Secondary battery and electric device

By employing a wound electrode assembly in a lithium-ion battery and using two different separator structures in the corner area, the interface performance is optimized, solving the problem that separators cannot simultaneously achieve both cycle performance and safety performance, thus achieving a balance between high-efficiency cycle performance and safety performance.

CN118920011APending Publication Date: 2024-11-08NINGDE AMPEREX TECHNOLOGY LTD
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202410939396.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-11-08

AI Technical Summary

Technical Problem

Existing lithium-ion battery separators struggle to balance cycle performance and safety performance.

Method used

The electrode assembly employs a wound structure and uses two different diaphragms in the corner area. The first diaphragm has high liquid retention capacity and low adhesion, while the second diaphragm has high adhesion and low liquid retention capacity. Combined with specific materials and coating design, the interfacial performance of the electrode assembly is optimized.

Benefits of technology

It improves the cycle performance and safety performance of lithium-ion batteries, balancing energy density and safety.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118920011A_ABST
    Figure CN118920011A_ABST
Patent Text Reader

Abstract

The invention provides a secondary battery and a power utilization device, the secondary battery comprises an electrode assembly of a winding structure, the electrode assembly comprises a positive pole piece, a negative pole piece, a first diaphragm and a second diaphragm, the negative pole piece is located between the first diaphragm and the second diaphragm, the negative pole piece comprises a first negative pole material layer and a second negative pole material layer, the first diaphragm in the corner area comprises a first base membrane, a first bonding layer and a first ceramic coating, the first ceramic coating is arranged on the side, away from the first negative electrode material layer, of the first base membrane, the first bonding layer is arranged on the surface of the first ceramic coating, and the second diaphragm in the corner area comprises a second base membrane, a second bonding layer and a second ceramic coating, the second bonding layers are arranged on the two sides of the second base film, the second ceramic coating is arranged on the side, away from the second negative electrode material layer, of the second base film, and the second ceramic coating is located between the second base film and the second bonding layers. And the obtained secondary battery has good cycle performance and safety performance at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of electrochemical technology, and in particular to a secondary battery and an electrical device. Background Art

[0002] Secondary batteries (such as lithium-ion batteries) are widely used in digital products, electric vehicles, energy storage power stations and other equipment due to their advantages such as high output voltage and energy density, long cycle life and green environmental protection. As one of the four key components of lithium-ion batteries, the diaphragm plays the role of isolating the positive and negative electrodes and providing a lithium ion transmission channel in lithium-ion batteries. Although the diaphragm does not directly participate in the internal reaction of lithium-ion batteries, its structure and properties directly affect the comprehensive performance of lithium-ion batteries. However, the existing diaphragms used in lithium-ion batteries often cannot take into account the cycle performance and safety performance of lithium-ion batteries. Summary of the invention

[0003] The purpose of the present application is to provide a secondary battery that takes into account both the cycle performance and safety performance of the secondary battery, and at the same time provides an electrical device using the secondary battery.

[0004] It should be noted that in the invention content of this application, lithium-ion batteries are used as an example of secondary batteries to explain this application, but the secondary batteries of this application are not limited to lithium-ion batteries. The specific technical solutions are as follows:

[0005] The first aspect of the present application provides a secondary battery, which includes an electrode assembly of a wound structure, the electrode assembly includes a positive electrode sheet, a negative electrode sheet, a first separator and a second separator, the negative electrode sheet is located between the first separator and the second separator, and the electrode assembly includes a straight area and a corner area; the negative electrode sheet includes a negative electrode collector and a first negative electrode material layer and a second negative electrode material layer located on both sides of the thickness direction of the negative electrode collector, the first separator is adjacent to the first negative electrode material layer, and the second separator is adjacent to the second negative electrode material layer; the first separator in the corner area includes a first base film, a first bonding layer and a first ceramic coating, the first base film is in contact with the first negative electrode material layer, and the first ceramic coating is arranged on the first base film away from the first base film On one side of the first negative electrode material layer, the first bonding layer is arranged on the surface of the first ceramic coating; the second diaphragm in the corner area includes a second base film, a second bonding layer and a second ceramic coating, the second bonding layer is arranged on both sides of the second base film, the second ceramic coating is arranged on the side of the second base film away from the second negative electrode material layer, and the second ceramic coating is located between the second base film and the second bonding layer; in the corner area, a positive electrode plate corner section is adjacent to a first negative electrode material layer corner section, the positive electrode plate corner section is farther away from the winding center of the electrode assembly than the first negative electrode material layer corner section, the first diaphragm is located between the positive electrode plate corner section and the first negative electrode material layer corner section, and the positive electrode plate corner section is in contact with the first bonding layer. The secondary battery of the present application is used in combination with the first diaphragm and the second diaphragm, each of which plays a different advantage, so that the cycle performance and safety performance of the secondary battery can be taken into account.

[0006] In some embodiments of the present application, along the winding direction of the electrode assembly, the length of the first negative electrode material layer is greater than the length of the second negative electrode material layer.

[0007] In some embodiments of the present application, the positive electrode sheet includes a positive electrode current collector and a first positive electrode material layer and a second positive electrode material layer located on both sides of the positive electrode current collector in the thickness direction. In the same winding layer, the first positive electrode material layer is closer to the winding center of the electrode assembly than the second positive electrode material layer. At the winding end of the electrode assembly, the length of the first positive electrode material layer along the winding direction of the electrode assembly is greater than the length of the second positive electrode material layer along the winding direction of the electrode assembly.

[0008] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the surface of the particles of the first negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W1 of the coating element is 0.05% to 0.5% based on the mass of the first negative electrode material layer. The cycle performance of the secondary battery is further improved, and both safety performance and energy density can be taken into account.

[0009] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, the surface of the particles of the second negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and based on the mass of the second negative electrode material layer, the mass percentage content W2 of the coating element is 0.05% to 0.5%. The cycle performance of the secondary battery is further improved, and the safety performance and energy density can be taken into account.

[0010] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the first negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and based on the mass of the first negative electrode material layer, the mass percentage content W1' of the doping element is 0.05% to 0.5%. The cycle performance of the secondary battery is further improved, and the safety performance and energy density can be taken into account.

[0011] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, the second negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and based on the mass of the second negative electrode material layer, the mass percentage content W2' of the doping element is 0.05% to 0.5%. The cycle performance of the secondary battery is further improved, and the safety performance and energy density can be taken into account.

[0012] In some embodiments of the present application, the first negative electrode active material and the second negative electrode active material each independently include natural graphite, artificial graphite, mesophase microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x 、Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12 、Li-Al alloy or metallic lithium, where 0 < x < 2. By selecting the above first negative electrode active material and second negative electrode active material and containing the above coating element or doping element, the cycle performance of the secondary battery can be further improved, the energy density can be taken into account, and by combining the first separator and the second separator in the present application, the cycle performance and safety performance of the secondary battery can be better taken into account.

[0013] In some embodiments of the present application, the porosity P1 of the first base film is greater than the porosity P2 of the second base film, 40% ≤ P1 ≤ 70%, 5% ≤ P2 ≤ 50%. In some embodiments of the present application, 50% ≤ P1 ≤ 60%, 10% ≤ P2 ≤ 40%. The first base film has a higher porosity, which is beneficial for the first diaphragm to store more electrolyte. When the first diaphragm is located on the side of the first negative electrode material layer, it is beneficial to store more electrolyte on the side of the first negative electrode material layer of the negative electrode sheet of the secondary battery, and better improve the interface problems caused by insufficient electrolyte between the positive electrode sheet and the negative electrode sheet in the corner area, thereby further improving the cycle performance of the secondary battery. At the same time, by regulating the porosity P1 of the first base film and the porosity P2 of the second base film within the scope of the present application, the mechanical strength of the first diaphragm and the second diaphragm is high, and the secondary battery obtained also has good safety performance.

[0014] In some embodiments of the present application, the pore size D1 of the first base membrane is larger than the pore size D2 of the second base membrane, 80nm≤D1≤700nm, 50nm≤D2≤200nm. In some embodiments of the present application, 250nm≤D1≤520nm, 100nm≤D2≤150nm. The first base membrane has a larger pore size, which can further increase the liquid retention of the first diaphragm, improve the transmission of lithium ions, and better improve the interface problems of the positive electrode and the negative electrode in the corner area caused by insufficient electrolyte, thereby further improving the cycle performance of the secondary battery. At the same time, by regulating the pore size D1 of the first base membrane and the pore size D2 of the second base membrane within the scope of the present application, the mechanical strength of the first diaphragm and the second diaphragm is relatively high, and the secondary battery obtained also has good safety performance.

[0015] In some embodiments of the present application, the coating weight CW1 of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight CW2 of the first adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 By regulating the coating weight CW1 of the first ceramic coating and / or the coating weight CW2 of the first bonding layer within the above range, the first separator has high liquid retention capacity and good structural stability and adhesion, which is conducive to further improving the cycle performance of the secondary battery while taking into account safety performance and energy density.

[0016] In some embodiments of the present application, the coating weight CW3 of the second ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight CW4 of the second adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2By regulating the coating weight CW3 of the second ceramic coating and / or the coating weight CW4 of the second adhesive layer within the above range, the second separator has high structural stability and adhesion and good liquid retention capacity, which is conducive to further improving the safety performance of the secondary battery while taking into account the cycle performance and energy density.

[0017] In some embodiments of the present application, the first adhesive layer includes a first adhesive, the second adhesive layer includes a second adhesive, and the first adhesive and the second adhesive each independently include at least one of polyvinylidene fluoride, polyacrylonitrile, polyethylene oxide, or polyimide. By providing the first adhesive layer and the second adhesive layer, and selecting the first adhesive and the second adhesive within the scope of the present application, it is beneficial to improve the bonding force between the first diaphragm and the positive electrode sheet, between the second diaphragm and the positive electrode sheet, and between the second diaphragm and the negative electrode sheet, and further improve the cycle performance and safety performance of the secondary battery.

[0018] In some embodiments of the present application, the first ceramic coating includes first ceramic particles, the second ceramic coating includes second ceramic particles, and the first ceramic particles and the second ceramic particles each independently include at least one of aluminum oxide, boehmite, silicon oxide, magnesium oxide, titanium oxide, tin oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, aluminum hydroxide, magnesium hydroxide, or calcium hydroxide. By providing the first ceramic coating and the second ceramic coating, and selecting the first ceramic particles and the second ceramic particles within the scope of the present application, the liquid retention capacity of the first diaphragm and the second diaphragm can be further improved, and the interface problem caused by insufficient electrolyte between the positive electrode plate and the negative electrode plate in the corner area can be improved, thereby further improving the cycle performance of the secondary battery.

[0019] In some embodiments of the present application, the mass percentage of the first ceramic particles is 10% to 50% based on the mass of the first ceramic coating; the mass percentage of the second ceramic particles is 10% to 50% based on the mass of the second ceramic coating. By regulating the mass percentage of the first ceramic particles in the first ceramic coating and the mass percentage of the second ceramic particles in the second ceramic coating within the above range, the first ceramic particles and the second ceramic particles can fully play their respective roles, and the first and second diaphragms with good liquid storage capacity and wetting performance are obtained. The application of the diaphragms in secondary batteries is conducive to making the secondary batteries have good cycle performance and taking into account the safety performance of the secondary batteries.

[0020] In some embodiments of the present application, the thickness H1 of the first diaphragm is 6.0 μm to 10.5 μm, and the thickness H2 of the second diaphragm is 6.3 μm to 11.0 μm. By regulating the thickness H1 of the first diaphragm and the thickness H2 of the second diaphragm within the scope of the present application, it is helpful to reduce the risk of lithium dendrites generated during the secondary battery cycle piercing the first diaphragm or the second diaphragm and causing a short circuit in the secondary battery. The first diaphragm and the second diaphragm have good mechanical strength, and at the same time, the transmission distance of lithium ions during the secondary battery cycle is moderate. As a result, the secondary battery has a higher energy density and also has good cycle performance and safety performance.

