Electrolyte for lithium ion batteries and lithium ion batteries

A 6-membered heterocyclic group carboxylic acid anhydride additive forms a film on the positive electrode to address gas generation and oxidative decomposition issues in lithium-ion batteries, enhancing stability and cycle performance.

JP7575497B2Active Publication Date: 2024-10-29BYD CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022579962
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-23
Filing Date
2021-06-21
Publication Date
2024-10-29
Estimated Expiration
2041-06-21

AI Technical Summary

Technical Problem

Lithium-ion batteries face issues with gas generation due to parasitic reactions at the interface, leading to increased interfacial resistance and reduced service life, especially at high voltages, and current electrolytes pose safety risks due to oxidative decomposition and HF release.

Method used

Incorporation of a 6-membered heterocyclic group carboxylic acid anhydride additive in the electrolyte, which forms a film on the positive electrode, inhibiting interfacial deterioration and enhancing ion conductivity, thereby suppressing gas generation and improving high voltage and high temperature stability.

Benefits of technology

The additive effectively prevents electrolyte decomposition, reduces battery expansion, and extends the service life by improving cycle performance and high temperature stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575497000001
    Figure 0007575497000001
  • Figure 0007575497000002
    Figure 0007575497000002
  • Figure 0007575497000003
    Figure 0007575497000003
Patent Text Reader

Abstract

The present disclosure relates to an electrolyte for a lithium-ion battery, the electrolyte comprising an organic solvent, a lithium salt, and an additive. The electrolyte comprises a six-membered heterocyclic carboxylic acid anhydride additive, which can effectively suppress gas generation and an increase in interfacial resistance in the battery, improve the high-temperature stability of the battery, and extend the service life of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (CROSS REFERENCE TO RELATED APPLICATIONS) This application is filed based on the Chinese patent application having application number 202010584645.X (filing date June 23, 2020) and claims priority to the said Chinese patent application, the entire contents of which are incorporated herein by reference.

[0002] The present disclosure relates to the field of lithium batteries, and in particular to lithium-ion battery electrolytes and lithium-ion batteries. [Background technology]

[0003] Lithium-ion batteries have a large energy density and are always an indispensable battery system in the battery market. However, during the use of the battery system, gas is always generated due to the parasitic reaction between the interface and the electrolyte, and the interface resistance increases, which causes the battery to expand and the service life of the battery to decrease. In particular, in recent years, with the demand for battery energy density and the continuous development of positive electrode materials suitable for high voltage, the research of electrolytes suitable for high voltage materials has also become of utmost importance. The limit voltage applied to the current electrolyte system is 4.2V. When the voltage exceeds 4.2V, the electrolyte is oxidized at the positive electrode, causing gas generation, the electrolyte is consumed too quickly, which causes battery safety risks and shortens the service life of the battery. Therefore, the research of electrolytes suitable for high voltage systems is currently urgent. The solution of the conventional technology is to use a fluorine-containing electrolyte solvent to increase the oxidative decomposition potential of the electrolyte. Although the oxidative decomposition potential of the fluorine-containing solvent is high, the electrolyte will release HF in the later stage, destroying the positive and negative electrode material particles and affecting the service life of the battery. Summary of the Invention

[0004] In order to further increase the oxidative decomposition potential of the electrolyte, solve the current problem of electrolyte decomposition at high voltages, and improve the high voltage stability and high temperature stability of lithium batteries, the present disclosure provides an electrolyte for lithium ion batteries and a lithium ion battery.

[0005] In order to achieve the above object, the electrolyte for a lithium ion battery according to the first aspect of the present disclosure contains an organic solvent, a lithium salt, and an additive containing a first additive represented by formula (1). [ka] (In formula (1), X 1 , X 2 , X 3 and X 4 are each independently selected from CR or N, and X 1 , X 2 , X 3 and X 4 At least one of is N, and X 1 , X 2 , X 3 and X 4 R is H, halogen, and C 1 ~C 4 Alkyl group, C 1 ~C 4 Substituted alkyl groups of C 4 ~C 7 Cycloalkyl groups of C 1 ~C 3 are independently selected from the alkoxy groups

[0006] The inventors of the present disclosure have surprisingly found that the additive represented by formula (1) can preferentially cause an oxidation reaction at the high-nickel positive electrode interface to form a film, and the formed positive electrode film layer has excellent ion conductive performance and effectively blocks the interfacial deterioration reaction during cycles and storage between the positive electrode and the electrolyte where the catalytic oxidation reaction has occurred, thereby preventing or reducing the increase in polarization due to the continuous increase in the interfacial film layer and the gas expansion due to the interfacial reaction, and have obtained the present application.

