Manufacturing method of conductive part, manufacturing method of electronic component including conductive part, manufacturing method of product assembled with electronic components including conductive part, conductive part, electronic component having conductive part, product incorporating electronic component including conductive part
By laminating and melting conductors with a melting laser to create a central hole in the insulating layer, the method addresses the challenge of forming conductive parts with insulating layers, achieving stable conductivity and reliable electrical connections.
Patent Information
- Application Number
- JP2020199675
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-01
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2040-12-01
AI Technical Summary
Existing methods struggle to form reliable conductive parts between conductors with insulating layers due to the difficulty in removing natural oxide layers and insulating coatings, which hinder conductivity, especially as conductors become thinner and more susceptible to oxidation.
A method involving laminating a second conductor on a first conductor with an insulating layer, followed by a melting process using a melting laser to create a molten region with a central hole, effectively removing the insulating layer and ensuring conductivity by forming a conductive part.
This approach enables easy formation of conductive parts with stable conductivity by efficiently removing insulating layers, even on thin conductors, reducing electrical resistance and ensuring reliable electrical connections.
Smart Images

Figure 0007575775000001 
Figure 0007575775000002 
Figure 0007575775000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a conductive structure using a fired metal ink, and the conductive structure. [Background technology]
[0002] Electronic components are made on a substrate with conductors as conductor wires. There are many different conductor materials, but titanium, aluminum, and their alloys, which form a nanometer-order natural oxide layer on the surface of the conductor, are sometimes used as conductor materials. These metals oxidize very easily in the atmosphere, forming a natural oxide layer. The natural oxide layer is an insulator, and all parts that come into contact with the atmosphere are covered with the natural oxide layer. In addition, as in Patent Document 2, an insulating layer such as SiO, SiN, or SiON may be formed by plasma CVD on a wiring layer such as aluminum instead of the natural oxide layer. Even if an attempt is made to pass electricity between wiring or electrodes that have a natural oxide layer or insulating layer on their surface by overlapping another wiring, the natural oxide layer or insulating layer will prevent electricity from passing between them simply by overlapping them (it will not become a conductive part). Therefore, as shown in Patent Document 1, a method is also used in which the native oxide layer is physically destroyed by scratching it with a polishing needle and then another conductor is layered on top of it to create a conductive portion. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2000-22306 A [Patent Document 2] Patent No. 6711614 Summary of the Invention [Problem to be solved by the invention]
[0004] However, physical operations such as scratching with a polishing needle become more difficult as the conductor becomes thinner, and workability deteriorates. Moreover, even if the natural oxide layer is destroyed and the metal is exposed, titanium and aluminum are easily oxidized in the atmosphere, and the natural oxide layer forms again in an extremely short time. For this reason, it has been difficult to form a conductive part with reliable conductivity. The same applies to the insulating layer that covers the surface of the metal wiring, and when overlapping another wiring, it is necessary to remove the insulating layer beforehand.
[0005] An object (object) of the present invention is to provide a manufacturing method for easily forming a conductive portion between a conductor having an insulating layer on its surface and another conductor, and to provide a new conductive portion. [Means for solving the problem]
[0006] The present invention solves this problem by providing a method for manufacturing a conductive part, which includes a first step of stacking a second conductor on a first conductor having an insulating layer on its surface, and a second step of melting the first conductor and the second conductor, including the insulating layer, to create a molten region, and forming a hole in the center of the molten region that is surrounded by the molten region.