[0021] The second aspect of the present application provides an electric device, the electric device comprising the secondary battery described in any of the above embodiments. Therefore, the electric device has good performance.

[0022] Beneficial effects of this application:

[0023] The present application provides a secondary battery and an electric device, wherein the secondary battery comprises an electrode assembly of a winding structure, wherein the electrode assembly comprises a positive electrode sheet, a negative electrode sheet, a first separator and a second separator, wherein the negative electrode sheet is located between the first separator and the second separator, wherein the negative electrode sheet comprises a first negative electrode material layer and a second negative electrode material layer, wherein the first separator in the corner region comprises a first base film, a first bonding layer and a first ceramic coating, wherein the first ceramic coating is arranged on a side of the first base film away from the first negative electrode material layer, wherein the first bonding layer is arranged on the surface of the first ceramic coating, wherein the second separator in the corner region comprises a second base film, a second bonding layer and a second ceramic coating, wherein the second bonding layer is arranged on both sides of the second base film, wherein the second ceramic coating is arranged on a side of the second base film away from the second negative electrode material layer, wherein the second ceramic coating is arranged between the second base film and the second bonding layer. Through the above arrangement, the secondary battery obtained has both good cycle performance and safety performance.

[0024] Of course, implementing any product or method of the present application does not necessarily require achieving all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application, and for ordinary technicians in this field, other embodiments can also be obtained based on these drawings.

[0026] Figure 1 This is a schematic diagram of the cross-sectional structure of an electrode assembly according to an embodiment of the present application, after being unfolded along the W direction, along its own thickness direction;

[0027] Figure 2 for Figure 1A schematic diagram of the cross-sectional structure of a wound structure electrode assembly wound along the W direction along its own thickness direction;

[0028] Figure 3 for Figure 2 A partial enlarged view of point A in the middle.

[0029] Figure numerals: electrode assembly 100; first separator 10; first base film 11; first bonding layer 12; first ceramic coating 13; second separator 20; second base film 21; second bonding layer 22; second ceramic coating 23; negative electrode plate 30; negative electrode collector 31; first negative electrode material layer 32; second negative electrode material layer 33; positive electrode plate 40; positive electrode collector 41; first positive electrode material layer 42; second positive electrode material layer 43; straight area 102 of the electrode assembly; corner area 101 of the electrode assembly. DETAILED DESCRIPTION

[0030] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all the embodiments. All other embodiments obtained by those skilled in the art based on the present application belong to the scope of protection of the present application.

[0031] It should be noted that in the specific implementation manner of the present application, the present application is explained by taking a lithium-ion battery as an example of a secondary battery, but the secondary battery of the present application is not limited to a lithium-ion battery.

[0032] The first aspect of the present application provides a secondary battery, which includes an electrode assembly of a winding structure, specifically, as Figure 2 As shown, the electrode assembly 100 is a wound structure, and the electrode assembly 100 includes a first separator 10, a second separator 20, a negative electrode plate 30 and a positive electrode plate 40. The electrode assembly 100 also includes a straight area 102 and a corner area 101. In the present application, the straight area refers to the straight part of the electrode assembly, and the corner area refers to the curved part of the electrode assembly.

[0033] like Figure 1 and Figure 3As shown, the electrode assembly 100 includes a positive electrode sheet 40, a negative electrode sheet 30, a first separator 10 and a second separator 20, the negative electrode sheet 30 is located between the first separator 10 and the second separator 20, and the electrode assembly 100 includes a straight area 102 and a corner area 101; the negative electrode sheet 30 includes a negative electrode collector 31 and a first negative electrode material layer 32 and a second negative electrode material layer 33 located on both sides of the negative electrode collector 31 in the thickness direction, the first separator 10 is adjacent to the first negative electrode material layer 32, and the second separator 10 is adjacent to the first negative electrode material layer 32. The membrane 20 is adjacent to the second negative electrode material layer 33; the first separator 10 in the corner area 101 includes a first base film 11, a first bonding layer 12 and a first ceramic coating 13, the first ceramic coating 13 is arranged on the side of the first base film 11 away from the first negative electrode material layer 32, and the first bonding layer 12 is arranged on the surface of the first ceramic coating 13, that is, the first separator 10 includes a first bonding layer 12 and a first ceramic coating 13; and the first base film 11 is in contact with the first negative electrode material layer 32. The second separator 20 in the corner area includes a second base film 21, a second bonding layer 22 and a second ceramic coating 23, the second bonding layer 22 is arranged on both sides of the second base film 21, the second ceramic coating 23 is arranged on the side of the second base film 21 away from the second negative electrode material layer 33, and the second ceramic coating 23 is located between the second base film 21 and the second bonding layer 22, that is, the second separator includes two layers of second bonding layers 22 and a second ceramic coating 23. The positive electrode sheet 40 includes a positive electrode current collector 41 and a first positive electrode material layer 42 and a second positive electrode material layer 43 located on both sides of the positive electrode current collector in the thickness direction. In the corner area 101, a corner section of the positive electrode sheet 40 is adjacent to a corner section of the first negative electrode material layer 32, the corner section of the positive electrode sheet 40 is farther from the winding center of the electrode assembly 100 than the corner section of the first negative electrode material layer 32, the first separator 10 is located between the corner section of the positive electrode sheet 40 and the corner section of the first negative electrode material layer 32, and the corner section of the positive electrode sheet 40 is in contact with the first bonding layer 12.

[0034] The inventors found that the greater the bonding force between the diaphragm and the pole piece, the better the safety performance of the secondary battery. However, the bonding layer will reduce the gap between adjacent layers, which is prone to electrolyte bridge breakage and lithium precipitation at the interface between the electrolyte and the negative electrode, affecting the cycle performance of the lithium-ion battery. The smaller the bonding force between the diaphragm and the pole piece, the more electrolyte the diaphragm absorbs, the higher the transmission rate of the lithium-ion battery, and the better the cycle performance of the secondary battery, but it will deteriorate the safety performance of the secondary battery.

[0035] The electrode assembly 100 of the present application is a winding structure, and the electrode assembly includes a straight area 102 and a corner area 101, wherein the corner area 101 is more likely to have insufficient electrolyte or even electrolyte bridge failure, thereby affecting the cycle performance of the secondary battery. The present application arranges a first diaphragm 10 and a second diaphragm 20 of two different structures in the corner area 101 of the electrode assembly 100. The first diaphragm 10 includes a first adhesive layer 12, which is conducive to storing more electrolyte on the side of the first negative electrode material layer 32 of the negative electrode plate of the secondary battery. It has a high liquid retention capacity and a high transmission rate of the lithium-ion battery, which can effectively reduce the risk of lithium precipitation at the interface between the electrolyte and the negative electrode plate due to electrolyte bridge breaking in the late stage of the secondary battery cycle, thereby improving the cycle performance of the secondary battery; the second diaphragm 20 includes two second adhesive layers 22, which are conducive to improving the bonding between the second diaphragm 20 and the positive electrode plate 40 and between the second diaphragm 20 and the negative electrode plate 30, strengthening the interface between the second diaphragm 20 and the positive electrode plate 40 and the second diaphragm 20 and the negative electrode plate 30, and can effectively inhibit the thermal shrinkage of the second base film 21, improve the overall bonding strength of the electrode assembly 100, and improve the safety performance of the secondary battery. At the same time, the first ceramic coating 13 is arranged on the side of the first base film 11 away from the first negative electrode material layer 32, and the second ceramic coating 23 is arranged on the side of the second base film 21 away from the second negative electrode material layer 33. This is because the positive electrode active material particles on the positive electrode plate 40 are relatively hard, and occasionally there will be particles of positive electrode active material with larger particle size or sharper particle size protruding from the positive electrode plate 40. During the production or use of secondary batteries, the above-mentioned particles of positive electrode active material may puncture the diaphragm between the positive electrode plate 40 and the negative electrode plate 30, causing the positive electrode plate 40 to contact and short-circuit with the negative electrode plate 30. The ceramic coating has a high puncture resistance, which can effectively reduce the situation where the above-mentioned positive electrode active material punctures the diaphragm, thereby improving the cycle performance and safety performance of the secondary battery. In addition, the first negative electrode material layer 32 located on the outside of the corner area 101 is wrapped by the positive electrode sheet 40, and the winding radius of the positive electrode sheet 40 is larger than the winding radius of the first negative electrode material layer 32. The positive-negative electrode ratio (Cell Balance, CB, the ratio of the negative electrode capacity per unit area to the positive electrode capacity per unit area) at the first negative electrode material layer 32 is smaller. The first negative electrode material layer 32 side is more prone to lithium deposition, and is more prone to interface problems than the second negative electrode material layer 33 side on the inside. Based on this, setting a first diaphragm 10 with high liquid retention capacity adjacent to the first negative electrode material layer 32 is more conducive to improving the interface problem in the corner area 101; at the same time, since the first diaphragm 10 with high liquid retention capacity but low adhesion is used on one side of the first negative electrode material layer 32, in order to prevent the overall adhesion of the electrode assembly 100 from decreasing, a second diaphragm 20 with good adhesion is set adjacent to the second negative electrode material layer 33. Therefore, by using the first separator 10 and the second separator 20 with different structures in the corner area 101 of the electrode assembly 100, both the cycle performance and the safety performance of the secondary battery can be taken into consideration.

[0036] In some embodiments of the present application, along the winding direction of the electrode assembly, the length of the first negative electrode material layer 32 is greater than the length of the second negative electrode material layer 33. Figure 1 As shown, along the winding direction W of the electrode assembly 100, the first negative electrode material layer 32 is flush with one end of the second negative electrode material layer 33, and at the other end, the extension length of the first negative electrode material layer 32 is longer than that of the second negative electrode material layer 33. It can be understood that when the length of the first negative electrode material layer 32 is greater than the length of the second negative electrode material layer 33, it can also be that the extension length of the first negative electrode material layer 32 at one end along the winding direction and the other end opposite to the winding direction is longer than that of the second negative electrode material layer 33. The reason for this arrangement is that when the first diaphragm 10 is located on one side of the first negative electrode material layer 32 of the negative electrode plate 30, it is beneficial for the negative electrode plate 30 of the secondary battery to absorb more electrolyte, reducing the risk of lithium deposition at the interface between the electrolyte and the negative electrode plate 30 due to electrolyte bridge breaking in the late stage of the secondary battery cycle. The present application does not have any special restrictions on the difference in length between the first negative electrode material layer and the second negative electrode material layer, and can be selected according to the specific situation, as long as the purpose of the present application can be achieved.

[0037] In some embodiments of the present application, along the winding direction of the electrode assembly, the length of the first positive electrode material layer is equal to the length of the second positive electrode material layer.

[0038] In some embodiments of the present application, along the winding direction of the electrode assembly, the length of the first positive electrode material layer is greater than the length of the second positive electrode material layer. Figure 1 As shown, at the winding end of the electrode assembly 100, the length of the first positive electrode material layer 42 is greater than the length of the second positive electrode material layer 43, and the second positive electrode material 43 is farther away from the winding center of the electrode assembly 100 than the first positive electrode material layer 42. Figure 1 As shown, along the winding direction W, one end of the first positive electrode material layer 42 and the second positive electrode material layer 43 are flush, and at the other end, the extension length of the first positive electrode material layer 42 is longer than that of the second positive electrode material layer 43, wherein the other end is the winding end of the positive electrode sheet 40. It can be understood that when the length of the first positive electrode material layer 42 is greater than the length of the second positive electrode material layer 43, the extension length of the first positive electrode material layer 42 may be longer than that of the second positive electrode material layer 43 at one end along the winding direction and at the other end opposite to the winding direction. This is because Figure 2As shown, at the outermost side of the winding structure of the electrode assembly 100, a section of the positive electrode sheet 40 is coated on one side, that is, the first positive electrode material layer 42 is only provided on one side in the thickness direction of the positive electrode collector 41. This is mainly to save negative electrode active materials and to prevent electrochemical corrosion of the aluminum-plastic film of the packaging bag (not shown in the figure) by making the potential of the positive electrode collector 41 similar to that of the secondary battery packaging bag. The present application has no particular restriction on the difference in length between the first positive electrode material layer 42 and the second positive electrode material layer 43, and can be selected according to specific circumstances, as long as the purpose of the present application can be achieved.

