor mechanical properties of the polymer composite. Also, if the inorganic particles are contained in excess, the inorganic particles may aggregate to form non-uniform aggregates, which may result in poor light resistance. Therefore, the inorganic particles are preferably contained in an amount of 40 parts by weight or less, 35 parts by weight or less, 30 parts by weight or less, or 25 parts by weight or less, based on 100 parts by weight of the microcellulose fiber.
[0063] Meanwhile, the polymer composite includes the compatibilizer dispersed on the polymer matrix, which is a component that helps the polymer matrix and the microcellulose fibers to blend well with each other.
[0064] As the compatibilizer, any of those known in the art to which the present invention pertains can be used, taking into consideration the specific type of the polymer matrix.
[0065] The compatibilizer may preferably be a modified polyolefin, which refers to a resin obtained by modifying a polyolefin with an unsaturated carboxylic acid or a derivative thereof.
[0066] The polyolefin forming the modified polyolefin may be a linear olefin such as ethylene, propylene, butene, pentene, hexene, and heptene; a cyclic olefin such as cyclopentene, cyclohexene, and 1,3-cyclopentadiene; or an aromatic ring-substituted olefin such as styrene.
[0067] The unsaturated carboxylic acid forming the modified polyolefin may be fumaric acid, maleic acid, itaconic acid, citraconic acid, aconitic acid, and anhydrides thereof.
[0068] As a non-limiting example, the modified polyolefin may be polypropylene or polyethylene grafted with 0.1-50% by weight of maleic anhydride.
[0069] Preferably, the modified polyolefin has an acid number of 1 mgKOH / g to 40 mgKOH / g, or 5 mgKOH / g to 40 mgKOH / g, or 5 mgKOH / g to 35 mgKOH / g, or 10 mgKOH / g to 35 mgKOH / g, which may be advantageous for the development of the effects of the present invention. The acid number means the amount of KOH in mg-KOH / g-polymer required to neutralize the acid functionality when measured by titration. The acid number is measured according to the standard test method of ASTM D-1386 (2010).
[0070] Such modified polyolefins can further improve the compatibility of the microcellulose fibers with the polymer matrix, thereby further improving the mechanical properties of the polymer composite.
[0071] According to an embodiment of the invention, the polymer composite may comprise 30-90% by weight of the polymer matrix, 5-60% by weight of the microcellulose fibers, and 1-20% by weight of the compatibilizer.
[0072] Alternatively, the polymer composite may comprise 35-90% by weight of the polymer matrix, 5-55% by weight of the microcellulose fibers, and 5-20% by weight of the compatibilizer.
[0073] Alternatively, the polymer composite may comprise 35-85% by weight of the polymer matrix, 5-55% by weight of the microcellulose fibers, and 5-15% by weight of the compatibilizer.
[0074] In order to provide a polymer composite containing an appropriate amount of matrix, the polymer matrix is preferably contained in the polymer composite at 30 wt % or more, or 35 wt % or more, and in order to achieve the improved light resistance according to the present invention, the polymer matrix is preferably contained in the polymer composite at 90 wt % or less, or 85 wt % or less.
[0075] In order to achieve the improved light resistance of the present invention, the microcellulose fiber is preferably contained in the polymer composite at 5% by weight or more. However, an excessive amount of reinforcing material may inhibit compatibility with the polymer matrix, which may result in a decrease in the mechanical properties of the polymer composite. Therefore, the microcellulose fiber is preferably contained in the polymer composite at 60% by weight or less, or 55% by weight or less.
[0076] In order to achieve appropriate compatibility, the compatibilizer is contained in the polymer composite in an amount of 1 wt % or more, or 5 wt % or more. However, an excessive amount of the compatibilizer may deteriorate the mechanical properties of the polymer composite. Therefore, the compatibilizer is preferably contained in the polymer composite in an amount of 20 wt % or less, or 15 wt % or less.
