Carbon-containing agglomerate for blast furnace and method for operating blast furnace using same
Optimizing the composition of carbon-containing agglomerated ores with specific carbon and metallic iron ratios addresses the challenge of reducing the reducing agent ratio, achieving efficient blast furnace operations with reduced emissions.
Patent Information
- Application Number
- JP2021033864
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-03
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-03-03
AI Technical Summary
Existing carbon-containing agglomerated ores for blast furnaces do not have a suitable combination of metallic iron and carbon, limiting the reduction of the reducing agent ratio, which is essential for reducing carbon dioxide emissions.
A carbon-containing agglomerated ore composition with a total mass of 70% or more, comprising 15 to 25% carbon and a mass ratio of metallic iron to carbon between 0.4 to 0.8, optimized to enhance carbon gasification and catalytic effects, thereby reducing the reducing agent ratio.
The optimized composition significantly reduces the reducing agent ratio to 5 to 30 kg/t-HM, enhancing the efficiency of blast furnace operations while minimizing carbon dioxide emissions.
Smart Images

Figure 0007575683000003 
Figure 0007575683000004 
Figure 0007575683000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon-containing agglomerate for a blast furnace and a method for operating a blast furnace using the same. [Background technology]
[0002] In the steel industry, the blast furnace process is the mainstream of pig iron manufacturing processes. In the blast furnace process, iron-based raw materials for the blast furnace (mainly sintered ore) and coke are charged into the blast furnace alternately and in layers from the top of the blast furnace, while hot air is blown into the blast furnace from the tuyere at the bottom of the blast furnace. The hot air reacts with the pulverized coal blown in together with the hot air and the coke in the blast furnace to generate high-temperature reducing gas (mainly CO gas in this case). In other words, the hot air gasifies the coke and pulverized coal. The reducing gas rises in the blast furnace and reduces the iron-based raw materials while heating them. The iron-based raw materials descend in the blast furnace while being heated and reduced by the reducing gas. The iron-based raw materials are then melted and dripped into the blast furnace while being further reduced by the coke. The iron-based raw materials are finally stored in the hearth as molten pig iron (pig iron) containing just under 5% by mass of carbon. The molten iron in the hearth is taken out through a tap hole and is used in the next steelmaking process. Therefore, in the blast furnace process, carbonaceous materials such as coke and pulverized coal are used as reducing agents.
[0003] Recently, there has been a call for the prevention of global warming, and the reduction of carbon dioxide (CO2 gas), a greenhouse gas, has become a social issue. As mentioned above, the blast furnace process uses carbonaceous material as a reducing agent, which generates a large amount of CO2 gas. Therefore, the steel industry is one of the major industries in terms of CO2 gas emissions, and must respond to this social demand. Specifically, there is an urgent need to further reduce the reducing agent ratio (the amount of reducing agent used per ton of molten iron, also known as RAR) in blast furnace operation.
[0004] One of the techniques for reducing the reducing agent ratio is to use carbon-containing agglomerates as a partial replacement for sintered ore. Carbon-containing agglomerates are made by blending iron oxide raw materials such as iron ore with carbonaceous material and agglomerating them. In carbon-containing agglomerates, the iron oxide raw materials and the carbonaceous material are close to each other, so the carbon (C component) in the carbonaceous material is easily gasified due to the coupling effect. Therefore, it is expected that the reducing agent ratio can be reduced by using carbon-containing agglomerates as an iron-based raw material for blast furnaces.
[0005] On the other hand, it is well known that metallic iron has a catalytic effect in promoting the gasification of carbon (promoting carbon reactivity). Ferro-coke, which utilizes the catalytic effect of metallic iron, is also being widely studied. Ferro-coke is produced, for example, by mixing low-grade coal and iron ore, molding the mixture, and then heating it in an air-tight environment.
