Solid oxide fuel cell and method for producing same
The solid oxide fuel cell design with a two-dimensional uneven intermediate layer reduces reaction resistance by enhancing contact area, addressing the inefficiency caused by reaction prevention films.
Patent Information
- Application Number
- JP2020145383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-08-31
AI Technical Summary
The provision of a reaction prevention film in solid oxide fuel cells increases reaction resistance during power generation.
A solid oxide fuel cell design featuring an electrolyte layer with a surface having oxide ion conductivity, an intermediate layer with two-dimensional unevenness on both the cathode and electrolyte sides, characterized by projections and depressions, to enhance contact area and reduce reaction resistance.
The design effectively reduces reaction resistance by increasing the contact area between the intermediate layer and the cathode, thereby improving power generation efficiency.
Smart Images

Figure 0007575218000002 
Figure 0007575218000003 
Figure 0007575218000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a solid oxide fuel cell. [Background technology]
[0002] A solid oxide fuel cell has a structure in which a solid oxide electrolyte is sandwiched between an anode and a cathode. The cathode used in such a solid oxide fuel cell may react with the solid oxide electrolyte. Therefore, in order to suppress the reaction between the solid oxide electrolyte and the cathode, a technology has been disclosed in which a reaction prevention film such as GDC is provided between the cathode and the solid oxide electrolyte (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2017-504946 A Summary of the Invention [Problem to be solved by the invention]
[0004] However, providing a reaction-preventing film may increase reaction resistance during power generation.
[0005] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a solid oxide fuel cell capable of reducing reaction resistance. [Means for solving the problem]
[0006] The solid oxide fuel cell of the present invention comprises an electrolyte layer containing a solid oxide having oxide ion conductivity, an intermediate layer having oxide ion conductivity provided on the electrolyte layer, and a cathode provided on the intermediate layer, wherein the intermediate layer has a plurality of projections and recesses on its surface facing the cathode, the projections and recesses being arranged in a two-dimensional direction in a planar view, and the intermediate layer has a plurality of projections and recesses on its surface facing the electrolyte layer, the projections and recesses corresponding to the plurality of projections and recesses on the surface facing the cathode.
[0007] In the solid oxide fuel cell, the irregularities on the surface of the intermediate layer facing the cathode may be formed in the form of particles.
[0008] In the unevenness of the cathode side surface of the intermediate layer of the solid oxide fuel cell, a vertical distance a between a peak and a valley may be 0.05 μm or more and 3 μm or less.
[0009] In the unevenness on the cathode side surface of the intermediate layer of the solid oxide fuel cell, a horizontal distance b between adjacent peaks may be 0.1 μm or more and 5 μm or less.
[0010] In the unevenness of the cathode side surface of the intermediate layer of the solid oxide fuel cell, the ratio a / b of the vertical distance a between peaks and valleys to the horizontal distance b between peaks and peaks may be 1 / 10 or more and 20 / 1 or less.
[0011] In the above solid oxide fuel cell, a surface of the electrolyte layer facing the intermediate layer may be provided with a plurality of projections and recesses in accordance with the projections and recesses on the surface of the intermediate layer facing the electrolyte layer.
[0012] In the unevenness on the surface of the electrolyte layer on the intermediate layer side of the solid oxide fuel cell, the perpendicular distance a' between a peak and a valley may be 0.05 μm or more and 3 μm or less.
[0013] In the unevenness on the surface of the electrolyte layer on the intermediate layer side of the solid oxide fuel cell, a horizontal distance b' between peaks may be 0.1 μm or more and 5 μm or less.
[0014] In the unevenness of the intermediate layer side surface of the electrolyte layer of the solid oxide fuel cell, the ratio a' / b' of the vertical distance a' between peaks and valleys to the horizontal distance b' between peaks and peaks may be 1 / 10 or more and 20 / 1 or less.
[0015] In the above solid oxide fuel cell, the vertical distance a between peaks and valleys of the unevenness on the cathode side surface of the intermediate layer and the vertical distance a' between peaks and valleys of a plurality of unevennesses provided on the intermediate layer side surface of the electrolyte layer so as to follow the unevenness on the electrolyte layer side surface of the intermediate layer may have a relationship of 0.5≦a / a'≦1.
[0016] In the above solid oxide fuel cell, the horizontal distance b between peaks in the unevenness of the cathode side surface of the intermediate layer and the horizontal distance b' between peaks in a plurality of unevennesses provided on the intermediate layer side surface of the electrolyte layer so as to follow the unevenness on the electrolyte layer side surface of the intermediate layer may have a relationship of 0.5≦b / b'≦1.
[0017] In the above solid oxide fuel cell, the vertical distance between a peak in the unevenness of the cathode side surface of the intermediate layer and a corresponding peak in the unevenness provided on the intermediate layer side surface of the electrolyte layer so as to follow the unevenness on the electrolyte layer side surface of the intermediate layer may be 10 nm or more and 3 μm or less. Effect of the Invention
[0018] According to the present invention, it is possible to provide a solid oxide fuel cell capable of reducing reaction resistance. [Brief description of the drawings]
[0019] [Figure 1] 2 is a schematic cross-sectional view illustrating a stack structure of a fuel cell. FIG. [Diagram 2] FIG. 2 is an enlarged cross-sectional view illustrating details of the support, the mixed layer, and the anode. [Diagram 3](a) is an enlarged cross-sectional view from the electrolyte layer to the cathode, and (b) is a plan view of the intermediate layer. [Figure 4] FIG. 2 is an enlarged cross-sectional view from the electrolyte layer to the cathode. [Diagram 5] FIG. 2 is a diagram for explaining each dimension. [Figure 6] FIG. 2 is a diagram illustrating a flow of a method for manufacturing a fuel cell. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0020] Hereinafter, an embodiment will be described with reference to the drawings.