[0077] Optionally, the polymer composite includes a colorant, the addition of which can advantageously act to reduce the color difference value of the polymer composite, and the colorant is added in an amount of 0.1 to 5 wt %, alternatively 0.5 to 5 wt %, alternatively 1 to 5 wt %, alternatively 1 to 3 wt %, based on the total weight of the polymer matrix, the microcellulose fiber, and the compatibilizer.
[0078] According to an embodiment of the invention, the polymer composite is obtained by mixing the above-mentioned components in a mixer and then curing. As a non-limiting example, the above-mentioned components are mixed in a batch mixer at 100 to 180°C, and then a master batch is prepared in a pellet form, and the master batch is fed into an extruder for extrusion and injection to obtain the polymer composite.
[0079] According to an embodiment of the invention, the polymer composite can be environmentally friendly and exhibit improved light resistance by including the above-mentioned components.
[0080] As an example, the polymer composite has a color difference value (ΔE* ab ) can have:
[0081] [Formula 1] 2≦ΔE* ab <= 15
[0082] In the above formula 1, the color difference value (ΔE* ab ) is calculated by dividing the L*a*b* chromaticity values measured using a color difference meter by [(L* t -L*0) 2 +(a* t -a*0) 2 +(b* t -b*0) 2 ] 1 / 2 It is obtained by the formula:
[0083] Here, the L*0, a*0 and b*0 values are the initial values of the chromaticity exhibited by the polymer composite. t , a* t and b* t The value of the polymer composite is 0.75 W / (m 2 The chromaticity value of the polymer composite after exposure to a light source (fluorescent UV lamp) for 480 hours under the conditions of (nm)@340 and 45±1°C.
[0084] The color difference value can also be obtained by measuring the amount of change in chromaticity after a weather resistance test of the polymer composite according to the standard test method of ISO4892-3.
[0085] Preferably, the polymer composite may have a color difference value of 15.0 or less, alternatively 14.5 or less; and 1.0 or more, alternatively 1.5 or more, alternatively 2.0 or more. Specifically, the polymer composite may have a color difference value of 1.0 to 15.0, alternatively 1.5 to 15.0, alternatively 2.0 to 15.0, alternatively 1.0 to 14.5, alternatively 1.5 to 14.5, alternatively 2.0 to 14.5.
[0086] The polymer composite may exhibit a tensile strength of 35 MPa or more, alternatively 40 MPa or more, alternatively 42 MPa or more; and 65 MPa or less, alternatively 60 MPa or less, as measured by the standard test method of ASTM D638-5 on a dog-bone test piece (or dumbbell-shaped specimen) according to ASTM D638-5 standard produced from the polymer composite. Preferably, the polymer composite has a tensile strength of 35 to 65 MPa, alternatively 40 to 65 MPa, alternatively 40 to 60 MPa, alternatively 42 to 60 MPa.
[0087] ASTM D638 provides a standard test method for determining the tensile properties of plastics. Tensile properties for the polymer composites are performed using ASTM D638 specimen type 5. ASTM D638 is performed by applying a tensile force to the specimen and measuring the tensile properties of the specimen under stress. This is performed on a conventional tensile testing machine at a constant pulling speed ranging from 1 to 500 mm / min until the specimen fails (yields or breaks). The tensile strength is the amount of force that can be applied until the specimen yields or breaks.
[0088] As another example, the polymer composite may exhibit a flexural strength of 50 MPa or more, alternatively 55 MPa or more, and 85 MPa or less, alternatively 80 MPa or less, as measured by the standard test method of ISO 178 on a 80 mm x 10 mm x 4 mm test piece produced from the polymer composite. Preferably, the polymer composite may have the flexural strength of 50 to 85 MPa, alternatively 50 to 80 MPa, alternatively 55 to 80 MPa.