[0007] A lithium ion battery according to a second embodiment of the present disclosure contains the lithium ion battery electrolyte according to the first embodiment of the present disclosure.

[0008] According to the above technical solution, the present disclosure provides an electrolyte for lithium ion batteries and a lithium ion battery, and the lithium ion battery containing the electrolyte of the present disclosure has excellent high-temperature stability performance and battery cycle performance at high voltage.

[0009] Other features and advantages of the present disclosure are described in detail in the following specific embodiments. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Specific embodiments of the present disclosure will be described in detail below. It should be understood that the specific embodiments described herein are merely for the purpose of explaining and interpreting the present disclosure, and are not intended to limit the present disclosure.

[0011] The electrolyte for lithium ion batteries according to the first embodiment of the present disclosure contains an organic solvent, a lithium salt, and an additive containing a first additive represented by formula (1). [ka] (In the formula, X 1 , X 2 , X 3 and X 4 are each independently selected from CR or N, and X 1 , X 2 , X 3 and X 4 At least one of is N, and X 1 , X 2 , X 3 and X 4 R is H, halogen, and C 1 ~C 4 Alkyl group, C 1 ~C 4 Substituted alkyl groups of C 4 ~C 7 Cycloalkyl groups of C 1 ~C 3 are independently selected from the alkoxy groups

[0012] The lithium ion battery electrolyte of the present disclosure contains a six-membered heterocyclic carboxylic acid anhydride additive, and can form a film on the surface of a positive electrode, that is, can form a positive electrode interfacial film with excellent lithium ion conductivity, can prevent the deterioration reaction of the positive electrode surface of the electrolyte under high voltage conditions, can prevent the battery from continuously generating gas during cycling, can reduce battery expansion, can inhibit decomposition of the electrolyte, and can extend the service life of the battery.

[0013] The six-membered heterocycle is In one embodiment, a six-membered ring group containing one N atom or two N atoms, In one embodiment, It is a six-membered ring group containing one N atom, because such a molecule has a lower reaction potential, is more useful for generating an oxidation reaction on the positive electrode surface to form a film, and the film-forming component has excellent ion-conducting performance.

[0014] In the present disclosure, in the lithium ion battery electrolyte, the content of the organic solvent, the content of the lithium salt, and the content of the additive may vary within a large range, In one embodiment The content of the organic solvent may be 50 to 90% by weight, the content of the lithium salt may be 1 to 20% by weight, and the content of the additive may be 0.1 to 10% by weight. In one embodiment In the preferred embodiment, the organic solvent content may be 60 to 85% by weight, the lithium salt content may be 5 to 15% by weight, and the additive content may be 0.5 to 8% by weight. In the preferred embodiment, an excellent membrane layer can be formed at the positive and negative electrode interfaces of the battery, which suppresses side reactions at the active sites of the positive and negative electrode interfaces of the electrolyte, suppresses gas generation and an increase in interface resistance of the battery, and improves the high-temperature performance of the battery, thereby extending the service life of the battery.

[0015] In the present disclosure, the additive includes, based on the total weight of the additive, The content of the first additive may be 30 to 100% by weight, and in one embodiment, it is 50 to 100% by weight. .

[0016] In the present disclosure, in formula (1), As an embodiment X 1 , X 2 , X 3 and X4 R1 is H. this In this case, the molecular weight is small, the oxidative decomposition potential is low, and the oxidation reaction on the positive electrode surface is more likely to occur preferentially.