[0007] In addition, another aspect of the present invention solves the problem by providing a conductive part comprising a first conductor, a second conductor, and a molten region, wherein the first conductor has an insulating layer on its surface and the second conductor is laminated on the first conductor, the molten region is a region in which the first conductor and the second conductor, including the insulating layer, are melted, and the molten region has a hole in the center of the molten region that is surrounded by the molten region. Effect of the Invention
[0008] It was possible to easily create a conductive portion between a conductor having an insulating layer on its surface and another conductor layered on top of it. [Brief description of the drawings]
[0009] [Figure 1]An explanatory diagram of the metal ink baking process. (A) A conceptual diagram of the baking process of a baked metal ink conductor by scanning with a baking laser. (B) An enlarged view of the metal ink. (C) An enlarged view of the baked metal ink. [Diagram 2] An explanatory diagram of the melting process. (A) A cross-sectional view of a fired metal ink conductor after firing the metal ink. (B) A cross-sectional view of a melted area created with a melting laser. (C) A cross-sectional view of the melting laser when the pulse energy is changed and the depth of its influence is changed by applying it to three locations. [Diagram 3] When a non-hole-forming welding laser is used, the range of heat influence as the irradiation process progresses. (A) Diagram of the state where the molten area does not reach the native oxide layer. (B) Diagram of the state where the molten area has exceeded the native oxide layer. (C) Diagram of the state where the molten area has exceeded the native oxide layer. [Figure 4] Conductivity test results. [Diagram 5] Photograph of the conductive part. (A) Scanning electron microscope photograph of the cross section of the conductive part. (B) An explanatory diagram of the scanning electron microscope photograph of Figure 5(A). [Figure 6] 6(A) is a plan view of a TFT liquid crystal panel according to a second embodiment of the present invention; [Figure 7] FIG. 11 is a cross-sectional view of a conductive part according to a third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the same reference numerals in different drawings indicate parts with the same functions, and duplicated descriptions in each drawing will be omitted as appropriate. In addition, some of the drawings are intentionally deformed for the purpose of explanation, and are not drawn to exact scale.
[0011] [Distinguishing between before and after baking of metal ink] Hereinafter, the metal ink before baking will be simply referred to as "metal ink", and the metal ink after baking will be referred to as "baked metal ink" to distinguish them.
[0012] [conductor] The term "conductor" includes wiring and electrodes.
[0013] [Meaning of parentheses around terms] In addition, it may be written as "baked metal ink conductor (second conductor)", but the (second conductor) in parentheses indicates the term used in the corresponding claim.
[0014] [Meaning of insulating layer] The insulating layer includes a natural oxide layer (insulating layer) formed by natural oxidation on the surface of a metal conductor (first conductor) whose main material is aluminum or the like. The insulating layer includes not only natural oxidation but also those formed by artificial processes. For example, the present invention also includes a metal conductor (first conductor) coated with an insulating layer made of another material. In the present invention, the insulating layer also includes a layer having a higher electrical resistance than the metal conductor (first conductor), such as a layer having a stain on the surface of the metal conductor (first conductor).
[0015] [Electronic components] In the present invention, any element that is connected to another element by a conductor is included in the "electronic component" of the present invention. For example, the "electronic component" of the present invention also includes a circuit board such as a printed circuit board.
[0016] Example 1 Example 1 shown in Figs. 1 to 5 is an example in which a conductive part 9 is formed between a first conductor A having a natural oxide layer (insulating layer B) 721 on its surface, which is a metal conductor 72, and a second conductor C, which is a fired metal ink conductor 27. There is no limitation on the material of either the first conductor A or the second conductor C, but in Example 1, a metal ink 2 is used for the second conductor C. This is to explain how the metal ink 2 is used to repair a broken wire or the like. For example, the wiring of a circuit board of a flat panel display may be broken due to dirt or dust that adheres to the board during the manufacturing process. In such a case, the broken wire can be repaired by creating a detour path of the metal ink 2 as the second conductor C between the first conductor A before and after the break. Example 1 shows only one example, and the present invention does not exclude the use of a second conductor C made of a material different from the metal ink.
[0017] [Insulation layer] The metal conductor (first conductor A) 72 is mainly composed of a metal such as aluminum or titanium that naturally oxidizes in the atmosphere and forms a natural oxide layer (insulating layer B) 721 on the surface.