[0021] Fig. 1 is a schematic cross-sectional view illustrating a stacked structure of a solid oxide fuel cell 100. As illustrated in Fig. 1, the fuel cell 100 has a structure in which a mixed layer 20, an anode 30, an electrolyte layer 40, an intermediate layer 50, and a cathode 60 are stacked in this order on a support 10, for example. A plurality of fuel cells 100 may be stacked to form a fuel cell stack.
[0022] The electrolyte layer 40 is a dense layer that is mainly composed of a solid oxide having oxide ion conductivity and is gas impermeable. The electrolyte layer 40 is made of scandia-yttria stabilized zirconium oxide (ScYSZ), YSZ (yttria stabilized zirconium oxide), Gd (gadolinium) is added to CeO 2 It is preferable that the main component is GDC (Gd-doped ceria) doped with Y. 2 O 3 +Sc 2 O 3 The oxide ion conductivity is highest when the concentration is between 6 mol% and 15 mol%, and it is preferable to use a material with this composition. The thickness of the electrolyte layer 40 is preferably 20 μm or less, and more preferably 10 μm or less. The thinner the electrolyte, the better, but in order to manufacture the electrolyte so that gas does not leak from both sides, a thickness of 1 μm or more is preferable.
[0023] The cathode 60 is an electrode having electrode activity as a cathode, and has electronic conductivity and oxide ion conductivity. For example, the cathode 60 is mainly composed of a ceramic material having electronic conductivity and oxide ion conductivity. For example, the ceramic material is LaCoO 3 based material, LaMnO 3 LaFeO 3 For example, LaCoO 3 As the material, LSC (lanthanum strontium cobaltite) can be used. LSC is LaCoO doped with Sr (strontium). 3 It is.
[0024] The intermediate layer 50 is mainly composed of a component that prevents a reaction between the electrolyte layer 40 and the cathode 60. The constituent material of the intermediate layer 50 is different from the constituent material of the electrolyte layer 40. The intermediate layer 50 has oxide ion conductivity, but does not have electrode activity as a cathode. For example, the intermediate layer 50 is made of ceria (CeO 2 The additive is not particularly limited. For example, the intermediate layer 50 is made of GDC (e.g., Ce 0.8 Gd 0.2 O 2-x As an example, when the electrolyte layer 40 contains ScYSZ and the cathode 60 contains LSC, the intermediate layer 50 prevents the following reaction: Sr+ZrO 2 → SrZrO 3 La+ZrO 3 →La 2 Zr 2 O 7
[0025] Fig. 2 is an enlarged cross-sectional view illustrating the details of the support 10, the mixed layer 20, and the anode 30. As illustrated in Fig. 2, the support 10 is a member that has gas permeability and is capable of supporting the mixed layer 20, the anode 30, the electrolyte layer 40, the intermediate layer 50, and the cathode 60. The support 10 is a metal porous body mainly composed of a metal, such as a porous body of an Fe-Cr alloy.
[0026] The anode 30 is an electrode having electrode activity as an anode, and has an electrode skeleton made of a ceramic material. The electrode skeleton does not contain metal components. In this configuration, the decrease in the porosity of the anode due to the coarsening of the metal components during firing in a high-temperature reducing atmosphere is suppressed. In addition, alloying with the metal components of the support 10 is suppressed, and the decrease in catalytic function is suppressed.
[0027] The electrode skeleton of the anode 30 has electronic conductivity and oxide ion conductivity. The anode 30 contains an electronically conductive ceramic 31. The electronically conductive ceramic 31 may be, for example, a ceramic having a composition formula of ABO 3 In the present invention, a perovskite oxide represented by the formula (1) can be used, in which the A site is at least one selected from the group consisting of Ca, Sr, Ba, and La, and the B site is at least one selected from the group consisting of Ti, Cr, Ni, Mg, and Co. The molar ratio of the A site to the B site may be B≧A. Specifically, the electron conductive ceramic 31 may be LaCrO 3 based material, SrTiO 3 Materials such as those based on fluorine can be used.
[0028] The electrode skeleton of the anode 30 contains an oxide ion conductive ceramic 32. The oxide ion conductive ceramic 32 is ScYSZ or the like. For example, scandia (Sc 2 O 3 ) is 5 mol% to 16 mol%, and yttria (Y 2 O 3It is preferable to use ScYSZ having a composition range of 1 mol% to 3 mol% of scandia and yttria. It is more preferable to use ScYSZ having a total amount of scandia and yttria added of 6 mol% to 15 mol%. This is because the oxide ion conductivity is highest within this composition range. The oxide ion conductive ceramic 32 is, for example, a material having an oxide ion transport number of 99% or more. GDC or the like may be used as the oxide ion conductive ceramic 32. In the example of FIG. 2, the same solid oxide as the solid oxide contained in the electrolyte layer 40 is used as the oxide ion conductive ceramic 32.