[0017] As an embodiment In the preferred embodiment, the first additive represented by formula (1) is 2,3-pyridinedicarboxylic anhydride, 3,4-pyridinedicarboxylic anhydride, 2,3-pyrazinedicarboxylic anhydride, or 4,5-pyridazinedicarboxylic anhydride. In this preferred embodiment, the oxidative decomposition film-forming potential is low, and the film can be preferentially formed on the positive electrode surface. [ka] [ka] [ka] [ka]

[0018] In the present disclosure, the lithium salt For example, For example, LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 , LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN(C 2 F 5 SO 2 ) 2 , LiC(CF 3 SO 2 ) 3 and LiB(C 2 O 4 ) 2 may be one or more of the above.

[0019] In the present disclosure, the organic solvent CharcoalEthyl methyl carbonate, dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, ethylene sulfite, propylene sulfite, diethyl sulfite, γ-butyrolactone, dimethyl sulfoxide, ethyl acetate or Methyl acetate may be used.

[0020] In the present disclosure, based on the total weight of the additive, the additive further contains a second additive that is the remainder, and the second additive contains one or more of vinylene carbonate, lithium bis(oxalato)borate, and lithium bis(fluorosulfonylimide).

[0021] A lithium ion battery according to a second aspect of the present application includes a case, a cell housed in the case, and the lithium ion battery electrolyte according to the first aspect of the present disclosure.

[0022] In the present disclosure, a cell may include a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.

[0023] In the present disclosure, the positive electrode may include a positive electrode current collector and a positive electrode material, and the positive electrode material may include a positive electrode active material, a conductive agent, and a positive electrode binder. The positive electrode active material, the conductive agent, and the positive electrode binder may be a positive electrode active material, a conductive agent, and a positive electrode binder commonly used in this field. The positive electrode active material may be a nickel manganese positive electrode material having a spinel or layered structure and a lithium iron phosphate-based positive electrode material, As an embodiment Spinel LiNi 0.5 Mn 1.5 O 4 It is.

[0024] In the present disclosure, the negative electrode includes a negative electrode current collector and a negative electrode material, and the negative electrode material includes a negative electrode active material and a negative electrode binder. The negative electrode material may further include a conductive agent, which is a general conductive agent and may be the same as or different from the conductive agent in the positive electrode material layer. The negative electrode active material and the negative electrode binder may be a negative electrode active material and a negative electrode binder commonly used in this field. The negative electrode active material is a lithium or graphite negative electrode or a silicon carbon negative electrode material, As an embodimentis metallic lithium.

[0025] The present disclosure will now be described in more detail with reference to the following examples. All of the raw materials used in the examples are commercially available.

[0026] Example 1 (1) Preparation of non-aqueous electrolyte: In an argon glove box, 26 parts by weight of ethylene carbonate (EC), 61 parts by weight of diethyl carbonate (DEC), and 12 parts by weight of lithium hexafluorophosphate (LiPF 6 ) and 0.5 parts by weight of 2,3-pyridinedicarboxylic anhydride were uniformly mixed to obtain an electrolyte solution for lithium ion batteries of this example, designated as C1.

[0027] (2) Lithium-ion battery manufacturing: Cathode active material (LiNi 0.5 Mn 1.5 O 4 ), acetylene black, and polyvinylidene fluoride are uniformly mixed in a mixing ratio of 90:5:5, and then pressed onto aluminum foil to obtain a positive electrode plate. A metallic lithium plate is used as a negative electrode plate, a PE / PP composite separator is used as an ion exchange membrane, and the electrolyte C1 of this embodiment is used to manufacture a coin battery S1 by a general method in this field.

[0028] Example 2 An electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 0.5 parts by weight of 2,3-pyridinedicarboxylic anhydride was replaced with 1 part by weight of 3,4-pyridinedicarboxylic anhydride to obtain nonaqueous electrolyte solution C2 for lithium ion batteries and coin-type battery S2.

[0029] Example 3 A nonaqueous electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 0.5 parts by weight of 2,3-pyridinedicarboxylic anhydride was replaced with 3 parts by weight of 2,3-pyrazinedicarboxylic anhydride to obtain nonaqueous electrolyte solution C3 for lithium ion batteries and coin-type battery S3.

[0030] Example 4 A nonaqueous electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 0.5 parts by weight of 2,3-pyridinedicarboxylic anhydride was replaced with 5 parts by weight of 4,5-pyridazinedicarboxylic anhydride to obtain nonaqueous electrolyte solution C4 for lithium ion batteries and coin-type battery S4.