[0018] [Metal ink application process] FIG. 1 is an explanatory diagram of the baking process of metal ink 2. FIG. 1(A) is a conceptual diagram of the baking process of a baked metal ink conductor (second conductor C) 27 by scanning with a baking laser 3. A metal conductor (first conductor A) 72 is disposed on a substrate 7. The metal conductor (first conductor A) 72 is a conductor whose main component is aluminum, and a natural oxide layer (insulating layer B) 721 on the order of several nanometers is formed on its surface. Next, metal ink 2 is applied on top of the natural oxide layer (insulating layer B) 721 of the metal conductor (first conductor A).
[0019] [Metal ink baking process] Figure 1(B) is an enlarged view of metal ink 2. Metal ink 2 is made by forming highly conductive metals such as gold, silver, and copper into nanoparticles and dispersing them in an organic solvent 26. The melting point of metals is dramatically lowered by forming them into nanoparticles. Organic matter 25 is adsorbed onto the surfaces of metal nanoparticles 24, and this organic matter 25 allows the metal nanoparticles 24 to be dispersed in the organic solvent 26 without agglomerating together.
[0020] When the metal ink 2 is heated by irradiation with a baking laser 3 or infrared rays, the organic solvent 26 evaporates, the organic matter 25 on the surface of the metal nanoparticles 24 is desorbed, and the metal nanoparticles 24 aggregate and melt to become metal lumps that become conductive. Any suitable heating means can be used for baking. In Example 1, a firing laser 3 was used for firing. The absorption wavelength of the metal ink 2 varies depending on the type and particle size of the metal, but is around 400 nm for the metal ink 2 containing silver-based metal nanoparticles 24 with a particle size of 20 nm used in Example 1. The firing laser 3 used in Example 1 was a continuous oscillation semiconductor laser having a wavelength around the absorption wavelength.
[0021] 1(C) is an enlarged view of the fired metal ink conductor (second conductor C) 27, from which it can be seen that the metal nanoparticles 24 are fused together to form metal lumps. Only the area irradiated with the firing laser 3 is fired to become the fired metal ink conductor (second conductor C) 27, which becomes a conductive fired metal ink conductor (second conductor C) 27. As shown in FIG. 1(A), the firing laser 3 is scanned left and right along the metal ink 2 as indicated by the arrow, firing the metal ink 2 and laminating a fired metal ink conductor (second conductor C) 27 on the underlying metal conductor (first conductor A) 72.
[0022] The [metal ink application process] and [metal ink baking process] together constitute (first process) a process of laminating a baked metal ink conductor (second conductor C) 27 onto a metal conductor (first conductor A) 721 having a natural oxidation layer (insulating layer B) 721 on its surface.
[0023] Structurally, the laminated structure comprises a metal conductor (first conductor A) 72 and a fired metal ink conductor (second conductor C) 27, the metal conductor (first conductor A) 72 having a natural oxidation layer (insulating layer B) 721 on its surface, and the fired metal ink conductor (second conductor C) 27 being laminated on the natural oxidation layer (insulating layer B) 721 of the metal conductor (first conductor A) 72.
[0024] [Melting process] 2 is an explanatory diagram of the melting step. Fig. 2(A) is a cross-sectional view of a fired metal ink conductor 27 obtained by firing the metal ink 2. Fig. 2(A) shows the state after firing in the above-mentioned [metal ink firing step]. At this point, the natural oxide layer (insulating layer B) 721 is sandwiched between the metal conductor (first conductor A) 72 and the baked metal ink conductor (second conductor C) 27, so it does not have sufficient conductivity to function as a conductive part 9.
[0025] 2(B) is a cross-sectional view of the state where a melted region 8 has been created by the melting laser 4. The output of the melting laser 4 can vary depending on the thickness of the metal conductor (first conductor A) 72 and the fired metal ink conductor (second conductor C) 27, the type of metal, and other factors. It is undesirable for the influence of the melting laser 4 to extend to the substrate 7, and it is preferable that the output has an effect at least on the natural oxide layer (insulating layer B) 721. More preferably, the output has an effect beyond the natural oxide layer (insulating layer B) 721 and extends to the metal conductor (first conductor A) 72.
