CATALYST STRUCTURE FOR PRODUCING SYNTHETIC GAS, METHOD FOR USE THEREOF, APPARATUS FOR PRODUCING SYNTHETIC GAS, AND METHOD FOR PRODUCING CATALYST STRUCTURE FOR PRODUCING SYNTHETIC GAS

The catalyst structure with a porous zeolite-type compound carrier and embedded metal fine particles addresses agglomeration and coking issues, ensuring stable catalytic activity and efficient synthesis gas production.

JP7575274B2Active Publication Date: 2024-10-29FURUKAWA ELECTRIC CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020559940
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-12-03
Filing Date
2019-12-03
Publication Date
2024-10-29
Estimated Expiration
2039-12-03

AI Technical Summary

Technical Problem

Existing catalyst structures for producing synthesis gas suffer from agglomeration and coking at high temperatures, leading to decreased catalytic activity and the need for frequent regeneration through oxidation and reduction treatments, while methods using metal fine particles in zeolite encapsulation face issues with nano-sized particle maintenance and organic solvent residues affecting thermal stability.

Method used

A catalyst structure is developed with a porous zeolite-type compound carrier having a specific L/d ratio and passages, where metal fine particles like Ni are embedded within the carrier's pores, preventing agglomeration and coking, and maintaining catalytic activity through controlled particle size and distribution.

Benefits of technology

The catalyst structure achieves stable catalytic activity over a long period with reduced coking, enabling efficient production of synthesis gas containing carbon monoxide and hydrogen, with improved manufacturing efficiency and resource conservation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575274000005
    Figure 0007575274000005
  • Figure 0007575274000006
    Figure 0007575274000006
  • Figure 0007575274000007
    Figure 0007575274000007
Patent Text Reader

Abstract

The present invention provides a catalyst structure for synthesis gas production that can stably maintain excellent catalytic activity over long periods of time without decline and can efficiently produce synthesis gas containing carbon monoxide and hydrogen. The catalyst structure for synthesis gas production is a catalyst structure 1 for synthesis gas production used in producing synthesis gas containing carbon monoxide and hydrogen, and includes a carrier 10 having a porous structure made of a zeolite-type compound and at least one catalyst material 20 present in the carrier 10, the carrier 10 having passages 11 that communicate with each other, a ratio of the long side dimension L to the thickness dimension d of the carrier 10 (L / d ratio) of 5.0 or more, and the catalyst material 20 present in at least the passages 11 of the carrier 10.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a catalyst structure for producing synthesis gas, a precursor thereof, an apparatus for producing synthesis gas, and a method for producing a catalyst structure for producing synthesis gas. [Background technology]

[0002] In recent years, as a measure against global warming, attention has been focused on a technology (dry reforming) in which carbon dioxide, a causative substance of global warming, is brought into contact with methane and converted into a synthesis gas containing carbon monoxide and hydrogen.

[0003] As a catalyst for use in producing such a synthesis gas, for example, Patent Document 1 discloses a catalyst that uses an oxygen-deficient perovskite-type composite oxide containing Mn, a specific alkaline earth metal, and the like as a support and nickel as a supported metal.

[0004] However, the reaction of contacting carbon dioxide and methane to convert them into a synthesis gas containing carbon monoxide and hydrogen must be carried out at high temperatures of at least 800° C. In the catalyst disclosed in Patent Document 1, the supported metal is supported on the outer surface of the carrier, and therefore the supported metal particles tend to agglomerate together (sintering) at high temperatures and carbon deposition on the catalyst (coking), resulting in a decrease in catalytic activity.

[0005] As a method for suppressing adhesion between catalyst particles and increasing the specific surface area of ​​the catalyst particles, for example, Patent Document 2 discloses a method in which catalyst particles are fixed to the surface of a substrate and then oxidation and reduction treatments are performed under specified conditions.

[0006] Patent Document 3 describes a catalyst for dry reforming in which Ni is supported on a composite oxide. The dry reforming method is prone to coking on the catalyst surface, which tends to reduce catalytic activity. This is because the carbon content in the raw material is higher than in the steam reforming method in which methane and steam are reacted. In addition, this leads to problems such as the clogging of the catalyst layer in the reaction tube due to coking. In particular, Ni-supported catalysts have the advantage of high catalytic activity, but are prone to coking and make it difficult to maintain catalytic activity.

[0007] Although there is no mention of dry reforming, Patent Documents 4 and 5, for example, describe a method of preparing metal particles coated with amorphous silica by an emulsion method and hydrothermally treating the particles to encapsulate the metal particles in zeolite as a structure of a catalyst structure for maintaining the activity of catalyst particles. Metal particles coated with amorphous silica obtained by the emulsion method are prepared by adding a reducing agent to an emulsion in which a surfactant and a metal source are mixed in an organic solvent to form metal particles, then adding a silane coupling agent to form a silica layer on the surface of the metal particles, and then growing zeolite from the silica layer. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] JP 2013-255911 A [Patent Document 2] JP 2016-2527 A [Patent Document 3] JP 2014-200705 A [Patent Document 4] JP 2017-128480 A [Patent Document 5] International Publication No. 2010 / 097108 Summary of the Invention [Problem to be solved by the invention]

[0009] However, even in the catalyst structure in which catalyst particles are fixed on the substrate surface as disclosed in Patent Document 2, in a high-temperature reaction field such as a dry reforming reaction, the aggregation and coking of the catalyst particles progress with the lapse of reaction time, and the catalytic activity decreases. Therefore, in order to regenerate the catalytic function, it is necessary to carry out the oxidation treatment and reduction treatment again, which makes the work complicated. Furthermore, in consideration of practical application, further improvement of the catalytic activity is required.

[0010] In addition, when metal particles are produced by the emulsion method as in Patent Documents 4 and 5, the size of the resulting metal particles is affected by the size of the droplets when emulsified and the tendency of the metal particles to aggregate. In general, base metals are prone to aggregation, making it difficult to maintain the state of nanoparticles, and even in Patent Documents 5 and 6, it has been confirmed that the metal particles have a nano-sized particle size only when the metal particles are Rh, Au, Pt, and Pd among the precious metals. On the other hand, Patent Documents 5 and 6 do not state that when metal particles made of Ru or base metals that tend to aggregate or their oxides are encapsulated in zeolite, the metal particles or their oxides have a nano-sized particle size. Furthermore, in the emulsion method, organic solvents and surfactants used in forming the zeolite structure remain and become impurities, which tend to adversely affect the thermal stability of the zeolite. Furthermore, Patent Document 4 does not state zeolite encapsulating base metal particles such as Ni, which are prone to coking. Furthermore, in Patent Document 5, which uses a manufacturing method similar to Patent Document 4, it is believed that the organic solvents and surfactants cannot be completely removed and remain, resulting in a decrease in durability against high temperatures such as in the dry reforming reaction.

[0011] An object of the present invention is to provide a catalyst structure for producing synthetic gas, which can stably maintain excellent catalytic activity for a long period of time without deterioration, and which is capable of efficiently producing a synthetic gas containing carbon monoxide and hydrogen, and a precursor thereof, as well as a synthetic gas production apparatus including the catalyst structure or the precursor thereof, and a method for producing the catalyst structure for producing synthetic gas. [Means for solving the problem]

