Method for manufacturing spunbond nonwoven fabric with improved fiber opening quality and no residual harmful substances

By employing bismuth or a bismuth alloy in the frictional charging process, the method addresses the hazards of lead residues in spunbond nonwoven fabrics, achieving improved opening quality and safety for wider material applications.

JP7575576B2Active Publication Date: 2024-10-29KOLON INDUSTRIES INC
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023512353
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-05
Filing Date
2021-08-06
Publication Date
2024-10-29
Estimated Expiration
2041-08-06

AI Technical Summary

Technical Problem

The manufacturing of spunbond nonwoven fabrics using lead as a friction material in the triboelectrification method results in residual lead, which is hazardous and limits its application in life science materials due to potential health risks, while alternative methods like the Dokan system suffer from productivity and cost issues.

Method used

The use of a metal member containing bismuth or a bismuth alloy in the frictional charging process to produce spunbond nonwoven fabrics, which replicates the negative charge donating properties of lead without the health risks, ensuring improved opening quality and eliminating residual harmful substances.

Benefits of technology

The method produces nonwoven fabrics with enhanced opening quality and safety, allowing broader application in both industrial and life science materials, extending the replacement cycle of the friction material and improving operational efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575576000002
    Figure 0007575576000002
  • Figure 0007575576000001
    Figure 0007575576000001
Patent Text Reader

Abstract

The present invention relates to a spunbond nonwoven fabric that is free of harmful residuals and has improved fiber opening quality, as well as a manufacturing method and apparatus for the same. The manufacturing method for the spunbond nonwoven fabric according to the present invention includes a step of colliding a continuous filament bundle with a metal member containing bismuth (Bi) or a bismuth alloy to obtain opened filaments by frictional charging.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a spunbond nonwoven fabric which is free of residual harmful substances and has improved fiber opening quality, and a method and apparatus for producing the same. [Background technology]

[0002] Generally, the manufacturing process of spunbond nonwoven fabrics proceeds in the following order: spinning, cooling, stretching, web formation, bonding, and winding. The spunbonding method, which is carried out as a continuous process, has high productivity and excellent economic properties.

[0003] The manufacturing process of spunbond nonwoven fabrics is divided into Docan system and Reicofil system according to the difference from the spinning process to the drawing process, and is further subdivided according to the filament opening technology for web formation.

[0004] In the Lycofil system, molten polymer discharged from a rectangular spinning pack is spun into a filament curtain through a closed cooling / drawing section, and a web is formed by separation using aerodynamic force or corona charge. The Lycofil system has the advantages of high production volume and fast production speed, and low manufacturing costs for nonwoven fabrics. It is being applied in the fields of sanitary materials, protective clothing, and filters using olefin raw materials such as polyethylene and polypropylene. However, PET has difficulty entering the high value-added market due to its poor mechanical properties and appearance quality.

[0005] In the Dokan system, molten polymer discharged from a circular spin pack passes through an open cooling / drawing section and is fiberized into filament bundles, which are then opened by mechanical force, electrostatic charge, or a combination method to form a web. The Dokan system has excellent mechanical properties and a uniform appearance, making it suitable for high value-added products. However, it has the disadvantage of higher manufacturing costs due to its lower productivity compared to the Lycofil system.

[0006] Under the Dokan system, various spreading methods have been developed, such as forced charging by corona discharge and triboelectric charging by collision with a friction material (e.g., metal). However, even if the spreading of the filament bundle is improved by these spreading methods, there is still a need to improve the unevenness of the areal density of the web (i.e., uneven weight per unit area of ​​the web).

[0007] Meanwhile, the performance of the friction charging method is controlled according to the charging sequence of the friction material. For example, the polyester filaments are made to have a negative charge by friction (collision) between the polyester filaments and the metal plate. The filaments are opened by the Coulomb repulsive force between the filaments that have the same charge due to the friction.

[0008] Lead (Pb) has traditionally been used as the metal plate material in the friction charging method. However, lead is brittle and easily wears away due to friction with filaments. As a result, residual lead may remain in spunbond nonwoven fabrics manufactured using lead as a friction material in the friction charging method.

[0009] Lead (Pb) is one of the six major hazardous substances under the European Union (EU) Restriction of Hazardous Substances (RoHS) guidelines, and has potential risks to human health. As a result, lead (Pb) has permissible limits for different uses in life science materials, and it is currently recommended that it not be used. Summary of the Invention [Problem to be solved by the invention]

[0010] The present invention provides a method for producing a spunbond nonwoven fabric having improved fiber opening quality, using a friction material that has a negative charge donating ability equivalent to that of lead (Pb) but is not harmful to the human body.

[0011] The present invention provides an apparatus for producing the spunbonded nonwoven fabric.