[0026] The melting laser 4 destroys the natural oxidation layer (insulating layer B) 721, creating a molten region 8 that is a mixture of silver from the fired metal ink conductor (second conductor C) 27, aluminum from the metal conductor (first conductor A) 72, and aluminum oxide from the natural oxidation layer (insulating layer B) 721.
[0027] In the center where the melting laser 4 hits, a hole 74 is formed as a trace of evaporated metal, as shown in the figure. A melted region 8, indicated by hatching, is formed on the inner wall of the hole 74. The melted region 8 contains a large amount of highly conductive aluminum and silver, and is merely mixed with a natural oxide layer (insulating layer B) 721 of at most several nanometers, so it is a region with significantly high conductivity. As a result, the irradiation of the melting laser 4 (second process) melts the metal conductor (first conductor A) 72 and the fired metal ink conductor (second conductor C) 27, including the natural oxide layer (insulating layer B) 721, to create a melted region, and a process of forming a hole 74 surrounded by the melted region 8 in the center of the melted region 8 is performed.
[0028] As described above, a molten region 8 is formed in which the natural oxide layer (insulating layer B) 721, the baked metal ink conductor (second conductor C) 27, and the metal conductor (first conductor A) 72 are melted, and a hole 74 is formed in the center of the molten region 8 and is surrounded by the molten region 8.
[0029] [Another aspect of the melting process] Figure 2(C) is a cross-sectional view of the case where the melting laser 4 is applied to three locations with different pulse energies, changing the depth of the influence of the melting laser 4. (Note that Figure 2 is a conceptual diagram, and low, medium, and high powers are a comparison of the pulse energies in this diagram.)
[0030] In Fig. 2(C)(a), a melting laser 4 with low output pulse energy is irradiated. The melted region 8 remains within the range of the fired metal ink conductor (second conductor C) 27, and an improvement in the electrical conductivity between the metal conductor (first conductor A) 72 and the fired metal ink conductor (second conductor C) 27 cannot be expected.
[0031] 2(C)(b), a melting laser 4 with a medium output pulse energy is irradiated. The effect of the melting laser 4 reaches the vicinity of the natural oxide layer (insulating layer B) 721, and although the conductivity between the metal conductor (first conductor A) 72 and the baked metal ink conductor (second conductor C) 27 can be expected to improve, the thickness of the baked metal ink conductor (second conductor C) 27 is not uniform, so the conductivity may not improve as much as expected.
[0032] 2(C)(c), a melting laser 4 with high output pulse energy is irradiated. The melted region 8 is formed beyond the native oxide layer (insulating layer B) 721 of the metal conductor (first conductor A) 72, and the conductivity between the metal conductor (first conductor A) 72 and the fired metal ink conductor (second conductor C) 27 is reliably improved.
[0033] The metal ink 2 is applied to each location where the conductive portion 9 is to be formed, and the application conditions for each location are not exactly the same, so the conditions (thickness, etc.) of the fired metal ink conductor (second conductor C) 27 are not constant. Therefore, by irradiating the melting laser 4 to two or more locations, preferably three locations, with different pulse energies, it is possible to reliably ensure conductivity without having to conduct experiments to determine the output suitable for the conditions for each location where the conductive portion is to be formed. The pulse width and number of irradiations may also be changed.
[0034] 2(c), the melting laser 4 is applied to three locations with different pulse energies, but two or more locations may be used. To create melted regions 8 with different depths in two or more locations, a third process may be added following the second process to create another melted region with a different depth in a position different from the melted region formed in the second process.
[0035] Furthermore, two or more molten regions are provided, and the molten regions have different depths, so that electrical conductivity can be reliably ensured.