[0012] The gist and configuration of the present invention are as follows. 1. A catalyst structure for producing synthesis gas used in producing synthesis gas containing carbon monoxide and hydrogen, comprising a carrier having a porous structure composed of a zeolite-type compound and at least one catalyst substance present in the carrier, the carrier having passages communicating with each other, a ratio of the long side dimension L to the thickness dimension d of the carrier (L / d ratio) of 5.0 or more, and the catalyst substance present in at least the passages of the carrier. 2. The catalyst structure for producing synthetic gas according to item 1 above, characterized in that the L / d ratio of the support is 5.0 or more and 35.0 or less. 3. The catalyst structure for producing synthetic gas according to 1 or 2 above, characterized in that the L / d ratio of the support is 7.0 or more and 25.0 or less. 4. A catalyst structure for producing a synthesis gas used in producing a synthesis gas containing carbon monoxide and hydrogen, comprising a carrier having a porous structure composed of a zeolite-type compound and at least one catalyst substance present in the carrier, the carrier having passages communicating with each other, the ratio of the long side dimension L to the thickness dimension d of the carrier (L / d ratio) being 5.0 or more, the catalyst substance being present at least in the passages of the carrier, and having an average particle size of 1.00 nm or more and 13.0 nm or less. 5. The catalyst structure for producing a synthetic gas according to any one of 1 to 4 above, wherein the average particle size of the catalyst substance is larger than the average inner diameter of the passages. 6. The catalyst structure for producing synthetic gas as described in any one of 1 to 5 above, characterized in that the passages have any one-dimensional pores, two-dimensional pores, or three-dimensional pores of the framework structure of the zeolite-type compound, and an expanded diameter portion different from any one-dimensional pores, two-dimensional pores, or three-dimensional pores, and the catalyst substance is present at least in the expanded diameter portion. 7. The catalyst structure for producing synthesis gas according to claim 6, wherein the enlarged diameter portion connects a plurality of holes constituting any one of the one-dimensional holes, the two-dimensional holes and the three-dimensional holes. 8. The catalyst structure for producing synthetic gas as described in 6 or 7 above, wherein the average particle diameter of the catalyst substance is equal to or smaller than the inner diameter of the expanded portion. 9. The catalyst structure for producing synthetic gas according to any one of 1 to 8, wherein the catalyst substance is fine metal particles. 10. The average inner diameter D of the passage F The average particle diameter D of the metal fine particles C Percentage of (D C / D F 10. The catalyst structure for producing a synthetic gas, as described in 9 above, characterized in that the ratio of the surface area of ​​the catalyst to the surface area of ​​the synthetic gas is 0.05 or more and 130.0 or less. 11. The catalyst structure for producing synthetic gas according to 9 or 10 above, characterized in that the metal fine particles are fine particles composed of at least one metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni). 12. The catalyst structure for producing a synthetic gas as described in any one of 9 to 11 above, wherein the metal fine particles are fine particles made of nickel (Ni). 13. The catalyst structure for producing a synthetic gas according to any one of 1 to 8 above, wherein the catalyst substance is metal oxide fine particles. 14. The catalyst structure for producing a synthesis gas according to any one of 1 to 13 above, further comprising at least one other catalyst material held on the outer surface of the support. 15. The catalyst structure for producing synthesis gas described in paragraph 14, characterized in that the content of the at least one catalytic material present within the support is greater than the content of the at least one other catalytic material carried on the outer surface of the support. 16. The catalyst structure for producing a synthesis gas according to any one of 1 to 15 above, wherein the zeolite type compound is a silicate compound. 17. The catalyst structure for synthesis gas production is packed in an atmospheric flow reactor and is operated at GHSV5600h -117. The catalyst structure for producing a synthetic gas according to any one of 1 to 16, characterized in that when a dry reforming reaction is carried out under the conditions of supplying a raw material gas with a CO2 / CH4 ratio (volume ratio) of 1:1, holding the temperature at 100°C for 10 minutes, and then raising the temperature to 900°C at a rate of 20°C / min for a total heating time of 60 minutes at or above 100°C, the CH4 conversion at 700°C is 20% or more. 18. The catalyst structure for producing a synthetic gas according to 17, characterized in that, when the dry reforming reaction is carried out, the CH4 conversion rate at 700°C is 60% or more. 19. The catalyst structure for synthetic gas production according to claim 17 or 18, characterized in that, when the dry reforming reaction is carried out, the amount of coking in the catalyst structure for synthetic gas production after the reaction is analyzed by CHN measurement is less than 5.0 mass% with respect to the total amount of the catalyst structure for synthetic gas production. 20. The catalyst structure for synthesis gas production according to any one of paragraphs 17 to 19, characterized in that, when the dry reforming reaction is carried out, the amount of coking in the catalyst structure for synthesis gas production after the reaction is analyzed by CHN measurement is less than 0.3 mass% with respect to the total amount of the catalyst structure for synthesis gas production. 21. A precursor of the catalyst structure for producing synthetic gas according to any one of 1 to 20 above, characterized in that the precursor material of the catalyst material is fine particles of a metal oxide. 22. A synthesis gas production apparatus comprising the catalyst structure for producing synthesis gas according to any one of 1 to 20 above or a precursor of the catalyst structure for producing synthesis gas according to 21 above. 23. A method for producing a catalyst structure for synthetic gas production, comprising: a calcination step of calcining a precursor material (B) obtained by impregnating a precursor material (A) having pores with a pore diameter of 13.0 nm or less with a metal-containing solution to obtain a porous support composed of a zeolite-type compound; and a hydrothermal treatment step of hydrothermally treating a precursor material (C) obtained by calcining the precursor material (B) to obtain a catalyst structure in which the ratio of the long side dimension L to the thickness dimension d of the support (L / d ratio) is 5.0 or more. 24. The method for producing a catalyst structure for producing synthetic gas, as described in 23 above, characterized in that a nonionic surfactant is added in an amount of 50 mass % or more and 500 mass % or less to the precursor material (A) before the calcination step. 25. The method for producing a catalyst structure for producing synthetic gas as described in 23 or 24, characterized in that the metal-containing solution is added to the precursor material (A) in multiple batches prior to the calcination step, thereby impregnating the precursor material (A) with the metal-containing solution. 26. The method for producing a catalyst structure for producing synthetic gas as described in any one of 23 to 25 above, characterized in that when impregnating the precursor material (A) with the metal-containing solution prior to the calcination step, an amount of the metal-containing solution added to the precursor material (A) is adjusted so that a ratio (atomic number ratio Si / M) of silicon (Si) constituting the precursor material (A) to a metal element (M) contained in the metal-containing solution added to the precursor material (A) is 10 or more and 1,000 or less. 27. The method for producing a catalyst structure for producing a synthesis gas according to any one of the above 23 to 26, characterized in that in the hydrothermal treatment step, the precursor material (C) is mixed with a structure-directing agent. 28. The method for producing a catalyst structure for producing a synthesis gas according to any one of 23 to 26 above, wherein the hydrothermal treatment step is carried out in a basic atmosphere. 29. The method for producing a catalyst structure for producing a synthetic gas according to any one of the above 23 to 28, further comprising a step of subjecting the hydrothermally treated precursor material (C) to a reduction treatment in a reducing gas atmosphere. Effect of the Invention

[0013] According to the present invention, it is possible to provide a catalyst structure for producing synthetic gas and a precursor thereof, which can stably maintain excellent catalytic activity for a long period of time without deterioration and can efficiently produce a synthetic gas containing carbon monoxide and hydrogen, as well as a synthetic gas production apparatus and a method for producing a catalyst structure for producing synthetic gas, which include the catalyst structure or the precursor thereof. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram showing the internal structure of a catalyst structure for producing synthesis gas according to an embodiment of the present invention, in which FIG. 1(a) is a perspective view (partially shown in cross section), and FIG. 1(b) is a partially enlarged cross-sectional view. [Diagram 2] FIG. 2 is an SEM image showing the long dimension and thickness dimension of the support. [Diagram 3] 3A and 3B are partially enlarged cross-sectional views for explaining an example of the function of the catalyst structure for producing synthesis gas in FIG. 1, where FIG. 3A illustrates the sieving function and FIG. 3B illustrates the catalytic activity. [Figure 4] FIG. 4 is a flow chart showing an example of a method for producing the catalyst structure for producing synthesis gas shown in FIG. [Diagram 5] FIG. 5 is a schematic diagram showing a modification of the catalyst structure for producing synthesis gas shown in FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, the embodiments will be described in detail with reference to the drawings.

[0016] As a result of intensive research into achieving the above-mentioned object, the inventors have found that a catalyst structure for producing synthetic gas can be obtained, which comprises a carrier having a porous structure composed of a zeolite-type compound and having a ratio of long side dimension L to thickness dimension d (L / d ratio) of 5.0 or more, and at least one catalytic substance present in the carrier, wherein the carrier has passages that communicate with each other and the catalytic substance is present in at least the passages of the carrier, and which can stably maintain excellent catalytic activity without decreasing over a long period of time, and which can efficiently produce a synthetic gas containing carbon monoxide and hydrogen, and have completed the present invention based on this finding.

[0017] A catalyst structure for producing synthesis gas according to an embodiment is a catalyst structure for producing synthesis gas used in producing synthesis gas containing carbon monoxide and hydrogen, and comprises a carrier having a porous structure composed of a zeolite-type compound and at least one catalyst substance present in the carrier, the carrier having passages communicating with each other, a ratio of a long side dimension L to a thickness dimension d of the carrier (L / d ratio) of 5.0 or more, and the catalyst substance present in at least the passages of the carrier.

[0018] The method for producing a catalyst structure for producing synthetic gas according to the embodiment includes a calcination step of calcining a precursor material (B) obtained by impregnating a metal-containing solution with a precursor material (A) having pores with a pore diameter of 13.0 nm or less in order to obtain a carrier having a porous structure composed of a zeolite-type compound, and a hydrothermal treatment step of hydrothermally treating a precursor material (C) obtained by calcining the precursor material (B) to obtain a catalyst structure in which the ratio of the long side dimension L to the thickness dimension d (L / d ratio) of the carrier is 5.0 or more.

[0019] [Catalyst structure] 1 is a diagram showing a schematic configuration of a catalyst structure for producing synthetic gas according to an embodiment (hereinafter, simply referred to as "catalyst structure"), in which (a) is a perspective view (partially shown in cross section), and (b) is a partially enlarged cross-sectional view. Note that the catalyst structure in FIG. 1 shows only one example, and the shape, dimensions, etc. of each component are not limited to those in FIG. 1.

[0020] The catalyst structure 1 shown in FIG. 1(a) is a catalyst structure for producing a synthesis gas used in producing a synthesis gas containing carbon monoxide and hydrogen, and comprises a porous support 10 composed of a zeolite-type compound and at least one catalyst material 20 present within the support 10.

[0021] <Carrier> The carrier 10 is made of a zeolite type compound and has a porous structure. The "zeolite-type compounds" referred to here include not only crystalline aluminosilicates, but also various zeolite-like substances such as phosphate-based porous crystals having a similar structure, as described in Toyota Central R&D R&D Review Vol. 29, No. 2 (June 1994, pp. 11-22, New Developments in Zeolite Chemistry, Inagaki Shinji). Examples of the zeolite type compound include silicate compounds such as zeolite (aluminosilicate), cation-exchanged zeolite, and silicalite, zeolite-related compounds such as aluminoborates, aluminoarsenates, and germanates, and phosphate-based zeolite-like substances such as molybdenum phosphate, etc. Among these, the zeolite type compound is preferably a silicate compound.

[0022] The framework structure of the zeolite compound is selected from FAU type (Y type or X type), MTW type, MFI type (ZSM-5), FER type (ferrierite), LTA type (A type), MWW type (MCM-22), MOR type (mordenite), LTL type (L type), BEA type (beta type), etc., preferably MFI type, more preferably MFI type silicalite. In the zeolite compound, a plurality of pores having a pore size according to each framework structure are formed, for example, the maximum pore size of the MFI type is 0.636 nm (6.36 Å) and the average pore size is 0.560 nm (5.60 Å).

[0023] 1(b), the support 10 has a porous structure, and preferably has a plurality of pores 11a, 11a, ... formed therein, thereby providing mutually communicating passages 11. The catalytic material 20 is present in at least the passages 11 of the support 10, and is preferably held in at least the passages 11 of the support 10.

[0024] With this configuration, the movement of the catalytic material 20 within the carrier 10 is restricted, and the aggregation of the catalytic materials 20, 20 is effectively prevented. As a result, the catalytic structure 1 has improved sintering resistance, and the reduction in the effective surface area of ​​the catalytic material 20 can be effectively suppressed, and the catalytic activity of the catalytic material 20 is maintained for a long period of time. That is, according to the catalytic structure 1, the decrease in catalytic activity due to aggregation of the catalytic material 20 can be suppressed, and the catalytic structure 1 can be extended in life. Furthermore, the extended life of the catalytic structure 1 can reduce the frequency of replacement of the catalytic structure 1, and can significantly reduce the amount of waste of used catalytic structure 1, thereby saving resources.