[0012] The present invention provides a spunbond nonwoven fabric that is free of harmful residuals and has improved opening quality. [Means for solving the problem]

[0013] According to one embodiment of the present invention, melt spinning a thermoplastic resin to obtain a continuous filament bundle; impacting the continuous filament bundle against a metal member containing bismuth (Bi) or a bismuth alloy to obtain filaments opened by triboelectric charging; concentrating the spread filaments on a continuous conveyor net to form a fibrous web. A method for producing a spunbond nonwoven fabric is provided, comprising:

[0014] According to another embodiment of the present invention, a plurality of nozzle units arranged and configured to discharge a continuous filament bundle; an impingement unit adjacent each of the nozzle units in a position for impinging with the continuous filament bundle discharged by the nozzle units; and a continuous conveyor net for collecting and transporting the filaments opened by frictional charging with the collision unit, The collision unit includes a collision surface that is a metal member containing bismuth (Bi) or a bismuth alloy. An apparatus for producing a spunbond nonwoven fabric is provided.

[0015] According to yet another embodiment of the present invention, A fibrous web including thermoplastic filaments, having a residual amount of bismuth (Bi) of 0.01 ppmw to 10.0 ppmw; A spunbond nonwoven fabric is provided.

[0016] Hereinafter, a method for producing a spunbonded nonwoven fabric, an apparatus for producing a spunbonded nonwoven fabric, and a spunbonded nonwoven fabric produced by using the apparatus according to an embodiment of the present invention will be described in more detail.

[0017] Unless otherwise defined herein, all technical and scientific terms have the same meaning as commonly understood by a person of ordinary skill in the art to which the present invention belongs. The terms used in the description of the present invention are merely for the purpose of effectively describing a specific embodiment and are not intended to limit the present invention.

[0018] As used herein, the singular forms include the plural forms unless the context clearly dictates to the contrary.

[0019] As used herein, the meaning of "comprising" is to embody certain features, regions, integers, steps, operations, elements, components and / or components, and does not exclude the presence or addition of other certain features, regions, integers, steps, operations, elements, components and / or groups.

[0020] Although the present invention can be modified in various ways and has various forms, specific embodiments are described in detail below. However, it is not intended to limit the present invention to the specific disclosed embodiments, and it should be understood that the present invention includes all modifications, equivalents, and alternatives within the spirit and technical scope of the present invention.

[0021] In this specification, when the positional relationship of two parts is described using, for example, "on," "at the top," "below," "to the side," etc., one or more other parts may be located between the two parts, unless the expressions "directly" or "indirectly" are used.

[0022] In this specification, when a temporal relationship is described using, for example, "after," "next," "after," or "before," the terms "directly" or "indirectly" are not used, and therefore non-consecutive cases may also be included.

[0023] As used herein, the term "at least one" should be understood to include all possible combinations of one or more of the associated items.

[0024] I. Manufacturing method of spunbond nonwoven fabric According to one embodiment of the invention, melt spinning a thermoplastic resin to obtain a continuous filament bundle; impacting the continuous filament bundle against a metal member containing bismuth (Bi) or a bismuth alloy to obtain filaments opened by triboelectric charging; concentrating the spread filaments on a continuous conveyor net to form a fibrous web. A method for producing a spunbond nonwoven fabric is provided, comprising:

[0025] Conventionally, the opening process of the Docan system is controlled by the generation of electrostatic force due to friction between the filament bundle and the lead plate material, and the kinetic energy of the filaments causes the lead plate material to be worn away, leaving trace amounts of lead remaining in the nonwoven fabric.

[0026] However, unlike industrial materials, residual lead can be exposed in consumer materials through the mouth, respiratory system, or skin, and these potential risks have made it difficult to enter the market.

[0027] However, as a result of the inventors' continued research, it was confirmed that when a metal component containing bismuth (Bi) or a bismuth alloy is applied to the friction material in the production of spunbond nonwoven fabric using the Dokan system, it is possible to produce a spunbond nonwoven fabric that exhibits the same level of negative charge donating ability as conventional metal components made of lead (Pb), does not contain residual harmful substances, and has improved fiber opening quality.

[0028] FIG. 1 is a schematic diagram of an apparatus for producing a spunbond nonwoven fabric according to one embodiment of the present invention.

[0029] First, (i) a step is performed in which a thermoplastic resin is melt spun to obtain a continuous filament bundle.

[0030] As the thermoplastic resin, any resin commonly used in the technical field to which the present invention pertains can be used without any particular limitation.

[0031] The thermoplastic resin having a melting point of 200° C. or higher can be advantageous in terms of ensuring the mechanical properties of the filaments.