[0006] Patent Document 1 and Non-Patent Documents 1 and 2 disclose a technique that combines the techniques of carbon-containing agglomerates and ferro-coke, that is, a technique in which metallic iron (M.Fe) is further mixed with carbon-containing agglomerates. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2012-92389 A [Non-patent literature]
[0008] [Non-Patent Document 1] Iguchi et al.: Iron and Steel, Vol. 88 (2002), No. 9, pp. 479-486 [Non-Patent Document 2] Nishimura et al.: CAMP-ISIJ, Vol. 18 (2005), p. 929 Summary of the Invention [Problem to be solved by the invention]
[0009] However, in carbon-containing agglomerates containing metallic iron, suitable combination conditions of metallic iron and carbon have not been known at all so far, and it is difficult to say that the advantages of the carbon-containing agglomerates and ferro-coke described above are being fully utilized.
[0010] The present invention has been made in view of the above problems, and an object of the present invention is to provide a carbon-containing agglomerated ore for blast furnaces that can further reduce the reducing agent rate, and a method for operating a blast furnace using the same. [Means for solving the problem]
[0011] In order to solve the above problems, according to one aspect of the present invention, there is provided a carbon agglomerate for blast furnaces containing 70 mass% or more of carbon, metallic iron, and iron oxide in total, characterized in that the carbon content is 15 to 25 mass% with respect to the total mass of the carbon agglomerate for blast furnaces, and the mass ratio of metallic iron to carbon is 0.4 to 0.8.
[0012] According to another aspect of the present invention, there is provided a method for operating a blast furnace using the above-mentioned carbon-containing agglomerated ore for blast furnaces, characterized in that the carbon consumption rate derived from the carbon-containing agglomerated ore for blast furnaces is 5 to 30 kg / t-HM. Effect of the Invention
[0013] According to the above-mentioned aspects of the present invention, it is possible to provide a carbon-containing agglomerated ore for blast furnaces that can further reduce the reducing agent rate, and a method for operating a blast furnace using the same. [Brief description of the drawings]
[0014] [Figure 1] 1 is a graph showing a comparison between the range of combinations of metallic iron and carbon according to the present embodiment and the conventional range. [Diagram 2] 1 is a graph illustrating a preferred mass ratio of metallic iron to carbon. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] A preferred embodiment of the present invention will be described in detail below with reference to the accompanying drawings. The present inventors have intensively studied the composition of carbon-containing agglomerates for blast furnaces (hereinafter, simply referred to as "carbon-containing agglomerates") containing metallic iron, and as a result, have been able to find a suitable combination condition of metallic iron and carbon. Based on such knowledge, the present inventors have been able to conceive of the carbon-containing agglomerates according to this embodiment and the operation method of a blast furnace using the same. In this embodiment, "carbon" does not mean the "carbon material" itself used in carbon-containing agglomerates, etc., but rather means the "carbon (C) component" contained in the "carbon material". "Iron oxide" includes wustite (FeO), magnetite (Fe3O4), and hematite (Fe2O3). In addition, the unit " / t-HM" according to this embodiment indicates the amount required to produce 1 ton of molten iron, so-called unit value. In this embodiment, a numerical range expressed using "~" means a range including the numerical values written before and after "~" as the lower and upper limits. Hereinafter, the carbon-containing agglomerated ore according to the present embodiment and the method for operating a blast furnace using the same will be described in detail.
[0016] <1. Composition of carbon-bearing agglomerates> The carbon-containing agglomerates according to this embodiment contain at least carbon, metallic iron, and iron oxide in a total amount of 70 mass% or more based on the total mass of the carbon-containing agglomerates. If this condition is not met, the reducing agent ratio cannot be sufficiently reduced. In other words, the carbon-containing agglomerates are mainly composed of carbon, metallic iron, and iron oxide, with the remainder being composed of slag (CaO, SiO2, Al2O3, etc.), crystal water, etc. A low content of carbon, metallic iron, and iron oxide means that the slag components increase accordingly. Therefore, the reducing agent required to dissolve the slag components in the blast furnace increases, and the reducing agent ratio increases accordingly.
[0017] Furthermore, in the carbon-containing agglomerates according to this embodiment, the carbon content is 15 to 25 mass% with respect to the total mass of the carbon-containing agglomerates for blast furnace. When the carbon content is within this range, the effect of carbon is effectively exhibited, and the reducing agent ratio is reduced. Here, examples of the effect of carbon include the gasification promotion effect of carbon due to the proximity of carbon to iron oxide (so-called coupling effect), and the gasification promotion effect of carbon due to the catalytic action of metallic iron. The preferable upper limit of the carbon content is 20 mass%. That is, the carbon content is preferably 15 to 20 mass%.
