UV-active derivatives of Pd(AcAc)2-catalyzed polycycloolefin compositions as optical materials

A single-component composition for OLEDs using olefin monomers and palladium compounds addresses refractive index mismatch and environmental sensitivity, enhancing photon transmission and stability in OLED devices.

JP7575461B2Active Publication Date: 2024-10-29SUMITOMO BAKELITE CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022539647
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-30
Filing Date
2020-12-30
Publication Date
2024-10-29
Estimated Expiration
2040-12-30

AI Technical Summary

Technical Problem

Existing OLEDs face challenges with photon loss due to mismatched refractive indices between organic layers and glass substrates, and are sensitive to moisture and temperature, requiring improved organic fillers with high transmittance and thermal stability.

Method used

A single-component, bulk polymerizable composition comprising olefin monomers, organopalladium compounds, photoacid generators, and photosensitizers that undergo rapid vinyl addition polymerization upon actinic radiation, forming transparent films with refractive indices matching OLED layers and providing adhesion and stability.

Benefits of technology

The composition enhances photon transmission, reduces plasmon loss, and provides stable, uniform optical layers with low shrinkage, suitable for OLED devices, offering improved adhesion and protection against environmental factors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575461000132
    Figure 0007575461000132
  • Figure 0007575461000133
    Figure 0007575461000133
  • Figure 0007575461000134
    Figure 0007575461000134
Patent Text Reader

Abstract

An embodiment of the present invention is a composition comprising an organopalladium compound, a photoacid generator, a photosensitizer, and one or more olefin monomers, which undergo vinyl addition polymerization to form a substantially transparent film upon exposure to suitable actinic radiation. The monomers employed in the present invention have a wide range of optical and mechanical properties, allowing the composition to be tailored to form films with a variety of optoelectronic properties. Thus, the compositions of the present invention are useful as coatings, encapsulants, fillers, and levelers, among other applications.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] Cross-reference to related applications This application claims the benefit of U.S. Provisional Application No. 62 / 954,911, filed December 30, 2019, which is incorporated herein by reference.

[0002] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention generally relates to single-component, bulk-polymerizable polycycloolefin monomer compositions that have excellent optical transparency and suitable refractive indexes that match the refractive index of layers in optical sensors, light emitting diodes (LEDs), and organic light emitting diodes (OLEDs), among other optical devices. More specifically, the present invention relates to single-component compositions that include norbornene (NB)-based olefin monomers that undergo vinyl addition bulk polymerization to form optical layers for use in a variety of optoelectronic applications, including as encapsulants, coatings, and fillers. [Background technology]

[0003] Organic light-emitting diodes (OLEDs) play an important role in a variety of applications, especially in flexible displays, such as flat TVs. However, existing OLEDs, especially bottom-emitting OLEDs, have the disadvantage that only about half of the generated photons are incident on the glass substrate, and 25% of them are emitted into the air. The other half of the photons are guided and dissipated inside the OLED stack. This photon loss is mainly due to the mismatch of the refractive index (n) of the organic layers (n=1.7-1.9) and the glass substrate (n=1.5). By matching the refractive index (n=1.8) of the substrate and the organic layers and increasing the distance of the emission area to the cathode to suppress plasmonic losses, the photons incident on the substrate can be increased to 80-90%. See, for example, G.Gaertner et al., Proc.of SPIE, Vol.6999, 69992T pp1-12(2008).

[0004] OLEDs also face another challenge: OLEDs, made of organic materials, are generally very sensitive to moisture, oxygen, temperature, and other weather conditions. Therefore, it is important to protect OLEDs from these harsh weather conditions. See, for example, U.S. Patent Publication No. 2012 / 0009393.

[0005] In order to solve the problems faced in this field to some extent, U.S. Patent No. 8,263,235 discloses a method of using an organic light-emitting material and a light-emitting layer formed from at least one aliphatic compound having no aromatic ring, and the refractive index of the emitted light is 1.4 to 1.6. The aliphatic compound described in the patent is generally polyalkyl ethers, etc., and it is well known that the material is unstable at high temperatures. For an example, see Rodriguez et al., I&EC Product Research and Development, Vol.1, No.3, 206-210 (1962).

[0006] U.S. Patent Nos. 9,944,818 and 10,266,720 disclose two-component bulk polymerizable compositions that can be tailored to a desired refractive index, are suitable as fillers and protective coatings, and can be used in the manufacture of various OLED devices.

[0007] Copending U.S. application Ser. No. 15 / 861,801, filed Jan. 4, 2018, discloses single-component vinyl addition bulk polymerizable compositions that can be thermally activated, tuned to a desired refractive index, and are suitable as fillers and protective coatings and can be used to fabricate a variety of OLED devices.

[0008] However, there remains a need for organic fillers that complement the refractive index of OLEDs while exhibiting high transmittance and excellent thermal properties, among other desirable properties. Furthermore, among the various applications described herein, it is desirable for the organic fillers to be available as single-component compositions that readily form permanent protective coatings upon exposure to appropriate actinic radiation at ambient temperature and that can be dispersed in OLED layers. Summary of the Invention [Problem to be solved by the invention]

[0009] It is therefore an object of the present invention to provide organic materials that overcome the problems faced in the art. More specifically, it is an object of the present invention to provide single-component compositions that are bulk polymerizable when exposed to suitable actinic radiation under OLED device manufacturing conditions. It is another object of the present invention to provide a stable single-component bulk polymerizable composition that does not exhibit viscosity changes at or below normal storage conditions, e.g., that undergoes bulk polymerization only when exposed to suitable actinic radiation.

[0010] Another object of the present invention is to provide a single component composition that is useful in a variety of other applications such as 3D printing, inkjet coating, encapsulants, etc.

[0011] Further objects and scope of applicability of the present invention will be set forth in the detailed description below. [Means for solving the problem]

[0012] The inventors have found that by adopting a single-component composition, it is possible to manufacture various devices, such as OLED devices having transparent optical layers, having properties that have been difficult to obtain so far, i.e., a refractive index in the range of 1.4 to 1.6 or more, high colorless light transmittance, a film thickness of the filler layer that is usually in the range of 10 to 20 μm but can be adjusted according to the application, compatibility with the OLED stack, especially the cathode layer (the very thin layer at the top of the OLED stack), compatibility with the formulation polymerization on the OLED stack (including fast polymerization time, whether photolysis treatment can be performed under atmospheric manufacturing conditions), adhesion to the OLED stack and glass cover, etc. Furthermore, the composition of the present invention can be expected to have a uniform leveling effect in the entire OLED layer, which generally requires low viscosity. Furthermore, since the composition of the present invention contains a rigid polycycloolefin structure, it is highly likely that the shrinkage rate is very low. When high-speed bulk polymerization is performed with the components disclosed in the present invention, no fugitive small molecules that may damage the OLED stack are left behind. Generally, no other small molecule additives are required to obtain further benefits. The most important fact is that the compositions of the present invention remain stable (i.e., do not change in viscosity) under ambient atmospheric conditions, e.g., exposure to temperatures up to 40° C. for several days, and undergo bulk polymerization only when exposed to suitable actinic radiation. When exposed to suitable actinic radiation, the compositions undergo very rapid vinyl addition bulk polymerization to form a solid object within minutes, e.g., within 1 to 10 minutes, more typically within 1 hour.

[0013] The compositions of the present invention are also compatible with "one drop fill" (ODF). In the typical ODF process, which is often used in the manufacture of top-emitting OLED devices, a special optical fluid is applied to enhance the transmission of light from the device to the top cover glass, which is then dispersed by the ODF process. Although the name ODF may be misleading, in reality, a few drops or strings of material are usually dispersed inside the seal line. After application, the fluid spreads out in a manner similar to die-attach epoxies upon lamination of the top glass. The process is typically performed under vacuum to prevent air from being trapped inside. The present invention provides a low viscosity material that utilizes rapid flow to easily and uniformly coat the substrate in a short time. The present invention also overcomes the disadvantages of the prior art, particularly in that a single component composition is more convenient than adopting a two-component system in the ODF process.

[0014] Thus, the present invention provides a single component composition comprising: a) one or more olefin monomers; b) an organopalladium compound of formula (I) as described below; c) a photoacid generator as described below; and d) a photosensitizer.

[0015] In another aspect of the invention, kits are provided that include compositions of the invention that form three-dimensional objects, such as transparent films. [Brief description of the drawings]

[0016] Embodiments according to the present invention will now be described with reference to the following accompanying drawings and / or images, which depict various embodiments of the invention in a simplified manner and for illustrative purposes only. [Figure 1] FIG. 1 is a graphical depiction of the viscosity change of an embodiment of a composition according to the present invention. [Diagram 2] FIG. 2 is a graphical depiction of the viscosity change of an embodiment of a composition according to the present invention. [Diagram 3] FIG. 3 shows an embodiment of a film of the present invention having a light transmission of 90%. [Figure 4] FIG. 4 illustrates a 3D printed object formed with an embodiment of a composition of the present invention. [Diagram 5] 5A and 5B show optical micrographs of a typical patterned surface of a conventional digital video disc (DVD) taken at different resolutions: 10 μm in FIG. 5A and 20 μm in FIG. 5B. [Figure 6] Figures 6A and 6B show optical micrographs taken at different resolutions of a patterned surface obtained with an embodiment of the composition of the present invention, with Fig. 6A at a magnification of 10 μm and Fig. 6B at a magnification of 20 μm, which is an identical replica of the patterned surface of a DVD having a channel surface periodicity of approximately 760 nm ± 20 nm. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] As used herein, the terms have the following meanings:

[0018] The use of the articles "a," "an," and "the" is deemed to include a plurality of referents unless expressly limited to one referent.

[0019] All numbers, values ​​and / or formulas expressing quantities of ingredients, reaction conditions, and the like in this specification and the claims appended hereto reflect uncertainties of the measurements performed to obtain such numbers, values ​​and / or formulas, and therefore are deemed to include the term "about" unless otherwise indicated.

[0020] When a range of numbers is disclosed herein, the range is considered continuous and includes the maximum and minimum values ​​of the range, as well as all values ​​between the maximum and minimum values. When the range refers to integers, it includes all integers between the maximum and minimum values ​​of the range. Furthermore, when multiple ranges are presented for the purpose of describing a feature or characteristic, the multiple ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein include all subranges that the range encompasses. For example, when a range of "1 to 10" is presented, the range should be considered to include all subranges from the minimum value of 1 to the maximum value of 10. Examples of subranges from 1 to 10 include, but are not limited to, 1 to 6.1, 3.5 to 7.8, 5.5 to 10, etc.

[0021] Symbols used in this specification [ka] indicates the position at which a bond is formed with another repeating unit or with another atom, molecule, group, or moiety, depending on the structure of the group shown.

[0022] "Hydrocarbyl" as used herein refers to a group containing carbon and hydrogen atoms, including, but not limited to, alkyl, cycloalkyl, aryl, aralkyl, alkaryl, alkenyl, and the like. "Halohydrocarbyl" refers to a hydrocarbyl group in which at least one hydrogen has been replaced with a halogen. "Perhalocarbyl" is a hydrocarbyl group in which all hydrogens have been replaced with halogens.

[0023] In this specification, "(C1-C6) alkyl" includes methyl and ethyl groups, as well as linear or branched propyl, butyl, pentyl, and hexyl groups. In particular, alkyl groups refer to methyl, ethyl, n-propyl, isopropyl, tert-butyl, and the like. Derived expressions such as "(C1-C4) alkoxy", "(C1-C4) thioalkyl", "(C1-C4) alkoxy(C1-C4) alkyl", "hydroxy(C1-C4) alkyl", "(C1-C4) alkylcarbonyl", "(C1-C4) alkoxycarbonyl(C1-C4) alkyl", "(C1-C4) alkoxycarbonyl", "diphenyl(C1-C4) alkyl", "phenyl(C1-C4) alkyl", "phenylcarboxy(C1-C4) alkyl", "phenoxy(C1-C4) alkyl", and the like should be construed in the same manner.

[0024] As used herein, "cycloalkyl" includes all known cyclic groups. Representative examples of "cycloalkyl" include, but are not limited to, cyclopropyl, cyclobutyl, cyclopentyl, cyclohexyl, cycloheptyl, cyclooctyl, and the like. Derived expressions such as "cycloalkoxy", "cycloalkylalkyl", "cycloalkylaryl", "cycloalkylcarbonyl", and the like, should be construed in the same manner.

[0025] In this specification, "(C1-C6) perfluoroalkyl" refers to an alkyl group in which all hydrogen atoms are replaced with fluorine atoms. Examples include trifluoromethyl, pentafluoroethyl, linear or branched heptafluoropropyl, nonafluorobutyl, undecafluoropentyl, and tridecafluorohexyl. Derived expressions such as "(C1-C6) perfluoroalkoxy" should be interpreted in the same way. Furthermore, some alkyl groups described in this specification, such as "(C1-C6) alkyl", may be partially fluorinated. That is, derived expressions should be interpreted in the same way, meaning that only a portion of the hydrogen atoms in the alkyl group may be replaced with fluorine atoms.

[0026] In this specification, "(C6-C 10 )aryl" refers to substituted or unsubstituted phenyl or naphthyl. Specific examples of substituted phenyl or substituted naphthyl include o-, p-, m-tolyl, 1,2-, 1,3-, 1,4-silyl, 1-methylnaphthyl, 2-methylnaphthyl, and the like. In addition, "substituted phenyl" or "substituted naphthyl" is considered to include all possible substituents defined herein or known in the art.

[0027] In this specification, "(C6-C 10 "(C1-C4)arylalkyl" means (C6-C 10 ) aryl is linked to (C1-C4) alkyl as defined herein. Representative examples include benzyl, phenylethyl, 2-phenylpropyl, 1-naphthylmethyl, 2-naphthylmethyl, and the like.

