Martensitic stainless steel cutlery
A tailored martensitic stainless steel composition with controlled elements and heat treatment improves both sharpness and corrosion resistance, addressing the dual challenges of rust and edge retention in cutlery.
Patent Information
- Application Number
- JP2021070081
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-19
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-04-19
AI Technical Summary
Martensitic stainless steel cutlery with high carbon content faces issues with corrosion resistance due to exposure to acidic conditions, leading to rust formation and reduced sharpness, compromising both corrosion resistance and sharpness.
A specific composition of martensitic stainless steel with controlled amounts of C, N, Cr, and other elements, combined with heat treatment processes, enhances hardness, sharpness, and corrosion resistance.
The solution maintains high hardness and sharpness while improving toughness and corrosion resistance, ensuring durability and resistance to rust formation.
Smart Images

Figure 0007575785000004 
Figure 0007575785000001 
Figure 0007575785000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a cutting tool made of martensitic stainless steel. [Background technology]
[0002] Common blades, such as kitchen knives, are required to have a sharp cutting edge in order to cut things. In other words, if the cutting edge is sharp, the blade will be sharper and less force will be required to cut (cut) things. For this reason, martensitic stainless steels, which contain a relatively large amount of carbon in the material, are often used (see Patent Documents 1 and 2).
[0003] Among them, SUS440C, which contains more carbon than SUS420J2, is used. Because the steel contains a large amount of carbon, the hardness of the material increases and the blade can be finished to a sharper edge, improving cutting performance. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2002-212679 A [Patent Document 2] JP 2011-161064 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, if the material contains a large amount of carbon, its corrosion resistance will actually decrease. For example, when a knife made of martensitic stainless steel containing a large amount of carbon is washed in a dishwasher, the knife is exposed to high temperatures and an acidic atmosphere, which makes it prone to rust. In addition, there is also the problem that rust is likely to occur when highly acidic ingredients or seasonings adhere to the knife. Due to these factors, once small pieces of rust appear on the surface of the knife, the rust will become a resistance when cutting something, affecting the sharpness of the knife.
[0006] On the other hand, when the cutting edge of a highly corrosion-resistant knife, which is resistant to corrosion even when highly acidic food materials are attached to it or when it is washed in a dishwasher, is sharpened, the strength of the material decreases compared to martensitic stainless steel, which contains a lot of carbon, and there is a problem that the sharpness of the knife decreases. In other words, the corrosion resistance and sharpness of a knife are contradictory characteristics. This problem of achieving both corrosion resistance and sharpness is not limited to knives, but is a common problem for any object with a blade that cuts things.
[0007] Therefore, an object of the present invention is to provide a blade made of martensitic stainless steel that maintains the sharpness of the blade while ensuring corrosion resistance. [Means for solving the problem]
[0008] In order to solve the above-mentioned problems, the martensitic stainless steel which is the material for the blade of the present invention contains, by mass, C: 0.75-0.84%, Si: 0.25-0.45%, Mn: 0.65-0.75%, P: 0.035% or less, S: 0.010% or less, Cr: 17.00-19.00%, Ni: 0.30% or less, Cu: 0.25% or less, Mo: 1.50-1.90%, W: 0.40% or less, V: 0.20-0.40%, Co: 0.30% or less, Al: 0.20% or less, N: 0.16-0.25% and the remainder being Fe and unavoidable impurities.
[0009] The total content of C (carbon) and N (nitrogen) in the martensitic stainless steel is C+N≧1.00% (unit: mass%). Furthermore, the surface hardness is 62HRC or more on the Rockwell C scale.
[0010] Here, the term "blade" in the present invention includes not only kitchen knives and other knives used as cooking utensils, but also tools such as cutters and drills, and all other tools equipped with a blade for cutting objects. Effect of the Invention
[0011] In the present invention, by adding a specific amount of C (carbon), N (nitrogen), and Cr (chromium) to conventional martensitic stainless steel, the corrosion resistance of the blade is maintained while the blade has a high hardness, which allows it to be sharpened, improving the sharpness (cutting characteristics) of the blade. In addition, by ensuring sufficient toughness, ductility, and fatigue strength, the blade tip is less likely to break, and good sharpness can be maintained. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] An embodiment of the martensitic stainless steel blade of the present invention will be described. The reasons for specifying the chemical components of the martensitic stainless steel constituting the blade of the present invention within a predetermined range will be described for each component (element).
[0013] First, the C (carbon) content is 0.75 to 0.84%. If it is less than 0.75%, the amount of hard carbides formed in the structure is small, and as a result, the hardness after quenching and tempering cannot be secured. If it exceeds 0.84%, the amount of carbides formed in the structure is large, and the amount of solid solution of Cr, Mo, etc. in the matrix is reduced, so the corrosion resistance is reduced. In addition, large carbides are precipitated in the structure, which also reduces the toughness and fatigue strength.