[0018] If the carbon content is less than 15% by mass, the effect of carbon cannot be fully enjoyed and the reducing agent ratio is not sufficiently reduced. In other words, reducing gas (CO) is easily generated from the carbon-containing agglomerates, which contributes to reducing the reducing agent ratio. However, if the carbon content is less than 15% by mass, the reducing gas generated from the carbon-containing agglomerates is reduced in the first place, so the reducing agent ratio is not sufficiently reduced.
[0019] On the other hand, when the carbon content exceeds 25% by mass, the iron oxide content in the carbon-containing agglomerates, i.e., the amount of oxygen to be reduced (the amount of oxygen bonded to iron oxide), becomes extremely small. Therefore, the effect of carbon cannot be fully enjoyed. In other words, reducing gas (CO) is easily generated from the carbon-containing agglomerates. However, when the carbon content exceeds 25% by mass, the amount of oxygen to be reduced in the immediate vicinity of the reducing gas decreases, so the effect of the reducing gas cannot be fully enjoyed. In other words, the effect of carbon cannot be fully enjoyed. Furthermore, when the carbon content exceeds 25% by mass, the hot strength of the carbon-containing agglomerates decreases, which may cause operation to become unstable. As a result of these, not only is the reducing agent ratio not reduced sufficiently, but it may even increase.
[0020] Furthermore, the mass ratio of metallic iron to carbon (M.Fe / TC) is 0.4 to 0.8. In this case, the effect of promoting carbon gasification due to the catalytic action of metallic iron is sufficiently obtained, and the reducing agent ratio is reduced. When the mass ratio of metallic iron to carbon is less than 0.4, the effect of promoting carbon gasification is not sufficiently obtained, and the reducing agent ratio is not sufficiently reduced, particularly when blast furnace operation is performed at 50 to 150 kg / t-HM. On the other hand, when the mass ratio of metallic iron to carbon exceeds 0.8, the amount of carbon becomes relatively low, and the effect of carbon cannot be fully enjoyed. In other words, since metallic iron is present in sufficient amount, carbon gasification is sufficiently promoted, but the reducing gas itself generated in the first place is reduced, so the reducing agent ratio is not sufficiently reduced. In other words, the effect of carbon cannot be fully enjoyed. The preferable lower limit of the mass ratio of metallic iron to carbon (M.Fe / TC) is 0.5, and the preferable upper limit is 0.7.
[0021] FIG. 1 is a graph showing a comparison between the range of combinations of metallic iron and carbon according to this embodiment and the conventional range.
[0022] The horizontal axis of Fig. 1 indicates the carbon (TC) content (mass%) contained in the carbon-containing agglomerates, and the vertical axis indicates the metallic iron (M.Fe) content (mass%) contained in the carbon-containing agglomerates. Graph L1 indicates M.Fe / TC = 0.8, and graph L2 indicates M.Fe / TC = 0.4. Graphs L3 and L4 indicate carbon contents of 15 mass% and 25 mass%, respectively. Therefore, an area A1 surrounded by graphs L1 to L4 indicates the conditions (combination conditions of metallic iron and carbon) that the carbon-containing agglomerates according to this embodiment should satisfy.
[0023] On the other hand, region B indicates the range disclosed in Non-Patent Document 2, and points C1, C2, and the graph C connecting them indicate the range disclosed in Patent Document 1. Although not shown, Non-Patent Document 1 specifies the carbon content as approximately 10 mass%. Therefore, both ranges are outside the range that the carbon-containing agglomerated ore according to the present embodiment should satisfy.