[0036] In the embodiment, a melting laser 4 is used that is set to form a hole 74 by pulse energy. The hole 74 is formed in the center of the melting region 8, surrounded by the melting region 8, so that the depth of the melting region 8 can be known. Furthermore, the formation of the hole 74 allows heat to be released through the hole 74, and the melting region 8 can be cooled quickly. In general, thermal energy affects members near the melting region 8, and in particular, when a laser is irradiated on a substrate 7 in which an organic layer or the like is close to the melting region 8, the organic layer may be altered. However, the melting laser 4 of the present invention that is set to form a hole 74 by irradiating a nanosecond pulse laser at high power as in the present invention forms a minute hole 74 that penetrates the natural oxide layer (insulating layer B) 721. The heat of the melting region 8 is also released from the hole 74, accelerating the cooling speed, and the effect of the heat can be limited to only a very small area around the melting region 8.
[0037] On the other hand, when a welding laser 41 that does not form holes 74 is used, the melted region 8 becomes larger and the range affected by heat also becomes larger.
[0038] Fig. 3, which corresponds to a comparative experiment, is an explanatory diagram of the range of the thermal influence as the irradiation process progresses when laser irradiation is performed using a welding laser 41 that does not form a hole 74. Fig. 3(A) is a diagram of the state immediately after irradiation, Fig. 3(B) is a diagram of the state where the molten region 8 has not reached the natural oxide layer (insulating layer B) 721, and Fig. 3(C) is a diagram of the state where the molten region 8 has exceeded the natural oxide layer (insulating layer B) 721.
[0039] As shown in FIG. 3(A), the melted area 8 immediately after irradiation is small, but heat is diffused by thermal conduction from the irradiation area of the welding laser 41 where no hole 74 is formed. If irradiation is continued, the melted area 8 gradually expands as shown in FIG. 3(B). If irradiation is continued further, the heat conduction continues, and the melted area 8 gradually expands, and a melted area 8 larger than the irradiation area of the welding laser 41 where no hole 74 is formed is formed as shown in FIG. 3(C), melting the natural oxide layer (insulating layer B) 721. The temperature of the melted area 8 reaches the melting point of the metal and is very high, and the area around the melted area 8 becomes an area 412 affected by heat due to thermal conduction. At this time, heat is dissipated only from the surface of the baked metal ink conductor (second conductor C) 27, and the larger the volume of the melted area 8 becomes, the less the heat dissipation proportional to the surface area can keep up. The area 412 affected by heat expands greatly due to the high-temperature metal accumulated in the melted area 8 whose volume has increased.
[0040] In the first embodiment, as shown in FIG. 2, a hole 74 is provided in the center of the molten region 8, so that the metal in the molten region 8 cools quickly. In this way, when the melting laser 4 that forms the hole 74 is used, the area 412 affected by heat can be made significantly smaller than when the welding laser 41 that does not form the hole 74 is used.
[0041] Experimental examples of the present invention will now be described. (Experiment 1: Experiment showing the relationship between electrical resistance and pulse energy) Experiment 1 is an experiment to investigate how the electrical resistance changes before and after the destruction of the natural oxide layer (insulating layer B) 721 by changing the depth of the melted region 8. In experiment 1, a sample for irradiation with the welding laser 4 was prepared by applying metal ink 2 onto a metal conductor 72 on a substrate 7 and baking it to form a baked metal ink conductor 27. The melting laser 4 was then irradiated onto the sample under different conditions. To change the depth of the melted region 8 formed by the melting laser 4, the pulse energy of the melting laser 4 was changed among four conditions: 100, 200, 250, and 300 μJ. Moreover, the conditions other than the pulse energy were the same.