[0028] "Halogen" or "halo" means chloro, fluoro, bromo, or iodo.

[0029] In the broadest sense, "substituted" can be construed to include all permissible substituents of organic compounds. In certain embodiments disclosed herein, "substituted" refers to substitution with one or more substituents independently selected from the group consisting of (C1-C6) alkyl, (C2-C6) alkenyl, (C1-C6) perfluoroalkyl, phenyl, hydroxy, -CO2H, ester, amide, (C1-C6) alkoxy, (C1-C6) thioalkyl, and (C1-C6) perfluoroalkoxy. However, other suitable substituents known to those of skill in the art may be used in the embodiments.

[0030] In the text, schemes, examples and tables, when an atom does not satisfy a valence, it is assumed to have the appropriately numbered hydrogen atom which satisfies the valence.

[0031] As used herein, "derived" means that the repeating units of a polymer are polymerized (formed) from polycyclic norbornene type monomers, for example according to formula (I) or (IV), in which case the resulting polymer is formed with a 2,3 double bond of the norbornene type monomer as follows:

[0032] [ka]

[0033] Thus, in accordance with the practice of the present invention, in a single component composition: a) one or more olefin monomers; b) An organopalladium compound of formula (I): [ka] (where: Each A is independently a bidentate monoanionic ligand of formula (II): [ka] n is an integer of 0, 1 or 2; X and Y are each independently selected from O, N, and S; R1, R2, R3, R4, R5, R6, and R7 may be the same or different and may be hydrogen, methyl, ethyl, straight-chain or branched (C3-C 16 ) alkyl, (C1-C 16 ) Perfluoroalkyl, some (C1-C 16 ) Fluoroalkyl, (C3-C 10 )Cycloalkyl, (C6-C 10 )Aryl(C1-C 16 ) alkyl, and substituted or unsubstituted (C6-C 10 )aryl, and when any one of X or Y is O or S, R1 and R5 are each absent; c) a photoacid generator, [ka] (where: a is an integer from 0 to 5; An - is Cl - , Br - , I - , N3 - , BF4 - , tetrakis(pentafluorophenyl)borate, tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, tetrakis(2-fluorophenyl)borate, tetrakis(3-fluorophenyl)borate, tetrakis(4-fluorophenyl)borate, tetrakis(3,5-difluorophenyl)borate, tetrakis(2,3,4,5-tetrafluorophenyl)borate, tetrakis(3,4,5,6-tetrafluorophenyl)borate, tetrakis(3,4,5-trifluorophenyl)borate, methyl tris(perfluorophenyl)borate, ethyl tris(perfluorophenyl)borate, phenyl tris(perfluorophenyl)borate, tetrakis(1,2,2-trifluoroethylenyl)borate, tetrakis(4-tri-1 -propylsilyltetrafluorophenyl)borate, tetrakis(4-dimethyl-tert-butylsilyltetrafluorophenyl)borate, (triphenylsiloxy)tris(pentafluorophenyl)borate, (octyloxy)tris(pentafluorophenyl)borate, tetrakis[3,5-bis[1-methoxy-2,2,2-trifluoro-1-(trifluoromethyl)ethyl]phenyl]borate, tetrakis[3-[1-methoxy-2,2,2-trifluoro-1-(trifluoromethyl)ethyl]-5-(trifluoromethyl)phenyl]borate, and tetrakis[3-[2,2,2-trifluoro-1-(2,2,2-trifluoroethoxy)-1-(trifluoromethyl)-ethyl]-5-(trifluoromethyl)phenyl]borate, PF6 - , SbF6 - , n-C4F9SO3 - , CF3SO3 - , and p-CH3(C6H4)-SO3 - selected from the group consisting of; R8, R9, R10 , R 11 , and R 12 are the same or different and are halogen, methyl, ethyl, linear or branched (C3-C 20 )Alkyl, (C3-C 12 )Cycloalkyl, (C6-C 12 )bicycloalkyl, (C7-C 14 )tricycloalkyl, (C6-C 10 )Aryl, (C6-C 10 )aryl(C1-C3)alkyl, (C1-C 12 )Alkoxy, (C3-C 12 )Cycloalkoxy, (C6-C 12 )bicycloalkoxy, (C7-C 14 )tricycloalkoxy, (C6-C 12 )aryloxy(C1-C3)alkyl, (C6-C 12 )aryloxy, (C6-C 12 )aryloxy(C1-C6)alkyl, (C6-C 12 )thioaryl, (C1-C6)alkanoyl(C6-C 12 )thioaryl, (C1-C6)alkoxy(C6-C 12 ) aroyl(C1-C6) alkyl, and (C6-C 12 )-Thioaryl-(C6-C 12 ) a photoacid generator selected from the group consisting of diaryl sulfonium salts; and d) Photosensitizer The present invention provides a composition comprising:

[0034] Thus, various olefin monomers that undergo vinyl addition polymerization can be employed in the composition of the present invention. The olefin monomers may include, but are not limited to, cycloaliphatic olefins such as ethylene, propylene, butylene, styrene, etc. Other olefin monomers include cyclo-olefins, bicyclo-olefins, etc.

[0035] In one embodiment of the present invention, the olefin monomer suitable for the composition of the present invention is represented by formula (V): [ka] Where: m is an integer of 0, 1 or 2; [ka] is a single or double bond; R 13 , R 14 , R 15 , and R 16 are the same or different and are each independently selected from the group consisting of hydrogen, halogen, a hydrocarbyl group or a halohydrocarbyl group, said hydrocarbyl group or halohydrocarbyl group being methyl, ethyl, straight or branched (C3-C 20 )Alkyl, Perfluoro(C1-C 12 )Alkyl, (C3-C 12 )Cycloalkyl, (C6-C 12 )bicycloalkyl, (C7-C 14 )tricycloalkyl, (C6-C 10 )Aryl, (C6-C 10 )Aryl(C1-C6)alkyl, perfluoro(C6-C 10 )Aryl, Perfluoro(C6-C 10 )aryl(C1-C3)alkyl, methoxy, ethoxy, linear or branched (C3-C 16 )Alkoxy, perfluoro(C1-C 12 )Alkoxy, (C3-C 12 )Cycloalkoxy, (C6-C 12 )bicycloalkoxy, (C7-C 14 )tricycloalkoxy, (C6-C 12 )aryloxy, (C6-C 12 )aryloxy(C1-C6)alkyl, (C6-C 12 )Aryl(C1-C6)alkoxy, perfluoro(C6-C 12 )Aryloxy, Perfluoro(C6-C 12 )aryl(C1-C3)alkoxy, [ka] is selected from Here, Z is O, CO, C(O)O, OC(O), OC(O)O, S, (CR 17 R 18 ) b , O(CR 17 R 18 ) b , (CR 17 R 18 ) b O, C(O)(CR 17 R 18 ) b , (CR 17 R 18 ) b C(O), C(O)O(CR 17 R 18 ) b , (CR 17 R 18 ) b C(O)O, OC(O)(CR 17 R 18 ) b , (CR 17 R 18 ) b O.C. (O), (CR 17 R 18 ) b O.C.O.(O)O, (CR 17 R 18 ) b O C (O) O (CR 17 R 18 ) b , O C (O) O (CR 17 R 18 ) b , S(CR 17 R 18 ) b , (CR 17 R 18 ) b S, (SiR 17 R 18 ) b , O(SiR 17 R 18 ) b , (SiR 17 R 18 ) b O, R 17 and R18 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C3-C 12 ) alkyl, substituted or unsubstituted (C6-C 14 )aryl, methoxy, ethoxy, linear or branched (C3-C6)alkyloxy, (C2-C6)acyl, (C2-C6)acyloxy, and substituted or unsubstituted (C6-C 14 ) aryloxy; and b is an integer from 0 to 12; Aryl is selected from the group consisting of substituted or unsubstituted phenyl, substituted or unsubstituted biphenyl, substituted or unsubstituted naphthyl, substituted or unsubstituted terphenyl, substituted or unsubstituted anthracenyl, substituted or unsubstituted fluorenyl, wherein the substituents are halogen, methyl, ethyl, linear or branched (C3-C6) alkyl, perfluoro(C1-C6) alkyl, ... 12 )Alkyl, (C3-C 12 )Cycloalkyl, (C6-C 10 )Aryl, (C6-C 10 )Aryl(C1-C6)alkyl, perfluoro(C6-C 10 )Aryl, Perfluoro(C6-C 10 )aryl(C1-C3)alkyl, methoxy, ethoxy, linear or branched (C3-C 16 )Alkoxy, perfluoro(C1-C 12 )Alkoxy, (C3-C 12 )Cycloalkoxy, (C6-C 12 )aryloxy, (C6-C 12 )aryloxy(C1-C6)alkyl, (C6-C 12 )Aryl(C1-C6)alkoxy, perfluoro(C6-C 12 )aryloxy, and perfluoro(C6-C 12 ) aryl(C1-C3)alkoxy; k is an integer from 1 to 12; R 23 , R 24 , and R 25are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C3-C 12 )Alkyl, Perfluoro(C1-C 12 ) alkyl, methoxy, ethoxy, linear or branched (C3-C 12 )Alkoxy, (C3-C 12 )Cycloalkyl, (C6-C 12 )bicycloalkyl, (C7-C 14 )tricycloalkyl, (C6-C 10 )Aryl, (C6-C 10 )Aryl(C1-C6)alkyl, perfluoro(C6-C 10 ) aryl, and perfluoro(C6-C 10 )aryl(C1-C3)alkyl; or R 23 and R 24 represents a substituted or unsubstituted (C5-C 14 ) cyclic, (C5-C 14 ) bicyclic, or (C5-C 14 ) tricyclic ring; Arylene is a substituted or unsubstituted divalent (C6-C 14 ) aryl; or Any one of R1 and R2, together with the carbon atom bonded to any one of R3 and R4, may be a substituted or unsubstituted (C5-C 14 ) cyclic, (C5-C 14 ) bicyclic, or (C5-C 14 ) forms a tricyclic ring.

[0036] More specifically, Aryl as defined herein is [ka] and R in each case x is methyl, ethyl, straight or branched (C3-C 12 ) alkyl or (C6-C 10 ) aryl.

[0037] The monomers of formula (V) described herein are either known in the literature or may be prepared by any method known in the art for the preparation of said monomers or monomers of a similar type.

[0038] Furthermore, the monomers described herein can be readily polymerized in bulk through vinyl addition, i.e., when in neat form, without the use of any solvent, using certain transition metal catalysts, such as the organopalladium compounds described herein. See, for example, U.S. Patent Nos. 7,442,800 and 7,759,439, incorporated herein by reference.

[0039] "Bulk polymerization" refers to a concept generally accepted in the art. In other words, it refers to a polymerization reaction that proceeds substantially without a solvent. However, in some cases, a small amount of solvent may be present in the reaction medium. For example, a small amount of solvent can be used to dissolve or carry the organopalladium compound of formula (I) described herein, the photoacid generator or the photosensitizer to the reaction medium. Some solvents can also be used to reduce the viscosity of the monomer. The amount of solvent present in the reaction medium may range from 0 to 5% by weight based on the total weight of the monomer. In the present invention, the type of solvent is not limited as long as it can dissolve the organopalladium compound of formula (I), the photoacid generator or the photosensitizer and / or the monomer. Examples of the solvent include alkanes, cycloalkanes, aromatics such as toluene, ester solvents such as ethyl acetate, THF, dichloromethane, dichloroethane, etc.

[0040] The inventors have found that one or more monomers can be used to dissolve the organopalladium compound of formula (I), the photoacid generator or the photosensitizer, thereby eliminating the need for a solvent. Moreover, one of the monomers can function as a solvent for another monomer, thereby eliminating the need for an additional solvent. For example, if a first monomer of formula (V) is solid at room temperature, a second monomer of formula (V) that is liquid at room temperature can be used as a solvent for the first monomer of formula (V) that is solid, and vice versa. Thus, in the above-mentioned situations, more than one monomer can be employed in the composition of the present invention.

[0041] In one embodiment, it has been found that the monomer of formula (V) functions as a high refractive index material that imparts a high refractive index to the polymer film obtained by carrying out the bulk polymerization. Generally, the monomer of formula (I) suitable for the present invention has a refractive index of at least 1.5. In one embodiment, the refractive index of the monomer of formula (V) is greater than 1.5. In another embodiment, the refractive index of the monomer of formula (V) is in the range of about 1.5 to 1.6. In another embodiment, the refractive index of the monomer of formula (V) is greater than 1.55, greater than 1.6, or greater than 1.65. In another embodiment, it may be greater than 1.7.

[0042] In another embodiment, monomers of formula (V) may generally be contemplated for use as viscosity modifiers, and thus monomers of formula (V) are generally liquid at room temperature and may be used with other monomers of formula (V) that are solids or highly viscous liquids.

[0043] In another embodiment of the present invention, the composition of the present invention comprises at least two different monomers represented by formula (V) and is in a transparent liquid state having a viscosity of less than 100 centipoise. Generally, the composition of the present invention has a low viscosity, which may be less than 100 centipoise. In one embodiment, the composition of the present invention has a viscosity of less than 90 centipoise. In another embodiment, the composition of the present invention has a viscosity in the range of about 10 to 100 centipoise. In another embodiment, the composition of the present invention has a viscosity of less than 80 cP, less than 60 cP, less than 40 cP, or less than 20 cP. In another embodiment, the viscosity may be less than 20 cP.