[0029] As shown in FIG. 2, in the anode 30, for example, an electron conductive ceramic 31 and an oxide ion conductive ceramic 32 form an electrode skeleton. This electrode skeleton forms a plurality of voids. An anode catalyst is supported on the surface of the electrode skeleton in the void portion. Therefore, in the electrode skeleton that is formed spatially continuously, a plurality of anode catalysts are arranged in a spatially dispersed manner. It is preferable to use a composite catalyst as the anode catalyst. For example, it is preferable that an oxide ion conductive ceramic 33 and a catalytic metal 34 are supported as the composite catalyst on the surface of the electrode skeleton. For example, Y-doped BaCe 1-x Zr x O 3 (BCZY, x=0~1), Y-doped SrCe 1-x Zr x O 3 (SCZY, x=0~1), Sr-doped LaScO 3(LSS), GDC, etc. can be used. Ni, etc. can be used as the catalytic metal 34. The oxide ion conductive ceramics 33 may have the same composition as the oxide ion conductive ceramics 32, or may have a different composition. The metal functioning as the catalytic metal 34 may be in the form of a compound when power is not being generated. For example, Ni may be in the form of NiO (nickel oxide). During power generation, these compounds are reduced by a reducing fuel gas supplied to the anode 30, and take the form of a metal that functions as an anode catalyst.
[0030] The mixed layer 20 contains a metal material 21 and a ceramic material 22. In the mixed layer 20, the metal material 21 and the ceramic material 22 are randomly mixed. Therefore, a structure in which a layer of the metal material 21 and a layer of the ceramic material 22 are laminated is not formed. The mixed layer 20 is also porous, and a plurality of voids are formed. The metal material 21 is not particularly limited as long as it is a metal. In the example of FIG. 2, the same metal material as that of the support 10 is used as the metal material 21. For example, ScYSZ, GDC, SrTiO 3 based material, LaCrO 3 Materials such as SrTiO 3 Materials based on LaCrO 3 Since the system material has high electronic conductivity, the ohmic resistance in the mixed layer 20 can be reduced.
[0031] The fuel cell 100 generates electricity through the following process. An oxidant gas containing oxygen, such as air, is supplied to the cathode 60. At the cathode 60, due to the effect of the electrode activity of the cathode 60, the oxygen that has reached the cathode 60 reacts with electrons supplied from an external electric circuit to form oxide ions. The oxide ions move to the anode 30 side through the intermediate layer 50 and the electrolyte layer 40. Meanwhile, a fuel gas containing hydrogen, such as hydrogen gas or reformed gas, is supplied to the support 10. The fuel gas reaches the anode 30 through the support 10 and the mixed layer 20. Due to the effect of the electrode activity of the anode 30, the hydrogen that has reached the anode 30 releases electrons at the anode 30 and reacts with the oxide ions that have been conducted through the electrolyte layer 40 from the cathode 60 side to form water (H 2 O). The emitted electrons are extracted to the outside by an external electric circuit. The extracted electrons are supplied to the cathode 60 after performing electrical work. Through the above-mentioned actions, electricity is generated.
[0032] In a fuel cell 100 provided with an intermediate layer 50, the location that contributes most to the cathode reaction is the interface where the intermediate layer 50 and the cathode 60 come into contact. The area of this contact interface is inversely proportional to the reaction resistance. Therefore, the larger the contact area per unit area, the lower the reaction resistance per unit area. For these reasons, the challenge in developing the fuel cell 100 is to increase the contact area between the intermediate layer 50 and the cathode 60.
[0033] Therefore, the fuel cell 100 according to this embodiment has a structure that improves the contact area between the intermediate layer 50 and the cathode 60. FIG. 3(a) is an enlarged cross-sectional view from the electrolyte layer 40 to the cathode 60. As illustrated in FIG. 3(a), the intermediate layer 50 is formed such that a plurality of recesses 51 and protrusions 52 are alternately arranged on the surface on the cathode 60 side. As illustrated in FIG. 3(b), the recesses 51 and protrusions 52 are alternately arranged not only in one direction but also in a two-dimensional direction within the plane of the intermediate layer 50. The two-dimensional direction does not necessarily have to be perpendicular within the plane of the intermediate layer 50, but may intersect. In a plan view of the intermediate layer 50, the protrusions 52 are in the form of particles and are randomly arranged within the plane of the intermediate layer 50. Note that the scales of FIG. 3(a) and FIG. 3(b) are different.
[0034] Since the intermediate layer 50 has an uneven surface on the cathode 60 side, the cathode 60 also has an uneven surface to match the uneven surface of the intermediate layer 50. That is, as illustrated in FIG. 4, the cathode 60 has a protrusion 61 protruding toward the intermediate layer 50 at the location where the recess 51 of the intermediate layer 50 is formed in FIG. 3(a), and has a recess 62 at the location where the protrusion 52 of the intermediate layer 50 is formed in FIG. 3(a). Therefore, the area of the contact interface between the intermediate layer 50 and the cathode 60 is large. In addition, since the directions in which the unevenness of the intermediate layer 50 and the cathode 60 are aligned are two-dimensional in the plane, the area of the contact interface between the intermediate layer 50 and the cathode 60 is larger. In this configuration, the reaction field per unit area is increased, and the reaction resistance of the cathode 60 can be reduced.