[0025] Usually, when a catalyst structure is used in a fluid, it may be subjected to an external force from the fluid. In this case, if the catalyst substance is attached only to the outer surface of the carrier 10, there is a problem that the catalyst substance is likely to be detached from the outer surface of the carrier 10 due to the influence of the external force from the fluid. In contrast, in the catalyst structure 1 of this embodiment, the catalyst substance 20 is held at least in the passages 11 of the carrier 10, so that the catalyst substance 20 is unlikely to be detached from the carrier 10 even if it is subjected to an external force from the fluid.

[0026] That is, when the catalyst structure 1 is in a fluid, the fluid flows into the passage 11 from the hole 11a of the carrier 10, and the speed of the fluid flowing in the passage 11 is considered to be slower than the speed of the fluid flowing on the outer surface of the carrier 10 due to the flow resistance (friction force). Due to the influence of such flow resistance, the pressure that the catalyst material 20 held in the passage 11 receives from the fluid is lower than the pressure that the catalyst material held outside the carrier 10 receives from the fluid. Therefore, it is possible to effectively suppress the catalyst material 20 contained in the carrier 10 from being separated, and it is possible to stably maintain the catalytic activity of the catalyst material 20 for a long period of time. It is considered that the flow resistance as described above increases as the passage 11 of the carrier 10 has multiple bends and branches and the inside of the carrier 10 has a more complex, three-dimensional structure.

[0027] In addition, the passage 11 preferably has one of one-dimensional, two-dimensional and three-dimensional pores defined by the framework structure of the zeolite compound, and an expanded diameter portion 12 different from any of the one-dimensional, two-dimensional and three-dimensional pores. In this case, the catalyst material 20 is preferably present at least in the expanded diameter portion 12, and more preferably is included in at least the expanded diameter portion 12. This further restricts the movement of the catalyst material 20 in the support 10, and can more effectively prevent the catalyst material 20 from being separated or the catalyst material 20 from agglomerating with itself. The inclusion refers to a state in which the catalyst material 20 is included in the support 10. In this case, the catalyst material 20 and the support 10 do not necessarily need to be in direct contact with each other, and the catalyst material 20 may be indirectly held in the support 10 with another material (e.g., a surfactant) intervening between the catalyst material 20 and the support 10.

[0028] The term "one-dimensional pore" as used herein refers to a tunnel- or cage-type pore forming a one-dimensional channel, or multiple tunnel- or cage-type pores (multiple one-dimensional channels) forming multiple one-dimensional channels. The term "two-dimensional pore" refers to a two-dimensional channel in which multiple one-dimensional channels are two-dimensionally connected, and the term "three-dimensional pore" refers to a three-dimensional channel in which multiple one-dimensional channels are three-dimensionally connected.

[0029] 1(b) shows a case where the catalytic material 20 is enclosed in the enlarged diameter portion 12, but the present invention is not limited to this configuration, and the catalytic material 20 may be present in the passage 11 with a part of it protruding outside the enlarged diameter portion 12. The catalytic material 20 may also be partially embedded in a part of the passage 11 other than the enlarged diameter portion 12 (for example, an inner wall part of the passage 11) or held therein by adhesion or the like.

[0030] In addition, it is preferable that the expanded diameter portion 12 communicates with the plurality of holes 11a, 11a constituting any one of the one-dimensional holes, the two-dimensional holes, and the three-dimensional holes, so that a separate passage different from the one-dimensional holes, the two-dimensional holes, or the three-dimensional holes is provided inside the support 10, thereby enabling the catalyst material 20 to exhibit its function more effectively.

[0031] Moreover, the passage 11 is formed three-dimensionally inside the carrier 10 including a branching portion or a junction portion, and the expanded diameter portion 12 is preferably provided at the branching portion or the junction portion of the passage 11 .

[0032] The average inner diameter D of the passages 11 formed in the carrier 10 F is calculated from the average value of the minor axis and major axis of the pores 11a constituting any one of the one-dimensional pores, the two-dimensional pores, and the three-dimensional pores, and is preferably 0.10 nm or more and 1.50 nm or less, and more preferably 0.50 nm or more and 0.80 nm or less. E The inner diameter D of the expanded diameter portion 12 is preferably 0.5 nm or more and 13.0 nm or less, more preferably 1.1 nm or more and 13.0 nm or less, and further preferably 1.1 nm or more and 3.3 nm or less. E is, for example, the pore size of the precursor material (A) described later and the average particle size D of the catalytic substance 20 to be enclosed. C The inner diameter D of the expanded diameter portion 12 depends on E is a size capable of encapsulating the catalyst material 20.

[0033] In addition, by making the carrier 10 have an appropriate shape, more specifically, by making the ratio of the long side dimension L to the thickness dimension d (L / d ratio) of the carrier 10 5.0 or more, the catalytic activity is improved. There are two reasons for the improvement in catalytic activity. Basically, the holes 11a of the catalyst structure 1 are formed on the surface where the long side dimension L exists, i.e., the upper surface or lower surface that defines the long side dimension L ((010) surface or (100) surface), and are not formed on the surface where the thickness dimension d exists, i.e., a specific surface ((101) surface) among the side surfaces that defines the thickness dimension. Therefore, the larger the value of the L / d ratio, the higher the ratio of holes to the total surface area of ​​the catalyst structure (number of holes / total surface area of ​​the catalyst structure), and therefore the higher the probability that the reaction gas contacts the region where the holes 11a exist, and the higher the probability that the reaction gas contacts the catalyst substance inside the catalyst structure 1. In addition, the larger the value of the L / d ratio, the more easily the reaction gas can penetrate the holes 11a when the catalyst structure 1 is packed in the catalyst layer in the reaction tube, since the packing density of the catalyst structure 1 in the catalyst layer is not excessive, and the route through which the reaction gas reaches the catalyst material can be secured. The L / d ratio of the support is 5.0 or more, preferably 5.0 to 35.0, and more preferably 7.0 to 25.0. By making the L / d ratio of the support 10 5.0 or more, the catalytic activity can be improved as described above. As the L / d ratio of the support 10 increases, the catalytic activity improves. In addition, when the L / d ratio is 35.0 or less, the yield is improved when manufacturing the highly active catalyst structure 1. In this way, the catalyst structure 1 having an L / d ratio of 5.0 to 35.0 has good manufacturing efficiency and high activity. Specific shapes of the support include a plate shape, a coffin shape, and the like.

[0034] FIG. 2 shows the long side dimension L and thickness dimension d of the carrier 10 in an SEM image taken with a scanning electron microscope (SEM). Here, the long side dimension L of the carrier 10 is the length of the longest line connecting any two points on the edge within the plane of the carrier 10 when the carrier 10 is viewed three-dimensionally. Furthermore, the thickness dimension d of the carrier 10 is the length of the shortest distance between the surface having the long side of the carrier 10 and the surface opposite to the surface having the long side of the carrier 10. As shown in FIG. 2, the long side dimension L is the length within the upper or lower surface of the carrier 10, and the thickness dimension d is the length within the side surface of the carrier 10.

[0035] For example, 200 carriers 10 are randomly selected from an SEM (SU8020, Hitachi High-Technologies Corporation) image, and the long side dimension L and thickness dimension d of each are measured to determine the average L / d ratio (N=200). The long side dimension L and thickness dimension d can be determined as appropriate.

[0036] In general, in the growth process of a zeolite-type compound, a spherical zeolite-type compound having a certain particle size (L), for example, a spherical zeolite-type compound having a particle size (L) of about 0.05 μm (L / d ratio of about 1), grows into a plate or coffin shape because the growth rate in a specific axial direction is fast. The growth rate in the long side direction is much faster than that in the thickness direction. It is believed that such a growth process of a zeolite-type compound can also be applied to the catalyst structure 1.

[0037] Thus, in the carrier 10 having a predetermined size, the growth rate in the long side direction is much higher than that in the thickness direction, and in the carrier 10 having a long side dimension L of 1.00 μm or more, the growth rate in the thickness direction is very slow. Therefore, the long side dimension L is also related to the catalytic activity of the catalyst structure 1, as in the above L / d ratio. From this viewpoint, the long side dimension L is preferably 1.00 μm or more, more preferably 1.00 μm or more and 50.00 μm or less, and even more preferably 1.00 μm or more and 25.00 μm or less. When the long side dimension L is 1.00 μm or more, the catalytic activity of the catalyst structure 1 is improved. As the long side dimension L increases, the catalytic activity is improved. Furthermore, when the long side dimension L is 50.00 μm or less, the yield is improved when manufacturing a highly active catalyst structure 1. Thus, the catalyst structure 1 having a long side dimension L of 1.00 μm or more and 50.0 μm or less has good manufacturing efficiency and high activity. The thickness dimension d of the carrier 10 is preferably 0.05 μm or more and 2.00 μm or less.

[0038] ≪Catalyst material≫ The catalytic material 20 will now be described in detail. The catalytic substance may be a metal consisting of one kind of metal element, a mixture of two or more kinds of metal elements, or metal fine particles in which at least a part of them is alloyed. The catalytic substance may also be an oxide of one or more kinds of metal elements, or metal oxide fine particles consisting of a composite material of these. In this specification, the "metal" (as a material) constituting the catalytic substance when used as a catalyst means a simple metal containing one kind of metal element (M) and a metal alloy containing two or more kinds of metal elements (M), and is a general term for metals containing one or more kinds of metal elements. The metal fine particles or metal oxide fine particles may be held in the passage 11 in the form of primary particles, or may be held in the form of secondary particles formed by agglomeration of primary particles.

[0039] The metal microparticles may be composed of any metal that is not oxidized, and may be composed of, for example, a single metal or a mixture of two or more metals. In this specification, the term "metal" (as a material) constituting the metal microparticles means a simple metal containing one metal element (M) and an alloy containing two or more metal elements (M), and is a general term for metals containing one or more metal elements.