[0044] When the composition of the present invention includes two monomers, they may be present in any desired amount to obtain the desired effect, including either refractive index modification, viscosity modification, or both, or other desired properties, depending on the intended end use. Thus, the molar ratio of the first monomer of formula (V) to the second monomer of formula (V) may range from 0:100 to 100:0. That is, in a particular application, only one monomer of formula (V) may be used. In other words, the amount of these two monomers is not particularly limited. In one embodiment, the molar ratio of the first monomer of formula (V) to the second monomer of formula (V) may range from 1:99 to 99:1, and in other embodiments, may range from 5:95 to 95:5, and may be 10:90 to 90:10, 20:80 to 80:20, 30:70 to 70:30, 60:40 to 40:60, 50:50, etc.

[0045] Generally, the compositions according to the invention comprise one or more monomers according to formula (V) above, and the embodiments can be tailored for various specific applications by selecting the various embodiments of the composition as described below to provide the embodiments with suitable properties to suit the desired application. Thus, in one embodiment, the compositions of the invention comprise two or more different monomers according to formula (V), which are different from one another. For example, the compositions may comprise three or four different monomers according to formula (V).

[0046] For example, as described above, by appropriately combining different monomers represented by formula (V), it is possible to tailor the composition to have the desired refractive index, viscosity, and optical transparency. In addition, as described below, it may be preferable to include other polymeric or monomeric materials that are compatible and provide favorable optical properties depending on the final application. Thus, the composition of the present invention may further include other highly refractive polymeric materials that can create desired benefits. Examples of such polymers include, but are not limited to, poly(α-methylstyrene), poly(vinyl-toluene), copolymers of α-methylstyrene and vinyl-toluene, and the like.

[0047] According to another discovery of the inventors, the composition of the present invention may further comprise a monomer different from the monomer represented by formula (V). In one embodiment, the composition of the present invention may further comprise one or more monomers selected from the monomer represented by formula (VI) or formula (VII).

[0048] The monomer of formula (VI) is [ka] where: o is an integer from 0 to 2; D is SiR 29 R 30 R 31 ,or [ka] is a group selected from c is an integer from 1 to 10, and one or more CH2 are (C1-C 10 ) alkyl or (C1-C 10 ) optionally substituted with perfluoroalkyl; R 26 , R 27 , and R 28 are the same or different and are each independently selected from hydrogen, halogen, and hydrocarbyl, wherein the hydrocarbyl is methyl, ethyl, linear or branched (C-C 12)Alkyl, (C3-C 12 )Cycloalkyl, (C6-C 12 )bicycloalkyl, (C7-C 14 )tricycloalkyl, (C6-C 10 )Aryl, (C6-C 10 )aryl(C1-C3)alkyl, (C1-C 12 )Alkoxy, (C3-C 12 )Cycloalkoxy, (C6-C 12 )bicycloalkoxy, (C7-C 14 )tricycloalkoxy, (C6-C 10 )aryloxy(C1-C3)alkyl and (C6-C 10 ) aryloxy; and R 29 , R 30 , and R 31 is methyl, ethyl, linear or branched (C3-C9) alkyl, substituted or unsubstituted (C6-C 14 )aryl, methoxy, ethoxy, linear or branched (C3-C9)alkoxy or substituted or unsubstituted (C6-C 14 ) aryloxy.

[0049] In the above aspect of the invention, the inventors have found that the monomer of formula (VI) confers further advantages to the composition. In other words, the monomer of formula (VI) can adjust the refractive index of the composition depending on the application by increasing or decreasing the refractive index depending on the nature of the monomer. Furthermore, the monomer of formula (VI) generally improves adhesion and can be used as an "adhesion modifier". Finally, the monomer of formula (VI) exhibits low viscosity and good solubility for latent catalysts and / or activators, among other advantages.

[0050] The monomer of formula (VII) is [ka] where: Z1 is a substituted or unsubstituted (C1-C 12) alkylene, -(CH2) d O(CH2) e - or -(CH2) d (SiR 38 R 39 )(OSiR 40 R 41 ) f (CH2) e - ( where d, e, and f are each independently an integer from 0 to 6; R 38 , R 39 , R 40 , and R 41 are the same or different and may be methyl, ethyl, straight or branched (C3-C 12 ) Alkyl are each independently selected from , and, An arylene selected from: From the group Selected: [ka] R 32 , R 33 , R 34 , R 35 , R 36 , and R 37 are the same or different, are each independently selected from hydrogen, halogen, and hydrocarbyl, wherein the hydrocarbyl is methyl, ethyl, linear or branched (C 12 )Alkyl, (C3-C 12 )Cycloalkyl, (C6-C 12 )bicycloalkyl, (C7-C 14 )tricycloalkyl, (C6-C 10 )Aryl, (C6-C 10 )aryl(C1-C3)alkyl, (C1-C 12 )Alkoxy, (C3-C 12 )Cycloalkoxy, (C6-C 12 )bicycloalkoxy, (C7-C 14 )tricycloalkoxy, (C6-C 10 )aryloxy(C1-C3)alkyl or (C6-C 10 ) aryloxy.

[0051] The monomer of formula (VII) is a bifunctional monomer, and can exhibit a high refractive index, especially when Z1 is an arylene group. When the monomer of formula (VII) is mixed into the composition of the present invention, the refractive index of the composition generally increases, and crosslinking with other molecules also increases. Therefore, by mixing the monomer of formula (VII) into the composition of the present invention according to the intended use, it is possible to increase the compatibility with other substances and improve the properties of the composition of the present invention.

[0052] In other aspects of the present invention, the composition of the present invention may contain only one monomer of formula (V), formula (VI) or formula (VII). That is, only one of the monomers of formula (V)-(VII) is sufficient to form the composition of the present invention. In other embodiments, the composition of the present invention contains any two of the monomers of formula (V)-(VII) in any preferred ratio. In other embodiments, the composition of the present invention contains any three of the monomers of formula (V)-(VII) in any preferred ratio and in any combination. The present invention encompasses all possible permutations and combinations of the monomers of formula (V)-(VII).

[0053] Therefore, any monomer that falls within the category of monomers represented by formula (V) may be adopted in the composition of the present invention without limitation. Representative examples of monomers of formula (V) are as follows, but are not limited thereto. [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka] [ka]

[0054] Next, we will consider the monomers of formula (VI) that form the composition of the present invention. The composition of the present invention can use any monomer that falls within the scope of the monomers of formula (VI). Examples of such types of monomers can be selected from the group consisting of, but are not limited to, the following materials: [ka] [ka]

[0055] Next, we will consider the monomers of formula (VII) that form the compositions of the present invention. The compositions of the present invention can use any monomer that falls within the scope of the monomers of formula (VII). Examples of such types of monomers can be selected from the group consisting of, but are not limited to, the following materials: [ka] [ka]

[0056] In other embodiments, the compositions of the present invention comprise one or more monomers of formula (V) and at least one monomer of formula (VI).

[0057] In yet another embodiment, the composition of the present invention comprises one or more monomers of formula (VI) and at least one monomer of formula (VII), and optionally further comprises one monomer of formula (V).

[0058] In yet another embodiment, the composition of the present invention comprises at least one monomer of formula (V) and at least one monomer of formula (VI), and optionally further comprises one monomer of formula (VII).

[0059] In yet another embodiment, the composition of the present invention comprises one monomer of formula (VI), and optionally further comprises one or more monomers of formula (V) or formula (VII).

[0060] In other embodiments of the present invention, the composition comprises any organopalladium compound according to formula (I) that undergoes bulk polymerization as described herein. In general, suitable organopalladium compounds of formula (I) comprise a bidentate monoanionic ligand selected from the group consisting of the following materials: [ka] [ka]

[0061] The organopalladium compounds of formula (I) suitable for use in the compositions of the present invention are known in the literature or can be readily prepared by any method known in the art, see, for example, U.S. Patent Nos. 7,442,800 and 7,759,439, which are incorporated herein by reference.

[0062] Illustrative, but non-limiting, examples of organopalladium compounds of formula (I) that may be employed in the compositions of the present invention are as follows: [ka] [ka] [ka]

[0063] The compositions of the present invention further comprise a photoacid generator which, when combined with an organopalladium compound of formula (I) and a photosensitizer and exposed to suitable radiation as described herein, induces bulk polymerization of the included monomers. Well-known photoacid generators can be used in the compositions of the present invention, such as certain halonium salts.

[0064] In one embodiment, the composition of the present invention includes a compound represented by the following formula (IV a ) photoacid generator is used. [ka]

[0065] wherein Aryl1 and Aryl2 are the same or different and independently selected from the group consisting of substituted or unsubstituted phenyl, biphenyl, and naphthyl; Hal is iodine or bromine; An - is a weakly coordinating anion (WCA) weakly coordinated to the cation complex. More specifically, the WCA anion functions as a stabilizing anion for the cation complex. The WCA anion is non-oxidizing, non-reducing, and non-nucleophilic, and is therefore relatively inert. In general, the WCA can be selected from borate, phosphate, arsenate, antimonate, aluminate, borate benzene anion, carborane, halocarborane anion, sulfonamidate, and sulfonate.

[0066] Formula (IV a Representative examples of the compound represented by the formula (I) are as follows: [ka]

[0067] Here, R 11 and R 12is as defined herein. Similarly, a variety of sulfonium salts can be used as photoacid generators, broadly including compounds of formula (III) as described herein.

[0068] Accordingly, examples of photoacid generators of formula (III) that may be employed in the compositions of the present invention include, but are not limited to, the following: [ka] [ka] [ka]

[0069] Examples of suitable photoacid generators having formula (IV) that can be used in the compositions of the present invention include, but are not limited to, the following: [ka] [ka] [ka]

[0070] Other examples of PAGs suitable for use in the compositions of the present invention include the following: [ka] [ka]

[0071] However, other known photoacid generators may also be used in the compositions of the present invention, provided that they are capable of activating the organopalladium compounds of formula (I) used in the present application when exposed to suitable radiation, and the present invention encompasses all such compounds.

[0072] The composition of the present invention further comprises a photosensitizer compound that further promotes the formation of an active catalyst when the composition is exposed to suitable radiation in the presence of the photoacid generator used in the present application. For that purpose, a suitable sensitizer compound that activates the photoacid generator and / or the organopalladium compound of formula (I) can be adopted in the composition of the present invention. Examples of suitable sensitizer compounds include anthracene, phenanthrene, chrysene, benzopyrene, fluoranthene, rubrene, pyrene, xanthone, indanthrene, thioxanthen-9-one, and mixtures thereof. In an exemplary embodiment, the suitable sensitizer component comprises a compound of formula (VIII) or a compound of formula (IX): [ka] Where: R 44 , R 45 , and R 46 are the same or different and are hydrogen, halogen, hydroxy, NO2, NH2, methyl, ethyl, linear or branched (C3-C 12 )Alkyl, (C3-C 12 )Cycloalkyl, (C6-C 12 )bicycloalkyl, (C7-C 14 )tricycloalkyl, (C6-C 10 )Aryl, (C6-C 10 )aryl(C1-C3)alkyl, (C1-C 12 )Alkoxy, (C3-C 12 )Cycloalkoxy, (C6-C 12 )bicycloalkoxy, (C7-C 14 )tricycloalkoxy, (C6-C 10 )aryloxy(C1-C3)alkyl, (C6-C 10 )aryloxy, C(O)(C1-C6)alkyl, COOH, C(O)O(C1-C6)alkyl, SO2(C6-C 10 ) aryl; R 47 and R 48 are the same or different and may be methyl, ethyl, straight or branched (C3-C12 )Alkyl, (C3-C 12 )Cycloalkyl, (C6-C 12 )bicycloalkyl, (C7-C 14 )tricycloalkyl, (C6-C 10 ) aryl, and (C6-C 10 )aryl(C1-C3)alkyl.

[0073] Representative examples of compounds of formula (VIII) or compounds of formula (IX) are as follows, but are not limited thereto. [ka] [ka] [ka]

[0074] Other suitable photosensitizer compounds include substituted or unsubstituted phenothiazine derivatives, such as: [ka]

[0075] Generally, a photosensitizer absorbs energy emitted from a light source and transfers the energy to a desired substrate / reactant. In the present invention, the photoacid generator employed in the composition of the present invention corresponds to the substrate / reactant. In one embodiment, the compound of formula (III) or the compound of formula (IV) can be activated by a specific wavelength of electromagnetic radiation, generally ranging from about 240 nm to 410 nm. Therefore, any compound activated by electromagnetic radiation can be utilized as a stable composition in various processes in which the composition of the present invention can be employed, such as OLED or 3D processes. In one embodiment, the wavelength of radiation for activating the compound of formula (III) or (IV) is 260 nm. In another embodiment, the wavelength of radiation for activating the compound of formula (V) is 310 nm. In another embodiment, the wavelength of radiation for activating the compound of formula (V) is 365 nm. In another embodiment, the wavelength of radiation for activating the compound of formula (V) is 395 nm.

[0076] As long as the composition of the present invention can obtain the desired results, there is no particular limitation on the content of the organopalladium compound of formula (I), the photoacid generator of formula (III) or (IV), and the photosensitizer of formula (VIII) or (IX). In general, the molar ratio of the monomer of formula (V) to the compound of formula (I) is in the range of 25,000:1 to 5,000:1 or less. In one embodiment, the molar ratio of the monomer of formula (V) to the compound of formula (I) is 10,000:1, 15,000:1:1, 20,000:1:1, or 30,000:1 or more. The monomer of formula (V) described herein may include one or more different monomers represented by formula (V) and may further include one or more monomers of formula (VI) or (VII). Thus, the above molar ratio indicates the molar amount of the total monomers selected. Similarly, the molar ratio of the organopalladium compound of formula (I), the photoacid generator of formula (III) or (IV), and the photosensitizer of formula (VIII) or (IX) may be in the range of 1:1:0.5 to 1:2:2, 1:2:1, 1:4:1, 1:2:4, 1:1:2, or 1:4:2, or may be outside the range as long as the desired results are obtained.

