Secondary battery cell and method of manufacturing same

The secondary battery cell with spaced coating portions on separation membranes and a manufacturing process addresses gas trapping issues, ensuring effective gas discharge and maintaining performance by using a gas adsorbent and adhesive binder, thus enhancing battery capacity and output.

JP7575593B2Active Publication Date: 2024-10-29LG ENERGY SOLUTION LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023524434
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-08-11
Filing Date
2022-08-11
Publication Date
2024-10-29
Estimated Expiration
2042-08-11

AI Technical Summary

Technical Problem

Secondary batteries experience gas trapping during the activation process, leading to deformation and performance issues due to insufficient gas discharge, especially from the central portion, affecting capacity and output.

Method used

A secondary battery cell design featuring separation membranes with spaced coating portions containing a gas adsorbent and adhesive binder, allowing gas adsorption and discharge through uncoated areas, combined with a manufacturing process that includes rolling to facilitate gas expulsion.

Benefits of technology

The design minimizes gas trapping, maintains performance by ensuring adhesive strength, and prevents capacity deterioration by effectively discharging generated gas, enhancing overall battery efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575593000002
    Figure 0007575593000002
  • Figure 0007575593000003
    Figure 0007575593000003
  • Figure 0007575593000004
    Figure 0007575593000004
Patent Text Reader

Abstract

The present invention relates to a secondary battery cell and a manufacturing method thereof. The secondary battery cell according to one aspect of the present invention is a secondary battery cell having at least one anode and at least one cathode alternately stacked with separators sandwiched therebetween, wherein at least one of the separators has a plurality of spaced-apart coating portions formed on at least one surface thereof, the coating portions including a mixture of a gas adsorbent and an adhesive binder. The secondary battery cell and manufacturing method thereof according to the present invention can minimize the amount of gas trapped inside the secondary battery cell and ensure adhesion between the separator and the electrodes.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a cell for a secondary battery and a method for manufacturing the same.

[0002] This application claims priority to Korean Patent Application No. 2021-0106329 filed on August 11, 2021, the entire contents of which are incorporated herein by reference in their entirety in the specification and drawings of that application. [Background technology]

[0003] Recently, interest in energy storage technology has been increasing. In particular, the fields of application are expanding to include energy for mobile phones, camcorders, notebook PCs, and even electric vehicles, and efforts in research and development of electrochemical devices are gradually being made. Electrochemical devices are the field that has attracted the most attention in this regard, and among them, secondary batteries having high energy density are becoming the focus of attention.

[0004] Typically, in terms of battery shape, there is high demand for prismatic batteries and pouch-type batteries that are thin and therefore applicable to products such as mobile phones, and in terms of materials, there is high demand for lithium secondary batteries that have high energy density, discharge voltage, and output stability.

[0005] Generally, secondary batteries are manufactured through an assembly process and an activation process. In the assembly process, the negative electrode, the positive electrode, and the separator are laminated, and then an electrolyte is injected and the battery case is sealed. The activation process includes a step of performing a process such as charging and discharging under conditions required for activation, but a large amount of gas is generated inside the secondary battery during the activation process.

[0006] If the generated gas is not removed, it will be trapped inside the secondary battery and occupy a certain amount of space, causing the center of the secondary battery to swell and deforming the battery, adversely affecting its performance, such as capacity and output, and its lifespan.

[0007] In order to remove gas generated during the activation process of a secondary battery, a degassing process is usually performed in which the battery case is opened to discharge the gas, and the gas discharge area is then sealed by heat welding. However, even after the degassing process, gas remains trapped inside the secondary battery. In particular, it is difficult to discharge gas from the center of the thickness direction of the secondary battery, so it takes a long time to discharge, and there is a problem that the gas cannot be discharged even by the degassing process. Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention provides a cell for a secondary battery that adsorbs gas generated inside the secondary battery and discharges unadsorbed gas to the outside, thereby minimizing gas trapped inside the secondary battery, and a method for manufacturing the same.

[0009] Another object of the present invention is to provide a cell for a secondary battery capable of ensuring adhesion between an electrode and a separator, and a manufacturing method thereof.

[0010] However, the technical problems that the present invention aims to solve are not limited to the problems described above, and other problems not mentioned will be clearly understood by those skilled in the art from the description of the invention below. [Means for solving the problem]

[0011] The present inventors have found that the above problems can be solved by the following secondary battery cell and manufacturing method thereof.

[0012] The first embodiment is A secondary battery cell in which at least one negative electrode and at least one positive electrode are alternately stacked with a separator sandwiched therebetween, At least one of the separation membranes has a plurality of coating portions formed on at least one surface thereof and spaced apart from each other, The coating portion includes a mixture of a gas adsorbent and an adhesive binder.