[0024] FIG. 2 is a graph for explaining a preferable mass ratio of metallic iron and carbon contained in the carbon-containing agglomerates. Specifically, FIG. 2 shows the relationship between the mass ratio of metallic iron and carbon contained in the carbon-containing agglomerates (M.Fe / TC) and the reducing agent ratio RAR (kg / t-HM) for each carbon content (mass % relative to the total mass of the carbon-containing agglomerates) contained in the carbon-containing agglomerates. The horizontal axis of FIG. 2 shows the mass ratio of metallic iron and carbon contained in the carbon-containing agglomerates (M.Fe / TC), and the vertical axis shows the reducing agent ratio RAR (kg / t-HM). The reducing agent ratio is a value measured in the examples described later. In the examples, the reducing agent ratio was measured using a BIS furnace (Naito et al.: Tetsu to Hagane, Vol. 87 (2001), No. 5, pp. 357-364) simulating a blast furnace. The detailed test conditions were the same as those in the examples described later, and the carbon consumption unit derived from the carbon-containing agglomerates was 20 kg / t-HM.
[0025] Point P10 indicates the measured values of M.Fe / TC and reducing agent ratio when the carbon content is 15% by mass, and graph L10 is a graph connecting the points P10. Point P20 indicates the measured values of M.Fe / TC and reducing agent ratio when the carbon content is 25% by mass, and graph L20 is a graph connecting the points P20. Graphs L30 and L40 indicate M.Fe / TC=0.4 and 0.8, respectively. Area A2 surrounded by graphs L10 to L40 indicates the conditions (combination conditions of metallic iron and carbon) that the carbon-containing agglomerates according to this embodiment should satisfy. Point P30 indicates base operation (operation with carbon content=0 by mass) in which carbon-containing agglomerates are not used. As is clear from FIG. 1 and FIG. 2, when the conditions of areas A1 and A2 are satisfied, the reducing agent ratio is significantly reduced compared to operation with carbon content=0 by mass. In addition, when comparing under the same carbon content condition, it is found that the reducing agent ratio is significantly reduced when the mass ratio of metallic iron to carbon (M.Fe / TC) is 0.4 to 0.8. In other words, since the object of this embodiment is to use the carbon in the carbon-containing agglomerates as efficiently as possible, it is necessary to compare the reducing agent ratio reduction effect between carbon-containing agglomerates with the same carbon content.
[0026] The carbon-containing agglomerates may satisfy the above conditions, but may further have a C / O of about 1.0 to 2.0. In this case, the reducing agent ratio may be further reduced. In addition, C in C / O indicates carbon in the carbon-containing agglomerates, and O indicates oxygen to be reduced in the carbon-containing agglomerates. C / O indicates the molar ratio of these. In addition, the particle size of the carbon-containing agglomerates is not particularly limited, and may be the same as that of conventional carbon-containing agglomerates. For example, the particle size of the carbon-containing agglomerates may be about 5 to 15 mm. In addition, the particle size of the carbon-containing agglomerates can be classified using sieves with different mesh sizes. The particle size of the carbon-containing agglomerates that fall through a sieve with a 15 mm mesh and remain on a sieve with a 5 mm mesh is within the range of 5 to 15 mm.
[0027] <2. Manufacturing method of carbon-containing agglomerates> Next, a method for producing the carbon-containing agglomerates according to the present embodiment will be described. The production method itself is not particularly limited, and it is sufficient to blend and mold the raw materials so that the carbon-containing agglomerates satisfy the above-mentioned conditions.
[0028] Examples of raw materials for producing carbon-containing agglomerates include iron oxide raw materials, carbonaceous materials, binders, etc. The type of iron oxide raw material is not limited, and iron oxide raw materials used in conventional carbon-containing agglomerates can be used without any particular restrictions. Examples of iron oxide raw materials include converter dust, blast furnace primary ash, sintered dust, etc., with compositions shown in Table 1. Each value in Table 1 is the mass% of each component with respect to the total mass of the iron oxide raw materials. In addition, "T.Fe" in Table 1 means total iron including metallic iron and iron oxide, and "TC" means carbon contained in the iron oxide raw materials. A mixture of multiple types of iron oxide raw materials may be used, or any one of the iron oxide raw materials may be used alone. However, in this embodiment, since it is necessary to blend metallic iron in the carbon-containing agglomerates, it is necessary to use an iron oxide raw material containing at least metallic iron. In this regard, the blast furnace primary ash shown in Table 1 contains 50 mass% or more of metallic iron, and is therefore suitable as an iron oxide raw material for producing carbon-containing agglomerates according to this embodiment. In other words, by using an iron oxide raw material containing 50% or more by mass of metallic iron, it becomes easy to adjust the mass ratio of metallic iron to carbon (M.Fe / TC). Also, if there is a shortage of metallic iron, a metallic iron source such as reduced iron powder or scrap may be purchased separately and used as appropriate. However, from the viewpoint of resource conservation and recycling, it is preferable to avoid using metallic iron sources as much as possible and to use converter dust, primary blast furnace ash, sintering dust, etc.