[0077] The inventors have found that the composition according to the present invention forms a substantially transparent film when exposed to suitable actinic radiation (UV radiation). In other words, when the composition of the present invention is exposed to a specific actinic radiation, the monomer undergoes bulk polymerization to form a film that is substantially transparent to visible light. That is, most of the visible light is transmitted through the film. In one embodiment, the film formed from the composition of the present invention has a visible light transmittance of 90% or more. In another embodiment, the film formed from the composition of the present invention has a visible light transmittance of 95% or more. Any actinic radiation suitable for carrying out the bulk polymerization can be adopted in the present invention without any particular restrictions, and for example, exposure is performed with actinic radiation having a wavelength of 200 nm to 400 nm. The wavelength may be greater than 400 nm. The wavelength of the actinic radiation adopted in one embodiment is 250 nm, 295 nm, 360 nm, 395 nm, or greater than 400 nm.

[0078] In another embodiment, the compositions of the present invention undergo bulk polymerization to form a substantially transparent film when exposed to suitable actinic radiation and heated. In another embodiment, the compositions of the present invention undergo bulk polymerization to form a substantially transparent film when exposed to suitable UV radiation at a temperature between 50° C. and 100° C.

[0079] Thus, illustrative but non-limiting examples of compositions of the present invention are as follows: 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate)2, triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate)2, triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, triylcumyl iodonium-tetrakis pentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, (4-(octyloxy)phenyl)(phenyl)iodonium hexafluorophosphate (OPPI-PF6), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, (4-(octyloxy)phenyl)(phenyl)iodonium hexafluoroantimonate (OPPI-SbF6), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate)2, triylcumyl iodonium-tetrakis pentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate)2, triylcumyl iodonium tetrakis pentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, triylcumyl iodonium tetrakis pentafluorophenylborate (Rhodorsil 2074), and 2-chloro-9H-thioxanthen-9-one (CTX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(acetylacetonate)2, triylcumyl iodonium-tetrakis pentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(tetramethylheptenoate)2, tolylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, (2-(4-methoxynaphthalen-1-yl)-2-oxoethyl)dimethylsulfonium tetrakis-pentafluorophenylborate (TAG 382), and 9,10-diethoxyanthracene (DEA); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, tris(4-((4-acetylphenyl)thio)phenyl)sulfonium tetrakis-pentafluorophenylborate (Irgacure PAG 290), and 9,10-diethoxyanthracene (DEA); 5-Phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate)2, iodonium, diphenyl-4,4'-di-(C 10 -C 13) alkyl derivatives, tetrakis(2,3,4,5,6-pentafluorophenyl)borate (SILCOLEASE UV CATA 243), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-Hexadecylbicyclo[2.2.1]hept-2-ene (HexaDecNB), palladium(hexafluoroacetylacetonate)2, iodonium, diphenyl-4,4'-di-(C 10 -C 13 ) alkyl derivatives, tetrakis(2,3,4,5,6-pentafluorophenyl)borate (SILCOLEASE UV CATA 243), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-Phenylbicyclo[2.2.1]hept-2-ene (PhNB), palladium(hexafluoroacetylacetonate)2, iodonium, diphenyl-4,4'-di-(C 10 -C 13 ) alkyl derivatives, tetrakis(2,3,4,5,6-pentafluorophenyl)borate (SILCOLEASE UV CATA 243), and 2-isopropyl-9H-thioxanthen-9-one (ITX); and 5-Decylbicyclo[2.2.1]hept-2-ene (DecNB), 5-(2-([1,1'-biphenyl]-2-yloxy)methyl)bicyclo[2.2.1]hept-2-ene (NBMeOPhPh), palladium(hexafluoroacetylacetonate)2, iodonium, diphenyl-4,4'-di-(C 10 -C 13 ) alkyl derivatives, tetrakis(2,3,4,5,6-pentafluorophenyl)borate (SILCOLEASE UV CATA 243), and 2-isopropyl-9H-thioxanthen-9-one (ITX).

[0080] In another aspect of the present invention, the present invention provides a kit for forming a substantially transparent film. The composition of the present invention is dispersed within the kit. Thus, in one embodiment, a kit is provided having dispersed therein one or more olefin monomers, an organopalladium compound of formula (I) as described herein, a photoacid generator of formula (III) or (IV) as described herein, and a photosensitizer of formula (VIII) or (IX). In one embodiment, the kit of the present invention may include one or more monomers of formula (V) together with one or more monomers of formula (VI) or (VII) as necessary to obtain a desired result or to suit the application.

[0081] In one embodiment, the kit includes one or more monomers of formula (V) and one or more monomers of formula (VI) or formula (VII) described herein. In another embodiment, the kit includes at least two monomers, the first monomer serving as a solvent for the second monomer. Any of the monomers of formulas (V)-(VII) described herein can be used in this embodiment. The molar ratio of the two monomers included in this embodiment is not fixed and may be 1:99-99:1, 10:90-90:10, 20:80-80:20, 30:70-70:30, 60:40-40:60, 50:50, or any other range. In another embodiment, the kit includes a composition in which two monomers are dispersed, the monomer of formula (V) and the other monomer of formula (VI). The monomer of formula (VI) is completely dissolved in the monomer of formula (V) to form a clear solution at room temperature. In one embodiment, the mixture of monomers is a clear solution at a slightly elevated temperature, e.g., 30°C, 40°C, or 50°C, prior to bulk polymerization. In another aspect of the present embodiment, the kit of the present invention, when exposed to suitable radiation for a sufficient period of time, undergoes bulk polymerization to form a polymer film. In other words, when the composition of the present invention is poured onto a substrate or surface that must be encapsulated and exposed to suitable actinic radiation, the monomers undergo polymerization to form a solid, clear polymer in the form of a clear film. As mentioned above, polymerization generally occurs with actinic radiation of various wavelengths, exemplary wavelengths being 265 nm, 315 nm, 365 nm, 395 nm, and the like. The bulk polymerization can be further accelerated by heating, which can be carried out in stages. For example, heating to 40°C, 50°C, or 60°C for 5 minutes, followed by further heating to 70°C for various periods of time, e.g., 5 to 15 minutes, as required. By carrying out the present invention, a polymer film can be formed on the substrate, which is a substantially transparent film. As used herein, the term "substantially transparent film" means that the film formed from the composition of the present invention is optically transparent to visible light.Thus, in one embodiment of the invention, the film has a visible light transmission of at least 90%, and in another embodiment, films formed from the compositions of the invention have a visible light transmission of at least 95%.

[0082] In one embodiment of the present invention, the kit described herein includes a composition further comprising one or more monomers selected from the monomers of formula (III) or (IV) described above. Any monomer of formula (III) or (IV) as described herein may be used in this embodiment without limitation, and the content may be varied depending on the desired application.

[0083] In one embodiment, the kits described herein include all of the exemplary compositions described above.

[0084] In another aspect, the present invention provides a method for forming a substantially transparent film for use in the manufacture of optoelectronic devices, comprising forming a homogeneous, transparent composition comprising one or more monomers of formula (V), an organopalladium compound of formula (I), a photoacid generator of formula (III) or (IV), and a photosensitizer of formula (VIII) or (IX), coating or pouring the composition onto a suitable substrate to form a film, and exposing the film to suitable actinic radiation to initiate polymerization of the monomers.

[0085] In the process of coating the desired substrate with the composition of the present invention to produce a film, the coating can be performed by a coating method described herein or known to those skilled in the art, such as spin coating. Other suitable coating methods include, but are not limited to, spray coating, doctor blading, meniscus coating, inkjet coating, and slot coating. The mixture can also be poured onto the substrate to form a film. There is no particular limitation as long as the substrate is suitable, and it may be a substrate used in electrical, electronic, or optoelectronic devices, such as a semiconductor substrate, a ceramic substrate, or a glass substrate.

[0086] Next, the coated substrate is baked. In other words, the substrate is heated, for example, at a temperature of 50°C to 100°C for about 1 to 60 minutes to promote bulk polymerization. Any suitable heating temperature and heating time other than those exemplified may be applied. In one embodiment, the substrate is baked at a temperature of about 60°C to about 90°C for 2 to 10 minutes. In another embodiment, the substrate is baked at a temperature of about 60°C to about 90°C for 5 to 20 minutes.

[0087] The optical properties of the formed films are evaluated by various methods known in the art. For example, the refractive index of the film in the visible spectrum can be measured by ellipsometry. The optical quality of the film is determined by visual observation. The transmittance can be quantitatively measured by visible spectroscopy. The films formed according to the present invention generally exhibit excellent optical transmittance and can be tailored to have a desired refractive index as described herein.

[0088] Thus, in one embodiment of the present invention, the present invention provides an optically transparent film obtained by bulk polymerization of the compositions described herein. In another embodiment, the present invention provides an optoelectronic device comprising the inventive transparent film described herein.

[0089] In another embodiment of the present invention, the composition of the present invention can be employed in various photoinduced nanoimprint lithography (NIL), such as UV-NIL. For example, the composition of the present invention can be used in various photocurable imprint techniques. In general, the composition of the present invention is conformally placed on a substrate (by coating or similar means), then covered with a suitable stamp and exposed to radiation to cure the composition of the present invention until it becomes solid. The stamp is then removed to obtain a nanoimprint film. The substrate can be a master digital video disc (DVD).

[0090] The following examples provide detailed descriptions of the preparation and use of specific compounds / monomers, polymers, and compositions of the present invention. The detailed preparation methods fall within and are exemplary of the general preparation methods described above. The examples are for illustrative purposes only and are not intended to be limiting of the present invention. In the examples and herein, the ratios of monomer to catalyst are molar ratios.

[0091] Working Example The following abbreviations are used herein to describe some of the compounds, devices and / or methods employed to illustrate certain embodiments of the present invention.

[0092] NBEtCl: 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene NBEtOPhPh: 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene NBMeOPhPh: 5-(2-([1,1'-biphenyl]-2-yloxy)methyl)bicyclo[2.2.1]hept-2-ene PENB: 5-phenethylbicyclo[2.2.1]hept-2-ene PhNB: 5-phenylbicyclo[2.2.1]hept-2-ene DecNB: 5-decylbicyclo[2.2.1]hept-2-ene HexaDecNB: 5-Hexadecylbicyclo[2.2.1]hept-2-ene TD: Tetracyclododecene Pd304: Palladium(acetylacetonate)2 Pd520: Palladium(hexafluoroacetylacetonate)2 Pd428: Palladium(1-phenylbutane-1,3-dionate)2 Pd473: Palladium(tetramethylheptenoate)2 Pd498: Palladium(2-((phenylimino)methyl)phenoate)2 Pd620: Palladium (1,1,1,5,5,6,6,6-octafluorohexane-2,4-dionate)2 Pd920: Palladium (1,1,1,2,2,3,3,7,7,8,8,9,9,9-tetradecafluorononane-4,6-dionate)2 Rhodorsil 2074: Triylcumyl iodonium tetrakis pentafluorophenylborate OPPI-SbF6: [4-(octyloxy)phenyl]phenyliodonium hexafluoroantimonate OPPI-PF6: [4-(octyloxy)phenyl]phenyliodonium hexafluorophosphate Irgacure PAG 290: Tris(4-(4-acetylphenylthio)phenyl)sulfonium tetrakis(pentafluorophenyl)borate TAG 382: (2-(4-Methoxynaphthalen-1-yl)-2-oxoethyl)dimethylsulfonium tetrakis(pentafluorophenyl)borate UV CATA 243: Iodonium, 4,4'-di-(C 10 -C 13 ) alkyl derivatives, tetrakis(2,3,4,5,6-pentafluorophenyl)borate ITX: 4-isopropylthioxanthone CTX: 2-chlorothioxanthone DEA: 9,10-diethoxyanthracene GPC: Gel Permeation Chromatography M w:Weight average molecular weight PDI: Polydispersity Index cP: Centipoise DSC: Differential scanning calorimeter TGA: Thermogravimetric analysis UV-NIL: Ultraviolet nanoimprint lithography

[0093] A variety of organopalladium compounds of formula (I) are commercially available or known in the literature and can be readily prepared by procedures described in the literature. Examples A-D illustrate the preparation of some of the organopalladium compounds of formula (I).

[0094] Example A Synthesis of Pd428 To a brown suspension of Pd(II) chloride (0.4 g, 2.26 mmol) in methanol (11.3 mL) was added sodium chloride (0.132 g, 2.26 mmol). The mixture was stirred overnight at ambient temperature, then filtered and diluted with 11.3 mL of methanol. To the resulting brown solution (5.6 mL) was added 1-benzoylacetone (0.235 g, 1.41 mmol) and sodium carbonate (0.051 g, 0.479 mmol). A yellow precipitate formed immediately. The solution was stirred overnight at ambient temperature and the solid was collected by filtration. To the yellow solid was added 5 mL of dichloromethane. The solution was filtered and concentrated in vacuo to give a yellow solid. The yield was 0.178 g. 1 H NMR (CD2Cl2, 500 MHz): δ 2.07 (s, 6H), 5.91 (s, 2H), 7.23 (d, 4H), 7.30 (m, 2H), 7.70 (d, 4H).

[0095] Example B Synthesis of Pd498 To a brown suspension of Pd(II) acetate (0.2 g, 0.89 mmol) in ethanol (5 mL) was added a solution of N-salicylideneaniline (0.351 g, 1.78 mmol) in ethanol (5 mL). The solution was refluxed for 3 h and the tan solid that formed was collected by filtration and washed three times with 5 mL of ethanol. Toluene (10 mL) was added to the resulting solid and stirred for 1 h. The solution was filtered and the solvent removed in vacuo to yield an orange solid. The yield was 0.32 g. 1 H NMR (C6D6, 500 MHz): δ 6.36 (t, 2H), 6.48(d, 2H), 6.74 (d, 2H), 6.99 (t, 1H), 7.08 (m, 10H), 7.22 (s, 2H).