[0089] Furthermore, the polymer composite can exhibit a flexural modulus of 1.0 GPa or more, alternatively 1.5 GPa or more, alternatively 1.7 GPa or more; and 3.5 GPa or less, alternatively 3.2 GPa or less, alternatively 3.0 GPa or less, as measured in accordance with ISO 178 on a test piece produced from the polymer composite and having dimensions of 80 mm x 10 mm x 4 mm. Preferably, the polymer composite can exhibit a flexural modulus of 1.0 GPa to 3.5 GPa, alternatively 1.5 GPa to 3.5 GPa, alternatively 1.5 GPa to 3.2 GPa, alternatively 1.7 GPa to 3.2 GPa, alternatively 1.7 GPa to 3.0 GPa.
[0090] ISO 178 provides a standard test method for determining flexural properties for plastics by performing a three-point bend test. The three-point bend test applies a force to the midpoint of a rectangular specimen supported freely at both ends. The applied force is measured by a load cell and the resulting deflection is measured by crosshead displacement or a direct strain measurement device. This is done in a conventional flexural tester, applying a force to the specimen at a constant rate in the range of 1-500 mm / min. The flexural strength is the maximum flexural stress achieved during the flexural test. The flexural stress is measured by the flexural tester as a function of the applied load, span, specimen width, and specimen thickness.
[0091] The polymer composite is environmentally friendly and can exhibit improved light resistance, and can be used in a variety of applications, such as lightweight materials for automobiles, such as interior and exterior materials for automobiles, interior and exterior materials for home appliances, and packaging materials. Effect of the Invention
[0092] According to the present invention, there is provided a polymer composite that is environmentally friendly and exhibits improved light resistance by containing microcellulose fibers fibrillated by the growth of inorganic particles as a reinforcing material. [Brief description of the drawings]
[0093] [Figure 1] FIG. 1 shows a schematic representation of (a) non-fibrillated microcellulose fibers and (b) microcellulose fibers containing nanofibrils and inorganic particles at magnification. [Diagram 2] FIG. 2 is a scanning electron microscope (SEM) image of cellulose fibers fibrillated by inorganic particle growth according to Preparation Example 1 below. [Diagram 3] FIG. 3 is an SEM image of cellulose fibers fibrillated by the growth of inorganic particles according to Preparation Example 4 below. [Figure 4] FIG. 4 is a scanning electron microscope (SEM) image of cellulose fibers fibrillated by inorganic particle growth according to Preparation Example 1 below. [Diagram 5] FIG. 5(a) is an SEM image of the microfibrillated cellulose fibers composited with inorganic particles according to Production Example 5 below, and FIG. 5(b) is an SEM image of (a) taken at a higher magnification. [Figure 6] Figure 6 shows the standard for dog-bone shaped test pieces (or dumbbell-shaped specimens) for measuring tensile strength according to ASTM D638 Type V (unit: mm). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0094] The functions and effects of the present invention will be described in more detail below with reference to specific examples of the present invention, however, these are presented as examples for understanding the invention and are not intended to limit the scope of the invention in any way.
[0095] Manufacturing Example 1 (Production of fibrillated cellulose fibers) As a cellulose raw material, hardwood kraft fiber (average fiber length 0.692 mm, average minor axis diameter 15.8 μm) was prepared. An aqueous solution was prepared by dissolving 20 g of zinc acetate in 1000 g of distilled water. 20 g of the fiber was added to the aqueous solution and stirred at 200 rpm for 1 hour to obtain a mixture.
[0096] To the mixture, 7.2 g of sodium hydroxide (NaOH) was added as a reducing agent at 50° C., and the mixture was heated to 95° C. and stirred at 200 rpm for 4 hours to grow inorganic particles on the fibers. The content of the inorganic particles was confirmed to be 8 parts by weight per 100 parts by weight of the fibers.
[0097] A scanning electron microscope (SEM) confirmed that fibrillation had occurred in the fiber portion where the inorganic particles (ZnO) had grown, as shown in Figure 2. Analysis of the SEM image confirmed that the inorganic particles had a uniform particle size of approximately 100 nm (see Figure 2). In addition, it was confirmed that (a) metal element (zinc) and (b) oxygen were uniformly distributed on the fibrillated cellulose fibers due to the growth of the inorganic particles (see Figure 4).