[0032] Preferably, the thermoplastic resin may be one or more resins selected from the group consisting of polyester, polyamide, polyolefin, and polyphenylene sulfide.

[0033] Specifically, the thermoplastic resin may be one or more resins selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polycyclohexane terephthalate, polyethylene naphthalate, nylon, polyethylene, polypropylene, polybutylene, and polyphenylene sulfide.

[0034] The thermoplastic resin is melted in a continuous extruder having a screw and a heater and continuously extruded through a spinneret to form a continuous filament bundle.

[0035] The continuous filament bundle is drawn by compressed air and an ejector in the cylindrical pipe of the nozzle unit 10 and discharged through a jet nozzle.

[0036] The denier and cross-sectional shape of the filaments constituting the continuous filament bundle are not particularly limited. As a non-limiting example, the filaments may have a denier of 1 to 10 and a circular or irregular cross section.

[0037] Subsequently, a step (ii) is performed in which the continuous filament bundle is collided with a metal member containing bismuth (Bi) or a bismuth alloy to obtain filaments opened by triboelectric charging.

[0038] The step (ii) is a step of inducing frictional charging by the charge sequence between the material of the collision surface and the filament bundle by colliding the continuous filament bundle 11 discharged through the jet nozzle of the nozzle unit 10 with the collision surface of the collision unit 20, and opening the filaments by the Coulomb repulsion between the filaments that now have the same charge.

[0039] In the step (ii), one of the main factors that determine the dispersion form and the spreading quality of the filament bundle 11 is the type of material that forms the collision surface of the collision unit 20.

[0040] Lead (Pb) has traditionally been used as the material for the impact surface of the impact unit 20. However, trace amounts of lead that fall off due to friction with the filaments remain in the nonwoven fabric, which poses a potential risk of harm to the human body.

[0041] According to an approach based on solid-state physics, lead (Pb) is classified as follows: Lead (Pb) has a concentration of 5×10 6With a conductivity of -23.0×10 S / m, lead (Pb) is classified as a conductor among conductors, semiconductors, and non-conductors. -6 cm 3 / mol (at 298K), it is classified as a diamagnetic material among ferromagnetic, paramagnetic, and diamagnetic materials. Lead (Pb) has a melting point of 600.61K (327.46℃, 621.43°F), so it is classified as a low-temperature melt among high-temperature melt and low-temperature melt thermally. And lead (Pb) has a Vickers hardness (Hv) of 8.11, so it is classified as a soft material among hard and soft materials, and as a tough material among brittle and tough materials mechanically.

[0042] According to one embodiment of the invention, the continuous filament bundle 11 is impinged against a metal member containing bismuth (Bi) or a bismuth alloy.

[0043] Bismuth (Bi) is 7.7 x 10 5 It is classified as a "conductor" electrically because it has a conductivity of -280.1×10 -6 cm 3 It is magnetically classified as "diamagnetic" with a magnetic susceptibility of 0.01 µm / mol (at 298 K); thermally classified as "low melt" with a melting point of 544.7 K (271.5 °C, 520.7 °F); and mechanically classified as "soft" and "tough" with a Vickers hardness (Hv) of 11.55.

[0044] Bismuth (Bi) can provide a similar level of negative charge compared to lead (Pb), but is harder and is not classified as a hazardous substance under the European Union's Restriction of Hazardous Substances (RoHS) guidelines.

[0045] Therefore, by applying bismuth or a bismuth alloy to the collision surface of the collision unit 20, a spunbond nonwoven fabric containing no residual harmful substances and having improved fiber opening quality can be obtained.

[0046] Preferably, a metal member made of bismuth can be applied to the collision surface of the collision unit 20 .

[0047] Also, a metal member made of a bismuth alloy can be applied to the collision surface. Preferably, the bismuth alloy contains 10% by weight or more, 20% by weight or more, 30% by weight or more, 40% by weight or more, 45% by weight or more, or 50% by weight or more of bismuth based on the weight of the bismuth alloy, which may be advantageous for the manifestation of the effects of the present invention. Specifically, the bismuth alloy may contain 10% by weight to 80% by weight, 20% by weight to 80% by weight, 20% by weight to 70% by weight, 30% by weight to 70% by weight, 30% by weight to 60% by weight, 40% by weight to 60% by weight, 45% by weight to 60% by weight, or 45% by weight to 55% by weight of bismuth based on the weight of the bismuth alloy.

[0048] The bismuth alloy further includes, in addition to bismuth, a metal that is not a hazardous substance according to the RoHS guidelines and does not impair the properties of bismuth. For example, the bismuth alloy may include one or more metals selected from the group consisting of copper (Cu), zinc (Zn), tin (Sn), aluminum (Al), molybdenum (Mo), and titanium (Ti). As a non-limiting example, the bismuth alloy may include 50% by weight of bismuth (Bi) and 50% by weight of copper (Cu). The metal other than bismuth included in the bismuth alloy can be selected in consideration of the physical properties of the metal, the physical properties to be imparted to the collision surface, and the like.