[0035] In order to reduce the reaction resistance of the cathode 60, it is desirable that the distance between the electrolyte layer 40 and the cathode 60 is short. Therefore, the surface of the electrolyte layer 40 facing the cathode 60 is also unevenly formed. The surface of the intermediate layer 50 facing the electrolyte layer 40 is also formed so as to follow the shape of the unevenness of the electrolyte layer 40. For example, as illustrated in FIG. 4, the electrolyte layer 40 has a plurality of recesses 41 and protrusions 42 alternately formed on the surface facing the cathode 60. In a plan view of the intermediate layer 50 and the electrolyte layer 40, the positions of the recesses 51 and the recesses 41 in FIG. 3(a) are approximately aligned, and the positions of the protrusions 52 and the protrusions 42 in FIG. 3(a) are approximately aligned. Therefore, the recesses 41 and the protrusions 42 are not aligned in only one direction, but are aligned in two-dimensional directions within the plane of the electrolyte layer 40. Therefore, in a plan view of the electrolyte layer 40, the protrusions 52 are in the form of particles and are randomly aligned within the plane of the electrolyte layer 40. In this way, in a plan view of the electrolyte layer 40, the positions of the recesses 51 and 41 are approximately aligned, and the positions of the protrusions 52 and 52 are approximately aligned, so that the intermediate layer 50 is prevented from becoming thicker in parts, and the distance between the electrolyte layer 40 and the cathode 60 is shortened. Therefore, the reaction resistance of the cathode 60 can be reduced.
[0036] 5 is a diagram for explaining the sizes of the recesses 51 and protrusions 52 of the intermediate layer 50. In order to measure the sizes, the fuel cell 100 is embedded in resin and polished to the extent that the laminated cross section of each layer can be exposed. Then, the polished surface is processed with a cross section polisher (CP) to reveal a clean cross section. Then, the cross section is observed by SED-EDS to measure the sizes.
[0037] 5, dimension a is the vertical distance between peaks and valleys in the uneven structure on the cathode 60 side of intermediate layer 50, and is the height from the bottom of recess 51 to the top of adjacent protrusion 52 in FIG. 3(a) (the height in the stacking direction of each layer of fuel cell 100). Dimension a is the average value of the vertical distance between peaks and valleys in the uneven structure on the cathode 60 side of intermediate layer 50 measured at 20 points by observing the CP processed cross section with a SEM (scanning electron microscope) and taking photographs of several points.
[0038] If the dimension a is large, the electrolyte layer 40 will appear thick. Therefore, it is preferable to set an upper limit to the dimension a. For example, the dimension a is preferably 3 μm or less, more preferably 1 μm or less, and further preferably 0.5 μm or less.
[0039] On the other hand, if the dimension a is small, the cathode material of the cathode 60 may not easily enter the uneven structure of the intermediate layer 50. Therefore, it is preferable to set a lower limit for the dimension a. For example, the dimension a is preferably 0.05 μm or more, more preferably 0.1 μm or more, and even more preferably 0.15 μm or more.
[0040] As illustrated in FIG. 5, dimension a' is the vertical distance between the peaks and valleys in the uneven structure on the cathode 60 side of the electrolyte layer 40, and is the height from the bottom of the recess 41 in FIG. 4 to the apex of the adjacent protrusion 42 (height in the stacking direction of each layer of the fuel cell 100). The dimension a' is the average value of the vertical distances between the peaks and valleys in the uneven structure on the cathode 60 side of the electrolyte layer 40 measured at 20 points by observing the CP processed cross section with an SEM and taking pictures of several points. In order for the dimension a of the intermediate layer 50 to be within a predetermined range, it is preferable that the dimension a' in the electrolyte layer 40, which is the base, has approximately the same value. Therefore, it is preferable that the dimension a' is within the range of 0.05 μm or more and 3 μm or less.
[0041] When the intermediate layer 50 becomes thicker, the unevenness of the intermediate layer 50 becomes flatter than the unevenness of the electrolyte layer 40. Therefore, it is preferable that the intermediate layer 50 is thin. Furthermore, by making the intermediate layer 50 thinner, the uneven shape of the intermediate layer 50 approximately matches the uneven shape of the electrolyte layer 40. In other words, a / a'=1. The thicker the intermediate layer 50 becomes, the smaller a / a' becomes. Therefore, if a / a'<0.5, the effect of increasing the contact area due to the uneven structure may not be obtained. Therefore, it is better to set a suitable range for a / a', and it is preferable that a / a'≧0.5, and it is preferable that a / a'≦1. Note that the unevenness of the intermediate layer 50 is formed by the unevenness of the electrolyte layer 40, so it is difficult for a / a'>1 to be satisfied.
[0042] Next, as illustrated in Fig. 5, dimension b is the horizontal distance between peaks in the uneven structure on the cathode side of the intermediate layer 50, and is the distance from a convex portion 52 to an adjacent convex portion 52 in Fig. 3(a). Dimension b is the average value of the vertical distance between peaks and valleys in the uneven structure on the cathode 60 side of the intermediate layer 50 measured at 20 points by observing the CP processed cross section with an SEM and taking photographs of several points.
[0043] If the dimension b is large, the number of concave-convex structures on the surface of the intermediate layer 50 facing the cathode 60 decreases. Therefore, it is preferable to set an upper limit on the dimension b. For example, the dimension b is preferably 5 μm or less, more preferably 3 μm or less, and even more preferably 1 μm or less.
[0044] On the other hand, if the dimension b is small, the cathode material of the cathode 60 may not easily enter the uneven structure of the intermediate layer 50. Therefore, it is preferable to set a lower limit for the dimension b. For example, the dimension b is preferably 0.1 μm or more, more preferably 0.2 μm or more, and even more preferably 0.3 μm or more.