[0096] Example C Synthesis of Pd620 To a brown suspension of Pd(II) chloride (0.085 g, 0.48 mmol) in methanol (2.8 mL) was added sodium chloride (0.028 g, 0.48 mmol). The mixture was stirred at 50 °C for 2 h, the reaction mixture was filtered and diluted with 2.8 mL of methanol. To the brown solution (5.6 mL) was added 1,1,1,5,5,6,6,6-octafluoro-2,4-hexanedione (0.51 g, 1.2 mmol) and sodium carbonate (0.051 g, 0.479 mmol). The solution was stirred overnight at ambient temperature and concentrated in vacuum. To the orange solid was added 5 mL of n-hexane and stirred for 1 h. The solution was filtered and the solvent removed in vacuum to give an orange solid. The yield was 0.338 g. 1 H NMR (CD2Cl2, 500 MHz): δ 6.43 (s, 2H). 19 F NMR (CD2Cl2, 470 MHz): δ -126.6, -118.0, -80.9.

[0097] Example D Synthesis of Pd920 To a brown suspension of Pd(II) chloride (0.1 g, 0.56 mmol) in methanol (2.8 mL) was added sodium chloride (0.033 g, 0.56 mmol). The mixture was stirred at 50 °C for 2 h, the reaction mixture was filtered and diluted with 2.8 mL of methanol. To the brown solution (5.6 mL) was added 1,1,1,2,2,3,3,7,7,8,8,9,9,9-tetradecafluoro-4,6-nonadione (0.364 g, 1.41 mmol) and sodium carbonate (0.06 g, 0.56 mmol). The solution was stirred overnight at ambient temperature and the solvent was removed in vacuum. To the orange solid was added 5 mL of n-hexane and stirred for 1 h. The solution was filtered and the solvent was concentrated in vacuum to give an orange solid. The yield was 0.182 g. 1 H NMR (CD2Cl2, 500 MHz): δ 6.41 (s, 2H). 19 F NMR (CD2Cl2, 470 MHz): δ -120.3, -82.7, -73.6.

[0098] The various monomers utilized in the present invention are commercially available or can be readily prepared according to the procedures described in co-pending US Pat. No. 9,944,818.

[0099] The following Examples 1-5 demonstrate that the compositions of the present invention remain stable at room temperature for at least up to 3 days and readily undergo bulk polymerization upon exposure to UV radiation. Additionally, Examples 2-5 demonstrate that bulk polymerization occurs upon exposure to radiation only in the presence of an organopalladium compound of formula (I), a photoacid generator of formula (III), and a photosensitizer of formula (V).

[0100] Example 1 Bulk polymerization of NBEtCl / PENB (5 / 95 molar ratio) In a glass bottle, Pd304 (1 molar part), Rhodorsil 2074 (2 molar parts), and CTX (1 molar part) were dissolved in NBEtCl (250 molar parts) and PENB (4750 molar parts) was added to form a clear solution. The solution was purged with N2 overnight. The solution was exposed to UV light (1 J / cm2) at room temperature for 4 seconds. 2, 395 nm). The solution turned solid within 1 min, suggesting polymerization of the monomer, which was later confirmed by TGA. The solid residue obtained by isothermal TGA (100 °C for 1 h) indicated >99% conversion. Dynamic TGA (20 °C / min) showed >99% conversion. d5 (5% wt. loss) was 340.2° C., with 97% remaining at 300° C. The unexposed solution remained free-flowing after 3 days at room temperature.

[0101] Examples 2 to 5 Bulk polymerization of PENB / NBEtCl (90 / 10 molar ratio) The process of Example 1 was repeated for Examples 2-5, except that Example 2 contained PENB / NBEtCl in a 90:10 molar ratio. As summarized in Table 1, Example 3 did not use a photosensitizer, Example 4 did not use a photoacid generator, and Example 5 did not use an organopalladium compound. All compositions were dispensed in glass bottles and exposed to UV light for 4 seconds at room temperature (1 J / cm 2 , 395 nm). According to the results summarized in Table 1, only the composition of Example 2 was converted to a hard solid in 1 minute, indicating that the monomers were polymerized. This result clearly indicates that all three components of the composition of the present invention are necessary for the bulk polymerization of the olefin monomers of the present invention.

[0102] [Table 1]

[0103] Examples 6-8 demonstrate that various molar ratios of photosensitizers can be used in the bulk polymerization of olefin monomers of the present invention.

[0104] Examples 6 to 8 Various ratios of ITX The process of Example 1 was repeated for Examples 6-8, except that the amount of ITX used was varied as summarized in Table 2. For Examples 6-8, Pd304 (1 molar part), Rhodorsil 2074 (2 molar parts), and various amounts of ITX (0.5, 2, and 8 molar parts, respectively) were dissolved in NBEtCl (250 molar parts) and PENB (4750 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight and the solution was exposed to UV light (1 J / cm) at room temperature for 4 seconds. 2 , 395 nm). All of the solutions in Examples 6 to 8 turned solid within 1 minute, suggesting that the monomers were polymerized, and this was confirmed by TGA, as summarized in Table 2. As is evident from the UV-DSC data in Table 2, the composition of Example 6, which contained 0.5 molar parts of ITX, showed almost similar reactivity to Example 7, which contained 2 molar parts of ITX. The example containing 8 molar parts of ITX showed a slight decrease in polymerization rate. Thus, it can be seen that a smaller amount of photosensitizer efficiently induces bulk polymerization of the composition of the present invention. This is made clearer by the percentage of solid residue remaining after bulk polymerization measured by isothermal TGA (100°C for 1 hour), where the percentage of solid residue remaining was slightly higher for the composition containing 0.5 molar parts of ITX than for the composition containing 2 molar parts of ITX and the composition containing 8 molar parts of ITX.

[0105] [Table 2]

[0106] Example 9 Bulk polymerization of PENB / NBEtCl and Pd520 (95 / 5 molar ratio) The process of Example 1 was repeated for Example 9, except that Pd520 was used instead of Pd304. In a glass bottle, Pd520 (1 molar part), Rhodorsil 2074 (2 molar parts), CTX (1 molar part) were dissolved in NBEtCl (250 molar parts) and mixed with PENB (4750 molar parts) to form a clear solution. The solution was purged with dry N2 overnight and exposed to UV light (1 J / cm2) at room temperature for 4 seconds. 2, 395 nm). The solution turned solid within 1 min, suggesting polymerization of the monomer, which was later confirmed by TGA. After UV exposure, the survival rate of the solid residue obtained by isothermal TGA (100 °C for 1 h) was >99%. Dynamic TGA (20 °C / min) showed that the T d5 (5% wt. loss) was 339.4° C., with 97% remaining at 300° C. The unexposed solution remained free-flowing after 3 days at room temperature.

[0107] Example 10 Bulk polymerization of PENB / NBEtOPhPh (90 / 10 molar ratio) Pd520 (1 molar part), Rhodorsil 2074 (4 molar parts), and ITX (1 molar part) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle, and PENB (4500 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight and exposed to UV light (1 J / cm2) at room temperature for 4 seconds. 2 , 395 nm). The solution turned solid within 1 min, suggesting that the monomer had polymerized, which was later confirmed by UV-DSC, TGA, and GC / MS. The results confirmed by UV-DSC showed that the monomer had polymerized after 4 s exposure to UV light (1 J / cm 2 After UV exposure, the solid residue showed a sharp exothermic peak (395 nm) and continued to release heat even after UV exposure. After UV exposure, the solid residue was found to remain >99% in isothermal TGA (100 °C for 1 h). d5 (5% wt. loss) at 267°C, with 93% remaining at 300°C. After UV exposure, <2% unreacted monomer remained by GC / MS. The unexposed solution remained free-flowing after 14 days at room temperature.

[0108] Example 11 Bulk polymerization of DecNB / NBEtOPhPh (90 / 10 molar ratio) Pd520 (1 molar part), Rhodorsil 2074 (1 molar part), ITX (0.5 molar parts) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle and DecNB (4500 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight and exposed to UV light for 4 seconds at room temperature (1 J / cm2). 2, 395 nm). The solution turned solid within a few minutes, suggesting that the monomer had polymerized, which was later confirmed by DSC, TGA, and GC / MS. The results were confirmed by UV-DSC, and the resulting solid was exposed to UV light for 4 seconds (1 J / cm 2 After UV exposure, the solid residue was found to be >99% by isothermal TGA (100°C for 1 h). d5 (5% wt. loss) at 332°C, with 97% remaining at 300°C. After UV exposure, <1% unreacted monomer remained by GC / MS. The unexposed solution remained free-flowing after 14 days at room temperature.

[0109] Example 12 Bulk polymerization of PENB / DecNB / NBEtOPhPh (45 / 45 / 10 molar ratio) Pd520 (1 molar part), Rhodorsil 2074 (2 molar parts), and ITX (1 molar part) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle, and a mixture of PENB (2250 molar parts) and DecNB (2250 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight and exposed to UV light (1 J / cm2) at room temperature for 4 seconds. 2 , 395 nm). The solution turned to a solid within 1 min, suggesting polymerization of the monomer, which was later confirmed by DSC, TGA, and GC / MS. After UV exposure, the survival rate of the solid residue obtained by isothermal TGA (100 °C for 1 h) was >99%. Dynamic TGA (20 °C / min) showed that T d5 (5% wt. loss) at 347°C, with 97% remaining at 300°C. After UV exposure, <1% unreacted monomer remained by GC / MS. The unexposed solution remained free-flowing after 14 days at room temperature.

[0110] Examples 13 and 14 below demonstrate the shelf-life stability of the compositions of the present invention at ambient and subambient conditions (5° C.), confirming that the compositions of the present invention remain stable at ambient or subambient temperatures and can be stored under the same conditions for several days.

[0111] Example 13 Shelf life study of PENB / DecNB / NBEtOPhPh (45 / 45 / 10 molar ratio) Pd520 (1 molar part), Rhodorsil 2074 (2 molar parts), and ITX (1 molar part) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle, and a mixture of PENB (2250 molar parts) and DecNB (2250 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight. The viscosity of the solution was measured at regular intervals and summarized in Table 3 and shown graphically in Figure 1. As shown in Figure 1, the viscosity remained relatively constant (less than 10% change) over 4 days, remained free-flowing after 2 weeks at room temperature, and began to gel after 15 days (Figure 1, Table 3).

[0112] [Table 3]

[0113] Example 14 Shelf life study of PENB / DecNB / NBEtOPhPh (40 / 40 / 20 molar ratio) In a glass bottle, Pd520 (1 molar part), Rhodorsil 2074 (4 molar parts), and ITX (1 molar part) were dissolved in NBEtOPhPh (1000 molar parts) and a mixture of PENB (2000 molar parts) and DecNB (2000 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight. The solution was divided into two portions, one stored at room temperature (RT) and the other at 5°C. The viscosity of the solution was measured at regular intervals and summarized in Table 4 and shown graphically in Figure 2. As shown in Figure 2, the viscosity remained almost unchanged over four days and remained free-flowing even after two weeks at room temperature (Figure 2, Table 4). The reactivity of the solution was measured by UV-DSC. As confirmed by UV-DSC, the reactivity remained almost the same after one week of storage at room temperature. However, the reactivity decreased after two weeks of storage at room temperature as confirmed by the enthalpy change by US-DCV. On the other hand, the solution stored at 5°C maintained its reactivity after one month as determined by UV-DSC, with almost no difference in reactivity to the fresh solution. The samples after UV-DSC exposure were examined by isothermal TGA (100°C for 1 hour), which showed a very high conversion rate (>98%). Table 4 summarizes the viscosity and enthalpy changes under various storage conditions.

[0114] [Table 4]

[0115] Examples 15-16 N 2 and bulk polymerization of DecNB / NBEtOPhPh (90 / 10 molar ratio) under air. Separately, two glass vials were prepared and Pd520 (1 molar part), Rhodorsil 2074 (1 molar part), and ITX (0.5 molar parts) were dissolved in a mixture of DecNB / NBEtOPhPh (5000 molar parts, 90 / 10 molar ratio) to form a clear solution. The solution of Example 15 was purged with dry N2 overnight, while the solution of Example 16 was not purged with dry N2 overnight. Both the solutions of Examples 15 and 16 were exposed to UV light for 4 seconds (1 J / cm2). 2, 395 nm). Both converted to hard solids within minutes, suggesting that the compositions have equivalent reactivity in N2 and air environments. In Examples 15 and 16, the solids remaining after UV exposure were ~99% as determined by isothermal TGA (100 °C for 1 h), indicating high conversion. The data are summarized in Table 5.

[0116] [Table 5]

[0117] Examples 17 to 18 N 2 and bulk polymerization of PENB / DecNB / NBEtOPhPh (40 / 40 / 20 molar ratio) under air. The process of Examples 15 and 16 was repeated for Examples 17 and 18, except that a mixture of PENB / DecNB / NBEtOPhPh monomers (5000 molar parts, 40 / 40 / 20 molar ratio), Pd520 (1 molar part), Rhodorsil 2074 (4 molar parts), and ITX (1 molar part) were used. The clear solution was purged with dry nitrogen or air and then applied to a glass slide with a doctor blade applicator to produce a uniform thin film with a thickness of 50-100 μm. The film was exposed to UV light (1 J / cm) for 4 seconds in air at room temperature. 2 , 395 nm). After a few minutes a solid film formed which was peeled off from the glass slide. After heating at 100° C. for 1 hour, the percent conversion was determined by TGA to determine the presence of solid residue. Both Examples 17 and 18 had high percent solid residue remaining (>98%), suggesting high conversion and therefore that the formulations were air insensitive. The TGA data are summarized in Table 6.