[0040] Examples of metal elements contained in such metal microparticles and metal oxide microparticles include rhodium (Rh), ruthenium (Ru), iridium (Ir), palladium (Pd), platinum (Pt), molybdenum (Mo), tungsten (W), iron (Fe), cobalt (Co), chromium (Cr), cerium (Ce), copper (Cu), magnesium (Mg), aluminum (Al), nickel (Ni), etc., and it is preferable that one or more of the above be used as the main component.

[0041] In particular, from the viewpoint of catalytic activity, the metal microparticles are preferably microparticles composed of at least one metal selected from the group consisting of rhodium (Rh), ruthenium (Ru), iridium (Ir), palladium (Pd), platinum (Pt), iron (Fe), cobalt (Co) and nickel (Ni), and among these, from the viewpoints of rarity and price, it is more preferable for the metal microparticles to be microparticles composed of at least one metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni).

[0042] In general, the dry reforming method has a higher carbon content in the raw material than the steam reforming method, which reacts methane with steam. This means that carbon deposition is more likely to occur on the catalyst surface, which can lead to a decrease in catalytic activity, and there is also the problem of coking, which can block the catalyst layer inside the reaction tube. In addition, since precious metal catalysts (Pd, Rh, Ru, Pt) are expensive, there is a demand for the use of non-precious metal catalysts. Among these, Fe, Co, and Ni have attracted attention because of their low price and ease of availability. Ni, which is known to have the highest catalytic activity among these, is particularly prone to coking. In addition, Fe and Co have low catalytic activity, so the amount of coking is less than Ni, but these metals also cause coking when the catalytic activity is improved. Thus, there is a particularly high demand for non-precious metal catalysts, including Ni, to improve their catalytic activity as well as their coking resistance.

[0043] Incidentally, coking occurs when reactants come into contact with metal particles and polymerize while moving along the metal particles. Therefore, if the particle size of the metal particles is large, the reactants are more likely to polymerize on the metal particles, and conversely, if the particle size of the metal particles is small, polymerization is less likely to occur.

[0044] Even when the metal fine particles are fine particles composed of at least one metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni), particularly Ni fine particles, which have high catalytic activity, the average particle size D of the metal fine particles is C If the temperature can be maintained within a certain range, coking is sufficiently suppressed.

[0045] Average particle size of metal particles D C Within a certain range, the average particle size of metal particles D C The average particle diameter D of the metal particles is preferably 1.00 nm or more and 13.00 nm or less. C When the average particle diameter D is within the range, the catalytic activity is sufficiently increased. C As the average particle diameter D of the metal particles decreases, the catalytic activity improves. Cis preferably 9.00 nm or less, more preferably 4.50 nm or less. In addition, when the metal fine particles are fine particles composed of at least one metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni), the average particle diameter D C When the amount of the catalyst falls within the range, both the catalytic activity and the coking resistance are sufficiently improved.

[0046] The average particle diameter D of the metal particles which are the catalytic material 20 C can be measured, for example, as follows. The cross section of the catalyst structure 1 was measured by SAXS (small angle X-ray scattering), and the average particle diameter D of the metal particles was calculated by fitting the obtained SAXS data to a spherical model using the Guinier approximation method. C The measurement by SAXS can be performed using, for example, the beamline BL19B2 at Spring-8.

[0047] In addition, the average particle size D of the catalyst material 20 C is preferably the average inner diameter D of the passage 11 F and the inner diameter D of the expanded diameter portion 12 is E It is more preferable that the F <D C ≦D E ). In the passages 11, the catalytic material 20 is preferably enclosed in the enlarged diameter portions 12, and the movement of the catalytic material 20 in the carrier 10 is restricted. Therefore, even if the catalytic material 20 is subjected to an external force from the fluid, the movement of the catalytic material 20 in the carrier 10 is restricted, and the catalytic materials 20, 20, ... enclosed in the enlarged diameter portions 12, 12, ... dispersedly arranged in the passages 11 of the carrier 10 can be effectively prevented from contacting each other.

[0048] Also, the average inner diameter D of the passage 11 F Average particle size of metal particles D C Percentage of (D C / D F) is preferably 0.05 or more and 130.0 or less, more preferably 0.1 or more and 90.0 or less, even more preferably 1.1 or more and 45.0 or less, and particularly preferably 1.4 or more and 6.3 or less.

[0049] Furthermore, when the catalyst material 20 is metal fine particles, the metal element (M) of the metal fine particles is preferably contained in an amount of 0.5 mass% to 7.6 mass%, more preferably 0.5 mass% to 6.9 mass%, and even more preferably 0.5 mass% to 2.5 mass%, relative to the catalyst structure 1. For example, when the metal element (M) is Ni, the content (mass%) of the Ni element is expressed as {(mass of Ni element) / (mass of all elements in the catalyst structure 1)}×100.

[0050] Furthermore, the ratio of silicon (Si) constituting the carrier 10 to the metal element (M) constituting the metal microparticles (atomic ratio Si / M) is preferably 10 or more and 1000 or less, and more preferably 50 or more and 200 or less. If the ratio is more than 1000, the catalytic activity may be low, and the effect of the catalytic substance may not be fully obtained. On the other hand, if the ratio is less than 10, the proportion of the catalytic substance becomes too large, and the strength of the carrier 10 tends to decrease. Note that the metal microparticles 20 referred to here refer to microparticles present inside or supported by the carrier 10, and do not include metal microparticles attached to the outer surface of the carrier 10.

[0051] [Functions of the catalyst structure] As described above, the catalyst structure 1 includes a carrier 10 having a porous structure and at least one catalyst material 20 present in the carrier. The catalyst structure 1 exerts catalytic activity according to the function of the catalyst material 20 by contacting the catalyst material 20 present in the carrier 10 with a fluid. Specifically, as shown in FIG. 3, a fluid that has come into contact with the outer surface 10a of the catalyst structure 1 flows into the inside of the carrier 10 through holes 11a formed in the outer surface 10a, is guided into the passage 11, moves through the passage 11, and exits the catalyst structure 1 through another hole 11a. In the path in which the fluid moves through the passage 11, the fluid comes into contact with the catalyst material 20 held in the passage 11, causing a catalytic reaction according to the catalyst material 20. In addition, the catalyst structure 1 has a molecular sieve function because the carrier has a porous structure.

[0052] First, the molecular sieving ability of the catalyst structure 1 will be described with reference to FIG. 3(a) using a case where the fluid is a methane-containing gas and carbon dioxide as an example. The methane-containing gas refers to a mixed gas containing methane and a gas other than methane. The catalyst structure 1 may be contacted with the methane-containing gas and carbon dioxide in sequence or simultaneously.

[0053] As shown in FIG. 3(a), compounds (e.g., methane, carbon dioxide) composed of molecules having a size equal to or smaller than the pore size of the hole 11a, in other words, equal to or smaller than the inner diameter of the passage 11, can flow into the carrier 10. On the other hand, gas components 15 composed of molecules having a size larger than the pore size of the hole 11a cannot flow into the carrier 10. In this way, when the fluid contains multiple types of compounds, the reaction of the compounds that cannot flow into the carrier 10 is restricted, and the compounds that can flow into the carrier 10 can be reacted. In this embodiment, the reaction between methane and carbon dioxide proceeds.

[0054] Of the compounds produced in the carrier 10 by the reaction, only compounds composed of molecules having a size equal to or smaller than the pore diameter of the pores 11a can exit the carrier 10 through the pores 11a and are obtained as reaction products. On the other hand, compounds that cannot exit the carrier 10 through the pores 11a can be released to the outside of the carrier 10 by converting them into compounds composed of molecules having a size that allows them to exit the carrier 10. In this way, by using the catalyst structure 1, a specific reaction product can be selectively obtained. In this embodiment, specifically, methane and carbon dioxide react with each other to produce a synthesis gas containing carbon monoxide and hydrogen as a reaction product.

[0055] In the catalyst structure 1, as shown in FIG. 3(b), the catalyst material 20 is enclosed in the enlarged diameter portion 12 of the passage 11. The average particle diameter D of the catalyst material 20 (metallic fine particles) C is the average inner diameter D of passage 11 F The inner diameter D of the expanded diameter portion 12 is larger than E If it is smaller than (D F <D C <D E ), small passages 13 are formed between the catalyst material 20 and the expanded diameter section 12. There, as shown by the arrows in FIG. 3(b), the fluid that flows into the small passages 13 comes into contact with the catalyst material 20. Since each catalyst material 20 is enclosed in the expanded diameter section 12, movement within the carrier 10 is restricted. This prevents the catalyst materials 20 from coagulating together within the carrier 10. As a result, a large contact area between the catalyst material 20 and the fluid can be stably maintained.

[0056] In this embodiment, by using the catalyst structure 1, a synthesis gas containing carbon monoxide and hydrogen can be produced using methane-containing gas and carbon dioxide as raw materials. This catalytic reaction is carried out at a high temperature of, for example, 800°C or higher, but since the catalyst material 20 is contained within the support 10, it is not easily affected by heating. As a result, the decrease in catalytic activity is suppressed, and the life of the catalyst structure 1 can be extended.

[0057] In addition, the catalyst structure 1 was packed in a normal pressure flow reactor and subjected to GHSV5600h -1When a dry reforming reaction is carried out under the conditions of a total heating time of 60 minutes at or above 100°C after holding at 100°C for 10 minutes while supplying a raw material gas with a CO2 / CH4 ratio (volume ratio) of 1:1, the CH4 conversion at 700°C is preferably 20% or more, and more preferably 60% or more. Such a catalyst structure 1 has high catalytic activity.

[0058] In addition, when the catalyst structure 1 is subjected to the dry reforming reaction, the amount of coking in the catalyst structure after the reaction is analyzed by CHN measurement, and the amount of coking is preferably less than 5.0 mass%, more preferably less than 0.3 mass%, based on the total amount of the catalyst structure. Such a catalyst structure 1 having high catalytic activity is also excellent in coking resistance.