[0029] [Table 1]
[0030] The type of carbonaceous material used as the raw material for the carbon-containing agglomerates is not particularly limited, and carbonaceous materials used in conventional carbon-containing agglomerates can be suitably used in this embodiment. For example, the carbonaceous material may be coke, coal, anthracite, coke dust (dust generated during the coke manufacturing process), coal char, etc.
[0031] The type of binder used as the raw material for the carbon-containing agglomerates is not particularly limited, and binders used in conventional carbon-containing agglomerates can be suitably used in this embodiment. For example, the binder may be a hydraulic binder, more specifically, cement (high-early-strength Portland cement, etc.).
[0032] The components of each raw material can be identified by a general chemical analysis method or a fluorescent X-ray analysis method. The raw materials are then blended and molded so that the carbon-containing agglomerates satisfy the above-mentioned conditions. For example, the blended raw materials and an appropriate amount of water are kneaded and molded in a granulator such as a pelletizer or a briquette machine, and then cured (the binder is hardened) to produce the carbon-containing agglomerates.
[0033] <3. Blast furnace operation method> Next, the operation method of the blast furnace according to the present embodiment will be described. In the present embodiment, the blast furnace is operated by replacing a part of the iron-based raw material (sintered ore, etc.) with the carbon-containing agglomerated ore according to the present embodiment. Here, it is preferable that the carbon consumption unit derived from the carbon-containing agglomerated ore is 5 to 30 kg / t-HM. In this case, the reducing agent rate is further reduced. If the carbon consumption unit derived from the carbon-containing agglomerated ore is less than 5 kg / t-HM, the reducing agent rate may not be reduced sufficiently. On the other hand, if the carbon consumption unit derived from the carbon-containing agglomerated ore exceeds 30 kg / t-HM, the effect of improving the reducing agent rate becomes saturated. The operation other than the above may be performed in the same manner as the conventional blast furnace operation method. EXAMPLES
[0034] Next, an example of this embodiment will be described. In this example, the following tests were performed to verify the effects of this embodiment. Of course, the present invention is not limited to the examples described below. It is clear that a person with ordinary knowledge in the technical field to which this invention belongs can think of various modified or revised examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
[0035] First, the iron oxide raw material, actual coke dust, reagent iron powder (purity 98%), and high-early-strength Portland cement shown in Table 1 were prepared. The components of the iron oxide raw material and the actual coke dust were identified by fluorescent X-ray analysis. The particle sizes of each raw material were 50 μm, 53 μm, 50 μm, and 13 μm in terms of d50 (volume basis). Here, the d50 of each raw material was measured by the following measurement method using a laser diffraction particle size distribution measuring device. That is, the sample to be measured was slurried with water, and a small amount of sodium hexametaphosphate solution was added as a dispersant. Next, the sample was dispersed in the mixed liquid by stirring and irradiating the mixed liquid with ultrasonic waves. Next, this mixed liquid was set in a laser diffraction particle size distribution measuring device, the particle size distribution was measured, and the d50 was identified.
[0036] Next, these raw materials were mixed with an appropriate amount of water and molded in a briquette machine. The molded granules were then cured. The above process was repeated while changing the type of iron oxide raw material and the mixing ratio of each raw material to produce carbon-containing agglomerates (Test Examples No. 1 to 22) with the compositions shown in Table 2. Of the produced carbon-containing agglomerates, those with particle sizes of 8 to 13 mm (those that fell through a sieve with 13 mm openings and remained on a sieve with 8 mm openings) were used in the following BIS furnace test.