[0013] The second embodiment is the same as the first embodiment, The present invention relates to a cell for a secondary battery, wherein the gas adsorbent contains silica gel, carbon fiber, a porous carbon material, a porous metal oxide, a porous gel, a zeolite, or two or more of these.

[0014] The third embodiment is the first or second embodiment, The adhesive binder is selected from the group consisting of polyvinylidene fluoride, styrene butadiene rubber, polytetrafluoroethylene, polyethylene glycol, polypropylene glycol, toluene diisocyanate, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, ethylene-co-vinyl acetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxymethyl cellulose, acrylonitrile-styrene-butadiene copolymer, polyimide, and two or more thereof.

[0015] A fourth embodiment is any one of the first to third embodiments, The present invention relates to a cell for a secondary battery, wherein the total area of ​​the coating portions formed to be spaced apart from each other on at least one surface of the separator is in the range of 20% to 50% relative to 100% of the total area of ​​one surface of the separator.

[0016] A fifth embodiment is any one of the first to fourth embodiments, The present invention relates to a cell for a secondary battery, wherein the coating portions formed on at least one surface of the separator and spaced apart from each other are spaced apart from each other by a distance of 1 to 20 mm.

[0017] A sixth embodiment is any one of the first to fifth embodiments, The separator having the coating portion is located at a center portion in a thickness direction of the secondary battery cell.

[0018] The seventh embodiment is: (S1) assembling a secondary battery cell by stacking at least one positive electrode and at least one negative electrode alternately with a separator therebetween; (S2) pressing and rolling the surface of the secondary battery cell at least once using a roller; At least one of the separators has a plurality of coating portions spaced apart from one another by coating at least one surface of the separator with a mixture of a gas adsorbent and an adhesive binder.

[0019] The eighth embodiment is the seventh embodiment, The coating unit is formed by coating the mixture of the gas adsorbent and the adhesive binder by a spray method.

[0020] The ninth embodiment is the seventh or eighth embodiment, The gas adsorbent includes silica gel, carbon fiber, a porous carbon material, a porous metal oxide, a porous gel, a zeolite, or two or more of these.

[0021] A tenth embodiment is any one of the seventh to ninth embodiments, The separator having the coating portion is located at a center portion in a thickness direction of the secondary battery cell.

[0022] An eleventh embodiment is any one of the seventh to tenth embodiments, The step (S2) pressing and primarily rolling a surface of the secondary battery cell using a roller; and then, after aging the primary-rolled secondary battery cell, pressing a surface of the secondary battery cell using a roller and performing a secondary rolling.

[0023] A twelfth embodiment relates to a method for manufacturing a cell for a secondary battery, characterized in that, in any one of the seventh to eleventh embodiments, a degassing process is performed after the step (S2). Effect of the Invention

[0024] The cell for a secondary battery according to the present invention can adsorb gas generated inside the secondary battery by including a plurality of coating parts containing a mixture of a gas adsorbent and an adhesive binder on one side of at least one separator. In addition, the plurality of coating parts are formed spaced apart from each other, so that unadsorbed gas can be discharged to the outside from the part where the coating parts are not formed. As a result, the cell for a secondary battery according to the present invention can minimize gas trapped inside the secondary battery and prevent deterioration of the performance and capacity of the secondary battery.

[0025] In addition, the coating portion formed on one surface of the separator contains an adhesive binder, thereby ensuring adhesion between the electrode and the separator.

[0026] The following drawings attached to this specification are for illustrating preferred embodiments of the present invention, and serve to further understand the technical idea of ​​the present invention together with the detailed description of the invention, so the present invention should not be interpreted as being limited to only the matters described in the drawings. In addition, the shape, size, scale, ratio, etc. of the elements in the drawings attached to this specification may be exaggerated in order to emphasize a clearer description. [Brief description of the drawings]

[0027] [Figure 1]1 is a cross-sectional view illustrating a cell for a secondary battery according to an embodiment of the present invention. [Diagram 2] 2 is a cross-sectional view illustrating a separator having a coating portion included in a secondary battery cell according to an embodiment of the present invention; [Diagram 3] 1 is a cross-sectional view showing a schematic diagram of a separator having a mesh pattern coating portion outside the scope of the present invention. [Figure 4] 1 shows the results of gas trapped inside secondary battery cells according to an embodiment and a comparative example of the present invention, as confirmed by an air scanner / full charge decomposition analysis. [Diagram 5] 1 shows the results of measuring the electrical resistance of secondary battery cells according to an embodiment of the present invention and a comparative example using EIS. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0028] Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the attached drawings. Prior to this, the terms and words used in the specification and claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as having meanings and concepts according to the technical ideas of the present invention, in accordance with the principle that the inventor himself can appropriately define the concepts of terms in order to best describe the invention.

[0029] In addition, throughout the specification, when a part "includes" a certain component, this does not mean excluding other components, but means that it may further include other components, unless specifically stated to the contrary.