[0039] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the surface of the particles of the first negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W1 of the coating element is 0.05% to 0.5% based on the mass of the first negative electrode material layer. For example, the mass percentage content W1 of the coating element can be 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5% or a range consisting of any two of the values. The first negative electrode active material includes a coating element within the scope of this application and regulates the mass percentage content W1 of the coating element within the scope of this application. On the one hand, the conductive network on the surface of the first negative electrode active material particle is more compact and has better kinetic performance; on the other hand, the specific surface area of ​​the first negative electrode active material can be reduced, and the side reaction between the first negative electrode active material and the electrolyte can be reduced; on the other hand, it is conducive to forming a passivation film on the surface of the first negative electrode active material particle, thereby improving its first effect and reversible capacity. Therefore, the use of the above-mentioned first negative electrode active material is more conducive to improving the interface problem of the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery, and the combination of the first diaphragm and the second diaphragm in this application can better take into account the cycle performance, safety performance and energy density of the secondary battery.

[0040] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, and the surface of the particles of the second negative electrode active material includes a coating element, and the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W2 of the coating element is 0.05% to 0.5% based on the mass of the second negative electrode material layer. For example, the mass percentage content W2 of the coating element can be 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5% or a range consisting of any two of the values. The second negative electrode active material includes a coating element within the scope of this application and regulates the mass percentage content W2 of the coating element within the scope of this application. On the one hand, the conductive network on the surface of the second negative electrode active material particle is more compact and has better kinetic performance; on the other hand, the specific surface area of ​​the second negative electrode active material can be reduced, and the side reaction between the second negative electrode active material and the electrolyte can be reduced; on the other hand, it is conducive to the formation of a passivation film on the surface of the second negative electrode active material particle, thereby improving its first effect and reversible capacity. Therefore, the use of the above-mentioned second negative electrode active material is more conducive to improving the interface problem of the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery, and the combination of the first diaphragm and the second diaphragm in this application can better take into account the cycle performance, safety performance and energy density of the secondary battery.

[0041] In some embodiments of the present application, the first negative electrode material layer includes a first negative electrode active material, the first negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and based on the mass of the first negative electrode material layer, the mass percentage content W1' of the doping element is 0.05% to 0.5%; for example, the mass percentage content W1' of the doping element can be 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5% or a range consisting of any two values ​​therein. The first negative electrode active material includes a doping element within the scope of the present application and regulates the mass percentage content W1' of the doping element within the scope of the present application. On the one hand, the conductive network of the first negative electrode active material particles as a whole is more compact and has better kinetic performance; on the other hand, it is conducive to reducing the side reaction between the first negative electrode active material and the electrolyte. Therefore, the use of the above-mentioned first negative electrode active material is more conducive to improving the interface problems between the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery. Moreover, the combined use of the first diaphragm and the second diaphragm in the present application can better take into account the cycle performance, safety performance and energy density of the secondary battery.

[0042] In some embodiments of the present application, the second negative electrode material layer includes a second negative electrode active material, the second negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu, or Ni, and based on the mass of the second negative electrode material layer, the mass percentage content W2' of the doping element is 0.05% to 0.5%. For example, the mass percentage content W2' of the doping element can be 0.05%, 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45%, 0.5%, or a range composed of any two of these values. The second negative electrode active material includes a doping element within the scope of the present application and regulates the mass percentage content W2' of the doping element within the scope of the present application. On the one hand, the overall conductive network of the second negative electrode active material particles is denser and the kinetic performance is better; on the other hand, the side reactions between the second negative electrode active material and the electrolyte are reduced. Thus, using the above-mentioned second negative electrode active material is more conducive to improving the interface problem between the positive electrode sheet and the negative electrode sheet in the corner area, thereby further improving the cycle performance of the secondary battery. Moreover, by combining the first separator and the second separator in the present application, the cycle performance, safety performance, and energy density of the secondary battery can be better balanced.

[0043] In some embodiments of the present application, the first negative electrode active material and the second negative electrode active material each independently include natural graphite, artificial graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12 , Li-Al alloy, or metallic lithium, where 0 < x < 2. By selecting the above-mentioned first negative electrode active material and second negative electrode active material and including the above-mentioned coating element or doping element, it is more conducive to improving the interface problem between the positive electrode sheet and the negative electrode sheet in the corner area, thereby further improving the cycle performance of the secondary battery. Moreover, by combining the first separator and the second separator in the present application, the cycle performance and safety performance of the secondary battery can be better balanced.

[0044] In the present application, natural graphite, artificial graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O 12 , Li-Al alloy, or metallic lithium containing the above-mentioned coating element, and natural graphite, artificial graphite, mesocarbon microbeads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel-structured lithium titanate Li4Ti5O12 , Li-Al alloy or metallic lithium, all of which can be purchased, and the mass percentage of the coating element or doping element in the negative electrode active material can be tested by the following test method, and the required negative electrode active material can be selected so that W1, W2, W1', W2' are within the above range.

[0045] The types of coating elements or doping elements in the first negative electrode active material can be tested in the following way: weigh a certain amount of the first negative electrode active material, and then use a scanning electron microscope combined with an energy spectrometer to test to obtain the types of coating elements and doping elements in the first negative electrode material layer. When the element is mainly distributed on the surface of the first negative electrode active material particles, the corresponding element is a coating element; when the element is mainly dispersed inside the first negative electrode active material particles, the corresponding element is a doping element. Thus, the types of coating elements or doping elements in the first negative electrode material layer are obtained. Replace the first negative electrode material layer in the above steps with the second negative electrode material layer, and the types of coating elements or doping elements in the second negative electrode material layer can be obtained.

[0046] The mass percentage of the coating element or the mass percentage of the doping element in the first negative electrode active material can be tested in the following manner: weigh a certain amount of the first negative electrode active material, add concentrated nitric acid for microwave digestion to obtain a solution, wash the obtained solution and filter residue multiple times and adjust the volume, test the plasma intensity of the doping element or coating element therein by inductively coupled plasma emission spectrometer (ICP-OES), calculate the content of the doping element or coating element in the solution according to the standard curve of the measured element, and thus calculate the mass percentage of the doping element or coating element in the first negative electrode active material. Replace the first negative electrode active material with the second negative electrode active material, and then the mass percentage of the coating element or the mass percentage of the doping element in the second negative electrode active material can be measured.

[0047] Generally, when other conditions remain unchanged, the mass percentage of the coating element in the first negative electrode active material layer can be adjusted by changing the mass percentage of the coating element in the first negative electrode active material. For example, by increasing the mass percentage of the coating element in the first negative electrode active material, the mass percentage of the coating element in the first negative electrode material layer increases; by decreasing the mass percentage of the coating element in the first negative electrode active material, the mass percentage of the coating element in the first negative electrode material layer decreases. The mass percentage of the coating element in the second negative electrode material layer can be adjusted in the same manner.

[0048] Generally, when other conditions remain unchanged, the mass percentage of the doping element in the first negative electrode active material layer can be regulated by changing the mass percentage of the doping element in the first negative electrode active material. For example, by increasing the mass percentage of the doping element in the first negative electrode active material, the mass percentage of the doping element in the first negative electrode material layer increases; by decreasing the mass percentage of the doping element in the first negative electrode active material, the mass percentage of the doping element in the first negative electrode material layer decreases. The mass percentage of the doping element in the second negative electrode material layer can be regulated in the same manner.

[0049] In some embodiments of the present application, the porosity P1 of the first base film is greater than the porosity P2 of the second base film, 40%≤P1≤70%, 5%≤P2≤50%. In some embodiments of the present application, 50%≤P1≤60%, 10%≤P2≤40%. For example, the porosity P1 of the first base film can be 40%, 45%, 50%, 55%, 60%, 65%, 70% or a range consisting of any two of the values, and the porosity P2 of the second base film can be 5%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of the values. The first base film has a higher porosity, which is conducive to the first diaphragm storing more electrolyte. When the first diaphragm is located on one side of the first negative electrode material layer, it is conducive to storing more electrolyte at the first negative electrode material layer of the electrode assembly 100, and better improves the interface problem caused by insufficient electrolyte between the positive electrode plate and the negative electrode plate in the corner area, thereby further improving the cycle performance of the secondary battery. At the same time, by regulating the porosity P1 of the first base film and the porosity P2 of the second base film within the scope of this application, the mechanical strength of the first diaphragm and the second diaphragm is high, and the secondary battery obtained also has good safety performance.

[0050] In some embodiments of the present application, the pore size D1 of the first base film is larger than the pore size D2 of the second base film, 80nm≤D1≤700nm, 50nm≤D2≤200nm. In some embodiments of the present application, 250nm≤D1≤520nm, 100nm≤D2≤150nm. For example, the pore size D1 of the first base film can be 80nm, 100nm, 150nm, 200nm, 250nm, 300nm, 350nm, 400nm, 450nm, 500nm, 550nm, 600nm, 650nm, 700nm or a range consisting of any two of the values, and the pore size D2 of the second base film can be 50nm, 60nm, 70nm, 80nm, 90nm, 100nm, 150nm, 180nm, 200nm or a range consisting of any two of the values. The first base film has a larger pore size, which can further increase the liquid retention of the first diaphragm, improve the transmission of lithium ions, and better improve the interface problem caused by insufficient electrolyte between the positive electrode and the negative electrode in the corner area, thereby further improving the cycle performance of the secondary battery. At the same time, by adjusting the pore size D1 of the first base film and the pore size D2 of the second base film within the scope of this application, the mechanical strength of the first diaphragm and the second diaphragm is relatively high, and the secondary battery obtained also has good safety performance.

[0051] In some embodiments of the present application, the thickness h1 of the first base film may be 4.5 μm to 8.0 μm, and the thickness h2 of the second base film may be 4.5 μm to 8.0 μm. The present application has no particular restrictions on the materials of the first base film and the second base film, as long as the purpose of the present application can be achieved. For example, the materials of the first base film and the second base film each independently include at least one of polyimide, polyamide, polysulfone, polyacrylonitrile, cellulose, polyetheretherketone, polyphenylene sulfide, polyacrylate, polyethylene terephthalate, polyphenylamide, polyarylethersulfoneketone, aramid, aromatic sulfone or polyolefin, and the polymerization monomer of the polyolefin includes at least one of ethylene, propylene, 1-butene, 1-pentene, 1-hexene, 1-octene, 4-methyl-1-pentene, cyclobutene, cyclopentene or cyclohexene. The present application has no particular restrictions on the weight average molecular weight of the material of the first base film, as long as the purpose of the present application can be achieved. For example, the weight average molecular weight of the material of the first base film may be 2×10 5 to 1.5×10 6 The present application has no particular limitation on the weight average molecular weight of the material of the second base film, as long as it can achieve the purpose of the present application. For example, the weight average molecular weight of the material of the second base film can be 2×10 5 to 1.5×10 6 The types of the first base film and the second base film may include at least one of a woven film, a nonwoven film, a microporous film, a composite film, a rolled film, or a spun film.