[0049] According to one embodiment of the invention, the continuous filament bundle 11 can collide with the metal member at a linear velocity of 4,000 m / min to 6,000 m / min, alternatively 4,500 m / min to 6,000 m / min, alternatively 4,500 m / min to 5,500 m / min.

[0050] The continuous filament bundle 11 can collide with the metal member at a mass flow rate of 2.0 kg / hr to 8.0 kg / hr, or 3.0 kg / hr to 8.0 kg / hr, or 3.0 kg / hr to 6.0 kg / hr per nozzle spraying the continuous filament bundle.

[0051] In order to ensure sufficient generation of frictional electrification due to collision with the metal member while also ensuring fiber spreading quality and operability, it is preferable that the continuous filament bundle 11 collide with the metal member within the linear velocity range and mass flow rate range.

[0052] According to one embodiment of the invention, the filaments 22 opened by the frictional charging may have a charge generation amount (measured by the Faraday cage method) of -3500nC / sec to -500nC / sec, or -3400nC / sec to -600nC / sec, or -3400nC / sec to -700nC / sec.

[0053] The filaments 22 spread by the frictional charging have the amount of charge generated within the above range, and are spread with a wide spread width and excellent quality.

[0054] The amount of charge generated by the spread filaments 22 is the amount of electrostatic discharge generated by the filaments due to collision with the metal member, and can be measured using a Faraday cage method.

[0055] The Faraday cage is divided into an inner cage and an outer cage. The insulated inner cage is installed to confine the filaments 22 that collide with the metal member and are opened. The grounded outer cage is installed to surround the entire surface of the inner cage. A digital coulomb meter is placed in contact with the inner cage. The time it takes for the charge difference between the inner cage and the outer cage to reach -9,000 nC is measured with the digital coulomb meter and normalized by time to obtain the amount of electrostatic discharge of the opened filaments.

[0056] According to one embodiment of the invention, the jet nozzle for spraying the filament bundle in step (ii) is connected to a shaft of a step motor and can be controlled at a nozzle rotation angle range of -15±5° to +15±5° and a nozzle reciprocating speed of 3 counter / sec to 12 counter / sec.

[0057] Subsequently, a step (iii) is performed of converging the opened filaments 22 onto a continuous conveyor net 30 to form a fibrous web 33.

[0058] The filaments, which have become negatively charged by the frictional charging, are opened by the Coulomb repulsion between the filaments and fall below the metallic continuous conveyor net 30. The negatively charged filaments are placed on the grounded conveyor net 30 by electrostatic force to form a fiber web 33.

[0059] According to one embodiment of the invention, the spread filaments 22 can be concentrated on the continuous conveyor net 30 with a spread width of 500 mm or more under conditions of a rotation angle range of -15±5° to +15±5° of the nozzle spraying the filament bundle and a reciprocating speed of the nozzle of 3 counter / sec to 12 counter / sec.

[0060] In order to ensure excellent spreading quality, the spread width of the spread filaments 22 is preferably 500 mm or more. Preferably, the spread width may be 500 mm or more, or 500 mm to 700 mm, or 500 mm to 650 mm, or 520 to 650 mm.

[0061] Here, the spread width refers to the maximum width based on the moving direction of the spread filaments 22 gathered on the continuous conveyor net 30. The spread width is based on the value indicated by the spread filaments obtained from one nozzle unit and the corresponding collision unit.

[0062] The fibrous web is then bonded, for example by thermal bonding, to obtain the spunbonded nonwoven fabric. The bonding is carried out using a calendar roll or an embossing roll.

[0063] II. Spunbond nonwoven fabric manufacturing equipment According to another embodiment of the invention, a plurality of nozzle units 10 configured and arranged to deliver a continuous filament bundle 11; an impingement unit 20 adjacent each of the nozzle units 10 in a position for impingement with the continuous filament bundle 11 discharged by the nozzle units 10; and a continuous conveyor net 30 for collecting and transporting the filaments 22 opened by frictional charging with the collision unit 20. The collision unit 20 includes a collision surface that is a metal member containing bismuth (Bi) or a bismuth alloy. An apparatus for producing a spunbond nonwoven fabric is provided.

[0064] The spunbond nonwoven fabric manufacturing apparatus is used to carry out the above-mentioned "I. Method for manufacturing spunbond nonwoven fabric".

[0065] FIG. 1 is a schematic diagram of an apparatus for producing a spunbond nonwoven fabric according to one embodiment of the present invention.