[0098] Manufacturing Example 2 (Production of fibrillated cellulose fibers) Fibrillated cellulose fibers were produced in the same manner as in Preparation Example 1, except that the content of zinc acetate was adjusted so that the content of the inorganic particles was 12.5 parts by weight per 100 parts by weight of the fibers.
[0099] As a result of analyzing the SEM image, it was confirmed that the inorganic particles had a uniform particle size of about 100 nm.
[0100] Production Example 3 (Production of fibrillated cellulose fibers) Fibrillated cellulose fibers were produced in the same manner as in Preparation Example 1, except that the content of zinc acetate was adjusted so that the content of the inorganic particles was 25 parts by weight per 100 parts by weight of the fibers.
[0101] As a result of analyzing the SEM image, it was confirmed that the inorganic particles had a uniform particle size of about 100 nm.
[0102] Production Example 4 (Production of fibrillated cellulose fibers) Fibrillated cellulose fibers were produced in the same manner as in Production Example 1, except that calcium carbonate (CaCO3) was used instead of zinc acetate and the content of calcium carbonate was adjusted so that the content of the inorganic particles was 45 parts by weight per 100 parts by weight of the fibers.
[0103] Analysis of the SEM image revealed that the inorganic particles were composed of 100 nm particles agglomerated to form non-uniform aggregates (~1 μm) (see FIG. 3).
[0104] Production Example 5 (Production of fine cellulose fibers) As a cellulose raw material, hardwood kraft fiber was prepared in the same manner as in Production Example 1. The surface of the fiber was oxidized using 2,2,6,6-tetramethylpiperidinyl-1-oxy radical (TEMPO) as a catalyst to obtain oxidized pulp.
[0105] 1 g of the oxidized pulp was dispersed in 99 g of distilled water, and the dispersion was subjected to a pulverization (fibrillation) treatment in a mixer for 30 minutes to obtain an aqueous dispersion of pulverized cellulose with a concentration of 1%.
[0106] A zinc acetate solution was prepared by dissolving 20 g of zinc acetate in 1000 g of distilled water. A sodium hydroxide solution was prepared by dissolving 3.6 g of sodium hydroxide (NaOH) in 10 ml of distilled water.
[0107] While stirring 100 g of the fine cellulose aqueous dispersion at 15° C., 50 ml of the zinc acetate aqueous solution and 10 ml of the sodium hydroxide aqueous solution were added, and the mixture was stirred at 500 rpm for 2 hours to produce a composite of zinc oxide (ZnO) particles and fine cellulose.
[0108] As a result of observing using a scanning electron microscope, as shown in Figures 5(a) and (b), it was confirmed that the composite of zinc oxide particles and fine cellulose obtained in Preparation Example 5 had strong bonding and aggregation between the fine cellulose particles, resulting in clumping of nanofibers and reduced particle dispersion.
[0109] Example 1 30 wt% of the fibrillated cellulose fiber of Preparation Example 1, 60 wt% of homopolypropylene (melt flow rate (MFR) 60g / 10min according to the standard test method of ASTM D1238), and 10 wt% of a compatibilizer were added to a batch mixer and mixed at 160°C for 20 minutes to prepare a master batch in the form of pellets. As the compatibilizer, maleic anhydride-grafted polypropylene (acid value 20mgKOH / g according to the standard test method of ASTM D-1386 (2010)) was used.
[0110] The master batch was compounded and extruded in a twin screw extruder, and the extruded mixture was again fed into an injector and extruded to obtain a polymer composite test piece.
[0111] Example 2 A polymer composite test piece was obtained in the same manner as in Example 1, except that the fibrillated cellulose fibers according to Preparation Example 2 were used instead of Preparation Example 1.
[0112] Example 3 A polymer composite test piece was obtained in the same manner as in Example 1, except that the fibrillated cellulose fibers according to Preparation Example 3 were used instead of Preparation Example 1.