[0052] In the present application, the first base film with different porosity and pore size can be purchased, and the first base film with the required porosity and pore size can be selected in combination with the "first base film and second base film porosity test" and "first base film and second base film pore size test" test methods of the present application. The second base film with different porosity and pore size can be purchased, and the second base film with the required porosity and pore size can be selected in combination with the "first base film and second base film porosity test" and "first base film and second base film pore size test" test methods of the present application.

[0053] In some embodiments of the present application, the coating weight CW1 of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 For example, the coating weight CW1 of the first ceramic coating may be 7 mg / cm 2 , 8mg / cm 2 , 9mg / cm 2 、10mg / cm 2 、11mg / cm 2 , 12mg / cm 2 、13mg / cm 2 Or a range consisting of any two of the values. By regulating the coating weight of the first ceramic coating within the scope of the present application, it is beneficial to improve the thermal stability and mechanical properties of the first diaphragm, reduce the possibility of large-area contact between the positive electrode plate and the negative electrode plate due to the shrinkage of the first diaphragm during the charging and discharging process of the secondary battery, and improve the binding capacity of the first diaphragm, thereby improving the safety performance of the secondary battery; at the same time, the first ceramic coating can absorb part of the electrolyte, which is beneficial to increase the liquid retention of the first diaphragm, thereby improving the liquid retention and wettability of the first diaphragm, which is beneficial to improve the cycle performance of the secondary battery, and take into account the energy density of the secondary battery.

[0054] In some embodiments of the present application, the coating weight CW2 of the first bonding layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 For example, the coating weight CW2 of the first adhesive layer may be 0.0004 mg / mm 2 , 0.0006mg / mm 2 , 0.0008mg / mm 2 , 0.001mg / mm 2 , 0.0012mg / mm 2 、0.0015mg / mm 2 、0.0018mg / mm 2 , 0.002mg / mm 2Or a range consisting of any two of the values. By adjusting the coating weight of the first adhesive layer within the scope of the present application, the first separator and the positive electrode plate have a higher bonding force, which can strengthen the interface between the first separator and the positive electrode plate, and the electrolyte is well infiltrated, which is conducive to the active metal ions (such as Li + ) transmission, while reducing the possibility of the first ceramic coating falling off. Thus, the cycle performance and safety performance of the secondary battery can be further improved, while taking into account the energy density of the secondary battery.

[0055] In some embodiments of the present application, the coating weight CW1 of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 The coating weight CW2 of the first adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 For example, the coating weight CW1 of the first ceramic coating may be 7 mg / cm 2 , 8mg / cm 2 , 9mg / cm 2 、10mg / cm 2 、11mg / cm 2 , 12mg / cm 2 、13mg / cm 2 Or a range consisting of any two of the values. For example, the coating weight CW2 of the first adhesive layer can be 0.0004 mg / mm 2 , 0.0006mg / mm 2 , 0.0008mg / mm 2 、0.001mg / mm 2 , 0.0012mg / mm 2 、0.0015mg / mm 2 、0.0018mg / mm 2 , 0.002mg / mm 2 Or a range consisting of any two of the values. By regulating the coating weight CW1 of the first ceramic coating and the coating weight CW2 of the first bonding layer within the above range, the first diaphragm has a high liquid retention capacity and good structural stability and adhesion, which is conducive to further improving the cycle performance and safety performance of the secondary battery while taking into account the energy density.

[0056] In some embodiments of the present application, the coating weight CW3 of the second ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 For example, the coating weight CW3 of the second ceramic coating may be 7 mg / cm 2 , 8mg / cm 2 , 9mg / cm2 、10mg / cm 2 、11mg / cm 2 , 12mg / cm 2 、13mg / cm 2 Or a range consisting of any two of the values. By regulating the coating weight of the second ceramic coating within the scope of the present application, it is beneficial to improve the thermal stability and mechanical properties of the second diaphragm, reduce the possibility of large-area contact between the positive electrode and the negative electrode due to the shrinkage of the second diaphragm during the charging and discharging process of the secondary battery, and improve the binding capacity of the second diaphragm, thereby improving the safety performance of the secondary battery; at the same time, the second ceramic coating can absorb part of the electrolyte, which is beneficial to increase the liquid retention of the second diaphragm, thereby improving the liquid retention and wettability of the second diaphragm, which is beneficial to improve the cycle performance of the secondary battery, and take into account the energy density of the secondary battery.

[0057] In some embodiments of the present application, the coating weight CW4 of the second bonding layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 For example, the coating weight CW4 of the second adhesive layer may be 0.0004 mg / mm 2 , 0.0006mg / mm 2 , 0.0008mg / mm 2 , 0.001mg / mm 2 , 0.0012mg / mm 2 、0.0015mg / mm 2 、0.0018mg / mm 2 , 0.002mg / mm 2 Or a range consisting of any two of the values. By adjusting the coating weight of the second adhesive layer within the scope of the present application, the second separator and the positive electrode sheet and the second separator and the negative electrode sheet have a higher bonding force, which can strengthen the interface between the second separator and the positive electrode sheet and the second separator and the negative electrode sheet, which is beneficial to the active metal ions (such as Li + ) transmission, while reducing the possibility of the second ceramic coating falling off. Thus, the cycle performance and safety performance of the secondary battery can be further improved, while taking into account the energy density of the secondary battery.

[0058] In some embodiments of the present application, the coating weight CW3 of the second ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 The coating weight of the second adhesive layer CW4 is 0.0004 mg / mm 2 To 0.002mg / mm 2 For example, the coating weight CW3 of the second ceramic coating may be 7 mg / cm2 , 8mg / cm 2 , 9mg / cm 2 、10mg / cm 2 、11mg / cm 2 , 12mg / cm 2 、13mg / cm 2 Or a range consisting of any two of the values. For example, the coating weight CW4 of the second adhesive layer can be 0.0004 mg / mm 2 , 0.0006mg / mm 2 , 0.0008mg / mm 2 , 0.001mg / mm 2 , 0.0012mg / mm 2 、0.0015mg / mm 2 、0.0018mg / mm 2 , 0.002mg / mm 2 Or a range consisting of any two of the values. By regulating the coating weight CW3 of the second ceramic coating and the coating weight CW4 of the second adhesive layer within the above range, the second diaphragm has high structural stability and adhesion and good liquid retention capacity, which is conducive to further improving the safety performance and cycle performance of the secondary battery while taking into account the energy density.

[0059] In some embodiments of the present application, the first adhesive layer includes a first adhesive, the second adhesive layer includes a second adhesive, and the first adhesive and the second adhesive each independently include at least one of polyvinylidene fluoride (PVDF), polyacrylonitrile (PAN), polyethylene oxide (PEO) or polyimide (PI). By setting the first adhesive layer and the second adhesive layer, and selecting the first adhesive and the second adhesive within the scope of the present application, it is beneficial to improve the bonding force between the first diaphragm and the positive electrode sheet, between the second diaphragm and the positive electrode sheet, and between the second diaphragm and the negative electrode sheet, strengthen the interface between the first diaphragm and the positive electrode sheet, between the second diaphragm and the positive electrode sheet, and between the second diaphragm and the negative electrode sheet, which is beneficial to the transmission of lithium ions, and at the same time reduces the possibility of the first ceramic coating and the second ceramic coating falling off, further improving the cycle performance and safety performance of the secondary battery. The present application has no special restrictions on the weight average molecular weight of the first adhesive and the second adhesive, as long as the purpose of the present application can be achieved. For example, the weight average molecular weight of the first adhesive and the second adhesive can be 1.5×10 4 to 9×10 6 .

[0060] In some embodiments of the present application, the first adhesive layer may further include a first thickener, and the second adhesive layer may further include a second thickener. Applying the first thickener to the first adhesive layer and the second thickener to the second adhesive layer is conducive to increasing the stability of the first adhesive layer slurry and the second adhesive layer slurry, and preventing the sedimentation of each component in the first adhesive layer slurry and the second adhesive layer slurry. The present application has no particular restrictions on the types of the first thickener and the second thickener, as long as the purpose of the present application can be achieved. For example, the first thickener and the second thickener are each independently selected from at least one of hydroxyethyl cellulose, methyl hydroxyethyl cellulose, sodium carboxymethyl cellulose, polyacrylamide or sodium alginate. The present application has no particular restrictions on the content of the first thickener in the first adhesive layer and the content of the second thickener in the second adhesive layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved. For example, based on the mass of the first adhesive layer, the mass percentage of the first thickener is 0.3% to 6%; based on the mass of the second adhesive layer, the mass percentage of the second thickener is 0.3% to 6%. The present application has no particular restrictions on the content of the first binder in the first adhesive layer and the content of the second binder in the second adhesive layer. Those skilled in the art can select according to actual needs as long as the purpose of the present application can be achieved. For example, based on the mass of the first adhesive layer, the mass percentage of the first binder is 94% to 99.7%; based on the mass of the second adhesive layer, the mass percentage of the second binder is 94% to 99.7%.

[0061] In some embodiments of the present application, the first ceramic coating includes first ceramic particles, the second ceramic coating includes second ceramic particles, and the first ceramic particles and the second ceramic particles each independently include at least one of aluminum oxide, boehmite, silicon oxide, magnesium oxide, titanium oxide, tin oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, aluminum hydroxide, magnesium hydroxide, or calcium hydroxide. By providing the first ceramic coating and the second ceramic coating, and selecting the first ceramic particles and the second ceramic particles within the scope of the present application, the liquid retention capacity of the first diaphragm and the second diaphragm can be further improved, and the interface problem caused by insufficient electrolyte between the positive electrode plate and the negative electrode plate in the corner area can be improved, thereby further improving the cycle performance of the secondary battery.

[0062] In some embodiments of the present application, based on the mass of the first ceramic coating, the mass percentage C1 of the first ceramic particles is 10% to 50%; based on the mass of the second ceramic coating, the mass percentage C2 of the second ceramic particles is 10% to 50%. For example, the mass percentage C1 of the first ceramic particles can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of the values, and the mass percentage C2 of the second ceramic particles can be 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50% or a range consisting of any two of the values. By regulating the mass percentage of the first ceramic particles in the first ceramic coating and the mass percentage of the second ceramic particles in the second ceramic coating within the above range, the first ceramic particles and the second ceramic particles can fully play their corresponding roles, and the first diaphragm and the second diaphragm with good liquid storage capacity and wetting performance are obtained. The application of the diaphragm in the secondary battery is conducive to making the secondary battery have good cycle performance and taking into account the safety performance of the secondary battery.

[0063] In some embodiments of the present application, the first ceramic coating also includes a first ceramic coating binder, and the second ceramic coating also includes a second ceramic coating binder. The present application has no particular restrictions on the types of the first ceramic coating binder and the second ceramic coating binder, as long as the purpose of the present application can be achieved. For example, the first ceramic coating binder and the second ceramic coating binder are each independently selected from at least one of styrene-butadiene rubber, polyvinyl alcohol, polyvinylidene fluoride, polyacrylic acid, polymethyl methacrylate, polybutyl acrylate or polyacrylonitrile. The present application has no particular restrictions on the content of the first ceramic coating binder in the first ceramic coating and the content of the second ceramic coating binder in the second ceramic coating, as long as the purpose of the present application can be achieved. For example, based on the mass of the first ceramic coating, the mass percentage of the first ceramic coating binder is 50% to 90%; based on the mass of the second ceramic coating, the mass percentage of the second ceramic coating binder is 50% to 90%.