[0066] A spunbond nonwoven manufacturing apparatus according to an embodiment of the invention includes a plurality of nozzle units 10 configured and arranged to discharge a continuous filament bundle 11.

[0067] The thermoplastic resin raw material is melted in a continuous extruder (not shown in FIG. 1) having a screw and a heater, and is continuously extruded through a spinneret to form a continuous filament bundle.

[0068] The nozzle unit 10 includes a cylindrical pipe connected to the spinneret and a jet nozzle formed on one side of the cylindrical pipe.

[0069] The continuous filament bundle is discharged through a jet nozzle while being stretched by compressed air and an ejector in the cylindrical pipe of the nozzle unit 10.

[0070] The jet nozzle is connected to the shaft of a step motor and controlled within a nozzle rotation angle range of -15±5° to +15±5° and a nozzle reciprocating speed of 3 counter / sec to 12 counter / sec.

[0071] The jet nozzle can discharge the continuous filament bundle 11 at a linear velocity of 4,000 m / min to 6,000 m / min, alternatively 4,500 m / min to 6,000 m / min, alternatively 4,500 m / min to 5,500 m / min.

[0072] The continuous filament bundle 11 can collide with the metal member of the collision unit 20 at a mass flow rate of 2.0 kg / hr to 8.0 kg / hr, or 3.0 kg / hr to 8.0 kg / hr, or 3.0 kg / hr to 6.0 kg / hr per jet nozzle that sprays the continuous filament bundle.

[0073] A spunbond nonwoven fabric manufacturing apparatus according to an embodiment of the invention includes collision units 20 adjacent to each of the nozzle units 10 in a position for collision with the continuous filament bundles 11 discharged by the nozzle units 10.

[0074] The collision unit 20 includes a collision surface that is a metal member containing bismuth (Bi) or a bismuth alloy. The collision surface refers to a surface of the collision unit 20 that directly collides with the continuous filament bundle 11.

[0075] Preferably, a metal member made of bismuth can be applied to the collision surface of the collision unit 20 .

[0076] Also, a metal member made of a bismuth alloy can be applied to the collision surface. Preferably, the bismuth alloy contains 10% by weight or more, 20% by weight or more, 30% by weight or more, 40% by weight or more, 45% by weight or more, or 50% by weight or more of bismuth based on the weight of the bismuth alloy, which may be advantageous for the manifestation of the effects of the present invention. Specifically, the bismuth alloy may contain 10% by weight to 80% by weight, 20% by weight to 80% by weight, 20% by weight to 70% by weight, 30% by weight to 70% by weight, 30% by weight to 60% by weight, 40% by weight to 60% by weight, 45% by weight to 60% by weight, or 45% by weight to 55% by weight of bismuth based on the weight of the bismuth alloy.

[0077] The bismuth alloy further contains, in addition to bismuth, a metal that is not a hazardous substance according to the RoHS guidelines and does not impair the properties of bismuth. For example, the bismuth alloy may contain one or more metals selected from the group consisting of copper (Cu), zinc (Zn), tin (Sn), aluminum (Al), molybdenum (Mo), and titanium (Ti). As a non-limiting example, the bismuth alloy may contain 50% by weight of bismuth (Bi) and 50% by weight of copper (Cu). The metal other than bismuth contained in the bismuth alloy can be selected in consideration of the physical properties of the metal, the physical properties to be imparted to the collision surface, and the like.

[0078] The collision unit 20 can be positioned to collide with the continuous filament bundle 11 discharged by the nozzle unit 10 at a predetermined angle such that the filaments 22 opened by frictional charging are collected on a continuous conveyor net 30.

[0079] The spunbond nonwoven fabric manufacturing apparatus according to an embodiment of the invention includes a continuous conveyor net 30 that collects and transports the filaments 22 that have been opened by frictional charging with the collision unit 20.

[0080] The continuous conveyor net 30 is preferably grounded, so that the opened filaments 22, which have become negatively charged due to frictional charging with the collision unit 20, can be deposited on the continuous conveyor net 30 by electrostatic forces.

[0081] The continuous conveyor net 30 continuously transports a fibrous web 33 formed by collecting the opened filaments 22 .

[0082] In addition, the spunbond nonwoven fabric manufacturing apparatus according to the embodiment of the present invention may include a bonding unit for adjusting and bonding the fiber web 33 to a predetermined thickness.

[0083] The bonding unit may have a conventional configuration, such as a calender roll and an embossing roll, used in the art for bonding nonwoven fabrics.

[0084] III. Spunbond nonwoven fabric According to yet another embodiment of the invention, Obtained by the above-mentioned production method, A fibrous web including thermoplastic filaments, Having a residual amount of bismuth (Bi) of 0.01 ppmw to 10.0 ppmw; A spunbond nonwoven fabric is provided.