[0113] Example 4 A polymer composite test piece was obtained in the same manner as in Example 1, except that the fibrillated cellulose fiber of Preparation Example 3 was used instead of Preparation Example 1, and 3 wt% of black colorant (NB9096) was additionally added and mixed with the compounds added to the batch mixer to prepare a master batch.
[0114] Example 5 A polymer composite test piece was obtained in the same manner as in Example 1, except that 55 wt % of the fibrillated cellulose fiber from Preparation Example 3, 35 wt % of polypropylene, and 10 wt % of the compatibilizer were added to a batch mixer.
[0115] Example 6 A polymer composite test piece was obtained in the same manner as in Example 1, except that 5 wt % of the fibrillated cellulose fiber from Preparation Example 3, 85 wt % of polypropylene, and 10 wt % of the compatibilizer were added to a batch mixer.
[0116] Comparative Example 1 A polymer composite test piece was obtained in the same manner as in Example 1, except that the fibrillated cellulose fibers according to Preparation Example 4 were used instead of Preparation Example 1.
[0117] Comparative Example 2 A polymer composite test piece was obtained in the same manner as in Example 1, except that the hardwood kraft fiber used in Preparation Example 1 was immersed in water and swollen instead of the fibrillated cellulose fiber used in Preparation Example 1.
[0118] Comparative Example 3 A polymer composite test piece was obtained in the same manner as in Example 1, except that the fine cellulose fibers of Preparation Example 5 were used instead of Preparation Example 1.
[0119] Test Example The physical properties of the test pieces produced in the Examples and Comparative Examples were evaluated by the following methods, and the results are shown in Tables 1 and 2 below.
[0120] (1) Short axis diameter of fiber The minor axis diameter (the shortest diameter in the cross section of the fiber) of the cellulose fibers of the Production Examples was measured using a scanning electron microscope.
[0121] Specifically, for microcellulose fibers, the short axis diameter of 10 microfibers per sample was measured and expressed as a range excluding the maximum and minimum values; for nanofibrils, the short axis diameter of 20 nanofibrils per sample was measured and expressed as a range excluding the maximum and minimum values.
[0122] Unlike Production Examples 1 to 4, Production Example 5 is a product in which cellulose fibers are finely divided (defibrated) and then composited with particles. In Table 1 below, the minor axis diameter of the nanofibrils in Production Example 5 means the minor axis diameter of the finely divided cellulose after composited with particles.
[0123] (2) Light resistance Using a weather resistance tester (model name: QUV ACCELERATED WEATHERING TESTER, manufacturer: Q-LAB), the test piece was heated at 0.75 W / (m 2 The specimen was exposed to a light source (fluorescent UV lamp) at 340 nm and 45±1°C for 480 hours.
[0124] The chromaticity values of the test piece before and after exposure were measured using a color difference meter (model name: Ci7860, manufacturer: X-rite). From the measured L*a*b* chromaticity values, [(L* t -L*0) 2 +(a* t -a*0) 2 +(b* t-b*0) 2 ] 1 / 2 The color difference value (ΔE* ab ) was obtained.
[0125] In the above formula, the L*0, a*0 and b*0 values are the initial values of chromaticity exhibited by the test piece before the exposure; t , a* t and b* t The value is the chromaticity value exhibited by the test strip after said exposure.
[0126] (3) Tensile strength The following test specimen (FIG. 6) was prepared according to the standard of ASTM D638 Type V. The test specimen was left in a constant temperature and humidity room adjusted to a temperature of 23° C. and a relative humidity of 50% for 24 hours, and then used for the tensile test.
[0127] The tensile strength (MPa) of the test specimen was measured using a universal testing machine (UTM) manufactured by Instron in accordance with the standard test method of ASTM D638. Based on the standard test method of ASTM D638, the grip distance for holding the test specimen at both ends was set to 25.4 mm, and the test was performed at a constant tensile speed of 5 mm / min at a crosshead speed.
[0128] (4) Flexural strength and flexural modulus A test piece with a size of 80 mm x 10 mm x 4 mm was prepared according to the standard test method of ISO 178. The test piece was left in a constant temperature and humidity room adjusted to a temperature of 23°C and a relative humidity of 50% for 24 hours, and then used for a bending test.