[0064] In some embodiments of the present application, the thickness H1 of the first diaphragm is 6.0 μm to 10.5 μm, and the thickness H2 of the second diaphragm is 6.3 μm to 11.0 μm. For example, the thickness H1 of the first diaphragm can be 6.0 μm, 6.3 μm, 6.5 μm, 6.8 μm, 7.0 μm, 7.3 μm, 7.5 μm, 7.8 μm, 8.0 μm, 8.3 μm, 8.5 μm, 8.8 μm, 9.0 μm, 9.3 μm, 9.5 μm, 9.8 μm, 10.0 μm, 10.3 μm, 10.5 μm, and the thickness H2 of the second diaphragm can be 6.3 μm, 6.5 μm, 6.8 μm, 7.0 μm, 7.3 μm, 7.5 μm, 7.8 μm, 8.0 μm, 8.3 μm, 8.5 μm, 8.8 μm, 9.0 μm, 9.3 μm, 9.5 μm, 9.8 μm, 10.0 μm, 10.3 μm, 10.5 μm. 4μm, 6.5μm, 6.6μm, 6.7μm, 6.8μm, 6.9μm, 7.0μm, 7.1μm, 7.2μm, 7.3μm, 7.5μm, 7.8μm, 8.0μm, 8.3μm, 8.5μm, 8.8μm, 9.0μm, 9.3μm, 9.5μm, 9.8μm, 10.0μm, 10.3μm, 10.5μm, 10.8μm, 11.0μm. By regulating the thickness H1 of the first diaphragm and the thickness H2 of the second diaphragm within the scope of the present application, it is beneficial to reduce the risk of lithium dendrites generated during the secondary battery cycle piercing the first diaphragm or the second diaphragm and causing a short circuit in the secondary battery. The first diaphragm and the second diaphragm have good mechanical strength, and at the same time, the transmission distance of lithium ions during the secondary battery cycle is moderate. Therefore, the secondary battery has a higher energy density, and the secondary battery has good cycle performance and safety performance.

[0065] The present application has no particular restrictions on the preparation method of the first diaphragm, as long as the purpose of the present application can be achieved. For example, the preparation method of the first diaphragm includes but is not limited to the following steps: (1) uniformly mixing the first ceramic particles and the first ceramic coating binder to obtain a first ceramic coating slurry; (2) uniformly mixing the first binder and the first thickener to obtain a first bonding layer slurry; (3) coating the first ceramic coating slurry on one surface of the first base film, and after drying, forming a first ceramic coating on one surface of the first base film; coating the first bonding layer slurry on the surface of the first ceramic coating away from the first base film, and after drying, forming a first bonding layer on the surface of the first ceramic coating away from the first base film, thereby obtaining the first diaphragm.

[0066] In the present application, the coating weight of the first ceramic coating layer and the coating weight of the first bonding layer can be controlled by means known to those skilled in the art. For example, when the first ceramic coating slurry is coated on the surface of the first base film, the coating amount of the first ceramic coating slurry is increased on the basis of a certain solid content of the first ceramic coating slurry to increase the coating weight of the first ceramic coating; when the first bonding layer slurry is coated on the surface of the first base film, the coating amount of the first bonding layer slurry is increased on the basis of a certain solid content of the first bonding layer slurry to increase the coating weight of the first bonding layer. This application is not particularly limited, as long as the purpose of this application can be achieved.

[0067] The present application has no particular restrictions on the preparation method of the second diaphragm, as long as the purpose of the present application can be achieved. For example, the preparation method of the second diaphragm includes but is not limited to the following steps: (1) uniformly mixing the second binder and the second thickener to obtain a second bonding layer slurry; (2) uniformly mixing the second ceramic particles and the second ceramic coating binder to obtain a second ceramic coating slurry; (3) coating the second bonding layer slurry on one surface of the second base film, and after drying, forming a second bonding layer on one surface of the second base film; coating the second ceramic coating slurry on the other surface of the second base film, and after drying, forming a second ceramic coating on the other surface of the second base film; coating the second bonding layer slurry on the surface of the second ceramic coating away from the second base film, and after drying, forming a second bonding layer on the surface of the second ceramic coating away from the second base film, thereby obtaining the second diaphragm.

[0068] In the present application, the coating weight of the second ceramic coating layer and the coating weight of the second bonding layer can be controlled by means known to those skilled in the art. For example, when the second ceramic coating slurry is coated on the surface of the second base film, the coating amount of the second ceramic coating slurry is increased on the basis of a certain solid content of the second ceramic coating slurry to increase the coating weight of the second ceramic coating; when the second bonding layer slurry is coated on the surface of the second base film, the coating amount of the second bonding layer slurry is increased on the basis of a certain solid content of the second bonding layer slurry to increase the coating weight of the second bonding layer. This application is not particularly limited, as long as the purpose of this application can be achieved.

[0069] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or composite current collector (such as lithium copper composite current collector, carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector, etc.). In the present application, there is no particular restriction on the thickness of the negative electrode current collector and the negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 15μm, the thickness of the single-sided negative electrode material layer is 30μm to 130μm, the thickness of the first negative electrode material layer is 30μm to 130μm, and the thickness of the second negative electrode material layer is 30μm to 130μm. Optionally, the negative electrode material layer, the first negative electrode material layer and the second negative electrode material layer may also include a conductive agent and a negative electrode binder. The present application has no particular restrictions on the type of conductive agent in the negative electrode material layer, the first negative electrode material layer and the second negative electrode material layer, as long as the purpose of the present application can be achieved. For example, for example, the conductive agent may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, flake graphite, Ketjen black, graphene, metal materials or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers, and specifically, the metal may include but are not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole. The present application does not particularly limit the type of negative electrode binder in the first negative electrode material layer and the second negative electrode material layer, as long as the purpose of the present application can be achieved. For example, the negative electrode binder may include but is not limited to at least one of polyvinylidene fluoride, vinylidene fluoride-hexafluoropropylene copolymer, polyamide, polyacrylonitrile, polyacrylate, polyacrylic acid, polyacrylate, polyvinyl pyrrolidone, polyvinyl ether, polymethyl methacrylate, polytetrafluoroethylene or polyhexafluoropropylene. The present application has no particular limitation on the mass ratio of the negative electrode active material, the conductive agent and the negative electrode binder in the first negative electrode material layer and the second negative electrode material layer, as long as the purpose of the present application can be achieved.

[0070] The present application has no particular restrictions on the positive electrode current collector, as long as the purpose of the present application can be achieved. For example, the positive electrode current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The positive electrode material layer of the present application includes a positive electrode active material, and the present application has no particular restrictions on the type of positive electrode active material, as long as the purpose of the present application can be achieved. For example, the positive electrode active material may include at least one of nickel cobalt manganese oxide (NCM811, NCM622, NCM523, NCM111), nickel cobalt aluminum oxide, lithium iron phosphate, lithium-rich manganese-based materials, lithium cobalt oxide (LiCoO2), lithium manganese oxide, lithium iron manganese phosphate or lithium titanate. In the present application, the positive electrode active material may also include non-metallic elements, such as non-metallic elements including at least one of fluorine, phosphorus, boron, chlorine, silicon or sulfur. In the present application, there is no particular restriction on the thickness of the positive electrode current collector and the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the thickness of the positive electrode current collector is 9μm to 15μm. The thickness of the single-sided positive electrode material layer is 30μm to 120μm. In the present application, the positive electrode material layer may also include a conductive agent and a positive electrode binder. The present application has no special restrictions on the type of binder in the positive electrode material layer, as long as the purpose of the present application can be achieved. For example, the positive electrode binder may be the same type as the negative electrode binder in the above-mentioned first negative electrode material layer and the second negative electrode material layer. The present application has no special restrictions on the type of conductive agent in the positive electrode material layer, as long as the purpose of the present application can be achieved. The conductive agent may be the same type as the conductive agent in the above-mentioned first negative electrode material layer and the second negative electrode material layer. The present application has no special restrictions on the mass ratio of the positive electrode active material, the conductive agent and the positive electrode binder in the positive electrode material layer. Those skilled in the art can choose according to actual needs, as long as the purpose of the present application can be achieved.

[0071] The secondary battery in the present application includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include at least one of LiPF6, LiNO3, LiBF4, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalate borate) (LiBOB), lithium bis(trifluoromethanesulfonyl imide) (LiTFSI) or lithium difluoroborate. The present application does not limit the content of lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. The present application has no special restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved. For example, the non-aqueous solvent may include but is not limited to at least one of a carbonate compound, a carboxylate compound, an ether compound or other organic solvents. The above-mentioned carbonate compound may include but is not limited to at least one of a chain carbonate compound, a cyclic carbonate compound or a fluorinated carbonate compound. The above-mentioned linear carbonate compound may include but is not limited to at least one of dimethyl carbonate, diethyl carbonate, dipropyl carbonate, methyl propyl carbonate, ethyl propyl carbonate or ethyl methyl carbonate. The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate, propylene carbonate (PC), butylene carbonate or vinyl ethylene carbonate. Fluorinated carbonate compounds may include but are not limited to at least one of fluoroethylene carbonate, 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include but is not limited to at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decanolactone, valerolactone or caprolactone. The above-mentioned ether compound may include but is not limited to at least one of dibutyl ether, tetraethylene glycol dimethyl ether, diethylene glycol dimethyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran. The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, cyclopentane, methyl cyclopentane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0072] The secondary battery of the present application also includes a packaging bag for containing a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, as well as other components known in the art in the secondary battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.

[0073] The secondary battery of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In one embodiment of the present application, the secondary battery may include, but is not limited to: a lithium metal secondary battery, a lithium ion secondary battery (lithium ion battery), a lithium polymer secondary battery, or a lithium ion polymer secondary battery, etc. In some embodiments of the present application, the secondary battery includes a lithium ion battery.

[0074] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and there is no particular limitation in the present application. For example, the preparation process of the secondary battery may include but is not limited to the following steps: stacking the positive electrode sheet, the first diaphragm, the negative electrode sheet, and the second diaphragm in order, winding them to obtain an electrode assembly of a winding structure, placing the electrode assembly in a shell, injecting the electrolyte into the shell and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the shell as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.

[0075] The second aspect of the present application provides an electrical device, which includes the secondary battery in any of the above embodiments. The secondary battery provided in the present application has high energy density while having a long cycle life and good safety performance. Therefore, the electrical device of the present application has a long service life.

[0076] The electrical device of the present application is not particularly limited, and it can be any electrical device known in the prior art. For example, the electrical device can include, but is not limited to, a laptop computer, a pen-input computer, a mobile computer, an electronic book player, a portable phone, a portable fax machine, a portable copier, a portable printer, a head-mounted stereo headset, a video recorder, an LCD television, a portable cleaner, a portable CD player, a mini-disc, a transceiver, an electronic notepad, a calculator, a memory card, a portable recorder, a radio, a backup power supply, a motor, a car, a motorcycle, a power-assisted bicycle, a bicycle, a lighting fixture, a toy, a game console, a clock, an electric tool, a flashlight, a camera, a large household battery, and a lithium-ion capacitor.

[0077] Example

[0078] The following examples and comparative examples are given to more specifically describe the embodiments of the present application. Various tests and evaluations were performed according to the following methods. In addition, unless otherwise specified, "parts" and "%" are based on mass.

[0079] Test methods and equipment:

[0080] Tests on the coating element type and its mass percentage W1, the doping element type and its mass percentage W1' in the first negative electrode material layer, and the coating element type and its mass percentage W2, the doping element type and its mass percentage W2' in the second negative electrode material layer:

[0081] The lithium-ion battery was disassembled after being discharged to 3V at 0.2C, the negative electrode sheet was taken out, and the negative electrode sheet was cleaned with dimethyl carbonate (DMC). Among them, the first negative electrode material layer is a longer layer, and the second negative electrode material layer is a shorter layer.