[0042] The conditions of Experiment 1 are described below. (1) Melting Laser 4 Wavelength 532nm Pulse width: 10ns Pulse count: 1 Melting process setting size 1μm×1μm Experiments were conducted with pulse energies of 100, 200, 250, and 300 μJ (see Figure 4). (2) Metal conductor (first conductor A) 72 Metal Type: Aluminum Wiring width 5μm (3) Baked metal ink conductor (second conductor C) 27 Metal type: Silver (nanoparticles) Wiring thickness: 0.4μm Under the above experimental conditions, samples were created by changing the pulse energy of the melting laser 4, and the electrical resistance between the metal conductor (first conductor A) 72 and the fired metal ink conductor (second conductor C) 27 was measured. The results are shown in FIG.
[0043] At a pulse energy of 100 μJ, the electrical resistance was 340 Ω on average, and there was no improvement in the electrical conductivity compared to before irradiation with the melting laser 4. It is presumed that the influence of the melting laser 4 was limited to the range of the baked metal ink conductor (second conductor C) 27, as shown in FIG. 2(C)(a).
[0044] At a pulse energy of 200 μJ, the electrical resistance was 50 Ω on average, and a significant improvement in electrical conductivity was observed. It is presumed that the influence of the melting laser 4 remains near the native oxide layer (insulating layer B) 721, as shown in FIG. 2(C)(b).
[0045] At pulse energies of 250 μJ and 300 μJ, the average electrical resistance drops sharply to nearly 0 Ω. It is assumed that the natural oxide layer (insulating layer B) 721 is melted, and the influence of the melting laser 4 is assumed to extend to the metal conductor (first conductor A) 72 as shown in FIG. 2(C)(c). At a pulse energy of 200 μJ, the error bars (3σ) remained at about 30 Ω on one side and 60 Ω on both sides, and there was a large variation in the observed electrical resistance, but at pulse energies of 250 μJ and 300 μJ, the error bars (3σ) were 2 to 3 Ω.
[0046] This indicates that the influence of the melting laser 4 reaches a point where electrical conductivity can be reliably ensured. It also indicates that the electrical resistance is sufficiently small, and that the conductive portion 9 is formed stably with little variation.
[0047] (Experiment 2: Confirmation of the melted area) In order to confirm the presence of the molten region 8, experiment 2 was carried out in which the conductive portion 9 was photographed using a scanning electron microscope. 5A and 5B are scanning electron microscope photographs of the conductive portion 9, and FIG. 5(A) is a scanning electron microscope photograph of the conductive portion 9, and FIG. 5(B) is an explanatory diagram of the scanning electron microscope photograph of FIG. 5(A).
[0048] The photographed samples were prepared and photographed as follows. (1) The substrate 7 having the conductive portion 9 produced as described above was used as a sample, and was covered with a protective film 73 as a pretreatment for the subsequent electron beam cutting. (2) The substrate 7 was cut with an electron beam, and a cross section was cut out. (3) The sample prepared as described above was photographed with a scanning electron microscope from an angle that allowed the cross section to be seen.
[0049] The hatched protective film 73 in FIG. 5(B) is a coating applied during sample preparation, and is not present on the original conductive portion 9. There is a natural oxide layer (insulating layer B) 721 on the surface of the metal conductor (first conductor A) 72, but it is only a few nanometers thick and is not visible at this magnification.
[0050] A hole 74 is formed in the area irradiated with the melting laser 4. On the side of the hole 74, the boundary between the fired metal ink conductor (second conductor C) 27 and the metal conductor (first conductor A) 72, which should originally exist, is blurred or has completely disappeared. This shows that the metal conductor (first conductor A) 72 and the fired metal ink conductor (second conductor C) 27, including the natural oxide layer (insulating layer B) 721, have melted to form the molten area 8.
[0051] (Summary of Experiments 1 and 2) From the above experiments, it was confirmed that the metal conductor (first conductor A) 72 and the baked metal ink conductor (second conductor C) 27, including the natural oxide layer (insulating layer B) 721, are melted by irradiation with the melting laser 4, forming a melted region 8. It was also confirmed that the electrical resistance between the metal conductor (first conductor A) 72 and the baked metal ink conductor (second conductor C) 27 is significantly reduced by irradiation with the melting laser 4, resulting in a result with little variation in the electrical resistance value. Since the electrical resistance value has little variation, it can be said that the present invention can be put to practical use.