[0037] [Table 2]
[0038] Each component in Table 2 indicates the mass %, molar ratio, and unit of each component in the carbon-bearing agglomerates. For example, "T.Fe" indicates the mass % of the total iron in the carbon-bearing agglomerates, "M.Fe" indicates the mass % of metallic iron in the carbon-bearing agglomerates, and "TC" indicates the carbon content (mass %) in the carbon-bearing agglomerates. "FeO" and "Fe2O3" indicate the content (mass %) of "iron oxide" in the carbon-bearing agglomerates. "Reduced oxygen content" indicates the mass % of oxygen bonded to "iron oxide." "C+M.Fe+FeO+Fe2O3" indicates the total mass % of carbon, metallic iron, and iron oxide in the carbon-bearing agglomerates. The mass % of each component is the mass % with respect to the total mass of the carbon-bearing agglomerates sample. "M.Fe / TC" indicates the mass ratio of metallic iron to carbon in the carbon-bearing agglomerates, and C / O indicates the molar ratio of carbon to reduced oxygen in the carbon-bearing agglomerates.
[0039] Next, a BIS furnace test was carried out. Details of the BIS furnace test are as described in "Naito et al.: Iron and Steel, Vol. 87 (2001), No. 5, pp. 357-364" and this test was also carried out according to the method described in this non-patent document. Specifically, the amount of sintered ore and the amount of coke were adjusted so that the TC and T.Fe per charge (TC and T.Fe here indicate the mass% of carbon and the mass% of total iron in the charge relative to the total mass of the entire charge) were constant.
[0040] The amount of carbon agglomerates used was adjusted so that the carbon consumption rate derived from the carbon agglomerates was the value shown in Table 2. That is, when carbon agglomerates with a TC of 15.0 mass% were used, the amount of carbon agglomerates used (consumption rate) was 133 kg / t-HM, and when carbon agglomerates with a TC of 25.0 mass% were used, the amount of carbon agglomerates used (consumption rate) was 80 kg / t-HM. Furthermore, the blast temperature was 1178°C and the blast moisture content was 18.6 g / Nm3 so that the reducing agent rate was 481 kg / t-HM and the coke rate was 349 kg / t-HM. 3 , and the bosh gas composition (CO: 36.0 vol%, H2: 7.0 vol%, N2: 57.0 vol%) and the airflow (1343 Nm 3 / t-HM) was set.
[0041] Here, the oxygen enrichment rate is roughly the volume ratio of oxygen in the hot air to the total volume of the hot air, and is expressed as follows: oxygen enrichment rate (%) = {(air flow rate (flow rate) [Nm 3 / min]×0.21+oxygen enrichment amount [Nm 3 / min]) / (Air flow rate [Nm 3 / min] + oxygen enrichment amount [Nm 3 / min])}×100-21. The ore / coke (mass ratio of sintered ore to coke) was set to 4.63.
[0042] In addition, in consideration of the alkali circulation in the blast furnace, the reagent KOH was added so that the K content was 1.8 mass% relative to the coke. Based on the shaft efficiency obtained in the BIS furnace, the heat and mass balance was taken to evaluate the reducing agent ratio. In this case, the reducing agent ratio was evaluated as the unit of the amount of pulverized coal + coke + carbonaceous material in the carbon-containing agglomerates (here, actual coke dust) blown in with the hot air corrected to the amount of coke. In addition, the effect of reducing the oxygen to be reduced by M.Fe in the carbon-containing agglomerates was indirectly evaluated by correcting the experimental data for hematite without changing the amount of reducing gas. In other words, since no oxygen to be reduced is bonded to M.Fe, if an operation is performed to reduce the amount of reducing gas by the amount of M.Fe, the more M.Fe in the charging charge, the more reduced iron will be produced with less reducing agent. However, the effect to be obtained by this embodiment is not the reduction in the reducing agent ratio due to the absence of oxygen to be bonded to M.Fe, but the reduction in the reducing agent ratio due to the catalytic action of M.Fe. Therefore, in this embodiment, the BIS test was performed without reducing the amount of reducing gas, and the obtained results were corrected to a state in which all M.Fe was hematite, and the reducing agent ratio was evaluated. For comparison, a base operation (operation corresponding to point P30 in Figure 2) in which no carbon-containing agglomerates were used was also performed.