[0082] Cut a cross section of the negative electrode sheet along the thickness direction, and use plasma polishing, then use a scanning electron microscope combined with an energy spectrometer to test to obtain the types of coating elements and doping elements in the first negative electrode material layer. When the element is mainly distributed on the surface of the first negative electrode active material particles, the corresponding element is a coating element; when the element is mainly dispersed inside the first negative electrode active material particles, the corresponding element is a doping element. Thus, the types of coating elements or doping elements in the first negative electrode material layer are obtained.

[0083] By replacing the first negative electrode material layer in the above step with the second negative electrode material layer, the types of coating elements or doping elements in the second negative electrode material layer can be obtained.

[0084] The first negative electrode material layer on the surface of the negative electrode current collector in the negative electrode sheet is scraped off, then weighed, concentrated nitric acid is added for microwave digestion to obtain a solution, and the obtained solution and filter residue are washed multiple times and fixed to volume, and the plasma intensity of the coating element therein is tested by inductively coupled plasma emission spectrometer (ICP-OES), and the content of the coating element in the solution is calculated according to the standard curve of the measured element, thereby calculating the mass percentage content W1 of the coating element in the first negative electrode active material layer. In the above steps, the plasma intensity of the coating element is changed to the plasma intensity of the doping element, and the mass percentage content W1' of the doping element in the first negative electrode material layer can be obtained accordingly.

[0085] By replacing the first negative electrode material layer in the above step with the second negative electrode material layer, the mass percentage content W2 of the coating element in the second negative electrode active material layer and the mass percentage content W2' of the doping element in the second negative electrode material layer can be obtained.

[0086] First and second diaphragm sampling methods

[0087] The lithium-ion batteries in the tested embodiments and comparative examples were disassembled, the first diaphragm and the second diaphragm were taken out, and the electrolyte residue was removed by soaking in dimethyl carbonate (DMC) for 20 minutes, and then the first diaphragm and the second diaphragm were placed in an oven and dried at 60°C for 12 hours to obtain the first diaphragm sample and the second diaphragm sample. The above method was used to obtain the first diaphragm and the second diaphragm in the following tests unless otherwise specified.

[0088] Sampling method of the first basement membrane and the second basement membrane:

[0089] The first diaphragm and the second diaphragm obtained above were placed in containers respectively, and an appropriate amount of N-methylpyrrolidone (NMP) was added. The containers were placed in an ultrasonic instrument with a heating function for ultrasonication, and the temperature was controlled at 45°C for 3 hours. When the first diaphragm and the second diaphragm became completely transparent, they were taken out to obtain the first basement membrane and the second basement membrane. The above method was used to obtain the first basement membrane and the second basement membrane in the following tests unless otherwise specified.

[0090] Porosity test of the first base film and the second base film:

[0091] The gas displacement method is adopted for testing, and the first basement membrane and the second basement membrane are punched out by molds to prepare samples respectively (technical personnel in this field can select molds of common sizes and shapes in this field according to factors such as the size and shape of the test object and the requirements of the test equipment), and the true volume V0 of the sample is measured by a true density tester. The apparent volume V of the sample can be calculated by measuring the area and thickness of the sample. Then, the percentage of the pore volume of the sample to the total area P = (V-V0) / V×100%, that is, the porosity of the first basement membrane or the second basement membrane is obtained respectively.

[0092] Pore ​​size test of the first base film and the second base film:

[0093] The specific steps are as follows:

[0094] ① Use anhydrous ethanol to completely wet and fill the pores of the base membrane to be tested, so that positive pressure is formed in the pores due to capillary phenomenon;

[0095] ②Put the basement membrane into a closed tank and use gas pressure to squeeze the liquid out of the capillary pores;

[0096] ③ According to the relative relationship between the pressure ΔP applied when the liquid in a single pore is completely squeezed out of the capillary pore and the pore diameter d, the basement membrane pore size can be obtained according to the Laplace equation. The Laplace equation is shown as follows:

[0097] d=-4γcosθ / ΔP×100%

[0098] Wherein, d is the pore diameter (aperture), ΔP is the pressure, γ is the surface tension of anhydrous ethanol, and θ is the contact angle between the diaphragm and anhydrous ethanol. At different pressures, the liquid in the basement membrane will be squeezed out successively and a certain gas penetration flow rate will be generated. The pore size and pore size distribution can be calculated based on the relationship between pressure and flow changes. The above basement membrane is the first basement membrane or the second basement membrane.

[0099] Thickness test of the first and second diaphragms:

[0100] The first diaphragm was subjected to argon ion polishing to obtain a cross section of the first diaphragm, and the cross section of the first diaphragm along the thickness direction was observed by a field emission scanning electron microscope (Philips, XL-30 model) and a scanning electron microscope photograph was taken, and the thickness H1 of the first diaphragm was measured by the scanning electron microscope. The first diaphragm was replaced by the second diaphragm, and the thickness H2 of the second diaphragm was measured.

[0101] Cycle performance test:

[0102] At 25°C, the lithium-ion battery was charged to 4.5V at 2C constant current, and then charged to 0.02C at 4.5V constant voltage. After standing for 5 minutes, it was discharged to 3.0V at 0.7C constant current. This was the first cycle, and the discharge capacity was recorded. The lithium-ion battery was charged and discharged according to the above process. When the cycle reached 1000 cycles (cls), the test was stopped and the capacity retention rate was calculated as an indicator for evaluating the cycle performance of the lithium-ion battery.

[0103] Capacity retention rate (%) = (discharge capacity after 1000 cycles / first cycle discharge capacity) × 100%.

[0104] Drop test

[0105] At 25℃, charge the lithium-ion battery to 4.5V at 2C, then charge it to 0.02C at 4.5V. At 20±5℃, clamp the lithium-ion battery and drop it from a height of 1m to a concrete drop floor. Perform one test, then perform one test from a height of 1.25m and one test from a height of 1.5m. Perform the above three tests on one side. The order of drop is to perform drop tests on the six sides of the lithium-ion battery, specifically the first three times, the last three times, the top three times, the bottom three times, the left three times, and the right three times. Judgment criteria: No fire, no explosion, no smoke, no leakage, no rupture, no deflation, no disintegration is considered to pass the drop test. Each group tests 10 batteries.

[0106] Drop test pass rate (%) = (number of lithium-ion batteries that passed the drop test / 10) × 100%. The greater the drop test pass rate, the better the safety performance of the lithium-ion battery.

[0107] Extrusion test

[0108] In an environment of 25℃, charge the lithium-ion battery with a current of 2C to 4.5V, and then charge it with a voltage of 4.5V to a current of 0.02C. In a test environment of 20±5℃, place the lithium-ion battery on the test table, with 5 lithium-ion batteries facing up and 5 lithium-ion batteries facing up (along the thickness direction of the lithium-ion battery, one side is the front side and the other side is the back side). Use a blunt nail with a diameter of 6mm, a falling speed of 300N / min, and an extrusion force of 1550N. Test the sample lithium-ion battery body 12mm away from the top seal. The judgment standard is: if there is no fire or explosion, it is considered to have passed the extrusion test. 10 batteries are tested in each group.

[0109] Extrusion test pass rate (%) = (number of lithium-ion batteries that passed the extrusion test / 10) × 100%. The greater the extrusion test pass rate, the better the safety performance of the lithium-ion battery.

[0110] Acupuncture test

[0111] At 25℃, charge the lithium-ion battery at 2C to 4.5V, then charge at 4.5V to 0.02C. Place the lithium-ion battery on the test table at 20±5℃. Use a 3mm diameter nail at a speed of 150mm / s to completely pierce the battery from the center of the lithium-ion battery. If there is no fire, explosion or smoke, the battery is considered to have passed the puncture test. Ten batteries are tested in each group.

[0112] The pass rate of the puncture test (%) = (the number of lithium-ion batteries that passed the puncture test / 10) × 100%. The greater the pass rate of the puncture test, the better the safety performance of the lithium-ion battery.

[0113] Energy density test:

[0114] Place the lithium-ion battery in a 25℃±2℃ constant temperature box and let it stand for 30 minutes to allow the lithium-ion battery to reach a constant temperature. Charge the lithium-ion battery that has reached a constant temperature at a constant current of 0.5C to a full charge voltage of 4.5V, then charge it at a full charge voltage of 4.5V to a current of 0.05C, and discharge it at a constant current of 0.2C to a voltage of 3.0V, and record the discharge energy.

[0115] Volume energy density = discharge energy / (length of lithium ion battery × width of lithium ion battery × thickness of lithium ion battery). The length, width and thickness of the secondary battery in Table 4 were measured by a micrometer, and each value was measured 3 times, and the average value was taken as the final result.

[0116] Example 1-1

[0117] <Preparation of First Separator>

[0118] A polyimide film with a thickness h1 of 5 μm is used as the first base film, the porosity P1 of the first base film is 55%, and the pore size D1 of the first base film is 380 nm.

[0119] The first binder polyvinylidene fluoride (PVDF, Mw = 8.5 × 10 6 ) and the first thickener sodium carboxymethyl cellulose (Mw = 8 × 10 5 ) are mixed in a mass ratio of 98.5:1.5, deionized water is added as a solvent, and the mixture is stirred evenly to form a first bonding layer slurry with a solid content of 75wt%.

[0120] The first ceramic particles of aluminum oxide (Al2O3), the first ceramic coating binder styrene butadiene rubber (Mw = 7 × 10 6 ), mixed in a mass ratio of 3:7, adding deionized water as a solvent, and stirring evenly to obtain a first ceramic coating slurry with a solid content of 45wt%.

[0121] A first ceramic coating slurry is coated on one surface of the first base film, and after drying at 60°C, a first ceramic coating is formed on one surface of the first base film; a first bonding layer slurry is coated on the surface of the first ceramic coating away from the first base film, and after drying, a first bonding layer is formed on the surface of the first ceramic coating away from the first base film, thus obtaining a first diaphragm. The coating weight CW2 of the first bonding layer is 0.0006 mg / mm 2 The coating weight CW1 of the first ceramic coating is 10 mg / cm 2 Based on the mass of the first ceramic coating, the mass percentage C1 of the first ceramic particles is 30%.

[0122] <Preparation of Second Separator>

[0123] A polyimide film with a thickness h2 of 5 μm is used as the second base film, the porosity P2 of the second base film is 28%, and the pore size D2 of the second base film is 120 nm.

[0124] The second binder polyvinylidene fluoride (PVDF, Mw = 8.5 × 10 6 ) and the second thickener sodium carboxymethyl cellulose (Mw = 8 × 10 5 ) are mixed in a mass ratio of 98.5:1.5, deionized water is added as a solvent, and after stirring evenly, a second bonding layer slurry with a solid content of 75wt% is formed.

[0125] The first ceramic particles of aluminum oxide (Al2O3), the first ceramic coating binder styrene butadiene rubber (Mw = 7 × 10 6 ), mixed in a mass ratio of 3:7, adding deionized water as a solvent, and stirring evenly to obtain a first ceramic coating slurry with a solid content of 45wt%.

[0126] A second bonding layer slurry is coated on one surface of the second base film, and after drying at 60°C, a second bonding layer is formed on one surface of the second base film; a second ceramic coating slurry is coated on the other surface of the second base film, and after drying at 60°C, a second ceramic coating is formed on the other surface of the second base film; a second bonding layer slurry is coated on the surface of the second ceramic coating away from the second base film, and after drying, a second bonding layer is formed on the surface of the second ceramic coating away from the second base film, thus obtaining a second diaphragm. The coating weight CW4 of the second bonding layer is 0.0006 mg / mm 2 The coating weight of the second ceramic coating CW3 is 10 mg / cm 2 Based on the mass of the second ceramic coating, the mass percentage content C2 of the second ceramic particles is 30%.