[0014] The content of Si (silicon) is 0.25 to 0.45%. Si is a deoxidizing element, and is added in place of Al, which is a similar deoxidizing element, to suppress the formation of AlN (aluminum nitride), which significantly reduces toughness and ductility. If the content is less than 0.25%, the effect as a deoxidizing material cannot be exhibited, and a large amount of oxygen remains, resulting in a decrease in toughness and ductility. If the content is more than 0.45%, the hot and cold workability as a martensitic stainless steel decreases, and the toughness also decreases. Furthermore, the content of Mn (manganese) is 0.65 to 0.75%. Mn is an element that is effective in increasing the amount of solid solution of N (nitrogen). It is also effective as a deoxidizing and desulfurizing element. If the content is less than 0.65%, a sufficient amount of solid solution of N cannot be secured. If the content is more than 0.75%, the amount of retained austenite increases, resulting in a decrease in tempering hardness and a decrease in corrosion resistance.
[0015] P (phosphorus) should be 0.035% or less. If it exceeds 0.035, segregation occurs at the grain boundaries, reducing toughness. S (sulfur) should be 0.010% or less. If it exceeds 0.010%, sulfides are formed in the structure, reducing toughness.
[0016] Cr (chromium) is 17.00 to 19.00%. If it is less than 17.00%, sufficient corrosion resistance as a martensitic stainless steel cannot be obtained. On the other hand, if it exceeds 19.00%, macrocarbides are precipitated in the structure, reducing toughness.
[0017] Ni (nickel) should be 0.30% or less. If it exceeds 0.30%, the amount of retained austenite in the structure increases, causing dimensional changes over time. It also reduces cold workability. Cu (copper) should be 0.25% or less. If it exceeds 0.25%, the amount of retained austenite in the structure increases, causing dimensional changes over time. It also reduces hot workability.
[0018] Mo (molybdenum) should be 1.50-1.90%. If it is less than 1.50%, corrosion resistance will decrease and secondary hardening by tempering will not be sufficient. If it exceeds 1.90%, giant carbides will precipitate in the structure and toughness will decrease. W (tungsten) should be 0.40% or less. If it exceeds 0.40%, giant carbides will precipitate in the structure and toughness will decrease.
[0019] The V (vanadium) content is 0.20% to 0.40%. If it is less than 0.20%, the secondary hardening after tempering is insufficient. If it is more than 0.40%, macrocarbides precipitate in the structure, reducing toughness.
[0020] Co (cobalt) should be 0.30% or less. Exceeding 0.30% will increase material costs, which will lead to higher manufacturing costs. Furthermore, Al (aluminum) should be 0.20% or less. Exceeding 0.20% will combine with O (oxygen) in the structure to form coarse oxides, or combine with N (nitrogen) to form aluminum nitride, reducing toughness and fatigue strength.
[0021] N (nitrogen) should be 0.16 to 0.25% (1600 to 2500 ppm by mass). If it is below 0.16%, sufficient corrosion resistance and hardness after quenching and tempering cannot be obtained. Also, if it exceeds 0.25%, blowholes (cavities) will occur inside the material.
[0022] The total content of C (carbon) and N (nitrogen) in the entire martensitic stainless steel must be C+N≧1.00% (unit: mass%). If it is less than 1.00%, it becomes difficult to achieve both sharpness and corrosion resistance when made into a blade.
[0023] In addition, as for heat treatment, after quenching, sub-zero treatment is performed to reduce the residual austenite, and by tempering treatment, toughness and ductility are imparted, and good sharpness and corrosion resistance can be obtained. [Brief description of the drawings]
[0024] [Figure 1]1 is a photograph of a polished surface after a salt spray test in Example 3 of the present invention. EXAMPLES
[0025] Example 1 In order to evaluate the sharpness of knives made from various materials, including martensitic stainless steel, we conducted a Honda sharpness test, and we will explain the results of that test below. In the Honda sharpness test, the blade to be tested (test piece) is fixed in a special machine (Honda sharpness tester) with the cutting edge facing up, and a stack of papers with a certain load applied is placed on the cutting edge.
[0026] After that, the tester is turned on and the stack of paper is cut by going back and forth once on the blade. The number of sheets of paper cut during this process is used to quantitatively evaluate the sharpness of the blade.
[0027] The materials of the blades used in this test were 10 types of steel, including the martensitic stainless steel invented material (1 type of steel) and comparative materials 1 to 9 (total of 9 types of steel), including conventional steels such as SUS440C and SUS420J2. The chemical compositions (unit: mass%) of these 10 types of steel are shown in Table 1.
[0028] [Table 1]
[0029] Other test conditions were as follows: Paper stack movement distance: 20mm -Width of paper used: 7.5mm Load capacity: 750g Table 2 shows the test results for each test piece used in this test.