[0059] [Method of manufacturing catalyst structure] Fig. 4 is a flow chart showing a method for producing the catalyst structure 1 of Fig. 1. Hereinafter, an example of the method for producing the catalyst structure will be described taking as an example a case where the catalyst substance 20 present in the carrier is metal fine particles.

[0060] (Step S1: Preparation process) As shown in FIG. 4, first, a precursor material (A) having pores with a pore diameter of 13.0 nm or less is prepared to obtain a carrier having a porous structure composed of a zeolite-type compound. The precursor material (A) is preferably an ordered mesoporous material, and can be appropriately selected according to the type (composition) of the zeolite-type compound constituting the carrier of the catalyst structure. When the pore diameter of the pores of the precursor material (A) is 13.0 nm or less, the average particle diameter of the catalyst substance is easily controlled, and excellent catalytic activity and coking resistance are exhibited. Therefore, the pore diameter is 13.0 nm or less, preferably 10.0 nm or less, and more preferably 6.0 nm or less. As the pore diameter becomes smaller, the catalytic activity and coking resistance are improved. In addition, from the viewpoint of the ease of production and availability of the precursor material (A), the pore diameter of the pores of the precursor material (A) is preferably 0.7 nm or more, and more preferably 1.0 nm or more.

[0061] Here, when the zeolite type compound constituting the support of the catalyst structure is a silicate compound, the ordered mesoporous material is preferably a compound consisting of a Si-O skeleton in which pores having a pore diameter of 1.0 nm or more and 13.0 nm or less are uniform in size and regularly developed in one, two or three dimensions. Such ordered mesoporous materials can be obtained as various synthetic products depending on the synthesis conditions, and specific examples of synthetic products include, for example, SBA-1, SBA-15, SBA-16, KIT-6, FSM-16, MCM-41, etc., and among them, MCM-41 is preferred.

[0062] The pore diameter of SBA-1 is 8.0 nm or more and 13.0 nm or less, that of SBA-15 is 6.0 nm or more and 10.0 nm or less, that of SBA-16 is 6.0 nm, that of KIT-6 is 9.0 nm, that of FSM-16 is 3.0 nm or more and 5.0 nm or less, and that of MCM-41 is 1.0 nm or more and 10.0 nm or less. Examples of such regular mesoporous substances include mesoporous silica, mesoporous aluminosilicate, and mesoporous metallosilicate.

[0063] The precursor material (A) may be either a commercially available product or a synthetic product. When synthesizing the precursor material (A), a known method for synthesizing an ordered mesoporous material can be adopted. For example, a mixed solution containing raw materials containing the constituent elements of the precursor material (A) and a template agent for defining the structure of the precursor material (A) is prepared, and the pH is adjusted as necessary, followed by hydrothermal treatment (hydrothermal synthesis). Thereafter, the precipitate (product) obtained by the hydrothermal treatment is collected (for example, filtered), washed and dried as necessary, and further calcined to obtain the precursor material (A), which is a powdered ordered mesoporous material.

[0064] Here, as the solvent for the mixed solution, for example, water, organic solvents such as alcohol, and mixed solvents thereof can be used. In addition, the raw material is selected according to the type of carrier, and examples thereof include silica agents such as tetraethoxysilane (TEOS), fumed silica, and quartz sand. In addition, various surfactants, block copolymers, and the like can be used as the template agent, and it is preferable to select according to the type of the compound of the ordered mesoporous material. For example, when preparing MCM-41, a surfactant such as hexadecyltrimethylammonium bromide is suitable. The hydrothermal treatment can be performed, for example, in a sealed container under the treatment conditions of 80°C to 800°C, 5 hours to 240 hours, and more than 0 kPa to 2000 kPa. The calcination treatment can be performed, for example, in air under the treatment conditions of 350°C to 850°C, 2 hours to 30 hours.

[0065] (Step S2: Impregnation process) Next, the prepared precursor material (A) is impregnated with a metal-containing solution to obtain a precursor material (B).

[0066] The metal-containing solution may be any solution containing a metal component (e.g., metal ion) corresponding to the metal element (M) constituting the metal microparticles, and may be prepared, for example, by dissolving a metal salt containing the metal element (M) in a solvent. Examples of such metal salts include chlorides, hydroxides, oxides, sulfates, and nitrates, and among these, nitrates are preferred. Examples of the solvent that can be used include water, organic solvents such as alcohol, and mixtures thereof.

[0067] The method of impregnating the precursor material (A) with the metal-containing solution is not particularly limited, but for example, it is preferable to add the metal-containing solution in small amounts in multiple batches while stirring the powdered precursor material (A) before the firing step described below. In addition, from the viewpoint of making it easier for the metal-containing solution to penetrate into the pores of the precursor material (A), it is preferable to add a surfactant as an additive to the precursor material (A) before adding the metal-containing solution. Such an additive has the function of coating the outer surface of the precursor material (A), and is thought to suppress the adhesion of the metal-containing solution added thereafter to the outer surface of the precursor material (A), making it easier for the metal-containing solution to penetrate into the pores of the precursor material (A).

[0068] Examples of such additives include non-ionic surfactants such as polyoxyethylene alkyl ethers, such as polyoxyethylene oleyl ether, and polyoxyethylene alkyl phenyl ethers. These surfactants have a large molecular size and cannot penetrate into the pores of the precursor material (A), so they do not adhere to the inside of the pores and are considered not to hinder the metal-containing solution from penetrating into the pores. As a method for adding the non-ionic surfactant, for example, it is preferable to add 50% by mass or more and 500% by mass or less of the non-ionic surfactant to the precursor material (A) before the firing step described below. This range is preferable because the above-mentioned suppression effect is appropriately expressed and the increase in viscosity is also moderate.

[0069] In addition, the amount of the metal-containing solution added to the precursor material (A) is preferably adjusted appropriately in consideration of the amount of the metal element (M) contained in the metal-containing solution impregnated into the precursor material (A) (i.e., the amount of the metal element (M) contained in the precursor material (B)). For example, when the metal-containing solution is impregnated into the precursor material (A) before the firing step described later, the amount of the metal-containing solution added to the precursor material (A) is preferably adjusted so that the ratio of silicon (Si) constituting the precursor material (A) to the metal element (M) contained in the metal-containing solution added to the precursor material (A) (atomic ratio Si / M) is 10 or more and 1000 or less, more preferably 50 or more and 200 or less. For example, when a surfactant is added as an additive to the precursor material (A) before the metal-containing solution is added to the precursor material (A), the amount of the metal-containing solution added to the precursor material (A) can be set to 50 or more and 200 or less in terms of the atomic ratio Si / M, so that the metal element (M) of the metal microparticles can be contained at 0.5% by mass or more and 7.6% by mass or less relative to the catalyst structure 1.

[0070] In the state of precursor material (B), the amount of metal element (M) present inside its pores is roughly proportional to the amount of metal-containing solution added to precursor material (A) under the same metal concentration of the metal-containing solution, the presence or absence of the above-mentioned additive, and other conditions such as temperature and pressure. In addition, the amount of metal element (M) present in precursor material (B) is proportional to the amount of metal element constituting the metal fine particles present in the support of the catalyst structure. Therefore, by controlling the amount of metal-containing solution added to precursor material (A) within the above range, the metal-containing solution can be sufficiently impregnated into the pores of precursor material (A), and thus the amount of metal fine particles present in the support of the catalyst structure can be adjusted.

[0071] After the precursor material (A) is impregnated with the metal-containing solution, a washing process may be performed as necessary. As the washing solution, water, an organic solvent such as alcohol, or a mixture of these solvents may be used. In addition, after the precursor material (A) is impregnated with the metal-containing solution and washed as necessary, it is preferable to further perform a drying process. Examples of the drying process include natural drying for about one night, and high-temperature drying at 150°C or less. Note that if the precursor material (A) is subjected to the firing process described below in a state in which a large amount of moisture contained in the metal-containing solution and the moisture from the washing solution remain, the skeleton structure of the precursor material (A) as a regular mesoporous material may be destroyed, so it is preferable to dry it thoroughly.

[0072] (Step S3: Firing process) Next, precursor material (A) for obtaining a porous support composed of a zeolite-type compound is impregnated with a metal-containing solution to obtain precursor material (B), which is then calcined to obtain precursor material (C).

[0073] The calcination treatment is preferably carried out in air within a predetermined temperature range for 2 to 30 hours, for example. The predetermined temperature range in the calcination treatment is preferably 350° C. to 850° C., more preferably 500° C. to 850° C. By such a calcination treatment, crystals of the metal component impregnated in the pores of the ordered mesoporous material grow, forming metal fine particles in the pores.

[0074] (Step S4: Hydrothermal treatment process) Next, the precursor material (C) obtained by calcining the precursor material (B) is hydrothermally treated to obtain a catalyst structure. Preferably, in the hydrothermal treatment step, the precursor material (C) is hydrothermally treated using a mixed solution in which the precursor material (C) and a structure directing agent are mixed.

[0075] The structure-directing agent is a template agent for defining the skeletal structure of the support of the catalyst structure, and for example, a surfactant can be used. The structure-directing agent is preferably selected according to the skeletal structure of the support of the catalyst structure, and for example, surfactants such as tetramethylammonium bromide (TMABr), tetraethylammonium bromide (TEABr), and tetrapropylammonium bromide (TPABr) are suitable.

[0076] The precursor material (C) and the structure-directing agent may be mixed during the hydrothermal treatment process or before the hydrothermal treatment process. The method for preparing the mixed solution is not particularly limited, and the precursor material (C), the structure-directing agent, and the solvent may be mixed at the same time, or the precursor material (C) and the structure-directing agent may be individually dispersed in the solvent, and then the respective dispersion solutions may be mixed. As the solvent, for example, water, an organic solvent such as alcohol, or a mixture thereof may be used. In addition, it is preferable to adjust the pH of the mixed solution using an acid or a base before performing the hydrothermal treatment.