[0127] <Preparation of negative electrode sheet>

[0128] The negative electrode active materials artificial graphite, styrene-butadiene rubber, and sodium carboxymethyl cellulose are mixed in a mass ratio of 97.6:1.1:1.3, and then deionized water is added as a solvent. After stirring evenly, a first negative electrode slurry with a solid content of 70wt% is obtained. At the same time, the first negative electrode slurry is also used as the second negative electrode slurry. The first negative electrode slurry is coated on one surface of a negative electrode current collector copper foil with a thickness of 6μm, and dried at 90°C to obtain a negative electrode sheet with a first negative electrode material layer coated with a thickness of 50μm. The second negative electrode slurry is coated on the other surface of the negative electrode current collector copper foil. After drying, the second negative electrode material layer coated on the surface has a thickness of 50μm, and then the total thickness of the negative electrode sheet is 106μm. The negative electrode sheet after coating is cold pressed and then cut into a specification of 74mm×824mm for standby use. Among them, the compaction density of the first negative electrode material layer is 1.735g / cm 3 , length is 720mm, and the compaction density of the second negative electrode material layer is 1.735g / cm 3 , with a length of 680 mm, one end of the first negative electrode material layer and the second negative electrode material layer are flush, and at the other end, the first negative electrode material layer is longer than the second negative electrode material layer.

[0129] <Preparation of positive electrode sheet>

[0130] The positive electrode active material lithium cobalt oxide, the conductive agent conductive carbon black and the positive electrode binder polyvinylidene fluoride are mixed in a mass ratio of 95:2.5:2.5, N-methylpyrrolidone (NMP) is added as a solvent, and the mixture is stirred and evenly mixed to form a positive electrode slurry with a solid content of 75wt%. The positive electrode slurry is evenly coated on one surface of a positive electrode current collector aluminum foil with a thickness of 10μm, and dried at 90°C to obtain a positive electrode sheet with a single-sided coating thickness of 55μm. The positive electrode slurry is coated on the other surface of the positive electrode current collector aluminum foil. After drying, the thickness of the positive electrode material layer coated on the surface is 55μm, that is, a positive electrode sheet with a double-sided coating of positive electrode material layers and a total thickness of 120μm is obtained. The positive electrode sheet after coating is cold pressed and then cut into a specification of 70mm×800mm for standby use. Among them, the compaction density of the first positive electrode material layer is 4.23g / cm 3 , length is 750mm, and the compaction density of the second positive electrode material layer is 4.23g / cm 3 , with a length of 680 mm, one end of the first positive electrode material layer and the second positive electrode material layer are flush, and at the other end, the first positive electrode material layer is longer than the second positive electrode material layer.

[0131] <Preparation of Electrolyte>

[0132] In a glove box filled with dry argon atmosphere, propylene carbonate (PC), diethyl carbonate (DEC), and ethylene carbonate (EC) are mixed at a mass ratio of 1:1:1 to obtain a base solvent, and then lithium hexafluorophosphate (LiPF6) lithium salt is added to the base solvent to dissolve and mix well to obtain an electrolyte. Among them, based on the mass of the electrolyte, the mass percentage of LiPF6 is 12%, and the remainder is the base solvent.

[0133] <Preparation of lithium-ion batteries>

[0134] The positive electrode sheet, the first separator, the negative electrode sheet, and the second separator prepared above are stacked in order, and then wound to obtain an electrode assembly. The positive electrode tab is spot welded out with an aluminum tab, and the negative electrode tab is spot welded out with a nickel tab. Among them, the first negative electrode material layer is close to the first separator, the first ceramic coating is located on the side of the first base film away from the first negative electrode material layer, the second negative electrode material layer is close to the second separator, the second ceramic coating is located on the side of the second base film away from the second negative electrode material layer, the first positive electrode material layer is close to the first separator and adjacent to the first bonding layer (the specific structure can be referred to Figure 1 The electrode assembly was placed in an aluminum-plastic film, dried in a vacuum oven at 80°C for 12 hours to remove moisture, and then injected with the above-prepared electrolyte. After vacuum packaging, standing, formation (charging at 0.02C constant current to 3.5V, and then charging at 0.1C constant current to 3.9V), capacity, and shaping processes, a lithium-ion battery was obtained.

[0135] Example 1-2 to Example 1-16

[0136] Except for adjusting the relevant preparation parameters according to Table 1, the rest is the same as Example 1-1. Among them, when the negative electrode material layer includes a doping element, the mass percentage of the doping element in the selected negative electrode active material = the mass percentage of the doping element in the negative electrode material layer / the mass percentage of the negative electrode active material in the negative electrode material layer × 100%; when the negative electrode material layer includes a coating element, the mass percentage of the coating element in the selected negative electrode active material = the mass percentage of the coating element in the negative electrode material layer / the mass percentage of the negative electrode active material in the negative electrode material layer × 100%. In the present application, the mass percentage of the negative electrode active material in the negative electrode material layer is 97.6%.

[0137] Example 2-1 to Example 2-14

[0138] Except for adjusting the relevant preparation parameters according to Table 2, the rest is the same as Example 1-1.

[0139] Example 2-15 to Example 2-23

[0140] Except for adjusting the relevant preparation parameters according to Table 2, the rest are the same as Example 1-2, Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-9, Example 1-16, Example 1-16, and Example 1-16.

[0141] Example 3-1 to Example 3-15

[0142] Except for adjusting the relevant preparation parameters according to Table 3, the rest is the same as Example 1-1.

[0143] Example 3-16 to Example 3-24

[0144] Except for adjusting the relevant preparation parameters according to Table 3, the rest are the same as Example 1-2, Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-9, Example 1-16, Example 1-16, and Example 1-16.

[0145] Example 4-1 to Example 4-10

[0146] Except for adjusting the relevant preparation parameters according to Table 4, the rest is the same as Example 1-1.

[0147] Example 4-11 to Example 4-16

[0148] Except for adjusting the relevant preparation parameters according to Table 4, the rest are the same as Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-16, and Example 1-16.

[0149] Example 5-1 to Example 5-14

[0150] Except for adjusting the relevant preparation parameters according to Table 5, the rest is the same as Example 1-1. When the mass percentage content C1 of the first ceramic particles changes, the content of the first ceramic coating binder changes accordingly, and the sum of the mass percentage content of the first ceramic particles and the mass percentage content of the first ceramic coating binder is 100%. When the mass percentage content C2 of the second ceramic particles changes, the content of the second ceramic coating binder changes accordingly, and the sum of the mass percentage content of the second ceramic particles and the mass percentage content of the second ceramic coating binder is 100%.

[0151] Example 5-15 to Example 5-20

[0152] Except for adjusting the relevant preparation parameters according to Table 5, the rest are the same as Example 1-2, Example 1-2, Example 1-9, Example 1-9, Example 1-16, and Example 1-16. When the mass percentage C1 of the first ceramic particles changes, the content of the first ceramic coating binder changes accordingly, and the sum of the mass percentage of the first ceramic particles and the mass percentage of the first ceramic coating binder is 100%. When the mass percentage C2 of the second ceramic particles changes, the content of the second ceramic coating binder changes accordingly, and the sum of the mass percentage of the second ceramic particles and the mass percentage of the second ceramic coating binder is 100%.

[0153] Comparative Example 1

[0154] Except that in the process of <Preparation of the Second Diaphragm>, only one second bonding layer is coated on the surface of the second diaphragm, that is, the second bonding layer is coated on the surface of the second ceramic coating, the rest is the same as Example 1-1.

[0155] Comparative Example 2

[0156] Except that during the <Preparation of the First Diaphragm>, the surface of the first diaphragm is coated with two first bonding layers, that is, the first bonding layer is coated on the surface of the first ceramic coating, and at the same time, the first adhesive layer is coated on the other surface of the first base film, the rest is the same as Example 1-1.

[0157] Comparative Example 3

[0158] Except that during the <Preparation of the First Diaphragm> process, the surface of the first diaphragm is coated with two layers of the first bonding layer, that is, the first bonding layer is coated on the surface of the first ceramic coating, and at the same time, the first adhesive layer is coated on the other surface of the first base film, during the <Preparation of the Second Diaphragm> process, the surface of the second diaphragm is only coated with one layer of the second bonding layer, that is, the second bonding layer is coated on the surface of the second ceramic coating, and the rest is the same as Example 1-1.

[0159] The preparation parameters and performance parameters of each embodiment and comparative example are shown in Tables 1 to 5.

[0160] Table 1

[0161]

[0162]

[0163] Note: “ / ” in Table 1 indicates no relevant preparation parameters.

[0164] It can be seen from Examples 1-1 to 1-16 and Comparative Examples 1 to 3 that the negative electrode sheet is located between the first diaphragm and the second diaphragm, the electrode assembly includes a straight area and a corner area, and the first diaphragm and the second diaphragm are used together to enable the lithium-ion battery to have a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate, and a higher puncture test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery are taken into account. In Comparative Example 1, the first diaphragm includes a bonding layer, and the second diaphragm includes a bonding layer. The lithium-ion battery has a lower extrusion test pass rate, a lower drop test pass rate, and a higher puncture test pass rate, indicating that the safety performance of the lithium-ion battery is poor; in Comparative Example 2, the first diaphragm includes two bonding layers, and the second diaphragm includes two bonding layers, and the capacity retention rate of the lithium-ion battery is low, indicating that the cycle performance of the lithium-ion battery is poor; in Comparative Example 3, the first diaphragm includes two bonding layers, and the second diaphragm includes one bonding layer, and the capacity retention rate of the lithium-ion battery is low, indicating that the cycle performance of the lithium-ion battery is poor. That is, Comparative Examples 1 to 3 cannot take into account both the cycle performance and the safety performance of the lithium-ion battery, while in Examples 1-1 to 1-16, the first diaphragm and the second diaphragm are within the scope of the present application, and the lithium-ion battery has a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate and a higher puncture test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery are taken into account.

[0165] The type of coating element in the first negative electrode active material layer and the mass percentage of the coating element, and the type of coating element in the second negative electrode active material layer and the mass percentage of the coating element usually affect the cycle performance of the lithium ion battery. It can be seen from Examples 1-1 and 1-2 to 1-8 that by regulating the type of coating element in the first negative electrode active material layer and the mass percentage of the coating element, and the type of coating element in the second negative electrode active material layer and the mass percentage of the coating element within the scope of the present application, the lithium ion battery has a higher capacity retention rate, and also has a higher extrusion test pass rate, a higher drop test pass rate and a higher puncture test pass rate, further improving the cycle performance of the lithium ion battery, indicating that the cycle performance and safety performance of the lithium ion battery can be taken into account.

[0166] The type of doping elements in the first negative electrode active material layer and the mass percentage of the doping elements, and the type of doping elements in the second negative electrode active material layer and the mass percentage of the doping elements usually affect the cycle performance of the lithium ion battery. It can be seen from Examples 1-1, 1-3, 1-9 to 1-16 that by regulating the type of doping elements in the first negative electrode active material layer and the mass percentage of the doping elements, and the type of doping elements in the second negative electrode active material layer and the mass percentage of the doping elements within the scope of the present application, the lithium ion battery has a higher capacity retention rate, and also has a higher extrusion test pass rate, a higher drop test pass rate and a higher puncture test pass rate, further improving the cycle performance of the lithium ion battery, indicating that the cycle performance and safety performance of the lithium ion battery can be taken into account.

[0167] Table 2

[0168]

[0169]

[0170] The porosity of the first base film and the porosity of the second base film usually affect the cycle performance and safety performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-2, 1-9, 1-16, and 2-1 to 2-23 that by regulating the porosity of the first base film and the porosity of the second base film within the scope of the present application and satisfying that the porosity of the first base film is greater than the porosity of the second base film, the lithium-ion battery can have a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate, and a higher puncture test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery can be taken into account.