[0031] Example 5 A nonaqueous electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 0.5 parts by weight of 2,3-pyridinedicarboxylic anhydride was replaced with 0.05 parts by weight of 2,3-pyridinedicarboxylic anhydride to obtain nonaqueous electrolyte solution C5 for lithium-ion batteries and coin-type battery S5.

[0032] Example 6 A nonaqueous electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 0.5 parts by weight of 2,3-pyridinedicarboxylic anhydride was replaced with 0.1 parts by weight of 2,3-pyridinedicarboxylic anhydride to obtain nonaqueous electrolyte solution C6 for lithium ion batteries and coin-type battery S6.

[0033] Example 7 A non-aqueous electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that 12 parts by weight of 2,3-pyridinedicarboxylic anhydride was added in step (1) to obtain electrolyte solution C7 for lithium-ion batteries.

[0034] Comparative Example 1 An electrolyte solution was prepared and a coin-type battery was manufactured in the same steps as in Example 1. In comparison with Example 1, the only difference is that in step (1), 2,3-pyridinedicarboxylic anhydride was not used to obtain a nonaqueous electrolyte solution DC1 for lithium-ion batteries and a coin-type battery DS1.

[0035] Comparative Example 2 A non-aqueous electrolyte was prepared in the same manner as in Example 1, a coin-type battery was manufactured, and compared with Example 1, The difference is that in step (1), 2,3-pyridinedicarboxylic anhydride is replaced with maleic anhydride to obtain the lithium-ion battery electrolyte DC2 and the coin-type battery DS2.

[0036] Comparative Example 3 An electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 2,3-pyridinedicarboxylic anhydride was replaced with pyridine to obtain lithium-ion battery electrolyte solution DC3 and coin-type battery DS3.

[0037] Comparative Example 4 An electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 2,3-pyridinedicarboxylic anhydride was replaced with pyrazine to obtain lithium-ion battery electrolyte DC4 and coin-type battery DS4.

[0038] Comparative Example 5 An electrolyte solution was prepared in the same steps as in Example 1, and a coin-type battery was manufactured. Compared to Example 1, this example differs in that in step (1), 2,3-pyridinedicarboxylic anhydride was replaced with pyridazine to obtain lithium-ion battery electrolyte DC5 and coin-type battery DS5.

[0039] Test Example (1) Oxidative decomposition potential measurement Using the three-electrode measurement method, a platinum plate is used as the working electrode, a lithium plate is used as the reference electrode, and C1 to C7 prepared in the examples and DC1 to DC5 prepared in the comparative examples are used as the electrolyte to assemble a battery, and the polymerization potential of the additive and the oxidative decomposition potential of the electrolyte are characterized. The measurement results are shown in Table 1.

[0040] (2) Battery charge / discharge performance test The coin type batteries S1 to S7 and DS1 to DS5 were charged at a constant current of 0.1 mA at room temperature to 4.95 V, and then discharged at a constant current of 0.1 mA to 2.8 V. The discharge capacity and charge capacity of the batteries were recorded, and the charge / discharge rate was calculated according to the formula: charge / discharge efficiency (%) = charge capacity / discharge capacity × 100%. The test results are shown in Table 2.

[0041] (3) Battery cycle test The battery is charged at a constant current and constant voltage of 1C rate (about 0.5mA) at room temperature to 4.95V, the charge cutoff current is 0.05mA, and then discharged at a constant current of 0.5mA to 2.8V to complete one cycle. The initial charge capacity and the initial discharge capacity are recorded, and the charge / discharge efficiency (%) is calculated. After repeating the charge / discharge cycle 100 times, the discharge capacity of the 100th cycle is recorded, and the capacity retention after cycling is calculated according to the formula: Capacity retention after cycling (%) = Discharge capacity after 100 cycles / Initial discharge capacity × 100%, and the cutoff voltage is set to 4.95V. The test results are shown in Table 3. [Table 1] [Table 2] [Table 3]

[0042] As can be seen from the data in Tables 1 to 3, the present disclosure effectively inhibits the decomposition of the electrolyte by adding a pyridinedicarboxylic anhydride additive to the electrolyte for lithium ion batteries, and improves the high temperature stability of the lithium ion battery, thereby extending the service life of the battery.