[0030] The present invention relates to a cell for a secondary battery and a method for manufacturing the same.

[0031] Secondary battery cells The secondary battery cell of the present invention is characterized in that at least one negative electrode and at least one positive electrode are alternately stacked with a separator sandwiched therebetween, at least one of the separators has a plurality of coating portions formed spaced apart from each other on at least one surface, and the coating portions include a mixture of a gas adsorbent and an adhesive binder.

[0032] A structure of a secondary battery cell according to an embodiment of the present invention is shown in Fig. 1. Referring to Fig. 1, a positive electrode 1 and a negative electrode 2 are alternately stacked with a separator 3 interposed therebetween, and at least one of the separators includes a plurality of coating portions 3a formed at a distance from each other.

[0033] In the present invention, a secondary battery cell includes at least one separator including a plurality of coating portions spaced apart from each other on at least one surface of the separator, thereby absorbing gas generated inside the secondary battery and discharging unabsorbed gas to the outside of the secondary battery, thereby minimizing gas trapped inside the secondary battery.

[0034] The coating parts are formed on at least one surface of the separator at a distance from each other. Specifically, the coating parts may be formed on one surface of the separator in a pattern of a plurality of dots at a distance from each other. For example, the dots may be circular, elliptical, rectangular, etc. For example, when the dots are circular, the diameter may be about 1 to 10 mm, when the dots are elliptical, the minor axis may be about 1 to 10 mm, and the major axis may be about 2 to 12 mm, and when the dots are rectangular, the length and width may each be 1 to 10 mm. In addition, the coating parts formed on one surface of the separator at a distance from each other may each have a distance of 1 to 20 mm. The coating parts formed to have a predetermined distance from each other may have a surface area that can sufficiently adsorb gas inside the secondary battery, and may provide a space where gas not adsorbed by each coating part can be located in a non-coated part described later.

[0035] In the present invention, the separation membrane includes an uncoated portion where at least one surface of the separation membrane is exposed. The uncoated portion is a portion where a coating portion is not formed on one surface of the separation membrane. The uncoated portion can serve as a gas exhaust passage through which gas that is not adsorbed by the gas adsorbent in the coating portion can be exhausted to the outside.

[0036] 2, the separation membrane 3 includes a plurality of coating portions 3a spaced apart from one another on at least one surface, and a non-coating portion 3b where no coating portion is formed. Gas 3c that is not adsorbed by the coating portion 3a may be located in the non-coating portion 3b.

[0037] In addition, the non-coated portion 3b may form a path through which gas 3c inside the secondary battery is discharged to the outside of the secondary battery. For example, gas 3c located in the non-coated portion 3b may move to the path indicated by the dotted arrow and be discharged to the outside. Any path indicated by the dotted arrow may be referred to as a gas discharge passage.

[0038] On the other hand, when the coated portions are formed on at least one surface of the separator so as to be connected to each other, the uncoated portions are not preferable because they cannot provide a gas exhaust passage.

[0039] For example, as shown in Fig. 3, when the coating portion 3a is formed in a mesh or lattice pattern, the gas 3c trapped inside the secondary battery cannot be discharged to the outside. The coating portion 3a formed in a mesh or lattice pattern is a form in which a plurality of coating portions formed on a separator are connected to each other, so that the non-coated portion 3b is surrounded by the coating portion 3a. As a result, the non-coated portion 3b cannot function as a gas discharge passage for discharging gas to the outside. Therefore, the gas 3c trapped inside the secondary battery located in the non-coated portion 3b cannot be discharged to the outside, which causes problems in the performance and capacity of the secondary battery.

[0040] In the present invention, a plurality of coating parts formed at a distance from each other on at least one surface of the separator may cover 20% to 50% of the total area of ​​one surface of the separator, which is 100%. By covering an area within this range, the coating parts can sufficiently adsorb gas generated inside the secondary battery, and the non-coated parts can provide a path for discharging gas that is not adsorbed by the coating parts.

[0041] In the present invention, the coating portion includes a mixture of a gas adsorbent and an adhesive binder. The coating portion according to an embodiment of the present invention may further include a solvent or a dispersion medium commonly used in the art.

[0042] Normally, the gas generated inside a secondary battery is hydrogen (H 2 ), carbon monoxide (CO), carbon dioxide (CO 2 ), methane (CH 4 ), acetylene (C 2 H 2 ), ethylene (C 2 H 4 ), ethane (C 2 H 6 ), propylene (C 3 H 6 ), propane (C 3 H 8 The gas adsorbent may be any material capable of adsorbing gas generated inside the secondary battery and having cavities therein, and may be, for example, one or more selected from the group consisting of molecular sieves and metal components having gas adsorption properties.

[0043] In this case, the molecular sieve may include silica gel, carbon fiber, a porous carbon material, a porous metal oxide, a porous gel, a zeolite, or two or more thereof.