[0077] The hydrothermal treatment can be carried out by a known method, and is preferably carried out in a sealed container under the treatment conditions of 80° C. to 200° C., 5 hours to 100 hours, and a pressure of more than 0 kPa and less than 2000 kPa. The hydrothermal treatment is preferably carried out in a basic atmosphere. Although the reaction mechanism here is not entirely clear, by carrying out hydrothermal treatment using precursor material (C) as a raw material, the skeletal structure of precursor material (C) as an ordered mesoporous substance gradually collapses, but the positions of the metal particles inside the pores of precursor material (C) are roughly maintained, and a new skeletal structure (porous structure) is formed as a support for the catalyst structure due to the action of the structure-directing agent. The catalyst structure thus obtained comprises a support with a porous structure and metal particles present in the support, and the support further has passages in which a plurality of pores are interconnected due to the porous structure, and at least a portion of the metal particles are present in the passages of the support.

[0078] In addition, in the present embodiment, in the above-mentioned hydrothermal treatment step, a mixed solution is prepared by mixing the precursor material (C) and the structure-directing agent, and the precursor material (C) is hydrothermally treated. However, this is not limited thereto, and the precursor material (C) may be hydrothermally treated without mixing the precursor material (C) with the structure-directing agent.

[0079] The ratio of the long side dimension L to the thickness dimension d (L / d ratio) of the carrier can be adjusted by the hydrothermal treatment process. The desired ratio of the long side dimension L to the thickness dimension d can be obtained by appropriately selecting the basicity, treatment temperature, treatment time, and treatment pressure. For example, by carrying out hydrothermal treatment under at least one of the treatment conditions of increasing the basicity, increasing the treatment temperature, extending the treatment time, and applying pressure, the shape of the support can be adjusted so that it first grows in the length direction and then grows in the thickness direction. The precipitate (catalyst structure) obtained after the hydrothermal treatment is preferably subjected to washing, drying and calcination as necessary after recovery (for example, filtration). As the washing solution, water, an organic solvent such as alcohol, a mixed solvent thereof, etc. can be used. As the drying treatment, natural drying for about one night, or high-temperature drying at 150°C or less can be used. If the calcination treatment is performed in a state where a large amount of moisture remains in the precipitate, the skeletal structure as a support of the catalyst structure may be broken, so it is preferable to dry it thoroughly. In addition, the calcination treatment can be performed, for example, in air under treatment conditions of 350°C to 850°C and 2 hours to 30 hours. The structure-directing agent attached to the catalyst structure is burned by such a calcination treatment. In addition, the catalyst structure can be used as it is without performing a calcination treatment on the precipitate after recovery depending on the purpose of use. For example, when the environment in which the catalyst structure is used is a high-temperature environment in an oxidizing atmosphere, the structure-directing agent is burned by exposing it to the use environment for a certain period of time. In this case, the catalyst structure is obtained similar to that obtained when the calcination treatment is performed, so that the calcination treatment is not necessary.

[0080] The above-described manufacturing method is an example in which the metal element (M) contained in the metal-containing solution to be impregnated into the precursor material (A) is a metal species that is difficult to oxidize (for example, a noble metal).

[0081] When the metal element (M) contained in the metal-containing solution to be impregnated into the precursor material (A) is a metal species (e.g., Fe, Co, Ni, etc.) that is easily oxidized, it is preferable to further perform a reduction treatment on the hydrothermally treated precursor material (C) after the hydrothermal treatment step. When the metal element (M) contained in the metal-containing solution is a metal species that is easily oxidized, the metal component is oxidized by the heat treatment in the steps (steps S3 to S4) after the impregnation treatment (step S2). Therefore, the support formed in the hydrothermal treatment step (step S4) will have metal oxide fine particles inside. Therefore, in order to obtain a catalyst structure in which metal fine particles are inside the support, it is desirable to perform a calcination treatment on the recovered precipitate after the hydrothermal treatment, and further a reduction treatment under a reducing gas atmosphere such as hydrogen gas. By performing a reduction treatment on the precipitate as a precursor of the catalyst structure, the metal oxide fine particles as the precursor material of the catalyst material inside the support are reduced, and metal fine particles corresponding to the metal element (M) constituting the metal oxide fine particles are formed. As a result, a catalyst structure in which metal fine particles are inside the support is obtained. In addition, such reduction treatment may be performed as necessary. For example, when the environment in which the catalyst structure is used is a reducing atmosphere, the metal oxide fine particles as the precursor material of the catalyst substance are reduced by exposing the catalyst structure to the use environment for a certain period of time. In this case, the catalyst structure obtained is the same as that obtained by the reduction treatment, so there is no need to perform the reduction treatment. In addition, the metal oxide remaining in the catalyst substance also corresponds to the precursor of the catalyst substance.

[0082] [Modification of catalyst structure 1] FIG. 5 is a schematic diagram showing a modification of the catalyst structure 1 of FIG. The catalyst structure 1 in FIG. 1 comprises a carrier 10 and a catalyst material 20 contained within the carrier 10, but is not limited to this configuration. For example, as shown in FIG. 5, the catalyst structure 2 may further comprise another catalyst material 30 supported on the outer surface 10a of the carrier 10.

[0083] The catalytic material 30 is a material that exhibits one or more catalytic activities. The catalytic activity of the other catalytic material 30 may be the same as or different from the catalytic activity of the catalytic material 20. In addition, when both the catalytic materials 20 and 30 are materials having the same catalytic activity, the material of the other catalytic material 30 may be the same as or different from the material of the catalytic material 20. According to this configuration, the content of the catalytic material held in the catalytic structure 2 can be increased, and the catalytic activity of the catalytic material can be further promoted.

[0084] In this case, the content of the catalytic material 20 present in the carrier 10 is preferably greater than the content of the other catalytic material 30 held on the outer surface 10a of the carrier 10. This makes the catalytic activity of the catalytic material 20 held inside the carrier 10 predominant, and the catalytic activity of the catalytic material is stably exhibited.

[0085] The synthesis gas production apparatus of the embodiment includes the above-mentioned catalyst structure 1 or catalyst structure 2, or a precursor of the catalyst structure 1 or a precursor of the catalyst structure 2. As the synthesis gas production apparatus including the above-mentioned catalyst structure, a synthesis gas production apparatus using dry reforming, a synthesis gas production apparatus using steam reforming, a synthesis gas production apparatus using a partial oxidation reaction, or a synthesis gas production apparatus using autothermal reforming is preferable. Such a synthesis gas production apparatus has excellent catalytic activity and coking resistance due to high sintering resistance, and can stably produce synthesis gas for a long period of time.

[0086] According to the embodiment described above, it is possible to provide a catalyst structure that has both high catalytic activity and high coking resistance. Therefore, the catalyst structure can efficiently produce synthesis gas for a long period of time.

[0087] Although the embodiment has been described above, the present invention is not limited to the above embodiment, and various modifications and changes are possible based on the technical concept of the present invention. EXAMPLES

[0088] (Examples 1 to 22) [Synthesis of precursor material (A)] A mixed aqueous solution was prepared by mixing a silica agent (tetraethoxysilane (TEOS), manufactured by Wako Pure Chemical Industries, Ltd.) with a surfactant as a template agent, and the pH was appropriately adjusted. The solution was subjected to hydrothermal treatment in a sealed container at 80°C to 350°C for 100 hours. The resulting precipitate was then filtered, washed with water and ethanol, and calcined in air at 600°C for 24 hours to obtain precursor material (A) with the type and pore size shown in Table 1. The following surfactants were used according to the type of precursor material (A) ("Type of precursor material (A): Surfactant"). MCM-41: Hexadecyltrimethylammonium bromide (CTAB) (Wako Pure Chemical Industries, Ltd.) SBA-1: Pluronic P123 (BASF)

[0089] [Preparation of precursor materials (B) and (C)] Next, nickel (II) nitrate hexahydrate (manufactured by Wako Pure Chemical Industries, Ltd.) was dissolved in water to prepare a Ni-containing aqueous solution.

[0090] Next, the Ni-containing aqueous solution was added in small amounts in several batches to the powdered precursor material (A), and the mixture was dried at room temperature (20° C.±10° C.) for 12 hours or more to obtain a precursor material (B).

[0091] Before the addition of the Ni-containing aqueous solution, the precursor material (A) was pretreated by adding an aqueous solution of polyoxyethylene (15) oleyl ether (NIKKOL BO-15V, manufactured by Nikko Chemicals Co., Ltd.) as an additive, and then the Ni-containing aqueous solution was added as described above.

[0092] The amount of the Ni-containing aqueous solution added to the precursor material (A) was adjusted so that the ratio of silicon (Si) constituting the precursor material (A) to the Ni element (M) contained in the Ni-containing aqueous solution (atomic number ratio Si / M) would be 100.

[0093] Next, the precursor material (B) impregnated with the Ni-containing aqueous solution obtained as described above was calcined in air at 600° C. for 24 hours to obtain a precursor material (C).

[0094] The precursor material (C) obtained as described above was mixed with the structure-directing agent tetrapropylammonium bromide (TPABr) to prepare a mixed solution, which was then subjected to hydrothermal treatment in a sealed container under the conditions of pH, time, and time shown in Table 1. The resulting precipitate was then filtered, washed with water, dried at 100°C for 12 hours or more, and then calcined in air at 600°C for 24 hours. In Examples 1 to 22, after the calcination treatment, the calcined product was collected and reduced at 700°C for 90 minutes under a flow of hydrogen gas to obtain a catalyst structure having a support and metal fine particles (Ni fine particles) shown in Table 2. The pH shown in Table 1 was measured when the resulting precipitate was filtered.

[0095] Comparative Example 1 In Comparative Example 1, alumina (manufactured by Wako) was impregnated with an aqueous solution of nickel nitrate and fired at 800°C for 2h (in an air atmosphere) to obtain a 1 mass% Ni / Al2O3 catalyst structure in which 1 mass% Ni fine particles were supported on the outer surface of a support made of Al2O3.

[0096] Comparative Example 2 In Comparative Example 2, a commercially available catalyst structure of 66 mass% Ni / Al2O3-SiO2 (manufactured by Alfa Aesar) was used, in which 66 mass% Ni fine particles were supported on the outer surface of a support made of Al2O3-SiO2.