[0045] As illustrated in FIG. 5, the dimension b' is the horizontal distance between peaks in the uneven structure on the cathode 60 side of the electrolyte layer 40, and is the distance from the bottom of the recess 41 to the apex of the adjacent protrusion 42 in FIG. 4. The dimension b' is measured by observing the CP processed cross section with an SEM and taking pictures of several points. The dimension b' is the average value of the horizontal distance between peaks in the uneven structure on the cathode 60 side of the electrolyte layer 40 measured at 20 points. In order for the dimension b of the intermediate layer 50 to be within a predetermined range, it is preferable that the dimension b' of the electrolyte layer 40, which is the base, is also approximately the same value. Therefore, it is preferable that the dimension b' is within the range of 0.1 μm or more and 5 μm or less. In addition, it is preferable that the unevenness of the intermediate layer 50 has the same shape as the unevenness of the electrolyte layer 40, and the closer to the same shape, the closer to b / b'=1. In addition, it is believed that having the same shape has the effect of increasing the contact area with the cathode due to the uneven structure, and therefore it is preferable that b / b' ≧ 0.5, and more preferably b / b' ≦ 1. Note that, since the unevenness of the intermediate layer 50 is formed by the unevenness of the electrolyte layer 40, it is difficult to obtain b / b' > 1.
[0046] Moreover, the higher the value of a / b, the more the cathode material is filled in the valley portion. In this embodiment, a / b is preferably 1 / 10 or more, more preferably 1 / 1 or more, and even more preferably 5 / 1 or more. On the other hand, if the value of a / b is too high, the structure of the cathode 60 is likely to collapse when the cathode 60 is printed. Therefore, it is preferable to set an upper limit for a / b. In this embodiment, a / b is preferably 20 / 1 or less, more preferably 15 / 1 or less, and even more preferably 10 / 1 or less.
[0047] As illustrated in Fig. 5, dimension c is the vertical distance between the peaks in the uneven structure of intermediate layer 50 and the peaks of the underlying electrolyte layer 40. Therefore, dimension c is the distance in the stacking direction between the apex of protrusion 42 in Fig. 4 and the apex of protrusion 52 in Fig. 3(a). Dimension c is the average of the vertical distances between the peaks in the uneven structure of intermediate layer 50 and the peaks of the underlying electrolyte layer 40 measured at 20 points by observing the CP processed cross section with an SEM and taking photographs at several points.
[0048] If the dimension c is large, there is a risk that the resistance value when ions diffuse may increase. Therefore, it is preferable to set an upper limit on the dimension c. In this embodiment, the dimension c is preferably 3 μm or less, more preferably 2 μm or less, and even more preferably 1 μm or less. Furthermore, if the dimension c is too small, it becomes difficult to cover the entire uneven surface of the electrolyte layer 40, so it is preferable to set a lower limit on the dimension c. In this embodiment, the dimension c is preferably 10 nm or more, more preferably 20 nm or more, and even more preferably 30 nm or more.
[0049] The following describes a method for manufacturing the fuel cell 100. Fig. 6 is a diagram illustrating an example of the flow of the method for manufacturing the fuel cell 100.
[0050] (Support material preparation process) (S1) The support material is made into a slurry by mixing metal powder (for example, particle size 10 μm to 100 μm), plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), dissipation material (organic matter), and binder (PVB, acrylic resin, ethyl cellulose, etc.). The support material is used as a material for forming the support 10. The volume ratio of the organic components (dissipation material, binder solids, plasticizer) to the metal powder is, for example, in the range of 1:1 to 20:1, and the amount of the organic components is adjusted depending on the porosity.
[0051] (Preparation process of materials for mixed layer) (S1) As the material for the mixed layer, ceramic material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the ceramic material 22, metal material powder with a small particle size (for example, particle size 1 μm to 10 μm) which is the raw material of the metal material 21, solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), vanishing material (organic matter), and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic component (vanishing material, binder solid content, plasticizer) to the ceramic material powder and metal material powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic component is adjusted depending on the porosity. The pore size of the voids is controlled by adjusting the particle size of the vanishing material. The ceramic material powder may contain an electron conductive material powder and an oxide ion conductive material powder. In this case, the volume ratio of the electron conductive material powder to the oxide ion conductive material powder is preferably in the range of, for example, 1:9 to 9:1. Furthermore, even if an electrolyte material such as ScYSZ or GDC is used instead of the electron conductive material powder, there is no peeling at the interface, and a cell can be fabricated. However, from the viewpoint of reducing the ohmic resistance, it is preferable to mix the electron conductive material powder with a metal powder.
[0052] (Anode material preparation process) (S1) As the anode material, a ceramic material powder constituting the electrode skeleton, a solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), a plasticizer (for example, adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), a dissipating material (organic material), and a binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. As the ceramic material powder constituting the electrode skeleton, an electron conductive material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the electron conductive ceramic 31, an oxide ion conductive material powder (for example, particle size 100 nm to 10 μm) which is the raw material of the oxide ion conductive ceramic 32, etc. may be used. The volume ratio of the organic components (dissipating material, binder solids, plasticizer) to the electron conductive material powder is, for example, in the range of 1:1 to 5:1, and the amount of the organic components is adjusted depending on the porosity. The pore size of the voids is controlled by adjusting the particle size of the dissipating material. The volume ratio of the electron conductive material powder to the oxide ion conductive material powder is set to a range of 3:7 to 7:3, for example.