[0044] Here, the porous carbon material may be at least one selected from the group consisting of carbon molecular sieves and activated carbon, and the metal material of the porous metal oxide may be at least one selected from the group consisting of zeolite, silica gel, alumina, and molecular sieves.

[0045] In addition, the metal component may be at least one selected from the group consisting of nickel (Ni), platinum (Pt), palladium (Pd), calcium (Ca), strontium (Sr), barium (Ba), thallium (Ti), zirconium (Zr), hafnium (Hf), vanadium (V), niobium (Nb), tantalum (Ta), chromium (Cr), molybdenum (Mo), and tungsten (W).

[0046] The content of the gas adsorbent may be, for example, 10 wt % to 50 wt % based on the total weight of the coating part. When the content is in this range, it is advantageous that the gas is sufficiently adsorbed by the gas adsorbent.

[0047] The adhesive binder is not limited as long as it exhibits adhesive strength with the electrode, and may include polyvinylidene fluoride, styrene butadiene rubber, polytetrafluoroethylene, polyethylene glycol, polypropylene glycol, toluene diisocyanate, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, ethylene-co-vinyl acetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxyl methyl cellulose, acrylonitrile-styrene-butadiene copolymer, polyimide, or two or more of these. For example, using polyvinylidene fluoride as an adhesive binder is advantageous for exhibiting adhesive strength with the electrode.

[0048] The content of the adhesive binder may be, for example, 10 wt % to 50 wt % based on the total weight of the coating part. When contained within this range, it has an advantage that it can act as a binder to prevent the gas adsorbent from being separated on the separation membrane and can exhibit sufficient adhesive strength with the electrode.

[0049] In the present invention, the coating portions formed on at least one surface of the separator at a distance from each other may be coated to a thickness of 0.1 μm to 10 μm, but are not particularly limited thereto. Specifically, the coating portions may be coated to a thickness of 0.5 μm to 10 μm. When the thickness of the coating portions is within the above range, it is possible to secure a passage for discharging unabsorbed gas without significantly affecting the increase in cell thickness. In addition, it is possible to secure sufficient adhesive strength with the electrodes.

[0050] In the present invention, the separator included in the secondary battery cell separates the positive electrode and the negative electrode and provides a passage for ion movement, and any separator commonly used in secondary batteries can be used without any particular limitation.

[0051] Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, an ethylene / methacrylate copolymer, etc., or a laminate structure of two or more layers thereof may be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of a high melting point glass fiber, a polyethylene terephthalate fiber, etc. may be used.

[0052] In addition, in order to ensure heat resistance or mechanical strength, a separator coated with inorganic particles, a binder polymer, or a mixture of inorganic particles and a binder polymer may be used, and may be selectively used as a single layer or multilayer structure. In addition, when a solid electrolyte such as a polymer is used as the electrolyte, the solid electrolyte may also serve as the separator.

[0053] In the present invention, the separator including a plurality of coating portions formed spaced apart on at least one surface of the separator may be stacked at any position within the secondary battery cell, but is preferably stacked at a position where it is difficult to exhaust gas.

[0054] In particular, since a secondary battery cell has a structure in which a separator and an electrode are laminated and stacked, gas is less likely to be discharged from the center in the thickness direction of the cell than from the outermost part. Thus, in order to reduce the amount of gas trapped in the center in the thickness direction of the secondary battery cell, a separator having a coating part may be included in the center in the thickness direction of the secondary battery cell. For example, in a secondary battery cell including three or more separators, at least one of the remaining separators, excluding the separators arranged at the outermost parts of the upper and lower parts, may include a coating part.

[0055] In addition, the separator may include a separator having a coating portion in another portion in addition to the separator included in the central portion. For example, the central portion may refer to a central portion when the thickness direction of the secondary battery cell is divided into thirds or a central portion when the thickness direction of the secondary battery cell is divided into fifths.

[0056] The positive electrode included in the secondary battery cell of the present invention is produced, for example, by applying a mixture of a positive electrode active material, a conductive material, and a binder onto a positive electrode current collector and drying the mixture, and a filler may be further added to the mixture as necessary.