[0085] The spunbond nonwoven fabric may be obtained by the above-mentioned "I. Method for producing spunbond nonwoven fabric".

[0086] The spunbond nonwoven fabric may be obtained using the above-mentioned "II. Spunbond nonwoven fabric manufacturing apparatus."

[0087] According to an embodiment of the invention, a spunbond nonwoven fabric comprises a fibrous web that includes thermoplastic filaments.

[0088] The thermoplastic resin filaments are obtained by using a thermoplastic resin.

[0089] As the thermoplastic resin, any resin commonly used in the technical field to which the present invention pertains can be used without any particular limitation.

[0090] The thermoplastic resin having a melting point of 200° C. or higher can be advantageous in terms of ensuring the mechanical properties of the filaments.

[0091] Preferably, the thermoplastic resin may be one or more resins selected from the group consisting of polyester, polyamide, polyolefin, and polyphenylene sulfide.

[0092] Specifically, the thermoplastic resin may be one or more resins selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polycyclohexane terephthalate, polyethylene naphthalate, nylon, polyethylene, polypropylene, polybutylene, and polyphenylene sulfide.

[0093] The denier and cross-sectional shape of the thermoplastic resin filament are not particularly limited. As a non-limiting example, the filament may have a denier of 1 to 10 and a circular or irregular cross section.

[0094] In order to ensure excellent mechanical properties, the spunbond nonwoven fabric has a density of 20 to 150 g / m 2 , or 50 to 120 g / m 2 The weight per unit area may be 1.0 to 1.0 mm.

[0095] In particular, the spunbond nonwoven fabric obtained by the above-mentioned "I. Manufacturing method of spunbond nonwoven fabric" is substantially free of residual harmful substances such as lead (Pb) and can exhibit improved fiber opening quality.

[0096] According to one embodiment of the invention, the spunbond nonwoven fabric may have a residual amount of lead (Pb) of 0.1 ppmw (ppm by weight) or less. Preferably, the spunbond nonwoven fabric does not contain residual lead.

[0097] According to one embodiment of the invention, the spunbond nonwoven fabric includes filaments that are opened by collision with a metal member containing bismuth (Bi) or a bismuth alloy, and may have a residual amount of bismuth (Bi) of 0.01 ppmw to 10.0 ppmw, alternatively 0.05 ppmw to 5.0 ppmw, alternatively 0.1 ppmw to 2.5 ppmw.

[0098] In the spunbond nonwoven fabric, the residual amount of metals other than bismuth contained in the bismuth alloy may be 0.1 ppmw or less. The bismuth alloy may include one or more metals selected from the group consisting of copper (Cu), zinc (Zn), tin (Sn), aluminum (Al), molybdenum (Mo), and titanium (Ti).

[0099] According to one embodiment of the invention, the spunbond nonwoven fabric may have a quality index (Q) of 350 or less, as defined by the following formula 1:

[0100] [Formula 1] Quality index (Q)=SD / OD

[0101] In the above formula 1, OD is the optical density of the spunbond nonwoven fabric as measured using a formation tester; SD is the standard deviation of the optical density (OD).

[0102] The optical density (OD) is a value obtained by the transmittance of a light source per unit area of ​​the spunbond nonwoven fabric and the distribution of the transmittance. The quality index (Q) is a value obtained by standardizing the standard deviation (SD) of the optical density by the optical density (OD). The OD and SD are obtained using a standard quality evaluation device in the technical field to which the present invention belongs.

[0103] In order to ensure uniform and excellent quality, the spunbonded nonwoven fabric preferably has the quality index (Q) of not more than 350. More preferably, the quality index (Q) of the spunbonded nonwoven fabric may be 250-350, or 270-350, or 275-300. Effect of the Invention

[0104] According to the present invention, a method and apparatus for producing a spunbond nonwoven fabric with improved fiber opening quality is provided using a friction material that has the same level of negative charge donating ability as lead (Pb) but is not harmful to the human body. The apparatus allows the replacement cycle of the friction material to be extended, which contributes to improving operability. The spunbond nonwoven fabric produced by the apparatus and method does not contain residual harmful substances and has improved fiber opening quality, and can be applied to industrial materials as well as life science materials, eliminating potential risks of harmfulness to the human body. [Brief description of the drawings]

[0105] [Figure 1] 1 is a schematic diagram of a spunbond nonwoven fabric manufacturing apparatus according to one embodiment of the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0106] Preferred examples are presented below for better understanding of the invention. However, the following examples are merely for illustrating the present invention and are not intended to limit the present invention thereto.