[0053] (Electrolyte layer material preparation process) (S1) As the material for the electrolyte layer, oxide ion conductive material powder (e.g., ScYSZ, YSZ, GDC, etc., with a particle size of D50%=10 nm to 1000 nm), solvent (toluene, 2-propanol (IPA), 1-butanol, terpineol, butyl acetate, ethanol, etc., 20 wt% to 30 wt% depending on the viscosity), plasticizer (e.g., adjusted to 1 wt% to 6 wt% to adjust the adhesion of the sheet), and binder (PVB, acrylic resin, ethyl cellulose, etc.) are mixed to form a slurry. The volume ratio of the organic components (binder solids, plasticizer) to the oxide ion conductive material powder is, for example, in the range of 6:4 to 3:4.
[0054] (Preparation process of material for uneven layer) (S1) The same material as the electrolyte layer material is used, and the viscosity, additives, solid content concentration, etc. are appropriately adjusted so that the dispersibility of the material is poor when preparing the slurry. Furthermore, in order to create an aggregation of materials such as ScYSZ, YSZ, and GDC, resin particles are added, and the size of the resin particles is preferably larger than the particle size of the material. For example, the particle size of the resin is 1.5 times that of the material. Furthermore, in order to increase the aggregation effect, the particle size of the resin is more preferably 3 times that of the material. Further, the particle size of the resin is more preferably 5 times that of the material. Note that the particle size of the oxide ion conductive material powder in the uneven layer material is preferably smaller than the particle size of the oxide ion conductive material powder in the electrolyte layer material. This is because unevenness is easily formed on the surface of the electrolyte layer 40. For example, the D50% particle size of the oxide ion conductive material powder in the uneven layer material is preferably 1 / 3 or less, more preferably 1 / 5 or less, and even more preferably 1 / 10 or less of the D50% particle size of the oxide ion conductive material powder in the electrolyte layer material.
[0055] (Firing process) (S2) First, a support material is applied onto a PET (polyethylene terephthalate) film to prepare a support green sheet. A mixed layer material is applied onto another PET film to prepare a mixed layer green sheet. An anode material is applied onto another PET film to prepare an anode green sheet. An electrolyte layer material is applied onto another PET film to prepare an electrolyte layer green sheet. An uneven layer green sheet is applied onto another PET film to prepare an uneven layer green sheet. The uneven layer green sheet is used as a green sheet to be attached to the surface layer of the electrolyte layer green sheet, so it is a thin sheet, for example, 1 μm or less. For example, multiple support green sheets, one mixed layer green sheet, one anode green sheet, one electrolyte layer green sheet, and one uneven layer green sheet are laminated in this order, cut to a predetermined size, and then heated to a temperature of 100°C or lower to 300°C. -20The mixture is fired in a reducing atmosphere of 1 atm or less at a temperature range of about 1100° C. to 1300° C. Thereby, a half cell including the support 10, the mixed layer 20, the electrode skeleton of the anode 30, the electrolyte layer 40, and the concave-convex layer can be obtained.
[0056] (Anode impregnation process) (S3) Next, the raw materials of the oxide ion conductive ceramics 33 and the catalytic metal 34 are impregnated into the electrode skeleton of the anode 30. For example, nitrates or chlorides of Zr, Y, Sc, Ce, Gd, and Ni are dissolved in water or alcohols (ethanol, 2-propanol, methanol, etc.) so that Gd-doped ceria or Sc, Y-doped zirconia and Ni are produced when fired at a predetermined temperature in a reducing atmosphere, and the half cell is impregnated, dried, and the heat treatment is repeated as many times as necessary.
[0057] (Intermediate layer formation process) (S4) The intermediate layer 50 is formed by depositing the oxide ion conductive ceramics contained in the intermediate layer 50 on the electrolyte layer 40 by, for example, PVD. 0.8 Gd 0.2 O 2-x The intermediate layer 50 is formed by depositing the above to a thickness of 1 μm.
[0058] (Cathode formation process) (S5) Next, a cathode material is applied onto the intermediate layer 50 by screen printing or the like, and dried. The cathode material is then sintered by heat treatment in an air atmosphere at a temperature of 1000° C. or less to form the cathode 60. To prevent oxidation of the metal, the heat treatment temperature is preferably 900° C. or less, and more preferably 800° C. or less.
[0059] According to the manufacturing method of this embodiment, since the dispersibility of the material for the uneven layer is adjusted to be poor in the manufacturing process, a plurality of recesses 41 and protrusions 42 are alternately formed on the surface of the electrolyte layer 40 on the cathode 60 side after firing. As a result, the intermediate layer 50 also conforms to the shape of the surface of the electrolyte layer 40 on the cathode 60 side. Therefore, on the surface of the intermediate layer 50 on the cathode 60 side, the recesses 51 are formed so as to substantially coincide with the positions of the recesses 41, and the protrusions 52 are formed so as to substantially coincide with the positions of the protrusions 42. In the printing method, it is difficult to form the unevenness only in one-dimensional directions in the plane, but in the manufacturing method of this embodiment, the unevenness can be formed in two-dimensional directions in the plane. Note that the unevenness is also formed on the surface of the intermediate layer 50 on the electrolyte layer 40 side along the surface of the electrolyte layer 40 on the cathode 60 side. Furthermore, on the surface of the intermediate layer 50 on the cathode 60 side, the protrusions 61 are formed at the positions where the recesses 51 are formed, and the recesses 62 are formed at the positions where the protrusions 52 are formed. EXAMPLES
[0060] A fuel cell 100 was produced according to the manufacturing method according to the above embodiment.