[0043] The results are shown in Table 2 and Figure 2. As described above, Figure 2 summarizes the data when the carbon consumption rate derived from the carbon-containing agglomerates is 20 kg / t-HM. Test Examples No. 1 to 6 in Table 2 are examples in which the carbon content (TC) contained in the carbon-containing agglomerates is 15 mass%, and Test Examples No. 7 to 12 are examples in which the carbon content (TC) contained in the carbon-containing agglomerates is 25 mass%. In Test Examples No. 1 to 12, the carbon consumption rate derived from the carbon-containing agglomerates is unified to 20 kg / t-HM. Test Examples No. 13 to 22 are examples in which the carbon content contained in the carbon-containing agglomerates is 15 mass% or 25 mass%, while the carbon consumption rate derived from the carbon-containing agglomerates or the total mass% of carbon, metallic iron, and iron oxide in the carbon-containing agglomerates is changed.
[0044] First, in the examination of the test samples No. 1 to No. 6, the carbon-containing agglomerates satisfied the requirements of the present embodiment, and further, in the test samples No. 3 to No. 5 in which the carbon consumption rate derived from the carbon-containing agglomerates was set to 20 kg / t-HM within the range of 5 to 30 kg / t-HM, an extremely good reducing agent rate was obtained. Specifically, the reducing agent rate was 490 kg / t-HM or less.
[0045] On the other hand, in test samples Nos. 1, 2, and 6, which did not satisfy other requirements for the carbon-containing agglomerates, the reducing agent ratio was increased compared to test samples 3 to 5, which had the same carbon content in the carbon-containing agglomerates. Specifically, in test samples Nos. 1 and 2, the mass ratio of metallic iron to carbon (M.Fe / TC) was less than 0.4, while in test sample No. 6, the mass ratio of metallic iron to carbon (M.Fe / TC) exceeded 0.8.
[0046] Next, when considering Test Examples No. 7 to 12, the carbon-containing agglomerates satisfied the requirements of this embodiment, and Test Examples No. 9 to 11, in which the carbon consumption rate derived from the carbon-containing agglomerates was set to 20 kg / t-HM within the range of 5 to 30 kg / t-HM, had an extremely good reducing agent rate. Specifically, the reducing agent rate was 480 kg / t-HM or less.
[0047] On the other hand, in test samples Nos. 7, 8, and 12, which did not satisfy other requirements for the carbon-containing agglomerates, the reducing agent ratio was increased compared to test samples 7 to 12, which had the same carbon content in the carbon-containing agglomerates. Specifically, in test samples Nos. 7 and 8, the mass ratio of metallic iron to carbon (M.Fe / TC) was less than 0.4, while in test sample No. 12, the mass ratio of metallic iron to carbon (M.Fe / TC) exceeded 0.8.
[0048] Next, test examples Nos. 13 to 16 will be considered. Test examples Nos. 13 to 16 are obtained by varying the carbon consumption unit derived from the carbon-containing agglomerates in test example No. 4. Specifically, in test example No. 13, the carbon consumption unit derived from the carbon-containing agglomerates is less than 5 kg / t-HM. Compared with test examples Nos. 1, 2, and 6, which have the same carbon content in the carbon-containing agglomerates, test example No. 13 also had a reducing agent rate reduction effect, but compared with test examples Nos. 3 to 5, the reducing agent rate was slightly increased.
[0049] In Test Examples 14 and 15, the carbon consumption rate derived from the carbon-containing agglomerates was changed to 5 kg / t-HM or 30 kg / t-HM, which are the boundary values of this embodiment, in Test Example 4. In Test Examples 14 and 15, the results were similar to those of Test Examples 3 to 5, which had the same carbon content in the carbon-containing agglomerates.