[0057] The positive electrode active material is lithium cobalt oxide (LiCoO 2 ), lithium nickel oxide (LiNiO 2 ) and compounds substituted with one or more transition metals; chemical formula Li 1+x Mn 2-x O 4 (where x is 0 to 0.33), LiMnO 3 , LiMn 2 O 3 , LiMnO 2 Lithium manganese oxides such as lithium copper oxide (Li 2CuO 2 );LiV 3 O 8 , LiV 3 O 4 , V 2 O 5 , Cu 2 V 2 O 7 Vanadium oxides such as LiNi 1-x M x O 2 (wherein M=Co, Mn, Al, Cu, Fe, Mg, B or Ga, and x=0.01 to 0.3); Ni-site type lithium nickel oxide represented by the chemical formula LiMn 2-x M x O 2 (wherein M=Co, Ni, Fe, Cr, Zn or Ta, and x=0.01 to 0.1) or Li 2 Mn 3 MO 8 Lithium manganese oxides represented by the formula (where M=Fe, Co, Ni, Cu, or Zn); LiMn 2 O 4 ;Disulfide compounds;Fe 2 (MoO 4 ) 3 These include, but are not limited to:

[0058] The positive electrode current collector is usually made to a thickness of 3 to 500 μm. There are no particular limitations on the positive electrode current collector, so long as it does not induce chemical changes in the battery and has high conductivity. For example, stainless steel, aluminum, nickel, titanium, baked carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used. The positive electrode current collector may have fine irregularities on its surface to increase the adhesive strength of the positive electrode active material, and may be in various forms such as a film, sheet, foil, net, porous body, foam, nonwoven fabric, etc.

[0059] The conductive material is usually added in an amount of 1 to 50% by weight based on the total weight of the mixture containing the positive electrode active material. There are no particular limitations on the conductive material as long as it does not induce chemical changes in the battery and has conductivity. For example, graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fiber and metal fiber; metal powders such as carbon fluoride, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives may be used.

[0060] The binder is a component that aids in binding the active material and conductive material and binding to the current collector, and is usually added in an amount of 1 to 50% by weight based on the total weight of the mixture including the positive electrode active material. Examples of such binders include polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene terpolymer (EPDM), sulfonated EPDM, styrene-butylene rubber, fluororubber, and various copolymers.

[0061] The filler is selectively used as a component for suppressing the expansion of the positive electrode, does not induce chemical changes in the battery, and is not particularly limited as long as it is a fibrous material, for example, olefin polymers such as polyethylene and polypropylene, glass fiber, carbon fiber, and other fibrous materials.

[0062] The negative electrode included in the secondary battery cell of the present invention is manufactured by applying a negative electrode material onto a negative electrode current collector and drying the applied material, and may further include the above-mentioned components as required.

[0063] The negative electrode current collector is usually made to have a thickness of 3 to 500 μm. Such a negative electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, fired carbon, those with a surface treatment of carbon, nickel, titanium, silver, etc. on the surface of copper or stainless steel, aluminum-cadmium alloy, etc. can be used. Also, similar to the positive electrode current collector, it is possible to form fine irregularities on the surface to strengthen the binding force of the negative electrode active material, and it can be used in various forms such as films, sheets, foils, nets, porous bodies, foams, non-woven fabrics, etc.

[0064] The negative electrode material is, for example, carbon such as graphitizable carbon and graphite-based carbon; Li x Fe 2 O 3 (0 ≦ x ≦ 1), Li x WO 2 (0 ≦ x ≦ 1), Sn x Me 1-x Me’ y O z (Me: Mn, Fe, Pb, Ge; Me’: Al, B, P, Si, Group 1, Group 2, Group 3 elements of the periodic table, halogen; 0 < x ≦ 1; 1 ≦ y ≦ 3; 1 ≦ z ≦ 8) and other metal composite oxides; lithium metal; lithium alloy; silicon-based alloy; tin-based alloy; SnO, SnO 2 , PbO, PbO 2 , Pb 2 O 3 , Pb 3 O 4 , Sb 2 O 3 , Sb 2 O 4 , Sb 2 O 5 , GeO, GeO 2 , Bi 2 O 3 , Bi 2 O 4 and Bi 2 O 5 and other metal oxides; conductive polymers such as polyacetylene; Li-Co-Ni-based materials, etc. can be used.

[0065] Method for manufacturing secondary battery cells A method for producing a cell for a secondary battery according to an embodiment of the present invention includes the steps of: (S1) assembling a secondary battery cell by stacking at least one positive electrode and at least one negative electrode alternately with a separator therebetween; (S2) pressing the surface of the secondary battery cell with a roller and rolling it at least once, At least one of the separation membranes has a plurality of coating portions formed on at least one surface thereof and spaced apart from one another by coating a mixture of a gas adsorbent and an adhesive binder.

[0066] According to the method for manufacturing a secondary battery cell of the present invention, a plurality of coating portions containing a gas adsorbent are formed on a separator at intervals, thereby adsorbing gas generated inside the secondary battery, and gas that is not adsorbed by the gas adsorbent is discharged to the outside, thereby reducing the amount of gas trapped inside the secondary battery.

[0067] In particular, the present invention includes a step of manufacturing a secondary battery cell by stacking a positive electrode, a negative electrode, and a separator, and then pressing a surface of the secondary battery cell with a roller and rolling it at least once, so that gas present inside the secondary battery can be easily discharged to the outside, and the amount of gas trapped inside the secondary battery can be significantly reduced.