[0043] The present disclosure is as above. Fruit Although the embodiments have been described in detail, the present disclosure is not limited to the specific contents of the above embodiments, and within the technical spirit of the present disclosure, several simple modifications can be made to the technical solutions of the present disclosure, all of which fall within the scope of protection of the present disclosure.

[0044] It should be noted that the specific technical features described in the above specific embodiments may be combined in any suitable manner if not contradictory, and in order to avoid unnecessary duplication, the present disclosure does not separately describe various possible combination manners.

[0045] Furthermore, the various embodiments of the present disclosure can be combined in any manner and should belong to the contents disclosed in the present disclosure, unless they deviate from the concept of the present disclosure.

Claims

1. An electrolyte for a lithium ion battery comprising an organic solvent, a lithium salt, and an additive, the additive comprising a first additive represented by formula (1): 【Chemistry 1】 (In formula (1), X 1 , X 2 , X 3 and X 4 are each independently selected from CR or N, and X 1 , X 2 , X 3 and X 4 At least one of X is N; 1 , X 2 , X 3 and X 4 R is H, halogen, C 1 ~C 4 Alkyl group, C 1 ~C 4 a substituted alkyl group of C 4 ~C 7 a cycloalkyl group of C 1 ~C 3 are each independently selected from the alkoxy groups The electrolyte, wherein the first additive is 3,4-pyridinedicarboxylic anhydride or 4,5-pyridazinedicarboxylic anhydride.

2. X 1 , X 2 , X 3 and X 4 The electrolyte according to claim 1 , wherein R is H.

3. X 1 , X 2 , X 3 and X 4 The electrolyte according to claim 1 , wherein any one or two of the above is N.

4. 2. The electrolyte according to claim 1, wherein the content of the organic solvent is 50 to 90 wt %, the content of the lithium salt is 1 to 20 wt %, and the content of the additive is 0.1 to 10 wt %, based on the total weight of the electrolyte.

5. 5. The electrolyte according to claim 4, wherein the content of the organic solvent is 60 to 85 wt %, the content of the lithium salt is 5 to 15 wt %, and the content of the additive is 0.5 to 8 wt %, based on the total weight of the electrolyte.

6. 2. The electrolyte solution according to claim 1, wherein the content of the first additive in the additive is 30 to 100% by weight based on the total weight of the additive.

7. The electrolyte solution according to claim 6, wherein the content of the first additive in the additive is 50 to 100% by weight based on the total weight of the additive.

8. The electrolytic solution according to claim 1, wherein the organic solvent is at least one selected from the group consisting of ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, ethylene carbonate, propylene carbonate, butylene carbonate, ethylene sulfite, propylene sulfite, diethyl sulfite, γ-butyrolactone, dimethyl sulfoxide, ethyl acetate, and methyl acetate.

9. The lithium salt is LiPF 6 , LiBF 4 , LiClO 4 , LiAsF 6 , LiCF 3 SO 3 , LiN(CF 3 SO 2 ) 2 , LiN (C 2 F 5 SO 2 ) 2 , LiC(CF 3 SO 2 ) 3 and LiB(C 2 O 4 ) 2 The electrolyte according to claim 1, wherein the electrolyte is one or more of the following:

10. The additive further contains a second additive that is the remainder based on the total weight of the additive, and the second additive contains one or more of vinylene carbonate, lithium bis(oxalato)borate, and lithium bis(fluorosulfonylimide). The electrolyte solution according to claim 6 or 7.

11. A lithium ion battery comprising the electrolyte solution according to claim 1.

Citation Information

Patent Citations

  • Electrolytic solution for lithium storage battery and secondary battery using the same

    JP2001307770A

  • Electrolyte liquid and battery

    JP2005347222A

  • A specific lithium battery containing a non-aqueous electrolyte based on a sulfone compound

    JP2017505521A

  • Nonaqueous liquid electrolyte for lithium ion secondary battery

    JP2020047525A

  • Secondary battery

    WO2012147761A1