[0052] Example 2 Example 2 is an application example of the present invention. Figure 6 is an explanatory diagram of Example 2, in which Figure 6(A) is a plan view of a substrate 7 of a TFT liquid crystal panel, and Figure 6(B) is an enlarged view of a detour circuit provided in Figure 6(A).
[0053] A field effect transistor 12 is mounted on a substrate 7 of a TFT liquid crystal panel of an LCD (liquid crystal display), and metal conductors (first conductor A) 72, the main component of which is aluminum, are wired. One of the wires has a defect (disconnection) 722, and would normally be discarded as a defective product.
[0054] A substrate 7 having a defect (disconnection) 722 is repaired with a detour 76 made of a fired metal ink conductor (second conductor C) 27, thereby improving product yield.
[0055] There are various possible causes for the occurrence of the defect (disconnection) 722, but the main cause is the adhesion of dust. It is possible to directly connect the defect (disconnection) 722 in a straight line over the shortest distance, but since there is a possibility that dust or the like may remain, a detour route 76 is used instead. Of course, the defect (disconnection) 722 may also be repaired by directly connecting the defect (disconnection) 722 in a straight line over the shortest distance.
[0056] The detour path 76 using the silver metal ink 2 is fired by a firing laser 3 (not shown) to become a fired metal ink conductor (second conductor C) 27. As a result, in the conductive portion 9, the substrate 7, the metal conductor (first conductor A) 72, the natural oxidation layer (insulating layer B) 721, and the fired metal ink conductor (second conductor C) 27 are stacked in this order from the bottom up.
[0057] The melting laser 4 is irradiated to three points of each conductive portion 9 with different pulse energy intensities (see FIG. 2(C)).
[0058] The conductive portion 9 is formed in the molten region 8 formed around the three holes 74. If any one of the three molten regions 8 with different pulse energy intensities reaches the natural oxide layer (insulating layer B) 721, the electrical resistance between the metal conductor (first conductor A) 72 and the fired metal ink conductor (second conductor C) 27 is reduced to a level that does not affect the operation of the TFT liquid crystal panel. In addition, since a hole 74 surrounded by the molten region 8 is formed in the center of the molten region 8, the molten metal in the molten region 8 releases heat from the hole 74 and is quickly cooled, thereby reducing the thermal impact on the surrounding area of the molten region 8.
[0059] As in the second embodiment, the present invention can be used in a manufacturing method for a substrate (electronic component) of a TFT liquid crystal panel. Furthermore, the present invention can provide a substrate (electronic component) for a TFT liquid crystal panel having a conductive portion 9 provided with a molten area 8 in which the metal conductor (first conductor A) 72 and the baked metal ink conductor (second conductor C) 27, including the natural oxidation layer (insulating layer B) 721, are melted.
[0060] Furthermore, as described above, the TFT LCD panel substrate (electronic component) provided can be assembled with other components to create a product called a TFT LCD panel. In addition, the TFT LCD panel (electronic component) provided as described above can be assembled with other components to provide a product called an LCD display. The details of TFT LCD panels and LCD display technology and manufacturing methods are widely known and will not be described here.
[0061] Example 3 FIG. 7 is a cross-sectional view of a conductive portion 9 according to the third embodiment. In Examples 1 and 2, the natural oxide layer 721 was used as the insulating layer B. In Example 3, the insulating layer B is artificially created on the surface of the metal conductor (first conductor A). The second conductor C does not have to be a fired metal ink conductor. Furthermore, the first conductor A and the second conductor C may be made of the same metal material.
[0062] As one example, an example of a multilayer circuit board 5 is shown. In the multilayer circuit board 5, a large number of conductors are laminated with an insulating layer B sandwiched between them, such as a first conductor A, an insulating layer B, a second conductor C, an insulating layer B, the first conductor A, an insulating layer B, and a second conductor C.