[0118] [Table 6]

[0119] Examples 19-21 below demonstrate the use of the compositions of the present invention in a variety of applications, including, but not limited to, optically transparent coating films, 3D printing, and UV nanoimprint lithography.

[0120] Example 19 Optical Coatings and Transparent Thin Film Applications Pd520 (1 molar part), Rhodorsil 2074 (2 molar parts), and ITX (1 molar part) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle, and PENB (4500 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight, then applied to a glass slide with a spacer or doctor blade applicator to produce a uniform thin film with a thickness of 20-100 μm and exposed to UV light at room temperature for 4 seconds (1 J / cm). 2 After a few minutes, a transparent film was formed and peeled off from the glass slide (Figure 3). UV-vis tests showed that the transmittance of the 55 μm free-standing solid film was ~90% at visible wavelengths (400–700 nm).

[0121] Example 20 3D Object Formation In a glass bottle, Pd520 (1 molar part), Rhodorsil 2074 (4 molar parts), and CTX (1 molar part) were dissolved in a mixture of monomers PENB / NBEtOPhPh / NBEtCl (5000 molar parts, 90 / 5 / 5 molar ratio) to form a clear solution. The composition was placed in the resin tank of a 3D printer, Hunter DLP Resin 3D Printer (Flash Forge). The composition was then exposed to UV light (405 nm) to solidify, and a 3D object was built up layer by layer by digital light processing (DLP). The 3D printed object is shown in Figure 4. The composition maintained a relatively constant viscosity overnight in the resin tank during 3D printing. After overnight, the solution still remained reactive, as confirmed by UV-DSC, and after exposure to UV light for 4 seconds (1 J / cm 2 After 1 h of UV exposure, the reaction showed a rapid exothermic peak (395 nm) and continued to release heat even after UV exposure was discontinued. The reaction was complete within 1 min, with conversion reaching 90% within 0.5 min. After UV exposure, isothermal TGA (100 °C for 1 h) showed that the solids remained at ∼98%. The solution remained free-flowing after 4 days at room temperature.

[0122] Example 21 Stamp manufacturing (UV-NIL) A digital video disc (DVD) was separated using a razor blade to expose the channel patterned surface. It was washed with methanol to expose the hard polycarbonate channel pattern to finish the work preparation. Pd520 (1 molar part), Rhodorsil 2074 (4 molar parts), ITX (1 molar part) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle, and PENB (4500 molar parts) was added to form a clear solution. The formed composition was poured onto the surface of a glass substrate. The DVD (Verbatim) was separated using a razor blade and washed with methanol to expose the channel patterned surface. Figures 5A and 5B show optical micrographs taken at 10 μm and 20 μm resolution, respectively, of the patterned surface of the DVD. The exposed channeled surface of the DVD was then placed on the composition placed on the glass substrate and exposed to UV light (1 J / cm) for 4 seconds at room temperature. 2 , 395 nm). After a few minutes, a hardened solid film was formed, which was peeled off. The stamping film was observed under an optical microscope. Figures 6A and 6B show the pattern formed from the DVD at magnifications of 10 μm and 20 μm, respectively. As can be seen in Figures 5 and 6, the channel surface imprinted in the film is essentially similar to the original channels of the exposed DVD. The channel period was about 760 nm ± 20 nm. It was therefore demonstrated that the composition of the present invention can be used to form nanoimprints.

[0123] Examples 22-24 further illustrate organopalladium compounds of formula (I) that can be used to form the compositions of the present invention.

[0124] Examples 22 to 24 Separately, three glass bottles were prepared, and Pd304, Pd520, and Pd473 (1 mol part) were mixed with Rhodorsil 2074 (2 mol parts) and ITX (1 mol part), respectively, and dissolved in NBEtOPhPh (500 mol parts), and then a mixture of PENB / DecNB (4500 mol parts, the overall molar ratio of PENB / DecNB / NBEtOPhPh was 45 / 45 / 10) was added to form a transparent solution. The solution was exposed to UV light at room temperature for 4 seconds (1 J / cm 2 , 395 nm). The solution turned to a solid within a few minutes, suggesting that the monomers had polymerized, which was later confirmed by DSC and TGA. According to the TGA test, after UV exposure, the remaining solids were ~99% for the entire composition as confirmed by isothermal TGA (100°C for 1 h). As confirmed by UV-DSC, all the compositions showed an exothermic peak after 4 seconds of exposure to UV light, and continued to release heat even after UV exposure. The reactivity of each composition was compared by measuring the enthalpy change during a reaction time of 5 minutes. However, since monomer polymerization generally continues even after exposure to actinic radiation, it is recommended that the TGA measurement be performed at least 1 hour after exposure. According to the measured enthalpy change, the reactivity of the catalysts was shown to be in the order of Pd520>Pd304>Pd473. The enthalpy data are summarized in Table 7.

[0125] [Table 7]

[0126] The following examples demonstrate that a variety of photoacid generators (PAGs) and photosensitizers can be used in the compositions of the present invention as described herein.

[0127] Example 25 PENB and OPPI-SbF 6 Bulk polymerization of Pd520 (1 molar part), OPPI-SbF6 (2 molar parts), and DEA (1 molar part) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle, and PENB (4500 molar parts) was added to form a clear solution. The solution was purged with dry N2 for 2 hours and exposed to UV light (1 J / cm) at room temperature for 4 seconds.2 , 395 nm). The solution solidified within 1 min and became a hard solid after 5 min.

[0128] Example 26 Bulk polymerization of PENB and TAG382 In a glass bottle, Pd520 (1 molar part), TAG382 (2 molar parts), and ITX (1 molar part) were dissolved in PENB (5000 molar parts) to form a clear solution. The solution was purged with dry N2 overnight and exposed to UV light (1 J / cm2) at room temperature for 4 seconds. 2 , 395 nm). The solution became a viscous liquid in 1 min and a soft solid in 5 min, suggesting that the monomers were polymerized. When the solution was first heated at 70 °C and then exposed to UV light for 4 s (1 J / cm 2 , 395 nm), the solution became a hard solid within minutes, indicating that the monomer was fully polymerized. The unexposed solution remained free-flowing even after two weeks at room temperature, indicating good working life.

[0129] Example 27 Bulk polymerization of PENB and Irgacure PAG290 In a glass bottle, Pd520 (1 molar part), Irgacure PAG290 (2 molar parts), and DEA (1 molar part) were first dissolved in ethyl acetate (EA) solvent, and PENB (5000 molar parts) was added to form a clear solution. The solution was purged with dry N2 overnight. The solution was exposed to UV light at room temperature for 4 seconds (1 J / cm2). 2 , 395 nm), it became a viscous liquid in 1 minute and a soft solid in 5 minutes, suggesting that the monomers were polymerized. When the solution was first heated at 70 °C and then exposed to UV light for 4 seconds (1 J / cm 2 , 395 nm), the solution became a hard solid within minutes, indicating complete polymerization of the monomer. The unexposed solution remained free-flowing even after two months at room temperature, indicating good working life.

[0130] Examples 28 to 31 Bulk polymerization of PENB / NBEtOPhPh (90 / 10 molar ratio) with various organopalladium compounds. Four glass bottles were prepared separately, and Pd428, Pd498, Pd620, and Pd920 (1 mol part) were mixed with Rhodorsil 2074 (2 mol parts) and CTX (1 mol part), respectively, and dissolved in NBEtOPhPh (1000 mol parts), and then a mixture of PENB (9000 mol parts, the overall molar ratio of PENB / NBEtOPhPh was 90 / 10) was added to form a transparent solution. Each solution was exposed to UV light at room temperature for 4 seconds (1 J / cm 2 , 395 nm). All solutions turned solid within minutes, indicating polymerization of the monomers, which was later confirmed by DSC and TGA. After UV exposure, the remaining solids as confirmed by isothermal TGA (100°C for 1 hour) were >98% for all compositions, with the exception of Example 30. The results are summarized in Table 8. As confirmed by UV-DSC, all compositions showed an exothermic peak after exposure to UV light for 4 seconds, and continued to release heat after UV exposure. The reactivity of each composition was compared by measuring the enthalpy change over a 5 minute reaction time. The measured enthalpy data are summarized in Table 8.

[0131] [Table 8]

[0132] Example 32 In glass bottle A, Pd520 (1 molar part) was dissolved in PENB (2500 molar parts) to form a clear solution. Also, in glass bottle B, UV CATA 243 (2 molar parts) and ITX (1 molar part) were dissolved in PENB (2500 molar parts) to form a clear solution. Both were stored at room temperature and showed no change in viscosity over time. The solutions remained homogeneous and clear even after mixing, forming the composition of the present invention. When the composition was irradiated with UV (1 J / cm 2 , 395 nm), it gelled immediately and turned into a clear, hard solid within 1 min. The above composition was spin-coated onto a 2-inch quartz wafer at 500 rpm for 10 s and 1000 rpm for 30 s, and then exposed to UV light (1 J / cm 2A transparent solid film was formed within a few minutes at wavelengths of 300 nm to 395 nm, and the thickness of the film was measured by profilometry to be 3.03 ± 0.03 μm. The transmittance of the film formed on the quartz wafer was measured by UV-vis and was 92% in the range of 400 to 800 nm.

[0133] Example 33 TD, UV CATA 243, Bulk polymerization of Pd520 In a glass bottle, Pd520 (1 molar part), UV CATA 243 (4 molar parts), ITX (2 molar parts) were dissolved in TD (5000 molar parts) to form a clear solution. The solution was exposed to UV light at room temperature for 4 seconds (4 J / cm 2 , 395 nm). After UV exposure, the solution gelled in 1 min and became a hard solid within minutes, suggesting polymerization had occurred. After UV exposure, isothermal TGA (100 °C for 1 h) showed ~80% solid residue remaining. The unexposed solution remained free-flowing with no gelation even after 1 week at room temperature.

[0134] Example 34 Bulk polymerization of PhenylbutylNB, UV CATA 243, and Pd520 In a glass bottle, Pd520 (1 molar part), UV CATA 243 (4 molar parts), and ITX (2 molar parts) were dissolved in PhenylbutylNB (5000 molar parts) to form a clear solution. The solution was exposed to UV light at room temperature for 4 seconds (1 J / cm 2 , 395 nm). After UV exposure, the solution gelled in 1 min and became a hard solid within minutes, suggesting polymerization had occurred. After UV exposure, isothermal TGA (100 °C for 1 h) showed ~99% solid residue remaining. The unexposed solution remained free-flowing with no gelation even after 1 week at room temperature.

[0135] Example 35 Bulk polymerization of cyclohexylNB, UV CATA 243, and Pd520 In a glass bottle, Pd520 (1 molar part), UV CATA 243 (4 molar parts), and ITX (2 molar parts) were dissolved in CyclohexylNB (5000 molar parts) to form a clear solution. The solution was exposed to UV light at room temperature for 4 seconds (1 J / cm 2 , 395 nm). After UV exposure, the solution gelled within 1 min and became a hard solid within a few minutes, suggesting polymerization had occurred. After UV exposure, isothermal TGA (100 °C for 1 h) showed a solid residue retention of ∼94%. The unexposed solution remained free-flowing with no gelation even after 1 week at room temperature.

[0136] Example 36 Bulk polymerization of HexaDecylNB, UV CATA 243, and Pd520 In a glass bottle, Pd520 (1 molar part), UV CATA 243 (2 molar parts), and ITX (1 molar part) were dissolved in HexaDecylNB (5000 molar parts) to form a clear solution. The solution was exposed to UV light at room temperature for 4 seconds (1 J / cm 2 , 395 nm). After UV exposure, the solution gelled in 1 min and became a hard solid within a few minutes, suggesting polymerization had occurred. After UV exposure, isothermal TGA (100 °C for 1 h) showed that the solid residue remained at ~99%.

[0137] Example 37 Bulk polymerization of PhNB, UV CATA 243, and Pd520 In a glass bottle, Pd520 (1 molar part), UV CATA 243 (2 molar parts), and ITX (1 molar part) were dissolved in PhNB (5000 molar parts) to form a clear solution. The solution was exposed to UV light at room temperature for 4 seconds (1 J / cm 2 , 395 nm). After UV exposure, the solution gelled in 1 min and became a hard solid within a few minutes, suggesting polymerization had occurred. After UV exposure, isothermal TGA (100 °C for 1 h) showed that the solid residue remained at ~90%.

[0138] Example 38 Bulk polymerization of DecNB / NBMeOPhPh, UV CATA 243, and Pd520 In a glass bottle, Pd520 (1 molar part), UV CATA 243 (2 molar parts), and ITX (1 molar part) were dissolved in a mixture of DecNB / NBMeOPhPh (5000 molar parts, 80 / 20 molar ratio) to form a clear solution. The solution was exposed to UV light at room temperature for 4 seconds (1 J / cm). 2 , 395 nm). After UV exposure, the solution gelled in 1 min and solidified within a few minutes, suggesting polymerization had occurred. After UV exposure, isothermal TGA (100 °C for 1 h) showed that the solid residue remained at ~99%.

[0139] Comparative Examples 1-2 below are presented to demonstrate that only organopalladium compounds of formula (I) are effective under the conditions described herein, while similar catalysts such as nickel or platinum compounds are ineffective under similar conditions.