[0107] Example 1 A spunbond nonwoven fabric was produced using the apparatus according to FIG.

[0108] First, it has an intrinsic viscosity (IV) of 0.665 dl / g and a melting point (T m ) was melted at 284°C and continuously extruded. The filament bundle obtained by the extrusion was extruded through an EDJ nozzle (electric distribution jet nozzle) while being stretched at a speed of 5,000 m / min using compressed air and an ejector in a cylindrical pipe of a nozzle unit. The EDJ nozzle was connected to the shaft of a step motor, and the rotation angle range of the nozzle was controlled to -15±5° to +15±5° and the reciprocating speed of the nozzle was controlled to 10 counter / sec.

[0109] The discharged filament bundle collided at the above speed with a collision unit positioned adjacent to the nozzle unit at a predetermined angle. A metal member (metal plate having a thickness of 2.0±0.15 mm) made of bismuth (Bi) was used as the collision surface of the collision unit. At this time, the mass flow rate of the filaments colliding with the metal member was 5.0 kg / hr per nozzle spraying the continuous filament bundle, and the linear velocity of the filaments was controlled to 5,000 m / min.

[0110] The filaments, which have become negatively charged due to frictional charging with the collision unit, fall downward to the conveyor net while being opened by the Coulomb repulsion between the filaments. The negatively charged filaments are fixed by electrostatic forces on the grounded continuous conveyor net to form a fibrous web.

[0111] The fiber web was passed between calendar rollers maintained at 130°C and 35 N / mm to obtain a suitable thickness. Next, hot air was applied to the fiber web to thermally bond it to obtain a spunbond nonwoven fabric (thickness 0.27±0.03 mm, weight 60±2.0 g / m2). 2 ) was obtained.

[0112] Example 2 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of a bismuth / copper alloy (Bi 50 wt %, Cu 50 wt %) was used on the collision surface of the collision unit instead of the bismuth metal member.

[0113] Comparative Example 1 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of lead (Pb) was applied to the collision surface of the collision unit instead of the bismuth metal member.

[0114] Comparative Example 2 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of copper (Cu) was used on the collision surface of the collision unit instead of the bismuth metal member.

[0115] Comparative Example 3 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of tin (Sn) was used on the collision surface of the collision unit instead of the bismuth metal member.

[0116] Comparative Example 4 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of aluminum (Al) was applied to the collision surface of the collision unit instead of the bismuth metal member.

[0117] Comparative Example 5 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of zinc (Zn) was applied to the collision surface of the collision unit instead of the bismuth metal member.

[0118] Comparative Example 6 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of molybdenum (Mo) was used on the collision surface of the collision unit instead of the bismuth metal member.

[0119] Comparative Example 7 A spunbond nonwoven fabric was obtained in the same manner as in Example 1, except that a metal member made of titanium (Ti) was applied to the collision surface of the collision unit instead of the bismuth metal member.

[0120] Test Example (1) Charge generation amount (nC / sec) The amount of electrostatic discharge per unit time of the opened filaments was measured using a Faraday cage method.

[0121] The Faraday cage is divided into an inner cage and an outer cage. The insulated inner cage is installed so that it collides with the metal member and traps the spread filaments 22. The grounded outer cage is installed so as to surround the entire surface of the inner cage. A digital coulomb meter (NK-1002, KASUGA DENKI, Inc.) is placed in contact with the inner cage. The time it takes for the charge difference between the inner cage and the outer cage to reach -9,000 nC is measured with the digital coulomb meter and normalized by time to obtain the average amount of electrostatic discharge per unit time possessed by the spread filaments.

[0122] (2) Spreading width (mm) The spread width formed by the filaments spread by frictional charging with the collision unit was measured. Here, the spread width means the maximum width based on the moving direction of the spread filaments converged on the continuous conveyor net. The spread width is based on the value indicated by the spread filaments obtained from one nozzle unit and its corresponding collision unit. The spread width was shown as an average value after 10 measurements under the conditions of a rotation angle range of the EDJ nozzle of -15±5° to +15±5° and a reciprocating speed of the EDJ nozzle of 10 counters / sec.

[0123] (3) Quality index (Q) Using a quality evaluation device (Formation tester, FMT-III, manufactured by NOMURA SHOJI CO.), the optical density (OD) and the standard deviation (SD) of the optical density were measured based on the transmittance of the light source per unit area of ​​the spunbond nonwoven fabric and the distribution of the transmittance. The quality index was calculated using the above formula 1.

[0124] The quality evaluation device (FMT-III) is an image analysis type quality analyzer using a two-dimensional CCD camera. A nonwoven fabric sample is placed on a stage illuminated from below. The CCD camera captures an image of 320x230 pixels, and the light intensity is measured by each pixel. A PC linked to the CCD camera converts the light intensity into transmittance (%) and optical density (OD).