[0063] By irradiating the laminated conductors with a melting laser 4, a conductive portion 9 is formed in a melted region 8 that melts the first conductor A, the second conductor C, and the insulating layer B. The melted region 8 becomes the conductive portion 9, and all of the laminated conductors can be made conductive.
[0064] Although the first to third embodiments of the present invention have been described above in detail with reference to the drawings, the specific configurations are not limited to these embodiments, and the present invention also includes design changes and the like within the scope of the present invention that do not deviate from the gist of the present invention. Furthermore, the above-described embodiments can be combined by utilizing each other's techniques, so long as there are no particular contradictions or problems in the objects, configurations, and the like. [Explanation of symbols]
[0065] A First Conductor B Insulation layer C Second conductor 2 Metal Ink 24 Metal Nanoparticles 25 Organic matter 26 Organic Solvents 27 Baked metal ink conductor (second conductor) 3. Firing laser 4. Melting Laser 41 Welding Lasers 412 Area affected by heat 5. Multilayer circuit board 7 Substrate 72 Metal conductor (first conductor) 721 Natural oxide layer (insulating layer) 722 Defect (disconnection) 73 Protective film 74 holes 75 Field-effect transistor 76 Detour circuit 8. Molten Zone 9 Conductive Part
Claims
1. A first step of laminating a second conductor on a first conductor having an insulating layer on a surface thereof; a second step of melting the first conductor and the second conductor including the insulating layer to create a melted region and forming a hole in the center of the melted region and surrounded by the melted region; Following the second step, A method for manufacturing a conductive part, comprising a third step of forming another molten region at a position different from the molten region formed in the second step, the molten region having a different depth from the molten region formed in the second step.
2. A first step of laminating a second conductor on a first conductor having an insulating layer on a surface thereof; a second step of melting the first conductor and the second conductor including the insulating layer to create a melted region and forming a hole in the center of the melted region and surrounded by the melted region; the insulating layer is a native oxide layer formed by oxidizing a metal of the first conductor; The method for manufacturing a conductive part, wherein the second conductor is a sintered metal ink conductor formed by sintering a metal ink.
3. 3. A method for manufacturing an electronic component, comprising the steps of: forming the conductive portion according to claim 1 on a substrate; and forming the conductive portion on the substrate.
4. A method for manufacturing a product, comprising assembling the electronic component of claim 3 with other electronic components to produce the product.
5. a first conductor, a second conductor, and a fusion region; the first conductor has an insulating layer on a surface thereof; the second conductor is laminated on the first conductor; the molten region is a region in which the first conductor and the second conductor, including the insulating layer, are melted, and the molten region has a hole at its center that is surrounded by the molten region; The conductive portion is characterized in that the melted regions are provided in two or more places, and the melted regions have different depths.
6. a first conductor, a second conductor, and a fusion region; the first conductor has an insulating layer on a surface thereof; the second conductor is laminated on the first conductor; the molten region is a region in which the first conductor and the second conductor, including the insulating layer, are melted, and the molten region has a hole at its center that is surrounded by the molten region; the insulating layer is a native oxide layer derived from a metal of the first conductor, The conductive portion, wherein the second conductor is a fired metal ink conductor formed by firing a metal ink.
7. The first conductor is disposed on a substrate, and the electronic component has the conductive portion according to claim 5 or 6.
8. A product incorporating the electronic component according to claim 7.
Citation Information
Patent Citations
Circuit board and repairs thereof
JP1988183481A
Resistance-trimming method for semiconductor integrated circuit
JP1989096954A
Processing method of metal film
JP1994314745A
Method of repairing aluminum thin film wiring
JP2000022306A
Conductive-material-contained liquid for repairing wiring on electronic circuit substrate, and method of repairing wiring on electronic circuit substrate
JP2005354009A