[0097] Comparative Example 3 In Comparative Example 3, the catalyst structure shown in Table 2 was obtained using the raw materials and conditions shown in Table 1.

[0098] [evaluation] For the catalyst structures of Examples 1 to 22 and Comparative Examples 1 and 2, various property evaluations were carried out under the conditions shown below.

[0099] [A] Cross-section observation For the catalyst structures of Examples 1 to 22 and Comparative Examples 1 to 3, observation samples were prepared by a pulverization method, and cross-sections were observed using a transmission electron microscope (TEM) (TITAN G2, manufactured by FEI). As a result, it was confirmed that the catalytic substance was present and held inside the carrier made of silicalite in all of the catalyst structures of Examples 1 to 22 and the catalyst structure of Comparative Example 3. On the other hand, it was also confirmed that in Comparative Examples 1 and 2, the metal fine particles were only attached to the outer surface of the carrier and were not present inside the carrier.

[0100] In addition, cross sections of the catalyst structures of Examples 1 to 22 and Comparative Example 3 were cut out by FIB (focused ion beam) processing, and cross-sectional elemental analysis was performed using a SEM (SU8020, Hitachi High-Technologies Corporation) and an EDX (X-Max, Horiba, Ltd.) As a result, Ni elements were detected from inside the support. From the results of the above-mentioned cross-sectional observations by TEM and SEM / EDX, it was confirmed that nickel fine particles were present inside the carrier in all of the catalyst structures of Examples 1 to 22.

[0101] [B] The average inner diameter of the support passages and the average particle size of the catalyst material In the TEM image taken by the cross-sectional observation performed in the above evaluation [A], 500 passages of the carrier were randomly selected, the major axis and minor axis of each were measured, and the inner diameter of each was calculated from the average value (N=500). The average inner diameter was then calculated to obtain the average inner diameter D of the carrier passages. F It was decided.

[0102] In addition, to confirm the average particle size and dispersion state of the catalyst material, analysis was performed using SAXS (small angle X-ray scattering). SAXS measurements were performed using the beamline BL19B2 at Spring-8. The obtained SAXS data was fitted with a spherical model using the Guinier approximation method to calculate the particle size. As a result, it was found that in the catalyst structure of each embodiment having metal microparticles (Ni microparticles) with an average particle size in the range of 1.44 nm or more and 8.00 nm or less, the catalyst material has uniform particle size and is present in a highly dispersed state inside the support.

[0103] [C] Evaluation of carrier size The size of the carriers was evaluated using a SEM (SU8020, Hitachi High-Technologies Corporation). 200 carriers were randomly selected, and the long side dimension L and thickness dimension d of each were measured. Furthermore, the average value (N=200) of the ratio of the long side dimension L to the thickness dimension d (L / d ratio) was calculated.

[0104] For example, Example 3 (long side dimension 2.29 μm, thickness dimension 0.37 μm), Example 4 (long side dimension 3.76 μm, thickness dimension 0.52 μm), Example 5 (long side dimension 10.16 μm, thickness dimension 0.98 μm), Example 6 (long side dimension 11.97 μm, thickness dimension 0.69 μm), Example 7 (long side dimension 19.30 μm, thickness dimension 0.58 μm), and Example 9 (long side dimension 16.54 μm, thickness dimension 0.78 μm). Although only the long side dimension and thickness dimension for Examples 3 to 7 and 9 are disclosed above, in all Examples including Examples 3 to 7 and 9, the long side dimension L was 1.00 or more and 25.00 μm or less, and the thickness dimension d was 0.05 μm or more and 1.00 μm or less. On the other hand, in the catalyst structure of Comparative Example 3, the ratio of the long side dimension L to the thickness dimension d (L / d ratio) was 1.0.

[0105] [D] Performance evaluation The catalytic activity of the catalyst substance of the catalyst structures of the examples and comparative examples was evaluated. The results are shown in Table 3.

[0106] (1)Catalytic activity The catalytic activity in dry reforming was evaluated. 50 mg of the catalyst structures of Examples 1 to 22 and Comparative Examples 1 to 3 were packed in an atmospheric pressure flow reactor, and CO2 (5 ml / min), CH4 (5 ml / min), and GHSV 5600 h were used. -1While supplying the raw material gas at 100°C, the temperature was held at 100°C for 10 minutes, then the temperature was raised to 900°C at 20°C / min and held at that temperature for 10 minutes, for a total heating time of 60 minutes above 100°C. A single microreactor (Rx-3050SR, manufactured by Frontier Labs) was used as the atmospheric pressure flow reaction apparatus. The products were analyzed using gas chromatography mass spectrometry (GC / MS).

[0107] The catalytic activity in dry reforming was evaluated based on the CH4 conversion rate at a temperature of 700°C during the temperature increase process from 100°C to 900°C, using the following criteria. CH4 conversion rate of 60% or more: ◎ CH4 conversion rate is 40% or more but less than 60%: Yes CH4 conversion rate is between 20% and 40%: △ CH4 conversion rate is less than 20%: ×

[0108] (2) Caulking resistance For the catalyst structures evaluated for the catalytic activity (1) above, the amount of carbon on the catalyst (amount of coke produced) was analyzed using a CHN elemental analyzer (instrument name: CE-440, manufactured by EXETER ANALYTICAL, INC.). The coking resistance was evaluated based on the amount of coke relative to the total mass of the catalyst structure, using the following criteria. Coke content less than 0.3% by mass: ◎ Coke content is 0.3% by mass or more and less than 1.0% by mass: 〇 Coke content is 1.0% by mass or more and less than 5.0% by mass: △ Coke content is 5.0% by mass or more: ×

[0109] Since it is required that both catalytic activity and coking resistance are excellent, the lower of the two was judged as the overall evaluation of the catalyst, and thus the catalyst structure was evaluated accordingly.

[0110] [Table 1]

[0111] [Table 2]

[0112] [Table 3]

[0113] As is clear from Tables 1 to 3, the catalyst structures (Examples 1 to 22) in which it was confirmed by cross-sectional observation that the catalytic substance was retained inside the support exhibited superior catalytic activity and coking resistance in the dry reforming reaction, compared with the catalyst structures (Comparative Examples 1 and 2) in which the catalytic substance was simply attached to the outer surface of the support. In addition, when a similar performance evaluation measurement was performed on the catalyst structure of Comparative Example 3, in which the long side dimension L and the thickness dimension d were equal (L / d=1.0), the measurement was very unstable. The reason for this is considered to be that when the catalyst structure of Comparative Example 3 was packed in the catalyst layer of the atmospheric pressure flow-type reactor, the packing density of the catalyst structure became higher than that of the above-mentioned Examples, making it difficult for the raw material gas, which is the substrate, to enter the inside of the passages of the catalyst structure, and other factors, which made the measurement very unstable.

[0114] (3) Long-term testing of catalytic activity and coking resistance The catalyst structures of Examples 3 to 6, 9, 15 to 18 and Comparative Examples 1 and 2 were used to evaluate the catalytic activity and coking resistance in a long-term test. 50 mg of each of the catalyst structures of the Examples and Comparative Examples was packed into a normal pressure flow reactor, and CO2 (5 ml / min), CH4 (5 ml / min), and GHSV 5600 h were used. -1While supplying the raw material gas at 100°C, the temperature was held at 100°C for 10 minutes, then increased to 900°C at 20°C / min, and held so that the total heating time at 100°C or higher was 300 minutes. However, in Comparative Examples 1 and 2, which had a large amount of coking in the evaluation of "(2) Coking Resistance", the total heating time was set to 60 minutes. A single microreactor (Rx-3050SR, manufactured by Frontier Labs) was used as the normal pressure flow type reaction apparatus. The product was analyzed using gas chromatography (GC) and gas chromatography mass spectrometry (GC / MS). The analyzer for the generated gas was TRACE 1310GC (manufactured by Thermo Fisher Scientific, Inc., detector: thermal conductivity detector).

[0115] The CH4 conversion rate of the catalyst activity was judged using the same criteria as in "(1) Catalytic activity" above, and the amount of coke on the catalyst after 300 minutes of reaction was analyzed using the CHN elemental analyzer used in "(2) Coking resistance" above. The results are shown in Table 4. Table 4 also shows the initial catalyst activity results shown in Table 3. In Table 4, the symbol "※1" indicates that the coke amount could not be detected because the detection limit of the CHN elemental analyzer was less than 0.30 mass%. The symbol "※2" indicates that long-term test evaluation was not possible due to poor catalyst activity. The symbol "※3" indicates that a large amount of coke, 20.64 mass%, had already been generated at the initial reaction time (after 60 minutes), so long-term test evaluation after 300 minutes was abandoned. As shown in Table 4, the 1 mass% Ni / Al2O3 catalyst structure (Comparative Example 1) had poor initial catalytic activity, and even at an extremely low level of catalytic activity, the amount of coke was 1.20 mass%. The commercially available 66 mass% Ni / Al2O3-SiO2 catalyst structure (Comparative Example 2) had relatively high initial catalytic activity, but a large amount of coke (20 mass% or more) was formed on the catalyst after a total heating time of 60 minutes.

[0116] In contrast, the catalyst structures of Examples 3 to 6, 9, and 15 to 18 all maintained good catalytic activity even after 300 minutes of reaction, and the amount of coke was below the detection limit of the analytical instrument, confirming that they exhibited very good catalytic activity and coking resistance. Also, it is noteworthy that the amount of coke produced in the highly active Examples 3 to 6, 9, and 15 to 18 was suppressed to below the detection limit, even compared to Comparative Example 1, which had extremely low catalytic activity.