[0140] Comparative Example 1 PENB / NBEtCl and Ni(acac) 2 Bulk polymerization of Ni(acac)2 (1 molar part), Rhodorsil 2074 (2 molar parts), and CTX (1 molar part) were dissolved in NBEtCl (250 molar parts) in a glass bottle, and PENB (4750 molar parts) was added to form a solution. The solution was purged with dry N2 overnight and exposed to UV light (1 J / cm) at room temperature for 4 seconds. 2 , 395 nm). The solution remained in a free-flowing liquid state, suggesting that the monomer had not polymerized. The exposed solution was allowed to stand at room temperature for 3 days and still remained free-flowing.

[0141] Comparative Example 2 PENB / NBEtOPhPh and Pt(acac) 2 Bulk polymerization of Pt(acac)2 (1 molar part), Rhodorsil 2074 (2 molar parts), and CTX (1 molar part) were dissolved in NBEtOPhPh (500 molar parts) in a glass bottle, and PENB (4500 molar parts) was added to form a solution. The solution was purged with dry N2 overnight and exposed to UV light for 4 seconds at room temperature (1 J / cm 2, 395 nm). The solution remained in a free-flowing liquid state, suggesting that the monomer had not polymerized. The exposed solution was allowed to stand at room temperature for a day and still remained free-flowing.

[0142] Although the present invention has been described with reference to the above examples, the present invention is not limited to the examples, but generally encompasses the general area described above in this specification. Various modifications and embodiments are possible without departing from the spirit of the present invention. The matters disclosed in this specification include the following. 〔1〕 1. A composition comprising: a) one or more olefin monomers; b) An organopalladium compound of formula (I): [ka] (where: Each A is independently a bidentate monoanionic ligand of formula (II): [ka] n is an integer of 0, 1 or 2; X and Y are each independently selected from O, N, and S; R 1 、R 2 、R 3 、R 4 、R 5 、R 6 , and R 7 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C 3 -C 20 ) alkyl, (C 1 -C 16 ) perfluoroalkyl, (C 3 -C 10 ) cycloalkyl, (C 6 -C 10 )Aryl(C 1 -C 16 ) alkyl, and substituted or unsubstituted (C 6 -C 10 aryl, and when any one of X or Y is O or S, R 1 and R 5 does not exist respectively); a) a photoacid generator,

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

change

[17] , comprising at least two different first and second monomers of formula (V), the first monomer being completely dissolved in the second monomer, and forming a substantially transparent film having a transmittance of at least 90% of visible light when the composition is exposed to suitable actinic radiation for a sufficient time. 〔19〕 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , (4-(octyloxy)phenyl)(phenyl)iodonium hexafluorophosphate (OPPI-PF 6 ), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , (4-(octyloxy)phenyl)(phenyl)iodonium hexafluoroantimonate (OPPI-SbF 6 ), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-chloro-9H-thioxanthen-9-one (CTX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(acetylacetonate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(tetramethylheptenoate) 2 , triylcumyliodonium-tetrakispentafluorophenylborate (Rhodorsil 2074), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-Phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , (2-(4-methoxynaphthalen-1-yl)-2-oxoethyl)dimethylsulfonium tetrakis-pentafluorophenylborate (TAG 382), and 9,10-diethoxyanthracene (DEA); and 5-Phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , tris(4-((4-acetylphenyl)thio)phenyl)sulfonium tetrakis-pentafluorophenylborate (Irgacure PAG 290), and 9,10-diethoxyanthracene (DEA); The kit according to claim 17, wherein the compound is selected from the group consisting of: 〔20〕 A film formed from the composition described in [1] above.

Claims

1. 1. A composition comprising: a) one or more olefin monomers represented by formula (V) 【Chemistry 4】 Where: m is an integer of 0, 1 or 2; 【Chemistry 5】 is a single bond or a double bond; R 13 , R 14 , R 15 , and R 16 are the same or different and are each independently selected from the group consisting of hydrogen, halogen, a hydrocarbyl group or a halohydrocarbyl group, said hydrocarbyl group or halohydrocarbyl group being methyl, ethyl, straight or branched (C 3 -C 20 ) alkyl, perfluoro(C 1 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 6 ) alkyl, perfluoro(C 6 -C 10 ) aryl, perfluoro(C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, methoxy, ethoxy, linear or branched (C 3 -C 16 ) alkoxy, perfluoro (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 12 ) aryloxy, (C 6 -C 12 ) aryloxy (C 1 -C 6 ) alkyl, (C 6 -C 12 ) Aryl (C 1 -C 6 ) alkoxy, perfluoro (C 6 -C 12 ) aryloxy, perfluoro(C 6 -C 12 ) Aryl (C 1 -C 3 ) alkoxy, 【Chemistry 6】 is selected from Here, Z is O, CO, C(O)O, OC(O), OC(O)O, S, (CR 17 R 18 ) b , O(CR 17 R 18 ) b , (CR 17 R 18 ) b O, C(O)(CR 17 R 18 ) b , (CR 17 R 18 ) b C(O), C(O)O(CR 17 R 18 ) b , (CR 17 R 18 ) b C(O)O, OC(O)(CR 17 R 18 ) b , (CR 17 R 18 ) b O.C. (O), (CR 17 R 18 ) b OC(O)O, (CR 17 R 18 ) b O.C.O. 17 R 18 ) b ,OC(O)O(CR 17 R 18 ) b , S(CR 17 R 18 ) b , (CR 17 R 18 ) b S, (SiR 17 R 18 ) b , O(SiR 17 R 18 ) b , (SiR 17 R 18 ) b is selected from the group consisting of O; R 17 and R 18 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C 3 -C 12 ) alkyl, substituted or unsubstituted (C 6 -C 14 ) aryl, methoxy, ethoxy, linear or branched (C 3 -C 6 ) alkyloxy, (C 2 -C 6 ) acyl, (C 2 -C 6 ) acyloxy, and substituted or unsubstituted (C 6 -C 14 ) aryloxy; and b is an integer from 1 to 12; Aryl is selected from the group consisting of substituted or unsubstituted phenyl, substituted or unsubstituted biphenyl, substituted or unsubstituted naphthyl, substituted or unsubstituted terphenyl, substituted or unsubstituted anthracenyl, substituted or unsubstituted fluorenyl, said substituents being halogen, methyl, ethyl, linear or branched (C 3 -C 6 ) alkyl, perfluoro(C 1 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 6 ) alkyl, perfluoro(C 6 -C 10 ) aryl, perfluoro(C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, methoxy, ethoxy, linear or branched (C 3 -C 16 ) alkoxy, perfluoro (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) aryloxy, (C 6 -C 12 ) aryloxy (C 1 -C 6 ) alkyl, (C 6 -C 12 ) Aryl (C 1 -C 6 ) alkoxy, perfluoro (C 6 -C 12 ) aryloxy, and perfluoro(C 6 -C 12 ) Aryl (C 1 -C 3 ) alkoxy; k is an integer from 1 to 12; R 23 , R 24 , and R 25 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C 3 -C 12 ) alkyl, perfluoro(C 1 -C 12 ) alkyl, methoxy, ethoxy, linear or branched (C 3 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 6 ) alkyl, perfluoro(C 6 -C 10 ) aryl, and perfluoro (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, or R 23 and R 24 represents a substituted or unsubstituted (C 5 -C 14 ) cyclic, (C 5 -C 14 ) bicyclic, or (C 5 -C 14 ) forms a tricyclic ring; Arylene is a substituted or unsubstituted divalent (C 6 -C 14 ) aryl; or R 13 , R 14 Any one of the following is R 15 , R 16 A substituted or unsubstituted (C 5 -C 14 ) cyclic, (C 5 -C 14 ) bicyclic, or (C 5 -C 14 ) forming a tricyclic ring; b) An organopalladium compound of formula (I): 【Chemistry 1】 (where: Each A is independently a bidentate monoanionic ligand of formula (II): 【Chemistry 2】 n is an integer of 0, 1 or 2; X and Y are each independently selected from O, N, and S; R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , and R 7 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C 3 -C 20 ) alkyl, (C 1 -C 16 ) perfluoroalkyl, (C 3 -C 10 ) cycloalkyl, (C 6 -C 10 ) Aryl (C 1 -C 16 ) alkyl, and substituted or unsubstituted (C 6 -C 10 aryl; and when any one of X or Y is O or S, R 1 and R 5 do not exist); c) a photoacid generator, 【Chemistry 3】 (where: a is an integer from 0 to 5; A - , Cl - , B - , I - , B.F. 4 - , tetrakis(pentafluorophenyl)borate, tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, tetrakis(2-fluorophenyl)borate, tetrakis(3-fluorophenyl)borate, tetrakis(4-fluorophenyl)borate, tetrakis(3,5-difluorophenyl)borate, tetrakis(2,3,4,5-tetrafluorophenyl)borate, tetrakis(3,4,5,6-tetrafluorophenyl)borate, tetrakis(3,4,5-trifluorophenyl)borate, methyl tris(perfluorophenyl)borate, ethyl tris(perfluorophenyl)borate, phenyl tris(perfluorophenyl)borate, tetrakis(1,2,2-trifluoroethylenyl)borate, tetrakis(4-tri-1 tetrakis(4-dimethyl-tert-butylsilyltetrafluorophenyl)borate, (triphenylsiloxy)tris(pentafluorophenyl)borate, (octyloxy)tris(pentafluorophenyl)borate, tetrakis[3,5-bis[1-methoxy-2,2,2-trifluoro-1-(trifluoromethyl)ethyl]phenyl]borate, tetrakis[3-[1-methoxy-2,2,2-trifluoro-1-(trifluoromethyl)ethyl]-5-(trifluoromethyl)phenyl]borate, and tetrakis[3-[2,2,2-trifluoro-1-(2,2,2-trifluoroethoxy)-1-(trifluoromethyl)-ethyl]-5-(trifluoromethyl)phenyl]borate, PF 6 - , SbF 6 - , n-C 4 F 9 SO 3 - , C.F. 3 SO 3 - , and p-CH 3 (C 6 H 4 ) -SO 3 - and R 8 , R 9 , R 10 , R 11 , and R 12 are the same or different and are halogen, methyl, ethyl, linear or branched (C 3 -C 20 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 10 ) aryloxy (C 1 -C 3 ) alkyl, (C 6 -C 10 ) aryloxy, (C 6 -C 10 ) thioaryl, (C 1 -C 6 ) Alkanoyl (C 6 -C 10 ) thioaryl, (C 1 -C 6 ) Alkoxy (C 6 -C 10 ) Aroyl (C 1 -C 6 ) alkyl, and (C 6 -C 10 ) thioaryl-(C 6 -C 10 ) a photoacid generator selected from the group consisting of diarylsulfonium salts; and d) a photosensitizer comprising a compound of formula (VIII) and a compound of formula (IX) 【Chemistry 3-2】 (where: R 44 , R 45 , R 46 are the same or different and are hydrogen, halogen, hydroxy, NO 2 , N.H. 2 , methyl, ethyl, linear or branched (C 3 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 10 ) Alkoxy (C 1 -C 3 ) alkyl, (C 6 -C 10 ) alkoxy, C(O)(C 1 -C 6 ) alkyl, COOH, C(O)O(C 1 -C 6 ) alkyl, and SO 2 (C 6 -C 10 aryl; R 47 , R 48 are the same or different and are methyl, ethyl, linear or branched (C 3 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl); A composition comprising:

2. 10. The composition of claim 1, wherein the composition comprises at least two different monomers of formula (V) and is in the form of a clear liquid having a viscosity of less than 100 centipoise.

3. The composition of claim 1, wherein the composition comprises two different monomers of formula (V) in a molar ratio of 1:99 to 99:

1.

4. The composition of claim 1 , wherein the composition forms a substantially transparent film when exposed to appropriate actinic radiation.

5. The composition of claim 4 , wherein the film has a transmittance of 90% or greater for visible light.

6. The composition of claim 4 , wherein the film has a transmittance of 95% or greater for visible light.

7. The bidentate monoanionic ligand is 【Chemistry 7-1】 【Chemistry 7-2】 The composition of claim 1 selected from the group consisting of:

8. Further comprising one or more monomers selected from the group consisting of monomers of formula (VI) and monomers of formula (VII), The monomer of formula (VI) is 【Chemistry 8】 where: o is an integer from 0 to 2; D is SiR 29 R 30 R 31 ,or 【Chemistry 9】 is a group selected from c is an integer from 1 to 10, and one or more CH 2 (C 1 -C 10 ) alkyl or (C 1 -C 10 ) optionally substituted with perfluoroalkyl; R 26 , R 27 , and R 28 are the same or different and are each independently selected from hydrogen, halogen, and hydrocarbyl, wherein the hydrocarbyl is methyl, ethyl, linear or branched (C 3 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 10 ) aryloxy (C 1 -C 3 ) alkyl or (C 6 -C 10 ) aryloxy; and R 29 , R 30 , and R 31 is methyl, ethyl, straight or branched (C 3 -C 9 ) alkyl, substituted or unsubstituted (C 6 -C 14 ) aryl, methoxy, ethoxy, linear or branched (C 3 -C 9 ) alkoxy or substituted or unsubstituted (C 6 -C 14 ) aryloxy; The monomer of formula (VII) is 【Chemistry 10】 where: Z 1 is a substituted or unsubstituted (C 1 -C 12 ) alkylene, -(CH 2 ) d (SiR 38 R 39 ) (OSiR 40 R 41 ) f (CH 2 ) e - or - (CH 2 ) d O (CH 2 ) e - (wherein d, e, and f are each independently an integer from 0 to 6; R 38 , R 39 , R 40 , and R 41 are the same or different and are methyl, ethyl, linear or branched (C 3 -C 12 ) alkyl, and arylene selected from: 【Chemistry 11】 ; R 32 , R 33 , R 34 , R 35 , R 36 , and R 37 are the same or different and are each independently selected from hydrogen, halogen, and hydrocarbyl, wherein the hydrocarbyl is methyl, ethyl, linear or branched (C 3 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 10 ) aryloxy (C 1 -C 3 ) alkyl or (C 6 -C 10 ) aryloxy.