[0061] Example 1 SUS (stainless steel) powder was used as the support material. ScYSZ was used as the ceramic material for the electrolyte layer. LaCrO was used as the electronic conductive ceramic for the anode material. 3 The oxide ion conductive ceramics used were ScYSZ. The ceramic material for the intermediate layer was GDC. The ceramic material for the cathode was LSC. The ceramic material for the mixed layer was LaCrO 3 The mixed layer green sheet, anode green sheet, electrolyte layer green sheet, and uneven layer green sheet were laminated on the support green sheet, cut to a predetermined size, and then heated at 300°C until the oxygen partial pressure reached 10 -16 The anode was impregnated with GDC and Ni in a reducing atmosphere at or below 850°C. The anode was then fired in an air atmosphere at a temperature of 850°C or lower.0.8 Gd 0.2 O 2-x An intermediate layer is formed, and a cathode material is applied onto the intermediate layer by screen printing or the like, and dried. The cathode material is then sintered by heat treatment in an air atmosphere at a temperature of 1000°C or less to form a cathode. In Example 1, the dimension a was 120 nm, the dimension a' was 150 nm, the dimension b was 1 μm, the dimension b' was 1 μm, and the dimension c was 500 nm.
[0062] Example 2 In Example 2, NiO / YSZ was used as the support material. Other manufacturing conditions were the same as in Example 1. In Example 2, dimension a was 120 nm, dimension a' was 150 nm, dimension b was 1 μm, dimension b' was 1 μm, and dimension c was 500 nm.
[0063] Example 3 In Example 3, the manufacturing conditions of the concave-convex sheet were changed to reduce the dimensions of the concave-convex pattern. The other manufacturing conditions were the same as in Example 1. In Example 3, the dimension a was 50 nm, the dimension a' was 80 nm, the dimension b was 1 μm, the dimension b' was 1 μm, and the dimension c was 500 nm.
[0064] Comparative Example 1 In Comparative Example 1, the green sheet for the uneven layer was not provided. The other conditions were the same as those in Example 1. In Comparative Example 1, since the green sheet for the uneven layer was not provided, unevenness did not appear on the cathode side surface of the electrolyte layer, and unevenness did not appear on the intermediate layer and the cathode. The dimension c was 500 nm.
[0065] Comparative Example 2 In Comparative Example 2, the PVD treatment time was three times that of Example 1, and the thickness of the intermediate layer was three times (about 1.5 μm). The other conditions were the same as those of Example 1. The dimension c was 1.5 μm.
[0066] (Power generation evaluation) Impedance measurements were performed on the fuel cells of Examples 1 to 3 and Comparative Examples 1 and 2 to separate the resistance values and measure the ohmic resistance of the entire fuel cell and the reaction resistance of the cathode. The results are shown in Table 1. As shown in Table 1, in Example 1, the ohmic resistance was 0.25 Ω cm 2 In Example 2, the ohmic resistance was 0.30 Ω cm 2 In Example 3, the ohmic resistance was 0.25 Ω cm 2 Thus, the ohmic resistance was low in Examples 1 to 3. This is believed to be because the provision of unevenness on both sides of the intermediate layer made the resistance during ion conduction almost the same as that without the uneven structure (Comparative Example 1). The reason why the ohmic resistances of Examples 1 and 3 were lower than that of Example 2 is believed to be because a metal support with high electronic conductivity was used. In Comparative Example 1, the ohmic resistance was 0.25 Ω cm 2 The reason why the ohmic resistance in Comparative Example 1 is similar to that in Example 1 is believed to be because the ohmic resistance depends only on the thickness (dimension c) of the intermediate layer. On the other hand, the ohmic resistance in Comparative Example 2 is larger than those in Example 1 and Comparative Example 1, at 0.34 Ω cm 2 This is believed to be due to the increased ohmic resistance caused by the thicker intermediate layer. [Table 1]
[0067] In Example 1, the reaction resistance at the cathode is 0.27 Ω cm 2 In Example 2, the reaction resistance at the cathode was 0.27 Ω cm 2 In Example 3, the reaction resistance at the cathode was 0.31 Ω cm 2Thus, in Examples 1 to 3, the reaction resistance at the cathode was low. This is believed to be because the contact area between the intermediate layer and the cathode was increased by forming two-dimensional irregularities in a plan view on the cathode-side surface of the intermediate layer. The reason why the reaction resistance was lower in Examples 1 and 2 than in Example 3 is believed to be because the dimensions a and a' were larger, resulting in larger irregularities. In contrast, in Comparative Example 1, the reaction resistance at the cathode was 0.56 Ω cm 2 In Comparative Example 2, the reaction resistance at the cathode was 0.52 Ω cm 2 This is believed to be because the contact area between the intermediate layer and the cathode was not large enough due to the absence of projections and recesses in the intermediate layer.