[0117] [Table 4]

[0118] In addition, since it is not possible to directly compare with the above examples, Quan Luu Manh Ha et al. have reported a Ni-based catalyst in which a dry reforming reaction was carried out for 480 minutes at a reaction temperature of 600°C while supplying a mixed gas of CH4 / CO2 / He (45 volume% / 45 volume% / 10 volume%), and the amount of coke generated at this time was 0.65 mass% (Catalysts 2017, 7, 157:doi:10.3390 / catal7050157). Due to equipment restrictions, it is difficult to completely match the reaction conditions of Quan Luu Manh Ha et al., so it is difficult to make a general comparison, but while the amount of coke generated in the prior art was 0.65 mass%, in this example, the reaction temperature was 100°C higher than that of the prior art, but the amount of coke generated was below the detection limit (0.30 mass%). Generally, in a dry reforming reaction, the catalytic activity increases as the reaction temperature increases, but it is well known that the amount of coke produced also increases with the improvement in catalytic activity.

[0119] In fact, looking at Comparative Examples 1 and 2, which have different amounts of Ni, when the amount of Ni is large, the catalytic activity improves from "x" to "good", but this leads to a dramatic increase in the amount of coke produced (see Table 4). In contrast, this embodiment succeeded in suppressing the amount of coke produced, despite the reaction conditions under which coking is more likely to occur than with catalysts such as Quan Luu Manh Ha. This also shows that this embodiment is a catalyst structure that has both high activity and excellent coking resistance compared to the prior art. [Explanation of symbols]

[0120] 1, 2 Catalyst structure 10. Carriers 10a outer surface 11 Passage 11a hole 12 Expanded diameter part 20 Catalyst material 30 Catalyst material

Claims

1. A catalyst structure for producing a synthesis gas used in producing a synthesis gas containing carbon monoxide and hydrogen, A porous support composed of a zeolite-type compound; at least one catalytic material internal to said support; Equipped with The carrier has passages communicating with each other, The ratio of the long side dimension L to the thickness dimension d of the carrier (L / d ratio) is 5.0 or more; the catalytic substance is a metal fine particle composed of at least one metal element selected from the group consisting of rhodium (Rh), ruthenium (Ru), iridium (Ir), palladium (Pd), platinum (Pt), molybdenum (Mo), tungsten (W), iron (Fe), cobalt (Co), chromium (Cr), cerium (Ce), copper (Cu), magnesium (Mg), aluminum (Al), and nickel (Ni); the catalytic material is present in at least the passages of the support; the average particle size of the catalytic material is greater than the average inner diameter of the passages; the passage has one of one-dimensional pores, two-dimensional pores, and three-dimensional pores in the framework structure of the zeolite-type compound, and an expanded portion different from any of the one-dimensional pores, the two-dimensional pores, and the three-dimensional pores; the catalytic material is present at least in the expanded diameter portion; the average particle size of the catalyst material is equal to or smaller than the inner diameter of the expanded diameter portion; A catalyst structure for synthesis gas production, characterized in that the average inner diameter of the passages is calculated from an average value of the minor axis and the major axis of the pores constituting any one of the one-dimensional pores, the two-dimensional pores, and the three-dimensional pores.

2. A catalyst structure for producing a synthesis gas used in producing a synthesis gas containing carbon monoxide and hydrogen, A porous support composed of a zeolite-type compound; at least one catalytic material internal to said support; Equipped with The carrier has passages communicating with each other, The ratio of the long side dimension L to the thickness dimension d of the carrier (L / d ratio) is 5.0 or more; The catalytic material is present in at least the passages of the support, and has an average particle size of 1.00 nm or more and 13.00 nm or less; the average particle size of the catalytic material is greater than the average inner diameter of the passages; the passage has one of one-dimensional pores, two-dimensional pores, and three-dimensional pores in the framework structure of the zeolite-type compound, and an expanded portion different from any of the one-dimensional pores, the two-dimensional pores, and the three-dimensional pores; the catalytic material is present at least in the expanded diameter portion; the average particle size of the catalyst material is equal to or smaller than the inner diameter of the expanded diameter portion; A catalyst structure for synthesis gas production, characterized in that the average inner diameter of the passages is calculated from an average value of the minor axis and the major axis of the pores constituting any one of the one-dimensional pores, the two-dimensional pores, and the three-dimensional pores.

3. The catalyst structure for producing synthetic gas as described in claim 1 or 2, characterized in that the L / d ratio of the support is 5.0 or more and 35.0 or less.

4. The catalyst structure for producing synthetic gas as described in claim 1 or 2, characterized in that the L / d ratio of the support is 7.0 or more and 25.0 or less.

5. The catalyst structure for synthesis gas production according to any one of claims 1 to 4, wherein the expanded diameter portion connects a plurality of holes constituting any one of the one-dimensional holes, the two-dimensional holes, and the three-dimensional holes to each other.

6. 3. The catalyst structure for producing synthetic gas according to claim 2, wherein the catalyst material is fine metal particles.

7. The average inner diameter D of the passage F The average particle diameter D of the metal fine particles C The ratio of (D C / D F 7. The catalyst structure for producing synthesis gas according to claim 1, wherein the molecular weight ratio (Mg / mol) is 0.05 or more and 130.0 or less.

8. The catalyst structure for producing synthetic gas according to any one of claims 1 and 6 to 7, characterized in that the metal fine particles are fine particles composed of at least one metal selected from the group consisting of iron (Fe), cobalt (Co) and nickel (Ni).

9. 9. The catalyst structure for producing synthetic gas according to claim 1, wherein the metal particles are particles made of nickel (Ni).

10. 3. The catalyst structure for producing synthesis gas according to claim 2, wherein the catalyst material is fine metal oxide particles.

11. 11. The catalyst structure for producing synthesis gas according to claim 1, further comprising at least one other catalytic material supported on the outer surface of the support.

12. 12. The catalyst structure for producing synthesis gas according to claim 11, wherein the content of the at least one catalytic material present within the support is greater than the content of the at least one other catalytic material carried on the outer surface of the support.

13. 13. The catalyst structure for producing synthesis gas according to claim 1, wherein the zeolite type compound is a silicate compound.

14. The catalyst structure for producing synthetic gas is packed in an atmospheric pressure flow type reactor and is operated at a GHSV of 5600h. -1 , CO 2 / CH 4 The raw material gas was supplied at a ratio (volume ratio) of 1:1, and the temperature was held at 100°C for 10 minutes, then increased to 900°C at a rate of 20°C / min. The total heating time at or above 100°C was 60 minutes. When the dry reforming reaction was carried out under these conditions, 4 The catalyst structure for producing a synthesis gas according to any one of claims 1 to 13, characterized in that the conversion rate is 20% or more.

15. The catalyst structure for producing synthesis gas has a CH 4 The catalyst structure for producing synthesis gas according to claim 14, characterized in that the conversion rate is 60% or more.

16. 16. The catalyst structure for synthesis gas production according to claim 14 or 15, wherein, when the dry reforming reaction is carried out, the amount of coking in the catalyst structure for synthesis gas production after the reaction is analyzed by CHN measurement is less than 5.0 mass% with respect to the total amount of the catalyst structure for synthesis gas production.

17. The catalyst structure for synthesis gas production according to any one of claims 14 to 16, characterized in that, when the dry reforming reaction is carried out, the amount of coking when the catalyst structure for synthesis gas production after the reaction is analyzed by CHN measurement is less than 0.3 mass% with respect to the total amount of the catalyst structure for synthesis gas production.

18. A synthesis gas production apparatus comprising the catalyst structure for synthesis gas production according to any one of claims 1 to 17.

19. a calcination step of calcining a precursor material (B) impregnated with a metal-containing solution containing at least one metal element selected from the group consisting of rhodium (Rh), ruthenium (Ru), iridium (Ir), palladium (Pd), platinum (Pt), molybdenum (Mo), tungsten (W), iron (Fe), cobalt (Co), chromium (Cr), cerium (Ce), copper (Cu), magnesium (Mg), aluminum (Al), and nickel (Ni) in a precursor material (A) having pores with a pore diameter of 13.0 nm or less in order to obtain a carrier having a porous structure composed of a zeolite-type compound; a hydrothermal treatment step of subjecting a precursor material (C) obtained by calcining the precursor material (B) to a hydrothermal treatment to obtain a catalyst structure having a ratio of a long side dimension L to a thickness dimension d (L / d ratio) of the support of 5.0 or more; having A method for producing a catalyst structure for producing a synthetic gas, comprising mixing the precursor material (C) with a structure-directing agent in the hydrothermal treatment step.

20. 20. The method for producing a catalyst structure for producing a synthesis gas according to claim 19, characterized in that a nonionic surfactant is added in an amount of 50 mass % or more and 500 mass % or less to the precursor material (A) before the calcination step.

21. 21. The method for producing a catalyst structure for producing a synthesis gas according to claim 19 or 20, characterized in that, before the calcination step, the metal-containing solution is added to the precursor material (A) in a plurality of portions, thereby impregnating the precursor material (A) with the metal-containing solution.

22. 22. The method for producing a catalyst structure for synthesis gas production according to any one of claims 19 to 21, characterized in that, when impregnating the precursor material (A) with the metal-containing solution before the calcination step, an amount of the metal-containing solution added to the precursor material (A) is adjusted so that a ratio (atomic ratio Si / M) of silicon (Si) constituting the precursor material (A) to a metal element (M) contained in the metal-containing solution added to the precursor material (A) is 10 or more and 1000 or less.

23. The method for producing a catalyst structure for producing synthesis gas according to any one of claims 19 to 22, characterized in that the hydrothermal treatment step is carried out under a basic atmosphere.

24. The hydrothermally treated precursor material (C) is then subjected to a reduction treatment under a reducing gas atmosphere. The catalyst for producing synthetic gas according to any one of claims 19 to 23, further comprising A method for manufacturing a medium structure.

25. A method for using the catalyst structure for producing synthetic gas according to claim 1, which comprises exposing the catalyst structure for producing synthetic gas to a reducing atmosphere.

Citation Information

Patent Citations

  • Method of synthesizing MFI-type zeolite, MFI-type zeolite crystal, substrate coated with MFI-type zeolite, method of manufacturing zeolite film, and method for separation

    JP2003238147A

  • Catalyst for producing synthesis gas and production method of synthesis gas

    JP2013255911A

  • Catalyst and method for producing syngas

    JP2014200705A

  • Methods for producing and forming supported activated metal catalysts and precursors