[0068] Hereinafter, each step of the method for manufacturing a cell for a secondary battery according to the present invention will be described in detail.

[0069] According to the method for producing a secondary battery cell of the present invention, (S1) The method includes a step of assembling a secondary battery cell by stacking at least one positive electrode and at least one negative electrode alternately with a separator sandwiched therebetween.

[0070] At least one of the separators has a plurality of coating portions formed on at least one surface thereof and spaced apart from one another by coating a mixture of a gas adsorbent and an adhesive binder.

[0071] In the present invention, the coating portion, i.e., a plurality of coating portions formed at a distance from one another, may be formed by coating the mixture of the gas adsorbent and the adhesive binder by a spray method. For example, a spray gun may be used to realize the spray method. When the mixture is applied using a spray gun, it is advantageous in that the mixture can be controlled to a desired area and a desired loading amount on one side of the separator, and can be uniformly applied on one side of the separator.

[0072] In addition, in the present invention, at least one surface of the separator includes an uncoated portion that is not coated with the mixture of gas adsorbent and adhesive binder and is a portion of the surface of the separator that is exposed. The uncoated portion may serve as a gas exhaust passage through which gas that is not adsorbed in the coated portion is exhausted to the outside of the secondary battery.

[0073] In the method for manufacturing a secondary battery cell according to the present invention, a secondary battery cell is manufactured including one or more separators having the coating portion. The separator may be stacked at any position within the secondary battery cell, but is preferably stacked at a position where gas is less likely to be discharged.

[0074] In particular, since a secondary battery cell has a structure in which a separator and electrodes are laminated and stacked, gas is more difficult to discharge from the center of the thickness direction of the cell than from the outermost part. In response to this, in order to reduce the amount of gas trapped in the center of the thickness direction of the secondary battery cell, a separator having a coating portion in the center of the thickness direction of the secondary battery cell may be included. Also, a separator having coating portions in other parts in addition to the center portion may be included. For example, the center portion may refer to the center portion when the secondary battery cell is divided into thirds in the thickness direction or the center portion when the secondary battery cell is divided into fifths in the thickness direction.

[0075] In the present invention, at least one positive electrode and at least one negative electrode are alternately stacked with a separator sandwiched therebetween, and then a process known in the art may be included to manufacture a secondary battery cell. For example, the stacked positive electrode, negative electrode, and separator may be housed in a battery case, for example, a pouch case, to assemble a secondary battery. Then, an electrolyte solution may be injected into the battery case to impregnate the stacked positive electrode, negative electrode, and separator with the electrolyte solution, and then the battery case may be sealed. Then, an activation process may be performed to charge and discharge the assembled secondary battery cell.

[0076] Next, the present invention includes a step of (S2) pressing the surface of the secondary battery cell with a roller and rolling it at least once. By rolling the surface of the secondary battery cell with the roller, gas generated inside the secondary battery cell can be easily discharged to the outside of the cell. The surface of the cell can be pressed and rolled with the roller in a pressure range optimized for the size of the secondary battery. Specifically, the cell can be rolled in the electrical installation direction at a pressure of 10 to 50 kg load and a speed of 1 to 5 cm / sec. In the present invention, the electrical installation direction can mean the longitudinal direction between the positive electrode lead and the negative electrode lead.

[0077] When only pressure is applied to the surface of the secondary battery cell, for example, 0.5 to 5 kgf / cm 2 If only pressurization is performed within the pressure range, there is a problem that gas generated inside the secondary battery is dissolved in the electrolyte, and gas located in the center of the secondary battery cell is trapped and difficult to discharge to the outside. However, in the present invention, by applying pressure and rolling to the surface of the secondary battery cell, gas generated inside the secondary battery is not dissolved in the electrolyte, and the gas is easily discharged to the outside without being trapped inside. Gas can be easily discharged in a direction parallel to one surface of the separator provided with a coating portion inside the secondary battery cell (plane direction).

[0078] Furthermore, in the present invention, a gas adsorbent that adsorbs gas is included in the coating portion on one side of the separator, so that the gas inside the secondary battery can be adsorbed. Also, since the coating portions are formed separately from each other, the gas inside the secondary battery can be easily discharged to the outside through the non-coated portion where the coating portion is not formed. In particular, since the non-coated portion can act as a gas discharge passage, it is easier for the gas inside the secondary battery to be discharged to the outside when rolled by the roller.

[0079] Specifically, the method for manufacturing a secondary battery cell of the present invention may include a step of pressing a surface of an assembled secondary battery cell using a roller and rolling it twice. For example, after the primary rolling, the secondary battery cell may be subjected to an aging process and then a secondary rolling process. In this case, gas inside the secondary battery is discharged to the outside during the primary rolling, and gas is further generated inside the secondary battery during the aging process, but the amount of gas trapped inside the secondary battery can be further reduced by discharging the gas generated during the aging process to the outside through the secondary rolling.