[0030] [Table 2]
[0031] According to the test results shown in Table 2, the blade made of the material of the present invention cut 111 pieces of paper. In contrast, the comparative material 5, which had a low C ratio and C+N of less than 1%, cut 59 pieces of paper, and the most cut was 84 pieces of paper in the case of the comparative material 7, which used a blade made of SUS440C steel. Therefore, it was confirmed that the blade made of the material of the present invention has improved sharpness (cutting characteristics) compared to blades made of conventional steel.
[0032] Example 2 Next, a wear resistance test was conducted for each of the above-mentioned steel types to confirm their durability as blade materials, and the test results are described below. Test pieces (2 mm length × 10 mm width × 35 mm height) were prepared for each of the 10 steel types used in the above-mentioned Example 1 after quenching and tempering treatment, and each test piece was polished for 15 minutes with a polishing machine at a rotation speed of 200 rpm and a load of about 200 N, using emery paper (#80) as the mating material.
[0033] After polishing for 15 minutes under the above test conditions, the weight loss of each test piece was measured and the amount of wear was compared. The surface hardness (Rockwell C scale: HRC) and amount of wear (unit: g) of each test piece are shown in Table 3.
[0034] [Table 3]
[0035] As shown in Table 3, the test results of this example show that the wear amount of the material of the present invention, which has the highest hardness of HRC62.1, was 2.05 g. On the other hand, the test results of the comparative materials show that even the comparative material 5, which had a relatively small wear amount, had a wear amount of 2.18 g. From the above test results, it was found that the material of the present invention is superior to the other nine steel types in terms of wear resistance.
[0036] Example 3 Next, a salt spray test was conducted to confirm the corrosion resistance of the blade material. The blade materials used in this test were four steel types in total, including the inventive material used in Examples 1 and 2, comparative material 5, which has a low C ratio and C+N of less than 1%, comparative material 6, which is SUS420J2, and comparative material 7, which is SUS440C.
[0037] In this test, the material of the present invention and comparative material 5 were hardened at 1060°C, comparative material 6 at 1030°C, and comparative material 7 at 1050°C, and then sub-zero treated. The material of the present invention and comparative material 5 were further tempered at 180°C, and comparative materials 6 and 7 at 150°C.
[0038] After the heat treatment, each steel material was processed into a test plate of 18 mm x 18 mm, embedded in epoxy resin, and the end faces were polished to a roughness of 1000 to prepare a test specimen. For the evaluation, the number and depth of pits were measured in a 14 mm x 14 mm area excluding the ridges on the polished surface of the test specimen.
[0039] Other test conditions were as follows: Number of test pieces: N=3 · Solution used: 5% NaCl aqueous solution Spray conditions: 35℃, 75kPa, 24 hours of continuous spraying
[0040] Photographs of the polished surfaces of each steel material after this test are shown in Figure 1. Figure 1(a) is a photograph of the inventive material, Figure 1(b) is a photograph of comparative material 5, Figure 1(c) is a photograph of comparative material 6 (SUS420J2), and Figure 1(d) is a photograph of comparative material 7 (SUS440C).
[0041] As a result of evaluating the total number of pits and their depth for N=3, the inventive material had 3 pits, with the deepest pitting being 4.9 um. In contrast, comparative material 5 had 1 pit, with the deepest being 2.7 um. Comparative material 6 (SUS420J2) had 101 pits, with the deepest being 30 um. Comparative material 7 (SUS440C) had 87 pits, with the deepest being 108 um. From the above test results, it was found that the inventive material has corrosion resistance equivalent to comparative material 5, and has superior corrosion resistance compared to comparative materials 6 and 7.
Claims
1. A martensitic stainless steel blade characterized in that it is formed from a martensitic stainless steel having, by mass%, C: 0.75-0.84%, Si: 0.25-0.45%, Mn: 0.65-0.75%, P: 0.035% or less, S: 0.010% or less, Cr: 17.00-19.00%, Ni: 0.30% or less, Cu: 0.25% or less, Mo: 1.50-1.90%, W: 0.40% or less, V: 0.20-0.40%, Co: 0.30% or less, Al: 0.20% or less, N: 0.16-0.25%, with the remainder consisting of Fe and unavoidable impurities, and C+N≧1.00%.
2. 2. The martensitic stainless steel cutting tool according to claim 1, characterized in that the surface hardness is 62 HRC or more on the Rockwell C scale.
Citation Information
Patent Citations
Tool high molybdenum martensitic stainless steel with toughness and corrosion resistance superior to toughness and corrosion resistance of 9Cr18MoV and method
CN110923579A
Manufacture of high carbon containing stainless steel having uniformly fine carbide structure
JP1990166228A
Production of high carbon stainless steel strip having uniform fine carbite structure and excellent impact toughness
JP1994065639A
Stainless steel for cutting tool, excellent in corrosion resistance, durability of cutting quality, and workability
JP2000273587A
EDGE TOOL AND Fe-BASED ALLOY FOR EDGE TOOL USED THEREFOR
JP2002212679A