[0050] In test example No. 16, the carbon consumption rate derived from the carbon-containing agglomerates exceeded 30 kg / t-HM. Compared with test examples No. 1, 2, and 6, which had the same carbon content in the carbon-containing agglomerates, test example No. 16 also had a reducing effect on the reducing agent rate, but the reducing agent rate was slightly higher than that of test examples No. 3 to 5. In this case, the reducing agent rate reduction effect was saturated at 485 kg / t-HM. However, the amount of hot disintegration of the carbon-containing agglomerates increased, and the airflow resistance of the shaft increased, so the coke rate was increased to keep the airflow resistance constant, and as a result, the final RAR was 495 kg / t-HM.
[0051] Next, test samples Nos. 17 to 20 will be considered. Test samples Nos. 17 to 20 are obtained by varying the carbon consumption rate derived from the carbon-containing agglomerates in test sample No. 10. Specifically, in test sample No. 17, the carbon consumption rate derived from the carbon-containing agglomerates is less than 5 kg / t-HM. Compared with test samples Nos. 7, 8, and 12, which have the same carbon content in the carbon-containing agglomerates, test sample No. 17 also had a reducing effect on the reducing agent rate, but the reducing agent rate was slightly increased compared to test samples Nos. 9 to 11.
[0052] Test Examples No. 18 and 19 were obtained by changing the carbon consumption rate derived from the carbon-containing agglomerates in Test Example No. 10 to the boundary values of this embodiment, 5 kg / t-HM or 30 kg / t-HM. Test Examples No. 18 and 19 obtained results similar to those of Test Examples No. 9 to 11, which had the same carbon content in the carbon-containing agglomerates.
[0053] In test example No. 20, the carbon consumption rate derived from the carbon-containing agglomerates exceeded 30 kg / t-HM. Compared with test examples No. 7, 8, and 12, which had the same carbon content in the carbon-containing agglomerates, test example No. 20 also had a reducing effect on the reducing agent rate, but the reducing agent rate was slightly higher than that of test examples No. 9 to 11. In this case, the reducing agent rate reduction effect was saturated at 475 kg / t-HM. However, the amount of hot disintegration of the carbon-containing agglomerates increased, and the ventilation resistance of the shaft increased, so the coke rate was increased to keep the ventilation resistance constant, and as a result, the final RAR was 482 kg / t-HM.
[0054] In Test Examples 21 and 22, the total amount of carbon, metallic iron, and iron oxide was less than 70 mass %, and therefore the reducing agent ratio was not sufficiently reduced.
[0055] In Test Example 23, the carbon content of the carbon-containing agglomerates was changed in Test Example No. 4. Specifically, the carbon content of the carbon-containing agglomerates was less than 15%. Since the C / O ratio was not high enough, the reducing agent ratio was increased compared to Test Example No. 4.
[0056] In Test Example 24, the carbon content of the carbon-containing agglomerates was changed from Test Example No. 10. Specifically, the carbon content of the carbon-containing agglomerates was more than 25%. The C / O ratio was excessively high, and the effect was not efficiently achieved. In addition, the in-furnace powdering of the carbon-containing agglomerates was significant, making the blast furnace operation unstable. Therefore, the reducing agent rate was increased compared to Test Example No. 10.
[0057] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
Claims
1. A carbon-containing agglomerate for blast furnaces containing 70 mass% or more of carbon, metallic iron, and iron oxide in total, The carbon content is 15 to 25 mass% based on the total mass of the carbon-containing agglomerate for blast furnace, A carbon-containing agglomerate for blast furnaces, characterized in that a mass ratio of the metallic iron to the carbon is 0.4 to 0.
8.
2. A method for operating a blast furnace using the carbon-containing agglomerate ore according to claim 1, The method for operating a blast furnace is characterized in that the carbon consumption rate derived from the carbon-containing agglomerated ore for blast furnace is 5 to 30 kg / t-HM.
Citation Information
Patent Citations
Cold bonded iron-carbon pellets, and manufacturing method and applications thereof as ironmaking burden in shaft furnace or blast furnace
CN101768663A
JP1972007697U
Method for producing carbon-containing non-calcined pellet for blast furnace
JP2008095177A
Method of operating blast furnace while using ferro-coke
JP2010095759A
Agglomerated ore including carbonaceous material for iron-making, and producing method therefor
JP2011225926A