[0080] The aging step may be carried out for 0.5 to 72 days at a temperature in the range of 25 to 70° C., but the conditions are not limited.

[0081] In the present invention, a degassing process may be included after step (S2). The degassing process includes a process of opening the battery case to discharge gas, and then sealing the gas discharge portion by heat welding. Generally, in the industry, a degassing process is included to discharge gas generated inside the secondary battery after the secondary battery is assembled and a charge / discharge process is performed.

[0082] However, in the present invention, in consideration of efficient gas discharge, a step of discharging gas by rolling the surface of the secondary battery cell with a roller after the charge / discharge process and before the degassing process is performed is included, thereby reducing the amount of gas remaining in the secondary battery cell.

[0083] Hereinafter, the present invention will be described with reference to specific examples. However, the examples according to the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the following examples. The examples of the present invention are provided to more completely explain the present invention to those having ordinary skill in the art.

[0084] Working Example Each of the Examples and Comparative Examples was produced by the following method.

[0085] [Example 1] 1) Preparation of separation membrane The slurry was coated on one side of a polypropylene porous substrate (thickness: 9 μm, porosity: 45%) and then dried to prepare a separation membrane.

[0086] The slurry was prepared as follows. Polyvinylidene fluoride was added as a binder polymer to an acetone solvent and dissolved at 50° C. for about 4 hours to prepare a binder polymer solution. Alumina (Al 2 O 3 ) (particle size: 500 nm) was added. The weight ratio of inorganic particles to binder polymer was controlled to 70:30 to prepare a slurry for forming a porous coating layer. The solid content in the slurry (solid components excluding the slurry solvent) was 19 wt% relative to 100 wt% of the slurry.

[0087] An acrylic dispersant, zeolite as a gas adsorbent, and polyvinylidene fluoride (PVdF) as an adhesive binder were mixed in an acetone solvent on the separation membrane. The mixture was then applied using a spray gun and dried. The total weight of the mixture (based on solid content) was 1% by weight of the dispersant, 40% by weight of the zeolite, and 15% by weight of the adhesive binder.

[0088] The coating resulted in the formation of a coating pattern of multiple dots (circular patterns with a diameter of 3 mm and a spacing of 5 mm), and the total area of ​​the coating was 40% of the total area of ​​the separator.

[0089] 2) Preparation of positive and negative electrodes As a positive electrode active material, Li[Ni 0.6 Mn 0.2 Co 0.2 ]O 2 A slurry was prepared by mixing the graphite as a conductive material and polyvinylidene fluoride (PVdF) as a binder in a ratio of 97:1.5:1.5. The slurry was coated on an aluminum foil having a thickness of 20 μm, dried and pressed.

[0090] A negative electrode slurry was prepared by mixing a 5:5 mixture of artificial graphite and natural graphite as a negative electrode active material, super C as a conductive material, and SBR / CMC as a binder in a weight ratio of 98:1:1. The negative electrode slurry was then applied to one side of a copper current collector, dried, and rolled to prepare a negative electrode.

[0091] 3) Manufacture of lithium secondary batteries A secondary battery cell was manufactured by stacking the negative and positive electrodes alternately with a separator sandwiched therebetween, and the stacking was repeated 10 times so that the order was a separator with a coating portion / a separator without a coating portion / a separator without a coating portion, to manufacture a secondary battery cell.

[0092] After that, it was rolled in the electrical direction with a pressure of 20 kg load and a speed of 2 cm / sec, and then it was aged at 25°C for 24 hours and aged at 60°C for 24 hours. It was then rolled again under the same conditions as the first rolling. Then, it was subjected to a degassing process.

[0093] [Comparative Example 1] A secondary battery cell was prepared in the same manner as in Example 1, except that a separator having a coating portion formed on the entire surface of the separator using a bar coater was used and rolling was not performed.

[0094] [Comparative Example 2] A secondary battery cell was prepared in the same manner as in Example 1, except that rolling was not performed.

[0095] [Comparative Example 3] A secondary battery cell was prepared in the same manner as in Example 1, except that the coating portion formed on one side of the separator had a mesh pattern and rolling was not performed. In this case, the mesh pattern was coated with a line width of 3 mm and a line spacing of 5 mm, and the area of ​​the coated mesh pattern was 70% of the area of ​​one side of the separator.

[0096] evaluation Identification of trapped gas (air scanner and full charge decomposition analysis) For the above-mentioned Examples and Comparative Examples, gas trapped inside was observed using an air scanner (JAPAN PROBE, Model NAUT-SAT-S01).

[0097] In addition, a full charge disassembly analysis, in which the cell was disassembled after charging to SOC100, revealed that gas trapped inside prevented the cell from reaching 100% charge, and lithium was precipitated.