9. The monomer of formula (V) is 【Chemistry 12-1】 【Chemistry 12-2】 【Chemistry 12-3】 【Chemistry 12-4】 【Chemistry 12-5】 【Chemistry 12-6】 【Chemistry 12-7】 The composition of claim 1 selected from the group consisting of:

10. The monomer of formula (VI) or the monomer of formula (VII) is 【Chemistry 13-1】 【Chemistry 13-2】 【Chemistry 13-3】 The composition of claim 8 selected from the group consisting of:

11. The organopalladium compound of the formula (I) is 【Chemistry 14-1】 【Chemistry 14-2】 The composition of claim 1 selected from the group consisting of:

12. The compound of formula (III) or the compound of formula (IV) is 【Chemistry 15-1】 【Chemistry 15-2】 【Chemistry 15-3】 【Chemistry 15-4】 The composition of claim 1 , wherein each of the following is selected from the group consisting of

13. The photosensitizer is A compound of formula (VIII): 【Chemistry 16】 Where: R 44 , R 45 , and R 46 2. The composition of claim 1, wherein: are the same or different and are each independently selected from the group consisting of hydrogen, chlorine, methyl, ethyl, n-propyl, isopropyl, methoxy, ethoxy, propoxy, and phenoxy.

14. The compound of formula (VIII) or the compound of formula (IX) is 【Chemistry 17-1】 【Chemistry 17-2】 【Chemistry 17-3】 The composition of claim 1 selected from the group consisting of:

15. 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , (4-(octyloxy)phenyl)(phenyl)iodonium hexafluorophosphate (OPPI-PF 6 ), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , (4-(octyloxy)phenyl)(phenyl)iodonium hexafluoroantimonate (OPPI-SbF 6 ), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-chloro-9H-thioxanthen-9-one (CTX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(acetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(tetramethylheptenoate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , (2-(4-methoxynaphthalen-1-yl)-2-oxoethyl)dimethylsulfonium tetrakis-pentafluorophenylborate (TAG 382), and 9,10-diethoxyanthracene (DEA); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , tris(4-((4-acetylphenyl)thio)phenyl)sulfonium tetrakis-pentafluorophenylborate, and 9,10-diethoxyanthracene (DEA); and 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , iodonium, diphenyl-4,4'-di-(C 10 -C 13 ) alkyl derivatives, tetrakis(2,3,4,5,6-pentafluorophenyl)borate, and 2-isopropyl-9H-thioxanthen-9-one (ITX). The composition of claim 1 selected from the group consisting of:

16. 1. A kit for forming a substantially transparent film, comprising: a) one or more olefin monomers represented by formula (V) 【Chemistry 24】 Where: m is an integer of 0, 1 or 2; 【Chemistry 25】 is a single bond or a double bond; R 13 , R 14 , R 15 , and R 16 are the same or different and are each independently selected from the group consisting of hydrogen, halogen, a hydrocarbyl group or a halohydrocarbyl group, said hydrocarbyl group or halohydrocarbyl group being methyl, ethyl, straight or branched (C 3 -C 20 ) alkyl, perfluoro(C 1 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 6 ) alkyl, perfluoro(C 6 -C 10 ) aryl, perfluoro(C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, methoxy, ethoxy, linear or branched (C 3 -C 16 ) alkoxy, perfluoro (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 12 ) aryloxy, (C 6 -C 12 ) aryloxy (C 1 -C 6 ) alkyl, (C 6 -C 12 ) Aryl (C 1 -C 6 ) alkoxy, perfluoro (C 6 -C 12 ) aryloxy, perfluoro(C 6 -C 12 ) Aryl (C 1 -C 3 ) alkoxy, 【Chemistry 26】 is selected from Here, Z is O, CO, C(O)O, OC(O), OC(O)O, S, (CR 17 R 18 ) b , O(CR 17 R 18 ) b , (CR 17 R 18 ) b O, C(O)(CR 17 R 18 ) b , (CR 17 R 18 ) b C(O), C(O)O(CR 17 R 18 ) b , (CR 17 R 18 ) b C(O)O, OC(O)(CR 17 R 18 ) b , (CR 17 R 18 ) b O.C. (O), (CR 17 R 18 ) b OC(O)O, (CR 17 R 18 ) b O.C.O. 17 R 18 ) b ,OC(O)O(CR 17 R 18 ) b , S(CR 17 R 18 ) b , (CR 17 R 18 ) b S, (SiR 17 R 18 ) b , O(SiR 17 R 18 ) b , (SiR 17 R 18 ) b O; R 17 and R 18 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C 3 -C 12 ) alkyl, substituted or unsubstituted (C 6 -C 14 ) aryl, methoxy, ethoxy, linear or branched (C 3 -C 6 ) alkyloxy, (C 2 -C 6 ) acyl, (C 2 -C 6 ) acyloxy, and substituted or unsubstituted (C 6 -C 14 ) aryloxy; and b is an integer from 1 to 12; Aryl is selected from the group consisting of substituted or unsubstituted phenyl, substituted or unsubstituted biphenyl, substituted or unsubstituted naphthyl, substituted or unsubstituted terphenyl, substituted or unsubstituted anthracenyl, substituted or unsubstituted fluorenyl, said substituents being halogen, methyl, ethyl, linear or branched (C 3 -C 6 ) alkyl, perfluoro(C 1 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 6 ) alkyl, perfluoro(C 6 -C 10 ) aryl, perfluoro(C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, methoxy, ethoxy, linear or branched (C 3 -C 16 ) alkoxy, perfluoro (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) aryloxy, (C 6 -C 12 ) aryloxy (C 1 -C 6 ) alkyl, (C 6 -C 12 ) Aryl (C 1 -C 6 ) alkoxy, perfluoro (C 6 -C 12 ) aryloxy, and perfluoro(C 6 -C 12 ) Aryl (C 1 -C 3 ) alkoxy; k is an integer from 1 to 12; R 23 , R 24 , and R 25 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C 3 -C 12 ) alkyl, perfluoro(C 1 -C 12 ) alkyl, methoxy, ethoxy, linear or branched (C 3 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 6 ) alkyl, perfluoro(C 6 -C 10 ) aryl, and perfluoro (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, or R 23 and R 24 represents a substituted or unsubstituted (C 5 -C 14 ) cyclic, (C 5 -C 14 ) bicyclic, or (C 5 -C 14 ) forms a tricyclic ring; Arylene is a substituted or unsubstituted divalent (C 6 -C 14 ) aryl; or R 13 , R 14 Any one of the following is R 15 , R 16 A substituted or unsubstituted (C 5 -C 14 ) cyclic, (C 5 -C 14 ) bicyclic, or (C 5 -C 14 ) forming a tricyclic ring; b) An organopalladium compound of formula (I): 【Chemistry 18】 (where: Each A is independently a bidentate monoanionic ligand of formula (II); 【Chemistry 19】 n is an integer of 0, 1 or 2; X and Y are each independently selected from O, N, and S; R 1 , R 2 , R 3 , R 4 , R 5 , R 6 , and R 7 are the same or different and are hydrogen, methyl, ethyl, straight-chain or branched (C 3 -C 16 ) alkyl, (C 3 -C 10 ) cycloalkyl, (C 6 -C 10 ) Aryl (C 1 -C 16 ) alkyl, and substituted or unsubstituted (C 6 -C 10 aryl; and when any one of X or Y is O or S, R 1 and R 5 do not exist); c) a photoacid generator, 【Chemistry 20-1】 (where: a is an integer from 0 to 5; A - , Cl - , B - , I - , B.F. 4 - , tetrakis(pentafluorophenyl)borate, tetrakis(3,5-bis(trifluoromethyl)phenyl)borate, tetrakis(2-fluorophenyl)borate, tetrakis(3-fluorophenyl)borate, tetrakis(4-fluorophenyl)borate, tetrakis(3,5-difluorophenyl)borate, tetrakis(2,3,4,5-tetrafluorophenyl)borate, tetrakis(3,4,5,6-tetrafluorophenyl)borate, tetrakis(3,4,5-trifluorophenyl)borate, methyl tris(perfluorophenyl)borate, ethyl tris(perfluorophenyl)borate, phenyl tris(perfluorophenyl)borate, tetrakis(1,2,2-trifluoroethylenyl)borate, tetrakis(4-tri-1 tetrakis(4-dimethyl-tert-butylsilyltetrafluorophenyl)borate, (triphenylsiloxy)tris(pentafluorophenyl)borate, (octyloxy)tris(pentafluorophenyl)borate, tetrakis[3,5-bis[1-methoxy-2,2,2-trifluoro-1-(trifluoromethyl)ethyl]phenyl]borate, tetrakis[3-[1-methoxy-2,2,2-trifluoro-1-(trifluoromethyl)ethyl]-5-(trifluoromethyl)phenyl]borate, and tetrakis[3-[2,2,2-trifluoro-1-(2,2,2-trifluoroethoxy)-1-(trifluoromethyl)-ethyl]-5-(trifluoromethyl)phenyl]borate, PF 6 - , SbF 6 - , n-C 4 F 9 SO 3 - , C.F. 3 SO 3 - , and p-CH 3 (C 6 H 4 ) -SO 3 - selected from the group consisting of: R 8 , R 9 , R 10 , R 11 , and R 12 are the same or different and are halogen, methyl, ethyl, linear or branched (C 3 -C 20 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 10 ) aryloxy (C 1 -C 3 ) alkyl, (C 6 -C 10 ) aryloxy, (C 6 -C 10 ) thioaryl, (C 1 -C 6 ) Alkanoyl (C 6 -C 10 ) thioaryl, (C 1 -C 6 ) Alkoxy (C 6 -C 10 ) Aroyl (C 1 -C 6 ) alkyl, and (C 6 -C 10 ) thioaryl-(C 6 -C 10 ) a photoacid generator selected from the group consisting of diarylsulfonium salts; and d) a photosensitizer comprising a compound of formula (VIII) and a compound of formula (IX) 【Chemistry 20-2】 (where: R 44 , R 45 , R 46 are the same or different and are hydrogen, halogen, hydroxy, NO 2 , N.H. 2 , methyl, ethyl, linear or branched (C 3 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl, (C 1 -C 12 ) alkoxy, (C 3 -C 12 ) cycloalkoxy, (C 6 -C 12 ) bicycloalkoxy, (C 7 -C 14 ) tricycloalkoxy, (C 6 -C 10 ) Alkoxy (C 1 -C 3 ) alkyl, (C 6 -C 10 ) alkoxy, C(O)(C 1 -C 6 ) alkyl, COOH, C(O)O(C 1 -C 6 ) alkyl, and SO 2 (C 6 -C 10 aryl; R 47 , R 48 are the same or different and are methyl, ethyl, linear or branched (C 3 -C 12 ) alkyl, (C 3 -C 12 ) cycloalkyl, (C 6 -C 12 ) bicycloalkyl, (C 7 -C 14 ) tricycloalkyl, (C 6 -C 10 ) aryl, (C 6 -C 10 ) Aryl (C 1 -C 3 ) alkyl); A kit comprising a composition comprising:

17. 17. The kit of claim 16, comprising at least two different first and second monomers of formula (V), the first monomer being completely dissolved in the second monomer, and forming a substantially transparent film having at least 90% transmittance of visible light when the composition is exposed to an appropriate actinic radiation for a sufficient time.

18. 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(acetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-chloro-9H-thioxanthen-9-one (CTX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , (4-(octyloxy)phenyl)(phenyl)iodonium hexafluorophosphate (OPPI-PF 6 ), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , (4-(octyloxy)phenyl)(phenyl)iodonium hexafluoroantimonate (OPPI-SbF 6 ), and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-(2-chloroethyl)bicyclo[2.2.1]hept-2-ene (NBEtCl), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium(hexafluoroacetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-chloro-9H-thioxanthen-9-one (CTX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(acetylacetonate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), 5-(2-([1,1'-biphenyl]-2-yloxy)ethyl)bicyclo[2.2.1]hept-2-ene (NBEtOPhPh), 5-decylbicyclo[2.2.1]hept-2-ene (DecNB), palladium(tetramethylheptenoate) 2 , triylcumyl iodonium-tetrakispentafluorophenylborate, and 2-isopropyl-9H-thioxanthen-9-one (ITX); 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , (2-(4-methoxynaphthalen-1-yl)-2-oxoethyl)dimethylsulfonium tetrakis-pentafluorophenylborate, and 9,10-diethoxyanthracene (DEA); and 5-phenethylbicyclo[2.2.1]hept-2-ene (PENB), palladium (hexafluoroacetylacetonate) 2 , tris(4-((4-acetylphenyl)thio)phenyl)sulfonium tetrakis-pentafluorophenylborate, and 9,10-diethoxyanthracene (DEA); 17. The kit of claim 16, comprising a composition selected from the group consisting of:

19. A film formed from the composition of claim 1.

Citation Information

Patent Citations

  • Method for producing norbornene-based addition polymers containing ester groups or acetyl groups

    JP2005521785A

  • Photosensitive composition, optical waveguide, optical interconnection, opto-electric hybrid board, electronic equipment and method for forming optical waveguide

    JP2010260916A

  • UV-active derivatives of Pd(AcAc)2L-catalyzed polycycloolefin compositions as optical materials

    JP2023508493A

  • Hindered amine-stabilized, UV-active organopalladium-catalyzed polycycloolefin compositions as optical materials

    JP2023529013A

  • Chemical amplification photoresist monomers, polymers therefrom and photoresist compositions containing the same