[0129] The test pieces were subjected to measurement of flexural strength (MPa) according to ISO 178 using an Instron Universal Testing Machine (UTM). Based on ISO 178, a 3-point flexural test jig was used to set a supports span to 46 mm, and a flexural test was performed under test conditions of a crosshead speed of 5 mm / min to obtain the flexural strength.
[0130] [Table 1]
[0131] [Table 2]
[0132] Referring to Table 2, it can be seen that the polymer composites according to the examples have superior light resistance compared to the polymer composite according to Comparative Example 1.
Claims
1. a polymer matrix; microcellulose fibers; and a compatibilizer, The microcellulose fibers contain nanofibrils and zinc oxide, the zinc oxide growing on the fibers in particulate form; A polymer complex that satisfies the following formula 1: [Formula 1] 2≦ΔE* ab ≦15 In the above formula 1, ΔE* ab is a color difference value exhibited by the polymer composite, and the color difference value is calculated by subtracting [(L* t -L* 0 ) 2 + (a * t -a* 0 ) 2 + (b * t -b* 0 ) 2 ] 1/2 It is calculated by the formula: Said L* 0 , a * 0 and b* 0 value is an initial value of the chromaticity exhibited by the polymer composite, Said L* t , a * t and b* t The value of the polymer composite is 0.75 W / (m 2 Chromaticity is the chromaticity value of the polymer composite after 480 hours of exposure to a light source (fluorescent UV lamp) at 340 nm and 45±1° C.
2. The nanofibrils are attached to the surface of the microcellulose fibers; The zinc oxide is bound to the nanofibrils or to the surface or interior of the microcellulose fibers. The polymer composite of claim 1 .
3. The microcellulose fibers have a minor axis diameter of 1 μm to 30 μm, The nanofibrils have a minor axis diameter of 10 nm to 400 nm. The polymer complex according to claim 1 or 2.
4. The polymer composite according to any one of claims 1 to 3, wherein the zinc oxide comprises spherical particles having a diameter of 0.01 µm to 10 µm; columnar particles having one axis diameter of 0.01 µm to 10 µm and another axis diameter of 0.02 µm to 30 µm; or a mixture thereof.
5. The polymer composite according to any one of claims 1 to 4, wherein the zinc oxide is contained in an amount of 1 to 40 parts by weight per 100 parts by weight of the microcellulose fibers.
6. 30 to 90% by weight of said polymer matrix; 5 to 60% by weight of the microcellulose fibers; and 1 to 20% by weight of the compatibilizer The polymer complex of claim 1 , comprising:
7. The polymer composite according to claim 1 , wherein the polymer matrix is one or more polymers selected from the group consisting of polyolefins, polyamides, styrene-based polymers, and polycarbonates.
8. The polymer composite of claim 1 , wherein the compatibilizer comprises a modified polyolefin.
9. The polymer composite according to any one of claims 1 to 8, wherein a tensile strength measured according to ASTM D638-5 on an ASTM D638-5 standard test piece produced from the polymer composite is 35 MPa to 65 MPa.
10. The polymer composite according to any one of claims 1 to 9, wherein a test piece having a size of 80 mm x 10 mm x 4 mm produced from the polymer composite has a flexural strength of 50 MPa to 85 MPa as measured according to ISO 178.
11. The polymer composite according to any one of claims 1 to 10, wherein a flexural modulus measured according to ISO 178 for a test piece having a size of 80 mm x 10 mm x 4 mm produced from the polymer composite is 1.0 GPa to 3.5 GPa.
Citation Information
Patent Citations
Molded product composed of composite material and production method therefor
JP2011088997A
Composite filler, method for production thereof, and composite filler-blended resin composition
JP2012087199A
Microfibrillated cellulose and composite body
JP2016176055A
Cellulose resin composite
JP2017226754A
polymer composites
JP2022548882A