[0098] The results are shown in Fig. 4. It was confirmed that in the case of Example 1, the amount of gas trapped inside was smaller than in the cases of Comparative Examples 1 to 3.

[0099] Capacity (discharge capacity) measurement The examples and comparative examples were charged and discharged at 25° C. to measure the discharge capacity, and the value measured in Comparative Example 1 was used as the reference value (100%) to evaluate the capacity.

[0100] The evaluation results are shown in the following Table 1. It was confirmed that, compared to Example 1, in Comparative Examples 1 to 3, the presence of gas trapped inside the secondary battery caused a decrease in the secondary battery capacity. Charging conditions: 0.33C CC-CV Discharge condition: 0.33C CC

[0101] DCR The resistance was measured when the battery was discharged for 10 seconds at a current of 2 C. The value measured in Comparative Example 1 was used as the reference value (100%) for evaluation.

[0102] The evaluation results are shown in the following Table 1. It was confirmed that, compared to Example 1, in Comparative Examples 1 to 3, the resistance of the secondary battery increased due to the presence of gas trapped inside the secondary battery.

[0103] [Table 1]

[0104] Electrochemical Impedance Spectroscopy (EIS) The examples and comparative examples were charged at 25° C. and SOC 30, and the electrical resistance was measured using electrochemical impedance spectroscopy (EIS), and the results are shown in FIG.

[0105] In the case of Example 1, it was confirmed that the semicircle (arc) formed at a value greater than 0 was smaller than those in Comparative Examples 1 to 3, and therefore a lower resistance was exhibited.

Claims

1. A secondary battery cell in which at least one negative electrode and at least one positive electrode are alternately stacked with a separator sandwiched therebetween, The secondary battery cell includes three or more separators, At least one of the stacked separators, except for the separators disposed at the outermost portions of the upper and lower portions, has a plurality of coating portions formed on at least one surface thereof and spaced apart from each other, the coating portion includes a mixture of a gas adsorbent and an adhesive binder; The secondary battery cell is characterized in that, after being assembled, the surface of the secondary battery cell is pressed and rolled at least once by a roller.

2. 2. The cell for a secondary battery according to claim 1, wherein the gas adsorbent comprises silica gel, carbon fiber, a porous carbon material, a porous metal oxide, a porous gel, a zeolite, or two or more thereof.

3. 3. The cell for a secondary battery according to claim 1, wherein the adhesive binder comprises polyvinylidene fluoride, styrene butadiene rubber, polytetrafluoroethylene, polyethylene glycol, polypropylene glycol, toluene diisocyanate, polymethyl methacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinyl acetate, ethylene-co-vinyl acetate, polyethylene oxide, cellulose acetate, cellulose acetate butyrate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, cyanoethyl sucrose, pullulan, carboxyl methyl cellulose, acrylonitrile-styrene-butadiene copolymer, polyimide, or two or more thereof.

4. 2. The cell for a secondary battery according to claim 1, wherein a total area of ​​the coating portions formed to be spaced apart from each other on at least one surface of the separator is in the range of 20% to 50% of a total area of ​​one surface of the separator, which is 100%.

5. 2. The cell for a secondary battery according to claim 1, wherein the coating portions formed on at least one surface of the separator and spaced apart from each other are spaced apart from each other by a distance of 1 to 20 mm.

6. (S1) assembling a secondary battery cell by stacking at least one positive electrode and at least one negative electrode alternately with a separator therebetween; (S2) pressing the surface of the secondary battery cell with a roller and rolling it at least once; The secondary battery cell includes three or more separators, and wherein at least one of the separators among the stacked separators, except for the separators disposed on the outermost portions of the upper and lower parts, has a plurality of coating portions formed by coating a mixture of a gas adsorbent and an adhesive binder on at least one surface thereof and spaced apart from each other.

7. The method of claim 6, wherein the coating portion is formed by coating the mixture of the gas adsorbent and the adhesive binder by a spray method.

8. 7. The method for producing a cell for a secondary battery according to claim 6, wherein the gas adsorbent comprises silica gel, carbon fiber, a porous carbon material, a porous metal oxide, a porous gel, a zeolite, or two or more of these.

9. The step (S2) pressing and primarily rolling a surface of the secondary battery cell using a roller; 7. The method of claim 6, further comprising: aging the primary rolled secondary battery cell, and then pressing a surface of the secondary battery cell using a roller and performing secondary rolling.

10. The method of claim 6, further comprising a degassing process after the step (S2).

Citation Information

Patent Citations

  • Non-aqueous electrolytic liquid secondary battery

    JP2006049114A

  • Lithium secondary battery using separator membrane partially coated with gel polymer

    JP2006525624A

  • Separator structure, and manufacturing method of secondary battery using separator structure

    JP2007026730A

  • Separator for nonaqueous electrolyte secondary battery, nonaqueous electrolyte secondary battery, and battery pack