[0125] (4) Use period of metal parts (days) In the manufacturing process of a spunbond nonwoven fabric, the time when perforations in the thickness direction occurred in a metal member (metal plate having a thickness of 2.0±0.15 mm) included in a collision unit, or the time when operability decreased due to the occurrence of unevenness caused by wear, was measured. At this time, the mass flow rate of the filaments colliding with the metal member was 5.0 kg / hr per nozzle spraying the continuous filament bundle, and the linear velocity of the filaments was controlled in the range of 5,000 m / min.

[0126] (5) Inorganic residue amount (ppmw) The amount of residual inorganic matter in spunbond nonwoven fabric was measured using inductively coupled plasma (ICP). Spunbond nonwoven fabric specimens were pretreated with an aqueous solution that had been used to remove particles and organic matter using an acid digestion method. The amount of residual inorganic matter in the specimens was initially measured using inductively coupled plasma-atomic emission spectrometry (ICP-AES), and when no residual inorganic matter was detected, it was remeasured using inductively coupled plasma-mass spectrometry (ICP-MS) to improve resolution.

[0127] [Table 1]

[0128] Referring to Table 1, Comparative Example 1 was excellent in quality index and spread width, but residual lead was detected in the nonwoven fabric, making it unsuitable for use in life science materials.

[0129] In the examples, no residual harmful substances were detected in the nonwoven fabric, while the quality index and spread width were at the same levels as those in comparative example 1. In addition, the metal members applied to the examples had a usage cycle that was approximately twice as long as that of comparative example 1, and it was confirmed that the operability was significantly improved.

[0130] In Comparative Examples 2 and 3, the amount of inorganic substances remaining in the nonwoven fabric was low, but the quality index and spread width were poor. In Comparative Examples 4 to 7, no inorganic substances remaining in the nonwoven fabric were detected, but it was confirmed that the filament spread was poor. [Explanation of symbols]

[0131] 10: Nozzle unit 11: Filament bundle 20: Collision unit 22: Open filament 30: Conveyor net 33: Fiber web

Claims

1. melt spinning a thermoplastic resin to obtain a continuous filament bundle; impacting the continuous filament bundle against a metal member containing bismuth (Bi) or a bismuth alloy to obtain filaments opened by triboelectric charging; concentrating the spread filaments on a continuous conveyor net to form a fibrous web; Including, The continuous filament bundle is collided with the metal member at a linear speed of 4,000 m / min to 6,000 m / min and at a mass flow rate of 2.0 kg / hr to 8.0 kg / hr per nozzle spraying the continuous filament bundle.

2. The method for producing a spunbond nonwoven fabric according to claim 1 , wherein the bismuth alloy contains 10% by weight or more of bismuth based on the weight of the bismuth alloy.

3. 2. The method for producing a spunbond nonwoven fabric according to claim 1, wherein the bismuth alloy contains one or more metals selected from the group consisting of copper (Cu), zinc (Zn), tin (Sn), aluminum (Al), molybdenum (Mo), and titanium (Ti).

4. The method for producing a spunbond nonwoven fabric according to claim 1, wherein the opened filaments have a charge generation amount due to the frictional charging of -3500 nC / sec to -500 nC / sec (a value measured by a Faraday cage method).

5. 2. The method for producing a spunbonded nonwoven fabric according to claim 1, wherein the spread filaments are focused on the continuous conveyor net with a spread width of 500 mm or more under conditions of a rotation angle range of −15±5° to +15±5° of a nozzle spraying the filament bundle and a reciprocating speed of the nozzle of 3 counters / sec to 12 counters / sec (here, the spread width means a maximum width based on the moving direction of the spread filaments focused on the continuous conveyor net).

6. The thermoplastic resin has a melting point of 200° C. or higher, The thermoplastic resin is one or more resins selected from the group consisting of polyester, polyamide, polyolefin, and polyphenylene sulfide. A method for producing the spunbond nonwoven fabric according to claim 1.

7. 2. The method for producing a spunbonded nonwoven fabric according to claim 1, wherein the thermoplastic resin is one or more resins selected from the group consisting of polyethylene terephthalate, polybutylene terephthalate, polycyclohexane terephthalate, polyethylene naphthalate, nylon, polyethylene, polypropylene, polybutylene, and polyphenylene sulfide.

Citation Information

Patent Citations

  • Opening of continuous filament group

    JP1985119258A

  • Pad of air bag device and its manufacture

    JP1992078744A

  • Production of nonwoven fabric and equipment therefor

    JP1993093353A

  • Filament web making machine

    JP1994248556A

  • Production of web for broad nonwoven fabric

    JP1995268753A