[0171] Table 3

[0172]

[0173]

[0174] The pore size of the first base membrane and the pore size of the second base membrane usually affect the cycle performance and safety performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-2, 1-9, 1-16, and 3-1 to 3-24 that by regulating the pore size of the first base membrane and the pore size of the second base membrane within the scope of the present application and satisfying that the pore size of the first base membrane is larger than the pore size of the second base membrane, the lithium-ion battery can have a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate, and a higher puncture test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery can be taken into account.

[0175] Table 4

[0176]

[0177] The coating weight of the first ceramic coating and / or the coating weight of the second ceramic coating usually affects the cycle performance and safety performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-2, 1-9, 1-16, and 4-7 to 4-16 that by adjusting the coating weight of the first ceramic coating and / or the coating weight of the second ceramic coating within the scope of this application, the lithium-ion battery can have a higher energy density, a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate, and a higher puncture test pass rate, indicating that the lithium-ion energy density, battery cycle performance, and safety performance are taken into account. Compared with Examples 1-1, 4-7, and 4-8, the coating weight of the first ceramic coating and the coating weight of the second ceramic coating in Example 4-9 are smaller, less than 7 mg / cm 2 Although the energy density of lithium-ion batteries is relatively large, the electrolyte infiltration is slightly poor, the capacity retention rate of lithium-ion batteries is relatively low, and the improvement of the cycle performance of lithium-ion batteries is relatively weak; compared with Example 1-1, Example 4-7 and Example 4-8, the coating weight of the first ceramic coating and the coating weight of the second ceramic coating in Example 4-10 are larger, greater than 13 mg / cm 2 Although the mechanical properties of the diaphragm are good, the lithium-ion battery can have a higher pass rate of the extrusion test, a higher pass rate of the drop test and a higher pass rate of the puncture test, that is, the safety performance of the lithium-ion battery is higher, but the distance between the positive electrode and the negative electrode is large, and the active metal ions (Li +) The transmission path is long, the capacity retention rate of the lithium-ion battery is low, the improvement of the cycle performance of the lithium-ion battery is weak, and the energy density of the lithium-ion battery is low. It is shown that by adjusting the coating weight of the first ceramic coating and the coating weight of the second ceramic coating within the scope of the present application, the energy density, cycle performance and safety performance of the lithium-ion battery can be better taken into account. The coating weight of the first adhesive layer and / or the coating weight of the second adhesive layer usually affect the cycle performance and safety performance of the lithium-ion battery. It can be seen from Example 1-1, Example 1-2, Example 1-9, Example 1-16, Example 4-1 to Example 4-6, and Example 4-11 to 4-16 that by adjusting the coating weight of the first adhesive layer and / or the coating weight of the second adhesive layer within the scope of the present application, the lithium-ion battery can have a higher energy density, a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate and a higher puncture test pass rate, indicating that the energy density, cycle performance and safety performance of the lithium-ion battery can be taken into account. Compared with Example 1-1 and Example 4-1 to Example 4-4, the coating weight of the first adhesive layer and the coating weight of the second adhesive layer in Example 4-5 are smaller, less than 0.0004 mg / mm 2 The bonding between the diaphragm and the electrode is weak, and the active metal ions (such as Li + ) The transmission path is longer, and the improvement of the cycle performance of the lithium-ion battery is weak; compared with Example 1-1, Example 4-1 to Example 4-4, the coating weight of the first adhesive layer and the coating weight of the second adhesive layer in Example 4-6 are larger, greater than 0.002 mg / mm 2 , although the diaphragm has good adhesion with the pole piece, the lithium-ion battery can have a higher extrusion test pass rate, a higher drop test pass rate and a higher needle test pass rate, that is, the safety performance of the lithium-ion battery is higher, but the electrolyte infiltration is poor, the improvement of the cycle performance of the lithium-ion battery is weak, and the energy density of the secondary battery is affected. It is thus shown that by regulating the coating weight of the first adhesive layer and the coating weight of the second adhesive layer within the scope of the present application, the energy density, cycle performance and safety performance of the lithium-ion battery can be better taken into account. The thickness of the first diaphragm and the thickness of the second diaphragm usually affect the cycle performance and safety performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-2, 1-9, 1-16, 4-1 to 4-16 that by regulating the thickness of the first diaphragm and the thickness of the second diaphragm within the scope of the present application, the lithium-ion battery can have a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate and a higher needle test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery can be taken into account.

[0178] Table 5

[0179]

[0180] The type of the first binder and / or the type of the second binder usually affects the cycle performance and safety performance of the lithium-ion battery. It can be seen from Example 1-1 and Example 5-1 to Example 5-3 that the type of the first binder and / or the type of the second binder within the scope of the present application can enable the lithium-ion battery to have a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate and a higher puncture test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery can be taken into account.

[0181] The type of the first ceramic particles and / or the type of the second ceramic particles usually affect the cycle performance and safety performance of the lithium-ion battery. It can be seen from Example 1-1, Example 5-4 to Example 5-6 that the type of the first ceramic particles and / or the type of the second ceramic particles within the scope of the present application can enable the lithium-ion battery to have a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate and a higher puncture test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery can be taken into account.

[0182] The mass percentage of the first ceramic particles and / or the mass percentage of the second ceramic particles usually affect the cycle performance and safety performance of the lithium-ion battery. It can be seen from Examples 1-1, 1-2, 1-9, 1-16, 5-7 to 5-20 that by regulating the mass percentage of the first ceramic particles and / or the mass percentage of the second ceramic particles within the scope of the present application, the lithium-ion battery can have a higher capacity retention rate, a higher extrusion test pass rate, a higher drop test pass rate and a higher puncture test pass rate, indicating that the cycle performance and safety performance of the lithium-ion battery can be taken into account.

[0183] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the scope of protection of the present application.

Claims

1. A secondary battery, comprising an electrode assembly of a wound structure, the electrode assembly comprising a positive electrode sheet, a negative electrode sheet, a first separator and a second separator, the negative electrode sheet is located between the first separator and the second separator, and the electrode assembly comprises a straight area and a corner area; The negative electrode sheet comprises a negative electrode current collector and a first negative electrode material layer and a second negative electrode material layer located on both sides of the negative electrode current collector in a thickness direction, the first separator is adjacent to the first negative electrode material layer, and the second separator is adjacent to the second negative electrode material layer; The first separator in the corner area includes a first base film, a first bonding layer and a first ceramic coating, the first base film is in contact with the first negative electrode material layer, the first ceramic coating is arranged on a side of the first base film away from the first negative electrode material layer, and the first bonding layer is arranged on a surface of the first ceramic coating; The second separator in the corner area comprises a second base film, a second bonding layer and a second ceramic coating, wherein the second bonding layer is arranged on both sides of the second base film, the second ceramic coating is arranged on a side of the second base film away from the second negative electrode material layer, and the second ceramic coating is located between the second base film and the second bonding layer; In the corner area, a positive electrode sheet corner segment is adjacent to a first negative electrode material layer corner segment, the positive electrode sheet corner segment is farther away from the winding center of the electrode assembly than the first negative electrode material layer corner segment, the first diaphragm is located between the positive electrode sheet corner segment and the first negative electrode material layer corner segment, and the positive electrode sheet corner segment is in contact with the first bonding layer.

2. The secondary battery according to claim 1, wherein Along the winding direction of the electrode assembly, the length of the first negative electrode material layer is greater than the length of the second negative electrode material layer.

3. The secondary battery according to claim 1, wherein The positive electrode sheet includes a positive electrode current collector and a first positive electrode material layer and a second positive electrode material layer located on both sides of the positive electrode current collector in the thickness direction. In the same winding layer, the first positive electrode material layer is closer to the winding center of the electrode assembly than the second positive electrode material layer. Along the winding direction of the electrode assembly, the length of the first positive electrode material layer is greater than the length of the second positive electrode material layer.

4. The secondary battery according to claim 1, wherein The first negative electrode material layer includes a first negative electrode active material, the second negative electrode material layer includes a second negative electrode active material, and the secondary battery satisfies at least one of the following characteristics: (1) The surface of the particles of the first negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage W1 of the coating element is 0.05% to 0.5% based on the mass of the first negative electrode material layer; (2) The surface of the particles of the second negative electrode active material includes a coating element, the coating element includes at least one of Ag, Ni, Sn, Zn, Al, Mo, Cu or Fe, and the mass percentage content W2 of the coating element is 0.05% to 0.5% based on the mass of the second negative electrode material layer; (3) The first negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and the mass percentage content W1' of the doping element is 0.05% to 0.5% based on the mass of the first negative electrode material layer; (4) The second negative electrode active material includes a doping element, the doping element includes at least one of B, Ti, Cu or Ni, and the mass percentage W2' of the doping element is 0.05% to 0.5% based on the mass of the second negative electrode material layer.

5. The secondary battery according to claim 4, wherein The first negative electrode active material and the second negative electrode active material each independently include natural graphite, artificial graphite, mesophase micro carbon beads, hard carbon, soft carbon, silicon, silicon-carbon composite, SiO x , Li-Sn alloy, Li-Sn-O alloy, Sn, SnO, SnO2, spinel structure lithium titanate Li4Ti5O 12 , Li-Al alloy or at least one of metallic lithium, 0 <x<2。 6. The secondary battery according to any one of claims 1 to 5, wherein The porosity P1 of the first base film is greater than the porosity P2 of the second base film, 40%≤P1≤70%, 5%≤P2≤50%.

7. The secondary battery according to claim 6, wherein 50%≤P1≤60%, 10%≤P2≤40%.

8. The secondary battery according to any one of claims 1 to 5, wherein The pore size D1 of the first base film is larger than the pore size D2 of the second base film, 80nm≤D1≤700nm, 50nm≤D2≤200nm.

9. The secondary battery according to claim 8, wherein 250nm≤D1≤520nm, 100nm≤D2≤150nm.

10. The secondary battery according to any one of claims 1 to 5, wherein The coating weight of the first ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight of the first adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 .

11. The secondary battery according to any one of claims 1 to 5, wherein The coating weight of the second ceramic coating is 7 mg / cm 2 Up to 13mg / cm 2 , and / or, the coating weight of the second adhesive layer is 0.0004 mg / mm 2 To 0.002mg / mm 2 .

12. The secondary battery according to any one of claims 1 to 5, wherein The first adhesive layer includes a first adhesive, the second adhesive layer includes a second adhesive, and the first adhesive and the second adhesive each independently include at least one of polyvinylidene fluoride, polyacrylonitrile, polyethylene oxide or polyimide.

13. The secondary battery according to any one of claims 1 to 5, wherein The first ceramic coating includes first ceramic particles, and the second ceramic coating includes second ceramic particles, and the first ceramic particles and the second ceramic particles each independently include at least one of aluminum oxide, boehmite, silicon oxide, magnesium oxide, titanium oxide, tin oxide, calcium oxide, zirconium oxide, yttrium oxide, silicon carbide, aluminum hydroxide, magnesium hydroxide or calcium hydroxide.

14. The secondary battery according to claim 13, wherein Based on the mass of the first ceramic coating, the mass percentage of the first ceramic particles is 10% to 50%; based on the mass of the second ceramic coating, the mass percentage of the second ceramic particles is 10% to 50%.

15. The secondary battery according to any one of claims 1 to 5, wherein The thickness H1 of the first diaphragm is 6.0 μm to 10.5 μm, and the thickness H2 of the second diaphragm is 6.3 μm to 11.0 μm. 16 . An electric device comprising the secondary battery according to claim 1 .

Citation Information

Cited By

  • Secondary battery and electric device

    CN119650975A

  • Battery cell, battery and electric device

    CN119944101A

  • Battery, electric device, and box body

    WO2026123904A1