[0068] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to such specific embodiments, and various modifications and variations are possible within the scope of the gist of the present invention described in the claims. [Explanation of symbols]
[0069] 10 Support 20 mixed layer 21 Metal materials 22 Ceramic Materials 30 Anode 31 Electronically Conductive Ceramics 32 Oxide-ion conductive ceramics 33 Oxide-ion conductive ceramics 34 Catalytic Metals 40 Electrolyte layer 41 Recess 42 Convex 50 Middle Class 51 Recess 52 Convex 60 Cathode 61 Convex 62 Recess 100 fuel cell
Claims
1. an electrolyte layer including a solid oxide having oxide ion conductivity; an intermediate layer provided on the electrolyte layer and having oxide ion conductivity; a cathode provided on the intermediate layer; the intermediate layer has a plurality of projections and recesses arranged in a two-dimensional direction in a plan view on the surface of the intermediate layer facing the cathode; the intermediate layer has a surface on the electrolyte layer side that is provided with a plurality of projections and recesses that correspond to the plurality of projections and recesses on the surface on the cathode side; a plurality of projections and recesses are provided on a surface of the electrolyte layer facing the intermediate layer so as to conform to the projections and recesses on a surface of the intermediate layer facing the electrolyte layer; 2. A solid oxide fuel cell comprising: a surface of said electrolyte layer facing said intermediate layer, said surface having a vertical distance a' between a peak and a valley of said electrolyte layer being 80 nm or more and 150 nm or less.
2. 2. The solid oxide fuel cell according to claim 1, wherein the irregularities on the surface of the intermediate layer facing the cathode are formed in a granular shape.
3. 3. The solid oxide fuel cell according to claim 1, wherein the vertical distance a between a peak and a valley in the unevenness of the surface of the intermediate layer facing the cathode is 0.05 μm or more and 3 μm or less.
4. The solid oxide fuel cell according to claim 3, wherein the vertical distance a is greater than or equal to 50 nm and less than or equal to 120 nm.
5. 5. The solid oxide fuel cell according to claim 1, wherein the horizontal distance b between peaks in the unevenness of the cathode side surface of the intermediate layer is 0.1 μm or more and 5 μm or less.
6. 6. The solid oxide fuel cell according to claim 1, wherein in the unevenness of the cathode side surface of the intermediate layer, a / b, which is a ratio of a vertical distance a between peaks and valleys to a horizontal distance b between peaks, is 1 / 10 or more and 20 / 1 or less.
7. A solid oxide fuel cell described in any one of claims 1 to 5, characterized in that, in the unevenness of the cathode side surface of the intermediate layer, the ratio a / b of the vertical distance a between peaks and valleys to the horizontal distance b between peaks and peaks is 0.05 or more and 0.12 or less.
8. 8. The solid oxide fuel cell according to claim 6, wherein the horizontal distance b' between peaks in the unevenness of the surface of the electrolyte layer facing the intermediate layer is 0.1 μm or more and 5 μm or less.
9. 9. A solid oxide fuel cell according to claim 1, wherein in the unevenness of the surface of the electrolyte layer facing the intermediate layer, a ratio a' / b' of the vertical distance a' to the horizontal distance b' between peaks is 1 / 10 or more and 20 / 1 or less.
10. A solid oxide fuel cell described in any one of claims 1 to 8, characterized in that in the unevenness of the surface of the electrolyte layer facing the intermediate layer, the ratio a' / b' of the vertical distance a' to the horizontal distance b' between peaks is 0.08 or more and 0.15 or less.
11. 11. A solid oxide fuel cell as described in any one of claims 1 to 10, characterized in that the vertical distance a between peaks and valleys of the unevenness on the cathode side surface of the intermediate layer and the vertical distance a' between peaks and valleys of a plurality of unevennesses provided on the intermediate layer side surface of the electrolyte layer so as to follow the unevenness on the electrolyte layer side surface of the intermediate layer satisfy a relationship of 0.5≦a / a'≦1.
12. The solid oxide fuel cell as described in claim 11, characterized in that a / a' is greater than or equal to 0.625 and less than or equal to 0.
8.
13. 13. A solid oxide fuel cell as described in any one of claims 1 to 12, characterized in that a horizontal distance b between peaks in the unevenness on the cathode side surface of the intermediate layer and a horizontal distance b' between peaks in a plurality of unevennesses provided on the intermediate layer side surface of the electrolyte layer so as to follow the unevenness on the electrolyte layer side surface of the intermediate layer satisfy a relationship of 0.5≦b / b'≦1.
14. 14. A solid oxide fuel cell as described in any one of claims 1 to 13, characterized in that the vertical distance between a peak in the unevenness on the cathode side surface of the intermediate layer and a corresponding peak in the unevenness provided on the intermediate layer side surface of the electrolyte layer so as to follow the peak in the unevenness on the electrolyte layer side surface of the intermediate layer is 10 nm or more and 3 μm or less.
15. A method for producing an electrolyte layer comprising laminating and firing a roughness layer green sheet containing a powder of a solid oxide having oxide ion conductivity on an electrolyte layer green sheet containing the powder of the solid oxide and resin particles, thereby forming roughness on the surface of an electrolyte layer obtained from the electrolyte layer green sheet; forming an intermediate layer having oxide ion conductivity on a surface of the electrolyte layer to form irregularities on a surface of the intermediate layer opposite to the electrolyte layer; A method for producing a solid oxide fuel cell, comprising forming a cathode on a surface of said intermediate layer opposite to said electrolyte layer.
Citation Information
Patent Citations
Solid oxide fuel battery electrolyte sheet, manufacturing method thereof, and solid oxide fuel battery single cell
JP2012069418A
Electrochemical element, electrochemical module, electrochemical device, energy system, solid oxide fuel cell, and method of manufacturing electrochemical element
JP2017174516A
Method of producing sofc cathode diffusion barrier layer and sofc
JP2017504946A
Electrochemical element, electrochemical module, electrochemical device, energy system, solid oxide fuel cell, and manufacturing method of electrochemical element
JP2018174117A
Electrochemical cell
JP2020155338A